Dispersion liquid of hollow silica particle, and method of producing the same
Hollow silica particles with a silicon-containing outer shell and controlled properties address the trade-offs in resist materials, providing low refractive index, high developability, and sharp patterns while maintaining purity and stability in semiconductor manufacturing.
Patent Information
- Application Number
- JP2023054765
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing resist materials face challenges in achieving a balance between low refractive index and surface smoothness for sharp patterns, as well as high purity to prevent equipment contamination and electrical abnormalities, due to the trade-off between particle size and porosity, and high metal impurity content.
Development of hollow silica particles with a silicon-containing outer shell and a cavity inside, having a controlled average diameter, low metal impurity content, and optimized surface properties to enhance compatibility with alkaline developers, thereby improving developability and pattern resolution.
The hollow silica particles achieve a low refractive index, high developability, and sharp patterns while minimizing contamination and equipment issues, ensuring high purity and stability in semiconductor manufacturing processes.
Smart Images

Figure 2024142576000001 
Figure 2024142576000002 
Figure 2024142576000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a dispersion of hollow silica particles and a method for producing the same. [Background technology]
[0002] In recent years, photolithography, which is used in the manufacture of semiconductor elements, printed circuit boards, liquid crystal display panels, organic EL display panels, etc., is a widely used technology in which a photosensitive substance is applied to a substrate, and then exposed and developed in a pattern to process the substrate. The photosensitive material (resist material) used in this photolithography is a material that forms a functional film, such as a low refractive index film (or a high refractive index film) or an insulating film, in a pattern on the substrate surface. For this reason, high sensitivity, high resolution, and high transparency are required. Such functional films are formed by patterning into a desired shape using a resist material. This resist material is composed of components such as a resin component, a polymerization initiator, and a solvent.
[0003] It has been known that hollow silica particles or low-refractive-index particles with a porous interior are used in coating solutions as a means of lowering the refractive index of a film. For example, JP 2019-119848 A (Patent Document 1) and JP 2020-166156 A (Patent Document 2) disclose the use of silica particles containing gas in the particles as a photosensitive resin composition to lower the refractive index of the film. In addition, JP 2013-121911 A (Patent Document 3) describes silica-based hollow particles having an alkali metal oxide content of 5 ppm or less per silica-based fine particle. In addition, WO 2008 / 015943 (Patent Document 4) discloses a method for producing a silica particle dispersion in which the concentration of metal impurities in a silica sol is 1 ppm or less by using a high-purity silica raw material (alkoxysilane). Furthermore, Japanese Patent Laid-Open Publication No. 2009-020520 (Patent Document 5) describes a photosensitive resin composition that is excellent in low dielectric properties, adhesive strength, heat resistance, etc., and discloses the use of colloidal inorganic nanoparticles that have been surface-treated with an organic silane. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-119848 A [Patent Document 2] JP 2020-166156 A [Patent Document 3] JP 2013-121911 A [Patent Document 4] WO No. 2008 / 015943 [Patent Document 5] JP 2009-020520 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, with the increasing density of circuits, it is required to narrow the pitch width of the pattern part to about several hundred nm to several μm. In order to achieve this narrowing, the pattern part is required to have high linearity, high smoothness, and little residue on the substrate, and it is necessary to realize high developability as a resist film. In addition, as a means for lowering the refractive index of the resist film, it is possible to mix hollow particles with high porosity, that is, hollow particles with large particle diameter. However, when hollow particles with large particle diameter are mixed, the surface unevenness of the pattern part becomes large, making it difficult to obtain a sharp pattern. However, when hollow particles with small particle diameter are mixed to suppress the surface unevenness of the pattern part, the hollow particles have a low porosity and a high refractive index compared to hollow particles with large particle diameters, so the reduction in the refractive index of the film is insufficient. Thus, there is a correlation between the particle diameter and porosity of the hollow particles. In addition, even if the amount of hollow particles mixed is increased to lower the refractive index of the film, the surface unevenness becomes large due to the small amount of resin components that can exist between the particles, making it difficult to obtain a sharp pattern. That is, there is a trade-off between the refractive index and the surface roughness.
[0006] In resist applications, metal impurities that are mixed in during the manufacturing process of the resist film can contaminate the substrate and equipment, causing abnormalities in electrical properties and processed shapes. In addition, in recent years, the pitch width of the pattern part has been narrowed, and the allowable concentration of metal impurities required for resist materials has been reduced accordingly. Therefore, it is required to control the metal impurities at the ppb level for hollow silica particles that are blended with the aim of lowering the refractive index of the resist film. Furthermore, it is required to control the amount of elution of metal impurities from hollow silica particles in the alkaline solution (alkaline developer) used during development at the ppb level.
[0007] When the particles described in Patent Document 1, Patent Document 2, or Patent Document 3 are used in a resist material, it is expected that a film with a low refractive index can be obtained, but the content of metal impurities is high, so there are problems such as contamination of the substrate and manufacturing equipment, and abnormalities in electrical properties. In addition, the number density of silanol groups on the particle surface is low, so there are problems such as low compatibility with alkaline developers, making it difficult to form sharp patterns, and particle-derived residues on the substrate. When the particles described in Patent Document 4 are used, there is a problem that the refractive index of the particles is high, so the desired refractive index of the film cannot be obtained. Furthermore, raw materials with a low content of metal impurities have high raw material costs, so there is a problem of high manufacturing costs. Furthermore, the particles described in Patent Document 5 are surface-treated with an organic silane, so although they have high dispersibility in the resist film, they have low compatibility with alkaline developers, making it difficult to form sharp patterns, and there are problems such as particle-derived residues on the substrate. [Means for solving the problem]
[0008] In order to solve such problems, the following dispersion of hollow silica particles was found. The hollow silica particles have a shell containing silicon and a cavity inside. The particles have an average particle size of 15 to 150 nm and a refractive index of 1.08 to 1.35. Metal impurities contained in the particles include alkali metals, alkaline earth metals, Co, Cr, Cu, Fe, Mn, Ni, Ti, Zn, and Zr. The total content of these metal impurities in the particles is 1000 ppb or less in terms of metal.
[0009] Hereinafter, the hollow silica particles may be simply referred to as "particles" or "particles in a dispersion liquid".
[0010] These particles have a low refractive index and a low content of metal impurities. When these particles are used in resist materials, they cause less contamination in the semiconductor manufacturing process and exhibit excellent developability.
[0011] In order to obtain these particles, the following production method was found.
[0012] First, an alkaline aqueous solution is prepared (first step). A solution of a compound containing silicon and an aqueous solution of an alkali-soluble compound of an inorganic element other than silicon are simultaneously added to the aqueous solution so that the molar ratio (MOx / SiO2) of the reaction solution at the end of the addition is 0.2 to 15, where the oxide of silicon is represented as SiO2 and the oxide of the inorganic element other than silicon is represented as MOx, to prepare a dispersion of composite oxide particles a (second step). Next, a solution of a compound containing silicon and an aqueous solution of the alkali-soluble compound of an inorganic element other than silicon are added in a molar ratio (MOx / SiO2) smaller than that in the second step to prepare a dispersion of composite oxide particles b (third step). Next, an acid is added to the dispersion of composite oxide particles b to remove at least a part of the elements other than silicon that constitute the composite oxide particles b, to prepare a dispersion of silica-based particles (fourth step). Next, metal impurities selected from alkali metals, alkaline earth metals, Co, Cr, Cu, Fe, Mn, Ni, Ti, Zn, and Zr are removed until the content of the metal impurities in the silica-based particles is 1000 ppb or less (fifth step).The dispersion of silica particles obtained in the fifth step is heated to 60 to 200°C, and then cooled to less than 50°C (sixth step).
[0013] The properties of the particles in the dispersion obtained by this production method are similar to those of the particles in the dispersion described above. Effect of the Invention
[0014] The dispersion of the particles of the present invention has a low content of metal impurities in the particles. Therefore, it is used in resist materials that require high purity, and can achieve high developability during pattern formation. The resist film obtained here has a low refractive index, low haze, high resolution, and high density (fine pitch) of the number of patterns. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] [Particle dispersion] The particle dispersion according to the present invention (hereinafter, this may be simply referred to as "dispersion") will be described.
[0016] The dispersion of the present invention contains particles having a silicon-containing shell and a cavity therein, and a dispersion medium. The particles have an average particle size of 15 to 150 nm and a refractive index of 1.08 to 1.35. The total content of metal impurities selected from alkali metals, alkaline earth metals, Co, Cr, Cu, Fe, Mn, Ni, Ti, Zn, and Zr in the particles is 1000 ppb or less in terms of metal.
[0017] The particles have an average particle diameter of 15 to 150 nm, which is determined by taking a photograph at a specified magnification using a transmission electron microscope (TEM), randomly selecting 300 particles from the photograph (TEM photograph), processing the image to determine the particle area, and calculating the average value of the equivalent circle diameter from the area.
[0018] Here, particles with an average particle size of less than 15 nm have a small ratio of cavities (porosity) in the particles, and the refractive index is not sufficiently low, so the refractive index of the resist film may not be sufficiently low. Conversely, if the particle size exceeds 150 nm, depending on the content, it may be difficult to obtain a sharp pattern. The average particle size is preferably 20 to 100 nm, more preferably 20 to 75 nm, even more preferably 20 to 55 nm, and particularly preferably 25 to 45 nm.
[0019] The refractive index of the particles is 1.08 to 1.35. When the refractive index is within this range, a resist film with a low refractive index can be obtained by using the particles in a resist material. Here, it is difficult to obtain particles with a refractive index of less than 1.08. On the other hand, when the refractive index exceeds 1.35, the refractive index of the resist film may not be sufficiently reduced. The refractive index is preferably 1.08 to 1.30, more preferably 1.08 to 1.25.
[0020] The total content of metal impurities selected from alkali metals, alkaline earth metals, Co, Cr, Cu, Fe, Mn, Ni, Ti, Zn, and Zr contained in the particles is 1000 ppb or less as metal. If the content of metal impurities is high, the particles may coalesce with each other, and the stability of the dispersion liquid or coating liquid may decrease. In addition, in the semiconductor manufacturing process, the substrate or equipment may be contaminated, and abnormalities may occur in the electrical properties and processed shape, making it difficult to obtain a sharp pattern as a resist film, and the yield may decrease. In addition, in the manufactured semiconductor, the metal elements may cause poor insulation of the circuit or cause a short circuit in the circuit. Furthermore, there may be a decrease in the dielectric constant of the insulating film, an increase in the impedance of the metal wiring, a delay in the response speed, an increase in power consumption, etc. The total content of these metal impurities is preferably less than 500 ppb, more preferably less than 100 ppb, and even more preferably less than 10 ppb.
[0021] However, the particles may contain metal elements such as U and Th. These elements generate radioactivity, and even a trace amount of them is undesirable because they can cause semiconductors to malfunction due to radioactivity. The content of each of U and Th is preferably less than 0.1 ppb.
[0022] In order to obtain particles with a low content of such metal impurities, there is a method of removing the metal impurities from the particles. Specifically, there are washing with acid or alkali, ion exchange, filter removal, etc. In addition, it is preferable that the material of the equipment used for manufacturing the particles does not contain these elements and has high chemical resistance. For example, plastics such as Teflon (registered trademark), FRP, carbon fiber, and alkali-free glass are preferable. In addition, it is preferable to refine the raw materials used by distillation, ion exchange, and filter removal.
[0023] The total amount of the metal impurities eluted from the particles in an alkaline aqueous solution of pH 12.5 is preferably 100 ppb or less in terms of metal relative to the particles. Also, the amount of U and Th eluted from the particles in an alkaline aqueous solution of pH 12.5 is preferably less than 0.1 ppb each in terms of metal relative to the particles.
[0024] Incidentally, in the semiconductor manufacturing process, an "alkaline developer treatment" is performed to prepare a resist film. It is of course preferable that the particles have a low content of impurities, and it is also preferable that the elution of impurities is suppressed in this "alkaline development treatment". Examples of the alkaline developer used include a 0.3 mass% tetramethylammonium hydroxide (TMAH) aqueous solution (pH 12.5) and a 0.05 mass% potassium hydroxide (KOH) aqueous solution (pH 12.0). During the "alkaline developer treatment" to prepare a resist film using these alkaline developers, the particles come into contact with the alkaline developer and are in a state of, for example, pH 12.5, temperature 25°C, and development time 60 seconds. Therefore, "in an alkaline aqueous solution of pH 12.5" is a simulation of the atmosphere of the "alkaline developer treatment" during the preparation of a resist film in the semiconductor manufacturing process. However, in this "amount of elution of metal impurities in an alkaline aqueous solution of pH 12.5 of particles", the contact time between the particles and the alkaline developer is evaluated as 35 minutes in order to perform the elution test under more severe conditions.
[0025] Here, if the total amount of the above-mentioned metal impurities eluted from the particles in an alkaline aqueous solution of pH 12.5 exceeds 100 ppb as metal relative to the particles, there is a risk of causing contamination of the semiconductor process or insulation failure of the circuit. The total amount of the metal impurities eluted is more preferably 50 ppb or less, and even more preferably 10 ppb or less.
[0026] In addition, when the particles contain Al, the amount of Al eluted from the particles in an alkaline aqueous solution of pH 12.5 is preferably 1000 ppb or less as metal relative to the particles. If the amount of Al eluted is more than 100 ppb, it may cause contamination of the semiconductor process or insulation failure of the circuit. The amount of Al eluted is more preferably 500 ppb or less, and even more preferably 100 ppb or less.
[0027] The number density of silanol groups on the particle surface calculated by the Sears measurement method is 0.5 to 2.5 / nm 2 When the silanol group density is within this range, compatibility with an alkaline developer is high, and therefore a resist film with excellent developability can be obtained.
[0028] Here, the number density of silanol groups is 0.5 / nm 2 If the density is less than 2.5 particles / nm, the compatibility with the alkaline developer is low, which may make it difficult to form a sharp pattern or may cause particle-derived residues to be generated on the substrate. 2 If the silanol group density exceeds 0.8 to 2.2 / nm, the bond with the photosensitive resin becomes insufficient, and the bond with the resin becomes weak, which may make it difficult to form a pattern. 2 , more preferably 1.0 to 2.0 particles / nm 2 It is.
