Soft magnetic steel plate and production method thereof
The use of a single-roll liquid rapid solidification method and controlled impurity levels in iron scrap production addresses production challenges, resulting in high-quality soft magnetic steel sheets with improved magnetic properties and reduced waste.
Patent Information
- Application Number
- JP2023054834
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-30
AI Technical Summary
Conventional methods for producing electrical steel sheets from iron scrap face challenges in managing impurities like Cu, Sn, Ni, and Cr, which affect hot and cold workability and magnetic properties, leading to production issues and poor magnetic performance.
A soft magnetic steel sheet is manufactured using iron scrap with controlled impurity levels of Cu, Cr, Ni, and Sn, formed via a single-roll liquid rapid solidification method, followed by heat treatment in an inert atmosphere, and optionally warm or cold rolling to ensure good magnetic properties.
The method enables the production of high-quality soft magnetic steel plates with desirable magnetic properties and reduced waste generation by effectively managing impurities, ensuring magnetic flux density, orientation, and iron loss within specified limits.
Smart Images

Figure 2024142615000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a soft magnetic steel sheet and a manufacturing method thereof. [Background technology]
[0002] In recent years, efforts to significantly reduce waste through prevention, reduction, reuse, and recycling have become more common. To achieve this, research and development into the recycling of steel scrap is being conducted.
[0003] Conventionally, there is a technology for manufacturing electrical steel sheets used for iron cores, etc., in relation to the recycling of iron scraps. For example, a non-oriented electrical steel sheet is known that contains C; 0.0050 mass% or less, Si; 1.5 to 5.0 mass%, Mn; 0.2 to 3.0 mass%, sol.Al; 0.0030 mass% or less, P; 0.2 mass% or less, S; 0.0050 mass% or less, N; 0.0040 mass% or less, T.Ca; 0.0010 to 0.0080 mass%, TO; 0.0100 mass% or less, and REM; 0.0001 to 0.0050 mass%, with the balance being Fe and unavoidable impurities (see Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6989000 Summary of the Invention [Problem to be solved by the invention]
[0005] In the conventional technology described in Patent Document 1, when manufacturing an electrical steel sheet, a slab cast steel sheet, which is the raw material, is hot-rolled to form a hot-rolled steel sheet, and the hot-rolled steel sheet is further cold-rolled to form a cold-rolled steel sheet. When adopting such a manufacturing method that performs hot rolling, in order to avoid problems in manufacturing (e.g., occurrence of cracks in the steel sheet during rolling) while ensuring the required magnetic properties, it is necessary to limit the unavoidable impurities contained in the electrical steel sheet to a predetermined allowable value (e.g., Cu is 0.01 mass% or less).
[0006] On the other hand, unlike iron ore, which is a raw material for steelmaking, scrap iron contains relatively high concentrations of components that are impurities for electrical steel sheets. Some of these impurities (e.g., Cu, etc.) are difficult to remove even by refining using an electric furnace, etc., so it may be difficult to achieve the allowable values of unavoidable impurities in electrical steel sheets described in the above Patent Document 1. It is known that, among the unavoidable impurities contained in scrap iron, Cu and Sn cause precipitation embrittlement in high temperature / oxidizing atmospheres, thereby adversely affecting hot workability, and that this is further promoted when Cu and Sn are contained at the same time. In addition, Ni and Cr harden steel materials, and therefore adversely affect cold workability. Inclusions generated in the crystal structure by these impurity elements adversely affect cold workability and significantly deteriorate magnetic properties by pinning magnetic wall motion and generating magnetic domains.
[0007] In order to solve the above problems, the present invention aims to provide a soft magnetic steel sheet and a manufacturing method thereof that can ensure good magnetic properties even when impurities derived from iron scrap are contained in the raw materials, and ultimately contributes to a significant reduction in the generation of iron scrap as waste. [Means for solving the problem]
[0008] In order to solve the above problems, one embodiment of the present invention is a soft magnetic steel sheet manufactured from raw materials including iron scrap, and includes Fe as a base material, 1.0 to 7.0 wt% Si, and 0.1 to 1.0 wt% Cu, which is a component derived from the iron scrap.
[0009] According to this embodiment, even if the raw material contains Cu derived from iron scrap as an impurity, the soft magnetic steel sheet can have good magnetic properties.
