Coating composition, coating method and coated body

The coating composition with a specific acrylic resin, silane compound, and controlled solvent content addresses adhesion and rust prevention issues in low-solvent primer paints, ensuring high-quality coatings for metal substrates.

JP2024141943APending Publication Date: 2024-10-10DAI NIPPON TORYO CO LTD

Patent Information

Application Number
JP2023053831
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing primer paints with reduced organic solvent content face challenges in maintaining adhesion to metal substrates and rust prevention properties due to decreased viscosity, which affects the quality of the resulting paint film.

Method used

A coating composition comprising an acrylic resin with a specific acid value, a silane compound with an epoxy group, and a controlled organic solvent content, along with a nitrogen atom-containing monomer, is used to enhance adhesion and rust prevention properties while minimizing solvent use.

Benefits of technology

The composition achieves excellent adhesion to metal substrates and effective rust prevention, even with reduced organic solvent content, suitable for applications like aluminum alloy wheels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141943000001
    Figure 2024141943000001
  • Figure 2024141943000002
    Figure 2024141943000002
  • Figure 2024141943000003
    Figure 2024141943000003
Patent Text Reader

Abstract

To provide a coating composition excellent in adhesion and rust-prevention to a metal base, a coating method using the coating composition, and a coated body with the coating composition applied thereto.SOLUTION: A coating composition includes: a nitrogen atom-containing monomer (a1) as a polymerizable monomer; an acrylic resin (A) with an acid value of 15 mg KOH / g to 50 mg KOH / g, inclusive; a silane compound (B) having an epoxy group; and an organic solvent (C). A content of the nitrogen atom-containing monomer (a1) is 5 mass% or more and less than 30 mass% based on the polymerizable monomer 100 mass%, and a content of the organic solvent (C) is 700 g / L or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating composition, a coating method, and a coated body. [Background technology]

[0002] Wheels for automobiles and motorcycles are mainly made from aluminum alloys. Cast aluminum wheels in particular can be easily processed into complex shapes, allowing for a wide variety of designs and mass production. Cast aluminum wheels are machined and then gloss-treated, after which a clear coat is applied to the surface to protect the base material. The clear coat is generally applied in the following order: a primer clear coat, and then a top clear coat. As a primer coating, for example, Patent Document 1 discloses an acrylic resin coating containing N-butoxymethylacrylamide as a thermosetting resin and transparent fine powdered silica and / or alumina, while Patent Document 2 discloses a primer coating composition containing a copolymer resin, fumed silica, and a phosphoric acid compound containing magnesium to improve corrosion resistance.

[0003] Meanwhile, in recent years, China has been requiring the use of materials that comply with mandatory standards (GB standards) for low-VOC (volatile organic compound) paints, adhesives, etc., and as a result, there is a demand for primer paints with reduced organic solvent content. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP-A-1-194979 [Patent Document 2] International Publication No. 2014 / 181593 Summary of the Invention [Problem to be solved by the invention]

[0005] In order to prepare a paint with a reduced amount of organic solvent, it is necessary to design the viscosity of the resin to be low. However, simply lowering the viscosity of the paint by lowering the molecular weight of the resin tends to reduce the physical properties of the resulting paint film. In particular, for primer paints, the adhesion to metal substrates and the rust prevention properties of the resulting paint film tend to decrease. The present invention has been made in consideration of the above circumstances, and has an object to provide a coating composition having excellent adhesion to metal substrates and rust prevention properties, a coating method using the coating composition, and a coated body coated with the coating composition. [Means for solving the problem]

[0006] The present invention relates to a coating composition comprising an acrylic resin (A) which contains a nitrogen-containing monomer (a1) as a polymerizable monomer and has an acid value of 15 mgKOH / g or more and 50 mgKOH / g or less, a silane compound (B) having an epoxy group, and an organic solvent (C), in which the content of the nitrogen-containing monomer (a1) is 5 mass% or more and less than 30 mass%, relative to 100 mass% of the total polymerizable monomers, and the content of the organic solvent (C) is 700 g / L or less.

[0007] The nitrogen atom-containing monomer (a1) is preferably a compound having a functional group capable of reacting with a hydroxyl group.

[0008] The number average molecular weight of the acrylic resin (A) of the present invention is preferably 4,000 or more and 10,000 or less.

[0009] The coating method of the present invention involves coating a metal substrate that has been machined with the coating composition of the present invention.

[0010] The coated body of the present invention has a coating film made of the coating composition of the present invention on a machined metal substrate.

[0011] The coated body of the present invention may also have a surface protective layer on the coating film. Effect of the Invention

[0012] According to the present invention, it is possible to obtain a coating composition, a coating method, and a coated body that are excellent in adhesion to metal substrates and in rust prevention properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, one embodiment of the present invention will be described.

