Alkaline metal removal method
By mixing sulfur, calcium, and chlorine sources with alkali metal-containing materials and heating them, the method enhances alkali metal removal efficiency, allowing waste materials to be used as effective cement substitutes.
Patent Information
- Application Number
- JP2023053428
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing methods for removing alkali metals from clay substitute raw materials for cement are inefficient, particularly when the alkali metals are in a poorly soluble state, leading to a need for improved methods to utilize these materials effectively as cement substitutes for coal ash.
A method involving the mixing of a sulfur source, a calcium source, and a chlorine source with the alkali metal-containing material, followed by heating to convert alkali metals into volatile compounds, which can then be removed through volatilization or washing, allowing for the use of these materials as cement raw materials.
The method significantly increases the removal rate of alkali metals, enabling the effective use of waste materials like fly ash and construction soil as cement substitutes by reducing their alkali metal content to acceptable levels.
Smart Images

Figure 2024141654000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for removing alkali metals, and more particularly to a method for removing alkali metals in order to effectively utilize waste containing alkali metals as a raw material for cement or the like. [Background technology]
[0002] Following the Minister of Economy, Trade and Industry's phase-out of inefficient coal-fired power plants, the amount of coal ash generated is expected to decrease. Coal ash is used as a substitute for clay in cement production, but due to the above-mentioned circumstances, there is a possibility that coal ash will be in short supply in the future, so there is a demand to secure substitute clay for coal ash.
[0003] However, many of the other clay substitutes contain high concentrations of alkali metals, which are repelling cement, so in order to use the substitutes for coal ash as a cement raw material, it is necessary to remove the alkali metals.
[0004] Many of the alkali metals (especially potassium) contained in the clay substitute raw materials are in a water-insoluble (slightly soluble) state. For this reason, the applicant has previously proposed a method in which a chlorine source is added to the target material and heated (so-called chlorination roasting), the potassium contained in the target material is converted to KCl, and then removed by volatilization or washing with water (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2004-59754 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, even when the method proposed in Patent Document 1 was used, the amount (removal rate) of alkali metal removed from an object containing poorly soluble alkali metal was limited to a certain level, and therefore, additional measures were required to achieve further improvement.
[0007] In view of the above, an object of the present invention is to provide a method for removing alkali metals from an object more efficiently than ever before, thereby enabling the object to be effectively utilized as a cement raw material, etc. [Means for solving the problem]
[0008] As a result of extensive research, the present inventors have found that, when an alkali metal-containing material is subjected to chlorination roasting, the removal rate of the alkali metal can be further increased by heating the material together with the chlorine source in a state where a calcium source is mixed therein, rather than simply heating the material together with a chlorine source.
[0009] Furthermore, as a result of intensive research by the present inventors, it has been found that by mixing a sulfur source in addition to a calcium source with an alkali metal-containing material and heating the resulting mixture together with a chlorine source, the removal rate of alkali metals can be further increased, and that alkali metals can be removed by firing at a lower temperature than in conventional chlorination roasting.
[0010] That is, the present invention provides a method for removing an alkali metal from an alkali metal-containing material, comprising the steps of: (a) mixing a sulfur source, a calcium source, and a chlorine source with the alkali metal-containing material, either simultaneously or sequentially; and a step (b) of heating the mixture of the alkali metal-containing material in a state in which the hydraulic ratio has been adjusted by the step (a) to obtain a heat-treated product, The calcium source is characterized in that it is the same material as the sulfur source or is a material different from the sulfur source.
[0011] The alkali metal-containing material to be treated by the present invention is not particularly limited as long as it is a non-flammable alkali metal-containing material containing a high concentration of alkali metal components. However, the method of the present invention is particularly effective when the alkali metal-containing material has a raw material composition containing the alkali metal in a sparingly soluble state.
[0012] When the alkali metal-containing material is waste, the waste can be effectively used as a cement raw material by treating it with the method of the present invention, which is preferable from the viewpoint of the global environment. Examples of such materials include fly ash and bottom ash of wood biomass ash, construction waste soil, and recycled fine powder of waste concrete. These materials contain alkali metals in a sparingly soluble state.
[0013] The inventors consider the reason why the removal rate of alkali metals is further increased by mixing a calcium source with the alkali metal-containing material to be treated (hereinafter appropriately abbreviated as "target material") as follows.
[0014] In the process of heating a mixture of a chlorine source and an object, the object may melt or sinter depending on the heating temperature. In addition, the water-soluble alkali metal chloride (e.g., KCl) produced in this process may also melt.
[0015] After the heating process is completed, the molten object solidifies into a solid as the temperature decreases. At this time, the molten alkali metal chloride aggregates and crystallizes inside the molten object due to differences in surface tension, etc. As a result, the object after cooling contains some water-soluble alkali metal chloride. It is difficult to effectively remove the alkali metal chloride contained in the object even if it is subsequently washed with water.
[0016] In contrast, according to the above method, a chlorine source and a calcium source are mixed with the target material prior to the heating step (b). As a result, the Ca contained in the calcium source reacts with the constituent atoms of the target material in the heating step (b) to form a Ca-containing mineral. For example, when the target material is the waste material listed above, examples of the Ca-containing mineral formed include CaSiO3 (wollastonite), Ca2SiO4 (belite), CaAl2Si2O8 (anorthite), and Ca2Al2SiO7 (gehlenite). These Ca-containing minerals have a higher melting point than the waste material itself.
[0017] Therefore, by converting at least a part of the target into a Ca-containing mineral by the heating step (b), the amount of the target to be melted and sintered is reduced. As a result, the amount of molten alkali metal salt taken into the inside of the target can be reduced. For this reason, for example, by performing a water washing process to dissolve the target in water, a residue with a reduced alkali metal content can be obtained. In other words, the alkali metal removal method may include a step (c) of washing the heat-treated product obtained after the heating step (b).
[0018] Moreover, the alkali metal salt may be removed (separated) from the heat-treated product by a method other than washing with water.
[0019] However, depending on the conditions of the heating step (b), etc., it may happen that the amount of alkali metal contained in the target object that changes to a volatile substance by carrying out the heating step (b) increases. In this case, the alkali metal may be sufficiently removed from the heat-treated object obtained after heating without washing with water, etc. From this viewpoint, the water washing step (c) is not necessarily required in the present invention.
[0020] In particular, in the heating step (b) according to the present invention, the target material is heated in a state where a sulfur source is mixed with the calcium source. As a result, part of the alkali metals contained in the target material can be converted into sulfur compounds such as Na2SO4 and K2SO4, which are highly volatile. The generated sulfur compounds are desorbed from the target material as exhaust gas generated in the heating step (b). In other words, the addition of the sulfur source increases the amount of alkali metals contained in the target material that are converted into volatile compounds, so that the heat-treated material obtained after heating already has a high proportion of alkali metals removed, even before the water-washing treatment. Preferably, the heat-treated material is then subjected to a water-washing treatment or the like to remove (separate) alkali metal salts from the heat-treated material, thereby further improving the removal rate of alkali metals.
[0021] In this way, the heat-treated product obtained after carrying out the heating step (b), or the residue that has been subjected to a subsequent water-washing treatment or the like, has a significantly reduced alkali metal content compared to the target material before treatment, and can therefore be effectively used as a cement raw material in place of coal ash.
[0022] In addition, by adding a sulfur source and heating the target object, the sulfur source functions as a flux, and has the effect of melting the alkali metal-containing material, particularly the surface area thereof, at a lower temperature. As a result, it becomes possible to proceed with the reaction of removing the alkali metal from the target object even at a lower temperature than in conventional chlorination roasting.
[0023] From this viewpoint, the step (b) may be a step of heating at a temperature of 600° C. to 1200° C. This temperature is lower than that in the conventional method in which chlorination roasting is carried out at a temperature exceeding 1200° C.
[0024] If the heating step (b) is carried out at a temperature lower than 600°C, the alkali metal may not be easily converted into an alkali metal salt due to the low temperature. If the heating temperature exceeds 1200°C, the chlorine contained in the chlorine-containing material may be easily volatilized, and the amount of contact with the alkali metal may decrease, resulting in a decrease in reactivity. The temperature at which the step (b) is carried out is more preferably 800°C to 1100°C.
[0025] Such a heating step (b) can be carried out, for example, in a rotary kiln, which allows the mixture to be heated at high temperatures while being stirred.
[0026] In addition, by heating the calcium source and chlorine source in a mixed state, some of the Cl contained in the chlorine source reacts with the Ca contained in the calcium source and can be fixed as calcium chloride (CaCl2). The volatilization rate of CaCl2 is slower than that of Cl2 and HCl. As a result, the amount of Cl contained in the chlorine source that volatilizes without contributing to the reaction with the alkali metal contained in the target material can be suppressed.
