Flux-cored wire for submerged arc welding for high-tensile strength steel and submerged arc welding method for high-tensile strength steel

Optimized flux-cored wires with specific alloy compositions and sintered fluxes address the challenges of high-strength steel welding, achieving high-strength, tough weld metals with low hydrogen and improved workability, overcoming productivity and defect issues.

JP2024141460AActive Publication Date: 2024-10-10NIPPON STEEL WELDING & ENGINEERING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023053133
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Conventional flux-cored wires for submerged arc welding of high-strength steel face challenges in achieving weld metals with high strength and toughness, low diffusible hydrogen content, and good welding workability, often leading to productivity issues and weld defects.

Method used

Optimizing the alloy composition of flux-cored wires with specific ranges of C, Si, Mn, Ni, Mo, Al, and CaF2, along with appropriate amounts of alkali metal compounds, and combining them with sintered flux to achieve high-strength, high-toughness weld metals with low diffusible hydrogen and improved welding workability.

Benefits of technology

The solution results in weld metals with tensile strength of 780 MPa or more, excellent low-temperature toughness, good bead shape, and no defects, ensuring high-quality welded parts with low diffusible hydrogen content and stable arcs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141460000001
    Figure 2024141460000001
  • Figure 2024141460000002
    Figure 2024141460000002
  • Figure 2024141460000003
    Figure 2024141460000003
Patent Text Reader

Abstract

To provide a flux-cored wire for submerged arc welding with which a weld metal having good welding workability and excellent mechanical performance can be obtained in requirement of the high quality of high-tensile strength steel.SOLUTION: A flux-cored wire for submerged arc welding includes C: 0.03-0.15%, Si: 0.05-0.5%, Mn: 1.2-3.2%, Ni: 0.5-3.5%, Mo: 0.03-1.0%, and Al: 0.01-0.05% in the total of one or both of the steel outer skin and the filling flux in the total mass percent of the flux-cored wire; and, in a filling flux, CaF2: 2-12%, metallic carbonate CO2: 0.05-0.7%, and 0.01-0.2% total of alkali metallic compound Na2O converted value and Li2O converted value; the balance of Fe in the steel outer skin, Fe in alloyed powder, iron powder; and inevitable impurities.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to submerged arc welding of high tensile steel, and to a submerged arc welding method for high tensile steel which provides a weld metal with excellent strength and low temperature toughness, a low amount of diffusible hydrogen in the weld metal, is free of welding defects, and provides good welding workability such as bead shape and slag removability, and to a flux-cored wire for submerged arc welding of high tensile steel which is applied to said welding method. [Background technology]

[0002] Submerged arc welding is highly efficient and produces weld metal with good welding workability and excellent mechanical properties, and is therefore used in a wide range of fields, such as shipbuilding, steel frame construction, pipe construction, bridges, and vehicles.

[0003] In recent years, with the development of the energy industry, the need for higher strength and toughness in steel materials, as well as the need for extremely thick plates to accommodate larger structures, has been considered, and the ratio of applications of submerged arc welding is increasing year by year from the standpoint of quality and productivity. In the submerged arc welding of such high-tensile steel, further quality improvements are required to improve productivity in welding work and ensure safety and durability. In particular, there is a demand for high welding efficiency and strength and toughness of the weld metal that match the steel characteristics, and the demand for flux-cored wire for submerged arc welding of high-tensile steel is increasing.

[0004] Conventionally, solid wires containing alloying elements such as Ni, Mn, and Mo have been mainly used for submerged arc welding of high-tensile steels in order to toughen the weld metal. However, when the amount of alloying elements in the wire is increased to toughen the weld metal, the wire itself becomes strong, and the wire becomes even harder due to work hardening during the wire drawing process for manufacturing welding wire. When the wire becomes hard, die wear and wire breakage become frequent, which causes problems in productivity efficiency.

[0005] In addition, when a high-strength solid wire is used for welding, it is difficult to straighten the wire, and the center of the groove is easily shifted, making it difficult to obtain a good bead. Thus, the high-strength solid wire has the problem of reduced productivity and weldability.