[0014] [Paint composition] The coating composition of the present invention comprises an acrylic resin (A) which contains a nitrogen-containing monomer (a1) as a polymerizable monomer and has an acid value of 15 mgKOH / g or more and 50 mgKOH / g or less, a silane compound (B) having an epoxy group, and an organic solvent (C), wherein the content of the nitrogen-containing monomer (a1) in the acrylic resin (A) is 5 mass% or more and less than 30 mass%, and the content of the organic solvent (C) is 700 g / L or less. Each component will be described in detail below.

[0015] <Acrylic resin (A)> The acrylic resin (A) contains at least a nitrogen atom-containing monomer (a1) as a polymerizable monomer. The polymerizable monomer constituting the acrylic resin (A) includes, in addition to the nitrogen atom-containing monomer (a1), one or more acrylic components selected from acrylic acid, methacrylic acid, and their esters, amides, and nitriles; and polymerizable unsaturated monomers such as styrene and vinyl group-containing ester compounds (excluding acrylic components).

[0016] (Nitrogen atom-containing monomer (a1)) The nitrogen atom-containing monomer (a1) is preferably a compound having a functional group capable of reacting with a hydroxyl group. The nitrogen atom-containing monomer (a1) may be, for example, (meth)acrylamide or its derivative, more specifically, (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylamide, N,N-diethylaminoethyl (meth)acrylamide, N-methoxymethylacrylamide, N-butoxymethylacrylamide, N-isobutoxymethylacrylamide, N-dimethylaminopropyl (meth)acrylamide, N-methylolacrylamide, etc.

[0017] The content of the nitrogen atom-containing monomer (a1) is 5% by mass or more and less than 30% by mass, based on 100% by mass of all polymerizable monomers. When the content of the nitrogen atom-containing monomer (a1) is 5% by mass or more, adhesion to metal substrates is good. Furthermore, when the content of the nitrogen atom-containing monomer (a1) is less than 30% by mass, high rust prevention properties can be obtained. The content of the nitrogen atom-containing monomer (a1) is more preferably 5% by mass or more and less than 25% by mass, based on 100% by mass of all polymerizable monomers.

[0018] (Acrylic component) Examples of the acrylic component of the polymerizable monomer include the following compounds (a2) to (a6).

[0019] -(meth)acrylic acid and alcohol having 1 to 24 carbon atoms (a2)- Examples of the ester (a2) of (meth)acrylic acid and an alcohol having 1 to 24 carbon atoms include methyl (meth)acrylate, 2-isocyanatoethyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, lauryl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, tridecyl (meth)acrylate, and stearyl (meth)acrylate.

[0020] -Carboxyl group-containing monomer (a3)- Examples of the carboxyl group-containing monomer (a3) ​​include acrylic acid, methacrylic acid, maleic acid, and maleic anhydride.

[0021] -Hydroxyl group-containing monomer (a4)- Examples of the hydroxyl group-containing monomer (a4) include monoesters of (meth)acrylic acid and dihydric alcohols, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate, as well as (meth)acrylates having a polyoxyethylene chain whose molecular terminal is a hydroxyl group.

[0022] -Epoxy group-containing polymerizable unsaturated monomer (a5)- Examples of the epoxy group-containing polymerizable unsaturated monomer (a5) include glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and the like.

[0023] -Aminoalkyl(meth)acrylate (a6)- Examples of the aminoalkyl(meth)acrylate (a6) include N,N-dimethylaminoethyl(meth)acrylate, N,N-diethylaminoethyl(meth)acrylate, and N,N-dimethylaminopropyl(meth)acrylate.

[0024] (Polymerizable unsaturated monomer (a7)) As the polymerizable monomer other than the acrylic component, the following polymerizable unsaturated monomer (a7) can be mentioned. Examples of the polymerizable unsaturated monomer (a7) include vinyl group-containing aromatic compounds such as styrene, α-methylstyrene, and vinyl toluene, and vinyl group-containing compounds such as vinyl acetate.

[0025] <Silane compound having an epoxy group (B)> As the silane compound (B) having an epoxy group, a compound known as an epoxy group-containing silane coupling agent can be used. For example, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltriethoxysilane can be mentioned. The coating composition of the present invention contains the silane compound (B) having an epoxy group, thereby improving the adhesion and rust prevention properties of the coating film formed between the coating film and the metal substrate.

[0026] <Organic solvent (C)> Examples of the organic solvent (C) include xylene, ethylene glycol mono-normal propyl ether, toluene, methyl isobutyl ketone, isopropyl alcohol, butanol, acetone, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, methyl ethyl ketone, ethyl 3-ethoxypropionate, etc. Known commercially available products can be used as these solvents.