[0027] As the calcium source, one or more selected from the group consisting of industrial raw materials containing at least one of CaCO3 and CaO, paper sludge, paper sludge incineration ash, waste concrete fines, ready-mixed concrete sludge, chlorine bypass dust water-washing residue, chlorine bypass dust classified coarse powder, gypsum, and waste gypsum board can be used. Among the materials listed above, the chlorine bypass dust water-washing residue, chlorine bypass dust classified coarse powder, gypsum, and waste gypsum board can also be used as a sulfur source. In other words, in step (a), by mixing the chlorine bypass dust water-washing residue and / or the chlorine bypass dust classified coarse powder with the target, it is possible to mix both the calcium source and the sulfur source with the target.
[0028] The chlorine source may be one or more selected from the group consisting of chlorine-containing combustible waste and inorganic chlorine compounds. Examples of chlorine-containing combustible waste include waste plastics containing at least one organic chlorine in the monomer, such as waste polyvinyl chloride. Examples of inorganic chlorine compounds include CaCl2, MgCl2, PbCl2, etc.
[0029] The chlorine source is preferably 80 mm or less in size. By carrying out the heating step (b) while mixing a chlorine source of this size with the target material, the poorly soluble alkali metal contained in the target material can be converted into a water-soluble salt at a high rate. If the size of the chlorine source is larger than 80 mm, chlorine may not be sufficiently volatilized from the chlorine source during the heating step (b), making it difficult to chlorinate the target material. The size of the chlorine source referred to here is the size of the sieve opening, and a size of 80 mm or less refers to one that passes through a sieve with an opening of 80 mm.
[0030] As the sulfur source, one or more selected from the group consisting of gypsum, waste gypsum board, chlorine bypass dust washing residue, chlorine bypass dust classified coarse powder, sewage sludge, sewage sludge incineration ash, polyferric sulfate, and sulfur-containing combustible organic waste can be used.
[0031] The step (a) (a1) mixing the alkali metal-containing material with the sulfur source and the calcium source to adjust the hydraulic ratio and SO3 concentration of the alkali metal-containing material; The method may further include a step (a2) of mixing the chlorine source with the mixture obtained in the step (a1).
[0032] In particular, when the residue of the water washing of chlorine bypass dust is used as the sulfur source, the SO3 concentration and Cl concentration contained in the residue obtained by washing the chlorine bypass dust with water are affected by the water washing conditions, etc. For this reason, the mixing amounts of the sulfur source and calcium source are set so as to obtain the desired hydraulic ratio and SO3 concentration before mixing the chlorine source, and then the chlorine source is mixed in an amount adjusted to obtain a preferred Cl amount, whereby chlorination roasting can be performed under environmental conditions that allow a high alkali removal rate to be achieved.
[0033] The step (a) may include a step of adding the sulfur source and the calcium source in amounts adjusted so that the mixture obtained through the step (a) has a hydraulic ratio in the range of 0.2 to 1.0 and an SO3 concentration in the range of 2 to 10 mass%.
[0034] In this specification, the hydraulic ratio may be defined by the following formula based on the composition ratio of CaO, SiO2, Al2O3, and Fe2O3 contained in the mixture. Hydraulic rate (HM)=(CaO[%]) / {SiO2[%]+Al2O3[%]+Fe2O3[%]} The composition ratio of the mixture may be determined by X-ray fluorescence analysis (XRF).
[0035] By adding a calcium source so that the hydraulic coefficient is 0.2 or more, the removal rate of alkali metals contained in the target material is sufficiently increased. On the other hand, if the calcium source is added so that the hydraulic coefficient exceeds 1.0, the amount of target material that can be heated at one time in the heating step (b) decreases. This is because there is a limit to the amount of powder that can be added at one time to the combustion furnace in which the heating step (b) is performed. In other words, the amount of target material from which alkali metals can be removed in the same amount of time decreases, and the treatment speed decreases.
[0036] From this viewpoint, in the mixing step (a), it is preferable to add the calcium source in an amount adjusted so that the hydraulic coefficient of the mixture is 0.2 to 1.0.
[0037] In addition, if the SO3 concentration in the mixture is less than 2% by mass, the effect of increasing the removal rate of alkali metals is not sufficiently obtained. On the other hand, if the SO3 concentration exceeds 10% by mass, the action of the sulfur source as a flux in step (b) becomes too strong, and the entire object may be sintered or melted, or the sintering or melting may proceed too far. As a result, KCl, NaCl, K2SO4, Na2SO4, etc. produced by chlorination roasting are difficult to volatilize, and the effect of improving the removal rate of alkali metals may not be sufficiently obtained.
[0038] From this viewpoint, in the mixing step (a), it is preferable to add the sulfur source in an amount adjusted so that the SO3 concentration in the mixture falls within the range of 2 to 10 mass %.
[0039] The step (a) may include a step of introducing the chlorine source in an amount adjusted so that the Cl / K ratio, which is the ratio of the molar amount of Cl contained in the chlorine source to the molar amount of K (potassium) contained in the waste, is within a range of 1 to 4.
[0040] According to the above method, most of the sparingly soluble alkali metals contained in the target material can be efficiently converted into water-soluble salts. If the Cl / K ratio exceeds 4, chlorine that does not contribute to chlorination roasting remains, and some of the chlorine source may be wasted. Furthermore, the amount of slaked lime (Ca(OH)2) used to recover Cl and S from the exhaust gas discharged during the execution of the heating step (b) increases, which is uneconomical and may cause operational problems in the heating device. Conversely, if the Cl / K ratio is below 1, the heat-treated product obtained after the completion of the heating step (b) may still contain a certain amount of sparingly soluble alkali metals.
[0041] The step (a) may include a step of mixing one or both of the chlorine source and the calcium source recovered from the exhaust gas discharged through the step (b).
[0042] According to the above-mentioned method, the chlorine-containing substance and / or the calcium-containing substance contained in the exhaust gas can be reused as a chlorine source and / or a calcium source, respectively, in the treatment of removing alkali metals from a target object, which contributes to reducing material costs and making effective use of resources.
[0043] When sulfur-containing combustible organic waste is used as the sulfur source, the sulfur source may be charged from the front side of the kiln where the heating step is carried out.
[0044] If a combustible sulfur source is added from the bottom side of the kiln, the proportion of the sulfur source that is discharged as exhaust gas without coming into contact with the target material in the kiln may increase. In contrast, if a combustible sulfur source is added from the front side of the kiln, the burned sulfur content flows through the kiln toward the bottom side along with the flow of secondary air, and during this time the sulfur content comes into contact with the target material, increasing the reaction efficiency.
[0045] The method for removing an alkali metal includes, before the step (a), a step (d) of pulverizing the alkali metal-containing material, The step (a) may be a step of mixing the pulverized alkali metal-containing material with a sulfur source, a calcium source, and a chlorine source.
[0046] It is assumed that the alkali metal-containing material contains poorly soluble alkali metals evenly throughout. By subjecting the alkali metal-containing material to a crushing process, the exposed area of the alkali metal increases. Therefore, by mixing the crushed alkali metal-containing material with a sulfur source, a calcium source, and a chlorine source and then subjecting it to the heating step (b), the reactivity with Cl contained in the chlorine source is improved, and the material can be converted to an alkali metal chloride more efficiently.
[0047] In the step (d), the alkali metal-containing material after pulverization has a Blaine specific surface area of 7,000 cm 2 The Blaine specific surface area is preferably 1,000 cm 2 / g~7,000cm 2 / g is more preferable.
[0048] The method for removing an alkali metal includes a step (e) of pulverizing the mixture obtained in the step (a), The step (b) may be a step of heating the pulverized mixture.
[0049] The step (b) may be a step of heating in an air atmosphere, or a step of heating in an atmosphere with an oxygen concentration of 10% or less.
