Optical wave-guide element, optical modulation device using the same, and optical transmitter

By employing a SiN waveguide with a low refractive index layer and a TFLN rib-type waveguide with a thinner convex portion, the optical waveguide element achieves low-loss optical transfer and supports optical modulation devices and transmitters, addressing the challenges of integrating materials with small refractive index differences.

JP2024142673APending Publication Date: 2024-10-11SUMITOMO OSAKA CEMENT CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
JP2023054914
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing optical waveguide devices face challenges in achieving low-loss optical transfer between materials with small refractive index differences, such as SiN and TFLN rib-type optical waveguides, due to issues like optical loss and high manufacturing complexity.

Method used

The optical waveguide element features a first substrate with a SiN waveguide covered by a low refractive index layer, bonded to a second substrate with a TFLN rib-type waveguide, where a convex portion on the second substrate at the overlap boundary is thinner than the rest, and the first waveguide width is widened, enhancing optical confinement and reducing loss.

Benefits of technology

This configuration enables low-loss optical transfer between SiN and TFLN waveguides, supporting the integration of optical modulation devices and transmitters, even with small refractive index differences, by minimizing optical loss and manufacturing complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142673000001_ABST
    Figure 2024142673000001_ABST
Patent Text Reader

Abstract

To provide an optical wave-guide element which can perform optical migration between a SiN wave guide or a TFLN rib-type optical wave guide, even when a difference in refractive index is minimal as in the SiN wave guide or the TFLN rib-type optical wave guide.SOLUTION: An optical wave-guide element comprises: a first substrate 1 including a first optical wave guide 10, and a low refractive index layer 11 covering the first optical wave guide 10 and composed of a material lower in refractive index than the first optical wave guide; and a second substrate 2 joined to the first substrate 1 and having a rib-type optical wave guide 20 which is a second optical wave guide and composed of a material having an electro-optical effect, the first optical wave guide 10 and the second optical wave guide 20 having a section optically joined with each other. A protrusion 23 is formed on the second substrate at a boundary where the first optical wave guide and the second substrate overlap each other when the optical wave-guide element is viewed in a plan view, and the thickness of the second substrate 2 in the protrusion 23 is thinner than the thickness of the second substrate 2 in the second optical wave guide 20.SELECTED DRAWING: Figure 7
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical waveguide element, and an optical modulation device and optical transmission device using the same, and in particular to an optical waveguide element in which a first substrate on which a first optical waveguide is formed is joined to a second substrate on which a rib-type optical waveguide that is a second optical waveguide is formed, and the first optical waveguide and the second optical waveguide are optically coupled to each other, and an optical modulation device and optical transmission device using the same. [Background technology]

[0002] In recent years, Si waveguides have been used as optical waveguides when creating optical waveguide elements for optical communications, etc. (see Non-Patent Document 1). Si waveguides use CMOS processes, so they are scalable and have excellent cost reduction properties, and it is also possible to incorporate a Ge / Si light receiving element. On the other hand, they have disadvantages in that they cannot be used in the visible light range, and phase modulation is difficult to control, as it is performed by passing a current through the Si waveguide.

[0003] For this reason, new platforms using silicon nitride (SiN) or thin film LiNbO3 (TFLN, thin film LN) as the optical waveguide core are being considered as alternative technologies (see non-patent documents 2 and 3). In order to integrate optical functions, light sources, phase modulation, reception, and optical multiplexing / demultiplexing (power multiplexing / branching, wavelength multiplexing / demultiplexing, polarization multiplexing / demultiplexing, etc.) are essential. Since the optimal materials for each of these components are different, methods of integrating different materials have been developed.

[0004] In the case of joining different materials, epitaxial growth can also be used. In recent years, by using a direct bonding method in which materials with flattened surfaces are bonded, optical function integration has been realized using combinations of materials that cannot be grown epitaxially. Among these, elements that integrate optical multiplexing / demultiplexing and phase modulation have been developed by integrating silicon nitride (SiN) waveguides with TFLN.

[0005] In Non-Patent Document 4, a SiN waveguide is formed on TFLN to achieve phase modulation without processing LN into a waveguide. Compared with a monolithic TFLN modulator (see Non-Patent Document 2), this method has a weaker light confinement in the optical waveguide, so the bending radius is large at about several hundred μm, and the driving voltage (Vπ) is also large. However, productivity is ensured by processing SiN, which is easy to process, instead of processing LiNbO3 (LN), which is a material that is difficult to process (difficult to dry etch).

[0006] On the other hand, it has been proposed to replace the phase modulation part of an optical modulator using Si with a phase modulation using the electro-optic effect of LN or the like, thereby achieving both the same phase modulation as conventional LN and the ease of processing, mass production, and miniaturization of the Si waveguide (see Non-Patent Document 5). The refractive index of Si is about 3.45, which is considerably higher than that of LN, which is about 2.14. Increasing the dimensions of the Si waveguide increases the light confinement effect as an optical waveguide, and the light distribution can be concentrated only within the Si waveguide, making it less susceptible to the effects of light scattering due to structural changes in other materials in the vicinity of the Si waveguide. As a result, it is possible to suppress the optical loss at the end of the TFLN substrate placed on the substrate including the Si waveguide.

