Aqueous coating material

By integrating a tertiary amine compound and dicarboxylic acid into the aqueous epoxy resin and polyamine compound formulation, the coating material achieves extended pot life and rapid curing, addressing the limitations of conventional materials.

JP2024142681APending Publication Date: 2024-10-11BEKKU KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023054928
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional aqueous epoxy coating materials face issues with short pot life, which impede painting workability due to the rapid reaction between epoxy and amine components.

Method used

Incorporating a tertiary amine compound and dicarboxylic acid into an aqueous epoxy resin and polyamine compound formulation to enhance both pot life and quick curing properties.

Benefits of technology

The resulting coating material exhibits excellent pot life and rapid hardening capabilities, suitable for flooring applications, with improved workability and curing even at low temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142681000001
    Figure 2024142681000001
  • Figure 2024142681000002
    Figure 2024142681000002
Patent Text Reader

Abstract

To provide an aqueous coating material which is excellent in both a pot life and quick curability.SOLUTION: An aqueous coating material contains an epoxy resin and a polyamine compound, and further contains a tertiary amine compound and a dicarboxylic acid.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel water-based coating material. [Background technology]

[0002] 2. Description of the Related Art Conventionally, floors and rooftops of buildings such as houses, factories, warehouses, and sports facilities, as well as outdoor floors such as roads, sidewalks, pedestrian bridges, platforms, parks, plazas, and gardens, have been painted with a coating material to impart beauty and the like. In general, in order to ensure the strength of the coating film, reactive curing coating materials such as epoxy paints are used to paint such floor surfaces. Traditionally, solvent-based coating materials have been the norm, but in recent years, there has been a shift from solvent-based to water-based coating materials in order to reduce health hazards, improve safety, and reduce air pollution.

[0003] For example, as a water-based epoxy coating material, Patent Document 1 describes a pavement decorative material composition consisting of aggregate, a self-emulsifying room temperature curing epoxy resin, and a hydrophilic polyamine. When a pavement decorative material composition such as that described in Patent Document 1 is applied, the initial performance properties can be maintained due to the epoxy-amine reaction (described in paragraph 0018).

[0004] [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 8-48856 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the paving decorative material composition as described in Patent Document 1 is applied by mixing epoxy and amine, and it is necessary to apply it within the pot life (described in paragraph 0019), but the pot life is not fully considered. That is, in Patent Document 1, the pot life when epoxy and amine are mixed may be short, which may cause problems in coating workability. [Means for solving the problem]

[0007] As a result of intensive research to solve such problems, the present inventors have found that an aqueous coating material containing a tertiary amine compound and a dicarboxylic acid in addition to an aqueous epoxy resin and a polyamine compound is excellent in both pot life and rapid curing property, and have completed the present invention.

[0008] That is, the present invention has the following features. 1. An aqueous coating material comprising an aqueous epoxy resin and a polyamine compound, the polyamine compound is a polyamine compound containing a primary amine and / or a secondary amine, The aqueous coating material further comprises a tertiary amine compound (excluding the polyamine compound) and a dicarboxylic acid. 2. A two-liquid reactive curing type water-based coating material containing a base agent containing an aqueous epoxy resin and a curing agent containing a polyamine compound, the polyamine compound is a polyamine compound containing a primary amine and / or a secondary amine, The aqueous coating material further comprises a tertiary amine compound (excluding the polyamine compound) and a dicarboxylic acid. 3. The aqueous coating material according to 1 or 2, wherein the tertiary amine compound is an aromatic tertiary amine compound. 4. The aqueous coating material according to 1 or 2, wherein the dicarboxylic acid is a linear dicarboxylic acid. Effect of the Invention

[0009] The aqueous coating material of the present invention is excellent in both pot life and rapid curing property, and is suitable as an aqueous coating material for floors. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described in detail.

[0011] The aqueous coating material of the present invention is an aqueous coating material containing an epoxy resin and a polyamine compound, and further containing a tertiary amine compound and a dicarboxylic acid. According to the present invention, by containing both a tertiary amine compound and a dicarboxylic acid, it is possible to obtain an aqueous coating material that is excellent in both pot life and rapid curing properties.