[0050] By carrying out the heating step (b) under a low oxygen concentration, excessive volatilization of the chlorine contained in the chlorine source is suppressed, and the alkali metal contained in the target material is more easily converted into a water-soluble alkali metal chloride. Effect of the Invention
[0051] According to the present invention, alkali metals can be efficiently removed from alkali metal-containing materials, which allows waste materials such as construction waste soil and biomass ash to be utilized as raw materials for cement, etc. [Brief description of the drawings]
[0052] [Figure 1] 1 is a flow chart that illustrates a procedure of a method for treating an alkali metal-containing material. [Diagram 2] 2 is a diagram illustrating an example of an apparatus for carrying out the method shown in FIG. 1. [Diagram 3] 2 is a diagram illustrating a schematic diagram of another example of an apparatus for carrying out the method shown in FIG. 1. [Figure 4] 3 is a diagram showing a schematic diagram of an example of a treatment facility for the exhaust gas discharged from the apparatus shown in FIG. 2. [Diagram 5] FIG. 3 is a schematic diagram showing a case where a sulfur source is introduced from different positions in the apparatus shown in FIG. 2. [Figure 6] 10 is a flow chart that illustrates a schematic diagram of another procedure of the method for treating an alkali metal-containing material. [Figure 7] 7 is a diagram illustrating an example of an apparatus for carrying out the method shown in FIG. 6. [Figure 8] 10 is a flow chart that illustrates a schematic diagram of another procedure of the method for treating an alkali metal-containing material. [Figure 9] 10 is a flow chart that illustrates a schematic diagram of another procedure of the method for treating an alkali metal-containing material. [Figure 10] 10 is a diagram illustrating an example of an apparatus for carrying out the method shown in FIG. 9. [Figure 11]This is a graph comparing the effect on the K removal rate when the SO3 concentration in the mixture is changed. [Figure 12] 1 shows XRD spectra after heat treatment in levels #10, #18, and #P6. [Figure 13] This is a graph comparing the effect on the K removal rate when the heating and firing temperature conditions are different for the target material, decomposed granite soil. [Figure 14] This is a graph comparing the effect on the K removal rate when the hydraulic hardness of the mixture is changed. [Figure 15] This is a graph comparing the effect on K removal rate when the amount of chlorine source is adjusted to change the Cl / K ratio of the mixture. [Figure 16] This is a graph comparing the effect on the K removal rate when the heating and firing temperature conditions are changed using biomass ash as the target material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0053] The alkali metal-containing material to be treated in the present invention is not particularly limited as long as it is a non-flammable alkali metal-containing material that contains a high concentration of alkali metal components. Examples of the alkali metal-containing material include waste materials such as fly ash and bottom ash of wood biomass ash, construction waste soil, and recycled fine powder of waste concrete.
[0054] Wood biomass ash contains alkali metals (Na, K) as chlorides, carbonates, sulfates, and silicate glass, and in terms of RO (RO = Na2O + 0.658 x KO), the fly ash of wood biomass ash contains about 3% to 50% by mass, and the bottom ash of wood biomass ash contains about 3% to 20% by mass. Of the alkali metals listed above, the chlorides, carbonates, and sulfates are water-soluble, while the silicate glass is sparingly soluble.
[0055] In addition, recycled fine powder from construction soil and waste concrete contains alkali metals (Na, K) in the form of feldspar (albite, potassium feldspar), and contains about 2.5% to 8% by mass in terms of RO.
[0056] According to the present invention, the concentration of the alkali metal component contained in the alkali metal-containing material can be reduced to 2.5 mass% or less, more typically 2.0 mass% or less, calculated as RO. In particular, it is possible to remove 50% or more of the potassium (K) contained in the alkali metal-containing material. Therefore, the alkali metal-containing material after the treatment can be effectively used, for example, as a cement raw material. The concentration of the alkali metal in the alkali metal-containing material can be measured by a known method, such as a FP method using a fluorescent X-ray device or wet analysis (acid decomposition-ICP emission spectrometry).
[0057] The present invention will be described in more detail below with reference to the drawings. However, the present invention is not limited to the embodiments described with these drawings.
[0058] Fig. 1 is a flow chart showing a typical procedure of an alkali metal removal method. Fig. 2 is a block diagram showing a typical example of an apparatus (hereinafter referred to as "alkali metal removal apparatus") for carrying out the alkali metal removal method shown in Fig. 1. In Fig. 2, the flows of solids such as biomass ash and construction waste soil and liquids such as water are indicated by solid lines with arrows, and the flows of gas are indicated by dashed lines with arrows. This is the same in each of the figures described below.
[0059] 1, the alkali metal removal method of the present embodiment includes a mixing step S1, a mixing step S2, a heating step S3, and a water-washing step S4. Moreover, the alkali metal removal apparatus 1 shown in FIG. 2 includes a mixing device 5, a mixing device 6, a heating device 7, and a water-washing device 9.
[0060] The processing contents in each step shown in FIG. 1 will be described in detail below with reference to FIG. 2 as needed.
[0061] (Mixing process S1) The mixing step S1 is a step of mixing a calcium source CA and a sulfur source S with a treatment target such as biomass ash or construction generated soil (hereinafter referred to as "target BT"). In the alkali metal removal apparatus 1 shown in FIG. 2, the mixing step S1 is performed by a mixer 5.
[0062] 2, the target object BT is supplied from a storage tank 2 in which the target object BT is stored to a mixer 5. The storage tank 2 may be provided with a supply device capable of adjusting the amount of the target object BT supplied to the mixer 5.
[0063] The calcium source CA is not particularly limited as long as it contains calcium (Ca), but it is preferable that it contains at least one of CaCO3 and CaO. In addition, from the viewpoints of ease of availability and environmental considerations, industrial raw materials such as limestone, quicklime, and slaked lime, and waste materials such as paper sludge, paper sludge incineration ash, sewage sludge incineration ash, waste concrete fine powder, and ready-mixed concrete sludge can be suitably used as the calcium source CA. For example, the alkali metal removal device 1 may be provided with a storage tank for the calcium source CA (not shown), and the calcium source CA stored in this storage tank may be supplied quantitatively to the mixer 5. More preferably, the storage tank for the calcium source CA may be provided with a discharge adjustment device such as a discharge adjustment valve, and the supply amount of the calcium source CA may be adjusted by appropriately controlling this discharge adjustment device.
[0064] The calcium source CA preferably contains 10% by mass or more of Ca, more preferably 30% by mass or more, and particularly preferably 50% by mass or more. The Ca concentration in the calcium source CA can be measured by a known method, for example, the FP method and the calibration curve method using an X-ray fluorescence device, or wet analysis (acid decomposition-ICP atomic emission spectrometry).
[0065] The calcium source CA is added for the purpose of adjusting the hydraulic ratio of the target object BT. The hydraulic ratio is an index also called HM, and may be defined by the following formula based on the composition ratio of CaO, SiO2, Al2O3, and Fe2O3 contained in the target object BT. The composition ratio of the target object may be a value obtained by X-ray fluorescence analysis (XRF). Hydraulic rate (HM)=(CaO[%]) / {SiO2[%]+Al2O3[%]+Fe2O3[%]}
[0066] In the mixing step S1, the amount of the calcium source CA added is adjusted so that the hydraulic ratio of the mixture BC containing the target object BT and the calcium source CA is preferably 0.2 or more, more preferably 0.2 to 1.0.
[0067] The calcium source CA is mixed with the target object BT in a state where it is mixed therewith and the subsequent heating step S3 is carried out, so that it reacts with silicon components such as SiO2 and K2O·4SiO2 (potassium glass) contained in the target object BT to produce Ca-containing minerals. From this viewpoint, in order to form a good mixed state with the target object BT, the calcium source CA is preferably 5 mm or less in size, more preferably 3 mm or less in size, and particularly preferably 1 mm or less in size. The size of the calcium source CA refers to the smallest sieve opening through which the calcium source CA can pass.
[0068] From the above viewpoint, a classification device for removing coarse particles from the received calcium source CA and a crushing and classifying device for pulverizing the coarse particles to a predetermined particle size may be provided upstream of the storage tank for storing the calcium source CA. These classification devices and crushing and classifying devices may be used appropriately depending on the state of the received calcium source CA.
[0069] The sulfur source S is not particularly limited as long as it contains sulfur (S), but in view of ease of availability and environmental considerations, gypsum, waste gypsum board, chlorine bypass dust washing residue, chlorine bypass dust classified coarse powder, sewage sludge, sewage sludge incineration ash, polyferrous sulfate, sulfur-containing combustible organic waste, etc. can be suitably used. For example, the alkali metal removal device 1 may be provided with a storage tank for the sulfur source S (not shown), and the sulfur source S stored in this storage tank may be supplied quantitatively to the mixer 5. More preferably, the storage tank for the sulfur source S may be provided with an emission control device such as an emission control valve, and the supply amount of the sulfur source S may be adjusted by appropriately controlling this emission control device.
[0070] The sulfur source S is added for the purpose of adjusting the SO3 concentration of the target object BT. In the mixing step S1, the amount of the sulfur source S added is adjusted so that the SO3 concentration of the mixture BC containing the target object BT and the sulfur source S is preferably 2 to 10 mass%.
[0071] The purpose of mixing the sulfur source S is twofold. The first purpose is to react with some of the alkali metals contained in the target object BT in a state in which the sulfur source S and the target object BT are mixed together in the subsequent heating step S3, thereby producing highly volatile sulfur compounds such as Na2SO4 and K2SO4. The second purpose is to cause the sulfur source S to function as a flux and melt the alkali metal-containing object, particularly the surface area thereof, at a lower temperature than before in the heating step S3 that is performed in a state in which the sulfur source S and the target object BT are mixed together.
[0072] From the above viewpoint, it is preferable that the sulfur source S also forms a good mixed state with the target object BT, similarly to the calcium source CA. Specifically, the sulfur source S is preferably 5 mm or less in size, more preferably 3 mm or less in size, and particularly preferably 1 mm or less in size. The size of the sulfur source S refers to the smallest sieve opening through which the sulfur source S passes.
[0073] Incidentally, among the above materials listed as the sulfur source S, gypsum, waste gypsum board, residue of washing of chlorine bypass dust, and classified coarse powder of chlorine bypass dust also contain Ca components. Therefore, the sulfur source S and the calcium source CA can be the same material.
