Epoxy resin composition

By incorporating a liquid phenolic resin with an aliphatic carbon-carbon double bond, a microcapsule-type curing accelerator, and an imidazole compound with a triazine ring, the epoxy resin composition addresses curability and storage stability issues, providing enhanced adhesive strength for electronic and automotive applications.

JP2024141554APending Publication Date: 2024-10-10SHIN ETSU CHEMICAL CO LTD

Patent Information

Application Number
JP2023053277
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing epoxy resin compositions face challenges in achieving both curability and storage stability while maintaining sufficient adhesive strength, particularly when phenolic curing agents with allyl groups are used, necessitating high temperature and long curing times.

Method used

A liquid phenolic resin with an aliphatic carbon-carbon double bond, a microcapsule-type curing accelerator, and an imidazole compound with a triazine ring are blended to enhance curability, storage stability, and adhesive strength.

Benefits of technology

The resulting epoxy resin composition exhibits excellent curability, storage stability, and adhesive strength, allowing for efficient curing at high temperatures and in short times, suitable for applications in electrical and electronic equipment parts and power semiconductors.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide an epoxy resin composition which is excellent in curability and storage stability and gives a cured product excellent in adhesive force.SOLUTION: The present invention provides the epoxy resin composition containing: (A) an epoxy resin; (B) a phenolic resin which has one or more functional groups containing an aliphatic carbon-carbon double bond per molecule and is liquid at 25°C; (C) a microcapsule type curing accelerator; (D) an imidazole compound having a triazine ring; and (E) an inorganic filler. The present invention also provides a semiconductor element sealant comprising the epoxy resin composition, an adhesive comprising the epoxy resin composition, and a semiconductor device including a cured product of the epoxy resin composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an epoxy resin composition, and more particularly to an epoxy resin composition containing a liquid phenolic resin. [Background technology]

[0002] Epoxy resin compositions have excellent adhesive strength, heat resistance, and electrical properties, and are therefore used as sealants and adhesives in the fields of electrical and electronic equipment parts, automotive parts, and the like.

[0003] Epoxy resin compositions generally use a curing agent that reacts with epoxy groups, and examples of the curing agent include amine-based curing agents, phenol-based curing agents, acid anhydride-based curing agents, thiol-based curing agents, etc. Among them, phenol-based curing agents are used in the field of power semiconductors and the like because of their excellent heat resistance reliability and moisture resistance reliability (Patent Document 1).

[0004] By introducing an allyl group or an alkyl group into a solid phenolic curing agent, it can be used as a liquid phenolic resin. The cured product of epoxy resin and liquid phenolic resin has excellent moisture resistance and is therefore used in electronic materials such as underfill materials and adhesives (Patent Documents 2 and 3).

[0005] However, the introduction of allyl groups reduces the reactivity of phenolic hydroxyl groups, requiring high temperature and long curing times, and therefore imidazole compounds and phosphorus compounds are used as catalysts to improve reactivity (Patent Document 4). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent Publication No. 2021-063145 [Patent Document 2] JP 2010-241877 A [Patent Document 3] JP 2016-037529 A [Patent Document 4] International Publication No. 2020 / 262061 Summary of the Invention [Problem to be solved by the invention]

[0007] However, it is difficult to achieve both curability and storage stability, and there is also the problem of insufficient adhesive strength, and these problems remain unsolved. Therefore, an object of the present invention is to provide an epoxy resin composition that is excellent in curability and storage stability and that gives a cured product with excellent adhesive strength. [Means for solving the problem]

[0008] As a result of intensive research into solving the above problems, the present inventors have discovered that by combining a liquid phenolic resin having an aliphatic carbon-carbon double bond such as an allyl group with a microcapsule-type curing accelerator and an imidazole compound having a triazine ring, a cured product having excellent curability, storage stability, and adhesive strength can be obtained, and have completed the present invention.

[0009] That is, the present invention provides the following epoxy resin composition. [1] An epoxy resin composition comprising: (A) an epoxy resin; (B) a phenolic resin that is liquid at 25°C and has one or more functional groups containing an aliphatic carbon-carbon double bond in each molecule; (C) a microencapsulated curing accelerator; (D) an imidazole compound having a triazine ring; and (E) an inorganic filler.

[0010] The present invention also provides the above epoxy resin composition, which further has at least one constituent feature selected from the following [2] to

[10] : [2] The above epoxy resin composition, wherein the (A) epoxy resin has one or more aromatic rings in one molecule. [3] The above epoxy resin composition, wherein the (A) epoxy resin comprises one or more selected from the group consisting of bisphenol A type epoxy resins, bisphenol F type epoxy resins, naphthalene type epoxy resins, and aminophenol type epoxy resins. [4] The above epoxy resin composition, wherein in the liquid phenol resin (B), the functional group containing an aliphatic carbon-carbon double bond is an allyl group or a vinyl group. [5] The liquid phenolic resin (B) is represented by the following general formula (1): [ka] (In the formula, R 1 ~R 9 are each independently a hydrogen atom, a monovalent hydrocarbon group having 1 to 25 carbon atoms and no aliphatic carbon-carbon double bond which may have a substituent, an allyl group, a vinyl group, a (meth)acryloxy group, a styryl group, or a hydroxyl group; R 1 ~R 9 At least one of the groups is an allyl group or a vinyl group, n is a number from 0 to 10, and X is represented by the following formula: [ka] In the above formula, R 10 each independently represents a hydrogen atom or a methyl group. The epoxy resin composition represented by the formula: [6] The epoxy resin composition, wherein a molar equivalent ratio of a phenolic hydroxyl group contained in the liquid phenol resin (B) to 1 molar equivalent of an epoxy group contained in the epoxy resin (A) is 0.1 to 2.0. [7] The epoxy resin composition, wherein the amount of the microcapsule-type curing accelerator (C) is 1 to 200 parts by mass per 100 parts by mass of the epoxy resin (A). [8] The above epoxy resin composition, wherein the (C) microcapsule-type curing accelerator contains core particles made of a curing accelerator selected from a phosphorus compound, a tertiary amine compound, an imidazole compound, a urea compound, and an amine adduct compound. [9] The above epoxy resin composition, wherein the amount of the (D) imidazole compound having a triazine ring is 0.1 to 5 parts by mass per 100 parts by mass of the (A) epoxy resin.

