Near infrared radiation shield material powder, manufacturing method of near infrared radiation shield material powder, and near infrared radiation shield material
The composite tungsten oxide-based near-infrared shielding material addresses the challenge of high transmittance and absorption by using a specific composition and crystal structure, ensuring effective near-infrared shielding and weather resistance.
Patent Information
- Application Number
- JP2023054287
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing near-infrared shielding materials face challenges in achieving high visible light transmittance while maintaining strong near-infrared absorption and weather resistance, particularly when exposed to high temperature and humidity environments.
A near-infrared shielding material powder composed of composite tungsten oxide with a specific formula Cs x W y O z, where 0.32≦x/y≦0.35 and 2.5≦z/y≦2.8, is used, combined with a hexagonal crystal structure, to enhance light transmission in the visible range and absorption in the near-infrared range, while ensuring weather resistance.
The material achieves excellent transmittance in the visible light region, high absorption in the near-infrared region, and demonstrates superior weather resistance, maintaining these properties even under high temperature and humidity conditions.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a near-infrared shielding material powder, a method for producing a near-infrared shielding material powder, and a near-infrared shielding material. [Background technology]
[0002] In recent years, in order to conserve global resources and reduce the environmental burden, automobile and building windows are required to have the function of blocking near-infrared rays in sunlight. This is because blocking near-infrared rays in automobile and building windows can reduce the temperature rise inside the automobile or building, thereby reducing the cooling load.
[0003] On the other hand, in order to maintain the original functions of windows, such as ensuring visibility, window materials are required to have as high a brightness as perceived by the eye, that is, a visible light transmittance, as possible.
[0004] As an example of glass that blocks infrared rays, Patent Document 1 discloses an infrared absorbing green glass composition in which iron oxide or the like is added to glass as a coloring agent. Patent Document 2 discloses a heat-retaining sheet made of a woven fabric in which a belt-shaped film having infrared reflectivity and a belt-shaped film having infrared absorbing properties are used as warp and weft threads, respectively. It also discloses that, as the belt-shaped film having infrared reflectivity, a synthetic resin film is subjected to aluminum deposition processing, and further laminated with a synthetic resin film. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2006-264994 A [Patent Document 2] Japanese Patent Application Publication No. 9-107815 Summary of the Invention [Problem to be solved by the invention]
[0006] However, in Patent Document 1, there is a limit to the infrared absorbing power of iron oxide, etc. Therefore, when the visible light transmittance of the infrared absorbing green glass composition is increased, there is a problem that the infrared absorbing property decreases. In the case of the product disclosed in Patent Document 2, in which a synthetic resin film is subjected to aluminum deposition processing and further a synthetic resin film is laminated, there is also a problem that when the visible light transmittance is increased, the infrared shielding property decreases.
[0007] Furthermore, near-infrared shielding materials such as near-infrared shielding material powders are often placed in high temperature or high temperature and high humidity environments, and are therefore required to have weather resistance that does not cause significant changes in optical properties even when placed in high temperature or high temperature and high humidity environments.
[0008] Therefore, an object of one aspect of the present invention is to provide a near-infrared shielding material powder that has excellent light transmittance in the visible light region, exhibits high absorption of light in the near-infrared region, and has excellent weather resistance. [Means for solving the problem]
[0009] In one aspect of the present invention, there is provided a near-infrared shielding material powder comprising a composite tungsten oxide, The composite tungsten oxide has the general formula Cs x W y O z It is expressed as In the general formula, x, y, and z satisfy the relationships of 0.32≦x / y≦0.35 and 2.5≦z / y≦2.8, CIE-L * a * b * In the color system, a * ≦0 and b * Provided is a near-infrared shielding material powder that satisfies the viscosity of ≦-10. Effect of the Invention
[0010] According to one aspect of the present invention, there is provided a near-infrared shielding material powder that has excellent light transmittance in the visible light region, exhibits high absorption of light in the near-infrared region, and has excellent weather resistance. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic diagram of a near-infrared shielding material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The following describes a form for carrying out the present invention. However, the present invention is not limited to the following embodiment, and various modifications and substitutions can be made to the following embodiment without departing from the scope of the present invention.
[0013] Hereinafter, the following will be described in detail in the order of [1] near-infrared shielding material powder, [2] a method for producing the near-infrared shielding material powder, and [3] the near-infrared shielding material. [1] Near-infrared shielding material powder The inventors of the present invention have investigated near-infrared shielding material powders that have excellent light transmittance in the visible light region, high absorption of light in the near-infrared region, and excellent weather resistance. As a result, they have found that by including a composite tungsten oxide having a predetermined composition and setting the color within a predetermined range, it is possible to achieve excellent light transmittance in the visible light region, high absorption of light in the near-infrared region, and improved weather resistance, and have completed the present invention.
