Laminate, laminate film made of the same, and packaging body using the film

A laminate using hemicellulose and high-saponification polyvinyl alcohol resin addresses the insufficient oxygen barrier and mechanical strength issues of bio-derived materials, providing effective food packaging solutions.

JP2024142793APending Publication Date: 2024-10-11MITSUBISHI CHEM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023055120
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing bio-derived materials for oxygen barriers in food packaging, such as those based on polysaccharides and cellulose, do not provide sufficient oxygen barrier properties and mechanical strength.

Method used

A laminate comprising a layer containing hemicellulose and a polyvinyl alcohol resin with a high degree of saponification, specifically xylan and polyvinyl alcohol with a degree of saponification of 90 mol% or more, is used to enhance oxygen barrier and mechanical properties.

Benefits of technology

The laminate achieves a good balance between oxygen barrier properties and mechanical strength while utilizing biomass materials, suitable for food packaging applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142793000001
    Figure 2024142793000001
  • Figure 2024142793000002
    Figure 2024142793000002
Patent Text Reader

Abstract

To provide a laminate that has a good oxygen barrier property and an excellent mechanical property while also being environmentally friendly and conserving resources.SOLUTION: A laminate comprises a layer (I) containing hemicellulose (A) and a polyvinyl-based alcohol resin (B) having a saponification degree of 90 mol % or more on at least one surface of a base layer (II), wherein the base layer (II) is a resin base material or a paper base material, the hemicellulose (A) is preferably xylan, and an oxygen transmission rate per 1 μm of the layer (I) at 23°C×50%RH measured in accordance with JIS K7126-2 (2006) is more preferably 7.0 cc / m2 day atm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate suitable for use in food packaging and the like, a laminate film made of the same, and a package using the film. [Background technology]

[0002] In packaging applications for food and the like, materials with oxygen barrier properties are used to prevent deterioration of product quality due to oxidation. Conventionally, EVOH (ethylene vinyl alcohol) and PVOH (polyvinyl alcohol) have been used as materials with oxygen barrier properties, but these materials are derived from petroleum, and there is a demand for their replacement with renewable materials.

[0003] As renewable oxygen barrier materials, films based on polysaccharides such as starch and cellulose, and proteins have been investigated. For example, Patent Document 1 describes a resin composition containing modified starch and polyvinyl alcohol. Furthermore, Patent Document 2 describes a gas barrier laminate having a protective layer containing cellulose fibers having a fiber width of 1000 nm or less and having a phosphate group or a substituent derived from a phosphate group. Furthermore, US Pat. No. 5,399,633 describes a dispersion coating comprising colloidal particles of microfibrillated cellulose and polymers. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-105305 A [Patent Document 2] JP 2020-075514 A [Patent Document 3] Special Publication No. 2013-510222 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the techniques disclosed in the above Patent Documents 1 to 3 use bio-derived materials and are therefore environmentally friendly, but have the problem of insufficient oxygen barrier properties. Therefore, the present invention has been made in consideration of the above problems, and provides a laminate using a biomass-derived material, which has good oxygen barrier properties and excellent mechanical properties while being able to solve problems such as environmental friendliness and resource conservation, a laminate film made thereof, and a packaging material using the film. [Means for solving the problem]

[0006] The present invention has the following aspects.

[0007] [1] A laminate having a layer (I) containing hemicellulose (A) and a polyvinyl alcohol-based resin (B) having a saponification degree of 90 mol % or more on at least one surface of a base layer (II).

[0008] [2] The laminate according to [1], wherein the hemicellulose (A) is contained in the layer (I) in an amount of 10% by mass or more and 90% by mass or less.

[0009] [3] The laminate according to [1] or [2], wherein the substrate layer (II) is a resin substrate or a paper substrate.

[0010] [4] The storage modulus of the layer (I) at 100°C and a frequency of 10 Hz measured in accordance with JIS K7244-1 (1998) is 0.20 x 10 9 The laminate according to any one of [1] to [3], wherein the elastic modulus is 1.0 Pa or more.

[0011] [5] The laminate according to any one of [1] to [4], wherein the hemicellulose (A) is xylan.

[0012] [6] The oxygen permeability per 1 μm of the layer (I) at 23°C x 50% RH measured in accordance with JIS K7126-2 (2006) is 7.0 cc / m 2 The laminate according to any one of [1] to [5], wherein the maximum permeability is 100% by mass per day atm or less.

[0013] [7] The laminate according to any one of [1] to [6], wherein the polyvinyl alcohol-based resin (B) has a degree of polymerization of 400 or more.