[0029] The number density of silanol groups of particles is calculated from the Sears number and the specific surface area. The Sears number is measured by titration with sodium hydroxide (NaOH) according to the description by Sears in Analytical Chemistry 28 (1956), 12, 1981-1983. Specifically, 30 g of sodium chloride is added to 150 g of silica particles diluted with pure water to make the silica particle concentration 1% by mass, and the pH is adjusted to 4.0 with hydrochloric acid. Then, 0.1 N NaOH aqueous solution is titrated at 0.1 ml / sec., and the number density is expressed by the amount (Q) of NaOH aqueous solution required to reach pH 9.0. That is, the Sears number (A) is the amount of 0.1 N NaOH aqueous solution required to titrate 1.5 g of particles, and is expressed by the following formula (1). A=(Q×f×100×1.5) / (W×C) ···(1) (In the formula, f represents the titer of the 0.1N NaOH aqueous solution used, C represents the particle concentration (mass%) in the dispersion, and W represents the amount (g) of the dispersion collected.)
[0030] The number density (ρ) of silanol groups is expressed by the following formula (2). ρ = (B × N A ) / (10 18 ×M×S BET ) ···(2) (In the formula, B is the amount of NaOH (mol) required to change the pH from 4.0 to 9.0 per 1.5 g of particles calculated from the Sears number (A), N A is the Avogadro number (particles / mol), M is the particle mass (1.5g), and S BET is the specific surface area (m2) measured by the BET method using nitrogen adsorption. 2 / g).
[0031] The thickness of the shell of the particle is 3 to 12 nm. This is the average value of the following values: the area of the cavity of 300 random particles in a TEM photograph is determined by image processing, the equivalent circle diameter is calculated from the area, the equivalent circle diameter is subtracted from each particle diameter, and the result is divided by 2.
[0032] If the thickness of the shell is less than 3 nm, it may be difficult to obtain the strength required to maintain the particle shape. On the other hand, if the thickness exceeds 12 nm, it may be difficult to obtain a resist film with a low refractive index due to the high particle refractive index. The thickness of the shell is preferably 3 to 9 nm, more preferably 3 to 7 nm, and even more preferably 3 to 5 nm.
[0033] The ratio of the shell thickness to the particle diameter of the particles is preferably 3 to 30%. When this ratio is within this range, a resist film with a low refractive index can be obtained.
[0034] Here, if this ratio is less than 3%, it may be difficult to obtain the strength required to maintain the particle shape, and therefore it may be difficult to obtain the particles themselves. Conversely, if the ratio exceeds 30%, the refractive index may not be sufficiently low, and therefore it may be difficult to obtain the desired resist film. This ratio is more preferably 5 to 25%, and even more preferably 7 to 20%.
[0035] The difference between the density of a particle in helium gas and that in nitrogen gas is 0.2 to 1.2 g / cm 3 When the density difference is within this range, a resist film with a low refractive index can be obtained by blending the particles.
[0036] Here, the density difference is 0.2 g / cm 3 If it is less than 1.2 g / cm, the porosity of the particles will be small, and it may be difficult to obtain a resist film with a low refractive index. 3 It is difficult to obtain particles having a density difference exceeding this value. The difference between these densities is more preferably 0.3 to 1.0 g / cm 3 , more preferably 0.4 to 1.0 g / cm 3 It is.
[0037] The shape of the particles is not particularly limited. Examples include spherical, ellipsoidal (rugby ball), cocoon, confetti, chain, and cube shapes. Among these, spherical particles are preferred because they have high dispersibility and can be uniformly dispersed in the film.
[0038] The sphericity of the particles is preferably 0.80 to 1.00. When the sphericity is in this range, a sharp pattern can be formed.
[0039] If the sphericity is less than 0.80, the surface unevenness of the resist film will become large, making it difficult to form a sharp pattern. The sphericity is more preferably 0.85 to 1.00, further preferably 0.90 to 1.00, and particularly preferably 0.95 to 1.00.
[0040] The cavity inside the outer shell of the particle is preferably shaped to follow the outer shape of the particle. This is because, although it depends on the thickness of the outer shell, when stress is applied to the particle, the shell has a uniform thickness, which makes it easy to obtain the strength to maintain the particle shape. Furthermore, it is preferable that the cavity is also spherical in shape similar to the shape of the spherical particle.
[0041] In order to reduce the refractive index and obtain a transparent film, it is preferable that the cavity is substantially one cavity. Here, "substantially one cavity" means that the "ratio of particles having one cavity inside the shell" is 90% or more, although some particles may have "particles having multiple cavities inside the shell" due to particle coalescence or the like. The "number ratio of particles having one cavity inside the shell" is more preferably 95% or more, even more preferably 98% or more, particularly preferably 99% or more, and most preferably 100%.
[0042] The porosity of the particles is preferably 10 to 85%. When the porosity is in this range, a resist film with a low refractive index can be obtained.
[0043] Here, if the porosity is less than 10%, the refractive index is not sufficiently low, so it may be difficult to obtain a desired resist film. Conversely, if the porosity is more than 85%, it may be difficult to obtain the strength required to maintain the particle shape, so it may be difficult to obtain the particle itself. The porosity is more preferably 20 to 85%, and even more preferably 30 to 85%.
[0044] The specific surface area determined by the BET method using nitrogen gas adsorption of particles is 30 to 400 m 2 When the specific surface area is in this range, a resist film with a low refractive index and a sharp pattern can be obtained.
[0045] Here, the specific surface area is 30m 2 If the content is less than 400 m / g, it may be difficult to obtain a sharp pattern, although this depends on the content. 2If it exceeds 1 / g, the refractive index of the resist film may not be sufficiently low due to the small porosity. 2 / g, more preferably 80 to 200m 2 / g.
[0046] The content of silicon in the particles is preferably substantially 100 parts by mass as silica (SiO2) when the total amount of metal elements constituting the particles is expressed as 100 parts by mass on an oxide basis. If the SiO2 content is substantially 100 parts by mass, a film with a low refractive index is easily obtained. In addition, the occurrence of contamination or abnormality due to the elution of metal elements by an alkaline developer during semiconductor manufacturing as described above is suppressed.
[0047] Here, "substantially 100 parts by mass" means that metal elements other than silicon may be contained as impurities, but the total amount of metal elements other than silicon is 10 ppm or less on an oxide basis. Such high-purity particles are suitable for use in resist films used in semiconductor circuits such as highly integrated logic and memory, and optical sensors.
[0048] The ratio (A1 / A2) of the specific surface area (A1) determined by pulse NMR measurement of the aqueous dispersion of the particles to the specific surface area (A2) of the particles determined from the average particle diameter (D) by image analysis of the particles is preferably 0.60 or more. The upper limit of the ratio (A1 / A2) is 1.00. The ratio (A1 / A2) being in this range indicates high compatibility with an alkaline developer. When such particles are used in a resist material, a resist film with excellent developability can be obtained.
[0049] Here, if the ratio (A1 / A2) is less than 0.60, it may be difficult to obtain a sharp pattern. This ratio (A1 / A2) is more preferably 0.65 or more, and further preferably 0.70 or more.
[0050] Pulsed NMR is a measurement method in which magnetization in a thermal equilibrium state in a static magnetic field is excited by irradiating it with pulsed radio waves of several tens of MHz, and the phenomenon in which the excited magnetization returns to the original thermal equilibrium state over time is observed. Liquid molecules in contact with or adsorbed onto the particle surface respond differently to changes in the magnetic field than liquid molecules in a free state that are not in contact with the particle surface.
[0051] In general, the motion of liquid molecules adsorbed to particle surfaces is restricted, while liquid molecules not adsorbed to particle surfaces can move freely. As a result, the relaxation time of liquid molecules adsorbed to particle surfaces is shorter than the relaxation time of other liquid molecules. The relaxation time observed in a liquid containing dispersed particles is the average of two relaxation times reflecting the liquid volume concentration on the particle surfaces and the liquid volume concentration in the free state.
[0052] Incidentally, the specific surface area (A1) of particles in a dispersion liquid determined by pulse NMR measurement indicates the specific surface area of the part of the particle that is wetted by the dispersion medium. Particles that have been surface-treated with an organosilicon compound have fewer silanol groups on the particle surface than the original particles due to the reaction between the organosilicon compound and the silanol groups on the particle surface, so the specific surface area of the part of the particle that is wetted by the hydrophilic dispersion medium is smaller. For this reason, the value of this specific surface area (A1) changes depending on the degree of surface treatment of the particles with an organosilicon compound. The value of the specific surface area (A1) also changes depending on the type of dispersion medium used during measurement.
[0053] Therefore, the ratio (A1 / A2) is an index as to the amount of the organosilicon compound contained in the surface-treated particles.
[0054] The specific surface area (A1) of the particles is obtained from the following formula (4) using the volume concentration (Ψp) of the particles calculated from the following formula (3). Ψp=(Sc / Sd) / [(1-Sc) / Td] Formula (3) (where Sc is the solid concentration of the particles in the dispersion (% by mass), Sd is the density of the particles (g / cm 3 ), and Td is the density of the dispersion medium at 25°C (g / cm 3)
[0055] Here, the solid content concentration is the concentration of particles converted as solid content in the dispersion liquid (hereinafter the same). Sd is the sum of the value obtained by multiplying the density of the constituent component of the particle by its volume ratio and the value obtained by multiplying the density of the constituent component inside the particle by its volume ratio. Here, if the constituent component of the particle is silica, 2.2 is used (the unit is g / cm 3 ) If the constituent inside the particle is air, the density is 0.0 g / cm 3 , and in the case of other gases or liquids, the density corresponding thereto is used. For example, in the case of the particles of the present invention, the porosity is used as the volume ratio of the hollow parts. The porosity of a particle is defined as the ratio of the hollow parts in the particle to the total volume of the particle. Specifically, first, a TEM photograph of the particle is taken. At this time, the hollow parts of the particle have a low density, so the contrast of that part is low. Conversely, the outer shell part has a high density, so the contrast of that part is high. The hollow parts and the outer shell part of the particle can be confirmed by this contrast difference. More specifically, image processing is performed on any 300 particles in the TEM photograph to determine the area of the hollow parts, and the circle equivalent diameter is calculated from the area, which is taken as the average diameter of the hollow parts. The shape of the particles at this time is assumed to be a perfect sphere, and the average volume of the primary particles and the average volume of the hollow parts are calculated. The porosity is expressed as the ratio of the average volume of the hollow parts to the average volume of the primary particles. Furthermore, when the dispersion medium is water, for example, Td is 1.00 g / cm 3 If other types of dispersion media or mixtures of dispersion media are used, use the appropriate densities. A1={[(Ra / Rb)-1]×Rb} / (Ka×Ψp)...Equation (4) (In the formula, A1 is the specific surface area of the particle (m 2 / g), Ra is the inverse of the relaxation time of pulse NMR in the measurement of the dispersion liquid, Rb is the inverse of the relaxation time of pulse NMR in the measurement of the dispersion medium, and Ka is a coefficient depending on the dispersion medium and particles used.
[0056] The coefficient Ka is calculated assuming that the specific surface area (A2) obtained from the average particle diameter (D) of the particles is the same as the specific surface area (A3) obtained by pulse NMR measurement of a dispersion of particles that have not been surface-treated.
[0057] The specific surface area (A2) of the particles can be calculated using the average particle diameter (D) of the particles according to the following formula (5). A2=6000 / Sd / D...Formula (5) (where Sd is the particle density (g / cm 3 )
[0058] The specific surface area (A3) of particles that have not been surface-treated can be obtained from equation (6) using the particle volume concentration (Ψp) obtained from equation (3). A3={[(Rc / Rd)-1]×Rd} / (Ka×Ψp)...Equation (6) (In the formula, A3 is the specific surface area of the particle (m 2 / g), Rc is the inverse of the relaxation time of pulse NMR in the measurement of the particle dispersion, Rd is the inverse of the relaxation time of pulse NMR in the measurement of the dispersion medium, and Ka is a coefficient depending on the dispersion medium and particles used.
[0059] Here, the coefficient Ka is set so that the specific surface area (A2) and the specific surface area (A3) have the same value. Therefore, from the formulas (5) and (6), Ka={[(Rc / Rd)-1]×Rd} / (Ψp×A2)...Equation (7) It can be calculated as:
[0060] Particle 29 In the area Q1 of the peak appearing at a chemical shift of -78 to -88 ppm, the area Q2 of the peak appearing at a chemical shift of -88 to -98 ppm, the area Q3 of the peak appearing at a chemical shift of -98 to -108 ppm, and the area Q4 of the peak appearing at a chemical shift of -108 to -120 ppm in the Si-NMR spectroscopy, it is preferable that (Q4 / ΣQ)×100 is less than 90%, where ΣQ=Q1+Q2+Q3+Q4.
[0061] The peak assigned to Q1 is due to one (-OSi) group and three (-OH) groups bonded to a Si atom, the peak assigned to Q2 is due to two (-OSi) groups and two (-OH) groups bonded to a Si atom, the peak assigned to Q3 is due to three (-OSi) groups and one (-OH) group bonded to a Si atom, and the peak assigned to Q4 is due to four (-OSi) groups bonded to a Si atom. If the ratio of (Q4 / ΣQ) is within this range, the amount of silanol groups is high and compatibility with alkaline developer is high, resulting in a resist film with excellent developability.
[0062] Here, if the ratio of (Q4 / ΣQ) is 90% or more, the number of silanol groups is small, so the compatibility with the alkaline developer is low, which may make it difficult to form a sharp pattern or may cause particle-derived residues to be generated on the substrate.The ratio of (Q4 / ΣQ) is more preferably less than 85%.
[0063] As previously mentioned, the particles have a given number density of silanol groups.
[0064] In addition to the silanol group, the particle shell preferably contains at least one functional group selected from an alkyl group, an acryloyl group, a (meth)acryloyl group, a vinyl group, a mercapto group, and an epoxy group. When the particles contain these functional groups, the particles have high dispersibility in a dispersion liquid, a coating liquid for forming a resist film, and a resin, and the bond with the resin is also improved. Among them, the alkyl group, the epoxy group, the acryloyl group, and the (meth)acryloyl group are preferred because of their high bond with the resin.
[0065] Furthermore, the particle shell preferably contains at least one functional group selected from a hydroxyl group, a carboxyl group, and an amino group. Here, the hydroxyl group may be derived from a silanol group or may be other groups. When these functional groups are present in the particles, the compatibility of the particles with an alkaline developer is improved. Among them, hydroxyl groups and carboxyl groups are more preferred in terms of ease of introduction of functional groups into the particle shell.
[0066] These functional groups can be identified by measuring and analyzing the dry powder of the particles using a Fourier transform infrared spectrometer (FT-IR).