[0014] For this reason, the near-infrared shielding material powder of the present embodiment contains a composite tungsten oxide. The near-infrared shielding material powder of the present embodiment may be composed of only a composite tungsten oxide, but this does not exclude the inclusion of inevitable impurities even in this case. (1) Composition of composite tungsten oxide The composite tungsten oxide contained in the near-infrared shielding material powder of the present embodiment is represented by the general formula Cs x W y O z In the above general formula, x, y, and z satisfy the relationships 0.32≦x / y≦0.35 and 2.5≦z / y≦2.8.
[0015] Composite tungsten oxide has a composition in which cesium is added to tungsten trioxide (WO3). Since tungsten trioxide does not contain effective free electrons, it cannot exert an infrared absorbing effect unless the ratio of oxygen to 1 mole of tungsten is less than 3. However, in composite tungsten oxide, the addition of cesium generates free electrons, and it is possible to obtain an infrared absorbing effect.
[0016] Therefore, the composite tungsten oxide can exhibit an infrared absorbing effect by containing cesium, but by setting x / y, which indicates the content ratio of cesium to tungsten in terms of the amount of substance, to 0.32 or more, the light absorbing function in the near-infrared region can be enhanced. Furthermore, by setting x / y to 0.35 or less, the inclusion of different phases can be suppressed, and the light absorbing function in the near-infrared region can be enhanced. Furthermore, by suppressing the inclusion of different phases, the color of the near-infrared shielding material powder can be easily adjusted within a desired range.
[0017] In addition, in the composite tungsten oxide, the oxygen content ratio in terms of the amount of substance to tungsten, z / y, can be set to 3 or less because of the supply of free electrons by cesium. However, the crystal phase of WO2 may cause absorption and scattering of light in the visible light range, and may reduce the absorption of light in the near infrared range. Therefore, in order to suppress the generation of WO2, it is preferable that the ratio of oxygen to 1 mole of tungsten is greater than 2.
[0018] Furthermore, according to the investigations of the present inventors, by selecting a prescribed range for z / y, which is the content ratio in terms of substance amount of oxygen to tungsten, it is possible to achieve excellent light transmittance in the visible light region, high absorption of light in the near-infrared region, and improved weather resistance.
[0019] Specifically, by making z / y 2.5 or more, oxidation can be suppressed even when placed in a high temperature or high temperature and high humidity environment. Therefore, by making z / y 2.5 or more, weather resistance can be improved and the absorption of light in the near infrared region can be maintained at a high level even after being placed in a high temperature or high temperature and high humidity environment.
[0020] Furthermore, by setting z / y to 2.8 or less, the incorporation of different phases can be suppressed and the absorption of light in the near infrared region can be increased.
[0021] For this reason, in the composite tungsten oxide contained in the near-infrared shielding material powder of this embodiment, z / y, which is the content ratio in terms of substance amount of oxygen to tungsten, is preferably 2.5 or more and 2.8 or less. (2) Crystal structure and crystallite size of composite tungsten oxide The crystal structure of the composite tungsten oxide contained in the near-infrared shielding material powder of the present embodiment is not particularly limited, but the composite tungsten oxide is preferably composed only of hexagonal crystals.
[0022] When the composite tungsten oxide has a hexagonal crystal structure, the particles have improved light transmittance in the visible light region and improved light absorption in the near-infrared region.
[0023] Even when the composite tungsten oxide has a tetragonal or cubic crystal structure, it functions as a near-infrared shielding material. However, the absorption position of light in the near-infrared region tends to change depending on the crystal structure of the composite tungsten oxide. The absorption position of light in the near-infrared region tends to move to the longer wavelength side in the tetragonal crystal than in the cubic crystal, and further to the longer wavelength side in the hexagonal crystal than in the tetragonal crystal. In addition, accompanying the change in the absorption position, the absorption of light in the visible light region is the least in the hexagonal crystal, followed by the tetragonal crystal, and among these, the absorption of light in the visible light region is the greatest in the cubic crystal. Therefore, it is preferable to use a hexagonal composite tungsten oxide for applications in which more light in the visible light region is transmitted and more light in the infrared region is shielded.
[0024] As described above, when the composite tungsten oxide has a hexagonal crystal structure, the transmittance of the composite tungsten oxide in the visible light region and the absorption of the composite tungsten oxide in the near infrared region are particularly improved. Therefore, it is preferable that the near infrared shielding material powder is made of only the composite tungsten oxide with a hexagonal crystal structure. And, when the composite tungsten oxide contains cesium, it is easy to form a hexagonal crystal. Therefore, as shown in the above general formula, it is preferable that the composite tungsten oxide contains cesium.
[0025] The crystallite size of the composite tungsten oxide contained in the near-infrared shielding material powder of the present embodiment is not particularly limited, but is preferably, for example, 20 nm or less. The lower limit of the crystallite size is not particularly limited, but can be, for example, 5 nm or more.
[0026] The crystallite size of the composite tungsten oxide preferably satisfies the above range, for example, after the dispersion step described below.
