Scarfing method and scarfing device
The method stabilizes the cutting reaction in steel materials by using a controlled flow rate ratio of combustible gas and oxygen, achieving a thin cutting thickness and reducing defects in high-grade steel materials.
Patent Information
- Application Number
- JP2023054366
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Existing melt cutting methods for steel materials face issues with turbulence and instability due to excessive oxygen flow, leading to inadequate control of cutting thickness and yield reduction, particularly in high-grade steel materials.
A method and apparatus that utilize a preheating step with a controlled flow rate ratio of combustible gas and oxygen, followed by a cutting process with a shielding gas containing combustible gas and oxygen, where the calorific value ratio exceeds 0.11, to stabilize the cutting reaction and achieve a thin cutting thickness.
Stabilizes the cutting reaction, allowing for a minimum cutting thickness of 2 mm or less, reducing defects and improving yield by utilizing the combustion heat of the shielding gas to maintain oxygen concentration and suppress turbulence.
Smart Images

Figure 2024142251000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method and an apparatus for laser cutting. [Background technology]
[0002] Patent Document 1 describes a method for thermally cutting a steel material by thermally cutting the surface of the steel material, characterized in that in a front shielding gas, the flow rate ratio O / G of oxygen (O) to combustible gas (G) is set so that the amount of oxygen is greater than the theoretical amount of oxygen required for complete combustion of the combustible gas.
[0003] Patent Document 2 describes that in the preheating step before surface cutting, the flow rate ratio of oxygen gas to propane gas is controlled to satisfy the range of 5.0±0.5. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-041422 [Patent Document 2] JP 2009-233689 A Summary of the Invention [Problem to be solved by the invention]
[0005] In the steel manufacturing process, the surface of the steel may be treated by shave. For example, cracks on the surface of the steel are quality defects and must be removed. In particular, in high-grade steel and automotive steel sheets, which place importance on surface quality, it is required to remove surface cracks. In addition, surface defects such as iron oxide on the surface of the slab 1A, inclusions and casting powder that have become embedded in the surface layer during casting, or air bubble marks are removed by surface treatment. When shave is applied to the steel manufacturing process as a surface treatment method, it is required to achieve a thin shave thickness in order to avoid a decrease in yield.
[0006] However, in the technology described in Patent Document 1, the flow rate ratio is set so that the amount of oxygen in the front shielding gas used in the thermal cutting is greater than the theoretical amount of oxygen required to completely combust the combustible gas. In this case, the front shielding gas may cause disturbances in the flow of oxygen for thermal cutting due to an increase in the amount of material after the reaction and an expansion of the gas volume due to an excessive temperature rise, which may adversely affect the thermal cutting. In addition, in the technology described in Patent Document 2, the flow rate ratio of propane gas and oxygen gas in the preheating process is taken into consideration, but the flow rate ratio in the shielding gas in the thermal cutting process is not taken into consideration.
[0007] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a cutting method and a cutting device that can achieve a thin cutting thickness. [Means for solving the problem]
[0008] In order to solve the above problems, according to one aspect of the present invention, there is provided a method for laser cutting, which includes a preheating process in which combustible gas and oxygen are sprayed onto a surface of a steel material to cause combustion, and a laser cutting process in which oxygen for laser cutting is sprayed onto the surface of the steel material while transporting the steel material and laser cutting the surface of the transported steel material, wherein in the laser cutting process, a shielding gas containing the combustible gas and the oxygen is sprayed forward in the direction of laser cutting of a hot point formed by an oxidation reaction of the oxygen for laser cutting with the steel material, and wherein the heat ratio κ in the shielding gas, calculated by equation (1), satisfies the following relationship (2). κ = heat of combustion of combustible gas / heat of formation of FeO (1) κ>0.11 (2)
[0009] The flow rate of the oxygen contained in the shielding gas may be smaller than the flow rate of oxygen required for complete combustion of the combustible gas, and the flow rate ratio of the combustible gas to the oxygen may be a flow rate ratio at which the combustible gas continues to burn.
[0010] When the target area is removed by thermal cutting in the thermal cutting step, the target area may be an area that is 2 mm or less from the surface of the steel material in a thickness direction.
[0011] In the above-mentioned surface cutting step, when the target area is removed by surface cutting, the conveying speed of the above-mentioned steel material may be set to 10 m / min or less.
[0012] The steel material may be a steel material to be subjected to hot rolling.