[0027] The content of the organic solvent (C) in the coating composition of the present invention is 700 g / L or less. In the coating composition of the present invention, the content of the organic solvent (C) can be further set to 650 g / L or less, more preferably 600 g / L or less. When the content of the organic solvent (C) is 700 g / L or less, spray coating is possible without diluting the coating composition. In the present invention, when a paint composition is provided with an even lower content of organic solvent (C), for example, 430 g / L or less, the concentration of organic solvent (C) can be 700 g / L or less even when diluted to a level that allows spray painting. Therefore, the paint composition of the present invention is an environmentally friendly paint composition. Furthermore, even if the coating composition of the present invention has a low content of organic solvent (C) as described above, the adhesion of the coating to metal substrates and the rust prevention properties of the coating film are not impaired.

[0028] <Other ingredients> The coating composition of the present invention can appropriately use additives necessary for a coating composition. For example, various coating additives that are generally known and commonly used in the art, such as pigments, pigment dispersants, defoamers, antisagging agents, UV absorbers, light stabilizers, and antifungal agents, can be used in conventional amounts. Furthermore, the coating composition of the present invention can also be used in combination with other resins, such as acrylated alkyd resins, alkyd resins, silicone resins, fluororesins, or epoxy resins, as appropriate, for the purpose of improving performance within a range that does not affect the effects of the present invention.

[0029] (Hydroxyl value) The hydroxyl value of the acrylic resin (A) is preferably 10 mgKOH / g or more and 80 mgKOH / g or less. When the hydroxyl value of the acrylic resin (A) is 10 mgKOH / g or more, the crosslinking reaction with the nitrogen atom-containing monomer is easily progressed, and a coating film having a dense crosslinked structure with excellent rust prevention properties can be obtained, and when the hydroxyl value is 80 mgKOH / g or less, the crosslinking reaction with the nitrogen atom-containing monomer reduces the number of unreacted hydroxyl groups, and a coating film with good rust prevention properties can be obtained. The hydroxyl value of acrylic resin (X) is the number of milligrams of potassium hydroxide required to completely acetylate the hydroxyl groups in 1 g of resin with acetic anhydride and then neutralize the free acetic acid generated by acetylation.

[0030] (Acid value) The acid value of the acrylic resin (A) is 15 mgKOH / g or more and 50 mgKOH / g or less. When it is 15 mgKOH / g or more, the crosslinking reaction of the nitrogen atom-containing monomer proceeds easily, and a coating film with good adhesion to the metal substrate can be obtained. When it is 50 mgKOH / g or less, the amount of residual acid groups remaining due to the reaction with the silane compound (B) having an epoxy group is reduced, and a coating film with good rust prevention properties can be obtained. In the present invention, the acid value of the acrylic resin (A) is a value determined in accordance with JIS K 5601-2-1:1999.

[0031] (Number average molecular weight Mn) The number average molecular weight Mn of the acrylic resin (A) is preferably 4000 or more and 10000 or less. When it is 4000 or more, a coating film having good adhesion to a metal substrate can be obtained as a coating film of a high molecular weight substance after a crosslinking reaction, and when it is 10000 or less, an acrylic resin with low viscosity can be obtained, so that the organic solvent content in the coating material can be 700 g / L or less. In this specification, the number average molecular weight Mn of the acrylic resin (A) is measured by the measurement method shown in the examples described later.

[0032] (Weight average molecular weight Mw) The weight average molecular weight Mw of the acrylic resin (A) is preferably 10,000 or more and 40,000 or less. When it is 10,000 or more, a coating film having good adhesion to a metal substrate can be obtained as a coating film of a high molecular weight substance after a crosslinking reaction, and when it is 40,000 or less, an acrylic resin with low viscosity can be obtained, so that the organic solvent content in the coating material can be 700 g / L or less. In this specification, the weight average molecular weight Mw of the acrylic resin (A) is measured by the measurement method shown in the examples described later.

[0033] (glass transition temperature Tg) The glass transition temperature Tg of the acrylic resin (A) is preferably −40° C. or higher and 50° C. or lower. When the glass transition temperature Tg is in this range, adhesion to metal substrates and rust prevention properties tend to be good.

[0034] <Total light transmittance> When the coating composition of the present invention is used as a clear coating, the coating film obtained by coating to a dry film thickness of 25 μm preferably has a total light transmittance of 90% or more.

[0035] [Painting method] The coating method of the present invention involves coating the coating composition of the present invention on a metal substrate that has been machined. Examples of coating methods include dipping, electrostatic coating, spin coating, flow coating, roll coating, spray coating, and blade coating. Air knife coating methods are also included. Among these, spray coating and roll coating are preferred from the viewpoint of easy control of film thickness.