[0027] The crystallite size of the composite tungsten oxide can be calculated from the (200) plane peak in the X-ray diffraction pattern according to Scherrer's formula. (3) Color of near-infrared shielding powder The near-infrared shielding material powder of the present embodiment is CIE-L * a * b * In the color system, a * ≦0 and b * It is preferable that the value satisfies ≦−10.
[0028] a * represents the intensity of the color from green to red, with 0 being neither green nor red, negative values representing green, and positive values representing red. * By setting the ratio to ≦0, the color will have a greenish tint or no reddish tint. By setting the color in this way, it is possible to increase the transmittance of light in the visible light region.
[0029] b *represents the intensity of the color from blue to yellow, with 0 being neither blue nor yellow, negative values representing blue, and positive values representing yellow. * By setting the ratio to ≦−10, a bluish color is obtained. By setting the color to such a value, it is possible to increase the absorption of light in the near infrared region. [2] Manufacturing method of near-infrared shielding material powder Next, a method for producing the near-infrared shielding material powder of the present embodiment will be described.
[0030] According to the method for producing a near-infrared shielding material powder of the present embodiment, the near-infrared shielding material powder already described can be produced, so the description of the matters already described will be omitted. Note that, here, only a configuration example of the method for producing a near-infrared shielding material powder is shown, and the method for producing a near-infrared shielding material powder already described is not limited to the following configuration example.
[0031] The near-infrared shielding material powder of the present embodiment can be produced by heat treating a mixture of raw materials in a reducing atmosphere.
[0032] Hereinafter, (1) a tungsten raw material and (2) a cesium raw material, which are raw materials for the near-infrared shielding material powder of the present embodiment, will be described, and further (3) a method for producing the near-infrared shielding material powder will be described.
[0033] (1) Tungsten raw materials As the tungsten raw material (tungsten source) containing tungsten, for example, tungsten compound powder can be used.As the tungsten compound powder, one or more selected from tungsten acid powder, tungsten trioxide powder, tungsten dioxide powder, tungsten oxide hydrate powder obtained by dissolving tungsten hexachloride powder in alcohol and then drying, tungsten oxide hydrate powder obtained by dissolving tungsten hexachloride powder in alcohol and then adding water to precipitate and drying the precipitate, and tungsten compound powder obtained by drying ammonium tungstate aqueous solution can be used.
[0034] Furthermore, it is also preferable to use a liquid tungsten compound as the tungsten raw material. When using a liquid tungsten compound as the tungsten raw material, it is easy to uniformly mix the liquid tungsten compound with the cesium raw material described later. From this point of view, it is also preferable to use an aqueous solution of ammonium tungstate or an aqueous solution of tungsten hexachloride as the tungsten raw material. (2) Cesium raw material As the cesium raw material (cesium source) containing cesium, one or more types selected from cesium carbonate, cesium hydroxide, cesium acetate, cesium oxide, and the like can be suitably used. (3) Manufacturing method of near-infrared shielding material powder The method for producing the near-infrared shielding material powder of the present embodiment may include the following mixing step and heat treatment step. Each step will be described below. (3-1) Mixing process In the mixing step, the above-mentioned tungsten raw material and cesium raw material are weighed and mixed to obtain a mixture.
[0035] In the mixing step, it is preferable to weigh and mix the tungsten raw material and the cesium raw material so that the ratio of the amount of substance of elemental cesium (Cs) to elemental tungsten (W) contained in the mixture, i.e., the amount of substance ratio of Cs / W in the mixture, is 0.32 or more and 0.35 or less.
[0036] By setting the substance ratio of cesium to tungsten in the mixture to 0.35 or less, it is possible to prevent the generation of heterogeneous phases in the near-infrared shielding material powder obtained after the heat treatment step. As described above, by suppressing the generation of heterogeneous phases in the near-infrared shielding material powder, it is possible to make the color of the near-infrared shielding material powder desired and to increase the absorption of light in the near-infrared region.
[0037] Furthermore, by setting the substance ratio of cesium to tungsten in the mixture to 0.32 or more, the cesium is uniformly dispersed in the composite tungsten oxide, and the absorption of light in the near-infrared region can be increased.
[0038] The method for mixing the tungsten raw material and the cesium raw material is not particularly limited, and a dry method or a wet method can be used. The dry method does not require a step such as drying after mixing, so that productivity can be increased.
[0039] From the viewpoint of obtaining a mixture in which each raw material component is uniformly mixed at the molecular level, a wet method in which each raw material is mixed in a solution can be suitably used. From this viewpoint, it is preferable to use raw material powder that can be dissolved in a solvent such as water or an organic solvent.
[0040] Therefore, the mixing method in the mixing step can be selected taking into consideration the productivity, the degree of uniformity required for the resulting mixture, and the like.
[0041] When mixing the tungsten raw material and the cesium raw material by the wet method, for example, the following procedure can be used. In the following explanation, an example will be explained in which H2WO4 powder is used as the tungsten raw material and Cs2CO3 powder is used as the cesium raw material.