[0013] In order to solve the above problem, according to another aspect of the present invention, there is provided a thermal cutting device comprising: an oxygen for thermal cutting jetting section that jets oxygen for thermal cutting; and a shielding gas jetting section that jets a shielding gas containing a combustible gas and oxygen, forward of the jet of oxygen for thermal cutting in the direction of thermal cutting progress; and in the shielding gas, the heat ratio κ calculated by equation (3) satisfies the following relationship (4). κ = heat of combustion of combustible gas / heat of formation of FeO (3) κ>0.11 (4) Effect of the Invention
[0014] As described above, according to the present invention, a cutting method and a cutting device capable of achieving a thin cutting thickness are provided. [Brief description of the drawings]
[0015] [Figure 1] 1 is a schematic diagram showing an example of a schematic configuration of hot rolling equipment according to a first embodiment of the present invention. [Diagram 2] 1 is a schematic diagram showing an example of a schematic configuration of a laser cutting apparatus according to a first embodiment of the present invention. [Diagram 3] 1 is a graph showing an example of the relationship between a cutting speed and a cutting thickness. [Figure 4] FIG. 2 is a schematic diagram showing an example of a state of thermal cutting according to the first embodiment of the present invention. [Diagram 5] 4 is a graph showing an example of a relationship between a heat amount ratio κ and a maximum thermal cutting rate acceleration amount η according to the first embodiment of the present invention. [Figure 6] 1 is a graph showing an example of a relationship between a heat amount ratio κ and a minimum cutting thickness change amount ξ according to a first embodiment of the present invention. [Figure 7] FIG. 2 is a schematic diagram showing an example of a target region according to the first embodiment of the present invention. [Figure 8] 2 is a flowchart showing an example of a thermal cutting method according to the first embodiment of the present invention. [Figure 9] FIG. 13 is a schematic diagram showing an example of a state of thermal cutting according to a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In this specification and the drawings, components having substantially the same functional configurations are designated by the same reference numerals, and duplicated explanations will be omitted.
[0017] <First embodiment> First, a schematic configuration of a hot rolling facility 10 according to a first embodiment of the present invention will be described with reference to Fig. 1. Fig. 1 is a diagram showing a schematic configuration of the hot rolling facility 10.
[0018] As shown in FIG. 1 as an example, the hot rolling equipment 10 is equipment for hot rolling a steel material 1. The hot rolling equipment 10 includes a heating furnace 20, a slag cutting device 30, a descaling device 40, a rough rolling device 50, and a finish rolling device 60. The heating furnace 20 heats the steel material 1 (for example, a slab 1A) obtained by cutting the steel material 1 discharged from the continuous casting machine 11 to a predetermined length to a predetermined temperature. The slab 1A is heated by the heating furnace 20 while being transported by a transport roll 22. Here, the steel material 1 is a steel material containing Cu, for example, a steel material containing 0.15 wt% or more of Cu, particularly a steel material containing 0.25 wt% or more of Cu. Note that, although the slab 1A is given as an example of the steel material 1 here, this is merely an example, and the steel material 1 may be a billet.
[0019] The slag cutting device 30 performs slag cutting on the slab 1A discharged from the heating furnace 20 to remove the surface portion of the slab 1A. The slag cutting device 30 will be described in detail later. The slag cutting device 30 is located downstream of the heating furnace 20 in the conveying direction of the slab 1A. The slag cutting device 30 is also located upstream of the descaling device 40. More specifically, the slag cutting device 30 is located downstream of the heating furnace 20 and upstream of the vertical rolls 24 that roll the slab 1A heated in the heating furnace 20 in the width direction. In this specification, the term "removal" includes complete removal, and refers to removal in the sense of insufficient removal within a range generally acceptable in the technical field to which the present invention belongs, and including insufficient removal to a degree that does not go against the spirit of the present invention.
[0020] The descaling device 40 removes scale (i.e., oxide film) formed on the surface of the slab 1A before rough rolling by the rough rolling device 50. The descaling device 40 removes scale by spraying a fluid (e.g., cooling water) from a nozzle 42 onto the slab 1A. That is, the descaling device 40 sprays cooling water W, which is supplied from a cooling water tank (not shown) and has a predetermined water pressure using a pump (not shown), onto the slab 1A from the nozzle 42. The descaling device 40 removes scale from the surface of the slab 1A, and the temperature of the surface of the slab 1A is set to 1100°C or less by heat extraction by the cooling water. Here, the surface temperature of the slab 1A after scale removal by the descaling device 40 (e.g., the side surface in the width direction of the slab 1A) is measured by a radiation thermometer.
[0021] The rough rolling device 50 performs rough rolling on the slab 1A to thin it down to a predetermined thickness. Specifically, the rough rolling device 50 rolls the slab 1A, which has been rolled in the width direction by the vertical rolls 24, from above and below to form a rough bar 1B. In the example shown in FIG. 1, the rough rolling device 50 includes four rolling mills 51-54. The rough rolling device 50 sandwiches the slab 1A between the rolls from above and below and continuously rolls it using the rolling mills 51-54. In the rough rolling device 50, the slab 1A is thinned down to a plate thickness of, for example, about 25-50 mm, and formed into a rough bar 1B.
[0022] The finishing rolling device 60 continuously hot-finish-rolls the rough bar 1B to a predetermined thickness. Specifically, the rough bar 1B, which has been reheated by the rough bar heating device 62 and transported, is finish-rolled to a thickness of about several mm (for example, 1 to 2 mm). These finishing rolling devices 60 pass the rough bar 1B through gaps between finishing rolling rolls 64 arranged vertically in a straight line across 6 to 7 stands, and gradually roll it down. The steel strip 1C obtained by finish-rolling to a predetermined thickness by this finishing rolling device 60 is sent to a cooling device 70. Note that, here, an example of the finishing rolling device 60 having 6 to 7 stands is shown, but this is merely an example, and the finishing rolling device 60 may have 5 stands.
[0023] The cooling device 70 cools the steel strip 1C after the finish rolling with cooling water W. The cooling device 70 is, for example, a pipe laminar nozzle type cooling device. The steel strip 1C cooled by the cooling device 70 is wound into a coil by a winding device 80 and transported from the hot rolling equipment 10 to the next process as a hot rolled coil 1D.