[0014] [8] A laminate film comprising the laminate according to any one of [1] to [7].

[0015] [9] The laminate film according to [8], wherein the laminate film is for food packaging.

[0016]

[10] A packaging body using the laminated film described in [8] or [9]. Effect of the Invention

[0017] The present invention provides a laminate having at least one layer containing hemicellulose (A) and a specific polyvinyl alcohol resin (B), thereby making it possible to obtain laminates and packages that use biomass materials and have a good balance between oxygen barrier properties and mechanical properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] An embodiment of the present invention will be described below, however, the present invention is not limited to this embodiment.

[0019] A laminate according to one embodiment of the present invention (hereinafter also referred to as the present laminate) has a layer (I) containing hemicellulose (A) and a polyvinyl alcohol-based resin (B) having a degree of saponification of 90 mol% or more on at least one surface of a base layer (II).

[0020] <This laminate> The laminate of the present invention comprises a layer (I) on at least one surface of a substrate layer (II), and may further comprise other layers such as a seal layer, etc. A preferred laminate structure will be described later.

[0021] <Layer (I)> The layer (I) of the present laminate contains hemicellulose (A) and a polyvinyl alcohol-based resin (B) having a degree of saponification of 90 mol % or more.

[0022] (Hemicellulose (A)) The hemicellulose (A) in the present laminate refers to polysaccharides that constitute the cell walls of plant cells, other than cellulose and lignin. Specific examples of the hemicellulose (A) include xylan, arabinoxylan, arabinan, mannan, galactan, xyloglucan, glucomannan, etc. Among these, xylan is preferred because of its relatively small molecular weight and low viscosity.

[0023] Xylan is a plant-derived (bio-derived) polymeric compound present in plants such as trees, grains, grasses, and medicinal herbs, and is a heterosaccharide with various side chains bound to the main chain of β(1,4)-linked xylose. The types of substituents bound to the side chains are not particularly limited, but examples include glucuronic acid, galactose, mannose, glucose, arabinose, and fucose.

[0024] Xylans are classified into heteroxylans and homoxylans, where homoxylans have a backbone of xylose residues and glucuronic acid or 4-O-methylglucuronic acid substituents, and heteroxylans have a backbone of xylose residues. An advantage of heteroxylans is that they are highly crystallizable compared to homoxylans, and the crystalline structure can reduce both gas permeability and moisture sensitivity.

[0025] From the viewpoint of improving the film-forming properties of the layer (I), the molecular weight of xylan is preferably 100 or more and 100,000 or less, more preferably 300 or more and 50,000 or less, and even more preferably 30,000 or more and 50,000 or less. The molecular weight of xylan can be measured by gel permeation chromatography (GPC).

[0026] Specifically, the hemicellulose (A) that can be used includes the product name "Xylan GX-1" (manufactured by PS Biotech Co., Ltd.: xylan content (active ingredient) of 85% by mass with a mass average molecular weight of 45,000). The content (active ingredient) of the hemicellulose (A) can be measured by ultra-performance liquid chromatography (UPLC) or the like after acid hydrolysis and fluorescent labeling. It is preferable to use one with a large content (active ingredient), but there is no particular limitation as long as the required hemicellulose (A) can be obtained. Usually, it is preferable to use one with a content of 50 mass% or more. Since it is derived from a plant, it may contain ingredients other than hemicellulose (A), such as lipids and proteins, within a range that does not impair the effects of the present invention.

[0027] The hemicellulose (A) is preferably 10% by mass or more and 90% by mass or less in the layer (I). When it is within the above range, the oxygen barrier property is not significantly reduced, and the heat resistance, for example, dimensional stability in a high-temperature environment, is also good. This is thought to be because the hydroxyl groups in the hemicellulose (A) make it easier to form a packing structure through hydrogen bonds, which tends to improve the oxygen barrier property. From this viewpoint, the upper limit is more preferably 85% by mass or less, even more preferably 80% by mass or less, and particularly preferably 75% by mass or less. The lower limit is more preferably 10% by mass or more, even more preferably 20% by mass or more, and particularly preferably 30% by mass or more.

[0028] (Polyvinyl alcohol resin (B)) The polyvinyl alcohol-based resin (B) of the present laminate includes polyvinyl alcohol resins and modified polyvinyl alcohol resins obtained by modifying polyvinyl alcohol resins, and has a degree of saponification of 90 mol % or more.

