Wallpaper and method for manufacturing the same
By integrating cellulose nanofibers with a number average fiber diameter of 100 nm or less in the adhesive layer, the issues of warping and wrinkling in cellulose-based wallpapers are mitigated, resulting in a more stable and durable product.
Patent Information
- Application Number
- JP2023054237
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional wallpapers made with cellulose-based materials are prone to warping and wrinkling during manufacturing and after installation due to the use of cellulose in the adhesive layer, which is exacerbated by moisture absorption.
Incorporating cellulose nanofibers with a number average fiber diameter of 100 nm or less in the adhesive layer, along with specific fiber length and degree of polymerization, to enhance mechanical strength and dispersibility, thereby reducing warping and wrinkling.
The use of cellulose nanofibers with specified properties in the adhesive layer significantly reduces warping and wrinkling during manufacturing and after installation, ensuring a more stable and durable wallpaper.
Smart Images

Figure 2024142187000001
Abstract
Description
[Technical field]
[0001] The present invention relates to wallpaper and a method for manufacturing wallpaper. [Background technology]
[0002] Conventionally, wallpaper sheets that are reworkable (able to be repositioned) have been known in which a decorative layer, a backing layer, and an adhesive layer having a predetermined adhesive strength are arranged in that order (see, for example, Patent Document 1).
[0003] Furthermore, a self-adhesive laminate that has excellent deodorizing and adsorbent properties and can be attached to wallpaper, flooring, wall materials, and the like is known, which comprises a self-adhesive foam sheet containing metal-containing oxidized cellulose nanofibers that contain metals other than sodium in the form of salts, and a substrate (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2022-54523 [Patent Document 2] JP 2022-101282 A Summary of the Invention [Problem to be solved by the invention]
[0005] Here, in the conventional wallpaper described above, warping or wrinkling may occur during the formation of the adhesive layer or after construction (affixing).
[0006] Therefore, an object of the present invention is to provide wallpaper that is less likely to warp or wrinkle during production or after application. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to achieve the above object, and have newly discovered that warping and wrinkling are likely to occur when a wallpaper substrate containing cellulose is used, and that the inclusion of a specific cellulose nanofiber in the adhesive layer can suppress the occurrence of warping and wrinkling even when a wallpaper substrate containing cellulose is used, thereby completing the present invention.
[0008] That is, the present invention aims to advantageously solve the above problems, and [1] the wallpaper of the present invention comprises a wallpaper substrate and an adhesive layer provided on at least one surface of the wallpaper substrate, the wallpaper substrate containing cellulose, and the adhesive layer containing cellulose nanofibers having a number average fiber diameter of 100 nm or less. In this way, by incorporating cellulose nanofibers having a number average fiber diameter of 100 nm or less into the adhesive layer, it is possible to suppress the occurrence of warping and wrinkles during production and after application, even when a wallpaper substrate containing cellulose is used. In the present invention, the "number average fiber diameter" of the cellulose nanofibers can be determined by measuring the fiber diameters of five or more cellulose nanofibers using an atomic force microscope (e.g., Dimension FastScan AFM (BRUKER, Tapping mode)) and calculating the number average of the measured fiber diameters.
[0009] [2] In the wallpaper according to the above [1], the number average fiber length of the cellulose nanofibers is preferably 50 nm or more and 2000 nm or less. If the number average fiber length of the cellulose nanofibers is 50 nm or more and 2000 nm or less, the occurrence of warping and wrinkling can be further suppressed. In the present invention, the "number average fiber length" of cellulose nanofibers can be determined by measuring the fiber lengths of five or more cellulose nanofibers using an atomic force microscope (e.g., Dimension FastScan AFM (BRUKER, Tapping mode)) and calculating the average of the obtained measured values.
[0010] [3] In the wallpaper according to [1] or [2] above, it is preferable that the average degree of polymerization of the cellulose nanofibers is 100 or more and 2000 or less. If the average degree of polymerization is 100 or more, the adhesive layer can be provided with high mechanical strength. If the average degree of polymerization is 2000 or less, the dispersibility of the cellulose nanofibers in the adhesive layer can be ensured. In the present invention, the "average degree of polymerization" of cellulose nanofibers can be measured, for example, in accordance with Isogai, A., Mutoh, N., Onabe, F., Usuda, M., "Viscosity measurements of cellulose / SO2-amine-dimethylsulfoxide solution", Sen'i Gakkaishi, 45, 299-306 (1989).
[0011] Furthermore, [4] in the wallpaper according to any one of the above [1] to [3], it is preferable that the cellulose nanofibers are carboxylated cellulose nanofibers. Carboxylated cellulose nanofibers have excellent dispersibility and can satisfactorily exhibit the desired performance even when incorporated in a small amount.
[0012] [5] In the wallpaper according to any one of the above [1] to [4], the cellulose nanofibers are metal-containing oxidized cellulose nanofibers that contain a metal in the form of a salt, and the metal is preferably at least one selected from metals in Groups 2 to 14 and Periods 3 to 6 of the Long Periodic Table. By using metal-containing oxidized cellulose nanofibers that contain these metals in the form of a salt, it is possible to impart various properties to the wallpaper, such as deodorizing properties.
[0013] Here, [6] in the wallpaper described in [5] above, the metal is preferably copper, zinc or silver. By using metal-containing oxidized cellulose nanofibers containing copper, zinc or silver in the form of a salt, it is possible to impart excellent deodorizing properties to the wallpaper.
[0014] Furthermore, [7] in the wallpaper according to any one of the above [1] to [6], the adhesive layer is preferably made of a resin foam. Wallpaper having an adhesive layer made of a resin foam has excellent reworkability and leaves little adhesive residue.
[0015] Here, [8] in the wallpaper described in [7] above, it is preferable that the resin foam contains open cells in which a plurality of air bubbles are interconnected. Wallpaper having an adhesive layer made of a resin foam containing open cells can exhibit excellent adhesive strength.
[0016] [9] In the wallpaper according to any one of the above [1] to [8], the wallpaper base material preferably comprises a resin decorative layer and a backing material containing cellulose. By incorporating cellulose nanofibers having a number average fiber diameter of 100 nm or less in the adhesive layer, even when a backing material containing cellulose is used, it is possible to effectively prevent warping and wrinkling during production or after application.
[0017] Here,
[10] in the wallpaper according to the above item [9], the resin decorative layer preferably contains a vinyl chloride resin, because a resin decorative layer containing a vinyl chloride resin has excellent processability.
[0018]
[11] In the wallpaper according to [9] or
[10] above, the backing material preferably contains 50% by mass or more of cellulose. By incorporating cellulose nanofibers having a number average fiber diameter of 100 nm or less in the adhesive layer, even when a backing material containing 50% by mass or more of cellulose is used, it is possible to effectively prevent warping or wrinkling during production or after application.
[0019] The present invention also aims to advantageously solve the above problems, and
[12] the method for producing wallpaper of the present invention is characterized by comprising the steps of preparing a composition for adhesive layer containing cellulose nanofibers having a number average fiber diameter of 100 nm or less, and forming an adhesive layer on a wallpaper substrate containing cellulose using the composition for adhesive layer. By using such a production method, the above-mentioned wallpaper of the present invention can be easily obtained. Effect of the Invention
[0020] According to the present invention, it is possible to provide wallpaper that is less likely to warp or wrinkle during production or after application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] (wallpaper) The wallpaper of the present invention comprises a cellulose-containing wallpaper substrate and an adhesive layer provided on at least one surface of the wallpaper substrate, the adhesive layer containing cellulose nanofibers having a number average fiber diameter of 100 nm or less. The wallpaper of the present invention can be used, without any particular limitation, as wallpaper to be attached to a wall material or wallpaper to be attached over an existing wallpaper that is attached to a wall material or the like. The wallpaper of the present invention may have an optional layer other than the wallpaper substrate and the adhesive layer, and the adhesive layer may be formed directly on the wallpaper substrate, or may be formed on the wallpaper substrate via an optional layer. Specifically, without any particular limitation, the wallpaper of the present invention may have a release paper on the side of the adhesive layer opposite to the wallpaper substrate.