[0006] For this reason, various flux-cored wires for submerged arc welding have been developed. However, in order to obtain a weld metal with high toughness, the oxygen content of the weld metal must be low, and since welding of high-tensile steel is prone to cold cracking, the flux-cored wire must have a low hydrogen content, which has made it difficult to apply conventional flux-cored wires.

[0007] In consideration of these points, attempts have been made to develop a flux for submerged arc welding that can provide good mechanical properties of the weld metal and good welding workability, and to develop a wire for submerged arc welding that has good wire productivity and weldability.

[0008] For example, Patent Document 1 discloses a submerged arc welding method for low-temperature steels, which can obtain a weld metal with low oxygen and nitrogen contents and high toughness by combining a flux-cored wire with a molten flux. However, the technology disclosed in Patent Document 1 does not contain Al in an appropriate range, so that a weld metal having a strength of 780 MPa or more cannot be stably obtained. In addition, the technology disclosed in Patent Document 1 has a problem that cracks are likely to occur in the weld metal due to a high amount of diffusible hydrogen. Furthermore, in the technology disclosed in Patent Document 1, when the flux combined with the submerged arc welding of high-tensile steel is a molten flux, it is difficult to add alloy elements, so that the application of the technology to the submerged arc welding of high-tensile steels is not very preferable from the viewpoint of the amount of diffusible hydrogen in the weld metal. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2013-91082 A Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention has been devised in view of the above-mentioned problems, and has an object to provide a flux-cored wire for submerged arc welding which is capable of producing a weld metal having good welding workability and excellent mechanical properties in the high quality required for high tensile steel having a tensile strength of 780 MPa or more. [Means for solving the problem]

[0011] In order to solve the above problems, the inventors of the present invention have conducted detailed studies on the chemical composition of the flux-cored wire, and have found that optimizing the alloy composition of the flux-cored wire makes it possible to obtain a weld metal with high strength and high toughness due to low oxygen content, and thus to obtain good welding workability and bead shape, a low amount of diffusible hydrogen in the deposited metal, and a high-quality weld without welding defects.

[0012] That is, the gist of the present invention is characterized in that (1) the total of one or both of the steel sheath and the filled flux contains, in mass % relative to the total mass of the wire, 0.03-0.15% C, 0.05-0.5% Si, 1.2-3.2% Mn, 0.5-3.5% Ni, 0.03-1.0% Mo, and 0.01-0.05% Al, and further contains, in mass % relative to the total mass of the wire, 2-12% CaF2, 0.05-0.7% total of metal carbonates in terms of CO2, and 0.01-0.2% total of one or more of alkali metal compounds in terms of Na2O, K2O, and Li2O, with the remainder being Fe in the steel sheath, Fe in the alloy powder, iron powder, and unavoidable impurities.

[0013] (2) The welding is performed by combining a sintered flux consisting of, in mass % relative to the total mass of the sintered flux, 10-23% SiO2, 20-35% Al2O3, 20-30% MgO, 5-20% CaO, 5-20% CaF2, 2-7% total of one or more of CaCO3, MgCO3 and Li2CO3 calculated as CO2, and the remainder being alkali metal oxides and unavoidable impurities, with the flux-cored wire for submerged arc welding of high tensile steel according to (1). Effect of the Invention

[0014] According to the flux-cored wire for submerged arc welding of high tensile steel to which the present invention is applied, in submerged arc welding of high tensile steel having a tensile strength of 780 MPa or more, it is possible to obtain a weld metal having excellent strength and low temperature toughness, a low amount of diffusible hydrogen in the weld metal, and a high quality weld having good welding workability such as bead shape and slag removability and free from welding defects. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] In order to solve the above-mentioned problems, the inventors have investigated the chemical components and their contents in the total of one or both of the steel sheath and filled flux of a flux-cored wire for submerged arc welding (hereinafter referred to as flux-cored wire), as well as the chemical components and their contents of a baked flux to be used in combination with the wire for welding.