[0012] The aqueous epoxy resin of the present invention may be, for example, bisphenol A type epoxy resin, novolac type epoxy resin, bisphenol F type epoxy resin, brominated epoxy resin, cyclic aliphatic epoxy resin, or modified with polyester resin, phenol resin, melamine resin, or the like. Of these, water-soluble type, water-dispersed type, liquid, solid, or the like may be used. In the present invention, water-dispersed epoxy resin is particularly preferably used. By using water-dispersed epoxy resin, an aqueous coating material having both excellent pot life and fast curing property can be obtained.

[0013] The aqueous epoxy resin of the present invention preferably contains an aqueous epoxy resin having an epoxy equivalent of 250 g / eq or more and 1000 g / eq or less (preferably 300 g / eq or more and 800 g / eq or less, more preferably 350 g / eq or more and 700 g / eq or less). By containing such an aqueous epoxy resin, it is possible to achieve both a good pot life and good initial curing properties. The aqueous epoxy resin of the present invention further preferably contains an aqueous epoxy resin having an epoxy equivalent of less than 250 g / eq (preferably 100 g / eq or more and 230 g / eq or less) in a proportion of less than 50% by weight (preferably 10% by weight or more and 40% by weight or less) relative to the total amount (solid content) of the base resin. In particular, when the aqueous epoxy resin having an epoxy equivalent of 250 g / eq or more and 1000 g / eq or less is preferably 50% by weight or more and 100% by weight or less (more preferably 60% by weight or more and 90% by weight or less) of the total amount (solid content) of the aqueous epoxy resin, and the aqueous epoxy resin having an epoxy equivalent of less than 250 g / eq is preferably 0% by weight or more and less than 50% by weight (more preferably 10% by weight or more and 40% by weight or less) of the total amount (solid content) of the aqueous epoxy resin, an aqueous coating material having particularly excellent pot life and rapid curing properties can be obtained. In addition, an aqueous epoxy resin having an epoxy equivalent of 250 g / eq or more and 1000 g / eq or less is preferably a solid aqueous epoxy resin, and an aqueous epoxy resin having an epoxy equivalent of less than 250 g / eq is preferably a liquid aqueous epoxy resin.

[0014] In the present invention, the molecular weight of the aqueous epoxy resin is preferably 300 or more and 2000 or less (preferably 400 or more and 1800 or less, and more preferably 500 or more and 1500 or less). By being in such a range, it is possible to obtain an aqueous coating material that is particularly excellent in both pot life and rapid curing property. In particular, aqueous epoxy resins having an epoxy equivalent of 250 g / eq or more and 1000 g / eq or less preferably have a molecular weight of 500 or more and 2000 or less (preferably 700 or more and 1800 or less, more preferably 800 or more and 1500 or less). Also, aqueous epoxy resins having an epoxy equivalent of less than 250 g / eq preferably have a molecular weight of 300 or more and 1500 or less (preferably 400 or more and 1000 or less).

[0015] Regarding the amines of the present invention, the primary amine compound is a compound having the structure of the following structural formula (1), the secondary amine compound is a compound having the structure of the following structural formula (2), and the polyamine compound of the present invention is a compound having the structure of the following structural formula (1) and / or the following structural formula (2). The tertiary amine compound is a compound having the structure of the following structural formula (3): The tertiary amine compound of the present invention is a compound having the structure of the following structural formula (3). (1) R-NH2, (2) R-NH-R, (3) RN(-R)2 (R is an organic segment having one or more carbon atoms and may be the same or different.)