[0042] When mixing the tungsten raw material and the cesium raw material by the wet method, the mixing step can be carried out by, for example, putting weighed H2WO4 powder and Cs2CO3 powder into a mortar, adding water and mixing to obtain a mixture. Furthermore, the obtained mixture can be dried at 100°C in the air to obtain a dried product, and the obtained dried product can be crushed in a mortar to obtain a crushed mixture.
[0043] The amount of water added during mixing may be any amount that allows the weighed raw material powder to be mixed uniformly. The drying time at 100°C in air may be any amount that allows the water to completely evaporate, and is preferably, for example, about 12 hours.
[0044] The mixture obtained in the mixing step and subjected to the firing step preferably has an average particle size of 500 nm or less. For this reason, it is preferable to mix the tungsten raw material and the cesium raw material in the mixing step, and then perform a pulverization process as necessary. When the mixing step includes a pulverization process, the mixing step can also be called a mixing and pulverization step. In this case, the mixing and pulverization step can prepare a mixture by weighing, mixing, and pulverizing the above-mentioned tungsten raw material and cesium raw material according to the target composition.
[0045] In this specification, the average particle size refers to the particle size at 50% volume accumulated in the volume-based particle size distribution determined by a laser diffraction / scattering method.
[0046] The pulverization can be performed using a roller mill, a jet mill, a hammer mill, a pin mill, a rotary mill, a planetary mill, a vibration mill, a bead mill, or the like. The average particle size of the mixture after pulverization is preferably 500 nm or less. If the average particle size of the mixture is 500 nm or less, the mixture can be fired at a low temperature in the heat treatment step, and the particles do not become coarse, so that the haze value of the dispersion liquid or dispersion using the obtained near-infrared shielding material powder is low. In addition, the dispersion can be performed in a short time in the dispersion step.
[0047] When the average particle size of the mixture of the tungsten raw material and the cesium raw material is 500 nm or less, it is possible to subject the mixture to the heat treatment step without pulverization. (3-2) Heat treatment process In the heat treatment step, the mixture obtained in the above-mentioned mixing step or the mixing and pulverizing step is heat treated in a reducing atmosphere to prepare a near-infrared shielding material powder.
[0048] In the heat treatment step, the mixture obtained in the mixing step can be filled into a firing vessel such as a crucible and heat treated.
[0049] The heat treatment conditions are not particularly limited, but can be selected so that the amount of oxygen relative to tungsten (z / y) in the composite tungsten oxide contained in the near-infrared shielding material powder obtained after the heat treatment step is within a desired range. For example, the heat treatment temperature is preferably less than 500°C. The lower limit of the heat treatment temperature is also not particularly limited, but the heat treatment temperature is preferably higher than 400°C.
[0050] The rate of temperature rise up to the heat treatment temperature is not particularly limited, but can be, for example, 5°C / min to 15°C / min. By raising the temperature at a rate of 15°C / min or less, the particles constituting the mixture having an average particle size of 500 nm or less can be heated sufficiently to the center, and a near-infrared shielding material powder containing a composite tungsten oxide of the desired composition can be obtained. In addition, by raising the temperature at a rate of 5°C / min or more, the productivity of the near-infrared shielding material powder can be increased.
[0051] The heat treatment time, which is the time to hold the heat treatment temperature after reaching the heat treatment temperature, is not particularly limited, but is preferably 1 hour or more and 2 hours or less. By performing heat treatment at the heat treatment temperature for 1 hour or more, the particles constituting the mixture with an average particle size of 500 nm or less can be sufficiently heated to the center, and a near-infrared shielding material powder containing a composite tungsten oxide of the target composition can be obtained. In addition, by setting the heat treatment time to 2 hours or less, the productivity of the near-infrared shielding material powder can be increased.
[0052] The reducing atmosphere is not particularly limited, but may be an atmosphere containing a reducing gas and an inert gas, for example, an atmosphere containing hydrogen gas as a reducing gas with nitrogen gas as a carrier. The content ratio of the reducing gas in the reducing atmosphere is not particularly limited, but for example, when the reducing gas is hydrogen gas, it is preferable that the content is 1% or more and 10% or less by volume. By containing hydrogen at a volume ratio of 1% or more and 10% or less, the reduction of the mixture can be sufficiently promoted. (3-3) Dispersion process The method for producing the near-infrared shielding material powder of the present embodiment may include any step other than the mixing step and the heat treatment step, and may also include, for example, a dispersion step.
[0053] The dispersion step is a step of wet-pulverizing the near-infrared shielding material powder obtained in the heat treatment step and dispersing the near-infrared shielding material powder in an organic solvent, which is a liquid medium (dispersion medium). By carrying out the dispersion step, a near-infrared shielding material powder having a finer particle size can be obtained.
[0054] In the dispersion step, it is preferable to add a dispersant and an organic solvent to the near-infrared shielding material powder obtained in the heat treatment step, and then perform wet pulverization.