[10] The epoxy resin composition, wherein the amount of the (E) inorganic filler is 10 to 20,000 parts by mass per 100 parts by mass of the (A) epoxy resin.

[0011] The present invention further provides a semiconductor element encapsulant comprising the above epoxy resin composition, an adhesive comprising the above epoxy resin composition, and a semiconductor device comprising a cured product of the above epoxy resin composition. Effect of the Invention

[0012] The epoxy resin composition of the present invention is excellent in curability and storage stability, and gives a cured product having excellent adhesive strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below. The epoxy resin composition of the present invention contains (A) an epoxy resin, (B) a liquid phenol resin having one or more functional groups containing an aliphatic carbon-carbon double bond in each molecule, (C) a microcapsule-type curing accelerator, (D) an imidazole compound having a triazine ring, and (E) an inorganic filler.

[0014] (A) Epoxy resin The (A) epoxy resin is the main component of the present invention and may be any generally known epoxy resin. Examples of the epoxy resin include bisphenol type epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, and bisphenol S type epoxy resin; novolac type epoxy resins such as phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, and bisphenol F novolac type epoxy resin; alicyclic epoxy resins such as dicyclopentadiene type epoxy resin and 3,4-epoxycyclohexenylmethyl-3',4'-epoxycyclohexenecarboxylate; polyfunctional phenol type epoxy resins such as resorcinol type epoxy resin and resorcinol novolac type epoxy resin; aminophenol type epoxy resin, stilbene type epoxy resin, triazine skeleton-containing epoxy resin, fluorene skeleton-containing epoxy resin, triphenol alkane type epoxy resin, biphenyl type epoxy resin, xylylene type epoxy resin, biphenyl aralkyl type epoxy resin, naphthalene type epoxy resin, diglycidyl ether compounds of polycyclic aromatics such as anthracene; silicone-modified epoxy resin; and phosphorus-containing epoxy resins obtained by introducing a phosphorus compound into these. These may be used alone or in combination of two or more.

[0015] Among these, epoxy resins that are liquid at room temperature (25° C.) are preferred. The liquid state preferably has a viscosity of 1 mPa·s to 1000 Pa·s, and more preferably 10 mPa·s to 100 Pa·s at 25° C. Here, the viscosity is a value measured by the method described in JIS Z8803:2011.

[0016] Furthermore, from the viewpoint of heat resistance reliability and moisture resistance reliability, the component (A) is preferably an epoxy resin having one or more aromatic rings in one molecule, and examples of such epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, naphthalene type epoxy resins, and aminophenol type epoxy resins.

[0017] (B) Liquid phenolic resin (B) Liquid phenol resin is a curing agent for epoxy resin, and is added for the purpose of reacting with the epoxy group contained in (A) epoxy resin. Liquid phenol resin is liquid at room temperature (25°C). The liquid phenol resin preferably has a viscosity of 100 mPa·s to 500 Pa·s at 25°C, more preferably 1000 mPa·s to 50 Pa·s. If the viscosity is within this range, dispersion in the epoxy resin is easy. Here, the viscosity is a value measured by the method described in JIS Z8803:2011.

[0018] (B) Liquid phenol resin has one or more functional groups containing an aliphatic carbon-carbon double bond in one molecule. It may be a generally known liquid phenol resin as long as it has one or more functional groups containing an aliphatic carbon-carbon double bond in one molecule. The functional group containing an aliphatic carbon-carbon double bond is preferably an alkenyl group having 2 to 10 carbon atoms such as a vinyl group and an allyl group, an alkenylaryl group having 8 to 20 carbon atoms such as a styryl group, an acryloxy group, and a methacryloxy group. Among them, a liquid phenol resin having an allyl group or a vinyl group as a functional group containing an aliphatic carbon-carbon double bond is preferable.

[0019] The liquid phenol resin (B) is preferably represented by the following general formula (1). [ka] In the above formula (1), R 1 ~R 9 are each independently a hydrogen atom, a monovalent hydrocarbon group having 1 to 25 carbon atoms and no aliphatic carbon-carbon double bond which may have a substituent, an allyl group, a vinyl group, a (meth)acryloxy group, a styryl group, or a hydroxyl group; R 1 ~R 9 At least one of them is an allyl group or a vinyl group. More preferably, each aromatic ring has at least one allyl group or vinyl group. n is a number from 0 to 10, preferably 0 or 1 to 5. The liquid phenolic resin may be a mixture of compounds having a plurality of n's. X is a divalent linking group selected from the group consisting of the following formulas: [ka] (In the formula, R 10 are each independently a hydrogen atom or a methyl group.