[0016] The polyamine compound of the present invention is a compound having the above structural formula (1) and / or the above structural formula (2), and examples thereof include aliphatic polyamines, alicyclic polyamines, aromatic polyamines, heterocyclic polyamines, and modified polyamine compounds obtained by modifying the amino groups of these polyamine compounds. In addition, known methods can be used to modify the polyamine compound, such as amidation of amino groups, Mannich reaction of amino groups with carbonyl compounds, addition reaction of amino groups with epoxy groups, and addition reaction of amino groups with styrene, and among these, water-soluble and water-dispersed polyamine compounds can be used. In the present invention, water-soluble polyamine compounds are particularly preferably used. By using a water-soluble polyamine compound, it is possible to obtain an aqueous coating material that is particularly excellent in both pot life and rapid curing. Examples of aliphatic polyamines include methylene diamine, ethylene diamine, propylene diamine, butenediamine, diethylene triamine, dipropylene triamine, triethylene tetramine, tripropylene tetramine, tetraethylene pentamine, tetrapropylene pentamine, pentaethylene hexamine, trimethyl hexamethylene diamine, tetra(aminomethyl)methane, dimethylaminopropylamine, diethylaminopropylamine, dibutylaminopropylamine, aminoethyl propylene diamine, aminopropyl ethylene diamine, methylimino bis propylamine, polyoxypropylene diamine, and polyoxypropylene triamine. Examples of alicyclic polyamines include N-aminoethylpiperazine, bis(4-amino-3-methylcyclohexyl)methane, menthene diamine, isophorone diamine, 4,4'-diaminodicyclohexylmethane, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro[5.5]undecane (spiroacetal diamine), norbornane diamine, tricyclodecane diamine, and 1,3-bisaminomethylcyclohexane; Examples of aromatic polyamines include benzylamine, N-aminoethylpiperazine, xylylenediamine, N-benzylethylenediamine, phenylenediamine, diaminodiphenylmethane, and diaminodiphenyl ether. Among these, one or more kinds can be used.

[0017] The polyamine compound of the present invention preferably has an active hydrogen equivalent of 50 g / eq or more and 1000 g / eq or less (more preferably 80 g / eq or more and 800 g / eq or less, and even more preferably 100 g / eq or more and 600 g / eq or less).By using such an aqueous polyamine compound, an aqueous coating material having both excellent pot life and rapid curing properties can be obtained, and further, an aqueous coating material having excellent adhesion and gloss of the formed coating film can be obtained.

[0018] The polyamine compound preferably has a molecular weight of from 200 to 4000 (more preferably from 400 to 3000). When the molecular weight is within this range, an aqueous coating material having both excellent pot life and rapid curing properties can be obtained.

[0019] The tertiary amine compound of the present invention is a compound represented by the above structural formula (3), and examples thereof include trimethylamine, ethyldimethylamine, propyldimethylamine, N,N'-dimethylpiperazine, pyridine, picoline, benzyldimethylamine, benzyldiethylamine, tribenzylamine, N,N,N',N'-tetramethylethylenediamine, dimethylaminocyclohexane, 1,8-diazabiscyclo(5,4,0)-7-undecene, 2-(dimethylaminomethyl)phenol, 2,4,6-tris(dimethylaminomethyl)phenol, and the like. One or more of these may be used. In the present invention, it is particularly preferable to use one or more selected from 2-(dimethylaminomethyl)phenol and 2,4,6-tris(dimethylaminomethyl)phenol.

[0020] Examples of the dicarboxylic acid of the present invention include aliphatic dicarboxylic acids such as malonic acid, maleic acid, maleic anhydride, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, and dodecanedioic acid; alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid; and aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, orthophthalic acid, phthalic anhydride, terephthalic acid, 2,6-naphthalenedicarboxylic acid, paraphenylenedicarboxylic acid, and trimellitic acid. One or more of these may be used. In the present invention, it is particularly preferable to use an aliphatic dicarboxylic acid. In the present invention, by using such a tertiary amine compound in combination with a dicarboxylic acid, it is possible to obtain an aqueous coating material that is excellent in both pot life and rapid curing properties.