[0055] The dispersant to be added is not particularly limited, and can be any general dispersant capable of dispersing the near-infrared shielding material powder containing composite tungsten oxide.Preferred examples of dispersants include dispersants having an amine-containing group, a hydroxyl group, a carboxyl group, or an epoxy group as a functional group.This is because these functional groups are adsorbed to the surface of the particles contained in the near-infrared shielding material powder, and have the effect of preventing the particles contained in the near-infrared shielding material powder from agglomerating and dispersing them uniformly.
[0056] Specific examples of preferred dispersants include acrylic-styrene copolymer dispersants having a carboxyl group as a functional group, acrylic dispersants having an amine-containing group as a functional group, etc. However, the dispersant is not limited to these.
[0057] The organic solvent to be added is not particularly limited, and can be appropriately selected depending on the conditions required for forming a near-infrared shielding film or the like.
[0058] Specific examples of preferred organic solvents include alcohol solvents such as methanol, ethanol, isopropanol, butanol, benzyl alcohol, and diacetone alcohol; ketone solvents such as acetone, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), cyclohexanone, and isophorone; glycol derivatives such as propylene glycol methyl ether and propylene glycol ethyl ether; formamide, N-methylformamide, dimethylformamide (DMF), dimethylacetamide, dimethylsulfoxide (DMSO), and N-methyl-2-pyrrolidone (NMP), but are not limited to these.
[0059] When adding the dispersant and the organic solvent to the near-infrared shielding material powder, the mixing ratio is not particularly limited and can be selected arbitrarily. For example, it is preferable to mix 5 parts by mass or more and 15 parts by mass or less of the near-infrared shielding material powder, 5 parts by mass or more and 15 parts by mass or less of the dispersant, and 70 parts by mass or more and 90 parts by mass or less of the organic solvent.
[0060] The method for dispersing the near-infrared shielding material powder in the organic solvent is not particularly limited. Any method can be selected as long as it can pulverize the near-infrared shielding material powder and uniformly disperse the generated near-infrared shielding material powder in the organic solvent. Specifically, the near-infrared shielding material powder can be pulverized and the generated near-infrared shielding material powder can be uniformly dispersed in the organic solvent by using an apparatus or method such as a bead mill dispersion, a ball mill dispersion, a sand mill dispersion, or an ultrasonic dispersion. [3] Near-infrared shielding material Next, the near-infrared shielding material of the present embodiment will be described.
[0061] The near-infrared shielding material of the present embodiment can contain a liquid medium and the near-infrared shielding material powder contained in the liquid medium. That is, for example, as shown in FIG. 1, the near-infrared shielding material 10 of the present embodiment can contain the near-infrared shielding material powder 11 and a liquid medium 12. The near-infrared shielding material powder 11 is preferably dispersed in the liquid medium 12. Therefore, the near-infrared shielding material can also be called a near-infrared shielding particle dispersion.
[0062] It should be noted that Fig. 1 is a schematic diagram, and the near-infrared shielding material of this embodiment is not limited to this form. For example, in Fig. 1, each particle of the near-infrared shielding material powder 11 is represented by a circle and described as a spherical particle, but the shape of each particle of the near-infrared shielding material powder 11 is not limited to this form and can have any shape. The near-infrared shielding material 10 can contain other additives as necessary in addition to the near-infrared shielding material powder 11 and the liquid medium 12.
[0063] The near-infrared shielding material of the present embodiment can be obtained by using the near-infrared shielding material powder described above, in other words, by using the near-infrared shielding material powder obtained by the method for producing the near-infrared shielding material powder described above.
[0064] The near-infrared shielding material may further contain, if desired, a dispersant and other additives in addition to the near-infrared shielding material powder and the liquid medium. The near-infrared shielding material may also be used as an intermediate product of a near-infrared shielding particle dispersion in which the near-infrared shielding material powder is dispersed in a solid medium, or as a coating liquid.
[0065] The near-infrared shielding material of the present embodiment can be obtained by the above-mentioned dispersion process. Since the dispersant and the organic solvent have already been described, the description thereof will be omitted.
[0066] Although the properties of the near-infrared shielding material of the present embodiment are not particularly limited, it is preferable that the haze value is 0.3% or less when the total light absorption rate is 80%. By using the near-infrared shielding material powder of the present embodiment, the haze value can be set to satisfy the above range, which is preferable because light scattering can be suppressed. EXAMPLES
[0067] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. (Evaluation method) First, the evaluation methods used in the following Examples and Comparative Examples will be described. (Crystal structure, crystallite size) The crystal structure of the composite tungsten oxide contained in the near-infrared shielding material powder obtained after the heat treatment step in each of the examples and comparative examples was measured.
[0068] The X-ray diffraction pattern of the composite tungsten oxide was measured by powder X-ray diffraction (θ-2θ method) using a powder X-ray diffractometer (X'Pert-PRO / MPD manufactured by PANalytical, Spectris Co., Ltd.). From the obtained X-ray diffraction pattern, the crystal structure contained in the composite tungsten oxide and the presence or absence of heterophases other than hexagonal crystals were identified.
