Method for manufacturing substrate laminate

The pressure printing and molding method for forming patterns on substrates addresses the challenge of achieving a thick adhesive layer without sagging, enhancing the adhesion and reliability of substrate laminates in MEMS sensors.

JP2024142854APending Publication Date: 2024-10-11KANEKA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023055216
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing methods for manufacturing substrate laminates face challenges in achieving a thick adhesive layer without compromising filling properties or causing sagging, particularly in the production of MEMS sensors like image sensors, acceleration sensors, and pressure sensors.

Method used

A method involving a pressure printing technique to form a first pattern on a substrate, followed by molding to create a second pattern, which allows for bonding with a curable resin composition containing glycidyl or alicyclic epoxy groups, enhancing the adhesive layer's thickness and stability.

Benefits of technology

This approach enables easy thickening of the adhesive layer, improving filling properties and reducing sagging, thereby ensuring robust adhesion and reliability in substrate laminates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142854000001_ABST
    Figure 2024142854000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a substrate laminate which can easily achieve a thick film of an adhesive layer.SOLUTION: A method for manufacturing a substrate laminate includes the steps of: forming a first pattern 11 of a curable resin composition on a first substrate 21, using a pressurization printing method; and bonding the first substrate 21 and a second substrate 22, through the first pattern 11. A method for manufacturing a substrate laminate further includes a step of molding the first pattern 11 with a mold, and forming a second pattern 12, after the step of forming the first pattern 11, and the bonding step may bond the first substrate 21 and the second substrate 22, through the second pattern 12.SELECTED DRAWING: Figure 3A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a substrate laminate. [Background technology]

[0002] Conventionally, when manufacturing MEMS sensors such as image sensors, acceleration sensors, and pressure sensors, a semiconductor element substrate and a sealing substrate such as a glass substrate, a metal substrate, or a ceramic substrate are bonded via an adhesive layer disposed around the semiconductor element. Known methods for forming the adhesive layer include a method of screen printing an ultraviolet-curing adhesive and a method of applying an ultraviolet-curing adhesive using a dispenser (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-115104 A Summary of the Invention [Problem to be solved by the invention]

[0004] Here, in order to prevent the reflection of foreign matter that may adhere to the glass substrate, it is desirable to make the adhesive layer thicker. In this regard, for example, if the thickness of the emulsion of the screen printing plate is increased, the viscosity of the adhesive layer material (resin) reduces the filling ability of the screen printing plate. On the other hand, if the viscosity of the adhesive layer material is reduced in order to increase the filling ability of the screen printing plate, the adhesive layer will sag when the screen printing plate is removed.

[0005] An object of the present invention is to provide a method for manufacturing a substrate laminate that can easily realize a thick adhesive layer. [Means for solving the problem]

[0006] [1] A method for manufacturing a substrate laminate according to the present invention includes the steps of forming a first pattern of a curable resin composition on a first substrate by using a pressure printing method, and bonding the first substrate and a second substrate together via the first pattern.

[0007] [2] The method for manufacturing a substrate laminate described in [1] may further include, after the step of forming the first pattern, a step of forming a second pattern by molding the first pattern with a mold, and the bonding step may include bonding the first substrate and the second substrate together via the second pattern.

[0008] [3] In the method for producing a substrate laminate according to [1] or [2], the pressure printing method may be a vacuum pressure printing method.

[0009] [4] In the method for manufacturing a substrate stack according to any one of [1] to [3], one of the first substrate and the second substrate may be a semiconductor element substrate, and the other of the first substrate and the second substrate may be a transparent substrate.

[0010] [5] In the method for producing a substrate laminate according to any one of [1] to [4], the curable resin composition may contain at least one of a glycidyl group and an alicyclic epoxy group.

[0011] [6] In the method for producing a substrate laminate according to any one of [1] to [5], the curable resin composition may contain a polysiloxane compound.

[0012] [7] In the method for producing a substrate laminate according to any one of [1] to [6], the curable resin composition may contain a photosensitive resin.

[0013] [8] The method for producing a substrate laminate according to any one of [1] to [7] may further include a step of exposing to the first pattern.

[0014] [9] The method for producing a substrate laminate according to any one of [2] to [7] may further include a step of exposing to the second pattern. Effect of the Invention

[0015] According to the present invention, it is possible to easily realize a thicker adhesive layer in a substrate laminate. [Brief description of the drawings]

