Connected body

The connecting body with a specific adhesive composition and conductive particle design addresses interlayer adhesion deterioration and resistance issues, ensuring durability and performance in chemical environments.

JP2024142426AActive Publication Date: 2024-10-11PANAC +2

Patent Information

Application Number
JP2023054561
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Existing connecting bodies using isotropic and anisotropic conductive adhesives face issues with interlayer adhesion deterioration over time, particularly due to chemical influences like electrolytes, and struggle to maintain low resistance values.

Method used

A connecting body comprising a first metal base material, a conductive adhesive layer with a cured product of acid-modified polyolefin resin and glycidylamine-based epoxy compound, and a second metal base material, where the adhesive layer includes conductive particles with a conductive layer on a resin core, optimized to resist chemical degradation and maintain adhesion.

Benefits of technology

The solution effectively suppresses interlayer adhesion deterioration over time and maintains low resistance values, particularly in high-temperature environments, making it suitable for applications like lithium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142426000001_ABST
    Figure 2024142426000001_ABST
Patent Text Reader

Abstract

To provide a connected body which can suppress the deterioration of interlayer adhesion with time.SOLUTION: A connected body comprises a first metal substrate, a conductive adhesive layer, and a second metal substrate in this order. The conductive adhesive layer comprises an adhesive and conductive particles having a conductive layer on the surface of a resin core. The conductive adhesive layer comprises, as the adhesive, a cured product of an acid-modified polyolefin resin having an acid value of less than 20.0 mgKOH / g and a glycidylamine-based epoxy compound.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a connector. [Background technology]

[0002] 2. Description of the Related Art As a material for electric and electronic devices, a connection body in which two conductive members are electrically connected via an adhesive layer is sometimes used. The adhesive used in the connector includes an isotropic conductive adhesive and an anisotropic conductive adhesive.

[0003] A typical example of an isotropic conductive adhesive is an adhesive that uses carbon black as a conductive agent. The isotropic conductive adhesive needs to contain a large amount of conductive agent in order to achieve electrical connection. For this reason, a connection using an isotropic conductive adhesive has a problem that interlayer adhesion is easily reduced. Also, a connection using an isotropic conductive adhesive has a problem that the resistance value cannot be sufficiently reduced.

[0004] As a connector using an anisotropic conductive adhesive, one using conductive particles having a conductive layer on the surface of a resin core has been proposed (for example, Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-182709 A Summary of the Invention [Problem to be solved by the invention]

[0006] The connection body of Patent Document 1 is expected to have improved interlayer adhesion because it does not require a large amount of conductive particles in the adhesive. However, with the connection body of Patent Document 1, the interlayer adhesion sometimes deteriorates over time.

[0007] An object of the present invention is to provide a connector in which deterioration of interlayer adhesion over time is suppressed. [Means for solving the problem]

[0008] As a result of intensive research, the present inventors have found that the cause of the deterioration of the interlayer adhesion of the connector over time is the influence of chemicals such as an electrolyte. Then, as a result of further research, the present inventors have come to solve the above problem.

[0009] The present invention provides the following [1] to [9]. [1] A connection body having a first metal substrate, a conductive adhesive layer, and a second metal substrate in this order, the conductive adhesive layer including an adhesive and conductive particles having a conductive layer on the surface of a resin core, and the adhesive including a cured product of an acid-modified polyolefin resin having an acid value of less than 20.0 mg KOH / g and a glycidyl amine-based epoxy compound. [2] The connector according to [1], wherein the glycidyl amine-based epoxy compound has an epoxy equivalent of 70 g / eq or more and 140 g / eq or less. [3] The connector according to [1] or [2], comprising 0.1 parts by mass or more and 27.5 parts by mass or less of the glycidyl amine-based epoxy compound per 100 parts by mass of the acid-modified polyolefin resin. [4] The connector according to any one of [1] to [3], wherein the acid-modified polyolefin resin has an acid value of 0.1 mgKOH / g or more and less than 15.0 mgKOH / g. [5] The connector according to any one of [1] to [4], wherein the melting point of the cured product is 60°C or higher and 115°C or lower. [6] The connection body according to any one of [1] to [5], wherein the conductive particles are contained in an amount of 0.1 parts by mass or more and 2.0 parts by mass or less per 100 parts by mass of the adhesive. [7] The connection body according to any one of [1] to [6], wherein when the average thickness of the conductive adhesive layer is defined as Tn [μm] and the average diameter of the conductive particles in the thickness direction is defined as Dn [μm], the relationship Dn / Tn is 1.00 or more. [8] The connector according to [7], wherein Dn / Tn satisfies the relationship of 1.01 or more and 1.50 or less. [9] The connector according to any one of [1] to [8], which is for a lithium ion battery. Effect of the Invention

[0010] The connection body of the present invention can suppress deterioration over time of the interlayer adhesion of the connection body. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional view showing an embodiment of a connector of the present invention. [Diagram 2] FIG. 4 is a cross-sectional view showing another embodiment of the connector of the present invention. [Diagram 3] 1A to 1C are diagrams illustrating a manufacturing process of the connection body of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the connector of the present invention will be described.

[0013] [Connector] The connector of the present invention is A first metal substrate, a conductive adhesive layer, and a second metal substrate in this order; the conductive adhesive layer includes an adhesive and conductive particles having a conductive layer on a surface of a resin core; The adhesive contains a cured product of an acid-modified polyolefin resin having an acid value of less than 20.0 mgKOH / g and a glycidylamine-based epoxy compound.

[0014] In this specification, "conductive particles having a conductive layer on the surface of a resin core" and "acid-modified polyolefin resin having an acid value of less than 20.0 mg KOH / g" may be abbreviated as "conductive particles" and "acid-modified polyolefin resin".

[0015] 1 and 2 are cross-sectional views showing an embodiment of a connector of the present invention. The connection body 100 in Figures 1 and 2 has a conductive adhesive layer 30 and a second metal substrate 20 on a first metal substrate 10, in this order. In Figures 1 and 2, the conductive adhesive layer 30 contains an adhesive 31 and conductive particles 30. In Figures 1 and 2, the first metal substrate 10 and the second metal substrate 20 are electrically connected via the conductive particles 30. In the connection body of Fig. 1, the conductive adhesive layer 30 and the second metal base 20 are in contact with each other over the entire surfaces thereof. On the other hand, in the connection body of Fig. 2, the conductive adhesive layer 30 and the second metal base 20 are not in contact with each other at all surfaces thereof. 1 and 2, the particle diameter in the thickness direction of the conductive particles 30 is smaller than the particle diameter in the width direction. This state shows that the particle diameter in the thickness direction is reduced by the pressure during lamination.

[0016] <Metal base material> The metal constituting the first metal base material and the second metal base material may be one or more selected from copper, stainless steel, brass, silver, aluminum, nickel, and the like. The metals constituting the first metal base and the second metal base may be the same type or different types. In order to improve adhesion, the first metal substrate and the second metal substrate may have their surfaces roughened or may be subjected to treatment to remove residual oil from the surfaces of the metal substrate.