[0007] FIG. 1 is a plan view showing an example in which a second substrate 2 such as TFLN including a second optical waveguide 20 is superimposed on a first substrate 1 including a first optical waveguide 10 such as a Si waveguide. Cross-sectional views along dashed lines AA, BB, and CC in FIG. 1 are shown in (a) to (c) of FIG. 2. The first optical waveguide 10 is a core portion, and is covered with a low-refractive index layer 11 (cladding portion) made of a material with a lower refractive index than the material constituting the optical waveguide. In order to maintain mechanical strength, the first optical waveguide is supported by a holding substrate 12 as necessary. The second optical waveguide 20 is a rib-type optical waveguide in which a part of the second substrate is made higher than the surrounding area.

[0008] When the optical waveguide element is viewed in a plan view as shown in Figure 1, at the boundary portion where the first optical waveguide 10 and the second substrate 2 overlap (the edge portion of the second substrate), a portion 100 where the width of the first optical waveguide is widened is provided to enhance the optical confinement effect and suppress optical loss due to the influence of the edge portion of the second substrate 2.

[0009] In addition, the optical transition between the Si waveguide and the TFLN waveguide is achieved by reducing the cross-sectional dimension of the Si waveguide on the high refractive index side, thereby expanding the optical distribution and transferring the light wave to the TFLN waveguide. As a result, the optical transition between the Si waveguide and the TFLN waveguide can be achieved with low loss (see Non-Patent Document 6). For this reason, the first optical waveguide 101 that is recessed under the second substrate is tapered at the position where it overlaps with the second optical waveguide 20, as shown in FIG. 1.

[0010] The problem with Si waveguides is that they are opaque at wavelengths below 1.1 μm, making them unusable, and they also suffer from phenomena such as two-photon absorption, making it impossible to input high-intensity light. Therefore, by combining SiN waveguides and TFLN, it is possible to provide optical waveguide elements that can be used up to the visible range and can perform phase modulation by changing the electric field strength used in LN optical modulators. Naturally, the dry etching processing technology for SiN has also been established, so productivity is high, just like with Si waveguides.

[0011] However, the refractive index of SiN is about 2.00, which is close to the refractive index of LN (about 2.14). Therefore, even if the dimension of the SiN waveguide, which is the first optical waveguide, is increased at the edge of the TFLN, it will be affected by the TFLN. Also, it is difficult to simply apply the structure used for the Si waveguide to the optical transition between the SiN waveguide, which is the first optical waveguide, and the TFLN rib-type optical waveguide 20, which is the second optical waveguide. For example, it is possible to remove the periphery of the rib-type optical waveguide 20 as much as possible to make it thinner, or to narrow the width dimension of the second substrate 2, but this requires high processing accuracy, which leads to increased manufacturing costs and reduced yields.

[0012] Furthermore, in order to form a rib-type optical waveguide 20 in a TFLN second substrate on a first substrate 1 as shown in FIG. 2(c), after bonding the second substrate 2 to the first substrate 1 as shown in FIG. 3(a), a resist pattern PR1 is formed to cover the position where the second optical waveguide is to be formed and the portions of the first substrate 1 that should not be etched as shown in FIG. 3(b).

[0013] In particular, at the edge of the TFLN near which the first optical waveguide is located, the resist material is arranged to cover (overhang) the edge. If part of the first optical waveguide, the Si waveguide or SiN waveguide, is damaged by etching, a large optical loss will occur. As a result, as shown in Fig. 3(c), a protrusion 22 of the same height as the rib type optical waveguide 20 is formed at the edge of the TFLN. Fig. 4 is a plan view, and the protrusion 22 is formed at the edge of the second substrate 2 including the boundary with the first optical waveguide 10 (100). Fig. 5 is a cross-sectional view taken along dashed line DD in Fig. 4.

[0014] Regarding the influence of the convex portion 22, when the first optical waveguide is a Si waveguide, it is possible to enhance the optical confinement effect and suppress optical loss by configuring the portion 100 in which the width of the optical waveguide is increased; however, when the first optical waveguide is a SiN waveguide, it is difficult to solve this problem by configuring only the portion 100 in which the width is increased. [Prior art documents] [Non-patent literature]

[0015] [Non-Patent Document 1] Yikai Su, etc.,"Silicon Photonic Platform for Passive Waveguide Devices: Materials, Fabrication, and Applications", Advanced Materials Technologies. 1901153 (2020) [Non-Patent Document 2] Abdul Rahim, etc.,"Expanding the Silicon Photonics Portfolio With Silicom Nitride Photonic Integrated Circuits", Journal of Lightwave Technology, Vol.35, No.4, pp639(Feb. 15,2017) [Non-Patent Document 3] Mian Zhang, etc.,"Integrated Lithium Niobate Electro-optic Modulators: When performance meets scalability", Optica, Vol.8, No.5, pp652(2021) [Non-Patent Document 4] Sean Nelan, etc.,"Ultra-high Extinction Dual-output Thin-film Lithium Niobate Intensity Modulator", arXiv:2207.02608v1 (Jul. 6,2022) [Non-Patent Document 5] Shihao Sun, etc.,"Hybrid Silicon and Lithium Niobate Modulator", IEEE Journal of selected topics in Quantum Electronics, Vol.27, No.3, pp3300112(May / June 2021) [Non-Patent Document 6] Peter O. Weigel, etc.,"Bonded Thin Film Lithium Niobate Modulator on a Silicon Photonics Platform Exceeding 100 GHz 3-dB Electrical Modulation Bandwidth", Optics Express, Vol.26, No.18, pp.23728(Sep. 3,2018) Summary of the Invention [Problem to be solved by the invention]

[0016] The problem to be solved by the present invention is to provide an optical waveguide element that can perform optical transfer between two elements with low loss even when the refractive index difference between the two elements is small, such as a SiN waveguide or a TFLN rib-type optical waveguide, by solving the above-mentioned problems, and further to provide an optical modulation device and an optical transmission device using the optical waveguide element. [Means for solving the problem]

[0017] In order to solve the above problems, the optical waveguide element and the optical modulation device and optical transmission device using the same according to the present invention have the following technical features.