[0069] In addition, the near-infrared shielding material powder was recovered from the near-infrared shielding particle dispersion liquid, which is the near-infrared shielding material obtained in the dispersion process, and the crystallite size of the composite tungsten oxide was calculated using the Scherrer equation from the measured X-ray diffraction pattern.
[0070] The Scherrer formula is expressed by the following formula (1). In formula (1), D represents the crystallite diameter, β represents the diffraction line width, λ represents the wavelength of the X-ray, and θ represents the Bragg angle (diffraction angle). K is the Scherrer constant, which is 0.89. The peak of the (200) plane is used to calculate the crystallite diameter, so θ is 13.8976°. In addition, CuKα rays are used as the X-rays, so λ is 1.5418 Å. In calculating the diffraction line width β, which is the width of the diffraction line profile, the half-width of the diffraction peak by Kα1 was used after waveform separation into Kα1 and Kα2, and the broadening due to the optical system of the measuring device was corrected.
[0071] D = Kλ ÷ (β cos θ) (1) (Optical properties of near-infrared shielding materials) The optical properties of the near-infrared shielding material powders and the near-infrared shielding particle dispersions, which are the near-infrared shielding materials, obtained in the examples and comparative examples were measured as follows.
[0072] First, the near-infrared shielding material was diluted with methyl isobutyl ketone as a solvent in a glass cell for measuring the spectrophotometer, and the concentration of the near-infrared shielding material powder was adjusted to 1% by mass. Next, the diluted near-infrared shielding material was placed in a spectrophotometric cell, and transmittance was measured at a wavelength of 500 nm in the visible light region and at a wavelength of 1000 nm in the near-infrared region using a spectrophotometer (Hitachi, Model: U-4000). The evaluation results are shown in the "Transmittance" column of Table 3.
[0073] In addition, the color value L * a * b * The measurement was performed using a color difference meter (Konica Minolta Japan, Inc., Model: CR-5) and the results were compared with the "L * ","a * ", "b * The results are shown in the "" column. (Heat resistance test, moist heat resistance test) As a sample for the heat resistance test, the near-infrared shielding particle dispersion liquid, which is the near-infrared shielding material obtained after the dispersion process in each Example and Comparative Example, was coated on a glass substrate so that the total light absorption rate was 80%, and dried to prepare a sample for the heat resistance test (hereinafter also referred to as "heat resistance test sample"). The drying was performed at 70°C for 1 minute.
[0074] In addition, as a sample for the moist heat resistance test, the near infrared shielding material obtained after the dispersion process in each Example and Comparative Example was coated on a polyethylene terephthalate substrate so that the total light absorption rate was 80%, and then dried to prepare a sample (hereinafter also referred to as "moist heat resistance test sample"). The drying was performed at 70°C for 1 minute.
[0075] After drying, the haze value of the coating film of the heat resistance test sample was measured using a haze meter (HM-150N manufactured by Murakami Color Research Laboratory Co., Ltd.) and calculated based on JIS K 7136 (2000). The measurement results are shown in the "Haze" column of Table 3.
[0076] Before carrying out the heat resistance test and the moist heat resistance test, the transmittance of the heat resistance test sample and the moist heat resistance test sample was measured at wavelengths of 500 nm and 1000 nm using a spectrophotometer.
[0077] Then, as a heat resistance test, the heat resistance test sample was left for 120 hours in an incubator set at 120°C. The transmittance of the heat resistance test sample at wavelengths of 500 nm and 1000 nm after leaving it in the incubator for 120 hours was measured. The transmittance at each wavelength after 120 hours is shown in the "Transmittance after heat resistance" column of Table 3. In addition, the amount of change in transmittance after the heat resistance test and before the heat resistance test is shown in the "After heat resistance - Before heat resistance" column.
[0078] For the moist heat resistance test, the moist heat resistance test sample was placed in an incubator set at 85°C and a relative humidity of 90%. The moist heat resistance test sample was placed in the incubator for 120 hours, after which the transmittance at wavelengths of 500 nm and 1000 nm was measured. The transmittance at each wavelength after 120 hours is shown in the "Transmittance after moist heat resistance" column in Table 3. In addition, the amount of change in transmittance between after the moist heat resistance test and before the moist heat resistance test is shown in the "After moist heat resistance - Before moist heat resistance" column. [Example 1] A near-infrared shielding material powder was produced by the following procedure. (1)Mixing process A mixture was prepared by mixing H2WO4 (tungstic acid) powder, which is a tungsten raw material, and Cs2CO3 (cesium carbonate) powder, which is a cesium raw material.
[0079] The tungsten raw material and the cesium raw material were weighed out so that the ratio of the amount of cesium (Cs) to the amount of tungsten (W) contained in the mixture was Cs / W = 0.32, as shown in the Cs / W column in Table 1, and mixed in a mortar to form a mixture.