[0017] The thickness of the first metal base and the second metal base is preferably 1 μm or more and 200 μm or less, more preferably 3 μm or more and 100 μm or less, and even more preferably 6 μm or more and 50 μm or less. By making the thickness 1 μm or more, the strength of the connector can be easily improved. Furthermore, by making the thickness 1 μm or more, a predetermined strength can be imparted to the first metal base material and the second metal base material, and damage to the base material when tension is applied thereto can be easily suppressed. By setting the thickness to 200 μm or less, the first metal base and the second metal base can be easily wound up, and therefore the connection body can be easily produced by roll-to-roll production.

[0018] <Conductive adhesive layer> The conductive adhesive layer includes an adhesive and conductive particles having a conductive layer on a surface of a resin core.

[0019] "glue" The connector of the present invention is required to contain, as an adhesive, a cured product of an acid-modified polyolefin resin having an acid value of less than 20.0 mgKOH / g and a glycidylamine-based epoxy compound. By containing the cured product as an adhesive, resistance to chemicals such as an electrolyte can be improved, so that the interlayer adhesion of the connector can be suppressed from decreasing over time. In particular, it is preferable in that it can improve resistance to high-temperature chemicals. As the electrolyte, an electrolyte for a lithium ion battery can be mentioned. As the electrolyte for a lithium ion battery, for example, an electrolyte containing lithium hexafluorophosphate and a solvent such as ethylene carbonate can be mentioned. The electrolyte for a lithium ion battery is easily heated to a high temperature. For this reason, the connector of the present invention is particularly useful as a connector for a lithium ion battery.

[0020] - Acid-modified polyolefin resin - The acid-modified polyolefin resin having an acid value of less than 20.0 mgKOH / g serves as a base agent for the adhesive. When the acid value of the acid-modified polyolefin resin exceeds 20.0 mgKOH / g, the coating liquid for the conductive adhesive layer is likely to gel, and it is difficult to form a conductive adhesive layer. When the acid value of the acid-modified polyolefin resin exceeds 20.0 mgKOH / g, the crosslinking points of the cured product of the acid-modified polyolefin resin and the glycidylamine epoxy compound are likely to increase. When the crosslinking points increase, the cured product is less likely to follow the increase and decrease in volume due to temperature change, and the interlayer adhesion of the connecting body may decrease over time.

[0021] In order to help prevent the interlayer adhesion of the connector from decreasing over time, the acid-modified polyolefin resin having an acid value of less than 20.0 mg KOH / g preferably accounts for 80 mass % or more of the total amount of the base resin, more preferably 90 mass % or more, even more preferably 95 mass % or more, and most preferably 100 mass %.

[0022] The acid value of the acid-modified polyolefin resin is preferably less than 15.0 mgKOH / g, more preferably less than 10.0 mgKOH / g, and even more preferably less than 5.0 mgKOH / g. If the acid value of the acid-modified polyolefin resin is too low, the crosslink density of the cured product may be insufficient. If the crosslink density of the cured product is insufficient, the chemical resistance may decrease, and the interlayer adhesion of the connector may not be reduced over time. Therefore, the acid value of the acid-modified polyolefin resin is preferably 0.1 mgKOH / g or more, more preferably 0.5 mgKOH / g or more, and even more preferably 0.9 mgKOH / g or more.

[0023] The acid-modified polyolefin resin may be one obtained by grafting at least one of α,β-unsaturated carboxylic acid and its acid anhydride to at least one polyolefin resin selected from polyethylene, polypropylene, propylene-α-olefin copolymer, etc. The acid-modified polyolefin resin may be produced, for example, by a radical graft reaction.

[0024] Propylene-α-olefin copolymer is a copolymer of propylene as a main component with α-olefin. As the α-olefin, for example, at least one selected from ethylene, 1-butene, 1-heptene, 1-octene, 4-methyl-1-pentene, vinyl acetate, etc. can be used. Among the α-olefins, ethylene and 1-butene are preferred. The ratio of the propylene component to the α-olefin component in the propylene-α-olefin copolymer is not limited, but the propylene component is preferably 50 mol% or more, more preferably 70 mol% or more.

[0025] Examples of the α,β-unsaturated carboxylic acid and its acid anhydride include maleic acid, itaconic acid, citraconic acid and their acid anhydrides, etc. Among these, the acid anhydrides are preferred, and maleic anhydride is more preferred.

[0026] Specific examples of acid-modified polyolefin resins include maleic anhydride-modified polypropylene, maleic anhydride-modified propylene-ethylene copolymer, maleic anhydride-modified propylene-butene copolymer, and maleic anhydride-modified propylene-ethylene-butene copolymer.

[0027] The acid-modified polyolefin resin preferably has a weight average molecular weight of 20,000 or more and 200,000 or less, more preferably 40,000 or more and 150,000 or less, and even more preferably 60,000 or more and 100,000 or less. By making the weight-average molecular weight 20,000 or more, it is possible to easily suppress a decrease in adhesive strength after immersion in an electrolyte solution. By making the weight-average molecular weight 200,000 or less, it is possible to prevent an increase in melting point, improve lamination suitability, and further to prevent an increase in viscosity, making it possible to easily improve application suitability. In this specification, the weight average molecular weight means a polystyrene equivalent value measured by gel permeation chromatography.

[0028] - Glycidylamine epoxy compounds - The glycidylamine-based epoxy compound plays a role as a curing agent that cures the base material. There are many kinds of curing agents, but by using the glycidylamine-based epoxy compound as the curing agent, the interlayer adhesion of the connector can be suppressed from decreasing over time. In addition, the glycidylamine-based epoxy compound is preferable in that it can proceed with the curing reaction at low temperature and can suppress the oxidation of the metal substrate. Examples of hardeners other than glycidylamine-based epoxy compounds include glycidyl ether-based epoxy compounds and isocyanate-based compounds. When glycidyl ether-based epoxy compounds are used, the chemical resistance is insufficient, and the deterioration of the interlayer adhesion of the connector over time cannot be suppressed. When isocyanate-based compounds are used, carbon dioxide is generated as a by-product. Since the metal substrate has low gas permeability, carbon dioxide causes defects such as swelling. In this specification, a glycidyl ether epoxy compound means a compound having a glycidyl ether group in the molecule and having no nitrogen atom in the molecule.

[0029] The glycidylamine-based epoxy compound is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and most preferably 100% by mass, based on the total amount of the curing agent.

[0030] The glycidylamine-based epoxy compound may be a compound having glycidylamine as a structural unit of the molecule. The number of glycidyl groups in one molecule of the glycidylamine-based epoxy compound may be 1 or more, but is preferably 2 or more in order to more easily suppress the deterioration of the interlayer adhesion of the connector over time. If the number of glycidyl groups in one molecule of the glycidylamine epoxy compound is too large, the initial interlayer adhesion of the connector may be weakened. Therefore, the number of glycidyl groups in one molecule of the glycidylamine epoxy compound is preferably 6 or less, more preferably 4 or less.