[0074] In this case, the amount of sulfur source S added is determined so that the SO3 concentration of the mixture BC falls within the above-mentioned preferred range (specifically, 2 to 10% by mass), and then the hydraulic ratio of the mixture BC is calculated based on the amount of calcium source CA derived from the determined amount of sulfur source S added. Then, only when the calculated hydraulic ratio does not reach the above-mentioned preferred range (specifically, 0.2 or more), a necessary amount of calcium source CA may be added separately. The calcium source CA added additionally at this time may be selected from materials not containing S components.
[0075] This mixing step S1 corresponds to the step (a1).
[0076] (Mixing process S2) The mixing step S2 is a step of mixing the mixture BC having the hydraulic ratio adjusted as described above with a chlorine source CL to be used in the chlorination roasting.
[0077] The chlorine source CL is not particularly limited as long as it contains chlorine, but it is possible to suitably use waste plastics containing at least one organic chlorine in monomers such as waste polyvinyl chloride, or combustible waste mixed with inorganic chlorine compounds such as CaCl2, MgCl2, or PbCl2. For example, the alkali metal removal device 1 may be provided with a storage tank for a chlorine source (not shown), and the chlorine source CL stored in this storage tank may be supplied quantitatively to the mixer 6. More preferably, the storage tank for the chlorine source CL may be provided with an emission control device such as an emission control valve, and the supply amount of the chlorine source CL may be adjusted by appropriately controlling this emission control device.
[0078] The chlorine source CL preferably contains 0.8 mass% or more of chlorine (Cl), more preferably contains 1.2 mass% or more, and particularly preferably contains 2 mass% or more. The Cl concentration in the chlorine source CL can be measured by a known method, for example, FP method using a fluorescent X-ray device or wet analysis (Eschka decomposition-ion chromatography method).
[0079] The chlorine source CL is mixed with the target object BT in the subsequent heating step S3, for the purpose of efficiently causing chlorination and volatilization of the alkali metal contained in the target object BT. From this viewpoint, the chlorine source CL is preferably 80 mm or less in size, more preferably 40 mm or less in size, and particularly preferably 10 mm or less in size, so as to form a good mixed state with the target object BT and to facilitate volatilization of chlorine from the chlorine source CL. The size of the chlorine source CL refers to the smallest sieve opening through which the chlorine source CL passes.
[0080] From the above viewpoint, a classification device for removing coarse materials from the received chlorine source CL and a crushing and classifying device for making the coarse materials into a predetermined particle size may be installed upstream of the storage tank for storing the chlorine source CL. These classification devices and crushing and classifying devices may be used appropriately depending on the state of the received chlorine source CL.
[0081] The ratio of the target object BT to the chlorine source CL is preferably set so that the Cl / K ratio, which is the ratio of the molar amount of Cl contained in the chlorine source CL to the molar amount of potassium (K) contained in the target object BT, is 1 to 4. The Cl / K ratio is more preferably 2 to 4, and particularly preferably 2 to 3.
[0082] If the Cl / K ratio is below 1, the amount of chlorine contained in the mixture BC heated in the heating device 7 is small, and therefore, among the alkali metal components in the target object BT, many alkali metal components that cannot react with chlorine may remain. On the other hand, if the Cl / K ratio value exceeds 4, the amount of chlorine that volatilizes and dissipates may increase, accelerating the progress of corrosion of the equipment.
[0083] In addition, in Fig. 2, it is assumed that the mixture containing the target object BT, the calcium source CA, the sulfur source S, and the chlorine source CL are mixed in the mixing device 6, but the embodiment of the mixing step S2 is not limited to the configuration shown in Fig. 2. For example, as shown in Fig. 3, the chlorine source CL may be directly charged into the heating device 7. In this case, the heating device 7 also serves as the mixing device 6.
[0084] The mixing step S2 corresponds to the step (a2). The mixing steps S1 and S2 correspond to the step (a).
[0085] In the following, the explanation will be continued with reference to the alkali metal removal apparatus 1 shown in FIG. 2, but the same explanation can be applied to the case where the alkali metal removal apparatus 1 in FIG. 3 is used.
[0086] (Heating process S3) The heating step S3 is a step of heating the mixture BC containing the target object BT, the calcium source CA, the sulfur source S, and the chlorine source CL obtained through the mixing steps S1 and S2. The heating step S3 efficiently converts poorly soluble alkali metal salts contained in the target object BT into water-soluble or volatile alkali metal salts. In the alkali metal removal apparatus 1 shown in FIG. 2, the heating step S3 is performed by a heating device 7.
[0087] As described above, the heating device 7 heats the target object BT, the calcium source CA, the sulfur source S, and the chlorine source CL together. As a result, the alkali metal in the target object BT reacts with the chlorine volatilized from the chlorine source CL to generate water-soluble alkali metal chlorides. Furthermore, during the execution of the heating step S3, the S component contained in the sulfur source S reacts with the alkali metal to generate volatile sulfur compounds. Note that, since the temperature inside the heating device 7 is high, at least a portion of the generated alkali metal chlorides is also volatilized.
[0088] The heating temperature in the heating step S3 is preferably 600° C. to 1200° C., more preferably 800° C. to 1100° C., from the viewpoint of efficiently causing chlorination roasting by the alkali metal in the target object BT and the chlorine in the chlorine source CL while making it difficult for the target object BT itself to melt. If the heating temperature is less than 600° C., the reaction of chlorination roasting becomes insufficient, and in some cases, a water-soluble alkali metal salt may not be produced or may be produced at a low efficiency.
[0089] However, when the mixture of the target object BT and the chlorine source CL is simply heated at a high temperature of 1000°C or higher without mixing the calcium source CA, the target object BT may be sintered, and the particle surface or the entire particle may melt to increase the diameter, which may result in the inclusion of water-soluble alkali metal salts. In this case, even if the water washing process is performed in the subsequent water washing step S4, the alkali metal salts will not be dissolved in water and will remain. However, in this embodiment, the target object BT and the chlorine source CL, as well as the calcium source CA, are mixed and heated by the heating device 7. When such a mixture BC is heated at a high temperature, a part of the target object BT produces a mineral derived from Ca contained in the calcium source CA. Since this mineral has a higher melting point than the target object BT, the phenomenon of encapsulating the molten alkali metal salts is unlikely to occur. As a result, the rate of alkali metal salts removed by the subsequent water washing step S4 is increased.
[0090] The more preferable temperature conditions vary depending on the form of the alkali metal contained in the target BT. For example, when the target BT is construction waste soil or recycled fine powder of waste concrete, the alkali metal is contained in the form of feldspar. Even biomass ash may contain alkali metal in the form of feldspar. When only the calcium source CA is mixed with the target BT containing a large amount of alkali metal in the form of feldspar, the effect cannot be fully obtained unless the target is roasted under chlorination at an extremely high temperature.
[0091] However, as described above, in the method of the present embodiment, the target object BT is mixed with the sulfur source S together with the calcium source CA in the mixing step S1. In the heating step S3, the sulfur source S is heated and functions as a flux, resulting in the action of melting the surface vicinity of the alkali metal-containing object at a lower temperature. Meanwhile, in the heating step S3, the target object is transformed into a mineral derived from Ca contained in the calcium source CA, and this mineral has a higher melting point than the target object BT. Therefore, according to this heating step S3, while the surface vicinity of the target object BT is melted, overall melting and sintering are suppressed, so that the amount of alkali metal salt taken into the inside of the target object BT can be reduced.
[0092] In this way, in the heating step S3, the target object BT is heated together with the sulfur source S, so that even if the target object BT contains an alkali metal in the form of feldspar, it is possible to melt the alkali metal-containing object, particularly the surface vicinity, under lower temperature conditions. The preferred heating temperature is 600°C to 1200°C, and the more preferred heating temperature is 800°C to 1100°C.
[0093] The heating time in the heating step S3 may be appropriately set within a range of 5 minutes to 2 hours depending on the heating temperature. In order to sufficiently react the alkali metal in the target object BT with the chlorine in the chlorine source CL, the heating time needs to be short when the heating temperature is high and long when the heating temperature is low. Specifically, it is preferable to set the heating time to 30 minutes to 2 hours when the heating temperature is 600°C, 10 minutes to 90 minutes when the heating temperature is 800°C, and 5 minutes to 60 minutes when the heating temperature is 1000°C.
[0094] The atmosphere in the heating device 7 is not particularly limited, and may be an oxidizing atmosphere or a reducing atmosphere. In the example shown in FIG.
[0095] In the heating device 7, in order to efficiently generate a reaction for producing a water-soluble alkali metal salt, it is desirable to heat the target material BT and the chlorine source CL in a state of being sufficiently mixed. From this viewpoint, the heating device 7 can be configured with an internal combustion rotary kiln. If the calcination furnace is a rotary kiln in which rotational motion occurs, it is possible to perform a heat treatment while physically and continuously mixing and stirring the target material BT, the calcium source CA, the sulfur source S, and the chlorine source CL.