[0036] The reaction of the coating film formed by applying the coating composition is not yet complete when the coating film is formed, and the drying and curing reaction are terminated by baking (heat drying) to cause a curing reaction after the coating film is formed. The baking conditions are preferably 80 to 180°C and 5 to 90 minutes.

[0037] <Machined metal substrate> The "metal substrate" of the cutting-treated metal substrate in the present invention is not particularly limited, but its shape may be, for example, a plate, a sheet, or a foil. Metals constituting the metal substrate include steel, galvanized steel, stainless steel, magnesium alloys, aluminum, and aluminum alloys, among which aluminum alloys are preferred. In particular, the effect of the coating composition of the present invention is more pronounced in aluminum alloy castings, which are widely used for automobile wheels. That is, cutting is performed to give gloss to automobile wheels, and there is a problem that the cutting-treated metal surface is prone to rust, but the coating composition of the present invention has good adhesion and rust prevention properties when applied to a cutting-treated metal substrate. The effect of the coating composition of the present invention is more pronounced when applied to a metal substrate that has been machined, but the effect of the coating composition of the present invention is naturally sufficient even when the metal substrate is not machined.

[0038] Here, the metal substrate may be subjected to various surface treatments, such as oxidation treatment. As an example, a substrate in which aluminum is subjected to oxidation treatment by a method such as anodizing, phosphate treatment, chromate treatment, or non-chromate treatment can be used.

[0039] [Painted body] The coated body of the present invention has a coating film made of the coating composition of the present invention on a machined metal substrate. The coating film can be formed by the coating method of the present invention. The coated body of the present invention is coated with the coating composition of the present invention, and therefore has good adhesion between the metal substrate and the coating film, and also has excellent rust prevention properties. The coated body of the present invention may have a surface protective layer on the coating film.

[0040] [Surface protective layer] A general topcoat paint can be used as the paint for forming the surface protective layer, but it is preferable to use a paint capable of forming a coating film excellent in abrasion resistance, coating film hardness and chemical resistance. The coating film excellent in abrasion resistance may be a coating film having self-repairing properties even if the coating film is scratched. Examples of paints capable of forming a coating film having excellent coating film hardness and chemical resistance include heat-curable paints such as acrylic melamine resin paints and acrylic urethane resin paints, and active energy ray-curable paints. The surface protective layer provided on the coating film of the coating composition of the present invention is preferably formed from an acrylic melamine resin paint or an acrylic urethane resin paint which contains a nitrogen atom-containing resin component, and in particular, an acrylic melamine resin paint is more preferred. A more preferred acrylic melamine resin paint is a paint containing an acrylic resin (X) having a hydroxyl group number per number average molecular weight of 2.0 to 6.0, a crosslinking agent (Y) that reacts with hydroxyl groups, and an organic solvent (Z), the content of the organic solvent (Z) being 600 g / L or less. With such a paint, a paint film excellent in abrasion resistance, film hardness, and chemical resistance can be formed while being a low-VOC (volatile organic compound) paint. In addition, the surface protective layer is preferably a clear paint from the viewpoint of application to highly decorative substrates. In this specification, the clear paint is a paint that forms a transparent coating film, and when the thickness is 30 μm, the transmittance is 80% or more, preferably 90% or more, more preferably 95% or more, and even more preferably 97% or more. In this specification, the transmittance means the total light transmittance in the visible region (360 nm to 750 nm), and can be measured in accordance with JIS K 7375:2008. EXAMPLES

[0041] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the examples shown below.

[0042] [Preparation of acrylic resin solution] [Resin solution P1] A solution containing acrylic resin (A) (resin solution P1) was prepared according to the following procedure. Table 1 shows the monomers and solvents required for preparing the resin solution, as well as the properties of the acrylic resin (A). 30.0 parts by mass of xylene, 35.0 parts by mass of styrene, 45.3 parts by mass of 2-ethyl acrylate, 4.7 parts by mass of methacrylic acid, 10.0 parts by mass of 2-hydroxyethyl methacrylate, 5.0 parts by mass of N-butoxymethylacrylamide, and 1.5 parts by mass of 2-2'-azobis-2-methylbutyronitrile were reacted under nitrogen gas at 100°C for 8 hours, and then diluted with 50.3 parts by mass of xylene to obtain acrylic resin solution P1 with a heating residue of 55% by mass.

[0043] The acrylic resin (A) contained in the acrylic resin solution P1 had a hydroxyl value of 40 mgKOH / g, an acid value of 30 mgKOH / g, a number average molecular weight of 9,500, and a weight average molecular weight of 35,000.

[0044] [Resin solutions P2 to P7] Resin solutions P2 to P7 were prepared in the same manner as resin solution P1, except that the compounds and compositions were changed as shown in Table 1.