[0031] As the glycidylamine-based epoxy compound, a compound represented by the following general formula (1) is preferable. [ka]

[0032] In general formula (1), R is an aromatic hydrocarbon group which may have a substituent, or a saturated or unsaturated alicyclic hydrocarbon group which may have a substituent. When m is 1, the aromatic hydrocarbon group which may have a substituent includes an aryl group such as a phenyl group and a naphthyl group. When m is 1, the saturated or unsaturated alicyclic hydrocarbon group which may have a substituent includes a cycloalkyl group such as a cyclopentyl group, a cyclohexyl group, a cycloheptyl group. When m is 1, R is preferably a cycloalkyl group, more preferably a cyclohexyl group. When m is 2, examples of the aromatic hydrocarbon group which may have a substituent include arylene groups such as a phenylene group and a naphthylene group. When m is 2, examples of the saturated or unsaturated alicyclic hydrocarbon group which may have a substituent include cycloalkylene groups such as a cyclopentylene group, a cyclohexylene group, and a cycloheptylene group. When m is 2, R is preferably a cycloalkylene group, more preferably a cyclohexylene group. The substituent for R is not particularly limited, but examples thereof include an alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, a hydroxyl group, an amino group, a glycidyl group, a glycidylamino group, and a glycidyl ether group.

[0033] In general formula (1), X1 and X2 are each independently a linear alkylene group having 1 to 5 carbon atoms which may have a substituent, and preferably have 4 or less carbon atoms, more preferably 3 or less, and even more preferably 2 or less. The substituent is not particularly limited, but examples thereof include an alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, or an amino group.

[0034] In general formula (1), m is 1 or 2, and n is 1 or 2. Preferably, either m or n is 2, and more preferably, both m and n are 2.

[0035] Specific examples of the glycidylamine-based epoxy compound include 1,3-bis(diglycidylaminomethyl)cyclohexane, tetraglycidyldiaminodiphenylmethane, triglycidyl paraaminophenol, tetraglycidylbisaminomethylcyclohexanone, N,N,N',N'-tetraglycidyl-m-xylylenediamine, etc. Among these, 1,3-bis(diglycidylaminomethyl)cyclohexane is preferred.

[0036] The glycidyl amine-based epoxy compound preferably has an epoxy equivalent of 70 g / eq or more and 140 g / eq or less, more preferably 80 g / eq or more and 125 g / eq or less, more preferably 85 g / eq or more and 110 g / eq or less, and even more preferably 90 g / eq or more and 100 g / eq or less. By setting the epoxy equivalent to 125 g / eq or less, it is possible to more easily prevent the interlayer adhesion of the connector from decreasing over time. By setting the epoxy equivalent to 80 g / eq or more, it is possible to more easily prevent the initial interlayer adhesion of the connector from weakening.

[0037] The amount of the glycidyl amine-based epoxy compound is preferably 0.1 parts by mass or more and 27.5 parts by mass or less, more preferably 0.5 parts by mass or more and 20.0 parts by mass or less, even more preferably 0.7 parts by mass or more and 10.0 parts by mass or less, and even more preferably 1.0 parts by mass or more and 8.0 parts by mass or less, relative to 100 parts by mass of the acid-modified polyolefin resin. By setting the blending amount of the glycidylamine-based epoxy compound to 0.1 parts by mass or more, it is possible to more easily prevent the interlayer adhesion of the connector from decreasing over time.By setting the blending amount of the glycidylamine-based epoxy compound to 27.5 parts by mass or less, it is possible to more easily prevent the initial interlayer adhesion of the connector from weakening.

[0038] The melting point of the cured product of the acid-modified polyolefin resin and the glycidyl amine-based epoxy compound is preferably 60°C or higher and 115°C or lower, more preferably 65°C or higher and 110°C or lower, and even more preferably 70°C or higher and 95°C or lower. By setting the melting point to 60° C. or higher, it is possible to easily prevent the interlayer adhesion of the connector from decreasing due to heat. In particular, by setting the melting point to 60° C. or higher, it is possible to easily prevent the interlayer adhesion from decreasing when the connector is immersed in a high-temperature electrolyte. By setting the melting point to 115° C. or less, it becomes easy to bond the first metal base material and the second metal base material together. In addition, by setting the melting point to 115° C. or less, the lamination temperature when bonding the first metal base material and the second metal base material together can be set low, which makes it easy to suppress oxidation of the metal base material. In this specification, the melting point can be measured by a differential scanning calorimeter (DSC). Specifically, the melting point can be measured by the method described in the Examples. In addition, in this specification, when melting peaks are observed at multiple temperatures, the temperature of the melting peak on the lower temperature side is regarded as the melting point.

[0039] The melting point of the cured product can be adjusted, for example, by the weight average molecular weight of the acid-modified polyolefin resin and the amount of the curing agent. For example, the melting point tends to increase when the weight average molecular weight is increased, and the melting point tends to decrease when the weight average molecular weight is decreased. In addition, the melting point tends to increase when the amount of the curing agent is increased, and the melting point tends to decrease when the amount of the curing agent is decreased. In addition, the melting point tends to increase when the aging time is increased, and the melting point tends to decrease when the aging time is decreased. In addition, the melting point tends to increase when the aging temperature is increased, and the melting point tends to decrease when the aging temperature is decreased.

[0040] Conductive particles In the present invention, the conductive particles are particles having a conductive layer on the surface of a resin core. The conductive particles have a conductive layer on the surface, and therefore can electrically connect the first metal substrate and the second metal substrate. In addition, the conductive particles have a resin core, and therefore the particle diameter in the thickness direction is reduced by the pressure during lamination. The reduced particle diameter in the thickness direction of the conductive particles increases the contact area between the conductive adhesive layer and the second metal substrate, and makes it easier to improve the interlayer adhesion. Particles having a conductive layer on the surface of a resin core can be obtained, for example, by plating or vapor-depositing a metal on a resin core.

[0041] The conductive particles are preferably particles having protrusions on their surfaces. Even if an oxide film is formed on the surfaces of the first metal base material and the second metal base material, the conductive particles having protrusions on their surfaces can easily break through the oxide film with the protrusions, making it easier to electrically connect the first metal base material and the second metal base material. Particles having protrusions on their surface can be obtained, for example, by arranging a plurality of core substances that will form protrusions on the surface of a resin core, and then plating or vapor-depositing a metal. Examples of methods for attaching a core substance to the surface of a resin core particle include a method in which the core substance is added to a dispersion liquid of the resin core and the core substance is accumulated on the surface of the resin core particle by van der Waals forces or the like.

[0042] Examples of the resin constituting the resin core include benzoguanamine resin, acrylic resin, styrene resin, silicone resin, polybutadiene resin, etc. Examples of the resin constituting the resin core also include copolymers combining two or more of the monomers constituting the above-mentioned resins.