[0067] The particles may be surface-treated with an organosilicon compound. The organosilicon compound is preferably one having the above-mentioned functional group. For example, one represented by the following formula (8) can be mentioned. When the particles are surface-treated with such an organosilicon compound, they show high dispersibility in a dispersion liquid of the particles, a coating liquid for forming a resist film, or a resin, and a sharp pattern can be obtained. R n -SiX 4-n ...Equation (8) (In the formula, R represents an unsubstituted or substituted hydrocarbon group having 1 to 10 carbon atoms, and may be the same or different. Examples of the substituent include an alkyl group, a vinyl group, an epoxy group, an acryloyl group, a (meth)acryloyl group, an alkoxy group, a mercapto group, a glycidoxy group, a carboxyl group, an amino group, a phenyl group, and a phenylamino group. X represents an alkoxy group having 1 to 4 carbon atoms, a hydroxyl group, or a hydrogen atom, and n represents an integer of 0 to 4.)
[0068] Specific examples include the organosilicon compounds shown in Table 1. Among them, organosilicon compounds containing at least one of an alkyl group, an epoxy group, an acryloyl group, and a (meth)acryloyl group are more preferable because they have a high bond strength with the resin.
[0069] [Table 1]
[0070] The carbon content of the particles can be measured by a carbon-sulfur analyzer. For example, the organic silicon compound surface-treated on the particles is separated from the unreacted organic silicon compound by centrifugation. Only the particles surface-treated with the organic silicon compound are taken out and dried to obtain a particle powder, which is then measured to determine the carbon content of the particles.
[0071] The carbon content of the particles is preferably 3.0% by mass or less. When the carbon content is in this range, the particles have good dispersibility in a dispersion liquid and high compatibility with an alkaline developer, so that a resist film having excellent developability can be obtained.
[0072] Here, even if the carbon content exceeds 3.0% by mass, the dispersibility and stability are not improved, and a sharp pattern is not easily obtained. Rather, excessive bonding with the resin may cause development to become difficult, or the compatibility with the alkaline developer may decrease, causing particle-derived residues to occur on the substrate. The lower limit of the carbon content is not particularly set, but is, for example, 0.1% by mass. If the carbon content is less than 0.1% by mass, it may be difficult to obtain sufficient dispersibility and stability in the coating liquid for forming a resist film or in the resin. When such particles are used in a resist film, bonding with the resin may be insufficient, making it difficult to form a sharp pattern. This carbon content is more preferably 0.1 to 2.5% by mass, and even more preferably 0.1 to 2.0% by mass.
[0073] This carbon content varies depending on the structure and amount of the surface-treated organosilicon compound. It is preferable that this carbon content is derived from the functional group contained in the particle shell. Here, for example, when the raw material used to prepare the "original particles" before surface treatment with the organosilicon compound does not depend on the organosilicon compound, and the organosilicon compound of formula (8) is used as a surface treatment agent for the original particles, the above-mentioned preferable carbon content of 0.1 to 3.0 mass% is calculated by adding the organosilicon compound as a solid content (R n -SiO (4-n) / 2 The surface-treated particles contain about 0.2 to 7.5 parts by mass of silicon monoxide as the organic silicon compound raw material for preparing the "original particles." Examples of the organic silicon compound raw material for preparing the "original particles" include alkoxysilanes such as tetramethoxysilane (TMOS), tetraethoxysilane (TEOS), and phenyltrimethoxysilane.
[0074] Here, if the amount of the organosilicon compound contained in the surface-treated particles is less than 0.2 parts by mass relative to 100 parts by mass of the original particles, sufficient dispersibility and stability cannot be obtained, and when the particles are used in a resist film, the bond with the resin is insufficient, which may make it difficult to form a sharp pattern. Conversely, even if the amount of the above-mentioned organosilicon compound exceeds 7.5 parts by mass, the dispersibility and stability are not further improved, and a sharp pattern is not easily obtained. Rather, there is a risk that excessive bonding with the resin makes it difficult to develop, or that compatibility with the alkaline developer is reduced, resulting in particle-derived residues on the substrate. The amount of the surface treatment is more preferably 0.2 to 6.0 parts by mass, and even more preferably 0.2 to 4.5 parts by mass. Incidentally, when the "original particles" are prepared using an organosilicon compound as a raw material, the "original particles" contain carbon, so that the solid content of the organosilicon compound introduced into the particles as a surface treatment agent to obtain the target carbon content of the particles of the present invention is reduced according to the carbon content of the "original particles" compared to the case of surface-treating "original particles not containing carbon".
[0075] The carbon content of this particle is R A The number density of silanol groups on the particle surface calculated by the Sears measurement method described above is R B Then, (R B / R A ) is preferably 0.2 to 25. If this value is within this range, high dispersibility in the particle dispersion, in the coating liquid for forming a resist film, and in the resin, high binding property with the resin, and high compatibility between the particle and the alkaline developer can be obtained without excess or deficiency.
[0076] Here, if this value is less than 0.2, the compatibility with the alkaline developer is low, so that it may be difficult to form a sharp pattern, or particle-derived residues may be generated on the substrate. Conversely, if this value exceeds 25, the bond with the resin may be insufficient, so that the bond with the resin may be weak, and the formation of the pattern itself may be difficult. This value is more preferably 0.5 to 15, and further preferably 1.0 to 10.
[0077] The dispersion medium and concentration of the dispersion liquid are not particularly limited as long as the particles are stably dispersed in the liquid without causing aggregation or precipitation.
[0078] Examples of the dispersion medium include water, alcohols, esters, glycols, ethers, ketones, and aprotic polar solvents. These may be used alone or in combination of two or more. In particular, for resist materials, the dispersion medium is one that contains at least one organic solvent having a solubility parameter (SP value) of 10 or more and a boiling point of more than 100° C. under atmospheric pressure, taking into consideration the workability of the resist material. Here, if the SP value is less than 10, the particles have low dispersibility and may aggregate. In addition, if the organic solvent has a boiling point of 100° C. or less, the organic solvent dries quickly during application and forms a film before leveling, so that defects such as particle-derived aggregates may occur in the coating film.
[0079] Examples of organic solvents having an SP value of 10 or more and a boiling point exceeding 100° C. include propylene glycol monomethyl ether (PGME), propylene glycol monomethyl ether acetate (PGMEA), ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-normal butyl ether, acetylacetone, ethylene glycol, diphenyl ether, glycerol, formamide, benzyl alcohol, N-methylpyrrolidone, glycerin, cyclohexanone, diethylene glycol monoethyl ether, ethylene glycol monophenyl ether, γ-butyrolactone, diethyl phthalate, dimethyl phthalate, dimethyl sulfoxide, 4-hydroxy-4-methyl-2-pentanone, 1-butanol, 2-butanol, 1,3-butanediol, 1,4-butanediol, and 1,4-dioxane. Among these, PGME, PGMEA, and γ-butyrolactone are preferred for resist applications.
[0080] The concentration of the dispersion liquid is preferably 1 to 40% by mass in terms of the solid content of the particles. If the solid content is less than 1% by mass, the processing time may be long when producing the coating liquid. Conversely, if the solid content exceeds 40% by mass, the stability of the dispersion liquid may decrease. The concentration of the dispersion liquid is more preferably 5 to 35% by mass, and further preferably 10 to 30% by mass.
[0081] [Method of manufacturing particle dispersion liquid] The method for producing a particle dispersion according to the present invention includes a first step of preparing an alkaline aqueous solution, a second step of simultaneously adding to the alkaline aqueous solution a solution of a silicon-containing compound and an aqueous solution of an alkali-soluble compound of an inorganic element other than silicon, such that the molar ratio (MOx / SiO2) of the reaction solution at the end of the addition is 0.2 to 15, where the oxide of silicon is represented as SiO2 and the oxide of the inorganic element other than silicon is represented as MOx, to prepare a dispersion of composite oxide particles a, and a third step of adding a solution of a silicon-containing compound and an aqueous solution of an alkali-soluble compound of an inorganic element other than silicon in a molar ratio (MOx / SiO2) smaller than that in the second step to prepare a dispersion of composite oxide particles a. The method includes, in order, a third step of preparing a dispersion of composite oxide particles b, a fourth step of adding an acid to the dispersion of composite oxide particles b to remove at least a part of the elements other than silicon that constitute the composite oxide particles b to prepare a dispersion of silica-based particles, a fifth step of removing metal impurities selected from alkali metals, alkaline earth metals, Co, Cr, Cu, Fe, Mn, Ni, Ti, Zn, and Zr from the dispersion of silica-based particles to prepare a dispersion of silica particles having a total content of these metal impurities of 1000 ppb or less, and a sixth step of heating the dispersion of silica particles to 60 to 200°C and then lowering the temperature to less than 50°C. This results in a dispersion of hollow silica particles.
[0082] Here, by adjusting the average particle size of the composite oxide particles b prepared in the third step to 15 to 150 nm and the value obtained by subtracting the average particle size of the composite oxide particles a from the average particle size of the composite oxide particles b and dividing the result by 2 to 3 to 14 nm, it becomes easy to adjust the average particle size and shell thickness of the desired particles.
[0083] The particles produced in this way have a low refractive index and a low content of metal impurities. Therefore, they can be used in resist materials that require high purity. When these particles are used in resist films, high developability can be achieved during pattern formation. Each process is described below.
[0084] [First step] First, an alkaline aqueous solution is prepared.
[0085] Here, the alkaline aqueous solution preferably contains an element that becomes an amphoteric oxide. The element that becomes an amphoteric oxide means that an oxide containing the element dissolves in an acid having a pH of 3 or less and dissolves in an alkali having a pH of 10 or more. More specifically, it contains at least one element selected from Al, As, B, Bi, Cd, Co, Fe, Ga, Ge, In, Pb, Sb, Si, Sn, Ti, V, Zn, and Zr. Among them, Al is preferable because it reacts with a compound containing silicon to easily form a composite oxide particle. Similarly, Si (silicon) is preferable because it reacts with a compound containing silicon easily. Examples of alkaline aqueous solutions containing these suitable elements include aqueous solutions of sodium aluminate, aluminum hydroxide, and sodium silicate.
[0086] The alkaline aqueous solution is not particularly limited as long as it has a pH of more than 7. When an amphoteric element is dissolved and present, the pH is preferably 10 or more. This pH is more preferably 10.5 or more, even more preferably 11 or more, and particularly preferably 11 to 13. This alkaline aqueous solution may also contain particles containing the above-mentioned "element that becomes an amphoteric oxide". If particles are contained in the alkaline aqueous solution, it is preferable because particles having a relatively uniform particle size are easily obtained in the end. The particles containing the "element that becomes an amphoteric oxide" in this alkaline aqueous solution preferably have an average particle size of 5 to 25 nm.
[0087] Here, if the average particle diameter of the particles is less than 5 nm, it is difficult to obtain the particles themselves. Conversely, if the average particle diameter exceeds 25 nm, there is a risk that metal impurities will not be sufficiently removed in the process described below, or that the refractive index of the particles of the present invention finally obtained will not be sufficiently low. In addition, there is a risk that it will be difficult to obtain a desired resist film. This average particle diameter is more preferably 5 to 20 nm, and even more preferably 5 to 15 nm.
[0088] In addition, the particles containing "an element that becomes an amphoteric oxide" in the alkaline aqueous solution preferably have a sphericity of 0.6 to 1.0. If the sphericity is within this range, the sphericity of the final particles tends to be high. Note that a particle with a sphericity of 1.0 has a perfectly spherical shape.
[0089] If the sphericity of the particles is less than 0.6, the sphericity of the particles of the present invention finally obtained will be low, and it may be difficult to form a sharp pattern. The sphericity is more preferably 0.8 to 1.0, even more preferably 0.9 to 1.0, and most preferably 1.0.
[0090] The oxide-equivalent concentration of the element that becomes the amphoteric oxide in the alkaline aqueous solution is preferably less than 5.0% by mass. At this concentration, particles with a relatively uniform particle size and high sphericity are easily obtained. The lower limit of this concentration is not particularly set, but from the viewpoint of stably obtaining particles with a uniform particle size and high sphericity, it is, for example, 0.1% by mass. This concentration is more preferably less than 4.0% by mass, and even more preferably less than 3.5% by mass.
[0091] The ratio of the "element that becomes an amphoteric oxide" in the first step in the composite oxide particles a prepared in the second step is preferably 3 to 90 parts by mass on an oxide basis when the composite oxide particles a are taken as 100 parts by mass. If the ratio of the element that becomes an amphoteric oxide in the alkaline aqueous solution prepared in the first step is within this range, the formation of particle cavities and thinning of the outer shell become easier in the acid treatment in the fourth step described below, and particles with a low refractive index can be obtained.
[0092] If the ratio is less than 3 parts by mass, it may be difficult to form a thin shell, and it may be difficult to obtain particles with a low refractive index. Conversely, if the ratio exceeds 90 parts by mass, the particle growth in the second step may be insufficient. This ratio is more preferably 10 to 80 parts by mass, and even more preferably 20 to 70 parts by mass.
[0093] Silicon is one of the elements that become amphoteric oxides. However, if the proportion of "silicon that becomes amphoteric oxide" in the alkaline aqueous solution in the first step in the composite oxide particles a prepared in the second step is high, the refractive index of the particles finally obtained may be too high. Therefore, when the oxide of silicon contained in this alkaline aqueous solution is expressed as SiO2 and the oxide of an amphoteric element other than silicon is expressed as MOx, the molar ratio (MOx / SiO2) is preferably 10 or more. Since this alkaline aqueous solution may not contain silicon, no upper limit is set for the molar ratio (MOx / SiO2).
[0094] In addition, elements that are treated as impurities, such as alkali metals and alkaline earth metals, and that are not "elements that form amphoteric oxides" and are not "elements that constitute particles", are not included in the 100 parts by mass of the above complex oxide a.
[0095] [Second process] A solution of a compound containing silicon and an aqueous solution of an alkali-soluble compound of an inorganic element other than silicon are simultaneously added to the "alkaline aqueous solution containing an element that becomes an amphoteric oxide" prepared in the first step so that the molar ratio (MOx / SiO2) of the reaction solution at the end of the addition is 0.2 to 15, where SiO2 is the oxide of silicon and MOx is the oxide of an inorganic element other than silicon. To prepare a dispersion of composite oxide particles a.
[0096] Here, the compound containing silicon may be, for example, at least one selected from the group consisting of silicates, acidic silicic acid solutions, and organic silicon compounds.