[0020] In the formula (1), examples of the hydrocarbon group having 1 to 25 carbon atoms and not having a functional group containing an aliphatic carbon-carbon double bond, which may have a substituent, include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, cyclohexyl, octyl, decyl, pentadecane, and eicosane, aryl groups such as phenyl and tolyl, aralkyl groups such as benzyl and phenylethyl, and halogen-substituted monovalent hydrocarbon groups in which some or all of the hydrogen atoms of these hydrocarbon groups are substituted with halogen atoms or the like. Preferred are methyl, ethyl, isopropyl, and tert-butyl groups.

[0021] Among the liquid phenol resins represented by formula (1), allyl group-containing phenol resins such as bisphenol A type allylphenol resin, bisphenol F type allylphenol resin, novolac type allylphenol resin, aralkyl type allylphenol resin, and resorcinol type allylphenol resin are preferred from the viewpoint of viscosity and adhesive strength. These may be used alone or in combination of two or more.

[0022] The amount of the liquid phenolic resin (B) is such that the molar equivalent ratio of the phenolic hydroxyl group contained in the liquid phenolic resin (B) to 1 molar equivalent of the epoxy group contained in the epoxy resin (A) is preferably 0.1 to 2.0, more preferably 0.2 to 1.8, and even more preferably 0.4 to 1.5. If the ratio is less than 0.1, unreacted epoxy groups may remain, which may cause a decrease in adhesion. If the ratio exceeds 2.0, unreacted phenolic hydroxyl groups may remain, which may cause a decrease in strength during high-temperature storage.

[0023] (C) Microcapsule type hardening accelerator (C) Microcapsule type curing accelerator is blended for the purpose of promoting the curing of (A) epoxy resin and (B) liquid phenolic resin. The microcapsule type curing accelerator contains a shell material and a core made of a curing accelerator component covered with the shell material. In the microcapsule type curing accelerator, the curing accelerator component is isolated from the other components described above by being covered with the shell material, and the storage stability of the epoxy resin composition is improved. The curing accelerator (catalyst), which is an effective component for the core material (core particle) of the microcapsule, preferably has a reaction temperature (i.e., a temperature at which catalytic action is expressed) of 50°C or higher so as to exhibit storage stability and fast curing at a low temperature of a certain temperature or higher. Examples of such curing accelerators include phosphorus compounds, tertiary amine compounds, imidazole compounds, urea compounds, and amine adduct compounds such as alicyclic polyamines. It is also preferable to prepare a masterbatch type microcapsule type hardening accelerator by premixing the microcapsule type hardening accelerator with an epoxy resin, a hardening agent, etc. By preparing the masterbatch type, dispersibility is improved.

[0024] Examples of the phosphorus compound include triorganophosphine compounds such as tributylphosphine, triphenylphosphine, tri(methylphenyl)phosphine, tri(nonylphenyl)phosphine, tri(methoxyphenyl)phosphine, diphenyltolylphosphine, triphenylphosphine·triphenylborane, etc.; quaternary phosphonium salts such as tetraphenylphosphonium·tetraphenylborate, etc. Among these, triphenylphosphine and tri(methylphenyl)phosphine are preferred.

[0025] Examples of the tertiary amine compound include amine compounds having an alkyl group or an aralkyl group as a substituent bonded to a nitrogen atom, such as triethylamine, benzyldimethylamine, benzyltrimethylamine, and α-methylbenzyldimethylamine; cycloamidine compounds such as 1,8-diazabicyclo[5.4.0]undecene-7 and 1,4-diazabicyclo[2.2.2]octane, and their phenol salts, octylate salts, and oleate salts, and their salts with organic acids and salts or complex salts of quaternary boron compounds. Among these, 1,8-diazabicyclo[5.4.0]undecene-7 and 1,4-diazabicyclo[2.2.2]octane are preferred.

[0026] Examples of the imidazole compound include 2-methylimidazole, 2-ethylimidazole, 2-undecylimidazole, 2,4-dimethylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 1,2-diethylimidazole, 2-phenyl-4-methylimidazole, 2,4,5-triphenylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-benzyl-2-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-allyl-4,5-diphenylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. Among these, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-ethylimidazole, 1,2-dimethylimidazole, 1,2-diethylimidazole, 2,4-dimethylimidazole and 2-phenyl-4-methylimidazole are preferred.

[0027] Examples of the urea compound include N,N-dimethyl-N'-phenylurea, N,N-dimethyl-N'-(3,4-dichlorophenyl)urea, 4,4'-methylenebis(phenyldimethylurea), aromatic dimethylurea compounds, aliphatic dimethylurea compounds, toluenebisdimethylurea, N'-[3-[[[(dimethylamino)carbonyl]amino]methyl]-3,5,5-trimethylcyclohexyl]-N,N-dimethylurea, etc. Among these, aromatic dimethylurea compounds and aliphatic dimethylurea compounds are preferred.

[0028] Examples of the amine adduct compound include compounds having an amino group obtained by reacting at least one compound selected from the group consisting of carboxylic acid compounds, phenol compounds, isocyanate compounds, and epoxy resins with an amine compound. Of these, the core of the microcapsule is preferably mainly composed of an amine adduct compound obtained by reacting an isocyanate resin or an epoxy resin with an amine compound.

[0029] Examples of the carboxylic acid compound include succinic acid, adipic acid, sebacic acid, phthalic acid, and dimer acid.