[0043] The compression recovery rate of the resin core is preferably 55% or less, more preferably 47% or less, more preferably 40% or less, more preferably 30% or less, and more preferably 18% or less. By setting the compression recovery rate to 55% or less, the particle diameter of the conductive particles in the thickness direction is likely to become small due to the pressure during lamination. As a result, the contact area between the conductive adhesive layer and the second metal base material increases, making it easier to improve the interlayer adhesion of the connection body. The resin core preferably has a compression recovery rate of 5% or more, more preferably 6% or more, and even more preferably 7% or more. By making the compression recovery rate 5% or more, it is possible to prevent the particle diameter of the conductive particles in the thickness direction from becoming extremely small due to the pressure during lamination. This makes it easier to electrically connect the first metal base material and the second metal base material. The compression recovery rate of the resin core can be adjusted, for example, by the components of the resin constituting the resin core and the degree of crosslinking of the resin constituting the resin core. Specifically, the compression recovery rate tends to increase when the degree of crosslinking of the resin is increased, and tends to decrease when the degree of crosslinking of the resin is decreased.

[0044] In this specification, the compression recovery rate can be measured as follows. Resin cores are scattered on a sample table. A micro-compression tester is used to apply a load (reversed load value) toward the center of each resin core until the resin core is compressed and deformed by 30%. The load is then removed until the load value for the origin (0.40 mN) is reached. The load-compression displacement during this period is measured, and the compression recovery rate can be calculated from the following formula. The loading speed is 0.33 mN / sec. For example, a Fischerscope H-100 manufactured by Fischer is used as the micro-compression tester. Compression recovery rate (%) = [(L1-L2) / L1] x 100 L1: Compressive displacement from the load value for the origin to the reverse load value when applying a load L2: Unloading displacement from the reverse load value when releasing the load to the load value for the origin

[0045] The core material preferably has a Mohs hardness of 5 or more, more preferably 7 or more, and even more preferably 9 or more. Examples of the material for the core substance include nickel (Mohs hardness 5), zirconia (Mohs hardness 8 to 9), alumina (Mohs hardness 9), tungsten carbide (Mohs hardness 9), and diamond (Mohs hardness 10). The core substance may be used alone or in combination of two or more kinds.

[0046] The average particle size of the core material is preferably 50 nm to 250 nm, more preferably 100 nm to 200 nm. The number of protrusions formed on the surface of the resin core is preferably 1 to 500, more preferably 30 to 200.

[0047] The conductive layer is preferably made of a metal. Examples of the metal constituting the conductive layer include gold, palladium, nickel, copper, silver, tin, and aluminum. The metal constituting the conductive layer may be an alloy.

[0048] From the viewpoint of the balance between electrical conductivity and economic efficiency, the thickness of the conductive layer is preferably 50 nm or more and 250 nm or less, and more preferably 80 nm or more and 150 nm or less.

[0049] The content of the conductive particles is preferably 0.1 parts by mass or more and 2.0 parts by mass or less, more preferably 0.15 parts by mass or more and 1.8 parts by mass or less, and even more preferably 0.2 parts by mass or more and 1.7 parts by mass or less, relative to 100 parts by mass of the adhesive. By setting the content of the conductive particles to 0.1 parts by mass or more, the resistance value of the connector can be easily reduced. By setting the content of the conductive particles to 2.0 parts by mass or less, aggregation of the conductive particles can be easily suppressed, so that the resistance value of the connector can be easily reduced.

[0050] Thickness When the average thickness of the conductive adhesive layer is defined as Tn [μm] and the average diameter of the conductive particles in the thickness direction is defined as Dn [μm], it is preferable that the relationship Dn / Tn satisfies 1.00 or more. By making Dn / Tn 1.00 or more, the first metal base and the second metal base can be easily electrically connected to each other. Dn / Tn is preferably 1.01 or more, and more preferably 1.03 or more. In order to facilitate good interlayer adhesion of the connector, Dn / Tn is preferably 1.50 or less, more preferably 1.40 or less, and even more preferably 1.30 or less.

[0051] The difference between Dn and Tn (Dn-Tn) is preferably 0.01 μm or more, more preferably 0.03 μm or more, and even more preferably 0.05 μm or more. The difference between Dn and Tn (Dn-Tn) is preferably 1.0 μm or less, more preferably 0.8 μm or less, and even more preferably 0.7 μm or less.

[0052] In this specification, the average thickness Tn of the conductive adhesive layer is the average thickness of the conductive adhesive layer at 30 randomly selected locations. The thickness at the 30 locations can be measured, for example, from a cross-sectional photograph of the conductive adhesive layer taken by a SEM or the like.

[0053] In this specification, Dn, which indicates the average particle size of the conductive particles, can be measured, for example, by the following procedures A1 and A2. A1: Take a cross-sectional photograph of the conductive adhesive layer using an SEM or similar device. A2: The diameter of the conductive particles in the thickness direction shown in the cross-sectional photograph is measured. The average diameter of a total of 30 conductive particles in the thickness direction is defined as Dn.

[0054] The average thickness Tn of the conductive adhesive layer is preferably 1.0 μm or more and 10.0 μm or less, more preferably 2.0 μm or more and 8.0 μm or less, and even more preferably 3.0 μm or more and 6.0 μm or less. By setting Tn to 1.0 μm or more, it is possible to easily improve the interlayer adhesion of the connecting body, and to easily prevent the first metal base material and the second metal base material from contacting each other without the conductive particles. By setting Tn to 10.0 μm or less, it is possible to easily improve the coating stability of the conductive adhesive layer.

[0055] Dn, which indicates the average diameter of the conductive particles in the thickness direction, is preferably from 1.5 μm to 12.0 μm, more preferably from 2.5 μm to 9.0 μm, and even more preferably from 3.5 μm to 7.0 μm.

[0056] The CV value, which indicates the variation in the particle size distribution of the conductive particles, is preferably 10% or less, and more preferably 5% or less. By using a material with a small CV value, it is possible to suppress convex defects caused by fillers with large particle sizes in the appearance of the laminate. The CV value is an abbreviation for "coefficient of variation."