[0029] The polyvinyl alcohol-based resin (B) can be obtained, for example, by saponifying the acetate group of polyvinyl acetate, which is a polymer of vinyl acetate. The polyvinyl alcohol-based resin (B) may be partially modified, for example, butenediol-modified, silanol-modified, acetoacetyl-modified, etc.

[0030] The polyvinyl alcohol resin (B) has a degree of saponification of 90 mol % or more. The degree of saponification is the molar fraction of hydroxyl groups relative to the total of hydroxyl groups and ester groups in polyvinyl alcohol, and can be measured in accordance with JIS K6726 (1994). When the degree of saponification is within the above range, the crystallinity of polyvinyl alcohol increases, film strength improves, and oxygen barrier properties tend to improve. This is believed to be because the number of hydroxyl groups increases, making it easier to form a packing structure due to hydrogen bonds. From this viewpoint, the range of the saponification degree is more preferably 92 mol % or more, further preferably 95 mol % or more, and particularly preferably 98 mol % or more.

[0031] The degree of polymerization of the polyvinyl alcohol-based resin (B) is preferably not less than 400. When the degree of polymerization is within the above range, the strength of the layer (I) is improved, and the storage modulus, which will be described later, can be easily adjusted to a preferred range. From this viewpoint, the degree of polymerization is more preferably 450 or more, further preferably 500 or more, particularly preferably 600 or more, and most preferably 1,000 or more. The degree of polymerization is the number of repeating units when the repeating unit of a hydroxyl group and an ester group in polyvinyl alcohol is regarded as one unit.

[0032] Specific examples of the polyvinyl alcohol resin (B) that can be used include the product name "GOHSENOL NH-17Q" (manufactured by Mitsubishi Chemical Corporation: PVA with a degree of polymerization of 1700 and a degree of saponification of 99 mol%) and the product name "GOHSENOL NL-05" (manufactured by Mitsubishi Chemical Corporation: PVA with a degree of polymerization of 500 and a degree of saponification of 99 mol%).

[0033] The polyvinyl alcohol-based resin (B) is preferably contained in the layer (I) in an amount of 10% by mass or more and 90% by mass or less. When the amount is within the above range, the oxygen barrier property becomes sufficient. From this viewpoint, the lower limit is more preferably 15% by mass or more, even more preferably 20% by mass or more, and particularly preferably 25% by mass or more. The upper limit is more preferably 85% by mass or less, even more preferably 80% by mass or less, and particularly preferably 75% by mass or less.

[0034] (Other components of layer (I)) In addition to the hemicellulose (A) and the polyvinyl alcohol resin (B), the layer (I) may contain thermoplastic resins such as polyolefin resins, polyamide resins, polyester resins, and polystyrene resins, or may contain two or more types of resin components. Among these, polyolefin resins and polyamide resins are preferred.

[0035] Examples of polyolefin resins include low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), ethylene-vinyl acetate copolymer (EVA), ethylene-acrylic acid copolymer (EAA), ethylene-ethyl acrylate copolymer (EEA), ethylene-methacrylic acid copolymer (EMAA), ethylene-methyl methacrylate copolymer (EMMA), ethylene-methyl acrylate copolymer (EMA), ionomer resins, acid-modified polyolefin resins, and the like. When other resin components are contained, the smaller the content of the other resin components in Layer (I), the better; usually, the content is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less.

[0036] Layer (I) may contain "components other than the resin component" within the range that does not impair the effects of the present invention. Examples of the "other components other than the resin component" include, but are not limited to, antistatic agents, heat stabilizers, antifogging agents, antiblocking agents, lubricants, colorants, etc.

[0037] (Method of forming layer (I)) Layer (I) of the present laminate may be provided on at least one side of the base layer (II), and is not particularly limited, but is preferably formed by a method (coating) in which a coating liquid containing the hemicellulose (A) and the polyvinyl alcohol-based resin (B) is applied to the base layer (II).

[0038] The coating liquid is a mixture of the hemicellulose (A) and the polyvinyl alcohol-based resin (B) in a solvent such as water, and is preferably blended into the coating liquid in accordance with the blending ratio of the hemicellulose (A) and the polyvinyl alcohol-based resin (B) in the layer (I). For example, the blending ratio of the hemicellulose (A) and the polyvinyl alcohol-based resin (B) may be 90:10 to 10:90.

[0039] The coating method is not particularly limited, but examples thereof include a bar coater method, a comma coat method, a gravure coat method, a reverse coat method, a knife coat method, a dip coat method, a spray coat method, an air knife coat method, a spin coat method, a roll coat method, a print method, a dip method, a slide coat method, a curtain coat method, a die coat method, a casting method, and an extrusion coat method. Other than the coating method, examples of the method include a hydrous extrusion method, a sandwich lamination method, and an extrusion lamination method such as coextrusion.