[0016] As a result, it was found that the strength and low-temperature toughness of the weld metal can be ensured by appropriately adjusting the amounts of C, Si, Mn, Ni, and Mo in the chemical components of the flux-cored wire. It was also found that the oxygen content of the weld metal can be reduced by appropriately adjusting the amounts of C, Si, Mn, and Al, thereby improving the low-temperature toughness. It was also found that the amount of diffusible hydrogen can be reduced by appropriately adding CaF2 and metal carbonate. It was also found that the arc stability can be improved by appropriately adding an alkali metal compound, thereby improving the welding workability. It was also found that the flux-cored wire can be combined with a sintered flux to improve the high strength and low-temperature toughness of the weld metal and to reduce the amount of diffusible hydrogen. It is necessary to add a deoxidizer or the like to the sintered flux to maintain the mechanical performance of the weld metal, to keep the oxygen content of the weld metal low, and to improve the hardenability. It was also found that the amount of diffusible hydrogen in the weld metal can be further reduced by adjusting CaF2, CaCO3, etc.

[0017] From the above, it has been found that by limiting the total chemical components and their contents of either or both of the steel outer sheath and filled flux of a flux-cored wire, and further combining this with a sintered flux for welding, it is possible to obtain a weld metal with high strength and high toughness in submerged arc welding of high tensile steel, as well as to obtain good welding workability and bead shape, a low amount of diffusible hydrogen in the weld metal, and a high-quality weld without welding defects.

[0018] The reasons for limiting the composition of the flux-cored wire to which the present invention is applied will be described below. Note that % for the following components indicates mass % with respect to the total mass of the flux-cored wire.

[0019] [C: 0.03~0.15% in total for either or both of the steel sheath and filling flux] The C in the wire composition is an important element for ensuring the strength of the weld metal by solid solution strengthening. In addition, C has the effect of improving low-temperature toughness by reducing the oxygen content in the weld metal. If the C content is less than 0.03%, the effect of ensuring strength is insufficient, and the deoxidizing effect is insufficient, resulting in a decrease in low-temperature toughness. On the other hand, if the C content exceeds 0.15%, the C content in the weld metal becomes high, so that the strength becomes excessively high and the low-temperature toughness decreases. Therefore, the C content in the wire composition is set to 0.03 to 0.15%. In addition to the components contained in the steel sheath, C can be added from metal powder and alloy powder from the filling flux, and these metal powders and alloy powders are different from iron powders that are intentionally added to adjust the components.

[0020] [Si: 0.05~0.5% in total for either or both of the steel sheath and filling flux] The wire component Si has the effect of improving the strength of the weld metal and reducing the oxygen content of the weld metal by combining with oxygen during welding to form a slag component, thereby improving low-temperature toughness. If the Si content is less than 0.05%, the strength of the weld metal will be low and the oxygen content of the weld metal will be high, reducing low-temperature toughness. On the other hand, if the Si content exceeds 0.5%, the ferrite grains will become coarse, significantly reducing low-temperature toughness. Therefore, the Si content is set to 0.05 to 0.5%. In addition to being a component contained in the steel sheath, Si can be added from metal Si, Fe-Si, Fe-Si-Mn, and other alloy powders from the filling flux.

[0021] [Mn: 1.2-3.2% in total for either or both of the steel sheath and filling flux] Mn, a wire component, is an effective component for improving the hardenability and improving the strength and low-temperature toughness of the weld metal. If the Mn content is less than 1.2%, the hardenability is insufficient, resulting in low strength and low-temperature toughness. On the other hand, if the Mn content exceeds 3.2%, the hardenability becomes excessive, the strength of the weld metal becomes excessively high, and the low-temperature toughness decreases. Therefore, the Mn content is set to 1.2 to 3.2%. In addition to being a component contained in the steel sheath, Mn can be added from metallic Mn, Fe-Mn, Fe-Si-Mn, and other alloy powders from the filling flux.

