Production method for calcium carbonate block
The described method enhances the productivity of calcium carbonate block production by molding, sintering, and carbonating calcium hydroxide blocks, resulting in a cost-effective and efficient manufacturing process for bone substitute materials.
Patent Information
- Application Number
- JP2023054697
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing methods for producing calcium carbonate blocks are not sufficiently productive, and there is a need for improved manufacturing efficiency.
A method involving molding calcium hydroxide blocks, sintering them to form calcium oxide blocks, and then contacting the sintered blocks with carbon dioxide to produce calcium carbonate blocks, eliminating the need for an immersion step in a carbonate ion-containing aqueous solution.
This method significantly reduces manufacturing time and costs while producing a dense, highly pure calcium carbonate block suitable for bone substitute materials.
Smart Images

Figure 2024142536000001 
Figure 2024142536000002 
Figure 2024142536000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing calcium carbonate blocks. [Background technology]
[0002] In medical fields such as medicine and dentistry, autologous bone grafting to the defect or void is the first choice for repairing a wide range of bone defects or voids. However, harvesting autologous bone requires surgical invasion of healthy tissue, and there is a limit to the amount that can be harvested, so transplantation of bone substitutes as an alternative to autologous bone is widely practiced.
[0003] In recent years, calcium carbonate blocks have been developed as bone filling materials. One method for producing calcium carbonate blocks is to mold a block of calcium hydroxide, which is a calcium carbonate precursor, bring the calcium hydroxide block into contact with carbon dioxide to partially carbonate the surface of the block, and then immerse the block in an aqueous solution containing carbonate ions (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6259926 Summary of the Invention [Problem to be solved by the invention]
[0005] For such calcium carbonate blocks, higher productivity is desired.
[0006] An object of the present invention is to provide a method for producing a calcium carbonate block with improved productivity. [Means for solving the problem]
[0007] One aspect of the present invention is a method for producing a calcium carbonate block, comprising: a molding step of molding a calcium hydroxide block; a sintering step of sintering the block; and a contacting step of contacting the sintered block with carbon dioxide. Effect of the Invention
[0008] According to one aspect of the present invention, a method for producing a calcium carbonate block with improved productivity can be provided. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a diagram showing an X-ray diffraction chart of the embodiment (Example 1). [Diagram 2] FIG. 4 is a diagram showing an X-ray diffraction chart of the embodiment (Example 2). [Diagram 3] FIG. 13 is a diagram showing an X-ray diffraction chart of the embodiment (Example 3). [Figure 4] FIG. 13 is a diagram showing an X-ray diffraction chart of an embodiment (Example 4). [Diagram 5] FIG. 2 is a diagram showing an X-ray diffraction chart of the embodiment (Reference Example 1). [Figure 6] FIG. 13 is a diagram showing an X-ray diffraction chart of the embodiment (Reference Example 2). [Figure 7] FIG. 2 is a diagram for comparing the number of steps and the number of days required for production in the production method for a calcium carbonate block according to the embodiment (Examples 1 and 2) and the conventional method (Comparative Example 1). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Next, a mode for carrying out the present invention (hereinafter, referred to as an embodiment) will be described.
[0011] The method for producing a calcium carbonate block according to the embodiment includes a molding step of molding a calcium hydroxide block (hereinafter, may be referred to as a calcium hydroxide block molding step or step A).
[0012] In this specification, calcium carbonate block refers to a formed body of calcium carbonate (CaCO3) in which calcium carbonate is formed into a block shape.
[0013] In the calcium hydroxide block molding process (Process A), calcium hydroxide powder (Ca(OH)2) is molded as the raw material for calcium carbonate blocks to obtain a molded calcium hydroxide body (calcium hydroxide block).
[0014] In step A, the powdered calcium hydroxide may be used for molding alone, or another substance may be added to and mixed with the powdered calcium hydroxide, and then the mixture may be molded.