[0057] <Area ratio> When the area of ​​the connector when viewed in plan is S, the area of ​​the first metal base when viewed in plan is S1, and the area of ​​the second metal base when viewed in plan is S2, it is preferable to satisfy the following formulas (1) and (2). By satisfying the following formulas (1) and (2), alignment can be made unnecessary. Furthermore, by satisfying the following formulas (1) and (2), it is possible to easily electrically connect the first metal base and the second metal base. 0.99≦S1 / S≦1.01 (1) 0.99≦S2 / S≦1.01 (2)

[0058] When the area of ​​the conductive adhesive layer in a plan view of the connection body is S3, it is preferable that the above-mentioned S1, S2, and S3 satisfy the following formulas (3) and (4). By satisfying the following formulas (3) and (4), alignment can be made unnecessary. Furthermore, by satisfying the following formulas (3) and (4), it is possible to easily electrically connect the first metal base material and the second metal base material. 1.00≦S1 / S3≦1.02 (3) 1.00≦S2 / S3≦1.02 (4)

[0059] <Resistance value> The resistance of the connector is preferably 10.0 mΩ or less, more preferably 8.0 mΩ or less, and even more preferably 6.0 mΩ or less. There is no particular lower limit to the resistance of the connector, but it is preferably 1.0 mΩ or more, and more preferably 2.0 mΩ or more. The resistance value of the connector can be measured by a four-terminal method by placing one terminal on the first metal substrate and the other terminal on the second metal substrate.

[0060] [Manufacturing method] The connection body of the present invention can be produced, for example, by the following steps 1 and 2.

[0061] Step 1: A step of applying a coating liquid for a conductive adhesive layer, which contains a composition for an adhesive and conductive particles having a conductive layer on the surface of a resin core, onto a first metal substrate, and drying the coating liquid to form a conductive adhesive layer. The composition for the adhesive is a composition containing an acid-modified polyolefin resin having an acid value of less than 20.0 mgKOH / g and a glycidylamine-based epoxy compound. Step 2: A step of laminating a second metal substrate onto the conductive adhesive layer to obtain a connector having the first metal substrate, the conductive adhesive layer, and the second metal substrate in this order.

[0062] <Step 1> Step 1 is a step of applying a coating liquid for a conductive adhesive layer, which contains an adhesive and conductive particles having a conductive layer on the surface of a resin core, onto a first metal substrate, and drying the coating liquid to form a conductive adhesive layer.

[0063] In Step 1, when the average thickness of the conductive adhesive layer is defined as T1 [μm] and the average particle diameter of the conductive particles is defined as D1 [μm], it is preferable to satisfy the relationship of T1 < D1.

[0064] FIG. 3(a) is a cross-sectional view showing an embodiment of the state after Step 1. The laminate 50 in FIG. 3(a) has a conductive adhesive layer 30 on a first metal substrate 10. In FIG. 3(a), the conductive adhesive layer 30 has an adhesive 31 and conductive particles 32 having a conductive layer on the surface of a resin core.

[0065] In Step 1, it is preferable to satisfy the relationship of T1 < D1. By satisfying the relationship of T1 < D1, the first metal substrate and the second metal substrate can be electrically connected by a simple lamination process without performing processing at high temperature and high pressure during manufacturing.

[0066] The ratio of D1 to T1 (D1 / T1) is preferably 1.03 or more, more preferably 1.05 or more, and even more preferably 1.10 or more. By making the ratio 1.03 or more, the first metal base and the second metal base can be easily electrically connected. The ratio of D1 to T1 (D1 / T1) is preferably 1.50 or less, more preferably 1.30 or less, and even more preferably 1.20 or less. By setting the ratio to 1.50 or less, it is possible to easily improve the interlayer adhesion of the connector.

[0067] The difference between D1 and T1 (D1-T1) is preferably 0.1 μm or more, more preferably 0.3 μm or more, and even more preferably 0.4 μm or more. The difference between D1 and T1 (D1-T1) is preferably 2.0 μm or less, more preferably 1.0 μm or less, and even more preferably 0.7 μm or less.

[0068] T1, which indicates the average thickness of the conductive adhesive layer, is preferably 1.0 μm or more and 10.0 μm or less, more preferably 2.0 μm or more and 8.0 μm or less, and even more preferably 3.0 μm or more and 6.0 μm or less. By making T1 1.0 μm or more, it is possible to easily improve the interlayer adhesion of the connecting body, and to easily prevent the first metal base material and the second metal base material from contacting each other without the conductive particles. By making T1 10.0 μm or less, it is possible to easily improve the coating stability of the conductive adhesive layer.

[0069] D1, which indicates the average particle size of the conductive particles, is preferably 1.5 μm or more and 12.0 μm or less, more preferably 2.5 μm or more and 9.0 μm or less, and even more preferably 3.5 μm or more and 7.0 μm or less. As described above, the conductive particles are slightly crushed in the thickness direction due to the pressure during lamination. For this reason, it is preferable that D1 is slightly larger than Dn. The difference between D1 and Dn is about 0.05 μm or more and 0.70 μm or less.

[0070] In this specification, T1, which indicates the average thickness of the conductive adhesive layer, is the average value of the thicknesses of the conductive adhesive layer at 30 randomly selected locations. The thicknesses at the 30 locations are measured after the completion of step 1 and before the start of step 2. The thicknesses at the 30 locations can be measured, for example, from cross-sectional photographs of the conductive adhesive layer taken with an SEM or the like.

[0071] In this specification, D1, which indicates the average particle diameter of the conductive particles, can be measured, for example, by the following procedures B1 and B2. The following procedures B1 and B2 are performed after the completion of step 1 and before the start of step 2. B1: Take a cross-sectional photograph of the conductive adhesive layer using an SEM or similar. B2: The maximum diameter of the conductive particles shown in the cross-sectional photograph is measured. The average of the maximum diameters of a total of 30 conductive particles is designated as D1.

[0072] The coating liquid for the conductive adhesive layer preferably contains a solvent. Examples of the solvent include organic solvents such as ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.), aliphatic hydrocarbons (hexane, etc.), alicyclic hydrocarbons (cyclohexane, etc.), aromatic hydrocarbons (toluene, xylene, etc.), esters (methyl acetate, ethyl acetate, butyl acetate, etc.), alcohols (isopropanol, butanol, cyclohexanol, etc.), cellosolves (methyl cellosolve, ethyl cellosolve, etc.), and glycol ethers (propylene glycol monomethyl ether acetate, etc.). In addition, a mixed solvent of the organic solvent and water can also be used as the solvent. The solvent may be a single type of solvent or a mixed solvent of two or more types.

[0073] Examples of the coating means include general-purpose coating means such as gravure coating, bar coating, roll coating, reverse roll coating, comma coating, and die coating. The drying conditions may be adjusted depending on the characteristics of the metal substrate, the materials constituting the coating solution for the conductive adhesive layer, the coating amount of the coating solution, etc. For example, it is preferable that the drying temperature is 80° C. or higher and 120° C. or lower, and the drying time is 30 seconds or higher and 90 seconds or lower. If the temperature is within the above range, it is easy to suppress the expansion and oxidation of the metal substrate, and it is easy to improve the quality of the connection body. The curing reaction between the acid-modified polyolefin resin and the glycidylamine-based epoxy compound also proceeds due to the drying in step 1. In order to further proceed with the curing reaction, it is preferable to carry out step 3 after step 2.

[0074] <Process 2> Step 2 is a step of laminating a second metal substrate on the conductive adhesive layer to obtain a connection body having the first metal substrate, the conductive adhesive layer, and the second metal substrate in this order.