[0030] Examples of the phenol compound include monophenols such as phenol, cresol, xylenol, carvacrol, motil, and naphthol, and polyphenols such as catechol, resorcin, hydroquinone, bisphenol A, bisphenol F, pyrogallol, and phloroglucin.

[0031] Examples of the isocyanate compound include ethylene diisocyanate, propylene diisocyanate, butylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, isophorone diisocyanate, 4-4'-dicyclohexylmethane diisocyanate, norbornane diisocyanate, 1,4-isocyanatocyclohexane, 1,3-bis(isocyanatomethyl)-cyclohexane, 1,3-bis(2-isocyanatopropyl-2-yl)-cyclohexane, tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylene diisocyanate, and 1,5-naphthalene diisocyanate.

[0032] Examples of the epoxy compound include butyl glycidyl ether, hexyl glycidyl ether, phenyl glycidyl ether, allyl glycidyl ether, para-tert-butylphenyl glycidyl ether, paraxylyl glycidyl ether, bisphenol type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, and bisphenol S type epoxy resins, novolac type epoxy resins such as phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, and bisphenol F novolac type epoxy resins, dicyclopentadiene type epoxy resins, 3,4-ethylene glycol glycidyl ethers, and the like. Examples of epoxy resins include alicyclic epoxy resins such as epoxycyclohexenylmethyl-3',4'-epoxycyclohexenecarboxylate, polyfunctional phenol-type epoxy resins such as resorcinol-type epoxy resins and resorcinol novolac-type epoxy resins, stilbene-type epoxy resins, triazine skeleton-containing epoxy resins, fluorene skeleton-containing epoxy resins, triphenol alkane-type epoxy resins, biphenyl-type epoxy resins, xylylene-type epoxy resins, biphenyl aralkyl-type epoxy resins, naphthalene-type epoxy resins, and diglycidyl ether compounds of polycyclic aromatics such as anthracene, and phosphorus-containing epoxy resins obtained by introducing a phosphorus compound into these.

[0033] Examples of the amine compound include methylamine, ethylamine, propylamine, butylamine, ethylenediamine, 1,2-propanediamine, tetramethyleneamine, 1,5-diaminopentane, hexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 2,2,4-triethylhexamethyldiamine, 1,2-diaminopropane, diethylenetriamine, triethylenetetramine, tetraethylenepent, cyclohexylamine, isophoronediamine, 1,3-bisaminomethylcyclohexane, aminoethylpiperazine, diethylaminopropylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, dipentylamine, dihexylamine, dimethanolamine, diethanolamine, dipropanolamine, dicyclohexylamine, and piperazine.

[0034] The hardening accelerators contained in the microcapsules may be used either individually or in combination of two or more.

[0035] The shell material for microencapsulating the curing accelerator must have a melting point of 50 to 90° C. from the viewpoint of maintaining storage stability and ensuring fast curing. The material of the shell material is not particularly limited as long as it has such a melting point, and all known materials can be used, such as (meth)acrylic monomers, such as alkyl esters having 1 to 8 carbon atoms, such as acrylic acid esters, itaconic acid esters, and crotonic acid esters; alkyl esters in which the alkyl group has a substituent such as an allyl group; monofunctional monomers such as styrene, α-methylstyrene, acrylonitrile, methacrylonitrile, and vinyl acetate; and polymers obtained by (co)polymerizing one or more monomers selected from polyfunctional monomers such as ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, divinylbenzene, bisphenol A di(meth)acrylate, and methylene bis(meth)acrylamide. Among these, polymers of (meth)acrylate monomers are preferred.

[0036] The microcapsule type hardening accelerator contains the above-mentioned shell material and a core component covered with the shell material and made of the above-mentioned hardening accelerator such as the imidazole compound, the tertiary amine compound, etc. The method for producing the microcapsule type hardening accelerator is not particularly limited, but examples thereof include the following methods (a) to (c).

[0037] (a) A method in which a shell material and core particles of a microcapsule-type hardening accelerator are dissolved or dispersed in a solvent that is a dispersion medium, and then the solubility of the shell material in the dispersion medium is reduced to precipitate the shell on the surface of the core particles of the microcapsule-type hardening accelerator. (b) A method in which core particles of a microcapsule-type hardening accelerator are dispersed in a dispersion medium, and the above-mentioned shell material is added to the dispersion medium to precipitate on the core particles of the microcapsule-type hardening accelerator. (c) A method in which the above shell material is added to a dispersion medium, and the surface of the core particle of the microcapsule-type hardening accelerator is used as a reaction site to form a shell there.

[0038] Examples of the dispersion medium used in the above-mentioned (a) to (c) manufacturing methods include solvents and resins. Examples of the solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, n-butyl acetate, propylene glycol monomethyl ethyl ether acetate, benzene, toluene, xylene, cyclohexane, methanol, ethanol, isopropanol, n-butanol, butyl carbitol, and water. Examples of the resin include epoxy resin, phenol resin, maleimide resin, cyanate ester resin, and silicone resin. Among these, aromatic hydrocarbons such as toluene and alcohols such as n-butanol are preferred as dispersion media with good dispersibility.

[0039] The microcapsule type curing accelerator used in the composition of the present invention preferably has an average particle size of 0.1 to 10 μm, and particularly preferably has an average particle size of 1 to 5 μm. If the average particle size is too small, the specific surface area becomes large, and there is a risk that the viscosity of the epoxy resin composition becomes high when mixed. If the average particle size exceeds 10 μm, the dispersion in the epoxy resin composition becomes non-uniform, which may cause a decrease in reliability. The average particle size is a volume average particle size measured by a laser diffraction method.