[0024] In the hot rolling equipment 10 according to the present embodiment, the surface of the slab 1A is removed by the scavenging device 30. As shown in FIG. 2 as an example, the scavenging device 30 has a scarfer unit 31 arranged to face the surface of the steel material 1. The scarfer unit 31 includes a preheating gas jetting section 34 and a scavenging oxygen jetting section 36. In the preheating process, the preheating gas jetting section 34 jets preheating oxygen 32 and combustible gas 33. In the scavenging process, the preheating gas jetting section 34 jets a front shielding gas 35. That is, in the scavenging process, the preheating gas jetting section 34 functions as a shielding gas jetting section. The scavenging oxygen jetting section 36 jets scavenging oxygen 37.
[0025] As shown in Figure 2, the flow of oxygen for cutting 37 ejected from the oxygen for cutting ejection section 36 is positioned so as to collide forward in the conveying direction Y of the steel material 1 relative to the flow of preheating oxygen 32 and combustible gas 33 ejected from the preheating gas ejection section 34.
[0026] In the sintering device 30, first, a preheating process is performed as shown on the left side of Fig. 2. In the preheating process, preheating oxygen 32 and combustible gas 33 are ejected from a preheating gas ejection part 34 of the scarfer unit 31 toward the surface of the steel material 1, and the combustible gas 33 is burned. Then, a part of the surface of the steel material 1 is melted by the heat of the burning combustible gas 33, and a basin portion 1E is formed.
[0027] The length of the well portion 1E formed on the surface of the steel material 1 along the conveying direction Y is set to, for example, within a range of about 20 mm to 30 mm.
[0028] Next, as shown on the right side of FIG. 2, a laser cutting process is performed. In the laser cutting process, laser cutting oxygen 37 is ejected from the laser cutting oxygen ejection part 36 of the scarfer unit 31 toward the surface of the steel material 1, and the steel material 1 on which the basin part 1E is formed is transported in the transport direction Y. At this time, a front shielding gas 35 is ejected from the preheating gas ejection part 34. The front shielding gas 35 contains a combustible gas 35B and oxygen 35A. The flow of the front shielding gas 35 is located on the front side of the laser cutting oxygen 37 in the laser cutting advance direction (i.e., the opposite direction to the Y direction, which is the transport direction). The front shielding gas 35 is ejected as a protective gas for maintaining the oxygen concentration of the laser cutting oxygen 37. In addition, a rear shielding gas 38 is ejected on the rear side of the laser cutting oxygen 37 in the laser cutting advance direction. The rear shielding gas 38 is ejected as a protective gas for maintaining the oxygen concentration of the laser cutting oxygen 37. The rear shielding gas 38 is a combustible gas, for example, LPG. In other words, the front shielding gas 35 and the rear shielding gas 38 suppress the inflow of air (e.g., mainly nitrogen) from the outside into the oxygen for welding 37, or the outflow of oxygen to the outside, thereby suppressing the change in the oxygen concentration of the oxygen for welding 37.
[0029] In the laser cutting process, the jet of laser cutting oxygen 37 jetted from the laser cutting oxygen jetting portion 36 collides with the molten iron in the basin 1E of the steel material 1 being transported, causing an oxidation reaction between the molten iron and the laser cutting oxygen 37. The surface of the steel material 1 melts one after another due to the heat of this oxidation reaction, and the surface of the steel material 1 is laser cut. That is, the rear side of the basin 1E in the transport direction Y is laser cut by the heat of the oxidation reaction. In this way, the surface of the slab 1A after it has been heated in the heating furnace 20 is laser cut by the laser cutting device 30.
[0030] Incidentally, when performing a thin swarf cutting on the steel material 1, it is possible to consider a method of increasing the conveying speed of the steel material 1 during swarf cutting (hereinafter also simply referred to as the "swarf cutting speed") or decreasing the pressure of the swarf cutting oxygen 37. In general, when the swarf cutting speed is increased, the swarf cutting thickness becomes thinner in inverse proportion to the speed. As an example, as shown in FIG. 3, at a swarf cutting speed of 15 m / min or more, swarf cutting of less than 2.0 mm can be achieved (see high pressure (e.g., 0.76 MPa) in the figure). However, when the swarf cutting speed is further increased to 20 m / min or more, the swarf cutting reaction is interrupted, the swarf cutting area is not continuous, and intermittent swarf cutting defects (so-called tiger cutting phenomenon) occur. Thus, the swarf cutting phenomenon has a swarf cutting limit (see dotted line in FIG. 3) at which swarf cutting suddenly becomes impossible when a certain swarf cutting speed is exceeded. On the other hand, when the pressure of the oxygen for cutting 37 is lowered (see low pressure (e.g., 0.49 MPa) in the figure), the cutting thickness can be reduced at a low speed, but the cutting limit at which the cutting reaction stops also shifts to a low speed, and as a result, the achievable cutting thickness becomes thicker than when the pressure of the oxygen for cutting 37 is increased, and a cutting thickness of less than 2.0 mm cannot be achieved. Therefore, when there is a mechanical constraint on the cutting speed (e.g., an upper limit on the conveying speed), it is difficult to achieve a cutting thickness below the cutting limit even if the cutting conditions are adjusted, such as by lowering the oxygen pressure.