[0075] FIG. 3(b) is a cross-sectional view showing one embodiment after step 2. The connection body 100 in Fig. 3(b) has a conductive adhesive layer 30 and a second metal base material 20, in this order, on a first metal base material 10. In Fig. 3(b), the first metal base material 10 and the second metal base material 20 are electrically connected via conductive particles 30.

[0076] Comparing Fig. 3(a) with Fig. 3(b), the conductive particles 30 in Fig. 3(b) are crushed in the thickness direction, so that the particle diameter in the thickness direction is reduced. In this way, by crushing the conductive particles in the thickness direction, the adhesive present above the conductive particles (adhesive 31 present above the conductive particles 32 in Fig. 3(a)) is likely to spread in the width direction due to the pressure during lamination. This makes it easier to increase the contact area between the conductive adhesive layer and the second metal base material, making it easier to improve the interlayer adhesion of the connection body.

[0077] 3(b), the conductive adhesive layer 30 and the second metal base material 20 are not in contact with each other at both the left and right ends. These areas are air bubbles that were mixed in during lamination. As will be described later, air bubbles can be easily reduced by adjusting the temperature during lamination.

[0078] In step 2, the lamination temperature is preferably 55° C. or higher, more preferably 60° C. or higher, and even more preferably 70° C. or higher. By setting the lamination temperature at 55°C or higher, it is possible to suppress the inclusion of air bubbles during lamination and to easily reduce the resistance value. If air bubbles are introduced during lamination, the adhesive becomes less able to suppress the conductive particles from returning to their original shape, which may cause the resistance value of the connector to increase over time. For this reason, by setting the lamination temperature within the above range, it is possible to reduce the initial resistance value and easily suppress the increase in the resistance value of the connector over time. The upper limit of the lamination temperature is not particularly limited, but is preferably 110° C. or lower, more preferably 100° C. or lower, and further preferably 90° C. or lower.

[0079] The lamination pressure in step 2 is preferably 0.1 MPa or more and 1.0 MPa or less, more preferably 0.2 MPa or more and 0.7 MPa or less, and even more preferably 0.3 MPa or more and 0.5 MPa or less. By applying a pressure of 0.1 MPa or more, the conductive particles can be easily crushed in the thickness direction. Also, by applying a pressure of 0.1 MPa or more, the adhesive present above the conductive particles (adhesive 31 present above conductive particles 32 in FIG. 1) can be easily spread in the width direction by the pressure during lamination. By setting the pressure to 1.0 MPa or less, it is not necessary to apply high pressure, which simplifies and stabilizes the production of the connecting body, and also makes it easier to produce the connecting body continuously.

[0080] The lamination speed in step 2 is preferably 0.2 m / min to 30 m / min, more preferably 0.4 m / min to 2.0 m / min, and even more preferably 1.0 m / min to 15.0 m / min.

[0081] <Roll to Roll> In the above-mentioned method for producing a connection body, it is preferable that step 1 is performed by continuously feeding the first metal substrate from a roll of the first metal substrate, and step 2 is performed by continuously feeding the second metal substrate from a roll of the second metal substrate. By employing the above-mentioned means, the connectors can be manufactured continuously, and the manufacturing efficiency can be improved dramatically. After step 1, the laminate in which the conductive adhesive layer is formed on the first metal substrate may be temporarily wound up. Then, step 2 may be performed by continuously feeding the laminate from the wound roll of the laminate and continuously feeding the second metal substrate from the roll of the second metal substrate. In this way, even if a step of winding the laminate is included between steps 1 and 2, the production rate can be dramatically increased because it is a roll-to-roll production.

[0082] <Process 3> The method for producing the connection body may further include the following step 3. Step 3: Aging the connector.

[0083] By carrying out the aging treatment in step 3, the hardening of the acid-modified polyolefin resin and the glycidyl amine-based epoxy compound can be promoted. Therefore, the connection body having undergone step 3 can easily suppress the deterioration of the interlayer adhesion of the connection body over time. Furthermore, the connection body having undergone step 3 can easily suppress the change in the resistance value of the connection body over time because the adhesive can easily suppress the conductive particles from trying to return to their original shape.

[0084] In step 3, the temperature and time of the aging treatment are preferably in the following ranges.

[0085] The temperature of the aging treatment is preferably 55° C. or less, more preferably 50° C. or less, and even more preferably 47° C. or less. By setting the temperature of the aging treatment to 55° C. or less, it is possible to easily prevent the metal substrate from being oxidized. Furthermore, by setting the temperature of the aging treatment to 55° C. or less, it is possible to easily prevent the conductive particles from returning to their original shape during the aging treatment. The lower limit of the temperature for the aging treatment is preferably 25° C. or higher, more preferably 30° C. or higher, and even more preferably 40° C. or higher, in order to promote curing of the acid-modified polyolefin resin and the glycidylamine-based epoxy compound. The time for the aging treatment is not particularly limited, but is preferably from 1 to 9 days, and more preferably from 3 to 7 days. EXAMPLES

[0086] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0087] 1. Measurement 1-1.Resistance value The resistance values ​​of the connections made in the examples and comparative examples were measured. One pair of terminals was placed on a first metal substrate, and the other pair of terminals was placed on a second metal substrate, and the resistance values ​​were measured by a four-terminal method. A measuring device, a product name "Resistance Meter RM3544" manufactured by Hioki E.E. Corporation, was used. The results are shown in Table 1.

[0088] 1-2.Changes in interlayer adhesion over time (1) Measurement of initial interlayer adhesion The connectors produced in the examples and comparative examples were cut to a width of 15 mm and a length of 10 cm to produce two samples. A 10 mm portion of the second metal substrate was peeled off from the tip of one of the samples, and the peeled second metal substrate was held in a chuck and peeled off at a peel angle of 180° and a peel speed of 200 mm / min using Shimadzu Corporation's product name "AUTOGRAPH AGS-50D," to measure the peel force 1. The first metal substrate was peeled off from the tip of the other sample by 10 mm, and the peeled first metal substrate was held in a chuck and peeled off at a peel angle of 180° and a peel speed of 200 mm / min using Shimadzu Corporation's product name "AUTOGRAPH AGS-50D", to measure the peel force 2. Of peel strength 1 and peel strength 2, the weaker peel strength was defined as the "initial interlayer adhesion strength."

[0089] (2) Measurement of interlayer adhesion after 300 hours of durability testing For each of the connections in the Examples and Comparative Examples, two samples were prepared similar to (1) above. The pouch was filled with the durability test liquid described below, and then the sample was placed in the pouch. The pouch was immersed in an oil bath at 60°C for 300 hours, and then the sample was removed from the pouch. The peel strength of the two samples was then measured similar to (1) above. The measured peel strengths were designated as peel strengths 3 and 4. Of peel strengths 3 and 4, the weaker peel strength was designated as the "interlayer adhesion strength after 300 hours." <Durability test liquid> X1: Lithium hexafluorophosphate and a solvent were mixed so that the concentration of lithium hexafluorophosphate was 1 mol / L to prepare an electrolyte solution for lithium ion batteries. The solvent used was a mixed solvent of ethylene carbonate and diethyl carbonate in a mass ratio of 1:1. X2: 600 mg of water was added to 1 kg of the electrolyte obtained in X1. The reason for adding water is to generate hydrofluoric acid from lithium hexafluorophosphate.

