Positive electrode active material for secondary battery and method for producing the same
By optimizing lithium, manganese, and titanium content, and adjusting X-ray diffraction peak ratios and lattice constant, the charge-discharge curve stability of LiMnTi-containing oxides is improved, ensuring accurate capacity estimation and efficient performance.
Patent Information
- Application Number
- JP2023055132
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional LiMnTi-containing oxides with a rock salt-type structure exhibit inflection points in the charge-discharge curve due to repeated charge-discharge cycles, leading to inaccurate capacity estimation.
Adjusting the content of lithium, manganese, and titanium within specific ranges, along with controlling the intensity ratio of X-ray diffraction peaks and lattice constant, to stabilize the charge-discharge curve shape.
The proposed positive electrode active material achieves high charge/discharge capacity and efficiency with a stable charge-discharge curve shape even after repeated cycles.
Smart Images

Figure 2024142800000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode active material for a secondary battery and a method for producing the same. [Background technology]
[0002] In recent years, research and development has been conducted on positive electrode active materials for secondary batteries that contribute to energy efficiency in order to ensure that more people have access to affordable, reliable, sustainable, and advanced energy. LiMnTi-containing oxides, which are oxides containing lithium, manganese, and titanium and have a rock salt structure, are known as positive electrode active materials for secondary batteries (Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-96974 A [Patent Document 2] International Publication No. 2017 / 122663 [Patent Document 3] International Publication No. 2019 / 087717 Summary of the Invention [Problem to be solved by the invention]
[0004] By the way, it is desirable that the positive electrode active material for secondary batteries has high charge / discharge capacity and charge / discharge efficiency, and can perform stable charge / discharge even when the charge / discharge cycle is repeated. However, according to the study by the present inventors, the conventional rock salt structure LiMnTi-containing oxide is likely to have an inflection point in the charge / discharge curve and the shape of the charge / discharge curve is likely to change due to repeated charge / discharge cycles. The capacity of the secondary battery is estimated based on the charge / discharge curve of the secondary battery. In such capacity estimation, if the shape of the charge / discharge curve of the secondary battery changes, the capacity may not be accurately estimated. Therefore, it is preferable that the positive electrode active material for secondary batteries has a high stability of the shape of the charge / discharge curve when the charge / discharge cycle is repeated.
[0005] The present invention has been made in view of the above, and aims to provide a positive electrode active material for a secondary battery having high charge / discharge capacity and charge / discharge efficiency and having a highly stable shape of the charge / discharge curve when charge / discharge cycles are repeated, and a method for producing the same. [Means for solving the problem]
[0006] The present inventors have found that it is effective to adjust the lithium, manganese, and titanium contents of the LiMnTi-containing oxide, the intensity ratio of a predetermined X-ray diffraction peak in an X-ray diffraction pattern, and the lattice constant in order to solve the above problems, and have completed the present invention. Therefore, the present invention provides the following.
[0007] (1) An oxide containing lithium, manganese and titanium, wherein, when the total content of lithium, manganese and titanium is taken as 100 mol%, the lithium content is within the range of 43 to 60 mol%, the manganese content is within the range of 22 to 35 mol%, and the titanium content is within the range of 7 to 29 mol%, and in an X-ray diffraction pattern measured using a CuKα as an X-ray source, the angle of a maximum X-ray diffraction peak showing the highest peak intensity within a range of 5 to 90 degrees at 2θ is within a range of 43 to 45 degrees, and when the peak intensity of the maximum X-ray diffraction peak is taken as a and the maximum peak intensity among the X-ray diffraction peaks within a range of 15 to 22 degrees at 2θ is taken as b, the following formula is satisfied: 0.70 A positive electrode active material for a secondary battery, having a lattice constant in the range of 4.10 to 4.14 Å.
[0008] According to the positive electrode active material for a secondary battery of (1), the contents of lithium, manganese and titanium, a / (a+b) and the lattice constant are within the above-mentioned ranges, and therefore, the charge / discharge capacity and charge / discharge efficiency, as well as the stability of the shape of the charge / discharge curve when the charge / discharge cycle is repeated, are improved in a well-balanced manner.