[0018] (1) An optical waveguide element comprising: a first substrate having a first optical waveguide and a low refractive index layer covering the first optical waveguide and made of a material having a refractive index lower than that of the first optical waveguide; and a second substrate bonded to the first substrate and made of a material having an electro-optic effect, the second substrate having a rib-type optical waveguide as a second optical waveguide, the first optical waveguide and the second optical waveguide having a portion optically coupled to each other, the optical waveguide element being characterized in that, when the optical waveguide element is viewed in a plane, a convex portion is formed in the second substrate at a boundary portion where the first optical waveguide and the second substrate overlap, and the thickness of the second substrate at the convex portion is configured to be thinner than the thickness of the second substrate at the second optical waveguide.

[0019] (2) The optical waveguide element according to (1) above, wherein the length of the first optical waveguide in the light wave propagation direction at the protruding portion is 2 μm or less.

[0020] (3) In the optical waveguide element described in (1) above, a width of the first optical waveguide at the boundary is set to be wider than a width of the first optical waveguide located before or after the boundary.

[0021] (4) The optical waveguide element according to (1) above, wherein the difference in refractive index between the first optical waveguide and the second optical waveguide is 0.8 or less.

[0022] (5) The optical waveguide element according to (4) above, wherein the first optical waveguide is made of SiN, and the second substrate is made of lithium niobate.

[0023] (6) An optical modulation device comprising the optical waveguide element according to any one of (1) to (5) above housed in a housing and including an optical fiber for inputting or outputting a light wave to the first optical waveguide.

[0024] (7) In the optical modulation device described in (6) above, the second substrate has a modulation electrode for modulating an optical wave propagating through the second optical waveguide, and an electronic circuit for amplifying a modulation signal input to the modulation electrode is provided inside the housing.

[0025] (8) An optical transmission device comprising the optical modulation device according to (7) above, a light source for inputting an optical wave to the optical modulation device, and an electronic circuit for outputting a modulated signal to the optical modulation device. Effect of the Invention

[0026] The present invention provides an optical waveguide element comprising a first substrate having a first optical waveguide and a low refractive index layer covering the first optical waveguide and made of a material having a lower refractive index than the first optical waveguide, and a second substrate bonded to the first substrate, made of a material having an electro-optic effect, and having a rib-type optical waveguide as a second optical waveguide, wherein the first optical waveguide and the second optical waveguide have a portion optically coupled to each other, in which, when the optical waveguide element is viewed in a plane, a convex portion is formed in the second substrate at a boundary portion where the first optical waveguide and the second substrate overlap, and the thickness of the second substrate at the convex portion is configured to be thinner than the thickness of the second substrate at the second optical waveguide, thereby making it possible to suppress optical loss in the first optical waveguide caused by an edge portion of the second substrate. This makes it possible to provide an optical waveguide element that enables low-loss optical transfer between the two even when the refractive index difference between the two is small, such as in the case of a SiN waveguide or a TFLN rib-type optical waveguide, and further makes it possible to provide an optical modulation device and an optical transmission device that use this optical waveguide element. [Brief description of the drawings]