[0031] Therefore, in order to reduce the cutting thickness below the cutting limit, the inventors first conducted a detailed study on the mechanism by which cutting is interrupted when the cutting speed is increased. As a result, they came to the conclusion that, in order for cutting to proceed stably, it is necessary to raise the temperature to the ignition temperature of iron in the preheating zone HR so that the cutting reaction (e.g., Fe+1 / 2O2=FeO) proceeds reliably in the cutting zone WR, as shown in Fig. 4 as an example.
[0032] As described above, the front shielding gas 35 is injected as a protective gas for maintaining the oxygen concentration of the oxygen for cutting 37. The inventors have come up with the idea of making the front shielding gas 35 function as a gas that assists the progress of the cutting reaction by utilizing the combustion heat of the front shielding gas 35, in addition to the function of the front shielding gas 35 as a protective gas.
[0033] In order to increase the heat quantity of the front shielding gas 35, it is generally considered to set it close to complete combustion. For complete combustion, for example, when the combustible gas 35B is propane, five times the amount of oxygen is required in terms of substance compared to the propane gas. Furthermore, as a result of the combustion reaction (C3H8+5O2=3CO2+4H2O), the substance amount of the generated gas increases by 1.4 times. And, because the volume of the generated gas expands by nearly 10 times due to the temperature rise accompanying combustion, the momentum of the front shielding gas 35 increases excessively. Such expansion of the front shielding gas 35 may disturb the flow of the oxygen 37 for cutting, and may affect the stable progress of the cutting.
[0034] Therefore, by keeping the ratio of the oxygen flow rate to the combustible gas 35B in the front shielding gas 35 as small as possible, the combustion heat of the front shielding gas 35 can be made greater than when the flow rate ratio is set to a value that completely combusts the combustible gas 35B.
[0035] The flow rate of oxygen 35A contained in the front shielding gas 35 is set to be smaller than the amount of oxygen required for complete combustion of the combustible gas 35B. Here, complete combustion refers to the complete oxidation of the combustible gas by the combustion reaction. For example, in the case of propane gas, it refers to the progress of the combustion reaction (C3H8+5O2=3CO2+4H2O). Note that "complete" refers to completeness in the sense that it is within the range of error permitted in the technical field to which this embodiment belongs and includes an error that does not go against the spirit of the technology of the present disclosure.
[0036] Also, in the front shield gas 35, the flow rate ratio of the combustible gas 35B to the oxygen 35A is set to a flow rate ratio at which the combustible gas 35B can continue to burn. This is because if there is no oxygen 35A at all, the combustion reaction of the combustible gas 35B will not continue. That is, the flow rate ratio of the combustible gas 35B to the oxygen 35A is set to a flow rate ratio such that the combustible gas 35B does not remain as a reactant. Here, the flow rate ratio at which the combustion reaction can continue is expressed by the explosion limit. For example, in the case of propane gas, in a stationary state (i.e., when the flow velocities of the propane gas and oxygen are sufficiently small), the flow rate ratio at the explosion limit is 0.75 < O / G < 43. However, when the flow velocity of the front shield gas 35 increases, the lower limit of the flow rate ratio increases. Therefore, in order to actually stably ignite the front shield gas 35, the flow rate ratio is set to 2.0 ≤ O / G, and more oxygen is required compared to the stationary state. In this case, the upper limit of O / G can be appropriately set within the range that does not completely combust the combustible gas 35B and within the range of the flow rate ratio required to melt the steel material 1. For example, it is set to O / G < 5.0.
[0037] Also, if there is no oxygen 35A in the front shield gas 35 at all, the protection function will decrease due to the overall flow rate decrease of the front shield gas 35, and furthermore, the combustion of the front shield gas 35 will not continue, so the function of assisting melting by the combustion heat will be lost.
[0038] In order to further examine the auxiliary function of the combustion heat of the front shield gas 35 on the melting reaction, the inventors came up with the idea of comparing the combustion heat of the front shield gas 35 with the heat of formation of FeO in the melting reaction. In this case, the heat of formation of FeO was taken as the heat of formation of FeO when it was considered that all the Fe melted as the maximum value of the combustion heat of the molten iron changed to FeO. That is, the heat of formation of FeO can be expressed by the following formula (1).
[0039] Heat of formation of FeO = hWV s ρ·64 (Mcal / kmol) / 55.8 (kg / kmol) ···(1) Here, h: Melting thickness [m] W: Cutting width [m] V s : Cutting speed [m / h] ρ: Density of steel [kg / m 3 ] Heat per mole of FeO formation reaction: 64 (Mcal / kmol) Molecular weight of FeO: 55.8 (kg / kmol)
[0040] In addition, the calorific value of the flammable gas 35B can be expressed by the following formula (2) since the flammable gas 35B is, for example, LPG (Liquefied Petroleum Gas) containing propane as a main component. Calorific value of LPG = Q LPG 20.78Mcal / m 3 (2) Here, Q LPG : LPG flow rate [m 3 / h]
[0041] The ratio κ (kappa) of the calorific value of LPG to the calorific value of FeO formation can be expressed as the following formula (3). κ = LPG combustion heat ÷ FeO formation heat (3)
[0042] The maximum cutting speed acceleration amount η expressed by the following formula (4) is used as an index showing how much the cutting is stabilized by the combustion heat of the front shield gas 35. The maximum cutting speed acceleration amount η is the degree to which the maximum cutting speed is improved.