[0090] (3) Calculation of change in interlayer adhesion over time For the connections of each of the examples and comparative examples, the interlayer adhesion strength after 300 hours / initial interlayer adhesion strength was calculated. The results are shown in Table 1. In comparative example 4, the interface of the sample peeled off in the durability test liquid, and the interlayer adhesion strength after 300 hours could not be measured. For this reason, the evaluation of comparative example 4 in Table 1 is entered as "-".

[0091] 1-3. Melting point measurement The melting points of the cured products of the acid-modified polyolefin resin and the epoxy compound used in the examples and comparative examples were measured by the following method. <Melt point measurement method> The melting peak temperature was measured with a differential scanning calorimeter (product name: EXSTRA DSC6200, manufactured by Hitachi High-Tech Science Corporation) under the conditions of a measurement temperature of 0 to 160° C. and a heating rate of 20° C. / min. The melting peak of the first heating was regarded as the melting point of the cured product.

[0092] 2. Preparation of conductive particles with a conductive layer on the surface of a resin core In accordance with the description of Example 3 of JP 2020-97739 A, conductive particles were obtained (average particle diameter 3.1 μm) in which a conductive layer (nickel layer) approximately 0.1 μm thick was formed on the surface of a resin core (compression recovery rate: 9.8%).

[0093] 3. Manufacture of acid-modified polyolefin resin (1) Acid-modified polyolefin resin 1 In a 1L autoclave, 100 parts by mass of propylene-butene copolymer (Mitsui Chemicals' "Tafmer (registered trademark) XM7080"), 150 parts by mass of toluene, 1 part by mass of maleic anhydride, and 5 parts by mass of di-tert-butyl peroxide were added, and the temperature was raised to 140 ° C., followed by stirring for another 3 hours. After that, the obtained reaction liquid was cooled and poured into a container containing a large amount of methyl ethyl ketone to precipitate the resin. Then, the liquid containing the resin was centrifuged to separate and purify the acid-modified propylene-butene copolymer in which maleic anhydride was graft-polymerized, (poly)maleic anhydride, and low molecular weight substances. Then, the mixture was dried under reduced pressure at 70 ° C. for 5 hours to obtain an acid-modified polyolefin resin 1 (maleic anhydride-modified propylene-butene copolymer, acid value 1 mg KOH / g, weight average molecular weight 100,000).

[0094] (2) Acid-modified polyolefin resin 2 Except for changing the amount of maleic anhydride added to 19 parts by mass and the amount of di-tert-butyl peroxide added to 5 parts by mass, the same procedure as in Production Example 1 was carried out to obtain an acid-modified polyolefin resin 2 (maleic anhydride-modified propylene-butene copolymer, acid value 12 mg KOH / g, weight average molecular weight 100,000).

[0095] (3) Acid-modified polyolefin resin 3 An acid-modified polyolefin resin 3 (maleic anhydride-modified propylene-butene copolymer, acid value 12 mgKOH / g, weight average molecular weight 100,000) was obtained by the same procedure as in Production Example 1, except that the propylene-butene copolymer (Mitsui Chemicals, Inc.'s "TAFMER (registered trademark) XM7080") was changed to a propylene-butene copolymer (Mitsui Chemicals, Inc.'s "TAFMER (registered trademark) XM7090"), the amount of maleic anhydride charged was changed to 19 parts by mass, and the amount of di-tert-butyl peroxide charged was changed to 5 parts by mass.

[0096] 4. Preparation of the connector [Example 1] The connection body of Example 1 was produced by the following steps 1 to 3. The connection body of Example 1 had T1 of 2.9 μm, D1 of 3.1 μm, Tn of 2.9 μm, and Dn of 2.93 μm, as described in the specification.

[0097] Step 1: The following conductive adhesive layer coating solution 1 was applied onto a first metal substrate (aluminum foil having a thickness of 50 μm) by gravure coating. Then, the substrate was dried at 100° C. for 1 minute to form a conductive adhesive layer having an average thickness of 2.9 μm. Step 1 was carried out continuously by continuously feeding the first metal substrate from a roll of the first metal substrate.

[0098] <Coating solution for conductive adhesive layer 1> 0.27 parts by weight of conductive particles prepared in "2" above Base agent 100 parts by weight (Acid-modified polyolefin resin 1 above) Hardener 5 parts by weight (Glycidylamine epoxy compound) (1,3-Bis(diglycidylaminomethyl)cyclohexane) Dilution solvent (appropriate amount)

[0099] Step 2: A second metal base material (copper foil with a thickness of 8 μm) was laminated on the conductive adhesive layer to obtain a connection body having the first metal base material, the conductive adhesive layer, and the second metal base material in this order. The lamination conditions were as follows: Step 2 was carried out continuously by continuously feeding the second metal substrate from a roll of the second metal substrate. Steps 1 and 2 were carried out continuously in one line. <Lamination conditions> Laminate roll temperature: 80℃ Lamination pressure: 0.4MPa Lamination speed: 5m / min

[0100] Step 3: The connection body obtained in step 2 was wound up and subjected to aging treatment at 45° C. for 5 days.

[0101] [Example 2] A connection body of Example 2 was produced in the same manner as in Example 1, except that the conductive adhesive layer coating liquid 1 was changed to the conductive adhesive layer coating liquid 2 described below. <Coating solution for conductive adhesive layer 2> 0.28 parts by weight of conductive particles prepared in "2" above Base agent 100 parts by weight (Acid-modified polyolefin resin 2 above) Hardener 1.12 parts by weight (Glycidylamine epoxy compound) (1,3-Bis(diglycidylaminomethyl)cyclohexane) Dilution solvent (appropriate amount)

[0102] [Example 3] A connection body of Example 3 was produced in the same manner as in Example 1, except that the conductive adhesive layer coating liquid 1 was changed to the conductive adhesive layer coating liquid 3 described below. <Coating solution for conductive adhesive layer 3> 0.75 parts by weight of the conductive particles prepared in "2" above Base agent 100 parts by weight (Acid-modified polyolefin resin 3 above) Hardener 2.45 parts by weight (Glycidylamine epoxy compound) (1,3-Bis(diglycidylaminomethyl)cyclohexane) Dilution solvent (appropriate amount)

[0103] [Example 4] A connection body of Example 4 was produced in the same manner as in Example 1, except that the conductive adhesive layer coating liquid 1 was changed to the conductive adhesive layer coating liquid 4 described below. <Coating solution for conductive adhesive layer 4> 0.27 parts by weight of conductive particles prepared in "2" above Base agent 100 parts by weight (Acid-modified polyolefin resin 1 above) Hardener 25 parts by weight (Glycidylamine epoxy compound) (1,3-Bis(diglycidylaminomethyl)cyclohexane) Dilution solvent (appropriate amount)