[0021] The mixing amount of the epoxy resin and the polyamine compound is not particularly limited, but it is preferable that the solid content of the polyamine compound is 1 part by weight or more and 100 parts by weight or less (more preferably 2 parts by weight or more and 80 parts by weight or less) per 100 parts by weight of the solid content of the epoxy resin. In addition, the equivalent ratio of the epoxy equivalent of the epoxy resin to the active hydrogen equivalent of the polyamine compound, [active hydrogen equivalent of amine curing agent / epoxy equivalent of epoxy resin], is preferably 0.5 or more and 1.5 or less, more preferably 0.7 or more and 1.4 or less. The amount of the tertiary amine compound mixed is preferably 1.0 to 40 parts by weight (more preferably 3 to 20 parts by weight, and even more preferably 5.0 to 15 parts by weight) per 100 parts by weight of the solid content of the polyamine compound. The amount of dicarboxylic acid mixed is preferably 1.0 to 40 parts by weight (more preferably 3 to 20 parts by weight, and even more preferably 5.0 to 15 parts by weight) per 100 parts by weight of the solid content of the polyamine compound.

[0022] In addition to the above-mentioned components, additives can be added to the present invention as appropriate to the extent that the effects of the present invention are not impaired. Examples of additives that may be included include pigments, aggregates, dispersants, viscosity adjusters, solvents, film-forming aids, plasticizers, antifreeze agents, preservatives, antifungal agents, anti-algae agents, antifoaming agents, leveling agents, pH adjusters, anti-settling agents, anti-sagging agents, matting agents, UV absorbers, drying adjusters, coupling agents, dehydrating agents, light stabilizers, antioxidants, and water. Examples of acid compounds other than the dicarboxylic acids include organic carboxylic acid compounds such as formic acid, acetic acid, propionic acid, butyric acid, hexanoic acid, octylic acid, 2-ethylhexanoic acid, decanoic acid, dodecanoic acid, stearic acid, oleic acid, linoleic acid, palmitic acid, trimellitic acid, and pyrimellitic acid.

[0023] Examples of pigments include inorganic color pigments such as titanium oxide, zinc oxide, carbon black, ferric oxide (red oxide), lead chromate (molybdate orange), yellow lead, yellow iron oxide, ochre, ultramarine, and cobalt green; organic color pigments such as azo, naphthol, pyrazolone, anthraquinone, perylene, quinacridone, disazo, isoindolinone, benzimidazole, phthalocyanine, and quinophthalone; and volume pigments such as heavy calcium carbonate, clay, kaolin, talc, precipitated barium sulfate, barium carbonate, white carbon, and diatomaceous earth.

[0024] Examples of aggregates include volcanic rocks such as granite, andesite, and basalt, sedimentary rocks such as limestone and sandstone, metamorphic rocks such as gneiss, crushed stone, sand, wood, crushed ceramics, crushed glass, glass beads, synthetic resin beads, rubber-like elastic bodies, etc. Aggregates with colored coatings on the surface can also be used.

[0025] The dispersant is not particularly limited as long as it improves the dispersion stability of the epoxy resin and amine compound, and the dispersion stability of the pigment and aggregate, and any known dispersant can be used. In the present invention, a dispersant having an anionic group and / or a nonionic group is preferred, and a dispersant having an anionic group and a nonionic group is more preferred. Specifically, the dispersant has a segment having an anionic group and a segment having a nonionic group. In the present invention, a dispersant made of a graft polymer in which either or both of the segment having an anionic group and the segment having a nonionic group are main chains and either or both of the segment having an anionic group and the segment having a nonionic group are side chains is particularly preferred.

[0026] Examples of thickeners include organic thickeners such as sodium polyacrylate, ammonium polyacrylate, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxylpropoxylethyl cellulose, methyl cellulose, hexaethyl cellulose, polyacrylamide, and polyethylene oxide, and inorganic thickeners such as bentonite. In the present invention, methyl cellulose, hexaethyl cellulose, and the like are particularly preferred.