[0009] (2) The positive electrode active material for a secondary battery according to (1), wherein the lithium content is in the range of 45 to 58 mol %, the manganese content is in the range of 24 to 33 mol %, and the titanium content is in the range of 9 to 27 mol %, and the a / (a+b) satisfies the following formula: 0.78≦a / (a+b)≦0.86
[0010] According to the positive electrode active material for a secondary battery of (2), the contents of lithium, manganese, and titanium, and a / (a+b) are within the above-mentioned ranges, and therefore, the charge / discharge capacity and charge / discharge efficiency, as well as the stability of the shape of the charge / discharge curve when charge / discharge cycles are repeated, are improved in a more balanced manner.
[0011] (3) A method for producing a positive electrode active material for a secondary battery according to the above (1) or (2), comprising a step of hydrothermally treating a NaMnTi-containing oxide containing sodium, manganese, and titanium in an aqueous lithium solution.
[0012] According to the method for producing a positive electrode active material for a secondary battery of (3), since the NaMnTi-containing oxide is hydrothermally treated in an aqueous lithium solution, the above-mentioned positive electrode active material for a secondary battery can be produced industrially advantageously.
[0013] (4) The method for producing a positive electrode active material for a secondary battery according to (3), wherein the NaMnTi-containing oxide has a sodium content in a range of 0.40 to 0.60 mol and a titanium content in a range of 0.20 to 0.50 mol, when a total molar amount of the manganese and the titanium is taken as 1 mol.
[0014] According to the method for producing a positive electrode active material for a secondary battery of (4), the contents of sodium, manganese, and titanium in the NaMnTi-containing oxide are within the above-mentioned ranges, so that the above-mentioned positive electrode active material for a secondary battery can be reliably produced.
[0015] (5) The method for producing a positive electrode active material for a secondary battery according to (3) or (4), wherein the NaMnTi-containing oxide has a tunnel structure.
[0016] According to the method for producing a positive electrode active material for a secondary battery in (5), since the NaMnTi-containing oxide has a tunnel structure, the above-mentioned positive electrode active material for a secondary battery can be produced more reliably.
[0017] (6) The method for producing a positive electrode active material for a secondary battery according to any one of (3) to (5), wherein the lithium content of the lithium aqueous solution is in the range of 2.0 to 30.0 moles, where the total molar amount of the manganese and the titanium contained in the NaMnTi-containing oxide in the lithium aqueous solution is taken as 1 mole.
[0018] According to the method for producing a positive electrode active material for a secondary battery in (6), since the lithium content of the lithium aqueous solution is within the above range, the above-mentioned positive electrode active material for a secondary battery can be produced more reliably. Effect of the Invention
[0019] According to the present invention, it is possible to provide a positive electrode active material for a secondary battery having high charge / discharge capacity and charge / discharge efficiency and having a highly stable shape of the charge / discharge curve when charge / discharge cycles are repeated, and a method for producing the same. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a flow diagram showing a method for producing a positive electrode active material for a secondary battery according to one embodiment of the present invention. [Diagram 2] 1 shows X-ray diffraction patterns of the LiMnTi-containing oxide powders or the LiMn-containing oxide powders obtained in Examples 1 to 4 and Comparative Examples 1 and 2. [Diagram 3] 1 is a graph showing the initial charge / discharge curve of a two-electrode cell using the LiMnTi-containing oxide powder obtained in Example 1. [Figure 4] 1 is a graph showing the initial charge / discharge curve of a two-electrode cell using the LiMnTi-containing oxide powder obtained in Example 2. [Diagram 5] 1 is a graph showing the initial charge / discharge curve of a two-electrode cell using the LiMnTi-containing oxide powder obtained in Example 3. [Figure 6] 1 is a graph showing the initial charge / discharge curve of a two-electrode cell using the LiMnTi-containing oxide powder obtained in Example 4. [Figure 7] 1 is a graph showing the initial charge / discharge curves of a two-electrode cell using the LiMn-containing oxide powder obtained in Comparative Example 1. [Figure 8] 1 is a graph showing the initial charge / discharge curves of a two-electrode cell using the LiMnTi-containing oxide powder obtained in Comparative Example 2. [Figure 9]2 is a graph showing a charge / discharge curve at the second cycle and a charge / discharge curve at the seventh cycle of a two-electrode cell using the LiMnTi-containing oxide powder obtained in Example 1. [Figure 10] 1 is a graph showing a charge / discharge curve at the second cycle and a charge / discharge curve at the seventh cycle of a two-electrode cell using the LiMn-containing oxide powder obtained in Comparative Example 1. [Figure 11] 1 is a graph showing a charge / discharge curve at the second cycle and a charge / discharge curve at the seventh cycle of a two-electrode cell using the LiMnTi-containing oxide powder obtained in Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, embodiments of the present invention will be described. However, the embodiments described below are merely examples of the present invention, and the present invention is not limited to the following.