[0097] The silicate is preferably one or more silicates selected from alkali metal silicates, ammonium silicates, and silicates of organic bases. Examples of the alkali metal silicate include sodium silicate and potassium silicate. Examples of the organic base include quaternary ammonium salts such as tetraethylammonium salts, and amines such as monoethanolamine, diethanolamine, and triethanolamine. Examples of the ammonium silicate or the silicate of organic base include alkaline solutions in which ammonia, quaternary ammonium hydroxide, amine compounds, etc. are added to a silicic acid solution.
[0098] As the acidic silicic acid solution, a silicic acid solution obtained by removing the alkali by treating an aqueous alkali silicate solution with a cation exchange resin or the like can be used, and an acidic silicic acid solution having a pH of 2 to 4 is particularly preferred.
[0099] As the organosilicon compound, those in which n is 0 to 3 in the above-mentioned formula (8) are preferred.
[0100] Incidentally, in the organosilicon compound of formula (8), compounds in which n is 1 to 3 are poorly hydrophilic, so it is preferable to hydrolyze them in advance so that they can be mixed uniformly in the reaction system. Well-known methods can be adopted for the hydrolysis. When a basic catalyst such as an alkali metal hydroxide, aqueous ammonia, or amine is used as a hydrolysis catalyst, the basic catalyst can be removed after hydrolysis and the solution can be used as an acidic solution. When an acidic catalyst such as an organic acid or an inorganic acid is used to prepare a hydrolyzate, it is preferable to remove the acidic catalyst by ion exchange or the like after hydrolysis. The obtained hydrolyzate of the organosilicon compound is preferably used in the form of an aqueous solution. Here, the aqueous solution means that the hydrolyzate is not in a cloudy gel state and is transparent.
[0101] Examples of the organosilicon compound include those in which n is 0 to 3, as described in Table 1 above. Among them, the relationship between the carbon content of the particles and the number density of silanol groups on the particle surface (R B / R AIn terms of ease of adjusting the value of (R) to a desired range, for example, TMOS, TEOS, 3-methacryloxypropyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyldimethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, and 8-methacryloxyoctyltrimethoxysilane are preferred.
[0102] Examples of alkali-soluble compounds of inorganic elements other than silicon include alkali metal salts or alkaline earth metal salts, ammonium salts, and quaternary ammonium salts of metal or nonmetal oxoacids that form oxides of inorganic elements other than silicon, specifically sodium aluminate, sodium tetraborate, ammonium zirconyl carbonate, potassium antimonate, potassium stannate, sodium aluminosilicate, sodium molybdate, ammonium cerium nitrate, and sodium phosphate.
[0103] These "compounds containing silicon" and "compounds of inorganic elements other than silicon" have high solubility on the alkaline side. However, when the two are mixed in the pH range where they have high solubility, the solubility of oxo acid ions such as silicate ions and aluminate ions decreases, and these compounds precipitate to form colloidal particles.
[0104] Next, the molar ratio (MOx / SiO2) will be explained.
[0105] When the aforementioned "alkali-soluble compound of inorganic elements other than silicon" is expressed as an oxide, suitable examples include one or more of Al2O3, As2O3, B2O3, Bi2O3, CdO, CoO, Fe2O3, Ga2O3, GeO2, In2O3, PbO, Sb2O3, SnO2, TiO2, VO, ZnO2, and ZrO2. In addition, examples of composite oxides of inorganic elements other than silicon include zinc alumina oxide and indium tin oxide. These oxides are called MOx, and the number of moles is used to calculate the molar ratio. If multiple types of these oxides are present in the reaction system, the total number of moles of each oxide is used. In addition, the number of moles when the aforementioned "compound containing silicon" is expressed as SiO2 is used to calculate the molar ratio here.
[0106] The molar ratio in the second step is calculated including the "element that becomes an amphoteric oxide" used in the first step.
[0107] In addition, alkali metals and alkaline earth metals are not "elements that make up particles" but are treated as impurities, so they are not included in the above MOx.
[0108] These points will be similarly addressed in the third step described below.
[0109] When the molar ratio (MOx / SiO2) in the second step is 0.2 to 15, the structure of the composite oxide particles is mainly a structure in which silicon and elements other than silicon are alternately bonded with oxygen interposed therebetween. That is, many structures are generated in which oxygen atoms are bonded to the four bonds of a silicon atom, and an element M other than silicon is bonded to these oxygen atoms. As a result, when the element M other than silicon is removed in the fourth step described later, the shape of the composite oxide particles is not destroyed, and the silicon atoms can also be removed as silicic acid monomers or oligomers accompanying the element M.
[0110] If the molar ratio is less than 0.2, the ratio of "elements other than silicon" removed in the fourth step described below is small, so that the cavity volume of the finally obtained particles may not be sufficiently large. Conversely, if the molar ratio exceeds 15, the particle growth is suppressed, and the production efficiency until the desired average particle diameter of the composite oxide particles a is satisfied may be reduced. This molar ratio is preferably 0.4 to 10, more preferably 0.6 to 5.0.
[0111] In this way, the composite oxide particles a obtained in the second step are removed by acid treatment in the fourth step described below, forming a cavity inside the outer shell of the finally obtained particles. Therefore, the composite oxide particles a are preferably in a form that can be easily removed by acid treatment.
[0112] For example, when "a solution of a compound containing silicon" and "a solution of an alkali-soluble compound of an inorganic element other than silicon" are added in the second step to "an alkaline aqueous solution containing an element that becomes an amphoteric oxide" having a molar ratio (MOx / SiO2) of 10 or more in the first step, the molar ratio (MOx / SiO2) in the reaction solution can be reduced as the addition proceeds. By reducing the molar ratio (MOx / SiO2) in the reaction solution in this way, the molar ratio (MOx / SiO2) of the resulting composite oxide particles a can also be reduced from the center of the particles toward the outside. If there is a molar ratio gradient in the particles in this way, when removing at least a part of the elements other than silicon that constitute the composite oxide particles b in the acid treatment in the fourth step described later, the parts corresponding to the composite oxide particles a can be efficiently removed, which makes it easy to form particle cavities and thin the outer shell, and allows the production of particles with a low refractive index.
[0113] The concentration of the solution of the "silicon-containing compound" and the concentration of the aqueous solution of the "alkali-soluble compound of inorganic elements other than silicon" are preferably 0.05 to 3.0 mass% as SiO2 and MOx, respectively. When the concentrations are within this range, adhesion between particles is suppressed, and particles with high sphericity can be obtained.
[0114] Here, if the concentration of the solution of the "silicon-containing compound" and the concentration of the aqueous solution of the "alkali-soluble compound of inorganic elements other than silicon" are less than 0.05 mass% as SiO2 and MOx, respectively, the particle growth rate is slow, and the production efficiency until the desired average particle size of the composite oxide particles a is satisfied may be low. Conversely, if the concentration exceeds 3.0 mass%, the particles may coalesce with each other, resulting in irregular particle shapes or aggregation of the particles.
[0115] In the addition of the solution in this step, the pH of the reaction system is preferably 10 or more, and the temperature is preferably 50 to 98°C. If the pH and temperature are within these ranges, the composite oxide particles a can efficiently grow by adding the "solution of a silicon-containing compound" and the "aqueous solution of an alkali-soluble compound of an inorganic element other than silicon". The pH is more preferably 10.5 or more, and even more preferably 10.5 to 13. The temperature is more preferably 65 to 98°C, and even more preferably 80 to 98°C.
[0116] The composite oxide particles a are preferably adjusted so that their average particle size (Da) is approximately 10 to 145 nm.
[0117] Here, if the average particle diameter (Da) is less than 10 nm, the shell of the particles finally obtained may be thick, and the cavity volume of the particles may not be sufficiently large. Conversely, if it exceeds 145 nm, the removal of elements M other than silicon in the fourth step described below may be insufficient, and the cavity volume of the particles may not be sufficiently large, making it difficult to obtain particles with a low refractive index, or the particle diameter may be large, making it difficult to form a sharp pattern. The average particle diameter (Da) is more preferably 15 to 115 nm, even more preferably 20 to 75 nm, and particularly preferably 20 to 50 nm.
[0118] [Third step] In this step, a solution of a compound containing silicon and an aqueous solution of an alkali-soluble compound of an inorganic element other than silicon are added to the dispersion of composite oxide particles a in a molar ratio (MOx / SiO2) smaller than that in the second step, thereby growing the composite oxide particles a and preparing a dispersion of composite oxide particles b.
[0119] The composite oxide particles b are prepared so that the average particle diameter is 15 to 150 nm, and the value obtained by subtracting the average particle diameter of the composite oxide particles a from the average particle diameter of the composite oxide particles b and dividing the result by 2 is 3 to 14 nm.
[0120] In the composite oxide particle b, a layer having a lower molar ratio (MOx / SiO2) than the composite oxide particle a is formed around the composite oxide particle a. This layer is less susceptible to acid attack than the composite oxide particle a, and therefore forms the outer shell of the final particle.
[0121] The silicon-containing compound and the alkali-soluble non-silicon inorganic element compound used in the third step are selected from those exemplified in the second step. These compounds may be the same as those used in the second step, or may be different from those exemplified in the second step.
[0122] If the molar ratio (MOx / SiO2) in the second step is A and the molar ratio (MOx / SiO2) in the third step is B, it is preferable to set the ratio (B / A) to less than 0.40. If the ratio (B / A) is less than 0.40, the silica component in the surface layer of the composite oxide particles increases, and the formation of the outer shell becomes easy. As a result, even if elements other than silicon are removed in the fourth step described below, the shape of the composite oxide particles is not destroyed, and hollow silica particles can be stably obtained. If the ratio (B / A) is 0.40 or more, it is difficult to form an outer shell containing a large amount of silica components, so that the composite oxide particles are destroyed when removing elements other than silicon in the fourth step, making it difficult to maintain the particle shape. For this reason, there is a risk that it may be difficult to obtain hollow silica particles. The ratio (B / A) is more preferably 0.30 or less, and even more preferably 0.20 or less.
[0123] The average particle size (Db) of the composite oxide particles b after the addition is adjusted to be 15 to 150 nm.
[0124] Here, if the average particle size (Db) is less than 15 nm, the porosity of the particles will be small, and it may be difficult to obtain a film with a low refractive index. Conversely, if it exceeds 150 nm, the particle size will be large, and it may be difficult to form a sharp pattern. The average particle size (Db) is preferably 20 to 120 nm, more preferably 25 to 80 nm, and particularly preferably 25 to 55 nm.
[0125] Moreover, the value (Dc) obtained by dividing the difference between the average particle size (Db) and the average particle size (Da) by 2 is adjusted to be 3 to 14 nm.
[0126] Here, if the difference (Dc) is less than 3 nm, the shell finally obtained may be too thin, making it difficult to maintain the particle shape. Conversely, if the particle is more than 14 nm, the refractive index may not be sufficiently low, making it difficult to obtain a desired resist film, or metal impurities may not be sufficiently removed. The difference (Dc) is more preferably 3 to 10 nm, and even more preferably 3 to 6 nm.
[0127] The ratio (Dc / Db) is preferably from 0.03 to 0.35. When this ratio is in this range, a resist film with a low refractive index can be obtained.
[0128] Here, if this ratio is less than 0.03, it may be difficult to obtain the strength required to maintain the particle shape, and therefore it may be difficult to obtain the particles themselves. Conversely, if the ratio exceeds 0.35, the refractive index of the particles may not be sufficiently low, and therefore it may be difficult to obtain the desired resist film. The ratio (Dc / Db) is more preferably 0.04 to 0.28, and even more preferably 0.05 to 0.20.
[0129] The dispersion of composite oxide particles a used in this step preferably has a pH of 10 or more.
[0130] The concentration of the solution of the "silicon-containing compound" and the concentration of the aqueous solution of the "alkali-soluble compound of inorganic elements other than silicon" are preferably 0.05 to 3.0 mass% as SiO2 and MOx, respectively. When the concentrations are within this range, adhesion between particles is suppressed, and monodisperse particles can be obtained.
[0131] In the addition of the solution in this step, the pH of the reaction system is preferably 10 or more, and the temperature is preferably 50 to 98°C. If the pH and temperature are within these ranges, the composite oxide particles b can be efficiently grown by adding the "solution of a silicon-containing compound" and the "aqueous solution of an alkali-soluble compound of an inorganic element other than silicon". The pH is more preferably 10.5 or more, and even more preferably 10.5 to 13. The temperature is more preferably 65 to 98°C, and even more preferably 80 to 98°C.
[0132] [Fourth step] In this step, an acid is added to the dispersion of composite oxide particles b to remove at least a portion of the elements other than silicon that constitute composite oxide particles b, thereby preparing a dispersion of silica-based particles. The elements are removed, for example, by dissolving them using a mineral acid or an organic acid, by contacting them with a cation exchange resin to remove them by ion exchange, or by a combination of these methods.
[0133] The concentration of the composite oxide particles b in the dispersion liquid differs depending on the treatment temperature, but is preferably 0.1 to 30 mass % in terms of the composite oxide particles b converted into oxide.
[0134] Here, if the concentration is less than 0.1% by mass, the amount of dissolved silica increases, which may make it difficult to maintain the shape of the composite oxide particles. In addition, the treatment efficiency is low due to the low concentration. Conversely, if the concentration is higher than 30% by mass, the dispersibility of the particles may be insufficient. In addition, in the case of composite oxide particles having a high content of elements other than silicon, it may be difficult to remove the elements other than silicon uniformly or efficiently. The concentration of the dispersion of composite oxide particles b is more preferably 0.5 to 25% by mass.
[0135] The removal of the above elements is preferably carried out until the molar ratio (MOx / SiO2) of the resulting particles becomes 0.03 or less.
[0136] Here, if the molar ratio (MOx / SiO2) is greater than 0.03, it may be difficult to obtain the refractive index of the hollow silica particles finally obtained and the strength required to maintain the particle shape. The molar ratio (MOx / SiO2) is more preferably 0.01 or less.
[0137] The dispersion of silica-based particles from which at least a part of the elements other than silicon has been removed can be washed by a known washing method such as ultrafiltration as necessary. At least a part of the dissolved elements other than silicon is removed by washing. In this case, if a part of the alkali metal ions and the like in the dispersion is removed in advance and then ultrafiltration is performed, a dispersion of silica-based particles with high dispersion stability can be obtained.
[0138] [Fifth step] In this step, metal impurities selected from alkali metals, alkaline earth metals, Co, Cr, Cu, Fe, Mn, Ni, Ti, Zn, and Zr are removed from the dispersion of silica-based particles obtained in the fourth step to prepare a dispersion of silica particles having a total content of these metal impurities of 1000 ppb or less relative to the silica particles.