[0015] In the step A, the time required for molding is not limited, but is, for example, from 1 second to 3 hours.
[0016] In step A, the molding method is not particularly limited, and examples thereof include a method of pressurizing and molding powdered calcium hydroxide to form pellets (compression molding method), a method of adding water (distilled water) to powdered calcium hydroxide, mixing the slurry, pressurizing and molding the mixture to form pellets (pressure slurry molding method), and a method of mixing powdered calcium hydroxide with water to form a slurry, drying (dehydrating) and molding the slurry (slurry molding method).
[0017] Among these, the slurry molding method is preferable as the molding method. When the slurry molding method is used as the molding method, the mass ratio of water to calcium hydroxide is preferably 0.01 to 2.5, more preferably 0.15 to 2.0, and even more preferably 0.3 to 1.7. When the mass ratio of water to calcium hydroxide is 0.01 to 2.5, the slurry can be sufficiently kneaded and dried (dehydrated), and molding defects can be prevented.
[0018] The method for producing a calcium carbonate block according to the embodiment further includes a sintering step of sintering the block (hereinafter, may be referred to as a sintering step or step B).
[0019] In the sintering step (step B), the calcium hydroxide block obtained in step (A) is sintered. Through this sintering, the calcium hydroxide block is converted into a calcium oxide (CaO) molded body (calcium oxide block).
[0020] The sintering temperature in step B is not particularly limited and is, for example, 550°C or higher, preferably 600°C or higher and 1200°C or lower, and more preferably 600°C or higher and 1100°C or lower.
[0021] If the sintering temperature is 550°C or higher, the calcium hydroxide blocks are partially converted to calcium oxide blocks, and the subsequent conversion to calcium carbonate blocks can also be sufficiently performed. The upper limit of the sintering temperature is arbitrary, but is not more than a practicable heating temperature (e.g., 1500°C).
[0022] The sintering atmosphere in step B has an oxygen concentration of, for example, 10% or more.
[0023] The sintering time in step B is, for example, from 10 minutes to 12 hours, preferably from 20 minutes to 6 hours, and more preferably from 30 minutes to 3 hours. When the sintering time is from 10 minutes to 12 hours, the crystals of the calcium oxide block after sintering tend to be dense, and the crystals of the calcium carbonate block converted from the calcium oxide block thereafter tend to be dense as well.
[0024] In addition, if an organic binder is added to calcium hydroxide, which is the raw material of calcium carbonate blocks, the conversion to calcium oxide during sintering is inhibited and calcium hydroxide tends to remain, so it is preferable not to add an organic binder to calcium hydroxide. The organic binder component is, for example, a polymer resin such as an acrylic resin.
[0025] The method for producing a calcium carbonate block according to the embodiment further includes a contacting step of contacting the sintered block with carbon dioxide (hereinafter, may be referred to as a carbon dioxide contacting step or step C).
[0026] In the carbon dioxide contact step (step C), the calcium oxide block obtained in step (B) is brought into contact with carbon dioxide. By contacting the calcium oxide block with carbon dioxide, the calcium oxide block is converted into a calcium carbonate molded body (calcium carbonate block).
[0027] In step C, the contact with carbon dioxide may be performed using, for example, an apparatus for flowing carbon dioxide gas into a thermostatic bath. When such an apparatus is used, the temperature can be controlled by the thermostatic bath, and the carbon dioxide concentration can be controlled by the flow rate of the carbon dioxide gas.
[0028] The concentration of carbon dioxide in step C is, for example, 0.5 to 45%, preferably 1.5 to 32%, and more preferably 5 to 20%. When the concentration of carbon dioxide is 0.5 to 45%, the calcium oxide block is sufficiently converted into a calcium carbonate block, and a calcium carbonate block with high purity (without residual unreacted substances) is likely to be obtained.