[0027] [Figure 1] FIG. 1 is a plan view showing an example of an optical waveguide element. [Diagram 2] 2A is a cross-sectional view of the optical waveguide element of FIG. 1, (a) is a cross-sectional view taken along dashed line AA, (b) is a cross-sectional view taken along dashed line BB, and (c) is a cross-sectional view taken along dashed line CC. [Diagram 3] 1 is a diagram showing a part of the manufacturing process of an optical waveguide element, and in particular shows how convex portions 22 are formed on second substrate 2. FIG. [Figure 4] FIG. 4 is a plan view of the optical waveguide element shown in FIG. [Diagram 5] 5 is a cross-sectional view taken along dashed line DD in FIG. [Figure 6] FIG. 1 is a plan view showing an example of an optical waveguide element of the present invention. [Figure 7] 7 is a cross-sectional view taken along dashed line DD in FIG. 6. [Figure 8] FIG. 2 is a diagram showing a part (part 1) of a manufacturing process for the optical waveguide element of the present invention. [Figure 9] FIG. 4 is a diagram showing a second part of the manufacturing process for the optical waveguide element of the present invention. [Figure 10] 1A to 1C are diagrams illustrating an example in which two optical waveguides are optically coupled in an optical waveguide element of the present invention. [Figure 11] 1 is a diagram showing an example of effective refractive index changes in two optical waveguides in the propagation direction of light; [Figure 12] FIG. 13 is a diagram for explaining a simulation model in which TFLN is loaded on the upper side of a SiN waveguide. [Figure 13] 1 is a graph showing the relationship between the width of a SiN waveguide and the thickness of a TFLN. [Figure 14] FIG. 13 is a diagram showing the change in overlap integral (Loss) due to the change in the distance between the SiN waveguide and the TFLN and the change in the thickness of the TFLN when the height (thickness) of the SiN waveguide is constant. [Figure 15] FIG. 1 is a diagram illustrating a simulation model of light transfer between a SiN waveguide and a rib-type optical waveguide (TFLN). [Figure 16] 1 is a graph showing a change in optical loss with a change in wavelength. [Figure 17] FIG. 13 is a diagram illustrating a simulation model for evaluating the influence of a protrusion at an edge of a TFLN. [Figure 18] FIG. 13 is a diagram showing the influence of a protrusion of TFLN. [Figure 19] FIG. 1 is a diagram for explaining a part of a manufacturing process using a wafer constituting a plurality of optical waveguide elements (chips). [Figure 20] 1A to 1C are diagrams illustrating a part of a manufacturing process for an optical waveguide element that uses a second substrate (TFLN) for the active portion of an optical modulator. [Figure 21] 1 is a diagram illustrating an example of an optical transmitting device according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] The optical waveguide element of the present invention will be described in detail below using preferred examples. As shown in Figures 6 and 7, the optical waveguide element of the present invention comprises a first substrate 1 having a first optical waveguide 10, a low refractive index layer 11 covering the first optical waveguide 10 and made of a material having a refractive index lower than that of the first optical waveguide, and a second substrate 2 bonded to the first substrate 1, made of a material having an electro-optic effect, and having a rib-type optical waveguide 20 as a second optical waveguide, the first optical waveguide 10 and the second optical waveguide 20 having a portion optically coupled to each other, the optical waveguide element is characterized in that, when the optical waveguide element is viewed in plan, a convex portion 23 is formed on the second substrate at the boundary where the first optical waveguide and the second substrate overlap, and the thickness of the second substrate 2 at the convex portion 23 is configured to be thinner than the thickness of the second substrate 2 at the second optical waveguide 20.

[0029] In the optical waveguide element of the present invention, the first optical waveguide is mainly a SiN waveguide, and the second substrate is mainly TFLN, but the present invention is not limited to these materials. For example, it is also possible to use a Si waveguide as the first optical waveguide. However, the optical waveguide element of the present invention can be used more preferably when the difference in refractive index between the material used for the first optical waveguide and the material used for the second optical waveguide is small. For example, considering that the refractive index of SiN is in the range of 1.5 to 2.0 and the refractive index of LN is 2.1 to 2.3, it is more preferable to use the present invention when the refractive index difference is 0.8 or less. Below, the explanation will be mainly on the case where SiN is used, but in the case of pure SiN, it is possible to adjust the refractive index to 1.5 to 2.0 depending on the density, but a film with a low density is likely to change the refractive index due to the inclusion of moisture. For this reason, the SiN in the present invention can also contain silicon oxynitride (SiON) whose composition can be adjusted.

[0030] Fig. 6 is a plan view showing an example of an optical waveguide element of the present invention, and Fig. 7 is a cross-sectional view taken along dashed line DD in Fig. 6. When the first optical waveguide 10 is formed of a SiN waveguide, SiN is disposed in the first optical waveguide (core portion), and a cladding portion is formed of a material having a lower refractive index than the SiN of the core portion so as to cover the periphery. For example, the core portion of the optical waveguide of the first substrate 1 is formed of SiN, and the cladding portion 11 that covers the core portion 10 is formed of SiO2. This cladding portion 11 is called a low refractive index layer.

[0031] In the present invention, the substrate including the first optical waveguide 10 is called the first substrate 1, and the first substrate may include not only the first optical waveguide 10 and the low refractive index layer 11 covering it, but also a support substrate 12 for increasing the mechanical strength of the entire substrate. The support substrate may be made of Si or SiO2.

[0032] The second substrate 2 bonded to the first substrate 1 is made of a thin plate of a material having an electro-optic effect, such as lithium niobate (LN), lithium tantalate (LT), or PLZT (lead lanthanum zirconate titanate). The following explanation will focus on TFLN. A rib-type optical waveguide 20 is formed as a second optical waveguide on the surface of the second substrate 2. The first optical waveguide 10 and the second optical waveguide have an overlapping portion when viewed in a plan view as shown in Fig. 6, and are configured to transfer light waves between the first optical waveguide and the second optical waveguide by utilizing the overlapping portion. The shape of the overlapping portion will be described in detail later.

[0033] A feature of the optical waveguide element of the present invention is that, as shown in Fig. 6, a convex portion 23 is formed on the second substrate 2 at the boundary where the first optical waveguide 10 and the second substrate 2 overlap when the optical waveguide element is viewed in a plan view. As shown in Fig. 7, the thickness of the second substrate 2 at the convex portion 23 is configured to be thinner than the thickness of the second substrate 2 at the second optical waveguide 20. Note that, in Fig. 6, the convex portion 23 is formed only on the edge portion of the second substrate near the first optical waveguide 10, but this is not limiting, and for example, the convex portion 23 can be formed on the entire edge portion of the second substrate as shown in Fig. 10.