[0096] Furthermore, from the above viewpoint, it can be said that an embodiment in which a mixture BC in a mixed state of the target object BT, the calcium source CA, the sulfur source S, and the chlorine source CL is introduced into the heating device 7 is more preferable, as in the alkali metal removal apparatus 1 shown in Fig. 2. However, even in the embodiment in which the chlorine source CL is mixed with the target object BT in the heating device 7 as in Fig. 3, the reaction for producing a water-soluble alkali metal salt can be efficiently caused by performing a heat treatment after (or while) the target object BT is sufficiently mixed.
[0097] When the heating atmosphere in the heating device 7 (typically a rotary kiln) is the air G1, the air G1 as combustion air is supplied to the heating device 7 from an intake fan 33. In the rotary kiln, the air G1 used as the combustion air for the internal combustion burner 31 by the intake fan 33 flows inside the kiln in a countercurrent direction to the flow of the mixture BC, and then is discharged outside the kiln as combustion exhaust gas G2.
[0098] When the heating atmosphere is a gas with a low oxygen concentration (e.g., nitrogen), the gas with a low oxygen concentration is flowed into the heating device 7 instead of the atmosphere G1 in Fig. 2. The source of this gas with a low oxygen concentration may be an air separation device that separates oxygen from air, or a gas exhaust path through which exhaust gas from another combustion furnace is discharged. Furthermore, as shown in Fig. 2, the oxygen concentration of the atmosphere in the heating device 7 may be reduced by adjusting the amount of intake air and the amount of fuel burned while air is flowed into the heating device 7 through an intake fan 33.
[0099] The heating device 7 is not particularly limited as long as it can heat the mixture of the target object BT and the chlorine source CL at a high temperature, typically in the temperature range of 600° C. to 1200° C., and a heating furnace such as a fixed furnace, a stoker furnace, a rotary kiln, a fluidized bed furnace, a vertical furnace, a multi-stage furnace, etc. Among them, the above-mentioned rotary kiln is preferable from the viewpoint of physical stirring.
[0100] A heat-treated product P1 is discharged from the heating device 7. The heat-treated product P1 is a mixture of the target object BT or Ca-containing mineral in a state in which poorly soluble alkali metals have been converted into water-soluble salts, the calcium source CA, the sulfur source S, and the incineration residue of the chlorine source CL. The discharged heat-treated product P1 is sent to a water-washing device 9.
[0101] However, chlorine (Cl2), alkali metal chlorides such as KCl and NaCl generated in the heating step S3, and sulfur compounds are easily volatilized under the above temperature conditions. Therefore, these substances may be contained in the exhaust gas G2. Therefore, it is possible to recover the chlorine-containing substances and sulfur compounds contained in the exhaust gas G2 and reuse them as the chlorine source CL and the sulfur source S, respectively.
[0102] For example, as shown in Fig. 4, the exhaust gas G2 discharged through the exhaust gas tower 41 passes through a cyclone 42 to remove dust Z1 contained in the exhaust gas G2, and then the gaseous portion is guided to a pipe 43. The dust Z1 contains alkali metals such as KCl, K2SO4, and NaCl.
[0103] A treating agent ET is added from a treating agent supplying unit 44 to the combustion exhaust gas G2 flowing through the pipe 43. The treating agent ET is used to remove chlorine-containing substances (HCl, Cl2, etc.) and sulfur compounds (SO x Any material that can be reacted with thiocarbamate (Ca(OH)2), Mg(OH)2, and mixtures thereof (dolomite hydroxide) can be used.
[0104] When Ca(OH)2 is used as the treatment agent ET, chlorine-containing substances contained in the exhaust gas G2 react with Ca(OH)2 to produce CaCl2, CaClOH, etc., and sulfur compounds contained in the exhaust gas G2 react with Ca(OH)2 to produce CaSO4, CaSO3, Ca(HSO3)2, etc.
[0105] The exhaust gas G2, which is mixed with the products by being treated with the treating agent ET, is separated into solid and gas through a bag filter 45, and the gas component is discharged as exhaust gas G3. This gas can be released to the outside air because it has been desalted and desulfurized. Among the recovered solid components, CaCl2, CaClOH, etc. can be reused as the chlorine source CL, unreacted Ca(OH)2 can be reused as the calcium source CA, and CaSO4, CaSO3, Ca(HSO3)2, etc. can be reused as the sulfur source S and calcium source CA. In addition, when Mg(OH)2 is used as the treating agent ET, MgCl2, etc. can be reused as the chlorine source CL, and MgSO4, etc. can be reused as the sulfur source S. However, in this case, unreacted Mg(OH)2 cannot be reused as a raw material in this heating step S3.
[0106] Incidentally, when a combustible material (organic waste) containing sulfur is used as the sulfur source S, as shown in FIG. 2, if the combustible sulfur source S is charged from the end of the heating device 7 composed of a rotary kiln, it may be immediately vaporized and discharged together with the exhaust gas G2 through the exhaust gas tower 41. In this case, the time of contact with the target material BT is shortened, and the function as the sulfur source S may not be fully exerted. From this viewpoint, in the case of the combustible sulfur source S, it may be charged into the heating device 7 from the front side (the internal combustion burner 31 side) as shown in FIG. 5. In this way, the combustible sulfur source S is carried by the secondary air flow flowing in the opposite direction to the flow of the mixture BC in the heating device 7 toward the end of the kiln, and the time for contacting the mixture BC in the heating device 7 is secured.
[0107] This heating step S3 corresponds to step (b).
[0108] (Water washing process S4) The water-washing step S4 is a step of washing the heat-treated product P1 obtained in the heating step S3 with water. This water-washing step S4 dissolves and removes water-soluble alkali metal salts remaining in the heat-treated product P1. In the alkali metal removal apparatus 1 shown in FIG. 2, this water-washing step S4 is performed by a water-washing device 9.
[0109] The solvent used in this water washing step S4 is preferably water.
[0110] In the water washing device 9, the heat-treated material P1 supplied from the heating device 7 is mixed with water W1 to generate a slurry Lr1, and then the slurry Lr1 is continuously stirred to dissolve the water-soluble alkali metal salt in the heat-treated material P1 in the water.
[0111] As an example, the water washing device 9 shown in Fig. 2 is provided with a supply hopper 11 for the heat-treated material P1 and a supply device 13 for water W1. The water washing device 9 is also provided with a slurry agitator 35 for mixing the heat-treated material P1 and the water W1 and agitating the slurry Lr1 produced by the mixing. The slurry agitator 35 is preferably of a general paddle type or screw type, for example, and is provided with an agitator blade in the example shown in Fig. 2.
[0112] A crushing device for crushing large-diameter objects in the received heat-treated object P1 to an appropriate size may be provided upstream of the supply hopper 11. This crushing device may be used appropriately depending on the state of the heat-treated object P1 supplied from the heating step S3.
[0113] The solubility of water-soluble alkali metal salts in water is very high, and the solubility does not change significantly even if the water temperature is changed. Therefore, as the solvent used in the water-washing step S4, room temperature water may be used in an amount of at least three times, preferably at least four times, more preferably at least five times the mass of the heat-treated product P1 (hereinafter sometimes referred to as the "water-washed product").
[0114] In the water-washing step S4, the stirring time of the slurry Lr1 consisting of the washed material and water is preferably 10 minutes or more, more preferably 15 minutes or more, and particularly preferably 20 minutes or more. Since water-soluble alkali metal salts are usually very soluble in water, no special conditions are required for stirring the slurry Lr1.
[0115] The water washing step S4 dissolves the alkali metal remaining in the heat-treated product P1 in water. The slurry Lr1 in which the alkali metal is dissolved in water is separated by a solid-liquid separator 17 installed downstream into a solid (cake C1) that has a reduced moisture content and can be used as a cement raw material, etc., and wastewater W3.
[0116] When transporting the slurry Lr1 to the solid-liquid separator 17, a general-purpose slurry liquid transport device (not shown) such as a slurry centrifugal pump, a piston pump, a mono pump, or a hose pump may be used.
[0117] As the solid-liquid separator 17, a general-purpose filter such as a filter press, a pressurized leaf filter, a screw press, a belt press, a belt filter, etc. may be used. In the embodiment shown in Fig. 2, the solid-liquid separator 17 is illustrated as being composed of a filter press.
[0118] The solid-liquid separator 17 is provided with a supply device 15 for washing water W2, and separates the transported slurry Lr1 into a cake C1 (solid phase) of the washed product and wastewater W3 (liquid phase) containing alkali metals. At this time, the cake C1 is separated while being washed with the washing water W2. As the washing water W2, room temperature water may be used in an amount of at least three times, preferably at least four times, and more preferably at least five times the mass of the washed product.