[0080] The resulting mixed powder was pulverized by a jet mill to an average particle size of 500 nm, and then subjected to a heat treatment step. (2) Heat treatment process The mixed powder with an average particle size of 500 nm obtained in the mixing step was heated from room temperature to the heat treatment temperature of 450°C at a heating rate of 10°C / min in an atmosphere of 10% by volume hydrogen-90% by volume nitrogen. After reaching the heat treatment temperature, the powder was heat treated (fired) at the heat treatment temperature for 1 hour to obtain a near-infrared shielding material powder made of a composite tungsten oxide.
[0081] The XRD spectrum of the obtained near-infrared shielding material powder was measured. As a result, it was confirmed that the near-infrared shielding material powder is composed of composite tungsten oxide, the composite tungsten oxide has a hexagonal crystal structure, and does not contain any heterophase. The crystal structure of the composite tungsten oxide and the presence or absence of heterophase are shown in the "Crystal" column of Table 2.
[0082] The amount of cesium and the amount of tungsten in the obtained near-infrared shielding material powder were analyzed by an ICP emission spectrometer (Shimadzu Corporation, Model: ICPE-9000). The amount of oxygen was analyzed by an oxygen / nitrogen / hydrogen analyzer (LECO Japan, Model: ONH836).
[0083] As a result, it was confirmed that in the composite tungsten oxide contained in the near-infrared shielding material powder obtained in this example, Cs / W, which indicates the content ratio of cesium to tungsten in terms of substance amount, was 0.32. Also, it was confirmed that O / W, which indicates the content ratio of oxygen to tungsten in terms of substance amount, was 2.5. The evaluation results are shown in the "Substance amount ratio" column in Table 2. (3) Dispersion process 10% by mass of the near-infrared shielding material powder obtained in the heat treatment step, 10% by mass of a dispersing agent mainly composed of n-butyl acetate, and 80% by mass of methyl isobutyl ketone as an organic solvent were weighed out. These were loaded into a paint shaker containing zirconia beads of 0.3 mm in diameter, and subjected to a pulverization and dispersion treatment for 5 hours to obtain a near-infrared shielding particle dispersion liquid, which is the near-infrared shielding material according to Example 1.
[0084] The production conditions of the near-infrared shielding material powder and the near-infrared shielding material according to Example 1 are shown in Table 1.
[0085] The near-infrared shielding particle dispersion thus obtained was subjected to the above-mentioned evaluation of optical properties, heat resistance test, and moist heat resistance test. The evaluation results are shown in Tables 2 and 3. [Example 2] In the mixing step, the tungsten raw material and the cesium raw material were weighed out so that the ratio of the amount of cesium (Cs) to the amount of tungsten (W) contained in the mixture was Cs / W = 0.35, as shown in the Cs / W column in Table 1, and mixed in a mortar to obtain a mixed powder.
[0086] Except for the above, a near-infrared shielding material powder and a near-infrared shielding material were prepared under the same conditions and procedures as in Example 1, and were evaluated.
[0087] Table 1 shows the production conditions of the near-infrared shielding material powder, and Tables 2 and 3 show the evaluation results of the near-infrared shielding material powder and the near-infrared shielding material. [Comparative Example 1 and Comparative Example 2] In the mixing step, the tungsten raw material and the cesium raw material were weighed out so that the ratio of the amount of cesium element (Cs) to the amount of tungsten element (W) contained in the mixture was the value shown in the Cs / W column in Table 1, and mixed in a mortar to form a mixed powder.
[0088] Except for the above, a near-infrared shielding material powder and a near-infrared shielding material were prepared under the same conditions and procedures as in Example 1, and were evaluated.
[0089] Table 1 shows the production conditions of the near-infrared shielding material powder, and Tables 2 and 3 show the evaluation results of the near-infrared shielding material powder and the near-infrared shielding material. [Example 3] In the heat treatment step, the mixed powder with an average particle size of 500 nm obtained in the mixing step was heated from room temperature to the heat treatment temperature of 450°C at a heating rate of 10°C / min in an atmosphere of 1% by volume hydrogen-99% by volume nitrogen. After reaching the heat treatment temperature, the powder was heat treated (fired) at the heat treatment temperature for 1 hour to obtain a near-infrared shielding material powder made of a composite tungsten oxide.
[0090] Except for the above, a near-infrared shielding material powder and a near-infrared shielding material were prepared under the same conditions and procedures as in Example 1, and were evaluated.
[0091] Table 1 shows the production conditions of the near-infrared shielding material powder, and Tables 2 and 3 show the evaluation results of the near-infrared shielding material powder and the near-infrared shielding material. [Comparative Example 3] In the heat treatment step, the mixed powder with an average particle size of 500 nm obtained in the mixing step was heated from room temperature to the heat treatment temperature of 400°C at a heating rate of 10°C / min in an atmosphere of 1% by volume hydrogen-99% by volume nitrogen. After reaching the heat treatment temperature, the powder was heat treated (fired) at the heat treatment temperature for 1 hour to obtain a near-infrared shielding material powder made of a composite tungsten oxide.