[0022] <Wallpaper base material> Any wallpaper substrate containing cellulose can be used as the wallpaper substrate. The wallpaper substrate may be a substrate having a single layer structure or a substrate having a multilayer structure, but a substrate having a multilayer structure is preferable, and a substrate having a multilayer structure containing a resin decorative layer and a backing material containing cellulose, and optionally further containing an adhesive layer, etc. is more preferable. Wallpapers that have a wallpaper base material containing cellulose are prone to warping and wrinkling due to moisture absorption, etc., but the occurrence of warping and wrinkling can be suppressed by using an adhesive layer that contains cellulose nanofibers with a number average fiber diameter of 100 nm or less.
[0023] The cellulose contained in the wallpaper base material may be modified or chemically modified by a known method.
[0024] [Resin decorative layer] The resin decorative layer is not particularly limited, and a decorative layer containing a resin such as vinyl chloride resin or olefin resin can be used. Among them, it is preferable to use a decorative layer containing a vinyl chloride resin from the viewpoint of excellent processability.
[0025] The decorative resin layer may be subjected to various processes such as embossing, or may be decorated with various designs.
[0026] [Backing material] The backing material is not particularly limited, and any backing material containing cellulose can be used. Specific examples of the backing material include paper such as ordinary paper and flame-retardant paper; woven fabric; and the like.
[0027] The backing material preferably contains 50% by mass or more of cellulose, more preferably 80% by mass or more, and even more preferably consists of cellulose alone. By incorporating cellulose nanofibers having a number average fiber diameter of 100 nm or less into the adhesive layer, even when a backing material containing 50% by mass or more of cellulose is used, it is possible to effectively suppress the occurrence of warping or wrinkling during production or after application.
[0028] <Adhesive layer> The adhesive layer is required to contain cellulose nanofibers having a number average fiber diameter of 100 nm or less. The adhesive layer usually contains a polymer and may further contain optional additives. From the viewpoint of improving reworkability and suppressing residual glue, the adhesive layer is preferably made of a resin foam, and from the viewpoint of further improving adhesive strength, it is more preferable for the adhesive layer to be made of a resin foam containing open cells in which a plurality of bubbles are interconnected.
[0029] [Cellulose nanofiber] The cellulose nanofiber used in the adhesive layer is a component that suppresses the occurrence of warping and wrinkling in the wallpaper of the present invention. In addition, the cellulose nanofiber can impart strength to the resulting adhesive layer. Therefore, the adhesive layer can be made low-densified while maintaining its strength.
[0030] The number average fiber diameter of the cellulose nanofiber must be 100 nm or less, preferably 50 nm or less, more preferably 30 nm or less, and even more preferably 10 nm or less. By using cellulose nanofibers with a number average fiber diameter of the above upper limit or less, wallpaper that is less likely to warp or wrinkle during production or after application can be obtained. The number average fiber diameter of the cellulose nanofiber is usually 1 nm or more.
[0031] Here, the reason why the inclusion of cellulose nanofibers with a number average fiber diameter of 100 nm or less in the adhesive layer can suppress the occurrence of warping and wrinkling of wallpaper is not clear, but it is presumed to be as follows. That is, cellulose nanofibers with a number average fiber diameter of 100 nm or less have excellent dispersibility and can be dispersed in the adhesive layer to improve the strength of the adhesive layer, thereby suppressing the occurrence of warping and wrinkling. In addition, since they can absorb moisture in the same way as wallpaper substrates containing cellulose, the occurrence of warping due to differences in the degree of moisture absorption can be suppressed.
[0032] In addition, the number average fiber length of the cellulose nanofiber is preferably 50 nm or more, more preferably 70 nm or more, even more preferably 100 nm or more, particularly preferably 400 nm or more, preferably 2000 nm or less, more preferably 1500 nm or less, even more preferably 1000 nm or less, and particularly preferably 600 nm or less. If the number average fiber length is 50 nm or more, the adhesive layer can be given a sufficiently high mechanical strength. If the number average fiber length is 2000 nm or less, the dispersibility of the cellulose nanofiber can be ensured and the formability of the adhesive layer can be improved. Therefore, if cellulose nanofibers having a number average fiber length within the above range are used, the occurrence of warping and wrinkles in the wallpaper can be further suppressed.
[0033] The number average fiber length of cellulose nanofibers can be adjusted, for example, by changing the number average fiber length of the natural cellulose used as the raw material, the processing conditions, and the conditions for dispersing (defibrating) the cellulose nanofibers after processing. Specifically, the number average fiber length can be shortened by extending the time of the dispersion process (defibration process).
[0034] Furthermore, the cellulose nanofibers preferably have an average degree of polymerization (the average number of glucose units contained in a cellulose molecule) of 100 or more, more preferably 300 or more, even more preferably 500 or more, and preferably 2000 or less, more preferably 1500 or less, even more preferably 1000 or less, and particularly preferably 700 or less. If the average degree of polymerization is 100 or more, the adhesive layer can be given sufficiently high mechanical strength. Furthermore, if the average degree of polymerization is 2000 or less, the dispersibility of the cellulose nanofibers can be ensured. Therefore, by using cellulose nanofibers having an average degree of polymerization within the above range, the occurrence of warping and wrinkling of the wallpaper can be further suppressed.
[0035] The average degree of polymerization of cellulose nanofibers can be adjusted by changing the average degree of polymerization of the natural cellulose used as the raw material, the processing conditions, and the conditions for dispersing (defibrating) the cellulose nanofibers after processing.
[0036] The cellulose nanofibers may be cellulose nanofibers that have not been subjected to chemical treatments such as oxidation or modification, but are preferably oxidized cellulose nanofibers that have been subjected to oxidation, and are more preferably carboxylated cellulose nanofibers. Oxidized cellulose nanofibers such as carboxylated cellulose nanofibers have excellent dispersibility, and can exhibit the desired performance even when used in small amounts.
[0037] Here, the carboxylated cellulose nanofibers are those in which the primary hydroxyl groups at the 6-positions of the β-glucose units of the raw cellulose have been oxidized to carboxy groups via aldehyde groups. From the viewpoint of imparting the carboxylated cellulose nanofibers with sufficient desired properties, it is preferred that the primary hydroxyl groups in the carboxylated cellulose nanofibers are oxidized to carboxy groups by preferably 50 mol % or more, more preferably 70 mol % or more, and even more preferably 90 mol % or more.
[0038] The amount of carboxy groups in carboxylated cellulose nanofibers can be measured according to the method described in JP 2016-141777 A or JP 2019-199622 A.
[0039] Furthermore, the cellulose nanofiber is preferably a metal-containing oxidized cellulose nanofiber containing a metal in the form of a salt, and more preferably a metal-containing carboxylated cellulose nanofiber containing a metal in the form of a salt. By using a metal-containing oxidized cellulose nanofiber containing a metal in the form of a salt, various properties such as deodorizing properties can be imparted to the wallpaper.
[0040] Here, the metal contained in the metal-containing oxidized cellulose nanofibers can be a metal depending on the properties to be imparted to the metal-containing oxidized cellulose nanofibers. The metal can be, for example, at least one metal selected from metals in groups 2 to 14 and periods 3 to 6 of the long periodic table; more preferably at least one metal selected from the group consisting of magnesium, aluminum, calcium, titanium, chromium, manganese, iron, cobalt, nickel, copper, zinc, silver, tin, barium, and lead; even more preferably at least one metal selected from the group consisting of aluminum, calcium, iron, cobalt, copper, zinc, and silver; and particularly preferably at least one metal selected from the group consisting of silver, zinc, and copper. Metal-containing oxidized cellulose nanofibers containing copper and silver (copper-containing oxidized cellulose nanofibers, silver-containing oxidized cellulose nanofibers) are particularly excellent in deodorizing the odor of sulfur-based malodorous gases such as hydrogen sulfide and methyl mercaptan.