[0139] The metal impurities can be removed by subjecting the dispersion of silica-based particles obtained in the fourth step to an acid treatment or contacting the dispersion with at least one of a cation exchange resin and an anion exchange resin. In this case, it is preferable to repeatedly perform the operations of heating the dispersion, acid treatment, and contacting with an ion exchange resin, since this allows the metal impurities to be effectively removed.
[0140] Specifically, the acid treatment is preferably carried out at a pH of 3 or less and a temperature of 40° C. or more. If the pH and temperature are within these ranges, metal impurities can be removed more effectively. Moreover, the ion exchange is preferably carried out at a temperature of 40° C. or more. By repeatedly carrying out these operations such as the acid treatment and ion exchange, metal impurities can be removed more effectively.
[0141] By washing in this manner, it is possible to effectively reduce the content of impurities such as alkali metals in the particles obtained by heat-treating the silica particles in the sixth step, the content of which is in accordance with the content of impurities in the particles described above.
[0142] If the content of impurities in the silica-based particles obtained in the fourth step is within the range of impurities of the particles described above, washing in this step is not particularly required.
[0143] The concentration of the dispersion of silica particles in this step varies depending on the treatment temperature, but is preferably 0.1 to 20 mass % calculated as the oxide.
[0144] [Sixth step] In this step, the dispersion of silica particles obtained in the fifth step is heated to 60 to 200°C, and then cooled to less than 50°C.
[0145] In this way, the silica particle dispersion is heated to dissolve the silicon from the silica particles, and then the temperature of the dispersion is lowered to fix the dissolved silicon to the silica particles, thereby obtaining the particles of the present invention.
[0146] Here, if the heating temperature is less than 60°C, the silicon content in the particles will not dissolve sufficiently, and the particles may not be fixed in the shape of hollow particles. Conversely, if the temperature exceeds 200°C, the silicon content in the particles will dissolve excessively, the outer shell will dissolve, and the hollow shape may collapse. After heating to the target temperature, the temperature may be immediately lowered, but in order to produce stably, it is preferable to maintain the temperature for 30 minutes or more. The heating temperature is preferably 70 to 180°C, more preferably 80 to 160°C.
[0147] After heating the dispersion liquid, the temperature is lowered to less than 50° C. By lowering the temperature to less than 50° C., the dissolved silicon content can be easily fixed to the silica particles. The temperature may be lowered to room temperature to facilitate handling.
[0148] In the heating of the dispersion in this step, the heating rate is preferably 5.0° C. / min or less. At such a heating rate, the sudden dissolution of the silicon content in the particles is suppressed, and the shape of the hollow particles is easily maintained. Therefore, the desired properties such as the refractive index of the particles of the present invention are easily obtained stably. The lower limit of this heating rate is not particularly set, but is, for example, 0.3° C. / min. If the heating rate is extremely slow, it takes too long to raise the temperature to the target temperature, which may result in low production efficiency. The heating rate is preferably 0.5 to 4.0° C. / min, more preferably 0.8 to 3.0° C. / min.
[0149] The particle dispersion thus obtained satisfies the above-mentioned particle properties, and when the particles are used in a resist film, a low refractive index and excellent developability can be achieved.
[0150] [Particle surface treatment] In the present invention, after the fifth step, an organosilicon compound may be added to perform surface treatment of the particles. As the organosilicon compound to be used, it is preferable to use an organosilicon compound represented by the above formula (8) in which n is 1 to 3. Here, when an organosilicon compound in which n is 0 is used, it is preferable to use a partial hydrolyzate of the organosilicon compound. This makes it possible to adjust the number density of silanol groups on the particle surface calculated by the Sears measurement method. In addition, the introduction of a functional group improves the compatibility between the particles and the resin component, which is preferable in terms of obtaining particles with high dispersibility in the coating liquid and film. The organosilicon compounds may be used alone or in combination.
[0151] The method of surface treatment of particles is to first prepare a dispersion liquid of particles. As the dispersion medium, it is preferable to use alcohols such as methanol and ethanol. A predetermined amount of an organosilicon compound represented by formula (8) is added to the dispersion liquid, and the organosilicon compound is hydrolyzed. Water can be added to this hydrolysis as necessary. The ratio (Mw / Mo) of the number of moles of water (Mw) to the number of moles of the organosilicon compound (Mo) used is preferably 1 or more.
[0152] Here, if the ratio (Mw / Mo) is less than 1, hydrolysis may be insufficient, and the transparency and haze of the coating may be insufficient. There is no particular upper limit for this ratio, but if this ratio exceeds 500, the hydrolysis reaction may become intense, and the organosilicon compounds may polymerize with each other, making it difficult to efficiently treat the particle surface with the organosilicon compound. This ratio is more preferably 1 to 100.
[0153] In this hydrolysis, an acid or alkali can be used as a hydrolysis catalyst, if necessary. Among them, ammonia is preferred. This is because if ammonia is used, it is easy to remove even if it remains in the dispersion, and the stability of the dispersion is easily maintained. The number of moles of ammonia used (M N ) and the mole number (Mo) of the organosilicon compound (M N / Mo) is preferably in the range of 0.05 to 50.
[0154] Here, the ratio (M N If the ratio (R / Mo) is less than 0.05, the hydrolysis may be insufficient, and the transparency and haze of the coating may be insufficient. If the ratio exceeds 50, the hydrolysis reaction may become too vigorous, and the organosilicon compounds may polymerize with each other, making it difficult to efficiently treat the particle surfaces with the organosilicon compounds. This ratio is more preferably 0.1 to 10.
[0155] The surface treatment is preferably carried out in a homogeneous system, and in order to promote the reaction between the particles and the organosilicon compound, it is preferable to heat the particles at a temperature below the boiling point of the dispersion medium (for example, room temperature to 120° C.) for 0.5 to 48 hours.
[0156] When the particles, whose surfaces are chemically bonded to the organosilicon compound by this surface treatment, are used in a resist material, the particles have high dispersibility in the film, making it easy to obtain a sharp pattern.
[0157] Examples of the organosilicon compound include those shown in Table 1. The particles may contain one or more of these organosilicon compounds. In the surface treatment, the particles may be treated with one or more of these organosilicon compounds, or may be treated with the same or a mixture of ...
[0158] The amount of this organosilicon compound is 100 parts by mass of the "original particles" before surface treatment. n -SiO (4-n) / 2 ) is preferably 0.2 to 7.5 parts by mass.
[0159] Here, if the amount is less than 0.2 parts by mass, it may be difficult to obtain the sufficient effect of the addition. Conversely, if the amount is more than 7.5 parts by mass, the refractive index of the particles increases, so that it may be difficult to obtain particles having a desired refractive index. The amount of the organosilicon compound is more preferably 0.2 to 6.0 parts by mass, and even more preferably 0.2 to 4.5 parts by mass.
[0160] The amount of surface treatment should be such that only a desired amount of organosilicon compound is reacted with the particle surface and the carbon content of the finally obtained particles is within the range. This carbon content varies depending on the structure and amount of the chemically bonded organosilicon compound. Here, when the raw material used to prepare the "original particles" before surface treatment does not depend on the organosilicon compound, and the organosilicon compound of formula (8) is used as a surface treatment agent for the "original particles", the aforementioned carbon content of 0.1 to 3 mass% is calculated by adding the organosilicon compound to 100 parts by mass of the "original particles" as a solid content (R n -SiO (4-n) / 2 ) is surface-treated in an amount of about 0.2 to 7.5 parts by mass. Of course, when an organosilicon compound is used to prepare the "original particles" and the carbon content is present in the "original particles", the carbon content is also added to the carbon content of the particles finally obtained. Therefore, the amount of solid content of the organosilicon compound that is surface-treated to obtain the target carbon content of the particles of the present invention is reduced according to the carbon content of the "original particles" compared to the case where the surface treatment is performed on "original particles not containing carbon".
[0161] The physical properties and preferred ranges of the finally obtained particles and their dispersion are the same as those of the above-mentioned particles and their dispersion.
[0162] [Coating liquid for film formation] The particles of the present invention can be applied to a coating liquid for forming a coating film. This coating liquid contains particles, a matrix forming component, and a dispersion medium. This dispersion medium contains at least one of water and an organic dispersion medium. In addition to these, the coating liquid may contain additives such as a polymerization initiator, a leveling agent, and a surfactant.
[0163] The concentration of particles in the coating liquid is preferably 5 to 95% by mass as solid content based on the total amount of solid content of the particles, matrix forming components, etc. contained. If the particle concentration is less than 5% by mass, it may be difficult to sufficiently reduce the refractive index of the coating. Conversely, if it is more than 95% by mass, cracks may occur in the coating, the surface unevenness may become large, it may be difficult to obtain a sharp pattern, and transparency and haze may deteriorate. The particle concentration is more preferably 20 to 90% by mass, and even more preferably 35 to 85% by mass.
[0164] The matrix-forming component preferably contains an alkali-soluble group.
[0165] Examples of the alkali-soluble group include a hydroxyl group, a phenolic hydroxyl group, a carboxyl group, a fluorinated alcohol group, a sulfonimide group, a bis(alkylcarbonyl)methylene group, and an alkylene oxide group.
[0166] Examples of the matrix-forming component containing an alkali-soluble group include polycondensates of organosilicon compounds, ultraviolet-curable resins, thermosetting resins, and thermoplastic resins.
[0167] Here, examples of the ultraviolet-curable resin include (meth)acrylic resin, urethane resin, and vinyl resin.
[0168] Examples of the thermosetting resin include urethane resin, melamine resin, silicon resin, butyral resin, reactive silicone resin, phenol resin, epoxy resin, unsaturated polyester resin, and thermosetting acrylic resin.
[0169] Examples of the thermoplastic resin include polyester resin, polycarbonate resin, polyamide resin, polyphenylene oxide resin, thermoplastic acrylic resin, vinyl chloride resin, fluororesin, vinyl acetate resin, and silicone rubber.
[0170] These resins may be copolymers or modified products of two or more kinds, or may be used in combination. Furthermore, these resins may be emulsion resins, water-soluble resins, or hydrophilic resins.
[0171] The components forming these resins are preferably monomers or oligomers in view of particle dispersibility and ease of coating.
[0172] The concentration of the matrix-forming component in the coating liquid is preferably 5 to 95 mass % in terms of solid content with respect to the total amount of solid content of the particles, matrix-forming component, and the like contained therein.
[0173] Here, if the concentration of the matrix-forming component is less than 5% by mass, it is difficult to form a film. Even if a film is obtained, there is a possibility that cracks will occur in the film, the surface irregularities will become large, it will be difficult to obtain a sharp pattern, and transparency, haze, etc. will be deteriorated. Conversely, if it is more than 95% by mass, the amount of particles will be small, so that it may be difficult to sufficiently reduce the refractive index. The concentration of this matrix-forming component is more preferably 10 to 80% by mass, and further preferably 15 to 65% by mass.
[0174] As the organic dispersion medium, one that can uniformly disperse particles and dissolve or disperse additives such as matrix forming components and polymerization initiators is used. Among them, hydrophilic dispersion media and polar dispersion media are preferred. As shown in Table 2, examples of hydrophilic dispersion media include alcohols, esters, glycols, and ethers. Examples of polar dispersion media include esters, ketones, and aprotic dispersion media. These may be used alone or in combination of two or more.
[0175] [Table 2]
[0176] Any additive that can be used in the past for film formation can be used as the additive. For example, a polymerization initiator, a leveling agent, etc. can be used to promote polymerization of the matrix-forming components and improve film-forming properties.
[0177] Examples of the polymerization initiator include those shown in Table 3.
[0178] [Table 3]
[0179] Examples of the leveling agent include acrylic leveling agents, silicone leveling agents, fluorine leveling agents, nonionic leveling agents, cationic leveling agents, and anionic leveling agents. These may be used alone or in combination of two or more. The content of the leveling agent is preferably 0.001 to 1.0% by mass in 100% by mass of the non-volatile components of the dispersion. By containing a leveling agent in this range, it becomes easy to obtain a film with excellent coatability and small surface unevenness.
[0180] Regarding the concentration of these additives in the coating liquid, those contained as solids when the coating is formed are counted as matrix forming components for convenience, and after coating, they are counted as the matrix.
[0181] The solid content concentration of the coating liquid (the ratio of the total solid content of the particles and the solid content of the matrix-forming components to the coating liquid) is preferably 0.1 to 60% by mass.
[0182] Here, if the solid content concentration of the coating liquid is less than 0.1% by mass, it may be difficult to obtain a desired film thickness, or the processing time required for manufacturing the coated substrate may be long, resulting in a decrease in productivity. Conversely, if it is more than 60% by mass, the stability of the coating liquid may decrease. In addition, the viscosity of the coating liquid may increase, resulting in a decrease in coatability. The solid content concentration of the coating liquid is more preferably 1 to 50% by mass.
[0183] [Coated base material] The coating solution is used to form a coating on a substrate.
[0184] Specifically, a coating liquid is applied onto a substrate, and then dried to form a coating film on the substrate. The coating film is then irradiated (exposed) to ultraviolet light or the like, and developed to form a pattern in a desired shape. The pattern is preferably formed by wet etching.
[0185] The method of applying the coating liquid is not particularly limited as long as it can form a coating on the substrate. For example, well-known methods such as spraying, spin coating, roll coating, dip coating, and bar coating can be used. Drying is performed by heating to about 50 to 150°C, for example, to evaporate and remove the dispersion medium. Exposure is performed through a mask. Examples of actinic rays or radiation that can be applied to this exposure include ArF light, KrF light, F2 light, extreme ultraviolet light, vacuum ultraviolet light, electron beams, X-rays, soft X-rays, infrared light, g-rays, h-rays, and i-rays. Thereafter, a pattern is formed on the exposed portion of the coating using an alkaline developer. The coating is mainly formed of particles and a matrix.
[0186] In the case of a coating, the ratio of the particles and the solid content of the matrix-forming components in the coating liquid is the same as the ratio of the particles and the matrix in the coating. As mentioned above, the additives in the coating liquid that remain as solids are counted as the matrix.
[0187] The thickness of the coating is preferably, for example, 50 to 250 nm for an anti-reflection coating, and 500 nm to 5 μm for a resist coating.
[0188] The alkaline developer may be either an inorganic or organic alkaline compound.