[0040] The blending amount of the (C) component is preferably 1 to 200 parts by mass, more preferably 2.5 to 150 parts by mass, and even more preferably 3 to 100 parts by mass, relative to 100 parts by mass of the above-mentioned (A) epoxy resin. When the blending amount of the (C) component is within the above range, there is no risk of the balance between the storage stability and moisture resistance of the composition becoming poor, or the curing speed during molding becoming very slow or fast.

[0041] (D) Imidazole compound having a triazine ring The imidazole compound having a triazine ring is added for the purpose of promoting the reaction between the epoxy resin and the liquid phenolic resin and for the purpose of improving the adhesive strength with various substrates. The type of the imidazole compound having a triazine ring is not particularly limited. Any known imidazole compound having a triazine ring may be used, and examples thereof include 2,4-diamino-6-[2'-methylimidazolyl(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4-methylimidazolyl(1')]-ethyl-s-triazine, an isocyanuric acid adduct of 2,4-diamino-6-[2'-methylimidazolyl(1')]-ethyl-s-triazine, an isocyanuric acid adduct of 2-phenylimidazole, and an isocyanuric acid adduct of 2-methylimidazole.

[0042] The blending amount of the (D) component is preferably 0.1 to 10 parts by mass, and more preferably 0.2 to 5 parts by mass, based on 100 parts by mass of the above-mentioned (A) epoxy resin. When the blending amount of the (D) component is within the above range, there is no risk of the balance between the storage stability and moisture resistance of the composition being impaired.

[0043] (E) Inorganic filler is blended for the purpose of improving the resin strength and reducing thermal expansion of the epoxy resin composition. The type of the inorganic filler is not particularly limited, and any known inorganic filler may be used. Examples of the inorganic filler include silicas (e.g., fused silica, crystalline silica, cristobalite, etc.), alumina, silicon nitride, aluminum nitride, boron nitride, titanium oxide, glass fiber, and magnesium oxide. The average particle size and shape of the inorganic filler can be selected according to the application.

[0044] (E) Inorganic filler is preferably surface-treated in advance with a coupling agent such as a silane coupling agent or a titanate coupling agent in order to strengthen the bond strength between the epoxy resin and the inorganic filler. Examples of the coupling agent include epoxy silanes such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, N-β(aminoethyl)-γ-aminopropyltrimethoxysilane, reaction product of imidazole and γ-glycidoxypropyltrimethoxysilane, amino silanes such as γ-aminopropyltriethoxysilane and N-phenyl-γ-aminopropyltrimethoxysilane, and mercaptosilanes such as γ-mercaptosilane and γ-episulfidoxypropyltrimethoxysilane. The amount of the coupling agent used for surface treatment and the surface treatment method may be according to a conventionally known method, and are not particularly limited in the present invention.

[0045] The blending amount of the (E) inorganic filler is preferably 10 to 20,000 parts by mass, more preferably 15 to 10,000 parts by mass, and further preferably 20 to 3,000 parts by mass, based on 100 parts by mass of the (A) epoxy resin.

[0046] (F) Other Additives In addition to the components (A) to (E), the epoxy resin composition of the present invention may contain other additives (F) as needed within the range that does not impair the objects and effects of the present invention. Examples of such additives (F) include antioxidants, flame retardants, ion trapping agents, adhesion promoters, stress reducing agents, colorants, etc.

[0047] The antioxidant is blended for the purpose of preventing oxidation degradation when the cured product of the epoxy resin composition is stored at high temperatures. The antioxidant may be any generally known antioxidant and is not particularly limited, but among them, phenol-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants are preferred, and phenol-based antioxidants are particularly preferred. The melting point of the phenol-based antioxidant is preferably 80 to 250°C, more preferably 90 to 240°C, and particularly preferably 100 to 220°C.

[0048] Examples of phenol-based antioxidants include n-octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, n-octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)acetate, neododecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, dodecyl-2-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, ethyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)isobutyrate, octadecyl-3-( 3,5-di-t-butyl-4-hydroxyphenyl)isobutyrate, 2-(n-octylthio)ethyl-3,5-di-t-butyl-4-hydroxyphenylacetate, 2-(n-octadecylthio)ethyl-3,5-di-t-butyl-4-hydroxyphenylacetate, 2-(n-octadecylthio)ethyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2-(2-stearoyloxyethylthio)ethyl-7-(3-methyl-5-t-butyl-4-hydroxyphenyl)heptanoate , 2-hydroxyethyl-3-(3-methyl-5-t-butyl-4-hydroxyphenyl)propionate, pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 3-(3,5-di-tert-butyl-4-hydroxyphenyl)stearyl propionate, 1,3,5-tris[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1,1,3-tris(2-methyl 4,4'-butylidenebis(6-tert-butyl-m-cresol), pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2,2'-dimethyl-2,2'-(2,4,8,10-tetraoxaspiro[5.5]undecane-3,9-diyl)dipropane-1,1'-diyl bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propanoate], and the like.

[0049] Examples of sulfur-based antioxidants include dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, ditridecyl-3,3'-thiodipropionate, pentaerythrityl tetrakis(3-laurylthiopropionate), and 2,2-bis[[3-(dodecylthio)-1-oxopropyloxy]methyl]-1,3-propanediyl bis[3-(dodecylthio)propionic acid].