[0104] [Example 5] A connection body of Example 5 was produced in the same manner as in Example 1, except that the conductive adhesive layer coating liquid 1 was changed to the conductive adhesive layer coating liquid 5 described below. <Coating solution for conductive adhesive layer 5> 0.27 parts by weight of conductive particles prepared in "2" above Base agent 100 parts by weight (Acid-modified polyolefin resin 1 above) Hardener 30 parts by weight (Glycidylamine epoxy compound) (1,3-Bis(diglycidylaminomethyl)cyclohexane) Dilution solvent (appropriate amount)

[0105] [Comparative Example 1] A connection body of Comparative Example 1 was produced in the same manner as in Example 1, except that the conductive adhesive layer coating liquid 1 was changed to the conductive adhesive layer coating liquid 6 described below. <Coating solution for conductive adhesive layer 6> 0.14 parts by weight of conductive particles prepared in "2" above Base agent 100 parts by weight (Acid-modified polyolefin resin 2 above) Hardener 2.16 parts by weight (Glycidyl ether epoxy compound) (Nagase ChemteX Corporation, product name: Denacol EX-321L, solid content 100%) Dilution solvent (appropriate amount)

[0106] [Comparative Example 2] The connection body of Comparative Example 2 was produced in the same manner as in Example 1, except that the conductive adhesive layer coating liquid 1 was changed to the conductive adhesive layer coating liquid 6 described above, and the aging treatment in step 3 was changed to 120°C for 2 hours.

[0107] [Comparative Example 3] A connection body of Comparative Example 3 was produced in the same manner as in Example 1, except that the conductive adhesive layer coating liquid 1 was changed to the conductive adhesive layer coating liquid 7 described below, and the aging treatment in step 3 was changed to 120°C for 2 hours. <Coating solution for conductive adhesive layer 7> 0.14 parts by weight of conductive particles prepared in "2" above Base agent 100 parts by weight (Acid-modified polyolefin resin 2 above) Hardener 2.16 parts by weight (Glycidyl ether epoxy compound) (Nagase ChemteX Corporation, product name: Denacol EX-321L, solid content 100%) ·Curing catalyst 0.9 parts by mass (Shikoku Kasei, Curesol 2E4MZ, solid content 1%) Dilution solvent (appropriate amount)

[0108] [Comparative Example 4] A connection body of Comparative Example 4 was produced in the same manner as in Example 1, except that the conductive adhesive layer coating liquid 1 was changed to the conductive adhesive layer coating liquid 8 described below. <Coating solution for conductive adhesive layer 8> 0.24 parts by weight of conductive particles prepared in "2" above Base agent 100 parts by weight (Polyester resin) (Toyo Morton Co., Ltd., product name: AD76P1, solid content 51% by mass) Hardener 10 parts by weight (Isocyanate compounds) (Toyo Morton Co., Ltd., product name: CAT10L, solid content 53% by mass) Dilution solvent (appropriate amount)

[0109] [Comparative Example 5] A connection body of Comparative Example 5 was produced in the same manner as in Example 1, except that the conductive adhesive layer coating liquid 1 was changed to the conductive adhesive layer coating liquid 9 described below. <Coating solution for conductive adhesive layer 9> 0.27 parts by weight of conductive particles prepared in "2" above Base agent 100 parts by weight (Acid-modified polyolefin resin 1 above) Dilution solvent (appropriate amount)

[0110] [Table 1]

[0111] From the results in Table 1, it can be confirmed that the connections of the examples are capable of suppressing the decrease in interlayer adhesion over time. Note that in Examples 1 to 4, the interlayer adhesion strength increases after 300 hours. The reasons for this are thought to be that "softening of the adhesive layer during lamination in step 2 was insufficient" and "the adhesive layer that was not sufficiently softened in step 2 softened due to immersion in a 60°C oil bath for a long period of time, improving the adhesion between the metal substrate and the adhesive layer." Although not shown in Table 1, the initial interlayer adhesion strength, the interlayer adhesion strength after 100 hours, and the interlayer adhesion strength after 300 hours were all 0.20 N / mm or more for all of the connections of the examples, indicating that they had sufficient interlayer adhesion strength. Although not shown in Table 1, in the connections of the examples and comparative examples, S1 / S, S2 / S, S1 / S3, and S2 / S3 in the main text of the specification are all 1.00. [Explanation of symbols]

[0112] 10: First metal substrate 20: Second metal substrate 30: Conductive adhesive layer 31: Glue 32: Conductive particles having a conductive layer on the surface of a resin core 50: Laminate 100: Connector

Claims

1. A connection body having a first metal substrate, a conductive adhesive layer, and a second metal substrate in this order, the conductive adhesive layer includes an adhesive and conductive particles having a conductive layer on a surface of a resin core; The connecting body includes, as the adhesive, a cured product of an acid-modified polyolefin resin having an acid value of less than 20.0 mg KOH / g and a glycidyl amine-based epoxy compound.

2. 2. The connector according to claim 1, wherein the glycidyl amine-based epoxy compound has an epoxy equivalent of 70 g / eq or more and 140 g / eq or less.

3. 2. The connector according to claim 1, comprising 0.1 parts by mass or more and 27.5 parts by mass or less of the glycidyl amine-based epoxy compound relative to 100 parts by mass of the acid-modified polyolefin resin.

4. The connector according to claim 1 , wherein the acid-modified polyolefin resin has an acid value of 0.1 mgKOH / g or more and less than 15.0 mgKOH / g.

5. The connector according to claim 1 , wherein the melting point of the cured product is 60° C. or higher and 115° C. or lower.

6. The connection body according to claim 1 , wherein the conductive particles are contained in an amount of 0.1 parts by mass or more and 2.0 parts by mass or less relative to 100 parts by mass of the adhesive.

7. 2. The connection body according to claim 1, wherein when the average thickness of the conductive adhesive layer is defined as Tn [μm] and the average diameter of the conductive particles in the thickness direction is defined as Dn [μm], the relationship Dn / Tn is 1.00 or more.

8. The connector according to claim 7 , wherein Dn / Tn satisfies the relationship of 1.01 or more and 1.50 or less.

9. The connector according to any one of claims 1 to 8, which is for a lithium ion battery.

Citation Information

Patent Citations

  • Adhesive, laminate, battery member and battery

    JP2020100687A

  • Anisotropic conductive film as well as joining method and joined body using the same

    JP2023072774A

  • Adhesive composition, and coverlay film, bonding sheet, copper-clad laminate and electromagnetic shielding material, each using said adhesive composition

    WO2018116967A1

  • Electrically conductive one component (1K) epoxy formulation

    WO2022043160A1

  • Anisotropic conductive connection structure