[0040] The thickness of the layer (I) of the present laminate is not particularly limited, and may be appropriately set in consideration of the barrier properties and other layers such as the base layer (II). For example, the upper limit is 500 μm or less, and preferably 250 μm or less. The lower limit is also not particularly limited, but is preferably 0.5 μm or more, and preferably 1 μm or more, in consideration of productivity and the like.

[0041] (Storage modulus at 100℃) The layer (I) of the laminate has a storage modulus of 0.20×10 at 100° C. and a measurement frequency of 10 Hz, as measured in accordance with JIS K7244-1 (1998). 9 It is preferable that the viscosity is equal to or higher than Pa. If the viscosity is within this range, the shape of the film formed can be easily maintained in a high temperature environment (100° C.), which is preferable from the viewpoint of heat resistance. From this viewpoint, it is more preferable to use a ratio of 0.25×10 9 Pa or more, more preferably 0.30×10 9 Pa or more, and particularly preferably 0.40×10 9 The upper limit is not particularly limited, but is preferably 2.0×10 9 Pa or less is preferred.

[0042] (Storage modulus at 25℃) The layer (I) of the laminate has a storage modulus of 1.0×10 at 25° C. and a measurement frequency of 10 Hz, as measured in accordance with JIS K7244-1 (1998). 9 It is preferable that the viscosity is equal to or higher than 1 Pa. If the viscosity is within this range, the film can be easily handled in a room temperature environment (25° C.), which is preferable. From this viewpoint, it is more preferable that the concentration is 1.3×10 9 Pa or more, more preferably 1.5×10 9 Pa or more, particularly preferably 1.6×10 9 The upper limit is not particularly limited, but is preferably 8.0×10 9 Pa or less is preferred.

[0043] (Storage modulus at 150℃) The layer (I) of the laminate has a storage modulus of 0.1×10 at 150°C and a measurement frequency of 10 Hz, measured in accordance with JIS K7244-1 (1998). 9 It is preferable that the viscosity is equal to or higher than Pa. If the viscosity is within this range, the shape of the film formed can be easily maintained even when the film is subjected to retort sterilization treatment or the like (for example, at 100° C. or higher), which is preferable from the viewpoint of heat resistance. From this viewpoint, it is more preferable to use a ratio of 0.15×10 9 Pa or more, more preferably 0.20×10 9 Pa or more, particularly preferably 0.25×10 9 The upper limit is not particularly limited, but is preferably 2.0×10 9 Pa or less is preferred.

[0044] (Oxygen permeability) The layer (I) of the laminate has an oxygen permeability of 7.0 cc / m per 1 μm thickness at 23°C x 50% RH, measured in accordance with JIS K7126-2 (2006). 2 It is preferable that the temperature be less than 100°C / day atm. When the oxygen barrier property is within this range, it becomes sufficient for practical use. From this viewpoint, 5.0 cc / m is more preferable. 2 ·day·atm or less, more preferably 3.5cc / m 2 ·day·atm or less, particularly preferably 3.0cc / m 2 ·day·atm or less. The lower limit is not particularly limited, but the lower the better, and is preferably 0.10 cc / m 2 ·day·atm or higher is preferable.

[0045] (Biomass ratio) The biomass ratio of layer (I) of the present laminate is preferably 1% or more, more preferably 3% or more, further preferably 15% or more, and particularly preferably 30% or more, and the higher the ratio, the better. The higher the ratio, the more the environmental load is reduced, and the more environmentally friendly the packaging can be.

[0046] <Base material layer (II)> The substrate layer (II) of the present laminate can be in the form of, for example, a film, sheet, plate, tube, etc., and is preferably a resin substrate or a paper substrate.

[0047] (Resin substrate) The resin substrate is not particularly limited as long as it is made of various synthetic resin materials that can be formed into a layer such as a film, sheet, plate, tube, etc. The resin substrate may be made of one layer, or may be a laminate of two or more layers.

[0048] As the synthetic resin material, it is preferable to use a thermoplastic resin from the viewpoint of ease of handling, such as moldability and secondary processability. Examples of the thermoplastic resin include polyolefin resins such as polyethylene and polypropylene; polyester resins such as polyethylene terephthalate, polyethylene isophthalate, polyethylene naphthalate, and polybutylene terephthalate; polylactic acid; polyurethane; polyvinyl acetate; polyacrylonitrile; polyvinyl chloride; and polycarbonate resins.