[0034] In the optical waveguide element of the present invention, the height of the convex portion 23 is reduced in order to suppress scattering of the light wave propagating through the first optical waveguide 10 by the convex portion 23. By setting the height lower than at least the height of the second optical waveguide 20, the occurrence of optical loss is suppressed. In addition, the effective refractive index of a part of the first optical waveguide 10 that is disposed below the convex portion 23 is increased compared to the other parts, and the light confinement is strengthened, thereby making it possible to reduce scattering of the light wave by the convex portion. Specifically, as shown by reference numeral 100 in FIG. 6, the width of the optical waveguide is set wide. In this specification, the first optical waveguide is indicated by reference numeral 10, the part that becomes wider near the edge portion of the second substrate is indicated by reference numeral 100, and the part of the first optical waveguide located below the second substrate is indicated by reference numeral 101.

[0035] Furthermore, with regard to the shape of the protrusion 23, it is preferable that the length of the protrusion 23 in the propagation direction of the light wave of the first optical waveguide 10 is 2 μm or less. By setting the length in this range, it is possible to further suppress the optical loss. The details will be described later.

[0036] Next, a manufacturing process for the optical waveguide element of the present invention will be described with reference to Figures 8 and 9. The optical waveguide element described below uses a SiN waveguide and TFLN. (STEP 1) 8(a) is prepared. The SiN 101 is covered with a low refractive index layer 11 and supported by a support substrate 12. (STEP 2) A TFLN film having a thickness of about 0.5 μm is prepared as the second substrate 2. The TFLN film is attached to a holding member 25 via a release layer 24. Specific examples of the material for the release layer include WOx.

[0037] (STEP 3) The SiN waveguide (first substrate) and the TFLN (second substrate) are bonded (see Figs. 8(a) and (b)). The bonding method may be direct bonding or resin adhesion, but Fig. 8(b) shows direct bonding. Direct bonding is also described in Non-Patent Document 6.

[0038] (STEP4) The release layer 24 is side-etched with an appropriate chemical solution (see FIG. 8(c)). When side-etching WOx with a chemical solution, a mixture of ammonia water and hydrogen peroxide solution is appropriate as the etching solution. When side-etching is performed by dry etching, fluorine-based gases such as SF6 and XeF2 can also be used as the etching gas. At this time, the amount of side etching is arbitrary, but it is desirable for it to be equal to or greater than the thickness of the release layer 24.

[0039] (STEP5) An appropriate processing inhibiting film PR2 is formed on the above-mentioned sample (see FIG. 9(d)). A film formation method with step coverage is required for film formation. Specifically, sputtering film formation is performed, and "step coverage = film thickness at thinnest part / film thickness at flat part" (the ratio of film thickness at the thinnest part to the film thickness at the flat part) is set to about 0.5. Normally, the step coverage of vacuum deposition is close to 0, but the step coverage can be increased by increasing the pressure during film formation. When using a material with high dry etching resistance (described later) for film formation, it is preferable that the step coverage be smaller than 0.5.

[0040] The material used for the processing inhibition film PR2 is one that can obtain an appropriate selection ratio during TFLN processing and is one that is not removed at the same time when the release layer is side-etched. Specifically, when the release layer is WOx, Cr or the like is preferably used. It is also possible to commercialize the processing inhibition film while leaving it after TFLN processing. In this case, the additional conditions for the film material are that it does not absorb light and that its refractive index is lower than that of SiN or LN. Specific materials for the processing inhibition film include Al2O3, SiO2, HfO2, GeO2, and the like. However, since the material of the processing inhibition film differs depending on the dry etching conditions of TFLN, it is not limited to the above materials. The thickness of the processing inhibition film PR2 is required to be thick enough not to process not only the SiN waveguide (SiN) during processing when forming the TFLN waveguide, but also to the inside of the range including a part of the low refractive index layer 11 that has SiN as the core and functions as the cladding part. It is sufficient that the thickness of the processing inhibiting film PR2 is sufficient on the upper part of the edge portion of the TFLN, and it is preferable that the TFLN substrate 2 is exposed after the TFLN waveguide is formed.

[0041] (STEP 6) The release layer 24 is removed with an appropriate chemical solution, and the holding member is peeled off (see FIG. 9(e)). It is also possible to peel it off with the chemical solution used in STEP 4.

[0042] (STEP7) Resist is applied to a substrate "SiN waveguide substrate with TFLN" in which TFLN is bonded to a substrate (101, 11, 12) including a SiN waveguide 101, and a resist pattern PR3 is formed. The pattern is aligned with respect to the SiN waveguide 101. Here, the resist PR3 does not need to cover (overhang) the outer periphery of the TFLN (second substrate 2). The resist PR3 is a resist that protects the TFLN and is a resist for forming a rib-type optical waveguide 20 in the TFLN (see FIG. 9(f)). For example, in the case of overhanging as shown in FIG. 3(b), the thickness of the second substrate located under the resist PR3 becomes the same as the thickness of the second substrate in the rib-type optical waveguide 20. This makes it difficult to make the height of the convex portion of the edge portion of the second substrate lower than that of the rib-type optical waveguide, which is a feature of the optical waveguide element of the present invention.

[0043] (STEP8) Using the resist pattern PR3 as a mask, the TFLN is dry etched to form a rib type optical waveguide 20 in the TFLN (see FIG. 9(g)). Because the thickness of the processing inhibiting film PR2 at the edge of the TFLN is thinner than the thickness on the SiN waveguide, the LN may be exposed after the TFLN waveguide is formed. This state creates a magnitude relationship of "thickness of TFLN rib type optical waveguide 20" > "thickness of TFLN protrusion 23" > "thickness of TFLN processed portion 21", and is also desirable from the viewpoint of suppressing optical loss in the optical waveguide.