[0092] Except for the above, a near-infrared shielding material powder and a near-infrared shielding material were prepared under the same conditions and procedures as in Example 1, and were evaluated.
[0093] Table 1 shows the production conditions of the near-infrared shielding material powder, and Tables 2 and 3 show the evaluation results of the near-infrared shielding material powder and the near-infrared shielding material. [Comparative Example 4] In the heat treatment step, the mixed powder with an average particle size of 500 nm obtained in the mixing step was heated from room temperature to the heat treatment temperature of 500°C at a heating rate of 10°C / min in an atmosphere of 10% by volume hydrogen-90% by volume nitrogen. After reaching the heat treatment temperature, the powder was heat treated (fired) at the heat treatment temperature for 1 hour to obtain a near-infrared shielding material powder made of a composite tungsten oxide.
[0094] Except for the above, a near-infrared shielding material powder and a near-infrared shielding material were prepared under the same conditions and procedures as in Example 1, and were evaluated.
[0095] Table 1 shows the production conditions of the near-infrared shielding material powder, and Tables 2 and 3 show the evaluation results of the near-infrared shielding material powder and the near-infrared shielding material. [Comparative Example 5] In the mixing step, the tungsten raw material and the cesium raw material were weighed out so that the ratio of the amount of cesium (Cs) to the amount of tungsten (W) contained in the mixture was Cs / W = 0.32, as shown in the Cs / W column in Table 1, and mixed in a mortar to obtain a mixed powder.
[0096] The resulting mixed powder was then pulverized by a jet mill to an average particle size of 600 nm, and then subjected to a heat treatment step.
[0097] Except for the above, a near-infrared shielding material powder and a near-infrared shielding material were prepared under the same conditions and procedures as in Example 1, and were evaluated.
[0098] Table 1 shows the production conditions of the near-infrared shielding material powder, and Tables 2 and 3 show the evaluation results of the near-infrared shielding material powder and the near-infrared shielding material.
[0099] [Table 1]
[0100] [Table 2]
[0101] [Table 3] According to the results shown in Tables 2 and 3, it was confirmed that the near-infrared shielding material powders and near-infrared shielding materials of Examples 1 to 3 have high transmittance at a wavelength of 500 nm and low transmittance at a wavelength of 1000 nm. In other words, it was confirmed that the near-infrared shielding material powders and near-infrared shielding materials of Examples 1 to 3 have excellent transmittance for light in the visible light region and can exhibit high absorption of light in the near-infrared region.
[0102] Furthermore, according to the near-infrared shielding material powders and near-infrared shielding materials of Examples 1 to 3, no change in optical properties was observed before and after the heat resistance test and the moist heat resistance test, confirming that they have excellent weather resistance. [Explanation of symbols]
[0103] 10 Near-infrared shielding materials 11 Near-infrared shielding material powder 12 Liquid medium
Claims
1. A near-infrared shielding material powder containing a composite tungsten oxide, The composite tungsten oxide has the general formula Cs x W y O z It is expressed as In the general formula, x, y, and z satisfy the relationships of 0.32≦x / y≦0.35 and 2.5≦z / y≦2.8, CIE-L * a * b * In the color system, a * ≦0 and b * A near-infrared shielding material powder having a viscosity of ≦-10.
2. 2. The near-infrared shielding material powder according to claim 1, wherein the composite tungsten oxide is composed only of hexagonal crystals.
3. A method for producing a near-infrared shielding material powder containing a composite tungsten oxide, comprising the steps of: A mixing step of mixing a tungsten raw material containing tungsten and a cesium raw material containing cesium to obtain a mixture; A heat treatment step of heat treating the mixture in a reducing atmosphere at a heat treatment temperature of more than 400° C. and less than 500° C., In the mixing step, the tungsten raw material and the cesium raw material are mixed so that a ratio of an amount of substance of elemental cesium to elemental tungsten contained in the mixture is 0.32 or more and 0.35 or less; The method for producing a near-infrared shielding material powder, wherein the mixture has an average particle size of 500 nm or less.
4. A liquid medium; The near-infrared shielding material powder according to claim 1 or 2 contained in the liquid medium, A near-infrared shielding material having a haze value of 0.3% or less when the total light absorption rate is 80%.
Citation Information
Patent Citations
Ultraviolet ray- and near-infrared light-shielding dispersion, and ultraviolet ray- and near-infrared light-shielding item
JP2008231164A
Heat ray shielding fine particle and heat ray shielding fine particle dispersion
JP2017105705A
Production method of composite tungsten oxide particle
JP2019142730A
Infrared shielding material microparticle dispersion, infrared shield, process for producing infrared shielding material microparticle, and infrared shielding material microparticle
WO2005037932A1
Sheet for heat insulation
JP1997107815A