[0010] In the above embodiment, the components derived from the iron scrap may further include 0.01 to 0.5 wt% Cr, 0.01 to 0.5 wt% Ni, and 0.01 to 0.3 wt% Sn, and the total of Cu, Cr, Ni, and Sn may be 1.2 wt% or less.
[0011] According to this embodiment, even if the raw material contains Cu, Cr, Ni, and Sn derived from iron scrap as impurities, the soft magnetic steel sheet can have good magnetic properties.
[0012] In addition, in order to solve the above problems, one aspect of the present invention is a method for manufacturing the soft magnetic steel sheet, which includes a strip-shaped thin plate formation process in which a strip-shaped thin plate is formed from the raw material by a single-roll liquid rapid solidification method, and a heat treatment process in which the strip-shaped thin plate is heat-treated in an inert atmosphere at 600 to 1200°C.
[0013] According to this embodiment, even if the raw material contains impurities derived from iron scrap, the belt-shaped thin plate is formed by the single-roll liquid rapid solidification method, so that it is possible to avoid the occurrence of cracks in the steel plate, which occurs in the case of hot rolling of a slab cast piece. Furthermore, by rapidly solidifying the molten metal, the impurity elements are not segregated in specific parts of the crystal structure, and inclusions that hinder domain wall movement are not formed, so that good magnetic properties of the soft magnetic steel plate can be ensured.
[0014] In the above embodiment, the soft magnetic steel sheet may have a thickness of 0.03 to 0.15 mm, a magnetic flux density B100 of 1.6 T or more, a degree of magnetic orientation B10 / B100 of 0.78 or more, and an iron loss W10 / 400 of 10 W / kg or less.
[0015] According to this embodiment, a high-quality soft magnetic steel sheet can be obtained.
[0016] In the above aspect, it is preferable to perform at least one of warm rolling and cold rolling of the strip-shaped thin plate before the heat treatment step.
[0017] According to this embodiment, by performing at least one of warm rolling and cold rolling, the surface of the strip-shaped thin plate obtained by the strip-shaped thin plate forming process can be smoothed, and the thickness, width, and properties of the soft magnetic steel plate can be appropriately adjusted.
[0018] In the above-mentioned embodiment, the method may further include a Si-adding step of adding Si to the iron scrap as the raw material. The Si-adding step is performed by adding Si in the form of metal Si or an alloy containing Si during the refining step of the iron scrap in an electric furnace or during the melting of the raw material by a single-roll liquid quenching solidification method, to adjust the amount of Si.
[0019] According to this aspect, the magnetization characteristics of the soft magnetic steel plate can be appropriately improved. Effect of the Invention
[0020] According to the above aspect, good magnetic properties can be ensured even when impurities derived from iron scrap are contained in the raw material. [Brief description of the drawings]
[0021] [Figure 1] An explanatory diagram showing an outline of a manufacturing apparatus for soft magnetic steel sheets to which the single roll method is applied. [Diagram 2] Graph showing the relationship between iron loss and B10 / B100 in soft magnetic steel sheets [Diagram 3] A graph showing the relationship between the Cu and Sn content of soft magnetic steel sheets and whether they can be manufactured [Figure 4] A graph showing the relationship between the Cu content of soft magnetic steel sheet and iron loss W10 / 400 [Diagram 5] A graph showing the relationship between the Cu content of soft magnetic steel sheets and B10 / B100 [Figure 6] A graph showing the relationship between the impurity content (total of Cu, Cr, Ni, and Sn) of soft magnetic steel sheet and iron loss W10 / 400 [Figure 7] A graph showing the relationship between the impurity content (total of Cu, Cr, Ni, and Sn) of soft magnetic steel sheet and B10 / B100 [Figure 8] Photograph of the crystal structure of soft magnetic steel sheet (Example 13) observed by electron microscope [Figure 9] Photograph of the crystal structure of soft magnetic steel sheet (Example 14) observed by electron microscope [Figure 10] Photograph of the crystal structure of soft magnetic steel sheet (conventional technology 2) observed by electron microscope DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0023] As shown in Fig. 1, the soft magnetic steel sheet manufacturing apparatus 1 is an apparatus that applies the single roll method (single roll liquid quenching and solidification method). The manufacturing apparatus 1 includes a rotatable cooling roll 2 and a nozzle 4 that sprays molten metal 3, which is the raw material of the soft magnetic steel sheet.