[0045] The resin properties of resin solutions P1 to P7 were measured by the methods described below. The measurement results are shown in Table 1.

[0046] (heated residue) 1.0 g of the resin solution was precisely weighed into an aluminum cup and dried for 30 minutes in an oven at 150° C. After drying, the mass of the residue was precisely weighed, and the ratio of the mass of the residue to the original mass was calculated as the heating residue (mass %).

[0047] (Hydroxyl value) After the hydroxyl groups in 1 g of acrylic resin (A) were completely acetylated with acetic anhydride, the amount of potassium hydroxide (mg) required to neutralize the remaining free acetic acid was determined, and this value was taken as the hydroxyl value of acrylic resin (A).

[0048] (Acid value) The acid value of the acrylic resin (A) was determined in accordance with JIS K 5601-2-1:1999.

[0049] (Number average molecular weight Mn) The number average molecular weight Mn of the acrylic resin (A) was measured by SEC (size exclusion chromatography, product name "HLC-8420GPC", manufactured by Tosoh Corporation) equipped with a differential refractive index (RI) detector using a TSKgel column SuperMultiporeHZ-M (manufactured by Tosoh Corporation). The SEC conditions were tetrahydrofuran as the developing solvent, a flow rate of 0.35 ml / min, and a temperature of 40°C. TSK standard polystyrene (manufactured by Tosoh Corporation) was used as the standard substance.

[0050] (Weight average molecular weight Mw) The weight average molecular weight Mw of the acrylic resin (A) was measured by SEC (size exclusion chromatography, product name "HLC-8420GPC", manufactured by Tosoh Corporation) equipped with a differential refractive index (RI) detector using a TSKgel column SuperMultiporeHZ-M (manufactured by Tosoh Corporation). The SEC conditions were tetrahydrofuran as the developing solvent, a flow rate of 0.35 ml / min, and a temperature of 40°C. TSK standard polystyrene (manufactured by Tosoh Corporation) was used as the standard substance.

[0051] [Table 1]

[0052] Next, using the resin solutions P1 to P7, the coating compositions of the examples and comparative examples and the coating films formed by applying and curing the coating compositions were prepared. The components used in the coating compositions and their formulations are shown in Table 2. In Table 2, the amount of each component used is expressed in parts by mass.

[0053] [Example 1] (Preparation of Coating Composition) The coating composition of Example 1 was prepared by mixing 92.6 parts by mass of resin solution P1 as the acrylic resin (A), 2.0 parts by mass of KBM-403 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.) as the silane compound having an epoxy group (B), 4.0 parts by mass of butyl acetate and 30.0 parts by mass of xylene as the organic solvent (C), 1.0 part by mass of a hydroxyphenyltriazine-based ultraviolet absorber (trade name: TINUVIN400, manufactured by BASF) as an ultraviolet absorber, and 1.0 part by mass of a hindered amine-based light stabilizer (trade name: EVERSORB93, manufactured by EVERLIGHT CHEMICAL) as a light stabilizer, followed by stirring with a disperser.

[0054] (Preparation of painted body) The above coating composition was air spray coated onto a substrate made of aluminum, 0.8 mm thick and 150 mm x 70 mm in size, so that the dry film thickness was 25 μm. The coating composition was then dried at 140°C for 20 minutes to produce a coated body.

[0055] (Ford Cup viscosity in seconds when applied) The outflow time of the coating composition during application was measured at 20°C using a Ford cup #4 in accordance with a method in accordance with JIS K5600-2-2:1999.

[0056] [Examples 2 to 4, Comparative Examples 1 to 5] Except for changing the resin solution containing the acrylic resin (A) as shown in Table 2, coating compositions were prepared in the same manner as in Example 1, and coated bodies were produced.

[0057] [evaluation] The coated bodies of the above Examples and Comparative Examples were evaluated as follows. The evaluation results are shown in Table 2.

[0058] (Adhesive) In accordance with the test method of JIS K 5600-5-6:1999, the coated panels were immersed in deionized water at 40°C for 240 hours, then 100 2mm grids were made in the coating using a cutter knife and a cellophane tape peeling test was performed, after which the adhesion was visually judged according to the following criteria. -Judgment criteria- A: No peeling is observed in any of the 100 squares. B: Between 95 and 99 of 100 squares remain C: Peeling is observed in 6 or more of 100 squares.