[0189] Examples of inorganic alkaline compounds include sodium hydroxide, potassium hydroxide, sodium silicate, potassium silicate, sodium carbonate, potassium carbonate, and ammonia. Examples of organic alkaline compounds include tetramethylammonium hydroxide (TMAH), 2-hydroxyethyltrimethylammonium hydroxide, monomethylamine, dimethylamine, trimethylamine, monoethylamine, diethylamine, triethylamine, monoisopropylamine, diisopropylamine, and ethanolamine. These inorganic and organic alkaline compounds may be used alone or in combination of two or more. The concentration of the alkaline compound in the alkaline developer is preferably 0.01 to 5% by mass.
[0190] The refractive index of the coating is preferably 1.15 to 1.40.
[0191] Here, it is difficult to obtain a coating with a refractive index of less than 1.15. Conversely, if the refractive index exceeds 1.40, it may be difficult to obtain high developability during pattern formation, although this depends on the refractive index of the substrate or the refractive index of another film formed under the coating if necessary. The refractive index of the coating is more preferably 1.15 to 1.35, and even more preferably 1.15 to 1.30.
[0192] The light transmittance of the coated substrate is preferably 80.0% or more. If the light transmittance is less than 80.0%, the curing of the coating may be non-uniform, and it may be difficult to obtain high developability during pattern formation. The light transmittance is more preferably 85.0% or more, and even more preferably 90.0% or more.
[0193] The haze of the coated substrate is preferably 1.5% or less, more preferably 1.2% or less, and even more preferably 0.8% or less.
[0194] Furthermore, the surface irregularities of the pattern of the coated substrate are preferably less than 5 nm.
[0195] Here, if the surface unevenness is 5 nm or more, it may be difficult to obtain a sharp pattern by development.The surface unevenness is more preferably less than 4 nm, and further preferably less than 3 nm.
[0196] In addition, it is preferable that the linearity of the pattern of the coated substrate is such that no jagged edges are observed at the pattern edges, since the presence of jagged edges at the pattern edges may adversely affect the circuit pattern in a later process or may cause crosstalk between patterns.
[0197] It is also preferable that no residues derived from silica particles are present on the coated substrate, since the presence of residues on the substrate may adversely affect the circuit pattern in a later process or cause crosstalk between patterns.
[0198] The following describes an embodiment of the present invention.
[0199] [Example 1] <Preparation of Particle Dispersion> A sodium aluminate aqueous solution having an Al2O3 concentration of 22 mass % was added to pure water to prepare 10.0 kg of a sodium aluminate aqueous solution having an Al2O3 concentration of 1.0 mass % and a pH of 12.6 (first step).
[0200] Next, this was heated to 80°C, and 30.0 kg of a sodium silicate aqueous solution having a concentration of 1.5 mass% as SiO2 and 30.0 kg of a sodium aluminate aqueous solution having a concentration of 0.5 mass% as Al2O3 were added at the same time. After that, washing was performed by centrifugal sedimentation to obtain a dispersion of composite oxide particles (a1). The average particle diameter of this composite oxide particle (a1) was 27 nm (second step).
[0201] The dispersion of the composite oxide particles (a1) was heated to 95°C, and 138.0 kg of an aqueous solution of sodium silicate with a concentration of 1.5 mass% as SiO2 and 46.0 kg of an aqueous solution of sodium aluminate with a concentration of 0.5 mass% as Al2O3 were added at the same time. Then, the mixture was washed using an ultrafiltration membrane, and the solid content was adjusted to 13 mass%. Then, the mixture was filtered using a capsule filter with an opening of 1 μm to obtain a dispersion of the composite oxide particles (b1). The average particle diameter of the composite oxide particles (b1) was 39 nm (third step).
[0202] 11,250 g of pure water was added to 5,000 g of the dispersion of composite oxide particles (b1), and concentrated hydrochloric acid (concentration: 35.5% by mass) was added dropwise to adjust the pH to 1.0. While adding 10 L of an aqueous hydrochloric acid solution of pH 3 and 5 L of pure water, the dissolved aluminum salt was separated and washed using an ultrafiltration membrane to obtain silica-based particles (c1) with a concentration of 10% by mass (fourth step).
[0203] 1500g of pure water was added to 1000g of the dispersion of silica-based particles (c1), and concentrated hydrochloric acid (concentration 35.5% by mass) was added dropwise to adjust the pH to 1.0. Next, this was heated to 50°C, and the above-mentioned metal impurities were removed using an ultrafiltration membrane while adding 5L of a hydrochloric acid aqueous solution of pH 3 and 2.5L of pure water. In order to make the total content of the metal impurities 1000ppb or less, this series of "acid treatment" operations was repeated three times to obtain silica particles (d1) with a concentration of 10% by mass (fifth step).
[0204] Next, ammonia water was added to 500 g of the dispersion of silica particles (d1) to adjust the pH of the dispersion to 10.5, and the dispersion was transferred to a pressure-resistant container. Next, the container was heated to 140° C. at a rate of 1.5° C. / min, and held for 10 hours, and then cooled to 25° C. (Sixth step) Thereafter, ion exchange was performed for 3 hours using 800 g of a cation exchange resin (Diaion SK1B manufactured by Mitsubishi Chemical Corporation), and then ion exchange was performed for 3 hours using 400 g of an anion exchange resin (Diaion SA20A manufactured by Mitsubishi Chemical Corporation). Thereafter, ion exchange was further performed for 3 hours at 80° C. using 400 g of a cation exchange resin, followed by washing, to obtain an aqueous dispersion of particles (P1).
[0205] The solvent in this aqueous dispersion of particles (P1) was replaced with methanol using an ultrafiltration membrane to produce a methanol dispersion of particles (P1) with a solid content concentration of 20 mass %.
[0206] Surface treatment of particles with organosilicon compounds To 200 g of a methanol dispersion of the particles (P1), 0.4 g of ammonia water having a concentration of 28% by mass and 4.0 g of pure water were added, and the mixture was stirred at room temperature for 0.5 hours.
[0207] Next, 1.2 g of γ-methacryloxypropyltrimethoxysilane (KBM-503, manufactured by Shin-Etsu Chemical Co., Ltd.) was added as an organic silicon compound, and the mixture was stirred at 50° C. for 6 hours to obtain a dispersion of particles (S1) in which the particles (P1) were surface-treated. The solvent was replaced with methanol using an ultrafiltration membrane to produce a methanol dispersion of particles (S1) with a solid content concentration of 20 mass%.
[0208] In addition, the dispersion medium of the methanol dispersion of the particles (S1) was replaced with PGME using an evaporator to obtain a PGME dispersion of the particles (S1) with a solid content concentration of 20.5% by mass, which was used to produce a coating liquid for forming a resist film, as described below.
[0209] The particles and their dispersions were measured by the following methods.
[0210] The characteristics of each production step of the particles, and the properties of the particles and dispersion liquid are shown in Tables 4 to 12 (the same applies to the following Examples and Comparative Examples).
[0211] (1) Average particle size (D), shell thickness, average particle size (Da) of composite oxide particles a, and average particle size (Db) of composite oxide particles b The particle dispersion was diluted to 0.01% by mass, and then dried on a collodion film of a copper cell for an electron microscope. Next, this was photographed at a specified magnification using a field emission transmission electron microscope (HF5000, manufactured by Hitachi High-Technologies Corporation). The particle area of 300 random particles in the obtained photographic projection (TEM photograph) was calculated by image processing, and the circle equivalent diameter was calculated from the area. The average value of the circle equivalent diameters was taken as the average particle diameter (D) of the particles.
[0212] In addition, for 300 randomly selected particles, image processing was performed to determine the area of the cavity of the particle, and the equivalent circle diameter was calculated from the area. This was then subtracted from each particle diameter, and the average value obtained by dividing the result by 2 was used as the thickness of the outer shell.
[0213] Furthermore, the average particle size (Da) of the composite oxide particles a and the average particle size (Db) of the composite oxide particles b were determined in the same manner as in determining the average particle size (D) of the particles.
[0214] (2) Refractive index The particle dispersion was placed in an evaporator to evaporate the dispersion medium. It was then vacuum dried at 120°C for 24 hours to obtain a particle powder. A few drops of a standard refractive index liquid with a known refractive index were placed on a glass plate, and the powder was mixed into this. This operation was performed with various standard refractive index liquids, and the refractive index of the standard refractive index liquid when the mixed liquid became transparent was taken as the refractive index of the particles.
[0215] (3) Content of metal elements and metal impurities in particles The content of metal elements (alkali metals, alkaline earth metals, Al, Co, Cr, Cu, Fe, Mn, Ni, Si, Th, Ti, U, Zn, and Zr, etc.) in the particles was measured by dissolving the particles in hydrofluoric acid, heating to remove the hydrofluoric acid, adding pure water as necessary, and measuring the resulting solution using an ICP inductively coupled plasma optical emission spectrometer (ICPM-8500, manufactured by Shimadzu Corporation). Note that, for metal elements other than the above-mentioned impurity elements, the total amount of metal elements other than carbon contained in the particles was calculated to be 100 parts by mass on an oxide basis. Note that, the content of metal impurities in the particles is the total content (metal basis) of metal elements selected from the above-mentioned elements: alkali metals, alkaline earth metals, Co, Cr, Cu, Fe, Mn, Ni, Ti, Zn, and Zr. Note that, for U and Th, the content (metal basis) of each metal element is used.
[0216] (4) Amount of metal impurities and Al dissolved in the particles in an alkaline solution 45.0 g of an alkaline aqueous solution (0.3 mass% TMAH aqueous solution) with a pH of 12.5 was added to 5.0 g of a dispersion of particles with a solid content concentration of 20 mass%, and stirred at a temperature of 25° C. for 5 minutes. This was centrifuged for 30 minutes using a small ultracentrifuge (Hitachi Koki Co., Ltd. CS150GXL) at a temperature of 25° C. and a rotation speed of 1,370,000 rpm (1,000,000 G). The supernatant of this treatment solution was collected, and pure water was added as necessary. The obtained solution was measured using an ICP inductively coupled plasma optical emission spectrometer (Shimadzu Corporation ICPM-8500). The amount of metal impurities and Al eluted into the alkaline developer was calculated as the amount of elution relative to the total amount of metal elements other than carbon contained in the particles, which was set to 100 parts by mass on a metal basis.
[0217] (5) Number density of silanol groups on the particle surface The silanol group density of the particles is calculated from the Sears number and the specific surface area, specifically, by the above-mentioned formulas (1) and (2).
[0218] The Sears number is measured by titration with NaOH according to the description in Analytical Chemistry 28 (1956), 12, 1981-1983 by Sears. Specifically, the methanol dispersion of the particles is solvent-substituted with water using an evaporator, and the aqueous dispersion of the particles is diluted with pure water so that the silica particle concentration becomes 1% by mass. 30 g of sodium chloride is added to 150 g of the diluted dispersion, and the pH is adjusted to 4.0 with hydrochloric acid. Then, 0.1 N NaOH aqueous solution is titrated at 0.1 ml / sec., and the Sears number is expressed as the amount of NaOH aqueous solution required to reach a pH of 9.0. (That is, the Sears number is the titration amount of 0.1 N NaOH aqueous solution to 1.5 g of particles.) The titration with 0.1 N NaOH aqueous solution was performed using an automatic titrator with a fixed titration speed of 0.1 ml / sec.
[0219] The specific surface area is measured by the BET method using nitrogen adsorption. The measurement sample was prepared by drying an aqueous dispersion of particles at 105°C and powdering them.
[0220] (6) Density of particle in helium gas and nitrogen gas The particle dispersion was heated to 110°C and held for 3 hours to dry. The density of 3.0 g of the obtained powder was measured using a dry automatic density meter (AccuPic II1340, manufactured by Micromeritics Co., Ltd.). At this time, He and N2 were used as measurement gases, and the density was measured for each measurement gas.
[0221] (7) Particle shape The particle appearance of 300 randomly selected particles in the TEM photograph taken when determining the average particle diameter (D) of the above-mentioned particles was observed.
[0222] (8) Sphericity of particles For 300 randomly selected particles in the TEM photograph taken when determining the average particle diameter (D) of the above-mentioned particles, the ratio of the maximum diameter of each particle to the minor axis perpendicular thereto was determined, and the average value was regarded as the sphericity of the particle.
[0223] (9) The shape of the cavity inside the particle shell, the percentage of particles with one cavity, and the percentage of solid particles The cavity shape inside the outer shell of 300 randomly selected particles in the TEM photograph taken when determining the average particle diameter (D) of the above-mentioned particles was observed, and the percentage of particles with one cavity was calculated. The percentage of solid particles was also calculated.
[0224] (10) Particle porosity and density (Sd) The area of the hollow part of the particle was determined for 300 randomly selected hollow particles in the TEM photograph taken when determining the average particle diameter (D) of the above-mentioned particles, and the circle equivalent diameter was calculated from the area, and the average circle equivalent diameter was taken as the average cavity diameter. The shape of the particle and the cavity was assumed to be a perfect sphere, and the average volume of the particle and the average volume of the cavity were determined, and the porosity was calculated as the ratio of the average volume of the cavity to the average volume of the particle. In addition, the density of the particle (Sd) was calculated from the obtained porosity, the ratio of the constituent components of the particle, and its density.
[0225] (11) Specific surface area by BET method The specific surface area was calculated from the amount of adsorbed nitrogen by the BET method using a specific surface area measuring device (Multisorb 12 manufactured by Yuasa Ionics Co., Ltd.).
[0226] (12) Specific surface area (A1) by pulsed NMR The methanol dispersion of the particles was subjected to solvent replacement with water using an evaporator to prepare an aqueous dispersion with a silica particle concentration of 10.0% by mass. The relaxation times of the dispersion and the dispersion medium were measured using a pulse NMR (Acorn Area, manufactured by Xigo nanotools), and the specific surface area (A1) was calculated from the above-mentioned formulas (3) and (4). The measurement conditions were a magnetic field of 0.3 T, a measurement frequency of 13 MHz, and a measurement nucleus of 0.5 T. 1The H NMR measurement method was the CPMG pulse sequence method, with a sample amount of 1 ml, a Ka value of 0.000027, and a temperature of 25° C. Here, the Ka value was calculated from the above-mentioned formulas (5) to (7) by performing pulse NMR measurement at 25° C. on an aqueous dispersion prepared by replacing the solvent in a methanol dispersion of particles (P1) with water using an evaporator and adjusting the solid content concentration to 10.0 mass %, and on the aqueous dispersion medium.