[0041] The amount of metal in the metal-containing oxidized cellulose nanofibers is not limited as long as the desired properties can be imparted to the resulting foamed sheet. For example, in the metal-containing carboxylated cellulose nanofibers, the metal is preferably present in a ratio of 1 / 3 or more, more preferably 1 / 2 or more, of the molar amount of carboxy groups in the carboxylated cellulose nanofibers. The higher the metal content in the metal-containing oxidized cellulose nanofibers, the higher the level of various properties such as deodorizing properties that can be imparted to the wallpaper. The metals in the metal-containing cellulose nanofibers can be qualitatively and quantitatively analyzed by ICP-AES, for example, according to the method described in JP-A-2016-141777 or JP-A-2019-199622.
[0042] The above-mentioned cellulose nanofibers can be obtained, for example, by mechanically defibrating bleached kraft pulp. In addition, oxidized cellulose nanofibers can be produced, for example, according to the methods described in JP 2016-141777 A and JP 2019-199622 A. The cellulose nanofibers produced as described above are usually obtained as a dispersion in a dispersion medium such as water. When using solid cellulose nanofibers, the dispersion can be dried by known means.
[0043] [Polymer] The polymer used in the adhesive layer forms a resin matrix in the adhesive layer.
[0044] The polymer may be any polymer, and may include, but is not limited to, at least one monomer unit selected from the group consisting of (meth)acrylate monomer units, unsaturated carboxylic acid monomer units, vinyl cyanide monomer units, and alkenyl aromatic monomer units. The polymer preferably contains a (meth)acrylate monomer unit, because this provides flexibility to the resulting adhesive layer, enabling the adhesive layer to exhibit good adhesive power (self-adhesive power). In addition, the polymer may contain monomer units other than (meth)acrylate monomer units, unsaturated carboxylic acid monomer units, vinyl cyanide monomer units, and alkenyl aromatic monomer units (hereinafter referred to as "other monomer units").
[0045] <<(Meth)acrylate monomer unit>> The (meth)acrylate monomer unit is a repeating unit derived from a (meth)acrylate monomer. The (meth)acrylate monomer is not particularly limited, but examples thereof include (meth)acrylic acid alkyl ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, n-heptyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and n-dodecyl (meth)acrylate; (meth)acrylic acid alkoxy alkyl ester monomers such as 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, and ethoxymethyl (meth)acrylate; and the like. The (meth)acrylate monomers may be used alone or in combination of two or more. In the present invention, "(meth)acrylic" means acrylic and / or methacrylic.
[0046] Here, as the (meth)acrylate monomer, from the viewpoint of further increasing the flexibility of the adhesive layer and further ensuring the self-adhesive strength of the wallpaper, a (meth)acrylic acid alkyl ester monomer is preferred, and a (meth)acrylic acid alkyl ester monomer in which the carbon number of the alkyl group bonded to a non-carbonyl oxygen atom is 1 to 14 (hereinafter sometimes abbreviated as "C1-14 (meth)acrylic acid alkyl ester monomer") is more preferred.
[0047] Examples of C1-14 (meth)acrylic acid alkyl ester monomers include methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, sec-butyl acrylate, n-heptyl acrylate, n-hexyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, n-octyl methacrylate, and n-dodecyl methacrylate. Among these, n-butyl acrylate, ethyl acrylate, and 2-ethylhexyl acrylate are preferred from the viewpoints of self-adhesiveness and cost.
[0048] The proportion of (meth)acrylate monomer units in the polymer is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, particularly preferably 85% by mass or more, and preferably 99% by mass or less, more preferably 95% by mass or less, and even more preferably 92% by mass or less, based on 100% by mass of all repeating units (total monomer units) contained in the polymer. If the proportion of (meth)acrylate monomer units in the polymer is 60% by mass or more, the self-adhesive strength of the wallpaper can be sufficiently ensured. On the other hand, if the proportion of (meth)acrylate monomer units in the polymer is 99% by mass or less, the self-adhesive strength of the wallpaper will not be excessively increased. Therefore, the resin residue on the substrate of the wallpaper can be suppressed.
[0049] <<Unsaturated carboxylic acid monomer unit>> The unsaturated carboxylic acid monomer unit is a repeating unit derived from an unsaturated carboxylic acid monomer. Specific examples of the unsaturated carboxylic acid monomer include α,β-ethylenically unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid; α,β-ethylenically unsaturated polycarboxylic acids such as itaconic acid, maleic acid, and fumaric acid; and α,β-ethylenically unsaturated polycarboxylic acid partial esters such as monomethyl itaconate, monobutyl maleate, and monopropyl fumarate. In addition, those having a group that can be derived into a carboxylic acid group by hydrolysis, such as maleic anhydride and itaconic anhydride, can also be used. Among these, itaconic acid, acrylic acid, and methacrylic acid are preferred, and acrylic acid is more preferred, from the viewpoints of reactivity with the crosslinking agent described below, stability of the polymer latex, and cost. The unsaturated carboxylic acid monomers may be used alone or in combination of two or more kinds.
[0050] The proportion of the unsaturated carboxylic acid monomer units in the polymer is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, more preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 2.5% by mass or less, based on the total repeating units (total monomer units) contained in the polymer being 100% by mass. By having the proportion of the unsaturated carboxylic acid monomer units in the polymer be 0.1% by mass or more, the crosslinking reaction by the crosslinking agent described below can be sufficiently promoted. As a result, the adhesive layer can be given sufficient strength while suppressing the resin residue on the adherend of the wallpaper. On the other hand, by having the proportion of the unsaturated carboxylic acid monomer units in the polymer be 10% by mass or less, it becomes easy to keep the viscosity of the polymerization system during polymerization within an appropriate range, and the crosslinking of the polymer does not proceed excessively, thereby preventing the self-adhesive force of the adhesive layer from being impaired.
[0051] <<Vinyl cyanide monomer unit>> The vinyl cyanide monomer unit is a repeating unit derived from a vinyl cyanide monomer. A specific example of the vinyl cyanide monomer is an α,β-ethylenically unsaturated nitrile monomer. The α,β-ethylenically unsaturated nitrile monomer is not particularly limited as long as it is an α,β-ethylenically unsaturated compound having a nitrile group, and examples thereof include acrylonitrile; α-halogenoacrylonitrile such as α-chloroacrylonitrile and α-bromoacrylonitrile; α-alkylacrylonitrile such as methacrylonitrile and α-ethylacrylonitrile; and the like. Among these, acrylonitrile is preferred from the viewpoint of increasing the breaking strength of the adhesive layer. The vinyl cyanide monomers may be used alone or in combination of two or more.
[0052] The proportion of the vinyl cyanide monomer unit in the polymer is preferably 1% by mass or more, more preferably 3% by mass or more, even more preferably 5% by mass or more, preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, based on 100% by mass of all repeating units (all monomer units) contained in the polymer. If the proportion of the vinyl cyanide monomer unit in the polymer is 1% by mass or more, the resulting adhesive layer can be given sufficient strength while suppressing the resin residue on the adherend of the wallpaper. On the other hand, if the proportion of the vinyl cyanide monomer unit in the polymer is 30% by mass or less, the flexibility of the resulting adhesive layer can be sufficiently ensured, and wallpaper with good self-adhesive strength can be obtained.
[0053] <<Alkenyl aromatic monomer unit>> An alkenyl aromatic monomer unit is a repeat unit derived from an alkenyl aromatic monomer. Specific examples of alkenyl aromatic monomers include styrene, α-methylstyrene, α-chlorostyrene, vinyltoluene, etc. Among these, styrene is preferred from the viewpoints of polymerizability and cost. The alkenyl aromatic monomers may be used alone or in combination of two or more kinds.