[0043] η=V max / V max,0 (4) Here, V max Maximum cutting speed when increasing the amount of flammable gas 35B in the front shield gas 35 V max,0 Maximum cutting speed when the minimum flow rate of front shield gas is 35 for stable cutting
[0044] As described above, the front shielding gas 35 is necessary to maintain the oxygen concentration of the oxygen for cutting 37. In the front shielding gas 35 at the minimum flow rate at which the oxygen concentration of the oxygen for cutting 37 is maintained and cutting is stable, the ratio κ of the LPG combustion heat quantity to the FeO formation heat quantity is approximately 0.05. In this case, the maximum cutting speed acceleration amount η is 1.
[0045] As an example, as shown in Figure 5, in the relationship between the heat ratio κ and the maximum cutting speed acceleration η, there is a tendency that the maximum cutting speed acceleration η increases as the heat ratio κ increases. When the heat ratio κ is 0.36, the maximum cutting speed acceleration η is 2, indicating that the degree of increase in the maximum cutting speed due to combustible gas 35B is doubled. In addition, in the relationship between the heat ratio κ and the maximum cutting speed acceleration η, the increase in the cutting speed with respect to the heat ratio κ is roughly linear. At the intersection of the approximation line and the line with η = 1, the heat ratio κ = 0.11. Therefore, it can be seen that when κ > 0.11, η > 1.0, and the maximum cutting speed increases.
[0046] Moreover, the upper limit of the heat ratio κ may be set so that κ≦0.4. In order to increase the heat ratio κ, for example, the flow rate of the combustible gas 35B is increased. As a result, when the heat ratio κ becomes larger than 0.4, the flow of the front shielding gas 35 containing the combustible gas 35B may obstruct the flow of the oxygen 37 for laser cutting. This may cause the laser cutting to become unstable. Therefore, the heat ratio κ may be set so that κ≦0.4.
[0047] An increase in the maximum cutting speed means that the stability of the cutting is improved. In other words, in the steel manufacturing process, poor cutting (for example, the phenomenon in which the cutting portion is interrupted) is less likely to occur. On the other hand, by increasing the cutting speed (i.e., the conveying speed of the steel material to be cut) by the amount of increase in the maximum cutting speed, the cutting thickness becomes thinner. Therefore, the amount by which the cutting thickness becomes thinner by increasing the combustion heat of the combustible gas 35B of the front shielding gas 35 compared to the minimum cutting thickness when cutting with the front shielding gas 35 at the minimum flow rate is expressed by ξ as shown in the following formula (5).
[0048] ξ=h Vmax / h Vmax,0 (5) Here, ξ: Minimum change in thickness after machining h Vmax :V max Thickness of shavings in the case h Vmax,0 :V max,0 Thickness of shavings in the case
[0049] As an example, in the relationship between the heat ratio κ and the minimum swarf-cutting thickness change ξ, as shown in Fig. 6, the minimum swarf-cutting thickness change ξ decreases to 0.66. In other words, by using the combustion heat of the combustible gas 35B of the front shielding gas 35, the swarf-cutting thickness can be reduced by, for example, up to 34%.
[0050] In this way, the combustion heat of the combustible gas 35B in the front shielding gas 35 is utilized to stably progress the cutting reaction. Furthermore, the stable progress of the cutting reaction can reduce the minimum cutting thickness. That is, cutting can be achieved below the cutting limit when the combustion heat of the combustible gas 35B in the front shielding gas 35 is not utilized.
[0051] In recent years, iron sources other than iron ore have come to be used in order to reduce carbon dioxide emissions in the steel manufacturing process. For example, increasing the proportion of scrap iron used as the iron source has been considered.
[0052] However, when scrap iron is used as an iron source, surface defects may occur during the steel manufacturing process due to copper (Cu) contained in the scrap iron. For example, during the hot rolling process, red embrittlement cracking occurs due to the concentration of Cu on the surface of the steel, resulting in a decrease in the surface quality of the steel. For this reason, it is difficult to increase the proportion of scrap iron containing Cu in the iron source, which is an obstacle to realizing an environmentally friendly steel manufacturing process.
[0053] Therefore, the Cu-enriched layer on the surface of the slab 1A is removed after heating in the heating furnace 20 in the hot rolling. That is, in the thermal history of the hot rolling, after the steel material 1 leaves the heating furnace 20 and becomes 1000°C or less in the rough rolling process, it is not heated to 1000°C or more again. Therefore, if the Cu-enriched layer is removed after heating in the heating furnace 20, the generation of scale in the subsequent processes is suppressed. As a result, the Cu concentration phenomenon is suppressed, and red embrittlement cracking is also suppressed.
[0054] The Cu-enriched layer is formed only in the surface layer of less than 2 mm, and red embrittlement cracking can be suppressed by performing laser cutting to a thickness of at most about 2 mm, or to a thickness of 1.0 mm or less depending on the Cu content or heating conditions.
[0055] 7, the laser cutting device 30 removes a target area T that is an area including a Cu-enriched layer R. Here, the target area T is a range of a predetermined distance from the surface of the steel material 1 (i.e., the surface of the scale S) in the thickness direction t of the steel material 1. The predetermined distance is, for example, greater than 0 mm and equal to or less than 3 mm, preferably greater than 0 mm and equal to or less than 2 mm, and more preferably greater than 0 mm and equal to or less than 1 mm.