[0119] The cake C1 separated by the solid-liquid separator 17 has an alkali metal component concentration reduced to 2.0 mass % or less, more typically 1.5 mass % or less, and further typically 1.0 mass % or less, and can be effectively used as a cement raw material, etc. The alkali metal concentration here refers to an analytical value obtained by a well-known method, for example, an FP method using an X-ray fluorescence device, or an analytical value obtained by wet analysis (acid decomposition-ICP atomic emission spectrometry).
[0120] This water washing step S4 corresponds to step (c).
[0121] [Another embodiment] Another embodiment of the alkali metal removal method will be described below.
[0122] <1> As shown in Fig. 6, a step S5 of pulverizing the target object BT may be performed before the mixing step S1. This pulverizing step S5 is performed, for example, by a pulverizing device 4 shown in Fig. 7. Fig. 7 is a diagram showing a schematic view of a part of the alkali metal removal device 1 following Fig. 1, and a pulverizing device 4 has been added compared to Fig. 1.
[0123] The crushing step S5 is performed to previously reduce the particle size of the target object BT before the mixing step S1. The target object BT with the reduced particle size is mixed with the calcium source CA and the sulfur source S in the mixing step S1. The crushing step S5 and the mixing step S1 may be performed simultaneously by crushing the target object BT together with the calcium source CA and the sulfur source S.
[0124] It is assumed that the target object BT contains poorly soluble alkali metal salts evenly throughout. By carrying out the crushing step S5 before the heating step S3, the exposed area of the alkali metal increases, so that the reactivity with the chlorine contained in the chlorine source CL in the heating step S3 is improved, and the target object BT can be converted into an alkali metal salt more efficiently. Furthermore, in the heating step S3, the reactivity between the silicon content in the target object BT and the calcium contained in the calcium source CA is improved, so that the target object BT is more likely to become a Ca-containing mineral, and excessive melting and sintering of the target object BT can be suppressed.
[0125] The Blaine specific surface area of the target object BT after being pulverized in the pulverization step S5 is preferably 7,000 cm 2 / g or less, and more preferably 1,000 cm 2 / g~7,000cm 2 / g, and particularly preferably 4,000 cm 2 / g~7,000cm 2 / g. The finer the target object BT is, the more the reactivity between the alkali metal contained in the target object BT and the chlorine contained in the chlorine source CL is improved in the heating step S3, but on the other hand, the melting phenomenon of the target object BT itself is more likely to occur.2 When the target object BT is finely divided to a size exceeding 1 / g, melting occurs significantly during the heating step S3, and the alkali metal salt is easily encapsulated.
[0126] The lower limit of the particle size of the target object BT after being pulverized in the pulverization step S5 is a Blaine specific surface area of 7,000 cm 2 If the target object BT is pulverized to such an extent that the particle size is less than 0.5 μm, it will be easily melted and sintered in the subsequent heating step S3.
[0127] As the crushing device 4, a tube mill, a vertical roller mill, a jaw crusher, a gyratory crusher, a cone crusher, an impact crusher, a roll crusher, an aerofall mill, or the like can be suitably used.
[0128] This grinding step S5 corresponds to step (d).
[0129] <2> From the same viewpoint, a pulverizing step may be performed after the mixing step S1 or the mixing step S2. The flowchart shown in Fig. 8 illustrates a case where the pulverizing step S6 is performed after the mixing step S2. The pulverizing step S6 can be performed by the same device as the pulverizing step S5.
[0130] This pulverization step S6 corresponds to step (e). It is to be noted that both the pulverization step S5 and the pulverization step S6 may be carried out.
[0131] <3> As shown in Fig. 9, the calcium source CA, the sulfur source S, and the chlorine source CL may be mixed with the target object BT at the same time. In other words, the mixing step S1 may also serve as the mixing step S2. This mixing step S1 is performed, for example, by a mixing device 5 shown in Fig. 10. Fig. 10 is a schematic diagram of a part of the alkali metal removal device 1 following Fig. 1, similar to Fig. 7.
[0132] However, when the water-washed residue of chlorine bypass dust is used as the sulfur source S, the S concentration and Cl concentration contained in the residue obtained by washing the chlorine bypass dust with water are affected by the water-washing conditions, etc. For this reason, as in the embodiment described above with reference to Fig. 1, it is more preferable to set the mixing amounts of the sulfur source S and the calcium source CA so as to obtain the desired hydraulic ratio and SO3 concentration at a stage before mixing the chlorine source CL, and then mix the chlorine source CL in an amount adjusted to obtain a preferred Cl amount. EXAMPLES
[0133] Specific test examples are presented below to explain the present invention in more detail, but the present invention is not limited to the embodiments of these test examples.
[0134] (Test Explanation) The target object BT was mixed with various materials (calcium source CA, sulfur source S, chlorine source CL, etc.) under different conditions and a heating process was carried out, and the K concentration of the residue obtained after water washing was compared with that of the target object BT before treatment.
[0135] The target object BT was mixed with other materials by bag mixing. The mixture was heated by putting 100 g of the mixture into an alumina crucible and heating and baking it for 60 minutes in a high-speed heating electric furnace (MOTOYAMA, S7-2035D-OP). The mixture after the heat treatment was stirred at room temperature for 30 minutes with four times the amount of water, and the obtained slurry Lr1 was suction filtered, washed with the same amount of water as used for making the slurry Lr1, and filtered to produce cake C1. The K content of the obtained cake C1 was determined by analyzing the acid decomposition sample using ICP atomic emission spectroscopy, and the K removal rate was calculated by comparing it with that before treatment.
[0136] The materials used for the target object BT, sulfur source S, calcium source CA, and CL source are shown in Table 1.
[0137] [Table 1]
[0138] The chlorine bypass dust water-washing residue (KP water-washing residue) is a residue obtained after washing the raw powder of chlorine bypass dust with water. As described above in the embodiment, the KP water-washing residue contains calcium in addition to sulfur, and is therefore both a sulfur source S and a calcium source CA. However, in view of the fact that the KP water-washing residue (and KP before water-washing) are mixed with the primary purpose of adding sulfur, they are classified as "sulfur source S" in Table 1. In addition, gypsum (CaSO4·2H2O) is also classified as "sulfur source S" in Table 1 for the same reason.
[0139] Details of the materials used as the target object BT and the sulfur source S are shown in Tables 2 and 3. As shown in Tables 2 and 3, four patterns (SU2A, SU2B, SU2C, and SU2D) with different washing conditions were used as the KP water-washing residue.
[0140] Table 2 shows the chemical composition of each material shown in Table 1. In Table 2, the alkali metals were analyzed by ICP atomic emission spectroscopy of an acid-digested sample, and the other chemical components were analyzed by the fundamental parameter method (FP method) using an X-ray fluorescence device (Rigaku Corporation, ZSX Primus II). Table 3 shows the mineral composition of each material shown in Table 1, and is based on the results of XRD analysis. In Table 4, the presence of a substance confirmed by XRD analysis is indicated as "○", the presence of a trace amount is indicated as "△", and the absence of a substance at all is indicated as "×". In the following tables, the methods of composition analysis and alkali metal concentration analysis are the same as those described above.
[0141] [Table 2]
[0142] [Table 3]
[0143] As shown in Tables 4 and 5 below, 15 types of mixtures, mixtures BC1 to BC15, were prepared, with the mixing conditions and the composition of the mixtures being as shown in Tables 4 and 5. However, the mixing conditions of the chlorine source CL are not specified in Tables 4 and 5. The mixing conditions of the chlorine source CL will be described later with reference to Table 6 together with the heating conditions.
[0144] In addition, the "mixture description symbols" in the table are symbols that have been assigned for convenience according to the following rules.
[0145] The mixture description symbol consists of four symbols: "substance symbol - sulfur source symbol - calcium source symbol - water hardness symbol", with a sub-number added to the end if necessary.
[0146] The "object symbol" specifies whether the object BT used in the mixture is "decomposed granite soil" or "biomass" as shown in Table 1. If it is decomposed granite soil, it is given the symbol "BT1", and if it is biomass, it is given the symbol "BT2".
[0147] The sulfur source code, as shown in Tables 1 to 3, specifies whether the sulfur source S used in the mixture is "KP water-washing residue", "gypsum dihydrate", or no sulfur source is mixed. When the sulfur source is "KP water-washing residue", a code (SU2A, SU2B, SU2C, or SU2D) corresponding to the KP water-washing residue used is given as shown in Tables 2 to 3. When the sulfur source is "gypsum dihydrate", "SU3" is given. When no S source was added, "N" is given, which stands for Null.
[0148] The calcium source code specifies whether CaCO3 is mixed as the calcium source CA or not, as shown in Table 1. When CaCO3 is mixed as the calcium source CA, "C1" is added, and when CaCO3 is not mixed, "N" is added.