[0022] [Ni: 0.5~3.5% in total for either or both of steel sheath and filled flux] The Ni in the wire component is an effective component for improving the low-temperature toughness of the weld metal. If Ni is less than 0.5%, the low-temperature toughness of the weld metal decreases. On the other hand, if Ni exceeds 3.5%, the austenite grain size becomes coarse, degrading the low-temperature toughness of the weld metal. Therefore, the Ni in the wire component is set to 0.5 to 3.5%. In addition to being a component contained in the steel sheath, Ni can be added from metallic Ni from the filling flux, or from alloy powder such as Fe-Ni.

[0023] [Mo: 0.03~1.0% in total for either or both of steel sheath and filled flux] The Mo content of the wire is effective in ensuring the strength of the weld metal. If the Mo content is less than 0.03%, the strength of the weld metal will be low. On the other hand, if the Mo content exceeds 1.0%, the weld metal will be significantly hardened and its low-temperature toughness will be reduced. Therefore, the Mo content of the wire is set to 0.03 to 1.0%. In addition to being a component contained in the steel sheath, Mo can be added from metallic Mo in the filling flux or alloy powder such as Fe-Mo.

[0024] [Aluminum: 0.01-0.05% in total for either or both of the steel sheath and filling flux] The Al wire component has the effect of improving the strength of the weld metal and improving low-temperature toughness by reducing the amount of oxygen in the weld metal. If the Al content is less than 0.01%, the strength and low-temperature toughness of the weld metal will be reduced. On the other hand, if the Al content exceeds 0.05%, the amount of oxygen in the weld metal will be excessively reduced, and the low-temperature toughness will deteriorate due to an increase in the yield of C, Si, and Mn and coarse Al oxides. Therefore, the Al wire component is set to 0.01 to 0.05%. Note that Al can be added from the components contained in the steel sheath, metallic Al from the filling flux, and alloy powder such as Fe-Al.

[0025] [CaF2 in filled flux: 2-12%] CaF2 in the filled flux has the effect of improving low-temperature toughness by reducing the oxygen content of the weld metal, and also has the effect of reducing the amount of diffusible hydrogen in the weld metal. If the CaF2 content is less than 2%, the oxygen content of the weld metal increases, reducing low-temperature toughness, and the effect of reducing the amount of diffusible hydrogen in the weld metal cannot be obtained. On the other hand, if the CaF2 content exceeds 12%, the arc becomes unstable and the bead shape becomes poor. Therefore, the CaF2 content is set to 2-12%. CaF2 can be added from fluorite, etc., in the filled flux.

[0026] [Total CO2 equivalent value of metal carbonates in filled flux: 0.05~0.7%] The metal carbonate in the filling flux is effective in improving low-temperature toughness by reducing the nitrogen content of the weld metal. The metal carbonate also has the effect of reducing the amount of diffusible hydrogen in the weld metal. If the total CO2 equivalent value of the metal carbonate is less than 0.05%, the nitrogen content of the weld metal increases and the low-temperature toughness decreases. If the total CO2 equivalent value of the metal carbonate is less than 0.05%, the effect of reducing the amount of diffusible hydrogen in the weld metal cannot be obtained. On the other hand, if the total CO2 equivalent value of the metal carbonate exceeds 0.7%, pockmarks, undercuts, and even blowholes are likely to occur on the weld bead surface. Therefore, the total CO2 equivalent value of the metal carbonate is 0.05 to 0.7%. The metal carbonate can be added from calcium carbonate, magnesium carbonate, barium carbonate, etc. from the filling flux.