[0054] The proportion of the alkenyl aromatic monomer unit in the polymer is preferably 0.5% by mass or more, more preferably 1% by mass or more, even more preferably 1.5% by mass or more, preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on the total repeating units (total monomer units) contained in the polymer being 100% by mass. If the proportion of the alkenyl aromatic monomer unit in the polymer is 0.5% by mass or more, the hydrophobicity of the alkenyl aromatic monomer unit can prevent water from penetrating into the adhesive layer, and the water resistance of the wallpaper can be improved. On the other hand, if the proportion of the alkenyl aromatic monomer unit in the polymer is 20% by mass or less, the flexibility of the adhesive layer obtained can be sufficiently ensured, and wallpaper with good self-adhesive strength can be obtained.
[0055] <<Other monomer units>> The other monomer units are repeating units derived from other monomers copolymerizable with the above-mentioned monomers. Examples of the other monomers include conjugated diene monomers, α,β-ethylenically unsaturated polyvalent carboxylic acid complete ester monomers, vinyl cyanide monomers, carboxylic acid unsaturated alcohol ester monomers, olefin monomers, crosslinkable monomers, etc. These monomers may be used alone or in combination of two or more.
[0056] Specific examples of the conjugated diene monomer include butadiene, isoprene, 1,3-pentadiene, and cyclopentadiene.
[0057] Specific examples of the α,β-ethylenically unsaturated polyvalent carboxylic acid complete ester monomer include dimethyl fumarate, diethyl fumarate, dimethyl maleate, diethyl maleate, and dimethyl itaconate.
[0058] Specific examples of the vinyl cyanide monomer include acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, and α-ethylacrylonitrile.
[0059] Specific examples of the carboxylic acid unsaturated alcohol ester monomer include vinyl acetate.
[0060] Specific examples of the olefin monomer include ethylene, propylene, butene, and pentene.
[0061] The crosslinkable monomer is a monomer capable of efficiently crosslinking the inside of a polymer molecule and / or between polymer molecules. The crosslinkable monomer is not particularly limited as long as it can crosslink a polymer, and examples of the crosslinkable monomer include a polyfunctional monomer having a plurality of polymerizable unsaturated bonds (excluding the above-mentioned conjugated diene monomer) and a monomer having a crosslinkable functional group. When using a crosslinkable monomer, the proportion of the crosslinkable monomer unit in the polymer is preferably 0.1% by mass or more and 10% by mass or less, with the total repeating units (total monomer units) contained in the polymer being 100% by mass. If the proportion of the crosslinkable monomer unit in the polymer is within the above range, it becomes easy to keep the viscosity of the polymerization system during polymerization within an appropriate range, and it becomes easy to prevent the crosslinking of the polymer from proceeding excessively, which would impair the adsorption of the adhesive layer.
[0062] As the polyfunctional monomer, for example, a bifunctional monomer such as divinylbenzene, ethylene diacrylate, ethylene dimethacrylate, allyl methacrylate, etc.; a trifunctional monomer such as trimethylolpropane trimethacrylate, etc. can be used. The polyfunctional monomer preferably has an unsaturated bond at the end. The polyfunctional monomer may be used alone or in combination of two or more kinds.
[0063] Examples of the monomer having a crosslinkable functional group include monomers having a functional group such as an organic acid group other than a carboxy group, a hydroxyl group, an amino group, an amide group, a mercapto group, and an epoxy group.
[0064] The monomer having an organic acid group is not particularly limited, but a representative example thereof is a monomer having an organic acid group such as a sulfonic acid group. In addition, a monomer having a sulfenic acid group, a sulfinic acid group, a phosphoric acid group, or the like can also be used.
[0065] Specific examples of the monomer having a sulfonic acid group include α,β-unsaturated sulfonic acids such as allylsulfonic acid, methallylsulfonic acid, vinylsulfonic acid, and acrylamido-2-methylpropanesulfonic acid, and salts thereof.
[0066] When using the monomer having an organic acid group, the content of the monomer unit derived from the monomer having an organic acid group in the polymer is preferably 0.1% by mass or more and 10% by mass or less, more preferably 0.5% by mass or more and 5% by mass or less. When the content of the monomer unit derived from the monomer having an organic acid group in the polymer is within the above range, it becomes easy to keep the viscosity of the polymerization system during polymerization within an appropriate range, and it becomes easy to prevent the crosslinking of the polymer from proceeding excessively, which impairs the adsorption of the adhesive layer.
[0067] Incidentally, it is simple and preferable to introduce the monomer unit having an organic acid group into the polymer by polymerization of a monomer having an organic acid group, but the organic acid group may be introduced by a known polymer reaction after the polymer is produced.
[0068] When using a monomer having a functional group other than an organic acid group (hydroxyl group, amino group, amide group, epoxy group), the content of the monomer unit derived from the monomer having a functional group other than an organic acid group in the polymer is preferably 10% by mass or less. If the content of the monomer unit derived from the monomer having a functional group other than an organic acid group in the polymer is 10% by mass or less, it is easy to keep the viscosity of the polymerization system during polymerization within an appropriate range, and it is easy to prevent the crosslinking of the polymer from proceeding excessively, which impairs the adsorption of the adhesive layer.
[0069] In order to sufficiently suppress the generation of formaldehyde when the polymer is optionally foamed and cured to form an adhesive layer, it is preferable that the polymer does not have an N-methylol group. More specifically, it is preferable that the polymer does not contain a monomer unit having an N-methylol group. Here, examples of the monomer having an N-methylol group include N-methylol acrylamide and N-methylol methacrylamide.
[0070] <<Polymer properties>> The glass transition temperature of the polymer is preferably -10°C or lower, more preferably -13°C or lower, even more preferably -17°C or lower, and particularly preferably -20°C or lower. If the glass transition temperature of the polymer is -10°C or lower, the wallpaper can be well adhered to the adherend while the self-adhesive strength of the adhesive layer is sufficiently ensured. This makes it possible to prevent moisture from penetrating between the adherend and the adhesive layer, or between the adherend and the wallpaper. This makes it possible to increase the water resistance of the wallpaper. The lower limit of the glass transition temperature of the polymer is not particularly limited, but is preferably −40° C. or higher from the viewpoint of sufficiently suppressing adhesive residue on the substrate of the wallpaper. The glass transition temperature of the polymer can be obtained, for example, by measuring the glass transition temperature of a film obtained by drying a polymer latex containing the polymer using a differential scanning calorimeter in accordance with JIS K 7121. As the differential scanning calorimeter, for example, DSC7000X (manufactured by Hitachi High-Tech Science Corporation) can be used.
[0071] The gel fraction of the polymer is preferably 95% by mass or less, more preferably 93% by mass or less. If the gel fraction is 95% by mass or less, an adhesive layer having appropriate self-adhesive strength and excellent smoothness can be prepared. The lower limit of the gel fraction of the polymer is not particularly limited, but can be, for example, 50% by mass or more, and can be 70% by mass or more. The gel fraction of the polymer can be measured, for example, by the following method. First, the polymer is applied onto a 50 μm-thick polyethylene terephthalate (PET) film with a 250 μm applicator, and dried at room temperature for 24 hours to obtain a resin film. A predetermined amount (X) (about 500 mg) of this film is precisely weighed as a sample, and this is immersed in 100 ml of ethyl acetate at room temperature for 3 days, and then the insoluble matter is filtered through a 200-mesh wire net, air-dried at room temperature for 15 hours, then dried at 100° C. for 2 hours, cooled at room temperature, and the weight (Y) of the sample is measured. Then, the gel fraction is calculated by substituting X and Y into the following formula. Gel fraction (%) = (Y) / (X) x 100
[0072] <<Polymer Preparation Method>> The polymerization method for obtaining the polymer is not particularly limited, and may be any of solution polymerization, emulsion polymerization, suspension polymerization, bulk polymerization, etc., or other methods. There is no particular limit to the type or amount of the polymerization initiator, emulsifier, dispersant, etc. used in the polymerization. There is no particular limit to the method of adding the monomer, polymerization initiator, emulsifier, dispersant, etc. during the polymerization. There is also no particular limit to the polymerization temperature, pressure, stirring conditions, etc. Although the polymer can be used in a solid state, it is preferable to use the polymer in the form of a latex containing the polymer (polymer latex), such as a latex obtained by emulsion polymerization or a latex obtained by post-emulsification of a polymer. Here, the solids concentration of the polymer latex is preferably 40% by mass or more, more preferably 45% by mass or more, even more preferably 50% by mass or more, particularly preferably 52% by mass or more, from the viewpoint of maintaining the density of the obtained adhesive layer, and is preferably 70% by mass or less, and more preferably 58% by mass or less.