[0022] The positive electrode active material for a secondary battery of this embodiment is a LiMnTi-containing oxide that contains lithium, manganese, and titanium. The contents of lithium, manganese and titanium in the LiMnTi-containing oxide are set such that, when the total content of lithium, manganese and titanium is taken as 100 mol%, the lithium content is in the range of 43 to 60 mol%, the manganese content is in the range of 22 to 35 mol%, and the titanium content is in the range of 7 to 29 mol%. When the lithium content is 43 mol% or more, the charge / discharge capacity is improved. When the lithium content is 60 mol% or less, the charge / discharge efficiency is improved. When the manganese content is 35 mol% or less and the titanium content is 9 mol% or more, the shape stability of the charge / discharge curve when the charge / discharge cycle is repeated is improved. When the manganese content is 22 mol% or more and the titanium content is 29 mol% or less, the charge / discharge capacity is improved and the cycle characteristics are improved. For this reason, in this embodiment, the contents of lithium, manganese and titanium are set within the above ranges. The lithium content may be in the range of 45 to 58 mol %, the manganese content may be in the range of 24 to 33 mol %, and the titanium content may be in the range of 9 to 27 mol %.
[0023] The lithium, manganese and titanium contents of the LiMnTi-containing oxide may be in the range of 0.80 to 1.40 moles of lithium and 0.20 to 0.50 moles of titanium, when the total molar amount of manganese and titanium is taken as 1 mole. Furthermore, the lithium content may be in the range of 0.80 to 1.35 moles and the titanium content may be in the range of 0.22 to 0.49 moles.
[0024] The LiMnTi-containing oxide may contain other metals than lithium, manganese, and titanium. The content of the other metals may be in the range of 0.00 to 1.00 mol% when the total content of lithium, manganese, and titanium is taken as 100 mol%. The content of sodium may be in the range of 0.00 to 1.00 mol%.
[0025] In the X-ray diffraction pattern of the LiMnTi-containing oxide measured using CuKα as an X-ray source, the angle of the maximum X-ray diffraction peak, which shows the highest peak intensity within the range of 5 to 90 degrees at 2θ, is within the range of 43 to 45 degrees. The X-ray diffraction peak within the range of 43 to 45 degrees at 2θ coincides with the maximum X-ray diffraction peak of the LiMnTi-containing oxide having a rock salt structure. In other words, the LiMnTi-containing oxide contains the LiMnTi-containing oxide having a rock salt structure as a main component.
[0026] The LiMnTi-containing oxide satisfies the following formula, where a is the peak intensity of the above-mentioned maximum X-ray diffraction peak and b is the maximum peak intensity among the X-ray diffraction peaks within the range of 15 to 22 deg at 2θ. 0.70
[0027] The X-ray diffraction peaks in the range of 15 to 22 deg in 2θ coincide with the X-ray diffraction peaks of LiMnTi-containing oxides other than the rock-salt structure. The structures other than the rock-salt structure include, for example, a Li-rich layered structure, a layered rock-salt structure, a spinel structure, and a tunnel structure. a / (a+b) is an index of the proportion of the rock-salt structure contained in the LiMnTi-containing oxide.
[0028] In the LiMnTi-containing oxide, if the Li-excess layered structure is too much, the voltage of the charge / discharge curve may decrease when the charge / discharge cycle is repeated. If the layered rock salt structure is too much, the charge / discharge curve may be easily inflection-point-like when the charge / discharge cycle is repeated. If the spinel structure is too much, the charge / discharge capacity in a practical potential range (high potential) may decrease. If the tunnel structure is too much, the lithium content may decrease, and the discharge capacity may decrease. For this reason, in this embodiment, a / (a+b) is set within the above range. It is preferable that a / (a+b) satisfies 0.78≦a / (a+b)≦0.86.