[0027] Examples of the solvent include alcohols such as methanol, ethanol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, sec-butyl alcohol, t-butyl alcohol, and benzyl alcohol; ethylene glycol, propylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, diethylene glycol dibutyl ether, propyl propylene glycol, propylene glycol monomethyl ether, and propylene glycol monomethyl ether acetone. Examples of suitable organic solvents include glycols such as butyl ether, dipropylene glycol monomethyl ether, butyl propylene glycol, butyl propylene diglycol, phenyl propylene diglycol, hexyl glycol, hexyl diglycol, 2-ethylhexyl glycol, and 2-ethylhexyl diglycol; ketones such as n-methylpyrrolidone, acetone, methyl ethyl ketone, and methyl isobutyl ketone; aromatic hydrocarbons such as toluene and xylene; aliphatic hydrocarbons such as cyclohexane, isoparaffin, cyclohexanone, and mineral spirits; esters such as methyl acetate, ethyl acetate, n-propyl acetate, and isopropyl acetate, and mixtures thereof. In the present invention, diethylene glycol dibutyl ether, hexyl glycol, hexyl diglycol, 2-ethylhexyl glycol, 2-ethylhexyl diglycol, butyl propylene glycol, butyl propylene diglycol, propyl propylene glycol, and the like are preferred because they can further improve film-forming properties, pot life, and curing properties.

[0028] The amount of the solvent to be mixed may be about 50 parts by weight or less (more preferably 0.1 to 40 parts by weight, and even more preferably 0.3 to 30 parts by weight) per 100 parts by weight of the resin solid content of the aqueous epoxy resin. The amount of the dispersant to be mixed may be about 30 parts by weight or less (more preferably 0.1 to 25 parts by weight, and even more preferably 0.3 to 20 parts by weight) per 100 parts by weight of the resin solid content of the aqueous epoxy resin. The amount of the thickener to be mixed may be about 50 parts by weight or less (more preferably 0.1 to 40 parts by weight (even more preferably 0.3 to 30 parts by weight) per 100 parts by weight of the resin solid content of the aqueous epoxy resin.

[0029] The aqueous coating material of the present invention can be used as a one-liquid type aqueous coating material by mixing an aqueous epoxy resin, a polyamine compound, a tertiary amine compound, a dicarboxylic acid and other additives, or can be used as a two-liquid reactive curing type aqueous coating material consisting of a base agent containing an aqueous epoxy resin and a curing agent containing a polyamine compound. When used as a two-liquid reactive curing type aqueous coating material, the tertiary amine compound and the dicarboxylic acid are not particularly limited, but it is preferable to mix a tertiary amine compound and a dicarboxylic acid with the curing agent.

[0030] The aqueous coating material of the present invention is preferably applied to floor surfaces, and may be applied using a coating tool such as a brush or roller. It may also be applied directly on-site, or on a production line in a factory or the like. For example, it may be applied to floors and roofs of buildings such as houses, factories, warehouses, and sports facilities, or outdoor floors such as roads, sidewalks, pedestrian bridges, platforms, parks, squares, and gardens. Specific materials include, for example, hard soil and stone surfaces, concrete, mortar, and asphalt. It may also be used for the purpose of repairing and renovating floor surfaces such as interlocking and porous concrete. The aqueous coating material of the present invention has an excellent pot life and rapid curing properties, and can be cured in about 3 to 24 hours at normal room temperature (about 0°C to 40°C) to a walkable state. It also has excellent recoatability and adhesion, and further has excellent paintability and adhesion for topcoat materials, making it particularly suitable for use as an undercoat material. The present invention is particularly excellent in terms of rapid hardening even at low temperatures (approximately 0° C. to 10° C.), and can harden in approximately 3 to 24 hours to a walkable state. EXAMPLES

[0031] Example 1 The raw materials shown below and the raw material composition shown in Table 1 were uniformly mixed and stirred in a conventional manner to prepare base agent 1 and hardener 1. Furthermore, base agent 1 and hardener 1 were mixed in a ratio of 100:50 (weight ratio) in the combination shown in Table 2 to obtain an aqueous coating material.