[0044] 10(a) is a plan view showing a part of an optical waveguide element produced by the above-mentioned manufacturing process. The processing inhibiting film PR2 remains on the outside of the protruding portion 23 of the TFLN. The thickness of the protruding portion 23 is thinner than that of the rib-type optical waveguide 20 and thicker than the processing portion 21 that is mainly processed. Even when the SiN waveguide 10 with weak light confinement is used, light is scattered near the edge portion of the TFLN, just like the Si waveguide. Therefore, a waveguide width (100) with strong light confinement is used for a part of the SiN waveguide 10.

[0045] The optical transition from the SiN waveguide 10 to the TFLN rib-type optical waveguide 20 is achieved by continuously narrowing the width of the SiN waveguide to form a tapered shape 10A, thereby lowering the effective refractive index, while the TFLN rib-type optical waveguide 20 is continuously widened to form a tapered shape 20A, thereby increasing the effective refractive index. The optical transition is achieved when the effective refractive indices of both become equal.

[0046] The embodiment in Fig. 10(b) has a structure that takes manufacturing tolerance into consideration, and enables stable optical transition even if the relative positions of the SiN waveguide 10 and the rib-type optical waveguide 20 are slightly misaligned in the left-right direction of the drawing. A specific change in the width of the optical waveguide is shown in Fig. 11. As shown in Fig. 11, at the tapered portion 20B of the TFLN rib-type optical waveguide 20, the SiN waveguide 10 is an optical waveguide 10B of a constant width whose effective refractive index does not change, and by crossing the effective refractive indexes of the respective waveguides, low-loss optical transition and manufacturing tolerance can be ensured.

[0047] In the following, specific design conditions for realizing low-loss optical transition between the SiN waveguide and the TFLN rib-type optical waveguide will be described. First, consider a structure in which TFLN2 is loaded midway into a SiN waveguide 10, as shown in Figure 12(a). When light is incident on the SiN waveguide, the refractive index changes suddenly at the edge of the TFLN2, causing the light to scatter. The loss at this time can be calculated by the overlap integral of the guided light using the refraction distributions in Figures 12(b) and 12(c).

[0048] The SiN waveguide thickness (h) was fixed at 0.5 μm, and the SiN waveguide width (w), the distance between the SiN waveguide and the TFLN (d), and the TFLN thickness (t) were set as parameters that varied within the following numerical ranges, and the optical loss due to the TFLN loading was calculated as shown in Figure 13. The calculation was performed at a wavelength of 1.55 μm in TE mode. w=0.4~1.6μm d=0.1~0.5μm t=0.05~0.25μm

[0049] From Figure 13, we can see that the larger the distance d between the SiN waveguide and the TFLN, the smaller the interaction between the SiN waveguide and the TFLN, and therefore the smaller the optical loss. Similarly, the smaller the thickness t of the TFLN, the smaller the optical loss. It is noteworthy that the optical loss decreases as the SiN waveguide width w is increased, and becomes constant at 1.2 μm or more.

[0050] For this reason, the SiN waveguide width w is fixed at 1.4 μm, and the contour lines of the optical loss (overlap integral) when t and d are parameters are shown in FIG. When the optical loss due to TFLN loading is specified to be 0.1 dB or less, the following relational expression is obtained by approximating the 0.1 dB line in FIG. 14 with a straight line. t≦0.29d+0.072 However, the refractive index of the SiN film can be changed by making it a non-stoichiometric composition (SiNx,x ≠ 1.33) or by changing the density. Furthermore, not only can LN have a non-stoichiometric composition, but the refractive index can also be adjusted by doping with impurities (Mg, Zn, etc.). Therefore, the above formula is only true when the SiN film has a stoichiometric composition and the LN has a congruent melting composition.

[0051] Next, let us consider a state in which a rib structure is added to the TFLN. A case in which a directional coupler is used for optical connection between the SiN waveguide 10 and the TFLN rib-type optical waveguide 20 will be described. A perspective view of the simulated structure is shown in Fig. 15(a). Fig. 15(b) is a plan view of this structure, with the dimensional symbols of each waveguide. The width of the light input part of the SiN waveguide is fixed at SiN_w1 = 0.8 μm, and the width of the SiN waveguide at the edge of the loaded TFLN is made wider at SiN_w2 = 1.4 μm. This is to suppress the optical loss at the TFLN edge. By narrowing the width of the SiN waveguide inside the TFLN loading to SiN_w3, the light propagating through the SiN waveguide is made to be affected by the TFLN.

[0052] For the upper TFLN rib-type optical waveguide 20, the length of the region interacting with the SiN waveguide 10 (101) is DC_L, and the width of the rib waveguide is LN_w1. The width of the rib-type optical waveguide 20 is then increased to LN_w2 = 1.0 μm to confine the light within the waveguide. Cross-sectional views of the dashed lines EE and FF in Figure 15(b) are shown in Figures 15(c) and (d), respectively. The thickness of the SiN waveguide is fixed at h = 0.5 μm, and the thickness of the upper cladding layer is d. The thickness of the TFLN LN_t = 0.5 μm corresponds to the thickness of the rib structure core part.