[0227] (13) Specific surface area (A2) The specific surface area (A2) was calculated using the average particle diameter (D) and density (Sd) of the particles according to the above-mentioned formula (5).
[0228] (14) Particle 29 Percentage of peak area representing Q4 structure by Si-NMR analysis The particle dispersion is placed in a dedicated zirconia sample tube, and measured using a 6 mmφ sample tube probe for solids on an NMR device (Agilent Corp. VNMRS-600) using the single pulse non-decoupling method without sample rotation. Polydimethylsiloxane is used as the secondary standard, and the chemical shift is set to -34.44 ppm. The spectrum obtained is subjected to waveform separation using analysis software Origin, and the area of each peak is calculated. More specifically, 29 The area of the peak appearing at chemical shifts of -78 to -88 ppm (Q1), the area of the peak appearing at chemical shifts of -88 to -98 ppm (Q2), the area of the peak appearing at chemical shifts of -98 to -108 ppm (Q3), and the area of the peak appearing at chemical shifts of -108 to -120 ppm (Q4) in the Si-NMR spectroscopy were calculated as (Q4 / ΣQ) × 100, where ΣQ = Q1 + Q2 + Q3 + Q4.
[0229] (15) Functional groups contained in the outer shell of particles The presence or absence of functional groups contained in the particle outer shell and the type of such groups were determined by the following method.
[0230] First, the dispersion liquid was dried in an evaporator and then dried at 150° C. The dried powder was subjected to a diffuse reflection method using a Fourier transform infrared spectrometer (FT-IR) (FT / IR-6100 manufactured by JASCO Corporation) in a wave number range of 700 cm -1 ~4000cm -1 , detector: TGS, resolution: 4.0 cm -1 The measurement was performed with 50 accumulations, and the peaks were detected and the functional groups were identified by referring to the organic compound spectrum database SDBS (https: / / sdbs.db.aist.go.jp (National Institute of Advanced Industrial Science and Technology, 2021.01)).
[0231] (16) Carbon content The dispersion liquid was centrifuged for 30 minutes using a small ultracentrifuge (Hitachi Koki Co., Ltd., CS150GXL) at a temperature of 10°C and a rotation speed of 1,370,000 rpm (1,000,000 G). The precipitate in the treatment liquid was collected and vacuum dried at 120°C for 24 hours to obtain a particle powder. The carbon content of the particles in this powder was measured using a carbon-sulfur analyzer (LECO Japan Co., Ltd., CS844).
[0232] (17) Solid content of organosilicon compound having functional group The dispersion liquid was centrifuged for 30 minutes using a small ultracentrifuge (CS150GXL, manufactured by Hitachi Koki Co., Ltd.) at a temperature of 10°C and a rotation speed of 1,370,000 rpm (1,000,000 G). The precipitate from the treatment liquid was collected and vacuum dried at 120°C for 24 hours to obtain a particle powder. The mass loss of this powder before and after heating at 500°C was measured using a thermogravimetric differential thermal analyzer (TG / DTA EXSTAR6000 MSD, manufactured by Hitachi High-Tech Science Co., Ltd.), and the amount of silicon derived from the organosilicon compound was calculated from the difference with the original particle amount. Next, the solid content (R n -SiO (4-n) / 2 ) amount to determine the solid content of the organosilicon compound having a functional group.
[0233] <Production of Coating Solution for Forming Resist Film> 73.4 g of PGME, 3.0 g of an alkali-soluble UV-curable acrylic polymer (Acrit 8KQ-2001, manufactured by Taisei Fine Chemical Co., Ltd., solid content concentration 40.0% by mass), 0.05 g of 2,2-dimethoxy-1,2-diphenylethan-1-one (Omnirad 651, manufactured by IGM RESINS BV), 0.05 g of bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (Omnirad 819, manufactured by IGM RESINS BV), and 0.1 g of a fluorine-based leveling agent (Megafac RS-90, manufactured by DIC Corporation, solid content concentration 10% by mass) were mixed. Then, 23.4 g of a PGME dispersion of particles (S1) was mixed therewith to prepare a coating solution for forming a resist film with a solid content concentration of 6% by mass.
[0234] <Production of Resist-Coated Substrate> The resist film-forming coating solution was applied to a 2-inch square glass substrate (Corning #1737) using a spin coater, dried at 80°C for 1 minute, and then cured by irradiating an ArF excimer laser (193 nm) through a photomask (5 μm line & space pattern) using an exposure device (Nikon NSR-S302). Thereafter, a 0.3 mass% TMAH aqueous solution was sprayed to dissolve and remove the unexposed parts, and the substrate was heated at 150°C for 5 minutes to prepare a substrate with a resist coating.
[0235] The coated substrate was measured for the following items. The results are shown in Table 8 (the same applies to the following Examples and Comparative Examples). In order to make it easier to compare performance, the type of substrate, the ratio of particles and matrix in the coating, and the coating thickness were the same in each Example and Comparative Example.
[0236] (18) Film thickness and refractive index The film thickness and refractive index of the coated substrate were measured using an ellipsometer (EMS-1, manufactured by ULVAC Co., Ltd.) and the refractive index was evaluated according to the following classification. Coating refractive index rating criteria: ◎: 1.30 or less ○:1.31~1.35 △:1.36~1.40 ×: 1.41 or higher
[0237] (19) Total light transmittance and haze The total light transmittance and haze of the coated substrate were measured using a haze meter (NDH-5000, manufactured by Nippon Denshoku Industries Co., Ltd.) and were evaluated according to the following classification. Evaluation criteria for total light transmittance: ◎: 90% or more ○: 85%~89% △: 80%~84% ×: 79% or less Haze criteria: ◎: 0.8% or less ○: 0.9~1.2% △: 1.3~1.5% ×: 1.6% or more
[0238] (20) Surface irregularities of the pattern of the coated substrate The surface unevenness of the pattern of the coated substrate was evaluated as surface roughness by scanning with an atomic force microscope (Dimension Icon, manufactured by Bruker Japan Co., Ltd.) under the conditions of contact mode, scan speed of 0.50 Hz, and scan size of 20 μm × 20 μm. The surface roughness was evaluated by classifying it as follows. Evaluation criteria: ◎: Less than 3 nm ○: 3nm or more and less than 4nm △: 4nm or more and less than 5nm ×: 5nm or more
[0239] (21) Linearity and residue of patterns on coated substrates The linearity of the pattern edges and residues on the substrate originating from silica particles were evaluated using photographic projection images (SEM images) taken with an optical microscope and a field emission scanning electron microscope (S-5500, manufactured by Hitachi High-Technologies Corporation). These were categorized and evaluated as follows: Pattern linearity evaluation criteria: ◎: No jagged edges are observed on the pattern edges ○: Jagged edges are partially observed on the pattern edges. ×: Jagged edges are observed throughout the pattern edge. Residue evaluation criteria: ◎: No residue found on the substrate ○: Residue is partially observed on the substrate. ×: Residue is observed over the entire surface of the substrate.
[0240] [Example 2] A PGME dispersion of particles was prepared, and a coating liquid and a coated substrate were produced in the same manner as in Example 1, except that in the first step, 50.0 kg of a sodium aluminate aqueous solution having a pH of 12.6 was prepared, in the second step, 7.5 kg of a sodium silicate aqueous solution and 7.5 kg of a sodium aluminate aqueous solution were prepared, in the third step, 135.0 kg of a sodium silicate aqueous solution and 45.0 kg of a sodium aluminate aqueous solution were prepared, and in the sixth step, the heating rate was 0.5°C / min and the heating temperature was 60°C.
[0241] [Example 3] In the first step, 9840g of pure water was added to 160g of an aqueous dispersion of silica-based particles (LNA-2000 manufactured by JGC Catalysts and Chemicals Co., Ltd., average particle size 23nm, solid content concentration 12.5% by mass), and then a 1% by mass NaOH aqueous solution was added to prepare 10.0kg of an aqueous solution with a pH of 12.5. In the second step, the sodium silicate aqueous solution was 137.5kg, the sodium aluminate aqueous solution was 137.5kg, in the third step, the sodium silicate aqueous solution was 330.0kg, the sodium aluminate aqueous solution was 110.0kg, the temperature rise rate in the sixth step was 5.0°C / min, and the mixture was heated to 200°C and held for 10 hours, and then cooled to 48°C. Except for this, a PGME dispersion of particles was produced in the same manner as in Example 1, and a coating liquid and a coated substrate were produced.
[0242] [Example 4] A PGME dispersion of particles was prepared, and a coating liquid and a coated substrate were produced in the same manner as in Example 1, except that in the second step, the amount of the sodium silicate aqueous solution was 3.5 kg, the amount of the sodium aluminate aqueous solution was 3.5 kg, in the third step, the amount of the sodium silicate aqueous solution was 52.5 kg, the amount of the sodium aluminate aqueous solution was 17.5 kg, and in the sixth step, the heating temperature was 80°C.
[0243] [Example 5] In the first step, 9950.6 g of pure water was added to 49.4 g of an aqueous dispersion of silica-based particles (SI-40 manufactured by JGC Catalysts and Chemicals Co., Ltd., average particle size 17 nm, solid content concentration 40.5% by mass), and then a 1% by mass NaOH aqueous solution was added to prepare 10.0 kg of an aqueous solution with a pH of 12.5. In the second step, the amount of sodium silicate aqueous solution was 105.0 kg, the amount of sodium aluminate aqueous solution was 105.0 kg, in the third step, the amount of sodium silicate aqueous solution was 246.0 kg, the amount of sodium aluminate aqueous solution was 82.0 kg, and in the sixth step, the heating rate was 3.0 ° C. / min, and the heating temperature was 180 ° C., except that the same procedure as in Example 1 was followed to produce a PGME dispersion of particles, and a coating liquid and a coated substrate were produced.
[0244] [Example 6] In the first step, 9934.4 g of pure water was added to 65.6 g of an aqueous dispersion of silica-based particles (SI-30 manufactured by JGC Catalysts and Chemicals, average particle size 12 nm, solid content concentration 30.5% by mass), and then a 1% by mass NaOH aqueous solution was added to prepare 10.0 kg of an aqueous solution with a pH of 12.5. In the second step, the amount of the sodium silicate aqueous solution was 124.0 kg, and the amount of the sodium aluminate aqueous solution was 124.0 kg, and in the third step, the amount of the sodium silicate aqueous solution was 306.0 kg, and the amount of the sodium aluminate aqueous solution was 102.0 kg. Except for this, a PGME dispersion of particles was produced in the same manner as in Example 1, and a coating solution and a coated substrate were produced.
[0245] [Example 7] In the first step, 9840 g of pure water was added to 160 g of an aqueous dispersion of silica-based particles (LNA-2000 manufactured by JGC Catalysts and Chemicals, average particle size 23 nm, solid content concentration 12.5% by mass), and then a 1% by mass NaOH aqueous solution was added to prepare 10.0 kg of an aqueous solution with a pH of 12.5. In the second step, the amount of the sodium silicate aqueous solution was 145.0 kg, and the amount of the sodium aluminate aqueous solution was 145.0 kg, and in the third step, the amount of the sodium silicate aqueous solution was 246.0 kg, and the amount of the sodium aluminate aqueous solution was 82.0 kg. Except for this, a PGME dispersion of particles was produced, and a coating solution and a coated substrate were produced in the same manner as in Example 1.
[0246] [Example 8] Silica-based particles were obtained in the fourth step in the same manner as in Example 1, except that the amount of the sodium silicate aqueous solution in the second step was 71.0 kg, the amount of the sodium aluminate aqueous solution was 71.0 kg, and the amount of the sodium silicate aqueous solution in the third step was 169.5 kg, and the amount of the sodium aluminate aqueous solution was 56.5 kg.
[0247] In the fifth step, 1000 g of the dispersion of silica-based particles was washed by ion exchange at 80° C. for 3 hours using 1600 g of cation exchange resin. Then, 1500 g of pure water was added, and concentrated hydrochloric acid (concentration 35.5% by mass) was added dropwise to adjust the pH to 1.0. Next, the mixture was heated to 50° C., and the above-mentioned metal impurities were removed using an ultrafiltration membrane while adding 5 L of a hydrochloric acid aqueous solution of pH 3 and 2.5 L of pure water. This series of operations related to "contact with ion exchange resin" and "acid treatment" was repeated five times. In the sixth step, a PGME dispersion of particles was produced in the same manner as in Example 1, except that the heating rate was 0.8° C. / min and the heating temperature was 80° C., and a coating liquid and a coated substrate were produced.
[0248] [Example 9] A PGME dispersion of particles was prepared, and a coating liquid and a coated substrate were produced in the same manner as in Example 1, except that in the second step, 65.0 kg of the sodium silicate aqueous solution and 65.0 kg of the sodium aluminate aqueous solution were used, in the third step, 255.0 kg of the sodium silicate aqueous solution and 85.0 kg of the sodium aluminate aqueous solution were used, and in the fifth step, the "acid treatment" was repeated twice.
[0249] [Example 10] Silica-based particles were obtained in the fourth step in the same manner as in Example 1, except that the amount of the sodium silicate aqueous solution in the second step was 169.0 kg, the amount of the sodium aluminate aqueous solution was 169.0 kg, and the amount of the sodium silicate aqueous solution in the third step was 339.0 kg, and the amount of the sodium aluminate aqueous solution was 113.0 kg.
[0250] In the fifth step, 1000 g of the dispersion of silica-based particles was washed by ion exchange at 80° C. for 3 hours using 1600 g of cation exchange resin. Then, 1500 g of pure water was added, and concentrated hydrochloric acid (concentration 35.5% by mass) was added dropwise to adjust the pH to 1.0. Next, the mixture was heated to 50° C., and the above-mentioned metal impurities were removed using an ultrafiltration membrane while adding 5 L of a hydrochloric acid aqueous solution of pH 3 and 2.5 L of pure water. In the sixth step, a PGME dispersion of particles was produced in the same manner as in Example 1, except that the heating rate was 0.8° C. / min and the heating temperature was 80° C., and a coating liquid and a coated substrate were produced.
[0251] [Example 11] A PGME dispersion of particles was prepared in the same manner as in Example 1, except that the heating temperature in the sixth step was set to 180°C, 4.0 g of γ-methacryloxypropyltrimethoxysilane was used as an organosilicon compound in the surface treatment of the particles, and stirring was performed at 50°C for 24 hours. A coating solution and a coated substrate were produced in the same manner as in Example 1.