[0073] The content of cellulose nanofibers in the adhesive layer is preferably 0.1 parts by mass or more, and more preferably 0.5 parts by mass or more, relative to 100 parts by mass of the above-mentioned polymer, and is preferably 5 parts by mass or less, and more preferably 1 part by mass or less.
[0074] [Additives] The adhesive layer may contain various additives to improve the processability in the adhesive layer forming step and to improve the performance of the adhesive layer. Examples of such additives include crosslinkers, foam stabilizers such as higher fatty acid salts and surfactants, foaming assistants, thickeners, fillers, preservatives, fungicides, gelling agents, flame retardants, anti-aging agents, antioxidants, pigments, dyes, tackifiers, conductive compounds, water-resistant agents, and oil-resistant agents. Specific examples of the other additives mentioned above are not particularly limited, and known additives, such as those described in International Publication No. 2016 / 147679, can be used.
[0075] <<Crosslinking agent>> The crosslinking agent optionally contained in the adhesive layer is not particularly limited as long as it can form a crosslinked structure with the above-mentioned polymer (particularly the unsaturated carboxylic acid monomer unit of the above-mentioned polymer) in the adhesive layer. Examples of such crosslinking agents include carbodiimide-based crosslinking agents; epoxy-based crosslinking agents; oxazoline-based crosslinking agents; polyfunctional isocyanate-based crosslinking agents such as tolylene diisocyanate, trimethylolpropane tolylene diisocyanate, and diphenylmethane triisocyanate; metal salt-based crosslinking agents; metal chelate-based crosslinking agents; and peroxide-based crosslinking agents. Among them, epoxy-based crosslinking agents are preferably used, and compounds having two or more epoxy groups in one molecule are more preferably used. As the epoxy-based crosslinking agent, fatty acid polyglycidyl ether, glycerol polyglycidyl ether, and ethylene glycol diglycidyl ether are preferred.
[0076] Here, the epoxy-based crosslinking agent may be synthesized by a known method, or a commercially available product may be used. An example of a commercially available epoxy-based crosslinking agent is "Rikabond (registered trademark)" manufactured by Japan Coating Resin Co., Ltd. The epoxy-based crosslinking agent forms a crosslinked structure within or between the polymer molecules by reacting the epoxy group contained therein with a functional group in the polymer (for example, a carboxylic acid group derived from an unsaturated carboxylic acid monomer unit). By using an epoxy-based crosslinking agent, an adhesive layer having a moderate self-adhesive strength and excellent strength can be formed. Therefore, by using an adhesive layer containing an epoxy-based crosslinking agent as a crosslinking agent, the resin residue on the adherend of the wallpaper can be suppressed.
[0077] In the present invention, it is preferable not to use a crosslinking agent that generates formaldehyde, such as a melamine-formaldehyde resin, a urea-formaldehyde resin, or a phenol-formaldehyde resin.
[0078] Here, the blending amount of the crosslinking agent is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, even more preferably 3 parts by mass or more, preferably 20 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of the above-mentioned polymer. By blending the amount of the crosslinking agent within the above-mentioned range, it is possible to obtain an adhesive layer that maintains appropriate strength and elasticity. Therefore, it is possible to ensure the self-adhesive strength of the adhesive layer and to sufficiently suppress the resin residue on the wallpaper adherend.
[0079] <<Foam stabilizer>> As the foam stabilizer, fatty acid ammonium such as ammonium stearate; sulfonic acid type anionic surfactants such as alkyl sulfosuccinate; quaternary alkyl ammonium chloride; alkyl betaine amphoteric compounds; and fatty acid alkanolamines can be used.
[0080] <<Thickener>> As the thickener, acrylic polymers such as sodium polyacrylate; inorganic compound microparticles such as fine silica; and reactive inorganic compounds such as magnesium oxide can be used.
[0081] [Properties of adhesive layer] Here, the adhesive layer may be a foam or a non-foam, but from the viewpoints of smoothness of the adhesive layer, as well as improving reworkability and suppressing adhesive residue, it is preferable for it to be a foam, and it is more preferable for it to be made of a resin foam.
[0082] When the adhesive layer is made of a foam such as a resin foam, the adhesive layer preferably contains open cells formed by a plurality of air bubbles communicating with each other. If the adhesive layer contains such open cells, the air trapped between the adhesive layer and the adherend can be easily removed to the outside of the adhesive layer through the open cells, so that the air escape property of the adhesive layer is further improved, and the adhesive layer can be attached neatly and easily to the adherend. From the viewpoint of further improving the air escape property, the open cells in the adhesive layer preferably contain open cells extending in the planar direction of the adhesive layer. The presence of open cells in the adhesive layer can usually be confirmed by observing a cross section of the adhesive layer using, for example, a laser microscope, a digital microscope, a scanning electron microscope or the like.
[0083] In addition, when the adhesive layer is made of a foam such as a resin foam, the density of the adhesive layer is not particularly limited, but is preferably 0.3 g / cm 3 It is preferable that the content is 0.4 g / cm or more. 3 More preferably, it is 0.7 g / cm or more. 3 It is preferable that the concentration is 0.6 g / cm or less. 3 It is more preferable that the density of the adhesive layer is 0.3 g / cm or less. 3 If the density of the adhesive layer is 0.7 g / cm or more, the strength of the adhesive layer can be ensured. 3 If it is equal to or less than this, the air escape property (the ability to easily remove air pockets remaining between the adhesive layer and the adherend) can be sufficiently improved.
[0084] The thickness of the adhesive layer is preferably 30 μm or more, more preferably 50 μm or more, and even more preferably 100 μm or more, and is preferably 3 mm or less, more preferably 1 mm or less, even more preferably 500 μm or less, and particularly preferably 400 μm or less. If the thickness of the adhesive layer is 30 μm or more, the mechanical strength of the adhesive layer can be sufficiently ensured. On the other hand, if the thickness of the adhesive layer is 3 mm or less, a wallpaper with excellent repetitive attachment (rework performance) can be obtained.
[0085] The properties of the adhesive layer (density, thickness, presence or absence of open cells, hardness, etc.) can be adjusted by, for example, changing the bubble mixing ratio, composition, production conditions, etc.
[0086] (Wallpaper manufacturing method) The method for producing wallpaper of the present invention can be used when producing the above-mentioned wallpaper of the present invention, and includes a step of preparing a composition for an adhesive layer containing cellulose nanofibers having a number average fiber diameter of 100 nm or less (preparation step), and a step of forming an adhesive layer on a wallpaper substrate containing cellulose using the composition for an adhesive layer (layer formation step), and may optionally further include other steps such as a step of forming a layer other than the adhesive layer or a step of laminating a release paper to the adhesive layer.
[0087] <Preparation process> In the preparation step, a composition for an adhesive layer to be used for forming the adhesive layer is prepared.
[0088] [Adhesive layer composition] Here, the composition for the adhesive layer typically contains a polymer and cellulose nanofibers having a number average fiber diameter of 100 nm or less, and optionally further contains a solvent and other additives. The polymer, cellulose nanofibers and additives that can be contained in the composition for adhesive layer are the same as those described above in relation to the wallpaper of the present invention, and therefore a description thereof will be omitted here.