[0029] The temperature in step C is, for example, 10 to 80° C., preferably 17 to 60° C., and more preferably 23 to 42° C. When the temperature in the carbon dioxide contact step is 10 to 80° C., calcium oxide blocks are sufficiently converted into calcium carbonate blocks under appropriate carbon dioxide concentration and relative humidity, and calcium carbonate blocks with high purity are likely to be obtained.
[0030] The relative humidity in step C is, for example, 12% RH or more, preferably 60% RH or more, and more preferably 80% RH or more. When the relative humidity is 12% RH or more, the calcium oxide block is converted into a calcium carbonate block with a small amount of water under an appropriate carbon dioxide concentration, and a calcium carbonate block with high purity is easily obtained. The upper limit of the relative humidity is arbitrary, but is a practicable relative humidity (for example, 99%) or less.
[0031] The contact time in step C is, for example, 12 hours or more, preferably 3 days or more, and more preferably more than 6 days. When the contact time of carbon dioxide is 12 hours or more under appropriate contact temperature and relative humidity, calcium oxide blocks are sufficiently converted to calcium carbonate blocks via calcium hydroxide blocks, and calcium carbonate blocks with high purity are easily obtained. The upper limit of the contact time is arbitrary, but from the viewpoint of reducing production costs by shortening the production time, the contact time may be 14 days or less, preferably 10 days or less, and more preferably 8 days or less.
[0032] In the method for producing a calcium carbonate block according to the embodiment, a dense and highly pure calcium carbonate block (without residual unreacted matter) can be obtained without a time-consuming immersion step in a carbonate ion-containing aqueous solution as in the conventional method for producing a calcium carbonate block. This simplifies the production steps and shortens the production time when producing a calcium carbonate block, thereby improving the productivity of the calcium carbonate block.
[0033] In addition, the uses of the calcium carbonate block obtained by this manufacturing method are not particularly limited, but since a dense and highly pure (without residual unreacted materials) calcium carbonate block is obtained, it can be used as a biocompatible material, and is particularly suitable for use as a bone filling material.
[0034] In addition, in the manufacturing method of the calcium carbonate block according to the embodiment, by using the slurry molding method as described above as the molding method in the calcium hydroxide block molding process, since the slurry molding method does not include a pressurization process, it is easy to mold the calcium hydroxide block and manufacturing costs can be reduced. EXAMPLES
[0035] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0036] <Preparation of calcium carbonate block (test specimen)> As test specimens, calcium carbonate blocks were produced under the conditions of Examples 1 to 4, Reference Examples 1 and 2, and Comparative Example 1 shown below.
[0037] [Example 1] Powdered calcium hydroxide was compressed and molded to produce a calcium hydroxide molded body (calcium hydroxide block) (molding process). This calcium hydroxide block was placed in a sintering furnace and held at a sintering temperature of 600°C (heating rate of 400°C / hour) for 5 hours, and then allowed to cool naturally to obtain a calcium oxide molded body (calcium oxide block) (sintering process). This calcium oxide block was removed from the sintering furnace and placed in a thermostatic chamber and left to stand for 7 days in an environment with a CO2 concentration of 10%, a temperature of 28°C, and a humidity of 95%RH to obtain a calcium carbonate block (test specimen) (carbon dioxide contact process or slaking / carbonation process).
[0038] [Example 2] A test specimen was obtained in the same manner as in Example 1, except that the sintering temperature in the sintering step was 800°C.
[0039] [Example 3] A test specimen was obtained in the same manner as in Example 1, except that the sintering temperature in the sintering step was set to 1000°C.
[0040] [Example 4] In the molding process, instead of powder compaction, 74 parts by mass of calcium hydroxide was added to 80 parts by mass of water and mixed for 1 minute to prepare a calcium hydroxide slurry. This slurry was poured into a tray (mold) to evaporate the water and prepare a calcium hydroxide molded body (calcium hydroxide block). Except for this, the heating rate in the sintering process was set to 367°C / hour and the sintering temperature was set to 1100°C, and a test specimen was obtained in the same manner as in Example 1.