[0024] In the manufacturing apparatus 1, molten metal 3 is discharged from an injection hole 4a of a nozzle 4 toward a cooling roll 2 rotating at a predetermined speed (for example, 500 to 2000 rpm). The discharged molten metal 3 is quenched on the surface of the cooling roll 2, thereby forming a strip-shaped thin plate 5 along the surface of the cooling roll 2 (one example of a strip-shaped thin plate forming process). After being peeled off from the surface of the cooling roll 2, the strip-shaped thin plate 5 is continuously wound up by a winding device (not shown). In this way, a coil of the strip-shaped thin plate 5 is formed.
[0025] The chill roll 2 has a diameter of 200 mm and an outer circumferential surface formed of a Cu-Cr alloy or carbon steel. A heater 7 is attached around the nozzle 4, which maintains the temperature of the molten metal 3 in the nozzle 4 at an appropriate temperature. The molten metal 3 is ejected from the ejection hole 4a by the pressure of a gas (e.g., nitrogen gas) supplied into the nozzle 4.
[0026] The coil of strip 5 formed by the manufacturing apparatus 1 is heat treated (annealed) in an inert atmosphere in a heating furnace (not shown) (one example of a heat treatment process). This results in a soft magnetic steel sheet having predetermined magnetic properties. The inert atmosphere can be achieved by filling the furnace with an inert gas such as argon gas or helium gas. However, the furnace may also be filled with nitrogen gas, hydrogen gas, or the like.
[0027] The heat treatment temperature is set, for example, in the range of 600 to 1200° C., and more preferably in the range of 1050 to 1150° C. The heat treatment time is set, for example, in the range of 10 sec to 48 hr, and more preferably in the range of 3 to 24 hr. This removes internal stress from the strip-shaped thin plate 5 and improves the structure, thereby improving the magnetic properties (for example, iron loss) of the soft magnetic steel sheet finally obtained.
[0028] In addition, in the manufacture of the soft magnetic steel sheet, after forming the strip-shaped thin plate 5, at least one of warm rolling and cold rolling may be performed on the strip-shaped thin plate 5 before the heat treatment. Warm rolling is performed, for example, on the strip-shaped thin plate 5 in the temperature range of 600 to 900°C using a known warm rolling machine. In addition, cold rolling is performed on the strip-shaped thin plate 5 at room temperature using a known cold rolling machine. By performing warm rolling or cold rolling, the surface of the strip-shaped thin plate 5 can be smoothed, and the thickness, width, and properties of the finally obtained strip-shaped thin plate 5 (i.e., the soft magnetic steel sheet) can be appropriately adjusted.
[0029] The raw materials used in the manufacture of the soft magnetic steel sheet mainly include iron scrap. As the iron scrap, commercially available scrap that is generally available in the market can be used. For example, iron scrap discharged from a manufacturing plant for automobiles or the like, iron scrap collected from scrapped automobiles, etc. may be used as the raw material.
[0030] In addition to Fe (iron), which is the base material of soft magnetic steel sheets, scrap iron as a raw material may contain Cu (copper), Cr (chromium), Ni (nickel), Sn (tin), etc., which are impurities (i.e., unnecessary components) for soft magnetic steel sheets. In other words, Cu, Cr, Ni, and Sn in soft magnetic steel sheets are components derived from scrap iron.
[0031] From the viewpoint of stably producing the soft magnetic steel sheet and ensuring good magnetic properties, the content of impurities (that is, Cu, Cr, Ni, and Sn) is preferably set within a predetermined range.
[0032] The Cu content in the soft magnetic steel sheet is preferably 0.1 to 1.0 wt%. The Cr content in the soft magnetic steel sheet is preferably 0.01 to 0.5 wt%. The Ni content in the soft magnetic steel sheet is preferably 0.01 to 0.5 wt%. The Sn content in the soft magnetic steel sheet is preferably 0.01 to 0.3 wt%. In addition, the total of Cu, Cr, Ni, and Sn in the soft magnetic steel sheet is preferably 1.2 wt% or less, more preferably 1.0 wt% or less. Here, the lower limit of the content of each impurity is shown, but they are not essential components for the soft magnetic steel sheet. Therefore, the content of some of these impurities may be zero.