[0027] [Total of one or more of the Na2O equivalent, K2O equivalent, and Li2O equivalent values ​​of alkali metal compounds: 0.01 to 0.2%] The alkali metal compound in the filled flux has the effect of stabilizing the arc. If the total of one or more of the Na2O equivalent, K2O equivalent, and Li2O equivalent of the alkali metal compound is less than 0.01%, the effect is not sufficiently obtained and the arc becomes unstable. On the other hand, if the total of one or more of the Na2O equivalent, K2O equivalent, and Li2O equivalent of the alkali metal compound exceeds 0.2%, the bead wave becomes disordered and the bead shape becomes poor. Therefore, the total of one or more of the Na2O equivalent, K2O equivalent, and Li2O equivalent of the alkali metal compound is 0.01 to 0.2%. The alkali metal compound refers to a solid component of water glass made of sodium silicate or potassium silicate, a fluorine compound such as sodium fluoride, lithium fluoride, and potassium silicofluoride, and a complex compound such as potassium feldspar and lithium titanate.

[0028] In addition to the above-mentioned components of the flux-cored wire, Ti, B, etc. may be contained within a range that does not impair the effects of the present invention. The balance is Fe in the steel sheath, Fe in the alloy powder, iron powder added to adjust the components, Cu from the copper plating on the wire surface, and unavoidable impurities such as P and S.

[0029] Next, the chemical components of the sintered flux will be described. Note that the percentages for the components below indicate mass % relative to the total mass of the sintered flux.

[0030] [SiO2: 10-23%] SiO2 has the effect of adjusting the viscosity of slag and improving the slag removability. If SiO2 is outside the range of 10-23%, it is difficult to obtain these effects. SiO2 can be added from raw materials such as silica sand and water glass.

[0031] [Al2O3: 20~35%] Al2O3 has the effect of improving arc stability and slag removability. If Al2O3 is outside the range of 20-35%, it is difficult to obtain these effects. Al2O3 can be added from alumina, etc. as a raw material.

[0032] [MgO: 20~30%] MgO has the effect of improving low-temperature toughness by increasing the basicity of the slag and reducing the amount of oxygen in the weld metal. If the MgO content is outside the range of 20-30%, it is difficult to obtain these effects. MgO can be added from magnesia clinker and other raw materials.

[0033] [CaO: 5-20%] CaO is an important component for adjusting the melting point and fluidity of slag, and has the effect of improving slag removability. If CaO is outside the range of 5-20%, it is difficult to obtain these effects. CaO can be added from raw materials such as wollastonite and calcium oxide.

[0034] [CaF2: 5-20%] CaF2 is effective in improving low-temperature toughness. It also has the effect of reducing the amount of diffusible hydrogen in the weld metal. If the CaF2 content is outside the range of 5-20%, it is difficult to obtain these effects. CaF2 can be added from fluorite and other raw materials.

[0035] [CaCO3, MgCO3 and Li2CO3, one or more of which are converted into CO2: 2-7%] The CO2 conversion from CaCO3, MgCO3 and Li2CO3 is effective in improving low-temperature toughness by reducing the nitrogen content of the weld metal. If the total of one or more types of CaCO3, MgCO3 and Li2CO3 in CO2 conversion is outside the range of 2-7%, it is difficult to obtain these effects. CaCO3, MgCO3 and Li2CO3 can be added from calcium carbonate, magnesium carbonate, lithium carbonate, etc. as raw materials.

[0036] The remainder of the sintered flux is 5% or less, consisting of alkali metal oxides such as K2O and Na2O from the water glass, and unavoidable impurities such as P and S. In addition, since both P and S form compounds with low melting points and reduce toughness, it is preferable that the content is as low as possible.

[0037] [Wire form] The flux-cored wire used in the present invention has a structure in which a steel sheath is formed into a pipe shape and filled with a filling flux. The types of wire can be roughly divided into seamless wires that penetrate the steel sheath and wires that have a joint in the steel sheath. Of these, seamless wires that penetrate the steel sheath can be heat-treated by annealing in a temperature range of 650 to 1000°C for the purpose of reducing the total hydrogen content of the wire, and they do not absorb moisture after production, so that it is preferable to use seamless wires from the viewpoint of the amount of diffusible hydrogen.

[0038] [Total water content] The total hydrogen content in the flux-cored wire increases as the total hydrogen content in the weld metal increases, so although there is no particular regulation, it is preferable to keep the total hydrogen content in the wire at 200 ppm or less. EXAMPLES

[0039] The effects of the present invention will now be described in more detail with reference to examples.