[0059] (Rust prevention) A CASS test (240 hours) was conducted in accordance with JIS Z 2371:2015, and the rust prevention properties were evaluated according to the following criteria. -Judgment criteria- A: Rust width 0.5mm or less B: Rust width: over 0.5mm and less than 1.0mm C: Rust all over

[0060] [Table 2]

[0061] As shown in Table 2, in Examples 1 to 4, even when the organic solvent content was 700 g / L or less, both the adhesion to the metal member and the rust prevention properties of the coating film were good. On the other hand, Comparative Example 1, which did not contain the silane compound (B) having an epoxy group, was poor in both adhesion and rust prevention properties. Comparative Example 2, in which the resin solution P4 not containing the nitrogen atom-containing monomer (a1) was used, was inferior in adhesion. Comparative Example 3, which used resin solution P5 with a nitrogen atom-containing monomer (a1) content of 30 mass %, was poor in rust prevention properties. Comparative Example 4, which used resin solution P6 containing an acrylic resin (A) with an acid value of 4 mgKOH / g, was inferior in adhesion. Comparative Example 5, which used resin solution P7 containing an acrylic resin (A) with an acid value of 64 mgKOH / g, was inferior in rust prevention properties.

[0062] [Layered coating] Next, the coating compositions used in Examples 1 to 4 above were used as a primer, and a top coat was formed on the painted bodies of Examples 1 to 4 above to which the primer had been applied, to form a laminate coating film, and the laminate coating film was evaluated.

[0063] [Preparation of acrylic resin solution] First, a resin solution containing an acrylic resin to be used as a top coat paint was prepared. Table 3 shows the components required for the preparation of the resin.

[0064] [Resin solution T1] According to the following procedure, a resin solution T1 containing an acrylic resin was prepared. 30.0 parts by mass of xylene, 31.0 parts by mass of styrene, 12.0 parts by mass of 2-ethylhexyl acrylate, 43.0 parts by mass of 2-ethylhexyl methacrylate, 2.0 parts by mass of acrylic acid, 12 parts by mass of 2-hydroxyethyl methacrylate, and 4.0 parts by mass of 2-2'-azobis-2-methylbutyronitrile were reacted under nitrogen gas at 100°C for 8 hours. The mixture was then diluted with 32.7 parts by mass of xylene to obtain a resin solution T1 containing an acrylic resin with a heating residue of 60% by mass.

[0065] The acrylic resin contained in the resin solution T1 had a hydroxyl value of 45 mgKOH / g, an acid value of 11 mgKOH / g, a number average molecular weight of 3,500, and a weight average molecular weight of 6,000.

[0066] [Resin solution T2] Resin solution T2 was prepared in the same manner as resin solution T1, except that the compounds and compositions were changed as shown in Table 3.

[0067] The properties of the acrylic resins of the resulting resin solutions T1 and T2 were evaluated as follows. The evaluation results are shown in Table 3.

[0068] (heated residue) 1.0 g of the resin solution was precisely weighed into an aluminum cup and dried for 30 minutes in an oven at 150° C. After drying, the mass of the residue was precisely weighed, and the ratio of the mass of the residue to the original mass was calculated as the heating residue (mass %).

[0069] (Hydroxyl value) After the hydroxyl groups in 1 g of acrylic resin were completely acetylated with acetic anhydride, the amount of potassium hydroxide required in mg to neutralize the free acetic acid generated by acetylation was determined, and this value was taken as the hydroxyl value of the acrylic resin.

[0070] (Acid value) The acid value of the acrylic resin was determined in accordance with JIS-K-5601-2-1:1999.

[0071] (Number average molecular weight Mn) The weight average molecular weight Mn of the acrylic resin was measured by SEC (size exclusion chromatography, product name "HLC-8420GPC", manufactured by Tosoh Corporation) equipped with a differential refractive index (RI) detector using a TSKgel column SuperMultiporeHZ-M (manufactured by Tosoh Corporation). The SEC conditions were tetrahydrofuran as the developing solvent, a flow rate of 0.35 ml / min, and a temperature of 40°C. TSK standard polystyrene (manufactured by Tosoh Corporation) was used as the standard substance.

[0072] (Weight average molecular weight Mw) The weight average molecular weight Mw of the acrylic resin was measured by SEC (size exclusion chromatography, product name "HLC-8420GPC", manufactured by Tosoh Corporation) equipped with a differential refractive index (RI) detector using a TSKgel column SuperMultiporeHZ-M (manufactured by Tosoh Corporation). The SEC conditions were tetrahydrofuran as the developing solvent, a flow rate of 0.35 ml / min, and a temperature of 40°C. TSK standard polystyrene (manufactured by Tosoh Corporation) was used as the standard substance.

[0073] (Acrylic resin glass transition temperature Tg) The glass transition temperature Tg of the acrylic resin was calculated by the Fox formula.