[0089] The solvent is not particularly limited, but water is preferred. When water is used as the solvent, the water contained in the adhesive layer composition can be, for example, water derived from the polymer latex, and / or water derived from the aqueous dispersion of cellulose nanofibers, and / or water derived from other additives.
[0090] When the adhesive layer composition contains a solvent, the viscosity of the adhesive layer composition is preferably 800 mPa·s to 10,000 mPa·s, more preferably 900 mPa·s to 8,000 mPa·s, and even more preferably 1,000 mPa·s to 7,500 mPa·s. If the adhesive layer composition has a viscosity of 1,000 mPa·s or more, it is possible to prevent dripping during the formation of an adhesive layer using the adhesive layer composition, which makes it difficult to control the thickness. On the other hand, if the adhesive layer composition has a viscosity of 10,000 mPa·s or less, it is easy to form an adhesive layer. The viscosity of the adhesive layer composition can be measured at a temperature of 23° C. using a Brookfield viscometer (manufactured by RION Corporation, “VISCOTESTER VT-06”).
[0091] The pH of the adhesive layer composition is preferably 5 or more, more preferably 7 or more, and even more preferably 8 or more, and is preferably 10 or less, more preferably 9.7 or less, and even more preferably 9.5 or less. If the pH of the adhesive layer composition is 5 or more, precipitation and aggregation of cellulose nanofibers can be effectively prevented. On the other hand, if the pH of the adhesive layer composition is 10 or less, when a crosslinking agent is used, a decrease in the strength of the adhesive layer caused by the crosslinking reaction not proceeding easily can be effectively prevented. The pH of the adhesive layer composition can be measured at a temperature of 23° C. using a pH meter (pH METER F-52 manufactured by HORIBA).
[0092] [Method of preparing the adhesive layer composition] The adhesive layer composition can be produced by mixing the polymer and cellulose nanofibers with a solvent and other additives, if desired, by any method.
[0093] For example, when a polymer latex is used in preparing the composition for the adhesive layer, the cellulose nanofibers and other optional additives may be added to the polymer latex and mixed by a known method.
[0094] Furthermore, for example, when a dispersion of cellulose nanofibers is used when preparing a composition for an adhesive layer, a solid polymer or polymer latex and other optional additives can be added to this dispersion and mixed by a known method.
[0095] Furthermore, for example, when no solvent is used when preparing the adhesive layer composition, the solid polymer, the cellulose nanofibers, and any other solid additives that are used may be mixed using a known method, for example, a known roll, Henschel mixer, kneader, etc.
[0096] From the viewpoint of dispersing the cellulose nanofibers well in the adhesive layer composition, it is preferable to add a dispersion of the cellulose nanofibers (e.g., an aqueous dispersion) to the polymer latex under stirring to obtain a mixed solution, and then optionally add other additives to the mixed solution and further mix by a known method. It is preferable that the other additives, such as crosslinking agents and thickeners, which increase the viscosity in the system, are added as late as possible to maintain a uniform composition in the system.
[0097] <Layer formation process> In the layer forming step, an adhesive layer is formed on a wallpaper substrate containing cellulose using the adhesive layer composition prepared in the preparation step. As the wallpaper base material, the same materials as those described above regarding the wallpaper of the present invention can be used, and therefore a description thereof will be omitted here.
[0098] Here, the formation of the adhesive layer on the wallpaper substrate can be carried out, for example, by optionally foaming the above-mentioned adhesive layer composition on the wallpaper substrate and then forming it into a sheet. Alternatively, the formation of the adhesive layer on the wallpaper substrate can be carried out by obtaining the adhesive layer as an independent film and then laminating it onto the substrate by any known means such as an adhesive. Among these, the formation of the adhesive layer is preferably carried out by optionally foaming the above-mentioned adhesive layer composition on the wallpaper substrate and then forming it into a sheet.
[0099] Hereinafter, as an example, a method for forming an adhesive layer by foaming the above-mentioned composition for an adhesive layer on a wallpaper substrate and then forming it into a sheet will be described.
[0100] First, the adhesive layer composition is foamed to obtain an unsolidified foamed composition. When the adhesive layer composition is in the form of a dispersion, a foamed dispersion is obtained.
[0101] The foaming method is usually mechanical foaming. The foaming ratio may be adjusted as appropriate, but is usually 1.2 to 5 times, preferably 1.5 to 4 times. The mechanical foaming method is not particularly limited, but can be performed by mixing a certain amount of air into the dispersion of the adhesive layer composition and stirring it continuously or batchwise using an oak mixer, whipper, etc. The foamed dispersion obtained in this way becomes creamy. By forming pores by the mechanical foaming, an adhesive layer with excellent air escape properties can be finally obtained. When the foaming ratio is 1.2 times or more, the air escape properties can be prevented from decreasing, and when the foaming ratio is 5 times or less, the strength of the adhesive layer can be prevented from decreasing.
[0102] Next, the foaming composition is formed into a sheet. The method for forming the foaming composition into a sheet is not particularly limited. A suitable method is, for example, a method of applying the foaming composition into a sheet on a wallpaper substrate.
[0103] The foaming composition can be applied to a wallpaper substrate or the like using a commonly known coating device such as a roll coater, reverse roll coater, screen coater, doctor knife coater, or comma knife coater.
[0104] Next, the foam composition in the form of a sheet is solidified on the wallpaper substrate. The solidification of the foam composition is carried out, for example, by crosslinking the polymer of the foam composition. The method of crosslinking the polymer is not limited, but a method of heating and drying the foam composition is preferred. The method of heating and drying is not particularly limited as long as it is a method that can dry the foam composition on the wallpaper substrate and crosslink the polymer, and a known drying oven (for example, a hot air circulation type oven, a hot oil circulation hot air chamber, a far infrared heater chamber) can be used. The drying temperature can be, for example, 60°C or higher and 180°C or lower. In addition, it is preferable to perform multi-stage drying such that drying is performed from the inside at a low temperature in the early stage of drying and is sufficiently dried at a higher temperature in the later stage of drying, rather than performing drying at a constant temperature.
[0105] In this manner, wallpaper is formed, which comprises an adhesive layer formed by solidifying the sheet-like foam composition on the wallpaper substrate.
[0106] The obtained wallpaper is not particularly limited, but for example, a separator film as a release paper is attached to the surface on the adhesive layer side, and then the wallpaper is wound up by a winder and cut to an easy-to-use size by a press cutter, a slitter, or the like. EXAMPLES
[0107] Hereinafter, the present invention will be specifically described based on examples, but the present invention is not limited to these examples. In addition, in a polymer produced by polymerizing a plurality of types of monomers, the ratio of the monomer unit formed by polymerizing a certain monomer in the polymer is usually the same as the ratio (charge ratio) of the certain monomer in all the monomers used for the polymerization of the polymer, unless otherwise specified. And various measurements and evaluations in the examples and comparative examples were carried out according to the following methods.