[0056] When the steel material 1 is a rough bar 1B, the thickness of the steel material 1 is, for example, about 25 to 50 mm. Therefore, by removing a region that is 1 mm or less away from the surface of the steel material 1 as the target region T, it is possible to suppress a reduction in the thickness of the steel material 1 and improve the yield.
[0057] 7 shows an example in which one surface in the thickness direction of the steel material 1 is scarified, but the scarifying device 30 according to this embodiment also scarifies other surfaces in the thickness direction of the steel material 1. In this case, the scarifying device 30 includes scarfer units 31 at positions facing each of the one surface and the other surface of the steel material 1.
[0058] The target region T including the Cu-enriched layer R is removed by thermal cutting, and thus the cracks C present at the grain boundaries GB are removed. As a result, red embrittlement cracking on the surface of the steel material 1 is suppressed.
[0059] As described above, in this embodiment, the slag cutting reaction is stably carried out by utilizing the combustion heat of the combustible gas 35B in the front shielding gas 35. Furthermore, the slag cutting reaction is stably carried out, so that the minimum slag cutting thickness can be reduced. That is, slag cutting can be carried out at a thickness equal to or less than the slag cutting limit when the combustion heat of the combustible gas 35B in the front shielding gas 35 is not utilized. This allows stably carrying out slag cutting of 2 mm or less, preferably 1 mm or less, when removing the target region T, which is a region including the Cu-enriched layer R present on the surface of the steel material 1.
[0060] In addition, in hot rolling equipment, transportation may be performed at a low speed of 10 m / min or less in some parts. In this case, if the cutting is performed under conditions that do not utilize the combustion heat of the combustible gas 35B in the front shielding gas 35, it is difficult to perform the cutting stably at a cutting thickness of 2 mm or less due to the cutting limit (see FIG. 3). However, in this embodiment, the cutting reaction is stably advanced by utilizing the combustion heat of the combustible gas 35B in the front shielding gas 35. Furthermore, the stable progress of the cutting reaction allows the minimum cutting thickness to be reduced, and stable cutting is achieved at a cutting thickness of 2 mm or less.
[0061] Next, the thermal cutting method according to this embodiment will be described with reference to Fig. 8. Fig. 8 is a flow chart for explaining the thermal cutting method according to this embodiment. As shown in Fig. 8, first, in step ST10, combustible gas 33 and preheating oxygen 32 are sprayed onto the surface of the steel material 1 and combusted, thereby preheating the surface of the steel material 1. After the process of step ST10 is performed, the thermal cutting method proceeds to step ST12.
[0062] In step ST12, the surface of the steel material 1 preheated in step ST10 is sprayed with oxygen for cutting 37, and the steel material 1 is transported. As a result, the surface of the transported steel material 1 is cut by the heat of oxidation reaction between the oxygen for cutting 37 and the steel material 1. In this case, a front shielding gas 35 containing a combustible gas 35B and oxygen 35A is ejected, and the heat ratio κ calculated by the above formula (3) is set to κ>0.11 in the front shielding gas 35. After the process of step ST12 is executed, the method for cutting according to this embodiment is terminated.
[0063] As described above, the method for the laser cutting according to the present embodiment includes a step of preheating the surface of the steel material 1 and a step of laser cutting the surface of the steel material 1 by the heat of oxidation reaction between the oxygen for laser cutting 37 and the steel material 1. In the laser cutting step, a front shielding gas 35 containing a combustible gas 35B and oxygen 35A is sprayed. In the front shielding gas 35, the ratio κ of the heat of heat generated by the combustible gas 35B to the heat of heat generated by FeO is set to be κ>0.11. This allows the laser cutting reaction to proceed stably in the front shielding gas 35 by utilizing the combustion heat of the combustible gas 35B. Furthermore, the minimum laser cutting thickness can be reduced by the stable progress of the laser cutting reaction. That is, laser cutting can be achieved below the laser cutting limit when the combustion heat of the combustible gas 35B in the front shielding gas 35 is not utilized.
[0064] In the method for the thermal cutting according to the present embodiment, the flow rate of the oxygen 35A contained in the front shielding gas 35 is set to be smaller than the amount of oxygen required for complete combustion of the combustible gas 35B. In addition, in the front shielding gas 35, the flow rate ratio of the combustible gas 35B to the oxygen 35A is set to a flow rate ratio that allows the combustible gas 35B to continue to burn. This makes it possible to continuously cause the combustion reaction of the front shielding gas 35 while suppressing the influence on the stable progress of the thermal cutting caused by the expansion of the front shielding gas 35 accompanying complete combustion. As a result, the thermal cutting reaction proceeds stably, and the minimum thermal cutting thickness is reduced.
[0065] Moreover, in the method for thermal cutting according to this embodiment, a target region T of 2 mm or less from the surface of the steel material 1 in the thickness direction t is removed by thermal cutting. Most surface defects of the steel material 1 generally exist in a target region T of 2 mm or less from the surface. For example, the Cu-enriched layer R is generated only in a surface layer less than 2 mm deep, and red embrittlement cracking can be suppressed by performing thermal cutting to a thickness of at most about 2 mm. Furthermore, by setting the target region T to be removed by thermal cutting to 2 mm or less, the yield of the steel material 1 can be improved.