[0032] (Pot life evaluation) The pot life of the above aqueous coating material was measured by the following method. The test was carried out based on JIS K5600-2-6:1999 "Pot life". The evaluation is shown below. The results are shown in Table 2. ◎: More than 6 hours ○: 1 hour or more but less than 6 hours △: 20 minutes or more but less than 1 hour ×: Less than 20 minutes

[0033] (Rapid hardening evaluation) Five minutes after mixing the base agent 1 and the hardener 1, this water-based coating material was applied to a slate board (150 mm x 300 mm x 3 mm) with a roller in an amount of 150 g / m under various conditions (condition 1: temperature 5°C, relative humidity 50%, condition 2: temperature 23°C, relative humidity 50%). 2 To obtain a test specimen. After applying the water-based coating material to the above test specimens, the degree of surface hardening was evaluated after 4 hours and 16 hours under various conditions. The evaluation results are shown below. The results are shown in Table 2. ⊚: The coating surface was almost completely hardened and walkable. ◯: The coating surface was almost completely hardened and was almost walkable. Δ: Some tack remained on the coating surface. ×: Tack remained on the coating surface.

[0034] (Topcoat painting evaluation) After applying the water-based coating material to the above test specimens, 4 and 16 hours were allowed to pass under various conditions, and then the topcoat material (epoxy resin-based floor coating material) was applied with a brush in an amount of 150 g / m. 2 The paintability was evaluated. The evaluation results are shown in Table 2. ◎: The topcoat material was not repelled and could be applied evenly. ○: The topcoat material was barely repelled and could be applied evenly. △: Part of the topcoat material was repelled, making it difficult to apply evenly. ×: The topcoat material was repelled, making painting difficult.

[0035] (raw materials) Water-based epoxy resin 1: Water-dispersed solid epoxy resin (self-emulsifying bisphenol A type epoxy resin, solid content 70% by weight, epoxy equivalent 525g / eq) Water-based epoxy resin 2: Water-dispersible liquid epoxy resin (self-emulsifying bisphenol A type epoxy resin, solid content 55% by weight, epoxy equivalent 215g / eq) Additives: Dispersants, defoamers Polyamine compound 1: Water-soluble aliphatic polyamine (solid content 60% by weight, active hydrogen equivalent 135 g / eq) Polyamine compound 2: Water-dispersible aliphatic polyamine (solid content 50% by weight, active hydrogen equivalent 155 g / eq) Tertiary amine: 2,4,6-tris(dimethylaminomethyl)phenol Dicarboxylic acid: Maleic acid

[0036] (Examples 2 to 8, Comparative Examples 1 to 3) Using the raw materials and raw material compositions shown in Table 1 and the combinations shown in Table 2, aqueous coating materials were obtained in the same manner as in Example 1, test specimens were obtained, and tests were carried out in the same manner as in Example 1. The results are shown in Table 2. Example 9 Except for mixing the base agent 1 and the curing agent 2 in a ratio of 100:65 (weight ratio), an aqueous coating material was obtained, a test specimen was obtained, and a test was performed in the same manner as in Example 2. The results are shown in Table 2. Example 10 Except for mixing the base agent 1 and the curing agent 2 in a ratio of 100:35 (weight ratio), an aqueous coating material was obtained, a test specimen was obtained, and a test was performed in the same manner as in Example 2. The results are shown in Table 2.

[0037] [Table 1]

[0038] [Table 2]

Claims

1. An aqueous coating material comprising an aqueous epoxy resin and a polyamine compound, the polyamine compound is a polyamine compound containing a primary amine and / or a secondary amine, The aqueous coating material further comprises a tertiary amine compound (excluding the polyamine compound) and a dicarboxylic acid.

2. A two-liquid reactive curing type aqueous coating material containing a base material containing an aqueous epoxy resin and a curing agent containing a polyamine compound, the polyamine compound is a polyamine compound containing a primary amine and / or a secondary amine, The aqueous coating material further comprises a tertiary amine compound (excluding the polyamine compound) and a dicarboxylic acid.

3. 3. The aqueous coating material according to claim 1, wherein the tertiary amine compound is an aromatic tertiary amine compound.

4. 3. The aqueous coating material according to claim 1, wherein the dicarboxylic acid is a linear dicarboxylic acid.

Citation Information

Patent Citations

  • Water-permeation pavement ornamental composition and application thereof

    JP1996048856A