[0252] [Example 12] A PGME dispersion of particles was prepared, and a coating solution and a coated substrate were produced in the same manner as in Example 1, except that in the sixth step, the heating rate was set to 0.8°C / min, the heating temperature was set to 70°C, and 0.12 g of γ-methacryloxypropyltrimethoxysilane was used as the organosilicon compound in the surface treatment of the particles.
[0253] [Example 13] A PGME dispersion of particles was prepared, and a coating solution and a coated substrate were produced in the same manner as in Example 1, except that TEOS (Tama Chemicals Co., Ltd., orthosilicate ES28) was used as the organosilicon compound in the surface treatment of the particles.
[0254] [Example 14] A PGME dispersion of particles was prepared, and a coating solution and a coated substrate were produced in the same manner as in Example 1, except that γ-acryloxypropyltrimethoxysilane (KBM-5103 manufactured by Shin-Etsu Chemical Co., Ltd.) was used as the organosilicon compound in the surface treatment of the particles.
[0255] [Example 15] In the first step, a sodium aluminate aqueous solution having an Al2O3 concentration of 22 mass% and an aqueous dispersion of silica-based particles as SiO2 (SI-550 manufactured by JGC Catalysts and Chemicals Co., Ltd., average particle size 5 nm, solid content concentration 20 mass%) were added to pure water to prepare 10.0 kg of an aqueous solution having an Al2O3 concentration of 2.0 mass% and an SiO2 concentration of 0.2 mass%. In the second step, the amount of the sodium silicate aqueous solution was 55.0 kg, the amount of the sodium aluminate aqueous solution was 55.0 kg, and in the third step, the amount of the sodium silicate aqueous solution was 222.0 kg, and the amount of the sodium aluminate aqueous solution was 74.0 kg. Except for this, a PGME dispersion of particles was produced in the same manner as in Example 1, and a coating liquid and a coated substrate were produced.
[0256] [Example 16] In the first step, a sodium aluminate aqueous solution having an Al2O3 concentration of 22 mass% was added to pure water to prepare 10.0 kg of a sodium aluminate aqueous solution having an Al2O3 concentration of 4.5 mass% and a pH of 12.9, in the second step, 2.3 kg of the sodium silicate aqueous solution and 4.6 kg of the sodium aluminate aqueous solution were used, and in the third step, 95.5 kg of the sodium silicate aqueous solution and 50.5 kg of the sodium aluminate aqueous solution were used. Except for this, a PGME dispersion of particles was prepared and a coating solution and a coated substrate were produced in the same manner as in Example 1.
[0257] [Comparative Example 1] A PGME dispersion of particles was prepared, and a coating liquid and a coated substrate were produced in the same manner as in Example 1, except that in the first step, 50.0 kg of a sodium aluminate aqueous solution having a pH of 12.6 was prepared, in the second step, 1.6 kg of a sodium silicate aqueous solution and 1.6 kg of a sodium aluminate aqueous solution were prepared, in the third step, 132.0 kg of a sodium silicate aqueous solution and 44.0 kg of a sodium aluminate aqueous solution were prepared, and in the sixth step, the heating temperature was 80°C.
[0258] [Comparative Example 2] In the first step, 9920 g of pure water was added to 80 g of an aqueous dispersion of silica-based particles (LNA-2000 manufactured by JGC Catalysts and Chemicals, average particle size 23 nm, solid content concentration 12.5% by mass), and then a 1% by mass NaOH aqueous solution was added to prepare 10.0 kg of an aqueous solution with a pH of 12.5. In the second step, the amount of the sodium silicate aqueous solution was 260.0 kg, the amount of the sodium aluminate aqueous solution was 260.0 kg, and in the third step, the amount of the sodium silicate aqueous solution was 420.0 kg, and the amount of the sodium aluminate aqueous solution was 140.0 kg. Except for this, a PGME dispersion of particles was produced, and a coating solution and a coated substrate were produced in the same manner as in Example 1.
[0259] [Comparative Example 3] A PGME dispersion of particles was prepared, and a coating liquid and a coated substrate were produced in the same manner as in Example 1, except that the amount of the sodium silicate aqueous solution in the second step was 21.0 kg, the amount of the sodium aluminate aqueous solution was 21.0 kg, the amount of the sodium silicate aqueous solution in the third step was 360.0 kg, and the amount of the sodium aluminate aqueous solution was 120.0 kg, and the removal of metal impurities in the fifth step was performed four times.
[0260] [Comparative Example 4] A PGME dispersion of particles was produced in the same manner as in Example 1, except that the operation for removing metal impurities in the fifth step was not carried out. However, since the content of metal impurities in the obtained particles exceeded 1000 ppb, the amount of metal impurities eluted in an alkaline aqueous solution of pH 12.5 exceeded 100 ppb, and the amount of Al eluted in an alkaline aqueous solution of pH 12.5 exceeded 1000 ppb, the steps after the production of the coating solution were not carried out.
[0261] [Comparative Example 5] A PGME dispersion of particles was produced in the same manner as in Example 1, except that the amount of sodium silicate aqueous solution in the second step was 55.0 kg, the amount of sodium aluminate aqueous solution was 55.0 kg, the amount of sodium silicate aqueous solution in the third step was 225.0 kg, the amount of sodium aluminate aqueous solution was 75.0 kg, the operation of removing metal impurities in the fifth step was carried out once, and the heating temperature in the sixth step was 220° C. However, since the content of metal impurities in the obtained particles was more than 1000 ppb, the amount of elution of metal impurities in an alkaline aqueous solution of pH 12.5 was more than 100 ppb, and the amount of Al eluted in an alkaline aqueous solution of pH 12.5 was more than 1000 ppb, the steps subsequent to the production of the coating solution were not carried out.
[0262] [Comparative Example 6] A PGME dispersion of particles was produced in the same manner as in Example 5, except that the amount of sodium silicate aqueous solution in the second step was 20.0 kg, the amount of sodium aluminate aqueous solution was 20.0 kg, the amount of sodium silicate aqueous solution in the third step was 75.0 kg, the amount of sodium aluminate aqueous solution was 25.0 kg, the operation of removing metal impurities in the fifth step was carried out once, and the heating temperature in the sixth step was 50° C. However, since the content of metal impurities in the obtained particles was more than 1000 ppb, the amount of elution of metal impurities in an alkaline aqueous solution of pH 12.5 was more than 100 ppb, and the amount of Al eluted in an alkaline aqueous solution of pH 12.5 was more than 1000 ppb, the steps after the production of the coating solution were not carried out.
[0263] [Comparative Example 7] A PGME dispersion of particles was prepared in the same manner as in Example 1, except that the heating temperature in the sixth step was set to 220°C, 8.0 g of γ-methacryloxypropyltrimethoxysilane was used as an organosilicon compound in the surface treatment of the particles, and stirring was performed at 50°C for 24 hours. A coating solution and a coated substrate were produced in the same manner as in Example 1.
[0264] [Comparative Example 8] A PGME dispersion of particles was prepared, and a coating solution and a coated substrate were produced in the same manner as in Example 1, except that the heating temperature in the sixth step was set to 50°C and that the surface treatment of the particles with an organosilicon compound was not performed.
[0265] [Comparative Example 9] A PGME dispersion of particles was prepared, and a coating liquid and a coated substrate were produced in the same manner as in Example 1, except that in the second step, the amount of the sodium silicate aqueous solution was 41.5 kg, the amount of the sodium aluminate aqueous solution was 41.5 kg, in the third step, the amount of the sodium silicate aqueous solution was 192.0 kg, and the amount of the sodium aluminate aqueous solution was 64.0 kg, and in the sixth step, the heating rate was 7.5°C / min, and the heating temperature was 250°C.
[0266] [Comparative Example 10] In the first step, 8800 g of pure water was added to 1200 g of an aqueous dispersion of silica-based particles (LNA-2000 manufactured by JGC Catalysts and Chemicals, average particle size 23 nm, solid content concentration 12.5 mass%), and then a 1 mass% NaOH aqueous solution was added to prepare 10.0 kg of an aqueous solution with a pH of 12.5. In the second step, the amount of the sodium silicate aqueous solution was 8.0 kg, and the amount of the sodium aluminate aqueous solution was 8.0 kg, and in the third step, the amount of the sodium silicate aqueous solution was 135.0 kg, and the amount of the sodium aluminate aqueous solution was 45.0 kg. Except for this, a PGME dispersion of particles was produced, and a coating solution and a coated substrate were produced in the same manner as in Example 1.
[0267] [Comparative Example 11] A PGME dispersion of particles was produced, and a coating solution and a coated substrate were produced in the same manner as in Example 1, except that the amount of the sodium silicate aqueous solution in the second step was 50.0 kg, the amount of the sodium aluminate aqueous solution was 50.0 kg, and the amount of the sodium silicate aqueous solution in the third step was 111.0 kg, and the amount of the sodium aluminate aqueous solution was 37.0 kg. However, when the TEM photograph of the particles was observed, the particles were solid particles, and no hollow particles were obtained.
[0268] [Comparative Example 12] An aqueous dispersion of particles was obtained in the same manner as in Example 1, except that the amount of the aqueous sodium silicate solution in the second step was 65.5 kg, the amount of the aqueous sodium aluminate solution was 65.5 kg, and the amount of the aqueous sodium silicate solution in the third step was 252.0 kg, and the amount of the aqueous sodium aluminate solution was 84.0 kg. This aqueous dispersion was dried in an evaporator, heated to 500°C, and held for 3 hours, and then cooled to 25°C. Thereafter, a PGME dispersion of particles was produced, and a coating liquid and a coated substrate were produced in the same manner as in Example 1, except that the surface treatment of the particles with an organic silicon compound was not performed.
[0269] [Table 4]
[0270] [Table 5]
[0271]
Table 6
[0272]
Table 7
[0273]
Table 8
[0274]
Table 9
[0275]
Table 10
[0276]
Table 11
[0277]
Table 12
Claims
1. A particle having an outer shell containing silicon and a cavity therein, a dispersion liquid of hollow silica particles, characterized in that the particles have an average particle size of 15 to 150 nm and a refractive index of 1.08 to 1.35, and the total content of metal impurities selected from alkali metals, alkaline earth metals, Co, Cr, Cu, Fe, Mn, Ni, Ti, Zn, and Zr is 1000 ppb or less relative to the particles, as determined by the metal content.
2. 2. The dispersion according to claim 1, wherein the total amount of said metal impurities eluted from said particles in an alkaline aqueous solution having a pH of 12.5 is 100 ppb or less in terms of metal relative to said particles.
3. 3. The dispersion according to claim 1, wherein the amount of Al eluted from the particles in an alkaline aqueous solution having a pH of 12.5 is 1000 ppb or less as the metal relative to the particles.
4. The number density of silanol groups on the particle surface calculated by the Sears measurement method of the particles is 0.5 to 2.5 / nm 2 3. The dispersion according to claim 1 or 2,
5. The difference between the density of the particles in helium gas and the density in nitrogen gas is 0.2 to 1.4 g / cm 3 3. The dispersion according to claim 1 or 2,
6. 3. The dispersion according to claim 1, wherein a ratio (A1 / A2) of a specific surface area (A1) of the particles obtained by pulse NMR measurement of the aqueous dispersion of the particles to a specific surface area (A2) of the particles obtained from an average particle diameter of the particles is 0.60 or more.
7. The particles 29 In Si-NMR analysis, the chemical shift of silicon atom appears at -78 to -120 ppm. 1 ~Q 4 Q that appears at a chemical shift of -108 to -120 ppm relative to the sum of the areas of the peaks representing the structure 4 3. The dispersion according to claim 1, wherein the area ratio of the peak representing the structure is less than 90%.
8. the particles have at least one functional group selected from an alkyl group, an acryloyl group, a (meth)acryloyl group, a vinyl group, a mercapto group, and an epoxy group; at least one functional group selected from a hydroxyl group, a carboxyl group, and an amino group; 3. The dispersion according to claim 1, further comprising:
9. A first step of preparing an alkaline aqueous solution; A solution of a compound containing silicon and an aqueous solution of an alkali-soluble compound of an inorganic element other than silicon are mixed together, and the oxide of silicon is converted to SiO 2 When the oxide of the inorganic element is represented as MOx, the molar ratio of the reaction solution at the end of the addition (MOx / SiO 2 a second step of simultaneously adding the above-mentioned aqueous alkali solution to the above-mentioned aqueous alkali solution so that the average molecular weight of the composite oxide particles a is 0.2 to 15, thereby preparing a dispersion of the composite oxide particles a; Next, a molar ratio (MOx / SiO 2 a third step of adding a solution of a compound containing silicon and an aqueous solution of an alkali-soluble compound of an inorganic element other than silicon to prepare a dispersion of composite oxide particles b having an average particle size of 15 to 150 nm, and a value obtained by subtracting the average particle size of the composite oxide particles a from the average particle size and dividing the result by 2 is 3 to 14 nm; Next, a fourth step of adding an acid to the dispersion liquid of the composite oxide particles b to remove at least a part of the elements other than silicon constituting the composite oxide particles b, thereby preparing a dispersion liquid of silica-based particles; Next, a fifth step of removing metal impurities selected from alkali metals, alkaline earth metals, Co, Cr, Cu, Fe, Mn, Ni, Ti, Zn, and Zr from the silica-based particle dispersion liquid to prepare a dispersion liquid of silica particles having a total content of the metal impurities of 1000 ppb or less in terms of metal; Next, a sixth step of heating the dispersion liquid of the silica particles to 60 to 200° C. and then lowering the temperature to less than 50° C.; A method for producing a dispersion of hollow silica particles comprising the steps of:
10. The method for producing a dispersion according to claim 9 , wherein the aqueous alkaline solution in the first step contains an element that becomes an amphoteric oxide.
11. 10. The method for producing a dispersion according to claim 9, further comprising the step of adding at least one of an organosilicon compound represented by the following formula (8) and a partial hydrolyzate thereof to the dispersion after the sixth step: R n -SiX 4-n (8) (In the formula, R is an unsubstituted or substituted hydrocarbon group having 1 to 10 carbon atoms, X is an alkoxy group having 1 to 4 carbon atoms, a hydroxyl group, or a hydrogen atom, and n is an integer of 0 to 4.)
Citation Information
Patent Citations
Production of preform for optical fiber
JP1997124332A
Method of manufacturing silica-based fine particle and base material with coating film containing the silica-based fine particle
JP2004203683A
Preparation of quartz glass body
JP2020523278A
Particles having cavity inside shell including silica and method for producing the same, coating liquid containing the same, and base material with transparent film containing the same
JP2021054685A
Modified hollow particle and method for producing the same
JP2022089560A