[0066] In addition, in the method for removing the target region T by the cutting, the conveying speed of the steel material 1 is set to 10 m / min or less. Since there is a cutting limit in cutting at a low speed, it is difficult to perform cutting stably at a cutting thickness of 2 mm or less (see FIG. 3). In this configuration, the combustion heat of the combustible gas 35B is used in the front shielding gas 35 to stably advance the cutting reaction, thereby reducing the minimum cutting thickness and realizing stable cutting at a cutting thickness of 2 mm or less.
[0067] In the method for melt cutting according to the present embodiment, the steel material 1 is a steel material to be hot-rolled. In the steel material 1 in the hot rolling process, a Cu-enriched layer R is generated on the surface layer, which generates red embrittlement cracks during rolling. In this configuration, the melt cutting reaction proceeds stably by utilizing the combustion heat of the combustible gas 35B in the forward shielding gas 35, so that the minimum melt cutting thickness can be reduced and stable melt cutting of the Cu-enriched layer R is realized.
[0068] (Modification) In the above embodiment, the injection direction of the front shielding gas 35 and the injection direction of the oxygen for cutting 37 are the same, but this is merely an example. For example, as shown in Fig. 9, the injection direction of the front shielding gas 35 may be set at an angle so as to intersect with the injection direction of the oxygen for cutting 37.
[0069] In this case, the effect on the stable progress of the thermal cutting when the combustible gas 35B in the front shielding gas 35 is set to be close to complete combustion is greater than that in the above embodiment. That is, the front shielding gas 35 expands due to complete combustion of the combustible gas 35B, and the momentum increases excessively, which affects the injection of the oxygen for thermal cutting 37. This makes the thermal cutting reaction more likely to become unstable.
[0070] In this modification, similarly to the above embodiment, a front shielding gas 35 containing a combustible gas 35B and oxygen 35A is injected, and the ratio κ of the heat generated by the combustible gas 35B to the heat generated by FeO is set to be κ>0.11. This allows the front shielding gas 35 to utilize the combustion heat of the combustible gas 35B to stably progress the cutting reaction.
[0071] In the above embodiment, an example in which the slag cutting by the slag cutting device 30 is performed between the heating process by the heating furnace 20 and the rough rolling process in the hot rolling process has been described, but this is merely one example. For example, the slag cutting by the slag cutting device 30 may be performed during the rough rolling process. Specifically, the slag cutting device 30 is provided between each of the rolling mills that form the rough rolling device 50. In addition, for example, the slag cutting of the steel material 1 by the slag cutting device 30 may be performed after rough rolling and before finish rolling, or may be performed during the finish rolling process.
[0072] In the above embodiment, an example in which the slag cutting is performed by the slag cutting device 30 in the hot rolling process has been described, but this is merely one example. The slag cutting method according to this embodiment may be applied to a steelmaking process or before a heating furnace in a hot rolling process. Furthermore, the slag cutting method according to this embodiment does not have to be applied to a manufacturing line for the steel material 1, and the steel material 1 to be slag cut may be a steel pipe or an H-beam instead of a steel strip. EXAMPLES
[0073] In order to evaluate the performance of the thermal cutting method according to the present invention, a thermal cutting experiment was carried out to confirm whether the thermal cutting thickness was changed by the combustion heat of the front shield gas 35.
[0074] As a comparative example, the heat ratio κ was set to 0.05 at the minimum flow rate of the front shielding gas 35. Also, as an example, the heat ratio κ of the front shielding gas 35 was increased.
[0075] The heat of formation of FeO was calculated from the thickness of the scarification using the above formula (1). In addition, propane gas was used as the combustible gas 35B, and the heat of combustion of the combustible gas 35B was calculated using the above formula (2). The heat ratio κ was calculated using the above formula (3).
[0076] The minimum cut thickness change amount ξ was calculated from the cut thickness of the comparative example and the cut thickness of the example using the above formula (5). Therefore, the minimum cut thickness change amount ξ in the comparative example is 1.0.
[0077] The unit distance H was varied as a cutting condition. The oxygen pressure for cutting was the same for all cases. Only the center of the test steel plate width was cut, and the cut thickness was measured by measuring the depression of the cut area relative to the uncut area using a laser distance meter. The cut thickness was the average value measured at 10 points in the longitudinal direction (i.e., the direction in which the cutting proceeds). The test results are shown in Table 1.
[0078] [Table 1]
[0079] As shown in Table 1, in all of the conditions of Examples 1 to 9 where the heat ratio κ is greater than 0.11, the minimum shaving thickness change amount ξ is less than 1.0, and the minimum shaving thickness is reduced compared to Comparative Examples 1 to 4. In other words, it was shown that shaving with a thinner shaving thickness is possible compared to the case where the combustion heat of the front shield gas 35 is not used.
[0080] Next, Table 2 shows the test results in which the condition of the flow rate ratio O / G of the oxygen 35A and the combustible gas 35B in the front shielding gas 35 was changed.
[0081] [Table 2]
[0082] Since propane was used as the combustible gas 35B, O / G=5.0 was the condition for complete combustion. Therefore, even if the value of κ was almost the same, it was found that the effect of reducing the minimum cutting thickness change ξ was not as great under the condition of excess oxygen compared to the complete combustion condition of O / G>5.0 in Comparative Example 5. That is, it was shown that the minimum cutting thickness change ξ can be reduced at the flow rate ratio under the condition of O / G≦5.0, which is not the complete combustion condition.