[0029] The lattice constant of the LiMnTi-containing oxide is in the range of 4.10 to 4.14 Å. The lattice constant is that of the LiMnTi-containing oxide having a rock-salt structure. When the contents of lithium, manganese and titanium and a / (a+b) are within the above ranges and the lattice constant is within this range, the rock-salt structure becomes more stable, and the stability of the shape of the charge-discharge curve when the charge-discharge cycle is repeated is improved.
[0030] The positive electrode active material for secondary batteries of this embodiment can be produced by a method including a step of obtaining a precursor of LiMnTi-containing oxide and a step of obtaining a positive electrode active material for secondary batteries from the obtained precursor. The precursor is an NaMnTi-containing oxide containing sodium, manganese, and titanium. The method of producing the positive electrode active material for secondary batteries of this embodiment will be described with reference to FIG. 1.
[0031] As shown in FIG. 1, the process for obtaining the NaMnTi-containing oxide (precursor) includes a mixing step S1 and a firing step S2. In the mixing step S1, a sodium source, a manganese source, and a titanium source are mixed to obtain a raw material mixture. There are no particular limitations on the sodium source, manganese source, and titanium source, and various compounds such as oxides, carbonates, hydroxides, and chlorides can be used. In this embodiment, Na2CO3 is used as the sodium source, Mn2O3 is used as the manganese source, and TiO2 is used as the titanium source.
[0032] The mixing ratio of the sodium source, manganese source and titanium source is, for example, such that when the total molar amount of manganese and titanium is 1 mol, the amount of sodium is in the range of 0.40 to 0.60 mol and the amount of titanium is in the range of 0.20 to 0.50 mol. The method of mixing the sodium source, manganese source and titanium source is not particularly limited, and may be a dry method or a wet method.
[0033] In the firing step S2, the raw material mixture obtained in the mixing step S1 is fired to generate an NaMnTi-containing oxide. The firing conditions for the raw material mixture can be, for example, in air at a firing temperature of 900 to 1200° C. The firing time varies depending on conditions such as the composition of the raw material mixture and the firing temperature, but is, for example, within a range of 1 to 30 hours.
[0034] The NaMnTi-containing oxide obtained as described above may have a tunnel structure.
[0035] As shown in FIG. 1, the process for obtaining a positive electrode active material for a secondary battery from an NaMnTi-containing oxide includes a mixing step S3, a hydrothermal synthesis step S4, a water-washing step S5, a drying step S6, and a pulverization step S7. In the mixing step S3, the NaMnTi-containing oxide, the lithium source, and water are mixed to obtain a dispersion in which the NaMnTi-containing oxide is dispersed in a lithium aqueous solution. There is no particular limitation on the lithium source, and various compounds such as oxides, carbonates, hydroxides, and chlorides can be used. In this embodiment, LiOH·H2O is used as the lithium source. The content of lithium in the dispersion is, for example, in the range of 2.0 to 30.0 moles, assuming that the total molar amount of manganese and titanium contained in the NaMnTi-containing oxide in the dispersion is 1 mole.
[0036] In the hydrothermal synthesis step S4, the NaMnTi-containing oxide in the dispersion obtained in the mixing step S3 is hydrothermally treated to hydrothermally synthesize a LiMnTi-containing oxide. By hydrothermally treating the NaMnTi-containing oxide in a lithium aqueous solution, sodium in the NaMnTi-containing oxide is replaced with lithium, and the crystal structure of the NaMnTi-containing oxide is changed to generate a LiMnTi-containing oxide having a rock salt structure. The hydrothermal treatment can be performed, for example, by storing the dispersion in a sealed container and heating the sealed container in air at a temperature of 150 to 230°C. The treatment time for the hydrothermal treatment varies depending on conditions such as the ratio of the NaMnTi-containing oxide and the lithium source in the dispersion and the capacity of the sealed container, but is, for example, within the range of 1 to 30 hours.
[0037] In the water-washing step S5, the LiMnTi-containing oxide produced in the hydrothermal synthesis step S4 is collected and washed with water. By washing the LiMnTi-containing oxide with water, sodium substituted for lithium and unreacted lithium source are removed.
[0038] In the drying step S6, the LiMnTi-containing oxide washed in the water-washing step S5 is dried. The drying method is not particularly limited, and various methods used as a drying method for inorganic materials, such as a heat drying method, a vacuum drying method, a spray drying method, etc., can be used.