[0049] The resin substrate is preferably formed from a resin film made of one or more kinds selected from the thermoplastic resins. The resin film may be a porous film that has been subjected to a porosity treatment such as chemical foaming, physical foaming, or stretching to make the resin porous, or a stretched film that has been subjected to a uniaxial or biaxial stretching treatment.

[0050] Additives may be added to the resin substrate as necessary, for example, ultraviolet absorbers for imparting weather resistance, particles may be blended for the main purpose of imparting lubricity and preventing scratches during each process, and conventionally known antioxidants, antistatic agents, heat stabilizers, lubricants, dyes, pigments, etc. may be added as necessary. The surface of the resin substrate on which the layer (I) is to be formed may be subjected to a surface treatment such as a corona treatment, a plasma treatment, or a coating treatment for adjusting wettability.

[0051] The resin substrate can be produced by molding into a layer such as a film, sheet, plate, or tube by using a known method such as an inflation method or an extrusion method.

[0052] The resin substrate may be a laminated film, in which case a pre-prepared film may be produced using a thermoplastic resin composition forming each layer by the above-mentioned known method, or by a lamination method, etc. In particular, it is preferable to use a co-extrusion method, since the film-forming process is the same even when the number of layers of the film is large, and thickness control is relatively easy.

[0053] The thickness of the resin substrate is not particularly limited, but is preferably from 5 to 600 μm. When the thickness is within this range, the handleability can be improved. From this viewpoint, the thickness is more preferably from 10 to 500 μm, and further preferably from 15 to 450 μm.

[0054] (Paper base material) Examples of the paper base material include chemical pulps such as bleached hardwood kraft pulp (LBKP), bleached softwood kraft pulp (NBKP), unbleached hardwood kraft pulp (LUKP), unbleached softwood pulp (NUKP), sulfite pulp, and other such pulps, mechanical pulps such as stone grind pulp and thermomechanical pulp, wood fibers such as deinked pulp and waste paper pulp, and non-wood fibers obtained from kenaf, bamboo, hemp, and the like, which can be used in appropriate combinations. Among these, it is preferable to use chemical pulp or mechanical pulp of wood fiber, and it is more preferable to use chemical pulp, among which chemical pulp, for reasons such as the fact that foreign matter is unlikely to be mixed into the base paper, that discoloration is unlikely to occur over time when paper containers after use are recycled as waste paper raw materials, that the surface texture during printing is good due to the high whiteness, and that the value of the paper is particularly high when the paper is used as a packaging material.

[0055] The method for producing the paper base material (papermaking) is not particularly limited, and the paper base material can be produced by acidic papermaking, neutral papermaking, or alkaline papermaking using a known Fourdrinier former, on-top hybrid former, gap former machine, etc. The paper base material may be one layer, or may be composed of two or more layers. Furthermore, the surface of the paper substrate can be treated with various chemicals. Examples of chemicals that can be used include oxidized starch, hydroxyethyl etherified starch, enzyme-modified starch, polyacrylamide, polyvinyl alcohol, surface sizing agents, water-resistant agents, water retention agents, thickeners, and lubricants, and these can be used alone or in combination of two or more. Furthermore, these various chemicals can be used in combination with pigments. Examples of pigments include inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, and satin white, and organic pigments such as solid, hollow, or core-shell types can be used alone or in combination of two or more. Examples of the paper base material obtained in this manner include various known types of paper, such as fine paper, medium quality paper, coated paper, one-sided glossy paper, kraft paper, one-sided glossy kraft paper, bleached kraft paper, glassine paper, paperboard, white paperboard, and liner.

[0056] The basis weight of the paper base material is 25 g / m 2 More than 400g / m 2 Within this range, the material can be suitably used for packaging applications such as packaging materials for food, containers, cups, etc. From this perspective, 30g / m 2 More than 350g / m 2 More preferably, it is 30 g / m or less. 2 More than 300g / m 2 It is even more preferable that:

[0057] (Layer structure of the laminate) The laminate may have a two-layer structure of layer (I) and base layer (II), or may have a three-layer structure with other layers laminated therein. For example, the other layer preferably has a sealing layer. When the laminate has a sealing layer, it is preferable that the sealing layer is provided on at least one of the front and back sides. By providing the sealing layer in the laminate, the laminate can be heat-sealed with other films or laminates to form a package. Examples of layers other than the sealing layer include a gas barrier layer and an adhesive layer. In the present laminate, there are no limitations on the number of layers, the order of layers, or the type and number of layers other than the layer (I) and the base layer (II), and the layer (I) may be configured by laminating a plurality of layers. More specific examples of the laminate structure include a two-layer structure of Layer (I) / Layer (II); a three-layer structure such as Layer (I) / Layer (II) / Layer (I), Layer (I) / Layer (II) / Sealing layer, or Layer (II) / Layer (I) / Sealing layer; and a four-layer or more structure such as Layer (I) / Layer (II) / Adhesive resin layer / Sealing layer, Layer (I) / Layer (II) / Gas barrier layer / Adhesive resin layer / Sealing layer, or Layer (I) / Layer (II) / Adhesive layer / Gas barrier layer / Adhesive layer / Sealing layer.

[0058] <Application> The laminate is suitable for use as a laminate film for packaging foods such as meat, fish, vegetables, fruits, and desserts, although there is no particular limitation to such a laminate, and the laminate film can be used to produce food packages, particularly deep-draw packages, vacuum packages, and gas-replacement packages. The laminate has excellent oxygen barrier properties, and by utilizing this property, it is suitable for use as a package for extending the shelf life of foods that are susceptible to oxidation. EXAMPLES

[0059] An embodiment of the present invention will be described below, although the present invention is not limited to this embodiment.

[0060] The following raw materials were used to prepare laminates of the following examples, comparative examples, and reference examples.

[0061] <Hemicellulose (A)> Hemicellulose: Xylan GX-1 manufactured by PS Biotech Co., Ltd. (Xylan (mass average molecular weight 45,000) 85% by mass) *Contains 15% by mass of other ingredients

[0062] <Polyvinyl alcohol resin (B)> PVA1: Gohsenol NH-17Q manufactured by Mitsubishi Chemical Corporation, polymerization degree 1700, saponification degree 99 mol% PVA2: Gohsenol NL-05 manufactured by Mitsubishi Chemical Corporation, polymerization degree 500, saponification degree 99 mol% PVA3: Gohsenol GH-17R manufactured by Mitsubishi Chemical Corporation, polymerization degree 2100, saponification degree 88 mol%

[0063] <Ethylene vinyl alcohol resin (b)> EVOH: Mitsubishi Chemical Corporation's Soarnol DC3203RB, ethylene-vinyl alcohol resin, ethylene content 32 mol%

[0064] <Base material> PET substrate (A): Biaxially oriented polyester film (thickness: 38 μm, oxygen permeability: 34 cc / m 2 ·day·atm) PET substrate (B): Biaxially oriented polyester film (thickness: 24 μm, oxygen permeability: 50 cc / m 2 ·day·atm)

[0065] <Preparation of Laminate> [Example 1] The surface of the PET substrate (A) was subjected to a corona discharge treatment so that the surface had a wettability index of 56 or more, and the corona-treated surface was used as the coating surface. A coating liquid was prepared by dissolving hemicellulose (xylan content 85% by mass):PVA1 in a mass ratio of 85:15 in water to give a solid content concentration of 10%. The coating liquid was applied to the PET substrate (A) using a bar coater #30, and dried at 70° C. for 10 minutes to obtain a laminate.

[0066] [Example 2] A laminate was obtained in the same manner as in Example 1, except that a coating liquid was prepared in which hemicellulose (xylan content 85% by mass):PVA1 was dissolved in water in a mass ratio of 70:30 to give a solids concentration of 10%.

[0067] [Example 3] A laminate was obtained in the same manner as in Example 1, except that a coating liquid was prepared in which hemicellulose (xylan content 85% by mass):PVA1 was dissolved in water in a mass ratio of 50:50 to give a solids concentration of 10%.

[0068] [Example 4] A laminate was obtained in the same manner as in Example 1, except that a coating liquid was prepared in which hemicellulose (xylan content 85% by mass):PVA1 was dissolved in water in a mass ratio of 30:70 to give a solids concentration of 10%.

[0069] [Example 5] A laminate was obtained in the same manner as in Example 1, except that a coating liquid was prepared in which hemicellulose (xylan content 85% by mass):PVA1 was dissolved in water in a mass ratio of 15:85 to give a solids concentration of 10%.

[0070] [Example 6] A laminate was obtained in the same manner as in Example 1, except that the PET substrate (B) was used instead of the PET substrate (A) and PVA2 was used instead of PVA1.