[0053] The remaining thickness of the TFLN at the portion processed into the rib structure is t. For this structure, we fixed SiN_w3 = 1.0 μm, LN_w1 = 0.75 μm, d = 0.3 μm, and t = 0.1 μm, and calculated the results with DC_L as a parameter, as shown in Figure 16(a). The parameters used in the calculation are shown in Table 1.

[0054] [Table 1]

[0055] The vertical axis in Figure 16(a) is the value obtained by dividing the amount of emitted light (the amount of light emitted from the TFLN rib-type optical waveguide) by the amount of incident light (the amount of light incident on the SiN waveguide). It was found that by setting the coupling length DC_L = 8.0 μm, the transmittance becomes 95% (0.2 dB). For reference, the wavelength dependency (1500 to 1600 nm) when the coupling length DC_L = 8.0 μm is shown in Figure 16(b).

[0056] Furthermore, consider the case where a protrusion is formed on the edge of the TFLN. A perspective view of the simulated structure is shown in Fig. 17(a), a plan view in Fig. 17(b), and a cross-sectional view along the dashed line GG in the plan view in Fig. 17(c). The dimensional symbols used in Fig. 15 are the same in Fig. 17, with the only difference being the protrusion 23 on the edge of the TFLN. This protrusion is described by its length LN_L in the direction in which light propagates and its thickness LN_h, as shown in Fig. 17(c).

[0057] For this structure, the parameters (Table 1) used in Fig. 15 were fixed, and the optical loss calculation results using LN_h and LN_L as parameters are shown in Fig. 18. When the upper limit of optical loss is 0.5 dB, LN_h<0.17 µm or LN_L<1.2 µm. Furthermore, when the upper limit of optical loss is 1.0 dB, LN_h<0.21 µm or LN_L<2.0 µm. In other words, it is preferable that the length of the SiN waveguide in the light wave propagation direction in the convex portion 23 is 2 µm or less.

[0058] The above describes the bonding of the SiN waveguide and the TFLN at the chip level. The manufacturing process used in the present invention can also be realized at the wafer level. The numbers of each step below are related to the numbers of the steps in the manufacturing process in Figures 8 and 9. (STEP 1) A substrate containing a SiN waveguide is prepared. (STEP2-1) As shown in FIG. 19(a), a TFLN2 having a release layer 24 is prepared. (STEP2-2) As shown in Fig. 19(b), through holes are formed at the edges of the TFLN. The Si deep trench processing used in MEMS or laser processing is suitable. (STEP2-3) As shown in FIG. 19(c), unnecessary portions of the holding member 25 supporting the TFLN 2 are removed by a suitable method (dry etching, laser processing, mechanical processing such as a dicer, etc.).

[0059] (STEP 3) As shown in Fig. 19(d), after cleaning the above wafer, it is bonded to a wafer with a SiN waveguide. At this time, the edge of the TFLN is adjusted so that it comes to the wide part of the SiN waveguide (see reference numeral 100 in Fig. 6). (STEP4) As shown in FIG. 19(e), the release layer 24 is side-etched through the through-hole. (STEP5) The processing suppression film PR2 is formed (see FIG. 9(d)). (STEP 6) The release layer 24 is completely peeled off (see FIG. 9(e)). (STEP7,8) A film of the difficult-to-process material PR3 is formed, and the rib-type optical waveguide 20, the protrusions 23, and the like are processed (see FIGS. 9(f) and (g)). Then, electrodes are formed. It will be understood that the above-described manufacturing process makes it possible to manufacture the optical waveguide element of the present invention even at the wafer level.

[0060] Next, a method will be described in which, when the optical waveguide element of the present invention is used as an optical modulator, TFLN is used only in the action portion of the Mach-Zehnder type optical waveguide (the portion where the electric field of the electrodes acts on the optical waveguide). (STEP 1) As shown in FIG. 20(a), a SiN waveguide 10 is prepared. (STEP2,3) 20(b), a substrate with TFLN2 (including a holding member and release layer; referred to as "substrate with TFLN") is bonded to a substrate (including low refractive index layer 11) on which a SiN waveguide 10 is formed. At this time, the length of a wide portion 100 of the SiN waveguide becomes the manufacturing tolerance for "dimensions of substrate with TFLN" and "bonding accuracy." (STEP4,5,6) The release layer is side-etched, and a processing inhibiting film PR2 is formed as shown in Fig. 20(c), The release layer is removed, and the holding member is peeled off.

[0061] (STEP7) As shown in Fig. 20(d), the resist (difficult-to-process material) PR3 is patterned. The patterning is performed to align the portion to be protected on the substrate on which the rib-type optical waveguide is to be formed and the SiN waveguide is to be formed. (STEP8) As shown in Fig. 20(e), the TFLN is processed and the processing inhibition film PR2 and the difficult-to-process material PR3 are removed. Although the state where the recessed parts RC are formed above and below the MZ structure is shown, these parts do not have a waveguide, so there is no problem even if they are processed. Thereafter, electrodes and the like are formed.

[0062] Next, an example of application of the optical waveguide element of the present invention to an optical modulation device or an optical transmission device will be described. In the following, an example of a high bandwidth coherent driver modulator (HB-CDM) will be described, but the present invention is not limited to this, and can also be applied to an optical phase modulator, an optical modulator with a polarization synthesis function, an optical waveguide element integrating more or less Mach-Zehnder type optical waveguides, a junction device with an optical waveguide element made of other materials such as silicon, a device for sensor use, and the like.