[0050] Examples of phosphorus-based antioxidants include tridecyl phosphite, triphenyl phosphite, tris(2,4-di-t-butylphenyl)phosphite, 2-ethylhexyldiphenyl phosphite, diphenyltridecyl phosphite, 2,2-methylenebis(4,6-di-t-butylphenyl)octyl phosphite, distearyl pentaerythritol diphosphite, bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite, 2- [[2,4,8,10-tetrakis(1,1-dimethylethyl)dibenzo[d,f][1,3,2]dioxaphosphepin-6-yl]oxy]-N,N-bis[2-[[2,4,8,10-tetrakis(1,1-dimethylethyl)dibenzo[d,f][1,3,2]dioxaphosphepin-6-yl]oxy]-ethyl]ethanamine, 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, and the like. These may be used alone or in combination of two or more.

[0051] The flame retardant is added for the purpose of imparting flame retardancy. The flame retardant is not particularly limited, and may be any known one. For example, phosphazene compounds, silicone compounds, zinc molybdate-supported talc, zinc molybdate-supported zinc oxide, aluminum hydroxide, magnesium hydroxide, molybdenum oxide, etc. may be mentioned.

[0052] The ion trapping agent is added for the purpose of trapping ion impurities contained in the epoxy resin composition and preventing thermal deterioration and moisture absorption deterioration. The type of the ion trapping agent is not particularly limited, and may be any known one. For example, hydrotalcites, bismuth hydroxide compounds, rare earth oxides, etc. may be mentioned.

[0053] The adhesion promoter is added for the purpose of imparting adhesiveness or tackiness (pressure-sensitive adhesiveness). The adhesion promoter is not particularly limited and includes known agents such as urethane resins, phenolic resins, terpene resins, and silane coupling agents. Among these, silane coupling agents are preferred. Examples of the silane coupling agent include n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, β-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxytri(ethyleneoxy)propyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane, γ-isocyanatopropyltriethoxysilane, and the like.

[0054] The stress reducing agent is added for the purpose of reducing the elastic modulus and thermal expansion coefficient of the epoxy resin composition. The stress reducing agent is not particularly limited and includes known agents such as thermoplastic resins, thermoplastic elastomers, organic synthetic rubbers, silicones, etc.

[0055] Examples of the colorant include carbon black, titanium black, titanium oxide, etc., and these may be used alone or in combination of two or more kinds.

[0056] The amount of the other additives to be added varies depending on the purpose of the composition, but is usually 5% by mass or less of the entire epoxy resin composition excluding inorganic fillers.

[0057] The epoxy resin composition of the present invention is preferably liquid at room temperature (25° C.) and preferably has a viscosity of 0.1 to 850 Pa·s at 25° C. Here, the viscosity is a value measured by the method described in JIS Z8803:2011.

[0058] The epoxy resin composition of the present invention can be produced by the following method. For example, the components (A) to (E) are mixed, stirred, dissolved and / or dispersed, either simultaneously or separately, while being heated as necessary, to obtain a mixture of the components (A) to (E). Preferably, the mixture of the components (A) to (E) is obtained by adding the liquid phenolic resin (B) to the mixture of the components (A), (C), (D) and (E), and stirring, dissolving and / or dispersing the mixture. Depending on the purpose of use, at least one of other additives such as antioxidants, flame retardants, ion trapping agents, adhesion promoters, stress reducing agents and colorants may be added to the mixture of the components (A) to (E) and mixed. The device for mixing, stirring and dispersing is not particularly limited. For example, a mortar and pestle machine, a two-roll mill, a three-roll mill, a ball mill, a planetary mixer or a mass colloider equipped with a stirring and heating device may be used, and these devices may be used in appropriate combination.

[0059] The epoxy resin composition of the present invention can be used as a cured product by curing. The curing conditions of the epoxy resin composition of the present invention are not particularly limited, but for example, it may be heated at a temperature in the range of 60 to 250°C, preferably 80 to 230°C, for 30 seconds to 10 hours, preferably 1 minute to 5 hours. The epoxy resin composition of the present invention can be cured at a high temperature in a short time. Therefore, it can be cured well even at a temperature in the range of 180 to 230°C for about 30 seconds to 5 minutes.

[0060] The epoxy resin composition of the present invention has excellent adhesive strength, heat resistance, and electrical properties, and can therefore be used as a sealant or adhesive in the fields of electrical and electronic equipment parts, automobile parts, and the like. The epoxy resin composition of the present invention has excellent heat resistance reliability and moisture resistance reliability, and can therefore be suitably used in the field of power semiconductors, and the like. In particular, the epoxy resin composition is suitably used in a semiconductor device having a support, a semiconductor element disposed on the support, and a cured product of the epoxy resin composition that seals the semiconductor element, and in particular, in a semiconductor device in which the gap between the semiconductor element and the support is filled with the epoxy resin composition. EXAMPLES

[0061] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In Table 1, the blend amounts are shown in parts by mass. The "molar equivalent ratio" shown in Table 1 refers to the ratio of the phenolic hydroxyl group equivalent (active hydrogen equivalent) in component (B) to the epoxy equivalent in component (A), and means molar equivalent.