[0040] Using the steel outer sheath shown in Table 1, various flux-cored wires shown in Table 2 were prototyped, and in order to evaluate the welding workability and mechanical performance by combining them with sintered fluxes of various compositions shown in Table 3, a 780 MPa class steel plate with a thickness of 25 mm and made of the chemical composition shown in Table 4 was processed into a groove shape with a groove angle of 30° and a root spacing of 13 mm, and a backing metal was applied, and a multi-layer welding test was conducted under the welding conditions shown in Table 5.

[0041] The flux-cored wires shown in Table 2 were made using the steel sheaths shown in Table 1, and the steel strips were formed into a U-shape in the forming process, filled with flux, and then formed into an O-shape, the joints were welded, and then the wires were reduced in diameter, annealed, and plated. These wires were then drawn to a diameter of 4.0 mm. The filling rate of the filled flux was 9 to 20%.

[0042] The sintered flux shown in Table 3 was prepared by compounding and mixing various mineral raw materials, granulating them using water glass as a binder, and then sintering them at 400 to 550°C for 2 hours to granulate them to 1.4 x 0.15 mm.

[0043] [Table 1]

[0044] [Table 2]

[0045] [Table 3]

[0046] [Table 4]

[0047] [Table 5]

[0048] The combinations of various prototype flux-cored wires and baked fluxes are shown in Table 6. The evaluation of each test was carried out by investigating the arc stability during multi-pass welding, bead shape, slag removability, and the presence or absence of welding defects by X-ray examination, and also by investigating the mechanical performance of the weld metal.

[0049] (Arc Stability) The welding voltage was judged as stable when it was constant and had little fluctuation during welding. The welding voltage was judged as extremely stable when it was constant and had almost no fluctuation during welding.

[0050] (Bead shape) Beads with uniform width, waviness and surface condition, and free of pockmarks, undercuts, etc., were rated as "good."

[0051] (Slag removability) After welding, when the solidified slag was struck with a chipping hammer, if the slag cracked and could then be easily removed, it was judged as "good." If the slag peeled off after welding, it was judged as "extremely good."

[0052] (Welding defects) In the X-ray transmission test, the test was performed based on the radiographic transmission test for steel welded joints shown in JIS Z3104:1995, and cases where no blowholes or cracks were found were rated as "no."

[0053] (Machine performance evaluation) For the mechanical performance evaluation of the weld metal, impact test pieces (JIS Z 2242:2018 V-notch test pieces) and tensile test pieces (JIS Z 2241:2011 No. 10) were taken from the center of the steel plate of the welded test specimen, and mechanical tests were performed. The toughness was evaluated by impact testing at -60°C, and was evaluated from the average of three repetitions. The absorbed energy of the impact test was rated as good if it was 90 J or more. The tensile strength was rated as good if it was 780 to 890 MPa. The amount of diffusible hydrogen in the weld metal was measured in accordance with JIS Z3118:2007. The amount of diffusible hydrogen in the weld metal was rated as good if it was 2.5 ml / 100 g or less. The results of these investigations are also summarized in Table 5.

[0054] [Table 6]

[0055] In Table 6, test symbols T1 to T13 are examples of the present invention, and test symbols T14 to T25 are comparative examples. The flux-cored wires of test symbols T2, T3, T7, T9, T12, and T13, which are examples of the present invention, satisfy the constituent requirements of the present invention, so the arc is stable, the welding workability such as bead shape and slag removability is good, there are no welding defects, and the tensile strength and absorbed energy of the weld metal are also good, resulting in satisfactory results. For test symbols T1, T4 to T6, T8, T10, and T11, both the sintered flux combined with the flux-cored wire satisfy the constituent requirements of the present invention, so the arc is extremely stable, the bead shape is good, the slag removability is extremely good, the tensile strength of the weld metal is good, and the absorbed energy is 100 J or more, resulting in extremely satisfactory results.