[0063] As shown in FIG. 21, the optical waveguide element has an optical waveguide composed of a SiN waveguide 10 or a rib-type optical waveguide 20, and a control electrode (not shown) such as a modulation electrode that modulates the light wave propagating through the rib-type optical waveguide 20, and is housed in a housing CA. Furthermore, an optical modulation device MD can be configured by providing an optical fiber (F) that inputs and outputs light waves to the optical waveguide. In FIG. 21, the optical fiber F is optically coupled to the SiN waveguide 10 in the optical waveguide element using an optical block with an optical lens, a lens barrel, a polarization multiplexing unit OB, or the like. Not limited to this, the optical fiber may be introduced into the housing through a through hole penetrating the side wall of the housing, and the optical fiber may be directly bonded to an optical component or a substrate, or an optical fiber having a lens function at the end of the optical fiber may be optically coupled to the optical waveguide in the optical waveguide element. In addition, in order to stably bond the optical fiber and the optical block, a reinforcing member (not shown) may be overlapped and arranged along the end face of the substrate (including the low refractive index layer 11) including the SiN waveguide. In the polarization combining unit OB, the waveguide structure described in Non-Patent Document 3 is applied to the SiN waveguide, so that the spatial system can be replaced with a waveguide, thereby reducing the manufacturing and material costs.

[0064] An optical transmitter OTA can be configured by connecting an electronic circuit (digital signal processor DSP) that outputs a modulating signal So that causes the optical modulation device MD to perform a modulation operation to the optical modulation device MD. In order to obtain a modulating signal S to be applied to the optical waveguide element, it is necessary to amplify the modulating signal So output from the digital signal processor DSP. For this reason, in FIG. 21, a driver circuit DRV is used to amplify the modulating signal. The driver circuit DRV and the digital signal processor DSP can be placed outside the housing CA, but they can also be placed inside the housing CA. In particular, by placing the driver circuit DRV inside the housing, it is possible to further reduce the propagation loss of the modulating signal from the driver circuit.

[0065] The input light L1 to the optical modulation device MD may be supplied from outside the optical transmission device OTA, but it is also possible to use a semiconductor laser (LD) as a light source as shown in Fig. 21. The output light L2 modulated by the optical modulation device MD is output to the outside via an optical fiber F. [Industrial Applicability]

[0066] As described above, according to the present invention, it is possible to provide an optical waveguide element that can perform optical transfer between two waveguides with low loss even when the difference in refractive index between the two waveguides is small, such as a SiN waveguide or a TFLN rib-type optical waveguide. Furthermore, it is possible to provide an optical modulation device and an optical transmission device using the optical waveguide element. [Explanation of symbols]

[0067] 1 First board 10 First optical waveguide (SiN) 11 Low refractive index layer 12 Holding board 2 Second board (TFLN) 20 Second optical waveguide (rib-type optical waveguide) 23 Convex 24 Release Tier 25 Retaining member F Optical Fiber LD light source CA Cabinet MD Optical Modulation Device DRV Driver circuit DSP Digital Signal Processor OTA Optical Transmitter

Claims

1. a first substrate having a first optical waveguide and a low refractive index layer covering the first optical waveguide and made of a material having a refractive index lower than that of the first optical waveguide; a second substrate bonded to the first substrate and made of a material having an electro-optic effect, the second substrate having a rib-type optical waveguide as a second optical waveguide; In the optical waveguide element, the first optical waveguide and the second optical waveguide have a portion optically coupled to each other, an optical waveguide element, characterized in that, when the optical waveguide element is viewed in a plane, a convex portion is formed in the second substrate at a boundary portion where the first optical waveguide and the second substrate overlap, and a thickness of the second substrate at the convex portion is configured to be thinner than a thickness of the second substrate at the second optical waveguide.

2. 2. The optical waveguide element according to claim 1, wherein the length of said first optical waveguide in the light wave propagation direction at said convex portion is 2 [mu]m or less.

3. 2. The optical waveguide element according to claim 1, wherein a width of the first optical waveguide at the boundary portion is set to be wider than a width of the first optical waveguide located before or after the boundary portion.

4. 2. The optical waveguide element according to claim 1, wherein a difference in refractive index between said first optical waveguide and said second optical waveguide is 0.8 or less.

5. 5. The optical waveguide element according to claim 4, wherein the first optical waveguide is made of SiN, and the second substrate is made of lithium niobate.

6. The optical waveguide element according to any one of claims 1 to 5 is housed in a housing, An optical modulation device comprising an optical fiber for inputting or outputting a light wave to or from the first optical waveguide.

7. 7. The optical modulation device according to claim 6, the second substrate has a modulation electrode for modulating a light wave propagating through the second optical waveguide; An optical modulation device comprising: an electronic circuit disposed inside the housing for amplifying a modulation signal input to the modulation electrode.

8. An optical modulation device according to claim 7; a light source for inputting a light wave to the optical modulation device; and an electronic circuit for outputting a modulated signal to the optical modulation device.

Citation Information

Cited By

  • Optical waveguide element, optical modulation device and light transmitter using the same, and manufacturing method of optical waveguide element

    JP2025099620A

  • Optical device, and method for manufacturing optical device

    WO2026069627A1