[0071] [Example 7] A laminate was obtained in the same manner as in Example 6, except that a coating liquid was prepared in which hemicellulose (xylan content 85% by mass):PVA2 was dissolved in water in a mass ratio of 70:30 to give a solids concentration of 10%.

[0072] [Example 8] A laminate was obtained in the same manner as in Example 6, except that a coating liquid was prepared in which hemicellulose (xylan content 85% by mass):PVA2 was dissolved in water in a mass ratio of 60:40 to give a solids concentration of 10%.

[0073] [Example 9] A laminate was obtained in the same manner as in Example 6, except that a coating liquid was prepared in which hemicellulose (xylan content 85% by mass):PVA2 was dissolved in water in a mass ratio of 50:50 to give a solids concentration of 10%.

[0074] [Comparative Examples 1 to 3] Laminates were obtained in the same manner as in Example 1, except that no hemicellulose was added, PVA1 was used in Comparative Example 1, PVA2 was used in Comparative Example 2, and PVA3 was used in Comparative Example 3 as the polyvinyl alcohol, and a coating liquid was prepared in which the polyvinyl alcohol was dissolved in water so that the solids concentration was 10%.

[0075] [Comparative Example 4] A laminate was obtained in the same manner as in Example 1, except that PVA3 was used instead of PVA1.

[0076] [Comparative Example 5] A laminate was obtained in the same manner as in Comparative Example 4, except that a coating liquid was prepared in which hemicellulose (xylan content 85% by mass):PVA3 was dissolved in water in a mass ratio of 70:30 to give a solids concentration of 10%.

[0077] [Comparative Example 6] A laminate was obtained in the same manner as in Comparative Example 4, except that a coating liquid was prepared in which hemicellulose (xylan content 85% by mass):PVA3 was dissolved in water in a mass ratio of 60:40 to give a solids concentration of 10%.

[0078] [Comparative Example 7] A laminate was obtained in the same manner as in Comparative Example 4, except that a coating liquid was prepared in which hemicellulose (xylan content 85% by mass):PVA3 was dissolved in water in a mass ratio of 50:50 to give a solids concentration of 10%.

[0079] [Comparative Example 8] A laminate was obtained in the same manner as in Example 1, except that a coating liquid was prepared by dissolving only hemicellulose (xylan content: 85% by mass) in water to give a solids concentration of 10%.

[0080] [Reference example] A 30 μm thick film made of EVOH was used, and the film itself was used as a reference example.

[0081] (Physical property measurements) The laminates of Examples 1 to 9, Comparative Examples 1 to 8, and Reference Example were used to measure the following physical properties and were evaluated according to the following criteria. The results are shown in Tables 1 and 2 below. In addition, when measurements were not made, "-" is entered in the table. In addition, when evaluating the physical properties of the layer (I), the coating liquid was prepared in the same manner as in the above-mentioned Examples, except that the solid content concentration was 5%, and the coating liquid was poured into a plastic tray and dried at 23°C x 50% RH for 3 days to prepare the layer (I), and the physical properties were measured. In addition, the thickness of the laminate (after drying) was actually measured using a micrometer, and the thickness of the layer (I) was calculated by subtracting the thickness of the substrate.

[0082] <Oxygen permeability> The oxygen permeability of the laminate was measured at a temperature of 23° C. and a relative humidity of 50% using an oxygen permeability measuring device OX-TRAN 2 / 22 (manufactured by MOCON) in accordance with JIS K7126-2 (2006) (permeation method) and evaluated according to the following criteria. The oxygen permeability per 1 μm of the layer (I) was calculated by the following formula: The oxygen permeability of the base layer (II) had been measured in advance. Oxygen permeability per 1 μm of layer (I)=[thickness of layer (I)] / ([1 / oxygen permeability of laminate]-[1 / oxygen permeability of base layer (II)])

[0083] (Oxygen permeability per 1 μm of layer (I)) ○: 7.0cc / m 2 ·day / atm or less ×:7.0cc / m 2 Exceeds day / atm

[0084] <Tensile stress at break / tensile elongation at break (layer (I))> The tensile stress at break and the tensile elongation at break of the layer (I) were measured in accordance with JIS K7127 (1999). Samples were cut out at random to a width of 15 mm and a length of 60 mm, and tests were performed at a chuck distance of 25 mm and a tensile speed of 200 mm / min, and the results were evaluated according to the following criteria. Comparative Example 8 broke during the test, and measurements could not be made. ◎: Tensile stress at break is 20MPa or more and tensile elongation at break is 100% or more ○: Tensile stress at break is 20 MPa or more and tensile elongation at break is 3% or more and less than 100% ×: Tensile stress at break is less than 20 MPa or tensile elongation at break is less than 3%