[0108] <Number average fiber diameter> Using an atomic force microscope (Dimension FastScan AFM (manufactured by BRUKER, Tapping mode)), the fiber diameters of 5 cellulose nanofibers were measured, and the number average of the measured fiber diameters was calculated to obtain the value. <Appearance> The appearance of the wallpaper immediately after production and after 7 days of standing on a flat table was visually confirmed. <Coatability> Regarding the foaming composition or the composition for the adhesive layer, when applying using an automatic coater (main body: AFA-Standard KT-AB4420 manufactured by TQC sheen, applicator: Multi-applicator MA-250 manufactured by Coatec), the case where the applicator moved smoothly was regarded as "good", and the case where the applicator got stuck and did not move smoothly was regarded as "bad". <Planar smoothness> The appearance of the coated surface after coating the foaming composition or the composition for the adhesive layer was visually confirmed and evaluated according to the following criteria. A: Smooth B: Fine unevenness exists C: Large unevenness exists
[0109] (Production Example 1) <Preparation of TEMPO-oxidized cellulose nanofiber aqueous dispersion> 1 g of bleached softwood kraft pulp (dry weight equivalent), 5 mmol of sodium hypochlorite, 0.1 g (1 mmol) of sodium bromide, and 0.016 g (1 mmol) of TEMPO (2,2,6,6-tetramethylpiperidine 1-oxyl) were dispersed in 100 mL of water, gently stirred at room temperature for 4 hours, and washed with distilled water to obtain TEMPO-catalyzed oxidized pulp (oxidized cellulose). The amount of carboxyl groups in the obtained TEMPO-catalyzed oxidized pulp was 1.4 mmol / g. Distilled water was then added to the undried TEMPO-catalyzed pulp to prepare an aqueous dispersion with a solid content of 0.1%. The aqueous dispersion was then defibrated using a homogenizer (Microtech Nithion, Hiscotron) at 7.5×1000 rpm for 2 minutes, and an ultrasonic homogenizer (Nissei, Ultrasonic Generator) for 4 minutes with V-LEVEL4, TIP26D while cooling the container with ice to obtain an aqueous dispersion containing TEMPO-oxidized cellulose nanofibers. The undefibrated components were then removed from the aqueous dispersion of TEMPO-oxidized cellulose nanofibers by centrifugation (12000G (120×100 rpm / g), 10 minutes, 12℃) using a centrifuge (SAKUMA, M201-1VD, angle rotor 50F-8AL) to obtain an aqueous dispersion of TEMPO-oxidized cellulose nanofibers with a solid content of 0.1%. The TEMPO-oxidized cellulose nanofibers contained sodium derived from the co-oxidant in the form of a salt, i.e., the TEMPO-oxidized cellulose nanofibers were metal-containing carboxylated cellulose nanofibers that contained sodium in the form of a salt.
[0110] (Production Example 2) <Preparation of copper-containing TEMPO-oxidized cellulose nanofiber aqueous dispersion> To 100 mL of the TEMPO-oxidized cellulose nanofiber aqueous dispersion obtained in Production Example 1, 1 mL of 1 M hydrochloric acid was added under stirring to adjust the pH to 1. Stirring was then continued for 60 minutes. Thereafter, the TEMPO-oxidized cellulose nanofibers that had been gelled by the addition of hydrochloric acid were collected by centrifugation (12,000 G), and the collected TEMPO-oxidized cellulose nanofibers were washed successively with 1 M hydrochloric acid and a large amount of distilled water. Next, 100 mL of distilled water was added to obtain a 0.1% hydrogen-substituted TEMPO-oxidized cellulose nanofiber aqueous dispersion in which sodium was substituted with hydrogen. The carboxyl groups on the surface of the hydrogen-substituted TEMPO-oxidized cellulose nanofibers were measured by FT-IR (JASCO Corporation, FT / IR-6100) according to Biomacromolecules (2011, Vol. 12, pp. 518-522) and found to be substituted with carboxyl groups of 90% or more. 50 g of the resulting 0.1% hydrogen-substituted TEMPO-oxidized cellulose nanofiber aqueous dispersion was stirred, and 18 g of 0.1% copper (II) acetate aqueous solution was added thereto and stirred at room temperature for 3 hours. The oxidized cellulose nanofiber gelled by the addition of the copper (II) acetate aqueous solution was then collected by centrifugation (12000 G (120 x 100 rpm / g), 10 minutes, 12°C) using a centrifuge (SAKUMA, M201-1VD, angle rotor 50F-8AL), and the collected oxidized cellulose nanofiber was washed with a 0.1% copper (II) acetate aqueous solution, and then the collected oxidized cellulose nanofiber was washed with a large amount of distilled water. Then, 50 mL of distilled water was added, and the copper-substituted TEMPO-oxidized cellulose nanofibers were dispersed by ultrasonic treatment (2 minutes) using an ultrasonic homogenizer (Nissei, Ultrasonic Generator) with V-LEVEL4, TIP26D while cooling the container with ice. Then, undefibrated components were removed from the copper-substituted TEMPO-oxidized cellulose nanofiber aqueous dispersion by centrifugation (12000G (120×100 rpm / g), 10 minutes, 12° C.) using a centrifuge (SAKUMA, M201-1VD, angle rotor 50F-8AL). As a result, an aqueous dispersion of copper-containing TEMPO-oxidized cellulose nanofibers (hereinafter, simply referred to as “TOCN-Cu”) with a solid content concentration of 0.1% was obtained. The copper-containing TEMPO-oxidized cellulose nanofibers are metal-containing carboxylated cellulose nanofibers that contain copper in the form of a salt.
[0111] (Production Example 3) <Preparation of copper-containing TEMPO oxidized pulp aqueous dispersion> TEMPO-catalyzed oxidized pulp (oxidized cellulose) was obtained by dispersing 1 g of softwood bleached kraft pulp (dry weight equivalent), 5 mmol of sodium hypochlorite, 0.1 g (1 mmol) of sodium bromide, and 0.016 g (1 mmol) of TEMPO in 100 mL of water, gently stirring at room temperature for 4 hours, and washing with distilled water. The amount of carboxyl groups in the obtained TEMPO-catalyzed oxidized pulp was 1.4 mmol / g. 930 g of distilled water was added to 6 g of the above TEMPO oxidized pulp (solid concentration 15.5%), the aqueous dispersion was stirred, and then a 6.4% copper (II) acetate aqueous solution was slowly added dropwise thereto and stirred for 24 hours. The dispersion was filtered with a Kiriyama funnel (filter paper No. 5B, 95 Φm / m) to obtain a copper-containing TEMPO oxidized pulp aqueous dispersion with a solid concentration of 20.0%.
[0112] Example 1 200 g of acrylic polymer latex (solid concentration 58%) was weighed into a 500 ml disposable cup and stirred (1750 rpm) with a mixer (Tokushu Kika Kogyo, ROBOMICS). The copper-containing TEMPO oxidized cellulose nanofiber (TOCN-Cu) aqueous dispersion (solid concentration 0.5%) obtained in Production Example 2 was concentrated to a solid concentration of 1.1% with an evaporator, and 107 g of the concentrated aqueous dispersion (TOCN-Cu amount was 1 part by mass per 100 parts by mass of acrylic polymer latex) was gradually added in small portions to the stirred latex, and stirring was continued for 30 minutes after the addition. Then, while stirring the resulting mixture, 8g of ammonium stearate (San Nopco, Nopco DC-100A (concentration 30%)) as a foam stabilizer, 6g of fatty acid polyglycidyl ether (Japan Coating Resin, Rikabond EX-8) as an epoxy crosslinker, and 6g of sodium polyacrylate (Toagosei, Aron A-20L (concentration 15%)) as a thickener were added in that order, and the mixture was stirred for 30 minutes to obtain a composition for the adhesive layer. The composition for the adhesive layer had a concentration of 39%, a viscosity of 28 dPa·s (viscometer: RION, VISCO TESTER VT-06), and a pH of 9.3. The adhesive layer composition was foamed using a whisk (Tescom Co., Ltd., hand mixer THM272) to a foaming ratio of 2.0 times and a density of 0.42 g / cm 3 A foam composition of the formula: The obtained foam composition was applied to a wallpaper substrate (a two-layer structure substrate consisting of a resin decorative layer made of vinyl chloride resin and a backing material made of 100% cellulose paper, manufactured by Sangetsu Co., Ltd., TH30451) using an automatic coater (main body: AFA-Standard KT-AB4420 manufactured by TQC Sheen Co., Ltd., applicator: Multi-applicator MA-250 manufactured by Cortec Co., Ltd.). The coated wallpaper was placed in an 80°C oven (DNF400 manufactured by Yamato Scientific Co., Ltd.) for 80 seconds, then in a 120°C oven (DNF400 manufactured by Yamato Scientific Co., Ltd.) for 80 seconds, and then in a 140°C oven for 80 seconds to dry, resulting in a thickness of 120 μm and a density of 0.42 g / cm. 3 A wallpaper having the above adhesive layer (foam layer) on the wallpaper substrate was obtained. The appearance of the wallpaper was then observed. The results are shown in Table 1.