[0039] In the pulverization step S7, the LiMnTi-containing oxide dried in the drying step S6 is pulverized to adjust the particle size to a size usable as a positive electrode active material for a secondary battery. The pulverization method is not particularly limited, and pulverization can be performed using various pulverizing devices used for pulverizing inorganic materials, such as a ball mill, a bead mill, a jet mill, or a mortar and pestle.
[0040] The positive electrode active material for secondary batteries of the present embodiment can be used as a positive electrode active material for lithium secondary batteries. The lithium secondary battery has, for example, a positive electrode, a negative electrode, an electrolyte, a separator disposed between the positive electrode and the negative electrode, and an exterior body that houses them. A solid electrolyte may be used instead of the electrolyte.
[0041] The positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the surface of the positive electrode current collector. The positive electrode active material layer includes the positive electrode active material for secondary batteries of this embodiment. The positive electrode active material layer may include a conductive assistant and a binder. Since the positive electrode active material for secondary batteries of this embodiment is chemically stable, the conductive assistant and the binder are not particularly limited, and known materials used in the positive electrode active material layer of lithium secondary batteries can be used. In addition, the positive electrode current collector is not particularly limited, and known materials used in the positive electrode current collector of lithium secondary batteries, such as aluminum foil, can be used.
[0042] The negative electrode may be a laminate including a negative electrode current collector and a negative electrode active material layer formed on the surface of the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material. The negative electrode active material may be metallic lithium, a material capable of absorbing and releasing lithium, or a metal or metalloid that forms an alloy with lithium. Examples of materials capable of absorbing and releasing lithium include lithium transition metal oxides such as lithium titanate, transition metal oxides such as TiO2, Nb2O3, and WO3, SiO, metal sulfides, metal nitrides, and carbon materials such as artificial graphite, natural graphite, graphite, soft carbon, and hard carbon. Examples of metals or metalloids that form an alloy with lithium include Mg, Si, Au, Ag, In, Ge, Sn, Pb, Al, and Zn. When the negative electrode active material is in powder form, the negative electrode active material layer may include a conductive assistant and a binder. There are no particular limitations on the conductive assistant and binder, and known conductive assistants and binders used in the negative electrode active material layer of lithium secondary batteries may be used. The negative electrode current collector is not particularly limited, and any known negative electrode current collector such as copper foil that is used as a negative electrode current collector for lithium secondary batteries can be used.
[0043] The electrolytic solution includes an organic solvent and an electrolyte. Examples of the organic solvent include cyclic carbonates, chain carbonates, cyclic ethers, chain ethers, hydrofluoroethers, aromatic ethers, sulfones, cyclic esters, chain carboxylates, and nitriles. Examples of the cyclic carbonates include ethylene carbonate, propylene carbonate, vinylene carbonate, and fluoroethylene carbonate. Examples of the chain carbonates include dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. Examples of the cyclic ethers include tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, and 4-methyl1,3-dioxolane. Examples of the chain ethers include 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, and diethyl ether. Examples of hydrofluoroethers include 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, bis(2,2,2-trifluoroethyl)ether, 1,2-bis(1,1,2,2-tetrafluoroethoxy)ethane, and the like. Examples of aromatic ethers include anisole. Examples of sulfones include sulfolane and methylsulfolane. Examples of cyclic esters include γ-butyrolactone, and the like. Examples of chain carboxylates include acetates, butyrates, and propionates. Examples of nitriles include acetonitrile and propionitrile. The organic solvents may be used alone or in combination of two or more.
[0044] The electrolyte is a source of lithium ions, which are charge transfer media, and includes a lithium salt. Examples of the lithium salt include LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC(CF3SO2)3, LiN(CF3SO2)2(LiTFSI), LiN(FSO2)2(LiFSI), and LiBC4O8. The lithium salt may be used alone or in combination of two or more.
[0045] As the solid electrolyte, for example, a sulfide solid electrolyte, an oxide solid electrolyte, a nitride solid electrolyte, a halide solid electrolyte, or the like can be used. Examples of sulfide solid electrolytes include Li2S-P2S5 and Li2S-P2S5-LiI. Examples of oxide solid electrolytes include NASICON-type oxides, garnet-type oxides, and perovskite-type oxides. Examples of NASICON-type oxides include oxides containing Li, Al, Ti, P, and O (e.g., Li 1.5 Al 0.5 Ti 1.5 (PO4)3). Examples of garnet-type oxides include oxides containing Li, La, Zr, and O (e.g., Li7La3Zr2O 12 Examples of perovskite oxides include oxides containing Li, La, Ti, and O (for example, LiLaTiO3).