[0085] <Storage modulus (layer (I))> The storage modulus of layer (I) was measured by a tensile method using a dynamic viscoelasticity measuring device in accordance with JIS K7244-1 (1998). The storage modulus E' was measured at each temperature (25°C, 100°C, 150°C) with a temperature rise rate of 5°C / min and a frequency of 10Hz. Each sample was cut out to a width of 4.7mm, and the test was performed with a chuck distance of 25mm and a tensile speed of 200mm / min. (25℃) ○: Storage modulus is 1.0×10 9 MPa or more 8.0×10 9 MPa or less ×: Storage modulus is 1.0×10 9 Less than MPa or 8.0 x 10 9 Exceeds MPa (100℃) ○: Storage modulus is 0.2×10 9 MPa or more 2.0×10 9 MPa or less ×: Storage modulus is 0.2×10 9 Less than MPa or 2.0×10 9 Exceeds MPa (150℃) ○: Storage modulus is 0.1×10 9 MPa or more 2.0×10 9 MPa or less ×: Storage modulus is 0.1×10 9 Less than MPa or 2.0×109 Exceeds MPa

[0086] <Biomass level (layer (I))> The biomass degree of layer (I) was calculated from "biomass degree" (%) = "biomass degree of resin made from biomass resources" (%) × "mass proportion of resin made from biomass resources."

[0087] <Haze (Layer (I))> The haze of the layer (I) was measured using a haze meter (NDH-5000, manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with the light transmittance measuring method described in JIS K7136 (2000).

[0088] [Table 1]

[0089] [Table 2]

[0090] (result) Although each Example has a higher biomass content than Comparative Examples 1 to 3, which do not contain hemicellulose (A) in the layer (I), it has good oxygen barrier properties (oxygen permeability) and mechanical properties (storage modulus, stress at break, and elongation at break) that are acceptable for practical use. In addition, compared with Comparative Examples 4 to 8 in which the layer (I) contains a polyvinyl alcohol-based resin (B) having a degree of saponification of less than 90 mol%, it was confirmed that the oxygen barrier properties (oxygen permeability) and mechanical properties (storage modulus, stress at break, and elongation at break) were excellent. Furthermore, it was confirmed that it had the same oxygen barrier properties (oxygen permeability) and mechanical properties (stress at break and elongation at break) as the reference example (EVOH). [Industrial Applicability]

[0091] This laminate has good oxygen barrier properties and excellent mechanical properties, while also being able to solve issues such as environmental friendliness and resource conservation, making it ideal for use as a film or packaging material for food.

Claims

1. A laminate having a layer (I) containing hemicellulose (A) and a polyvinyl alcohol-based resin (B) having a saponification degree of 90 mol % or more on at least one surface of a substrate layer (II).

2. The laminate according to claim 1 , wherein the hemicellulose (A) is contained in the layer (I) in an amount of 10% by mass or more and 90% by mass or less.

3. The laminate according to claim 1 , wherein the substrate layer (II) is a resin substrate or a paper substrate.

4. The storage modulus of the layer (I) at 100° C. and a frequency of 10 Hz measured in accordance with JIS K7244-1 (1998) is 0.20×10 9 The laminate according to claim 1 , wherein the modulus is 1 Pa or more.

5. The laminate according to claim 1 , wherein the hemicellulose (A) is xylan.

6. The oxygen permeability per 1 μm at 23° C.×50% RH measured in accordance with JIS K7126-2 (2006) in the layer (I) is 7.0 cc / m 2 2. The laminate according to claim 1, wherein the thermal expansion coefficient is 0.05-0.55×day·atm or less.

7. The laminate according to claim 1 , wherein the polyvinyl alcohol-based resin (B) has a degree of polymerization of 400 or more.

8. A laminate film comprising the laminate according to any one of claims 1 to 7.

9. The laminate film according to claim 8, which is for food packaging.

10. A packaging material using the laminated film according to claim 8.

Citation Information

Patent Citations

  • High-barrier polyving akohol coating for coating lined paper and preparation method thereof

    CN103382677A

  • Hemicellulose-containing polymer film or coating

    JP2010527384A

  • Polyvinyl alcohol-based film, laminate using the same, package, press-through pack, and method for producing the polyvinyl alcohol-based film

    JP2014189690A

  • Coating substrate, method for manufacturing the coating substrate, package, and dispersion coating.

    JP2013510222A

  • Gas barrier laminate

    JP2020075514A