[0074] (Total number of hydroxyl groups per number average molecular weight Mn of acrylic resin) The total number of hydroxyl groups per number average molecular weight of the acrylic resin was calculated from the measurement results of the number average molecular weight Mn and the hydroxyl value according to the following formula (1). "Total number of hydroxyl groups per number average molecular weight Mn" = Number average molecular weight of acrylic resin × (hydroxyl value of acrylic resin (mgKOH / g) / 56100) (1)

[0075] (Total number of hydroxyl groups per weight average molecular weight Mw of acrylic resin) The total number of hydroxyl groups per weight average molecular weight Mw of the acrylic resin was calculated from the measurement results of the weight average molecular weight Mw and the hydroxyl value according to the following formula (2). "Total number of hydroxyl groups per weight average molecular weight Mw" = Weight average molecular weight of acrylic resin × (hydroxyl value of acrylic resin (mgKOH / g) / 56100) (2)

[0076] [Table 3]

[0077] [Preparation of topcoat paint] Next, the resin solutions T1 and T2 were used to prepare top coats. The composition of each component is shown in Table 4.

[0078] [Preparation of top coat 1] As the acrylic resin, 61.7 parts by mass of resin solution T1; as the crosslinking agent (Y) that reacts with hydroxyl groups, 26.5 parts by mass of melamine resin solution (mixed solution of n-butylated melamine resin in xylene and n-butanol (heating residue 60% by mass), product name: AMIDIR L-117-60, manufactured by DIC Corporation); as the organic solvent (Z), 3.0 parts by mass of propylene glycol monomethyl ether acetate, 1.0 part by mass of butyl acetate, and 2.8 parts by mass of Solvesso 150 (manufactured by JX Nippon Oil & Energy Corporation); as the ultraviolet absorber, 1.0 part by mass of a hydroxyphenyltriazine-based ultraviolet absorber (product name: TINUVIN400, manufactured by BASF Corporation); Top coat 1 was prepared by mixing 1.0 part by mass of the mixture (manufactured by Nippoh Chemical Co., Ltd.) and 3.0 parts by mass of methyl orthoacetate (trade name: MOA, manufactured by Nippoh Chemical Co., Ltd.) as a dehydrating agent, followed by stirring with a disperser.

[0079] [Preparation of top coat 2] Top coat 2 was prepared in the same manner as top coat 1, except that the resin solution containing an acrylic resin was changed to resin solution T2.

[0080] (Ford Cup viscosity in seconds when applied) For top coat 1 and top coat 2 when applied, the outflow time was measured at 20° C. using a Ford cup #4 according to a method in accordance with JIS K5600-2-2:1999.

[0081] [Preparation of topcoat coating (base material: polypropylene)] The above coating composition was spray-painted onto a substrate made of polypropylene, 3.0 mm thick, and 100 mm x 100 mm in size, so that the dry film thickness was 30 μm. The coating composition was then dried at 140°C for 20 minutes to form a coating film, producing a coated body (substrate: polypropylene). This coated body was used to measure the glass transition temperature Tg, the molecular weight between crosslinks, and the crosslink density of the coating film.

[0082] [Measurement of topcoat film properties (glass transition temperature, molecular weight between crosslinks, crosslink density)] (Glass transition temperature Tg of coating film) The coating films of Topcoat 1 and Topcoat 2 were peeled off from the polypropylene resin plate, and then cut to a length of 50 mm and a width of 8 mm to prepare a measurement sample. The dynamic viscoelasticity of the sample was measured using a dynamic viscoelasticity measuring device RSA G2 (manufactured by TA Instruments) at a measurement length of 24 mm, a frequency of 1 Hz, and a heating rate of 5°C / min. The dynamic glass transition temperature measured as the temperature showing the maximum value of tan δ (loss modulus / storage modulus) was taken as the glass transition temperature.

[0083] (Molecular weight between crosslinks, crosslink density of coating film) The molecular weight of the resin between crosslinks is called the inter-crosslink molecular weight, and is expressed as the reciprocal of the crosslink density. The higher the crosslink density, the smaller this value becomes. The intercrosslink molecular weight of the cured coating film of the present invention is a theoretically calculated value obtained by applying the minimum value of the storage modulus obtained during measurement of the glass transition temperature of the cured coating film to the following theoretical formula of rubber viscoelasticity. Formula 1:n=E' / 3RT Where: n:Crosslink density (mol / cc) 1 / n: Molecular weight between crosslinks (cc / mol) R: Gas constant (8.314 J / K / mol) T: Absolute temperature (K) at which the storage modulus is E' E': Minimum storage modulus (Pa)

[0084] [Table 4]

[0085] Next, the primers of Examples 1 to 4 and the above-mentioned top coats 1 and 2 were combined as shown in Table 5 to form a multilayer coating film.