[0056] Among the comparative examples, test code T14 had a low C content compared to wire code W14, so the tensile strength of the weld metal was low and the absorbed energy was low.

[0057] Test code T15 had a high C content compared to wire code F15, which resulted in an excessively high tensile strength of the weld metal and a low absorbed energy. In addition, the total of one or more of the Na2O equivalent, K2O equivalent, and Li2O equivalent values ​​of alkali metal compounds was low, resulting in an unstable arc.

[0058] Test code T16 had less Si than wire code W16, so the tensile strength of the weld metal was low and the absorbed energy was low.

[0059] Test code T17 had a higher Si content than wire code W17, so the absorbed energy of the weld metal was lower.

[0060] Test code T18 had a low Mn content compared to wire code W18, so the tensile strength of the weld metal was low and the absorbed energy was low. Also, the high CaF2 content caused the arc to become unstable, resulting in a poor bead shape.

[0061] Test code T19 had a higher Mn content than wire code W19, so the tensile strength of the weld metal was excessively high and the absorbed energy was low.

[0062] The test code T20 had a lower Ni content than the wire code W20, so the absorbed energy of the weld metal was lower.

[0063] Test code T21 had a higher Ni content than wire code W21, so the absorbed energy of the weld metal was low.

[0064] Test code T22 had low tensile strength of weld metal because it contained less Mo than wire code W22. Also, because it contained a large total of metal carbonate CO2 equivalent, pockmarks and undercuts occurred in the bead, the bead shape was poor, and blowholes occurred.

[0065] Test code T23 contains a large amount of Mo compared to wire code W23, so the tensile strength of the weld metal was excessively high and the absorbed energy was low.

[0066] Test code T24 had a low Al content compared to wire code W24, so the tensile strength of the weld metal was low and the absorbed energy was low. Also, the total of one or more of the Na2O equivalent, K2O equivalent, and Li2O equivalent values ​​of alkali metal compounds was high, so the bead wavy pattern was irregular and the bead shape was poor.

[0067] The test code T25 has a higher Al content than the wire code W25, so the absorbed energy of the weld metal was low.

[0068] Test code T26 had less CaF2 than wire code W26, so the absorbed energy of the weld metal was low and the amount of diffusible hydrogen in the weld metal was high.

[0069] Test code T27 had a lower total CO2 equivalent value of metal carbonate than wire code W27, so the absorbed energy of the weld metal was low, and the amount of diffusible hydrogen in the weld metal was high.

Claims

1. The total of the steel sheath and / or the flux filling, expressed as a percentage by mass relative to the total mass of the wire, C: 0.03-0.15%, Si: 0.05-0.5%, Mn: 1.2 to 3.2%, Ni: 0.5-3.5%, Mo: 0.03-1.0%, Al: 0.01 to 0.05%; Furthermore, in terms of mass% relative to the total mass of the wire, the filled flux contains CaF 2 : 2-12%, Metal carbonate CO 2 Total conversion value: 0.05-0.7%, Alkali metal compounds of Na 2 O equivalent value, K 2 O equivalent value and Li 2 One or more total amounts of O: 0.01 to 0.2%; A flux-cored wire for submerged arc welding of high tensile steel, the balance of which consists of Fe in the steel sheath, Fe in the alloy powder, iron powder, Cu from the copper plating on the wire surface, and unavoidable impurities.

2. The mass percentage of the total mass of the sintered flux is SiO 2 : 10-23%, A 2 O 3 : 20-35%, MgO: 20-30%, CaO: 5-20%, CaF 2 : 5-20%, CaCO 3 , MgCO 3 and Li 2 CO 3 One or more of the following CO 2 Total conversion: 2-7%, 2. A method for submerged arc welding of high tensile steel, comprising the steps of: combining a sintered flux, the balance of which is composed of alkali metal oxides and unavoidable impurities, with the flux-cored wire for submerged arc welding of high tensile steel as set forth in claim 1;

Citation Information

Patent Citations

  • Submerged arc welding method for low-temperature steel

    JP2013091082A