[0033] When the content of impurities is out of the above range (upper limit), it is possible to adjust it to be below the allowable value, for example, by selecting the type of iron scrap used as the raw material.
[0034] In addition, silicon (Si) is added to the raw material as an element that is insufficient in iron scrap in order to reduce iron loss. The Si content in the manufactured soft magnetic steel sheet is preferably 1.0 to 7.0 wt% (weight%).
[0035] The thickness of the finally obtained soft magnetic steel sheet is preferably 0.03 to 0.15 mm. The soft magnetic steel sheet preferably has magnetic properties such that the magnetic flux density B100 is 1.6 T or more, the degree of magnetic orientation B10 / B100 is 0.78 or more, and the iron loss W10 / 400 is 10 W / kg or less. Here, "magnetic flux density B100" indicates the magnetic flux density at a magnetic field strength of 10,000 A / m. "B10 / B100" is the ratio of "B10" to "B100", and is a measure of the degree of magnetic orientation. Furthermore, "iron loss W10 / 400" indicates the iron loss at a frequency of 400 Hz and a magnetic flux density of 1.0 T. EXAMPLES
[0036] As Examples 1-19, soft magnetic steel sheets were manufactured using raw materials in which the content of Cu, Cr, Ni, and Sn as impurities was changed relative to Fe as the base material (i.e., the main component excluding other components such as impurities), and the feasibility of manufacturing them and their magnetic properties were evaluated.
[0037] In the manufacture of the soft magnetic steel sheets according to Examples 1-19, first, raw materials each containing a predetermined content of impurities were prepared. More specifically, pure iron and ferrosilicon were mixed and melted, and the raw materials were adjusted so that the content of impurities when the total content of Fe, Si, and impurities (here, Cu, Cr, Ni, and Sn) was taken as 100 wt % were each a predetermined chemical composition.
[0038] Thereafter, as described above, a belt-shaped thin plate 5 was formed by the manufacturing apparatus 1 (see FIG. 1) using the single roll method. More specifically, the molten metal 3 was discharged from the injection hole 4a of the nozzle 4 onto the outer peripheral surface of the chill roll 2, and was rapidly cooled and solidified to form a belt-shaped thin plate 5 having a predetermined thickness (see Table 1) and a width of 20 mm. At this time, the temperature of the molten metal 3 was adjusted to 1400 to 1700°C, the peripheral speed of the chill roll 2 was adjusted to 5 to 20 m / s, the discharge pressure of the molten metal 3 was adjusted to 10 kPa to 40 kPa, and the gap between the tip of the nozzle 4 and the chill roll 2 was adjusted to 0.2 mm to 0.4 mm.
[0039] Furthermore, the obtained belt-shaped thin plate 5 was subjected to heat treatment in an inert atmosphere (here, Ar gas) in a heating furnace under predetermined conditions (see Table 1) as described above.
[0040] As Comparative Example 1-6, soft magnetic steel sheets were manufactured in the same manner as in Example 1-19 using raw materials that did not substantially contain Cu, Cr, Ni, and Sn as impurities, and the feasibility of manufacturing them and their magnetic properties were evaluated.
[0041] The chemical compositions and heat treatment conditions (temperature, time) for Examples 1-19 and Comparative Examples 1-6 are shown in Table 1. In Table 1, the products that could be formed into the strip-shaped thin plate 5 by the manufacturing apparatus 1 are indicated by a circle (◯) to show whether they could be manufactured, and the products that could not be formed into the strip-shaped thin plate 5 (including the products where cracks occurred in the steel plate) are indicated by a cross (the same applies to Table 2 described later).
[0042] In addition, soft magnetic steel sheets were manufactured using a conventional hot rolling technique (hereinafter referred to as "Conventional Techniques 1-3"), and their manufacturing feasibility and magnetic properties were evaluated. In Conventional Techniques 1-3, an ingot with its chemical composition adjusted using a vacuum melting furnace was hot rolled to a thickness of 2 mm at a temperature of 1100°C, and then cold rolled to form a steel sheet with a thickness of 0.1 mm. However, in Conventional Technique 3, cracks occurred during cold rolling and it was impossible to form the steel sheet. The obtained steel sheet was subjected to heat treatment in the same manner as in Example 1-19.