[0062] The components used in the examples and comparative examples are as follows. (A) Epoxy resin (A1) Bisphenol A type epoxy resin (jER828, viscosity at 25°C 5-15 Pa·s, epoxy equivalent 189 g / eq, manufactured by Mitsubishi Chemical Corporation) (A2) Aminophenol-type trifunctional epoxy resin (jER630, viscosity at 25°C 500-1500 mPa·s, epoxy equivalent 100 g / eq, manufactured by Mitsubishi Chemical Corporation) (A3) Naphthalene-type epoxy resin (HP4032D, viscosity at 25°C 20-30 Pa·s, epoxy equivalent 150 g / eq, manufactured by DIC Corporation)

[0063] (B) Liquid phenolic resin (B1) Novolac-type allylphenol resin represented by the following formula (MEH-8000H, viscosity at 25°C 1600 mPa s, hydroxyl equivalent 141 g / eq, manufactured by UBE) [ka] (n = an integer between 0 and 4) (B2) Resorcinol-type allylphenol resin represented by the following formula (MEH-8400, viscosity at 25°C 8000 mPa s, hydroxyl equivalent 107 g / eq, manufactured by UBE) [ka] (n = an integer between 0 and 4) (B3) 2,2'-diallyl bisphenol A (DABPA, viscosity at 25°C 20,000 mPa s, hydroxyl equivalent 154 g / eq, manufactured by Daiwa Chemical Industry Co., Ltd.) represented by the following formula: [ka] (B') Comparative epoxy resin curing agent (B'1) Solid epoxy resin curing agent represented by the following formula: Bisphenol A (solid at 25°C, melting point 158°C, hydroxyl equivalent 114g / eq, manufactured by Tokyo Chemical Industry Co., Ltd.) [ka]

[0064] (C) Microcapsule type hardening accelerator (C1) Masterbatch type curing accelerator containing imidazole-based microcapsules (Novacure HX-3722, average particle size 2 μm, manufactured by Asahi Kasei Corporation) (C2) Masterbatch type curing accelerator containing imidazole-based microcapsules (Novacure HX-3088, average particle size 2 μm, manufactured by Asahi Kasei Corporation) (C3) Masterbatch type curing accelerator containing imidazole microcapsules (Novacure HX-3741, average particle size 2 μm, manufactured by Asahi Kasei Corporation) (C4) Masterbatch type curing accelerator containing alicyclic polyamine microcapsules (Novacure HXA-5945HP, average particle size 2 μm, manufactured by Asahi Kasei Corporation)

[0065] (D) Imidazole compound having a triazine ring (D1) 2,4-diamino-6-[2'-methylimidazolyl(1')]-ethyl-s-triazine (2MZA-PW, manufactured by Shikoku Chemical Industry Co., Ltd.) (D2) 2,4-diamino-6-[2'-undecylimidazolyl(1')]-ethyl-s-triazine (C11Z-A, manufactured by Shikoku Chemical Industry Co., Ltd.) (D3) Isocyanuric acid adduct of 2,4-diamino-6-[2'-methylimidazolyl(1')]-ethyl-s-triazine (2MA-OK, manufactured by Shikoku Chemical Industry Co., Ltd.)

[0066] (E) Inorganic filler (E1) Fused spherical silica with an average particle size of 10 μm (manufactured by Tatsumori Co., Ltd.)

[0067] Ingredients for comparison (F1) Imidazole compound: 2-ethyl-4-methylimidazole (2E4MZ, manufactured by Shikoku Chemical Industry Co., Ltd.) (F2) Triazine compound: 2-vinyl-4,6-diamino-1,3,5-triazine (VT, manufactured by Shikoku Chemical Industry Co., Ltd.)

[0068] In the formulations of Examples 1 to 26 and Comparative Examples 1 to 6, the components were mixed in a conventional manner to prepare epoxy resin compositions. This epoxy resin composition was used for the following evaluations, the results of which are shown in Table 1.

[0069] [viscosity] The viscosity of the epoxy resin composition at 25° C. was measured in accordance with JIS Z8803:2011. That is, the viscosity was measured 2 minutes after the sample was set at a measurement temperature of 25° C. using an E-type viscometer.

[0070] [Viscosity after storage at 25℃] The viscosity of each epoxy resin composition after 8 hours at 25° C. was measured in the same manner as above. The ratio (%) of the viscosity after 8 hours to the initial viscosity was calculated to evaluate the storage stability.

[0071] [Initial adhesive strength] The deposition area is 4 mm on a copper frame with dimensions of 10 mm x 10 mm.2 A silicon chip was placed on the epoxy resin composition, and then heated at 200° C. for 1 minute to prepare a test piece. Using this test piece, the shear adhesive strength was measured at room temperature (25° C.) using a bond tester DAGE-SERIES-4000PXY (manufactured by DAGE Corporation) to evaluate the adhesive strength.

[0072] [Adhesive strength retention after storage at high temperature and humidity] The deposition area is 4 mm on a copper frame with dimensions of 10 mm x 10 mm. 2 The epoxy resin composition was applied so that the thickness of the resin layer was 100 mm, a silicon chip was placed on the composition, and the composition was heated at 200°C for 1 minute to prepare a test piece. Using this test piece, the shear adhesive strength at room temperature (25°C) was measured using a bond tester DAGE-SERIES-4000PXY (manufactured by DAGE Co., Ltd.) as an evaluation of adhesive strength. The test piece was also stored at PCT (121°C / humidity 100% / 2atm) for 48 hours, and then cooled to room temperature to measure the shear adhesive strength. More specifically, the adhesive strength retention rate after storage at high temperature and high humidity was calculated using the following formula. Adhesive strength retention rate after high temperature and high humidity storage = Shear adhesive strength after 48 hours storage at PCT / initial value x 100 (%)