[0149] The hydraulic ratio symbol is a number corresponding to two decimal places of the hydraulic ratio (HM) value targeted when producing the mixture BC. As described above, the hydraulic ratio can be increased by mixing the calcium source CA with the target BT. Therefore, when producing the mixture BC, the amount of the calcium source CA is adjusted so that the desired hydraulic ratio is obtained. As shown in Table 2, the KP water-washing residue (SU2A, SU2B, SU2C, and SU2D) contains CaO. Therefore, when CaCO3 is not mixed as the calcium source CA, the hydraulic ratio can be adjusted by the amount of the KP water-washing residue mixed as the sulfur source S. The hydraulic ratio symbol in the mixture description symbol corresponds to the value of the HM item in Table 4.
[0150] In Table 4, mixtures BC9 to BC12 are assigned sub-numbers. Although the type of target object BT, the type of sulfur source S, the type of calcium source CA, and the hydraulic hardness (HM) value are all set in common for each of the mixtures BC9 to BC12, the mixture ratio of the sulfur source S is different. Therefore, sub-numbers are assigned to distinguish them from each other.
[0151] For example, mixture BC3 is a mixture of decomposed granite soil as the target object BT, KP water washing residue SU2B as the sulfur source S, and CaCO3 as the calcium source CA, and has a hydraulic ratio of 0.35. Mixture BC15 is a mixture of biomass ash as the target object BT and CaCO3 as the calcium source CA, with no sulfur source S, and has a hydraulic ratio of 0.54.
[0152] [Table 4]
[0153] [Table 5]
[0154] In Table 5, SM is the silicate content and IM is the iron content. The values calculated using the following formulas are used. Silicate fraction (SM) = (SiO2 [%]) / {SiO2 [%] + Al2O3 [%] + Fe2O3 [%]} Iron rate (IM)=Al2O3[%] / Fe2O3[%]
[0155] Using the above-mentioned mixtures BC1 to BC15, several levels (#1 to #24, #P1 to P11) were set with different mixing conditions of the chlorine source CL and different heating temperatures. The conditions before the test for each level are as shown in Table 6.
[0156] [Table 6]
[0157] The analytical results of mixture BC after heating and water washing at each level shown in Table 6 are shown in Table 7. [Table 7]
[0158] The results of the examples will be examined below.
[0159] (Verification 1: Relationship between SO3 concentration of mixture and K removal rate) Table 8 below is an excerpt from Tables 6 to 7.
[0160] [Table 8]
[0161] Levels #1, #10, #15, and #16 shown in Table 8 were all identical in terms of the mixture constituent materials, HM, Cl / K, and heating temperature, but the SO3 concentrations of the mixtures before heating were different from one another. In the levels #17 to #20 shown in Table 8, the constituent materials of the mixture, HM, Cl / K, and heating temperature were all the same, but the SO3 concentrations of the mixture before heating were different from one another. Levels #1, #10, #15 to #20, and #P6 shown in Table 8 all had the same HM, Cl / K, and heating temperature.
[0162] The results for levels #1, #10, #15 to #20, and #P6 shown in Table 8 are shown in graph form in FIG.
[0163] FIG. 11 confirms that the K removal rate is improved by adding the sulfur source S even when the HM, Cl / K, and heating temperature are the same.
[0164] In addition, comparing levels #1, #10, #15, and #16 with levels #17 to #20, it can be seen that the improvement in the K removal rate is greater when KP water-washing residue is mixed as the sulfur source S than when gypsum is mixed. From this result, it is presumed that the S component in the KP water-washing residue is more reactive than the S component in gypsum. More specifically, since the S component in the KP water-washing residue exists as a mineral with a relatively low melting point and is highly reactive, it easily reacts with the K and Na components in the target object BT to generate K2SO4 and Na2SO4, and these are removed by volatilization (washing), which is thought to have improved the removal rate.
[0165] On the other hand, the S component contained in gypsum exists as a mineral with a higher melting point than the S component contained in the KP water-washing residue. For this reason, when gypsum is used as the sulfur source S, the effect of making it easier to melt near the surface of the target object BT can be obtained, just as in the case of using the KP water-washing residue, but the S component contained in the sulfur source S is less reactive than the KP water-washing residue. For this reason, it is presumed that when SO3 in the KP water-washing residue dissolves near the surface of the target object BT, which is in a partially molten state, liquid-liquid reactions become dominant and alkali sulfates are generated, whereas in the case of gypsum, which has poor reactivity of the S component, solid-liquid reactions become dominant between the S component contained in the gypsum and the alkali metal contained in the target object BT, and alkali sulfates are generated. For this reason, it is considered that the K removal rate of the KP water-washing residue is improved compared to that of gypsum because the reaction rate between the sulfur source S and the alkali metal is faster in the KP water-washing residue than in gypsum.
[0166] For reference, the XRD spectra after heat treatment in Standards #10, #18, and #P6 are shown in Figure 12, and the comparison results are shown in Table 9. According to the XRD analysis, in Standards #10 and #18, where the sulfur source S was added, K2SO4 and Na2SO4 were not confirmed, so it is believed that these sulfates were removed by volatilization.
[0167] [Table 9]
[0168] According to Fig. 11, in levels #15 and #20 where the SO3 concentration of the raw material (mixture BC) was as high as 11%, the K removal rate fell below 50%. This is believed to be due to the fact that the SO3 concentration was too high, in other words, the sulfur source S was mixed in too much, resulting in more pronounced low-temperature firing and the formation of an environment in which mixture BC is more likely to melt. From this perspective, it is understood that the SO3 concentration of mixture BC is preferably set to 2 to 10 mass%.
[0169] (Verification 2: Relationship between heating and firing temperature and K removal rate) Table 10 below is an excerpt from Tables 6 to 7.
[0170] [Table 10]
[0171] Levels #6 to #11 shown in Table 10 are all the same in terms of the mixture's constituent materials, HM, Cl / K, and the mixture's SO3 concentration and K concentration before heating, but the heating temperatures are different from one another. Levels #P2 to #P7 shown in Table 10 are all the same in terms of the mixture's constituent materials, HM, Cl / K, and the mixture's SO3 concentration and K concentration before heating, but the heating temperatures are different from one another.
[0172] The form of mixture BC differs between standards #6 to #11 and standards #P2 to #P7. In standards #6 to #11, KP water-washing residue SU2B was used as the sulfur source S, and this KP water-washing residue SU2B also served as the calcium source CA. On the other hand, in standards #P2 to #P7, no sulfur source S was added, and CaCO3 was added as the calcium source CA.
[0173] The results for levels #6 to #11 and levels #P2 to #P7 shown in Table 10 are shown in a graph in FIG.
[0174] 13, it can be seen that standards #6 to #11, in which KP water-washing residue SU2B was mixed as the sulfur source S, achieved a high K removal rate even in a low-temperature firing environment, compared with standards #P2 to #P7, in which no sulfur source S was mixed. This result is believed to be due to the fact that, as described above, the mixed sulfur source S functions as a flux, and the target object BT, especially the surface vicinity, melts early even at a relatively low temperature, changing into alkali metal chlorides or alkali metal sulfides, which are then removed by volatilization or water washing.
[0175] 13, it is confirmed that a high K removal rate is obtained up to about 1200°C. On the other hand, when the heating temperature exceeds 1300°C, the chlorine contained in the chlorine source CL is easily volatilized, and the amount of contact with the alkali metal decreases, which may result in a decrease in reactivity. On the other hand, when the temperature is 400°C, it is difficult to say that K is sufficiently removed. From this point of view, the heating and firing temperature is preferably 600°C to 1200°C, at which a K removal rate of 50% or more can be expected, and more preferably 800°C to 1100°C.
[0176] (Verification 3: Relationship between hydraulic hardness and potassium removal rate) Table 11 below is an excerpt from Tables 6 to 7.
[0177] [Table 11]
[0178] Levels #2, #3, #13, and #14 shown in Table 11 have the same Cl / K, the same SO3 concentration of the mixture before heating, and the same heating temperature, but have different hydraulic modulus (HM). In detail, levels #2, #3, #13, and #14 have different HM by varying the amount of calcium source CA contained in the mixture BC (level #2 has 0 amount).
[0179] The results for levels #2, #3, #13, and #14 shown in Table 11 are shown graphically in FIG.
[0180] FIG. 14 suggests that the K removal rate is improved by increasing the hydraulic ratio (HM) of the mixture BC. From the viewpoint of achieving a K removal rate of 50% or more, it is preferable that the HM is 0.2 or more. On the other hand, if the calcium source CA is added so that the hydraulic ratio exceeds 1.0, the ratio of the calcium source CA to the entire mixture BC increases, and the treatment speed of the target object BT may decrease. This is because there is a limit to the amount of powder that can be added at one time to the combustion furnace in which the heating step (b) is performed. In view of the above, it is preferable to adjust the amount of the calcium source CA and / or the sulfur source S containing Ca so that the hydraulic ratio is within the range of 0.2 to 1.0.