[0043] [Table 1]
[0044] Table 2 shows the thickness and magnetic properties of each of the soft magnetic steel sheets obtained for Examples 1-19 and Comparative Examples 1-6. In Table 2, "W10 / 400" indicates the iron loss at a frequency of 400 Hz and a magnetic flux density of 1.0 T. Also, "B10", "B50", and "B100" indicate the magnetic flux densities at magnetic field strengths of 1000 A / m, 5000 A / m, and 10000 A / m, respectively. Also, "B10 / B100" is the ratio of "B10" to "B100", and is a measure of the degree of magnetic orientation.
[0045] [Table 2]
[0046] Next, with reference to Figs. 2 to 7 based on the data shown in Tables 1 and 2, the evaluation results of the magnetic properties of the soft magnetic steel sheets of Examples 1 to 19 and Comparative Examples 1 to 6 will be described.
[0047] Figure 2 shows the relationship between iron loss and B10 / B100. The iron loss W10 / 400 of the soft magnetic steel sheet should be 10 W / kg or less to reduce energy consumption. In addition, the B10 / B100 of the soft magnetic steel sheet should be 0.78 or more from the viewpoint of magnetic orientation.
[0048] In Examples 14-17 in which the Cu content exceeded 1.0 wt%, the iron loss W10 / 400 exceeded 10 W / kg, and the B10 / B100 was less than 0.78. In other words, the Cu content of the soft magnetic steel sheet is preferably set to 1.0 wt% or less in order to ensure good magnetic properties.
[0049] In Comparative Examples 1-6, which did not contain impurities, the iron loss W10 / 400 of the soft magnetic steel sheet was 10 W / kg or less, and the B10 / B100 of the soft magnetic steel sheet was 0.78 or more. In Conventional Technique 2, the iron loss W10 / 400 exceeded 10 W / kg, and in Conventional Technique 3, which contained impurities, it was difficult to manufacture the soft magnetic steel sheet.
[0050] FIG. 3 shows the relationship between the Cu and Sn contents of the soft magnetic steel sheet and whether or not it can be manufactured. For Examples 1-17 and 19 (i.e., the Cu content is in the range of 0.10 to 3.60, and the Sn content is in the range of 0.1 to 0.70), it was possible to manufacture the soft magnetic steel sheet. On the other hand, for Example 18, in which the Cu content is 5.0 wt% and the Sn content is 1.0 wt%, it was difficult to manufacture the soft magnetic steel sheet. In other words, from the viewpoint of stably manufacturing the soft magnetic steel sheet, it is preferable to set the Cu content of the soft magnetic steel sheet to 3.6 wt% or less. Similarly, it is preferable to set the Sn content of the soft magnetic steel sheet to 0.7 wt% or less.
[0051] FIG. 4 shows the relationship between the Cu content of the soft magnetic steel sheet and the iron loss W10 / 400. Here, Example 12 (see the colored circles in FIG. 4) contains only Cu as an impurity. That is, the Cu content of the soft magnetic steel sheet is preferably set to 1.0 wt% or less from the viewpoint of reducing the iron loss W10 / 400 to 10 W / kg or less, as described above, regardless of whether it contains only Cu as an impurity or contains other impurities in addition to Cu. In this case, the Cr content is preferably 0.3 wt% or less. The Ni content is preferably 0.3 wt% or less. Also, the Sn content is preferably 0.25 wt% or less.
[0052] Fig. 5 shows the relationship between the Cu content of the soft magnetic steel sheet and B10 / B100. Here, Example 12 (see the colored circles in Fig. 4) contains only Cu as an impurity. In other words, the Cu content of the soft magnetic steel sheet is preferably set to 1.0 wt% or less from the viewpoint of making B10 / B100 0.78 or more, as described above, regardless of whether it contains only Cu as an impurity or contains other impurities in addition to Cu.