[0083] Although the preferred embodiment of the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited to the above examples. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified examples or application examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention.
[0084] In addition to the above-described embodiment, the following supplementary notes are further disclosed.
[0085] (Appendix 1) A preheating process in which combustible gas and oxygen are sprayed onto the surface of the steel material to cause combustion; a cutting process in which oxygen for cutting is blown onto a surface of the steel material while the steel material is being transported, and the surface of the transported steel material is cut; Including, In the above-mentioned thermal cutting process, a shielding gas containing the above-mentioned combustible gas and the above-mentioned oxygen is ejected toward a front side of a hot spot formed by an oxidation reaction between the above-mentioned oxygen for thermal cutting and the above-mentioned steel material in a thermal cutting proceeding direction, In the above shielding gas, the heat ratio κ calculated by the formula (A) satisfies the following relational formula (B). Melting method. κ = heat of combustion of combustible gas / heat of formation of FeO (A) κ>0.11 (B) (Appendix 2) the flow rate of the oxygen contained in the shielding gas is less than the flow rate of oxygen required for complete combustion of the combustible gas; The method for thermal cutting described in Appendix 1, wherein the flow rate ratio of the combustible gas to the oxygen is a flow rate ratio at which the combustible gas continues to burn. (Appendix 3) In the above-mentioned erosion process, when the target area is removed by erosion, The target area is an area of 2 mm or less from the surface of the steel material in the thickness direction. 3. The method of claim 1 or 2. (Appendix 4) In the above-mentioned machining process, when the target area is removed by machining, the conveying speed of the above-mentioned steel material is set to 10 m / min or less. 4. The method of claim 1, wherein the first and second electrodes are disposed on the first and second electrodes. (Appendix 5) The above steel material is a steel material to be subjected to hot rolling. 5. The method of claim 1, (Appendix 6) an oxygen jetting portion for jetting oxygen for cutting; a shielding gas jetting section for jetting a shielding gas containing a combustible gas and oxygen, the shielding gas jetting section being located forward of the jet of oxygen for the cutting in the direction of cutting; Equipped with In the above shielding gas, the heat ratio κ calculated by formula (C) satisfies the following relational formula (D). Melting equipment. κ = Heat of combustion of combustible gas / heat of formation of FeO (C) κ>0.11 (D) [Explanation of symbols]
[0086] 1 Steel material 1A Slab 1B coarse bar 1C steel strip 1D hot rolled coil 1E Bathtub 10. Hot rolling equipment 11 Continuous casting machine 20 Furnace 22 Transport roll 24 Vertical Roll 30 Cutting equipment 31 Scarfer Unit 32 Preheating oxygen 33 Flammable gases 34 Preheating gas outlet 35 Forward shielding gas 35A Oxygen 35B Flammable gases 36 Oxygen outlet for cutting 37 Oxygen for cutting 38 Rear Shielding Gas 40 Descaling device 42 Nozzle 50,50A,50B rough rolling equipment 51, 52, 53, 54 Rolling mill 60 Finishing rolling equipment 62 Rough bar heating device 64 Finishing Roll 70 Cooling device 80 Winding device R Cu enriched layer S scale T Target area W Cooling water Y Arrow t thickness direction
Claims
1. A preheating process in which combustible gas and oxygen are sprayed onto the surface of the steel material to cause combustion; a cutting process in which oxygen for cutting is blown onto the surface of the steel material while the steel material is being transported, and the surface of the transported steel material is cut; Including, In the thermal cutting process, a shielding gas containing the combustible gas and the oxygen is ejected forward in a thermal cutting advance direction of a hot spot formed by an oxidation reaction between the thermal cutting oxygen and the steel material, In the shielding gas, the heat ratio κ calculated by the formula (1) satisfies the following relational formula (2): Melting method. κ = heat of combustion of combustible gas / heat of formation of FeO (1) κ>0.11...(2)
2. a flow rate of the oxygen contained in the shielding gas is smaller than a flow rate of oxygen required for complete combustion of the combustible gas; The method of claim 1 , wherein a flow rate ratio of the combustible gas to the oxygen is a flow rate ratio at which the combustible gas continues to burn.
3. In the case where the target area is removed by erosion in the erosion process, The target area is an area of 2 mm or less in the thickness direction from the surface of the steel material. The method of claim 1 .
4. In the above-mentioned machining step, when the target area is removed by machining, the conveying speed of the steel material is set to 10 m / min or less. The method of claim 1 .
5. The steel material is a steel material to be hot rolled. The method of claim 1 .
6. an oxygen jetting portion for jetting oxygen for cutting; a shielding gas jetting section for jetting a shielding gas containing a combustible gas and oxygen, the shielding gas jetting section being located forward of the jet of oxygen for the cutting in the direction of the cutting; Equipped with In the shielding gas, the heat ratio κ calculated by the formula (3) satisfies the following relational formula (4): Melting equipment. κ = combustion heat of combustible gas / production heat of FeO (3) κ>0.11...(4)
Citation Information
Patent Citations
Novel burner of flame scarfing machine
CN202675280U
Scarfing nozzle
JP1997076060A
Steel product scarfing method
JP2021041422A
Scarfing method for steel material and scarfing device for steel material
JP2022167017A
Scarfing method for steel material and scarfing device for steel material
JP2022167018A