[0046] The separator is not particularly limited, and may be, for example, a porous sheet or a nonwoven sheet. Examples of materials for the porous sheet include polyolefins such as polyethylene and polypropylene, aramid, polyimide, and fluororesin. Examples of materials for the nonwoven sheet include glass fiber and cellulose fiber.
[0047] The exterior body is not particularly limited, and any known exterior body used for lithium secondary batteries, such as a metal container or a laminate film container, can be used.
[0048] According to the positive electrode active material for a secondary battery of the present embodiment configured as described above, the contents of lithium, manganese, and titanium, a / (a+b), and the lattice constant are within the above-mentioned ranges, and therefore, the charge / discharge capacity and charge / discharge efficiency, as well as the stability of the shape of the charge / discharge curve when charge / discharge cycles are repeated, are improved in a well-balanced manner.
[0049] According to the method for producing a positive electrode active material for a secondary battery of this embodiment, since the NaMnTi-containing oxide is hydrothermally treated in an aqueous lithium solution, the above-mentioned positive electrode active material for a secondary battery can be produced industrially advantageously. EXAMPLES
[0050] [Example 1] (Preparation of NaMnTi-containing oxide powder) Na2CO3, Mn2O3 and TiO2 were weighed out so that the total molar amount of Mn and Ti was 1 mole, the molar amount of Na (Na / (Mn+Ti)) was 0.5 moles, the molar amount of Ti (Ti / (Mn+Ti)) was 0.22 moles, and the total mass was 1.0 g. The weighed Na2CO3, Mn2O3 and TiO2 were mixed using a mortar and pestle. The obtained raw material mixture was placed in an alumina crucible and fired in air at a firing temperature of 1000°C for a firing time of 12 hours. After firing, the obtained fired product was pulverized using a mortar and pestle. The X-ray diffraction pattern of the obtained fired product powder was measured, and it was confirmed that the obtained fired product powder was a NaMnTi oxide powder having a tunnel structure.
[0051] (Preparation of LiMnTi-containing oxide powder) 2.00g of LiOH·H2O and 50mL of water were placed in a hydrothermal reaction vessel and stirred to dissolve LiOH·H2O, preparing a LiOH solution. Next, 0.5g of the NaMnTi oxide powder obtained above was placed in the LiOH solution and stirred to obtain a dispersion in which the NaMnTi oxide powder was dispersed in the LiOH solution. Next, the hydrothermal reaction vessel was sealed, and the sealed hydrothermal reaction vessel was placed in a thermostatic chamber and heated in air at a heating temperature of 180 degrees for a heating time of 24 hours to hydrothermally treat the NaMnTi oxide powder. After heating, the powder after hydrothermal treatment (LiMnTi-containing oxide powder) was collected from the hydrothermal reaction vessel. The collected LiMnTi-containing oxide powder was washed with water, and then centrifuged three times to remove moisture. The LiMnTi-containing oxide powder from which moisture had been removed was placed on a petri dish and vacuum-dried at a temperature of 100°C for 6 hours. The dried LiMnTi-containing oxide powder was pulverized using a mortar and pestle.
[0052] [Example 2] A LiMnTi-containing oxide powder was prepared in the same manner as in Example 1, except that in the preparation of the NaMnTi-containing oxide powder, Na2CO3, Mn2O3, and TiO2 were weighed out so that the molar amount of Ti was 0.33 mol when the total molar amount of Mn and Ti was 1 mol.
[0053] [Example 3] A LiMnTi-containing oxide powder was prepared in the same manner as in Example 1, except that in the preparation of the NaMnTi-containing oxide powder, Na2CO3, Mn2O3, and TiO2 were weighed out so that the molar amount of Ti was 0.44 mol when the total molar amount of Mn and Ti was 1 mol.
[0054] [Example 4] A Li-Mn-Ti oxide powder was prepared in the same manner as in Example 1, except that in preparing the NaMnTi-containing oxide powder, Na2CO3, Mn2O3, and TiO2 were weighed out so that the molar amount of Ti was 0.50 moles when the total molar amount of Mn and Ti was 1 mole.