[0041] [Reference example 1] A test specimen was obtained in the same manner as in Example 1, except that the sintering temperature in the sintering step was 400°C.
[0042] [Reference example 2] A test specimen was obtained in the same manner as in Example 4, except that the reaction time in the carbon dioxide contact step was changed to 3 hours.
[0043] [Comparative Example 1] Powdered calcium hydroxide was compressed and molded to produce a calcium hydroxide molded body (calcium hydroxide block) (molding process). This calcium hydroxide block was left to stand for 7 days in an environment with a CO2 concentration of 10%, a temperature of 28°C, and a humidity of 95% RH (slaking and provisional carbonation process), and then immersed in a 0.5N aqueous solution of sodium bicarbonate (NaHCO3) at a liquid temperature of 80°C for 7 days (full carbonation process). It was then washed with water (washing process) and dried (drying process) to obtain a test specimen.
[0044] [X-ray diffraction measurement] For each of the specimens obtained in Examples 1 to 4 and Reference Examples 1 and 2, the presence or absence of a crystalline layer was confirmed by powder X-ray diffraction using a measuring device (all-in-one XRD device manufactured by Empyrean). The measurement conditions were tension: 45 kV, current: 40 mA, and measurement range: 2θ = 10.0° to 60.0°. The presence or absence of a crystalline layer was determined based on the presence or absence of the main peaks of the following substances in each specimen. The measurement results of Examples 1 to 4 and Reference Examples 1 and 2 are shown in Figures 1 to 6, respectively. Note that the symbols (●, ◆, ▼) in Figures 1 to 6 indicate the following substances and peak angles. ●: Main peak of calcium hydroxide ◆: Main peak of calcium carbonate ▼: Main peak of calcium oxide
[0045] 1 to 4 (Examples 1 to 4), the main peak of calcium carbonate was confirmed. From these results, it was determined that the test specimens obtained in Examples 1 to 4 were all calcium carbonate.
[0046] On the other hand, in Fig. 5 (Reference Example 1), the main peaks of calcium hydroxide and calcium carbonate were confirmed. From this result, it was determined that the test specimen obtained in Reference Example 1 was a complex of calcium hydroxide and calcium carbonate.
[0047] Moreover, the main peaks of calcium hydroxide and calcium oxide were confirmed in Fig. 6 (Reference Example 2). From this result, it was determined that the test specimen obtained in Reference Example 2 was a complex of calcium hydroxide and calcium oxide.
[0048] [Production time] The number of days (production time) required to produce a test specimen was compared for Examples 1 and 2 and Comparative Example 1. The results of the comparison are shown in FIG.
[0049] In Comparative Example 1, the preparation time (total number of days) was 18 days (FIG. 7(C)). In contrast, in Example 1, the preparation time (total number of days) was 9 days, and in Example 2, the preparation time (total number of days) was 10 days (FIGS. 7(A) and (B)).
[0050] From the above, it was found that the manufacturing method of calcium carbonate blocks, which includes a calcium hydroxide block molding process, a sintering process, and a carbon dioxide contact process, simplifies the manufacturing process and shortens the manufacturing time, thereby improving the productivity of calcium carbonate blocks (Examples 1 to 4).
[0051] Although an embodiment of the present invention has been described above, the present invention is not limited to a specific embodiment, and various modifications and changes are possible within the scope of the invention described in the claims.
Claims
1. A molding process for molding a block of calcium hydroxide; a sintering step of sintering the block; and contacting the sintered block with carbon dioxide. Method for manufacturing calcium carbonate blocks.
2. In the molding step, the block is molded from a slurry of calcium hydroxide. A method for producing the calcium carbonate block according to claim 1.
3. The calcium carbonate block is used in biocompatible materials. A method for producing the calcium carbonate block according to claim 1 or 2.
Citation Information
Patent Citations
Calcium carbonate composition for medical use, compositions for medical use related with the same and method for producing these