[0113] Example 2 The same procedure as in Example 1 was repeated except that the aqueous dispersion of copper-containing TEMPO-oxidized cellulose nanofibers (TOCN-Cu) (solids concentration 0.5%) obtained in Production Example 2 was replaced with the aqueous dispersion of TEMPO-oxidized cellulose nanofibers having a concentration of 0.1% obtained in Production Example 1, resulting in a nanofiber with a thickness of 120 μm and a density of 0.42 g / cm. 3 A wallpaper having the above adhesive layer (foam layer) on the wallpaper substrate was obtained. The appearance of the wallpaper was then observed. The results are shown in Table 1.
[0114] Example 3 The adhesive layer composition was not foamed with a whisk, but was replaced with a foamed composition with a density of 1.00 g / cm 3 The adhesive layer composition was used in the same manner as in Example 1, except that the adhesive layer composition was used. 3 A wallpaper having the above adhesive layer (non-foamed layer) on the wallpaper substrate was obtained. The appearance of the wallpaper was then observed. The results are shown in Table 1.
[0115] Example 4 The same procedure as in Example 1 was repeated, except that a cellulose nanofiber (manufactured by Sugino Machine Ltd., BiNFi-s, number average fiber diameter 50 nm) obtained by mechanically defibrating bleached kraft pulp was used instead of the concentrated aqueous dispersion obtained by concentrating the copper-containing TEMPO-oxidized cellulose nanofiber aqueous dispersion in an evaporator. 3 A wallpaper having the above adhesive layer (foam layer) on the wallpaper substrate was obtained. The appearance of the wallpaper was then observed. The results are shown in Table 1.
[0116] Comparative Example 1 The same procedure as in Example 1 was repeated except that, without using the copper-containing TEMPO-oxidized cellulose nanofiber aqueous dispersion, 8 g of ammonium stearate (manufactured by San Nopco Ltd., Nopco DC-100A (concentration 30%)) as a foam stabilizer, 6 g of fatty acid polyglycidyl ether (manufactured by Japan Coating Resins Co., Ltd., Rikabond EX-8) as an epoxy crosslinker, and 6 g of sodium polyacrylate (manufactured by Toagosei Co., Ltd., Aron A-20L (concentration 15%)) as a thickener were added to the acrylic polymer latex in that order, and the mixture was stirred for 30 minutes to obtain a composition for adhesive layer. 3 A wallpaper having the above adhesive layer (foam layer) on the wallpaper substrate was obtained. The appearance of the wallpaper was then observed. The results are shown in Table 1.
[0117] Comparative Example 2 250 g of acrylic polymer latex (solid concentration 58%) was weighed into a 500 ml disposable cup and stirred (1750 rpm) with a mixer (Tokushu Kika Kogyo, ROBOMICS). 2.1 g (0.3 parts by mass of TOCN-Cu per 100 parts by mass of acrylic polymer latex) of the copper-containing TEMPO oxidized pulp aqueous dispersion (solid concentration 20.0%) obtained in Production Example 3 was gradually added to the stirred latex in small amounts, and stirring was continued for 30 minutes after the addition. Then, while stirring the resulting mixture, 10 g of ammonium stearate (manufactured by San Nopco, Nopco DC-100A (concentration 30%)) as a foam stabilizer, 7.5 g of fatty acid polyglycidyl ether (manufactured by Japan Coating Resins, Rikabond EX-8) as an epoxy crosslinking agent, and 7.5 g of sodium polyacrylate (manufactured by Toagosei, Aron A-20L (concentration 15%)) as a thickener were added in that order, and the mixture was stirred for 30 minutes to obtain a composition for adhesive layer. During stirring, the copper-containing TEMPO oxidized pulp was wrapped around the mixer blades, causing a loss in the content of the copper-containing TEMPO oxidized pulp in the composition for adhesive layer. The composition for adhesive layer had a concentration of 57%, a viscosity of 66 dPa·s (viscometer: manufactured by RION, VISCO TESTER VT-06), and a pH of 8.7. The adhesive layer composition was foamed using a whisk (Tescom Co., Ltd., hand mixer THM272) to a foaming ratio of 2.0 times and a density of 0.42 g / cm 3 A foam composition of the formula: The obtained foam composition was applied to a wallpaper substrate (a two-layer structure substrate consisting of a resin decorative layer made of vinyl chloride resin and a backing material made of 100% cellulose paper, manufactured by Sangetsu Co., Ltd., TH30451) using an automatic coater (main body: AFA-Standard KT-AB4420 manufactured by TQC Sheen Co., Ltd., applicator: Multi-applicator MA-250 manufactured by Cortec Co., Ltd.). The coated wallpaper was placed in an 80°C oven (DNF400 manufactured by Yamato Scientific Co., Ltd.) for 80 seconds, then in a 120°C oven (DNF400 manufactured by Yamato Scientific Co., Ltd.) for 80 seconds, and then in a 140°C oven for 80 seconds to dry, resulting in a thickness of 120 μm and a density of 0.42 g / cm. 3 A wallpaper having the above adhesive layer (foam layer) on the wallpaper substrate was obtained. The appearance of the wallpaper was then observed. The results are shown in Table 1.
[0118] [Table 1]
[0119] It can be seen from Table 1 that the wallpapers of Examples 1 to 4 were prevented from warping or wrinkling both during and after production, whereas the wallpapers of Comparative Examples 1 and 2 were warped or wrinkling. [Industrial Applicability]
[0120] According to the present invention, it is possible to provide wallpaper that is less likely to warp or wrinkle during production or after application.
Claims
1. A wallpaper comprising a wallpaper base material and an adhesive layer provided on at least one surface of the wallpaper base material, The wallpaper substrate contains cellulose, The adhesive layer contains cellulose nanofibers having a number average fiber diameter of 100 nm or less.
2. The wallpaper according to claim 1 , wherein the cellulose nanofibers have a number average fiber length of 50 nm or more and 2000 nm or less.
3. The wallpaper according to claim 1 , wherein the cellulose nanofibers have an average degree of polymerization of 100 or more and 2,000 or less.
4. 2. The wallpaper of claim 1, wherein the cellulose nanofibers are carboxylated cellulose nanofibers.
5. The cellulose nanofiber is a metal-containing oxidized cellulose nanofiber containing a metal in the form of a salt, The wallpaper according to claim 1, wherein the metal is at least one selected from metals in groups 2 to 14 and periods 3 to 6 of the long periodic table.
6. 6. Wallpaper according to claim 5, wherein the metal is copper, zinc or silver.
7. 2. The wallpaper according to claim 1, wherein the adhesive layer is made of a resin foam.
8. The wallpaper according to claim 7 , wherein the resin foam contains open cells formed by a plurality of cells interconnected with each other.
9. 2. The wallpaper of claim 1, wherein the wallpaper substrate comprises a resin decorative layer and a backing material containing cellulose.
10. The wallpaper according to claim 1 , wherein the resin decorative layer contains a polyvinyl chloride resin.
11. 11. Wallpaper according to claim 9 or 10, wherein the backing material contains 50% by weight or more of cellulose.
12. A step of preparing a composition for adhesive layer containing cellulose nanofibers having a number average fiber diameter of 100 nm or less; forming an adhesive layer on a wallpaper substrate containing cellulose using the adhesive layer composition; A method for manufacturing wallpaper, comprising:
Citation Information
Patent Citations
Wallpaper sheet, building material
JP2022054523A
Composition for self-adsorbable foamed sheets, self-adsorbable foamed sheet, self-adsorbable laminate, and method for producing self-adsorbable laminate
JP2022101282A