[0055] [Comparative Example 1] The LiMn-containing oxide powder was produced by carrying out the same operation as in Example 1, except that in the preparation of the NaMnTi-containing oxide powder, TiO2 was not used, and Na2CO3 and Mn2O3 were weighed out so that the molar ratio of Na to Mn was 0.5:1 and the total mass was 1.0 g.
[0056] [Comparative Example 2] A LiMnTi-containing oxide powder was prepared in the same manner as in Example 1, except that in the preparation of the NaMnTi-containing oxide powder, Na2CO3, Mn2O3, and TiO2 were weighed out so that the molar amount of Ti was 0.11 mol when the total molar amount of Mn and Ti was 1 mol.
[0057] [evaluation] The LiMnTi-containing oxide powders or LiMn-containing oxide powders obtained in Examples 1 to 4 and Comparative Examples 1 and 2 were evaluated for chemical composition, X-ray diffraction pattern, lattice constant, charge / discharge characteristics, and shape stability of charge / discharge curve by the following methods.
[0058] (chemical composition) The sample was dissolved in acid. The contents of lithium, manganese and titanium in the obtained solution were measured using an ICP emission spectrometer. From the obtained lithium, manganese and titanium contents, the contents of lithium, manganese and titanium when the total content of these metals was taken as 100 mol %, and the molar amounts of lithium, manganese and titanium when the total molar amount of manganese and titanium was taken as 1 mol were calculated. The results are shown in Table 1 below.
[0059] (X-ray diffraction pattern) The X-ray diffraction pattern was measured under the following conditions. The X-ray diffraction pattern is shown in FIG. 2. The angle of the maximum X-ray diffraction peak was measured from the X-ray diffraction pattern. Note that, for the LiMn-containing oxide powder obtained in Comparative Example 1, the angle of the maximum X-ray diffraction peak, 2θ, was outside the range of 43 to 45 deg, so the angle of the maximum X-ray diffraction peak was not measured. In addition, from the X-ray diffraction pattern, the maximum peak intensity a among the X-ray diffraction peaks within the range of 43 to 45 deg in 2θ was read, and the peak intensity a of the maximum X-ray diffraction peak and the maximum peak intensity b among the X-ray diffraction peaks within the range of 15 to 22 deg in 2θ were read, and a / (a+b) was calculated. The results are shown in Table 2. Measurement device: RINT-2550V, manufactured by Rigaku Corporation X-ray source:CuKα X-ray output: 40kV, 200mA Measurement conditions: 1.0 s, 0.03 deg interval
[0060] (Lattice constant) The lattice constant was calculated by the least squares method using the indices of the X-ray diffraction peaks due to the rock salt structure obtained from the X-ray diffraction pattern obtained under the above conditions and their interplanar spacings. The results are shown in Table 2.
[0061] (Charge / discharge characteristics) 5 mg of the sample was mixed with 5 mg of acetylene black as a conductive material and 1 mg of PTFE as a binder. The resulting mixture was formed into a sheet and pressed onto an Al mesh to form the working electrode, and the counter electrode was a metallic lithium foil. The working electrode and counter electrode were immersed in an electrolyte solution in which LiPF6 was dissolved in an EC+DMC solvent to prepare a two-electrode cell.
[0062] A charge / discharge test was performed using a two-electrode cell. The conditions for the charge / discharge test were a current density (per sample) of 10 mA / g, a potential range of 2.0-4.8 V, and constant current / constant voltage charging (until 2 hours had elapsed). The charge / discharge test was performed in an environment of 25°C. Seven cycles of the charge / discharge test were performed, with the voltage range being 2.0-4.3 V from the second cycle onwards. The initial (first cycle) charge / discharge curves are shown in Figures 3 to 8, and the initial charge capacity, discharge capacity and charge / discharge efficiency (initial discharge capacity / initial charge capacity x 100) are shown in Table 3.