[0086] [Layered coating example 1] The coating composition of Example 1 was applied as a primer to a substrate made of aluminum, 0.8 mm thick, and 150 mm x 70 mm in size by air spray coating to a dry film thickness of 25 μm, and the coating composition was then dried for 20 minutes at 140° C. Thereafter, top coat 2 was applied by air spray coating to a dry film thickness of 30 μm, and the coating was then dried for 20 minutes at 140° C. to produce a laminated coating film.

[0087] [Layered Coating Examples 2 to 8] Laminate Coating Examples 2 to 8 were prepared in the same manner as Laminate Coating Example 1, except that the primer and topcoat were changed as shown in Table 5.

[0088] [Evaluation of multilayer coating] The above laminate coating film examples 1 to 8 were evaluated for adhesion, rust prevention, chemical resistance, coating hardness, and scratch resistance. The adhesion and rust prevention were evaluated in the same manner as the above-mentioned evaluation method. The chemical resistance, coating hardness, and scratch resistance were evaluated by the following evaluation method. The evaluation results are shown in Table 5. Note that the evaluation of adhesion and rust prevention in Table 5 is the same as the evaluation of the coating compositions of Examples 1 to 4, which are described as the evaluation of the primer.

[0089] (Chemical resistance) On the surface of the coating film of the above laminate coating film examples 1 to 8, 1 ml of hydrofluoric acid solution (10% hydrofluoric acid) was dropped, and then the coating film was left in a test tank without forced convection at a temperature of 23°C for 2 hours for chemical treatment. After that, the hydrofluoric acid solution was removed by rinsing with water, and the appearance of the coating film after the chemical treatment was visually evaluated according to the following evaluation criteria. -Evaluation criteria- AA: No change in the appearance of the coating. A: The gloss of the coating film is slightly reduced. C: The gloss of the coating film is significantly reduced.

[0090] (Coating film hardness) The coating hardness of the above-mentioned laminate coating examples 1 to 8 was measured according to "JIS K5600-5-4:1999 Scratch hardness (pencil method)" and evaluated according to the following evaluation criteria. -Evaluation criteria- AA: Pencil hardness HB or higher A: Pencil hardness is 2B or more and B or less C: Pencil hardness is 3B or less

[0091] (Scratch resistance) The scratch resistance of the coating films of the above multilayer coating film examples 1 to 8 was evaluated as follows. Using a friction fastness tester (manufactured by DAIEI KAGAKU SEIKI), a load of 1 kg was applied to the surface of the laminated coating film and the film was moved back and forth 10 times using a white cloth for dye fastness testing conforming to JIS L 0849. After the 10 times of reciprocation, the coating surface was washed with running water and naturally dried, and the gloss of the laminated coating film was visually observed and evaluated according to the following evaluation criteria. -Evaluation criteria- AA: No change in gloss A: Very slightly dull C: Significant loss of gloss

[0092] [Table 5]

[0093] As shown in Table 5, the multilayer coating films of Multilayer Coating Film Examples 1 to 8 were evaluated as being good in terms of adhesion, rust prevention, chemical resistance, coating film hardness, and scratch resistance. [Industrial Applicability]

[0094] The coating composition of the present invention is suitable as a primer coating to be applied to metal substrates, and is particularly suitable as a primer coating for aluminum alloy cast wheels of automobiles.

Claims

1. An acrylic resin (A) containing a nitrogen atom-containing monomer (a1) as a polymerizable monomer and having an acid value of 15 mgKOH / g or more and 50 mgKOH / g or less; A silane compound (B) having an epoxy group, and Contains an organic solvent (C), the content of the nitrogen atom-containing monomer (a1) is 5% by mass or more and less than 30% by mass based on 100% by mass of the total polymerizable monomers; A coating composition having an organic solvent (C) content of 700 g / L or less.

2. 2. The coating composition according to claim 1, wherein the nitrogen atom-containing monomer (a1) is a compound having a functional group capable of reacting with a hydroxyl group.

3. 2. The coating composition according to claim 1, wherein the number average molecular weight of the acrylic resin (A) is 4,000 or more and 10,000 or less.

4. A coating method comprising coating a coating composition according to any one of claims 1 to 3 on a machined metal substrate.

5. A coated body having a coating film made of the coating composition according to any one of claims 1 to 3 on a machined metal substrate.

6. 6. The coated body according to claim 5, further comprising a surface protective layer on said coating film.

Citation Information

Patent Citations

  • Normal temperature curable resin composition, coating composition and its coated article

    JP2003155319A

  • Aluminum wheel primer coat composition

    WO2014181593A1

  • Method of coating aluminum foil

    JP1989194979A

Cited By

  • Water-based paint compositions, coatings, and articles

    JP2026115952A

  • Paint compositions, coatings, and articles

    JP2026115956A