[0053] 6 shows the relationship between the impurity content (total of Cu, Cr, Ni, and Sn) of the soft magnetic steel sheet and the iron loss W10 / 400. From the viewpoint of reducing the iron loss W10 / 400 to 10 W / kg or less, the impurity content of the soft magnetic steel sheet is preferably set to 1.2 wt% or less as the total of Cu, Cr, Ni, and Sn.
[0054] 7 shows the relationship between the impurity content (total of Cu, Cr, Ni, and Sn) of the soft magnetic steel sheet and B10 / B100. From the viewpoint of making B10 / B100 0.78 or more, the impurity content of the soft magnetic steel sheet is preferably set to 1.2 wt% or less as the total of Cu, Cr, Ni, and Sn.
[0055] 8 to 10 show photographs of the crystal structure of soft magnetic steel sheets observed by a scanning electron microscope (SEM). FIG. 8 shows the crystal structure of Example 13, and no inclusions due to impurity elements are observed. On the other hand, in the microstructure photograph of Example 14 (i.e., Cu content of 1.2 wt%) shown in FIG. 9, inclusions are present at the crystal grain boundaries. Moreover, in the microstructure photograph of Prior Art 2 shown in FIG. 10, inclusions due to impurity elements are also present, and these inclusions deteriorate the magnetic properties.
[0056] From the above results, from the viewpoint of stably producing soft magnetic steel sheets from raw materials including iron scrap and ensuring good magnetic properties (i.e., realizing magnetic properties equivalent to those of soft magnetic steel sheets with a low impurity content), it is preferable that the Cu content in the soft magnetic steel sheet is 1.0 wt% or less. It is also preferable that the Cr content is 0.3 wt% or less. It is also preferable that the Ni content is 0.3 wt% or less. It is also preferable that the Sn content is 0.25 wt% or less. Furthermore, it is preferable that the impurity content of the soft magnetic steel sheet is set to 1.2 wt% or less as the sum of Cu, Cr, Ni, and Sn.
[0057] Although the specific embodiment has been described above, the present invention is not limited to the above embodiment and its modified examples, and can be modified in a wide range of ways. [Explanation of symbols]
[0058] 1: Manufacturing equipment 2: Cooling roll 3: Molten metal 4: Nozzle 4a: Injection hole 5: Thin strip 7: Heater
Claims
1. A soft magnetic steel sheet manufactured from raw materials including iron scrap, Fe as a base material; 1.0 to 7.0 wt% Si; 0.1 to 1.0 wt % of Cu, which is a component derived from the iron scrap; Soft magnetic steel plate.
2. As the components derived from the iron scrap, 0.01 to 0.5 wt% Cr; 0.01 to 0.5 wt % Ni; 0.01 to 0.3 wt % Sn; Further comprising:
2. The soft magnetic steel sheet according to claim 1, wherein the total content of Cu, Cr, Ni and Sn is 1.2 wt % or less.
3. A method for producing a soft magnetic steel sheet according to claim 1 or 2, a strip-shaped thin plate forming step of forming a strip-shaped thin plate from the raw material by a single roll liquid quenching solidification method; a heat treatment step of heat treating the strip in an inert atmosphere at 600 to 1200°C; A method for producing a soft magnetic steel sheet, comprising:
4. The soft magnetic steel sheet has a thickness of 0.03 to 0.15 mm, a magnetic flux density B100 of 1.6 T or more, a magnetic orientation degree B10 / B100 of 0.78 or more, and an iron loss W10 / 400 of 10 W / kg or less. The manufacturing method of the soft magnetic steel sheet according to claim 3.
5. The method for producing a soft magnetic steel sheet according to claim 3, further comprising the steps of: warm rolling and / or cold rolling the strip-shaped thin plate prior to the heat treatment step.
6. The method for producing a soft magnetic steel sheet according to claim 3 , further comprising a Si addition step of adding Si to the iron scrap as the raw material.
Citation Information
Patent Citations
High-tension soft-magnetic thin steel strip of fe-base alloy
JP1986087848A
Production of nonoriented silicon steel sheet excellent in magnetic property
JP1996041542A
Production of nonoriented silicon steel sheet excellent in surface property and magnetic property
JP1996295936A
Production of nonoriented silicon steel sheet excellent in surface property
JP1999293338A
High grade nonoriented silicon steel sheet and its manufacturing method
JP2001172753A