[0181] (Verification 4: Relationship between Cl / K and K removal rate) Table 12 below is an excerpt from Tables 6 to 7. [Table 12]
[0182] Levels #4, #5, #10, and #12 shown in Table 12 are all the same in terms of the mixture's constituent materials, HM, SO3 concentration of the mixture before heating, K concentration, and heating temperature, but the Cl / K is different from one another. In levels #P1 and #P6 shown in Table 12, the constituent materials of the mixture, HM, SO3 concentration of the mixture before heating, K concentration, and heating temperature are all the same, but the Cl / K is different. The Cl / K value was adjusted by mixing different amounts of CaCl2 as a chlorine source (CL).
[0183] The group consisting of levels #4, #5, #10, and #12 and the group consisting of levels #P1 and #P6 have different aspects of mixture BC. In levels #4, #5, #10, and #12, KP water-washing residue SU2B was used as the sulfur source S, and this KP water-washing residue SU2B also served as the calcium source CA, and HM was adjusted to 0.54. On the other hand, in levels #P1 and #P6, no sulfur source S was added, and CaCO3 was added as the calcium source CA, and HM was adjusted to 0.54.
[0184] The results for levels #4, #5, #10, #12, #P1, and #P6 shown in Table 12 are shown graphically in FIG.
[0185] According to Fig. 15, it is suggested that the K removal rate can be improved by increasing the Cl / K value of the mixture BC. However, if the Cl / K is too high, the amount of chlorine source CL added is too much for the target object CT, resulting in a large amount of unreacted Cl, which is inefficient. Therefore, it is preferable to mix the chlorine source CL so that the Cl / K value is 1 to 4.
[0186] In addition, in FIG. 15, comparing level #4, where no chlorine source CL was added, with level #P1, level #4, where KP water washing residue was added as the sulfur source S, has a slightly higher K removal rate. Since the KP water washing residue originally contained water-insoluble Cl-containing and S-containing minerals, it is considered that even without the separate addition of the chlorine source CL, the Cl and S contained in the Cl-containing minerals reacted with the alkali metals contained in the target material BT to generate KCl and K2SO4, which were then removed by volatilization or water washing. On the other hand, the CaCO3 added as the calcium source CA in level #P1 does not contain Cl or S. For this reason, it is considered that the K removal rate in level #4 was slightly improved compared to level #P1.
[0187] (Verification 5: Relationship between the type of target BT and K removal rate) Table 13 below is an excerpt from Tables 6 to 7. [Table 13]
[0188] In levels #21 to #24 and levels #P8 to #P11 shown in Table 13, biomass ash BT2 is used as the target object BT.
[0189] Levels #21 to #24 shown in Table 13 are all the same in terms of the mixture constituent materials, HM, Cl / K, and the SO3 concentration and K concentration of the mixture before heating, but the heating temperatures are different from one another. Levels #P8 to #P11 shown in Table 13 are all the same in terms of the mixture's constituent materials, HM, Cl / K, and the mixture's SO3 concentration and K concentration before heating, but the heating temperatures are different from one another.
[0190] The form of mixture BC is different between standards #21 to #24 and standards #P8 to #P11. In standards #21 to #24, KP water-washing residue SU2A was used as the sulfur source S, and this KP water-washing residue SU2A also served as the calcium source CA. On the other hand, in standards #P8 to #P11, no sulfur source S was added, and CaCO3 was added as the calcium source CA.
[0191] The results for levels #21 to #24 and levels #P8 to #P11 shown in Table 13 are shown in a graph in FIG.
[0192] According to Fig. 16, it can be seen that the levels #21 to #24, in which KP water washing residue was mixed as the sulfur source S, achieved a high K removal rate even in a low-temperature calcination environment, compared to the levels #P8 to #P11, in which no sulfur source S was mixed. As described above, this result is thought to be due to the fact that the mixed sulfur source S functions as a flux, and the target BT, especially the surface area, melts early even at a relatively low temperature, changing into alkali metal chlorides or alkali metal sulfides, which are then removed by volatilization or water washing. In other words, it can be seen that Fig. 16 shows almost the same tendency as Verification 2 (Fig. 13), which compared the levels in which the target BT was decomposed sand BT1.
[0193] For example, according to Table 5, the mixture BC4 used in levels #6 to #11 of Verification 2 and the mixture BC13 used in levels #21 to #24 of this Verification 5 have different SM, IM, etc. ratios. This means that K removal treatment can be performed in the same way for target BT with different ratios, suggesting that the technology can be applied to a wide range of waste. [Explanation of symbols]
[0194] 1: Alkaline metal removal device 2:Storage tank 4: Crushing device 5,6, :Mixing device 7: Heating device 9:Water washing device 11: Supply hopper 13,15: Feeding device 17:Solid-liquid separator 31: Internal combustion burner 33: Intake fan 35: Slurry mixing device 41: Exhaust gas tower 42: Cyclone 43: Piping 44: Processing agent supply section 45: Bag filter BC: mixture BT: Object C1: Cake CA: Calcium source CL: Chlorine source ET: Treatment agent G1: Atmosphere G2: Exhaust gas G3: Exhaust gas Lr1: Slurry P1: Heat-treated material S: Sulfur source W1:Water W2: Cleaning water W3: Drainage Z1: Dust
Claims
1. 1. A method for removing alkali metals from an alkali metal-containing material, comprising the steps of: (a) mixing a sulfur source, a calcium source, and a chlorine source with the alkali metal-containing material, either simultaneously or sequentially; and a step (b) of heating the mixture of the alkali metal-containing material in a state in which the hydraulic ratio has been adjusted by the step (a) to obtain a heat-treated product, 2. The method for removing an alkali metal, wherein the calcium source is the same material as the sulfur source or is a material different from the sulfur source.
2. The step (a) The alkali metal-containing material is mixed with the sulfur source and the calcium source to obtain a hydraulic ratio and a SO 3 A step (a1) of adjusting the concentration; 2. The method for removing an alkali metal according to claim 1, further comprising the step (a2) of mixing the chlorine source with the mixture obtained by carrying out the step (a1).
3. 3. The method for removing an alkali metal according to claim 1, wherein the alkali metal-containing material has a raw material composition containing an alkali metal in a sparingly soluble state.
4. 3. The method for removing alkali metals according to claim 1 or 2, wherein the alkali metal-containing material is at least one selected from the group consisting of fly ash of woody biomass ash, bottom ash of woody biomass ash, construction waste soil, and recycled fine powder of waste concrete.
5. The step (a) is carried out to obtain a mixture having a hydraulic hardness in the range of 0.2 to 1.0, and a SO 3 3. The method for removing an alkali metal according to claim 1, comprising the step of adding the sulfur source and the calcium source in amounts adjusted to give concentrations within a range of 2 to 10 mass%.
6. 3. The method for removing an alkali metal according to claim 1, wherein the sulfur source is at least one selected from the group consisting of gypsum, waste gypsum board, residue of water washing of chlorine bypass dust, classified coarse powder of chlorine bypass dust, sewage sludge, sewage sludge incineration ash, polyiron sulfate, and sulfur-containing combustible organic waste.
7. The calcium source is CaCO 3 and CaO, paper sludge, paper sludge incineration ash, waste concrete fine powder, ready-mixed concrete sludge, chlorine bypass dust water washing residue, chlorine bypass dust classified coarse powder, gypsum, and waste gypsum board.
8. 3. The method for removing an alkali metal according to claim 1, wherein the chlorine source is at least one selected from the group consisting of chlorine-containing combustible waste and inorganic chlorine compounds.
9. 3. The method for removing an alkali metal according to claim 1, wherein the step (a) includes a step of introducing the chlorine source in an amount adjusted so that a Cl / K ratio, which is a ratio of a molar amount of Cl contained in the chlorine source to a molar amount of K (potassium) contained in the alkali metal-containing material, is within a range of 1 to 4.
10. 3. The method for removing an alkali metal according to claim 1, wherein the step (b) is a step of heating at a temperature of 600° C. to 1200° C.
11. 3. The method for removing an alkali metal according to claim 1 or 2, wherein the step (a) includes a step of mixing one or both of the chlorine source and the calcium source recovered from the exhaust gas discharged through the step (b).
12. The step (b) is a step of heating the mixture in a kiln; 3. The method for removing an alkali metal according to claim 1, wherein the step (a) includes a step of feeding sulfur-containing combustible organic waste as the sulfur source from a front side of the kiln.
13. 3. The method for removing an alkali metal according to claim 1, further comprising a step (c) of washing the heat-treated product obtained in the step (b) with water.
14. The method further includes a step (d) of pulverizing the alkali metal-containing material before the step (a), 3. The method for removing an alkali metal according to claim 1, wherein the step (a) is a step of mixing a sulfur source, a calcium source, and a chlorine source with the pulverized alkali metal-containing material.
15. A step (e) of pulverizing the mixture obtained in the step (a), 3. The method for removing an alkali metal according to claim 1, wherein the step (b) is a step of heating the pulverized mixture.
Citation Information
Patent Citations
Detoxification treatment of incineration ash or fly ash
JP1999156327A
Method for treating alkali metal-containing material
JP2022125641A
Method for treating waste material and method for manufacturing raw material of cement
JP2004059754A