[0063] (Charge / discharge curve shape stability) The charge / discharge curves at the second cycle and the seventh cycle obtained in the evaluation of the charge / discharge characteristics were compared, and the shape stability of the charge / discharge curves was judged from the viewpoint of whether a new inflection point was generated in the charge curve and the discharge curve at the seventh cycle. When a new inflection point was not generated, it was determined that there was no shape change, and when a new inflection point was generated, it was determined that there was a shape change. The results are shown in Table 3. The charge / discharge curves at the second cycle and the seventh cycle of the two-electrode cell using the LiMn-containing oxide powder obtained in Example 1 are shown in FIG. 9. The charge / discharge curves at the second cycle and the seventh cycle of the two-electrode cell using the LiMn-containing oxide powder obtained in Comparative Example 1 are shown in FIG. 10. The charge / discharge curves at the second cycle and the seventh cycle of the two-electrode cell using the LiMnTi-containing oxide powder obtained in Comparative Example 2 are shown in FIG. 11.
[0064] [Table 1]
[0065] [Table 2]
[0066] [Table 3]
[0067] From the results shown in Tables 1 to 3 and Figures 2, 3 to 6, and 9, the LiMnTi-containing oxide powders of Examples 1 to 4, in which the lithium, manganese, and titanium contents, a / (a+b), and lattice constants are within the ranges of the present invention, show a well-balanced improvement in charge / discharge capacity and charge / discharge efficiency, and the stability of the shape of the charge / discharge curve when the charge / discharge cycle is repeated, and are useful as a positive electrode active material for secondary batteries. On the other hand, the LiMn-containing oxide powder of Comparative Example 1, which does not contain titanium, showed a decrease in the initial charge / discharge efficiency. In addition, as shown in Figure 10, an inflection point occurred in the charge / discharge curve at the 7th cycle. As shown in Figure 11, the LiMnTi-containing oxide powder of Comparative Example 2, in which the titanium content and a / (a+b) are outside the ranges of the present invention, showed an inflection point in the charge / discharge curve at the 7th cycle.
Claims
1. An oxide containing lithium, manganese and titanium, When the total content of lithium, manganese and titanium is 100 mol%, The lithium content is in the range of 43 to 60 mol %, The manganese content is within the range of 22 to 35 mol %, The titanium content is in the range of 7 to 29 mole percent; In the X-ray diffraction pattern measured using CuKα as the X-ray source, the angle of the maximum X-ray diffraction peak, which shows the highest peak intensity within the range of 5 to 90 degrees at 2θ, is within the range of 43 to 45 degrees; When the peak intensity of the maximum X-ray diffraction peak is defined as a and the maximum peak intensity among the X-ray diffraction peaks within the range of 15 to 22 deg in 2θ is defined as b, the following formula is satisfied: 0.70<a / (a+b)<0.90 A positive electrode active material for a secondary battery, the lattice constant of which is within the range of 4.10 to 4.14 Å.
2. The lithium content is in the range of 45 to 58 mol %, the manganese content is in the range of 24 to 33 mol %, and the titanium content is in the range of 9 to 27 mol %.
2. The positive electrode active material for a secondary battery according to claim 1, wherein a / (a+b) is within the range of: 0.78≦a / (a+b)≦0.86
3. A method for producing a positive electrode active material for a secondary battery according to claim 1 or 2, A method for producing a positive electrode active material for a secondary battery, comprising: subjecting an NaMnTi-containing oxide, which contains sodium, manganese, and titanium, to a hydrothermal treatment in an aqueous lithium solution.
4. 4. The method for producing a positive electrode active material for a secondary battery according to claim 3, wherein the NaMnTi-containing oxide has a sodium content in the range of 0.40 to 0.60 mol and a titanium content in the range of 0.20 to 0.50 mol, when a total molar amount of the manganese and the titanium is taken as 1 mol.
5. The method for producing a positive electrode active material for a secondary battery according to claim 3 , wherein the NaMnTi-containing oxide has a tunnel structure.
6. 4. The method for producing a positive electrode active material for a secondary battery according to claim 3, wherein the lithium content of the lithium aqueous solution is in the range of 2.0 to 30.0 moles, when the total molar amount of the manganese and the titanium contained in the NaMnTi-containing oxide in the lithium aqueous solution is taken as 1 mole.
Citation Information
Patent Citations
Method for preparing cationic unordered rock salt structure anode material through high-valent-state transition metal ion replacement combination strategies
CN110372039A
Crystal material of alkali-transition metal oxide and its producing method
JP2005263583A
Positive electrode material for lithium secondary battery, its manufacturing method and lithium secondary battery using it
JP2005268127A
Lithium manganese-based compound oxide and method for manufacturing the same
JP2012041257A
Positive electrode active material
JP2016122549A