[0073] [Table 1]

[0074] [Table 2]

[0075] [Table 3]

[0076] As shown in Table 3, the epoxy resin compositions (Comparative Examples 2, 3, and 4) that do not contain either the microcapsule-type curing accelerator or the imidazole compound having a triazine ring are inferior in curability of the epoxy resin composition, initial adhesive strength and adhesive retention strength of the cured product, as can be seen from the comparison with the Examples. In particular, the composition of Comparative Example 3 that does not contain the microcapsule-type curing accelerator did not cure when heated at 200°C for 1 minute, and was inferior in curability. The epoxy resin composition of Comparative Example 4, which does not contain the microcapsule-type curing accelerator and has an increased amount of the imidazole compound having a triazine ring, had good curability, but increased in viscosity over time at room temperature and was inferior in storage stability. In addition, the epoxy resin compositions of Comparative Examples 5 and 6, which contain an imidazole compound or a triazine compound instead of the imidazole compound having a triazine ring, were inferior in storage stability at room temperature compared to the compositions of the Examples, and were also inferior in initial adhesive strength and adhesive retention strength. In Comparative Example 7, in which a solid epoxy resin curing agent having no aliphatic carbon-carbon double bond was used, a composition that was liquid at 25°C was not obtained. In contrast, as shown in Tables 1 and 2, the epoxy resin composition of the present invention is formulated by combining a liquid phenolic resin having an aliphatic carbon-carbon double bond, a microcapsule-type curing accelerator, and an imidazole compound having a triazine ring, so that the composition has excellent curability and storage stability and can give a cured product with excellent adhesive strength. [Industrial Applicability]

[0077] The epoxy resin composition of the present invention has excellent curability and storage stability, and can give a cured product having excellent adhesive strength. The epoxy resin composition of the present invention can be suitably used as a sealant or adhesive in the fields of electric / electronic device parts, automobile parts, etc.

Claims

1. An epoxy resin composition comprising (A) an epoxy resin, (B) a phenolic resin that is liquid at 25°C and has one or more functional groups containing an aliphatic carbon-carbon double bond in each molecule, (C) a microcapsule-type curing accelerator, (D) an imidazole compound having a triazine ring, and (E) an inorganic filler.

2. 2. The epoxy resin composition according to claim 1, wherein the epoxy resin (A) has one or more aromatic rings in one molecule.

3. 3. The epoxy resin composition according to claim 2, wherein the epoxy resin (A) comprises one or more selected from the group consisting of bisphenol A type epoxy resins, bisphenol F type epoxy resins, naphthalene type epoxy resins, and aminophenol type epoxy resins.

4. 2. The epoxy resin composition according to claim 1, wherein the functional group containing an aliphatic carbon-carbon double bond in the liquid phenol resin (B) is an allyl group or a vinyl group.

5. The liquid phenolic resin (B) is represented by the following general formula (1): [Formula 1] (In the formula, R 1 ~R 9 are each independently a hydrogen atom, a monovalent hydrocarbon group having 1 to 25 carbon atoms and no aliphatic carbon-carbon double bond which may have a substituent, an allyl group, a vinyl group, a (meth)acryloxy group, a styryl group, or a hydroxyl group; R 1 ~R 9 At least one of the groups is an allyl group or a vinyl group, n is a number from 0 to 10, and X is a group of the following formula: [Case 2] In the above formula, R 10 each independently represents a hydrogen atom or a methyl group. The epoxy resin composition according to claim 1,

6. 2. The epoxy resin composition according to claim 1, wherein a molar equivalent ratio of a phenolic hydroxyl group contained in said liquid phenolic resin (B) to 1 molar equivalent of an epoxy group contained in said epoxy resin (A) is 0.1 to 2.

0.

7. 2. The epoxy resin composition according to claim 1, wherein the amount of the microcapsule type curing accelerator (C) is 1 to 200 parts by mass per 100 parts by mass of the epoxy resin (A).

8. 2. The epoxy resin composition according to claim 1, wherein the microcapsule type curing accelerator (C) has a core containing a curing accelerator selected from a phosphorus compound, a tertiary amine compound, an imidazole compound, a urea compound, and an amine adduct compound.

9. 2. The epoxy resin composition according to claim 1, wherein the amount of the imidazole compound having a triazine ring (D) is 0.1 to 5 parts by mass per 100 parts by mass of the epoxy resin (A).

10. 2. The epoxy resin composition according to claim 1, wherein the amount of the inorganic filler (E) is 10 to 20,000 parts by mass per 100 parts by mass of the epoxy resin (A).

11. A semiconductor element encapsulant comprising the epoxy resin composition according to any one of claims 1 to 10.

12. An adhesive comprising the epoxy resin composition according to any one of claims 1 to 10.

13. A semiconductor device comprising a cured product of the epoxy resin composition according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Epoxy-based curable composition and electronic part

    JP2006160953A

  • Underfill agent, semiconductor device obtained by using the same and method for producing the semiconductor device

    JP2008189760A

  • Epoxy resin composition

    JP2010100730A

  • Resin composition and sealing material using the same

    JP2012077129A

  • Liquid epoxy resin composition for semiconductor encapsulation, and semiconductor device using the same

    JP2013032522A

Cited By

  • Adhesive film, adhesive film with metal layer, member for forming wiring, method for forming wiring layer, and wiring formation member

    WO2026121160A1