[0016] [Figure 1A] 5A to 5C are diagrams showing a step of forming a first pattern on a first substrate according to the embodiment. [Figure 1B] 5A to 5C are diagrams showing a step of forming a first pattern on a first substrate according to the embodiment. [Figure 1C] 5A to 5C are diagrams showing a step of forming a first pattern on a first substrate according to the embodiment. [Figure 1D] 5A to 5C are diagrams showing a step of forming a first pattern on a first substrate according to the embodiment. [Figure 2A] 4A to 4C are diagrams showing a process of forming a second pattern by molding the first pattern according to the embodiment. [Figure 2B] 4A to 4C are diagrams showing a process of forming a second pattern by molding the first pattern according to the embodiment. [Figure 2C] 4A to 4C are diagrams showing a process of forming a second pattern by molding the first pattern according to the embodiment. [Figure 3A] 5A to 5C are diagrams showing a process of bonding a first substrate and a second substrate via a second pattern according to the present embodiment. [Figure 3B] 5A to 5C are diagrams showing a process of bonding a first substrate and a second substrate via a second pattern according to the present embodiment. [Figure 4] 10A to 10D are diagrams showing a step of forming a first pattern on a first substrate according to a modified example of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0018] [Method of manufacturing substrate laminate] The method for producing a substrate laminate of this embodiment includes a step of forming a first pattern of a curable resin composition on a first substrate by using a pressure printing method, and a step of bonding the first substrate and a second substrate together via the first pattern. The method for producing a substrate laminate of this embodiment further includes a step of forming a second substrate by molding the first substrate with a mold after the step of forming the first substrate, and the bonding step includes bonding the first substrate and the second substrate together via the second substrate.

[0019] By using the pressurized printing method, even if the thickness of the printing plate (for example, the emulsion of a screen printing plate) is increased, the filling property of the printing plate can be improved. In addition, the viscosity of the material of the adhesive layer, i.e., the curable resin composition, can be increased, and the sagging of the adhesive layer when the printing plate is removed can be reduced. Therefore, it is easy to realize a thicker adhesive layer, i.e., a thicker pattern of the curable resin composition.

[0020] The first and second substrates are not particularly limited, but may be, for example, a semiconductor element substrate, a silicon wafer, a glass substrate, a transparent resin substrate, a colored resin substrate, a ceramic substrate, etc. The first and second substrates may be the same or different. For example, when manufacturing an image sensor, it is preferable that one of the first and second substrates is a semiconductor element substrate, and the other of the first and second substrates is a glass substrate or a transparent resin substrate.

[0021] The shape of the upper surface of the first substrate and the second substrate is not particularly limited, but may be, for example, a circular shape, a rectangular shape, etc. From the viewpoint of productivity of the substrate stack, it is preferable to use, as the first substrate and the second substrate, a rectangular substrate of 100 mm×100 mm or more, a substrate obtained by rearranging a substrate that has been singulated once in an area of ​​100 mm×100 mm or more, or a circular substrate of 4 inches to 12 inches. The size and shape of the first substrate and the second substrate may be the same or different.

[0022] The pattern of the curable resin composition functions as an adhesive layer that bonds the first substrate and the second substrate. The width and height of the adhesive layer can be set appropriately, and by selecting them appropriately, a hollow structure (substrate laminate) can be easily obtained. In particular, when the substrate laminate is applied to a CMOS / CCD sensor, if the height of the adhesive layer is too low, the sensor substrate may be damaged during assembly. In addition, if the height of the adhesive layer is too high, a good pattern may not be obtained. From these points of view, the height of the adhesive layer is preferably 10 μm or more and 1000 μm or less, more preferably 50 μm or more and 500 μm or less, and even more preferably 50 μm or more and 300 μm or less. The upper limit of the height of the adhesive layer may be 200 μm or 150 μm. If the width of the adhesive layer is too narrow, sufficient adhesive strength may not be obtained, and if the width of the adhesive layer is too wide, sufficient space for arranging the semiconductor element may not be obtained. From these points of view, the width of the adhesive layer is preferably 10 μm or more and 1000 μm or less, and more preferably 100 μm or more and 300 μm or less.

[0023] The arithmetic mean roughness Ra of the surface of the adhesive layer formed on the first substrate that contacts the second substrate is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. When Ra is 5 μm or less, the variation in the height of the adhesive layer is reduced, and the adhesion reliability is improved. Note that Ra can be measured using a 3D measuring laser microscope.

[0024] The curable resin composition can be prepared by various methods. The curable resin composition may be prepared by mixing the components immediately before use, or may be stored at low temperature in a one-liquid state prepared by mixing the components in advance. From the viewpoint of handleability, etc., the curable resin composition is preferably liquid. From the viewpoint of suppressing the exudation of the curable resin composition, the viscosity of the curable resin composition at 25°C is preferably 1 Pa·s or more. In addition, from the viewpoint of using a printing method, the viscosity of the curable resin composition at 25°C is preferably 250 Pa·s or less. The viscosity of the curable resin composition can be measured using a rheometer.

[0025] An example of a method for manufacturing a substrate laminate according to this embodiment will be described below with reference to Figs. 1A to 4. Figs. 1A to 1D are views showing a process of forming a first pattern on a first substrate according to this embodiment, and Figs. 2A to 2C are views showing a process of forming a second pattern by molding the first pattern according to this embodiment with a mold. Figs. 3A to 3B are views showing a process of bonding a first substrate and a second substrate via a second pattern according to this embodiment. Fig. 4 is a view showing a process of forming a first pattern on a first substrate according to a modified example of this embodiment.

[0026] First, as shown in FIG. 1A to FIG. 1D, a first pattern 11 of a curable resin composition is formed on a first substrate 21 by pressure printing. For example, as shown in FIG. 1A, a vacuum pressure printing method using a vacuum pressure printing device 100 and a printing plate 110 is used as the pressure printing method. In the vacuum pressure printing method, as shown in FIG. 1A and FIG. 1B, the pressure printing device 100 is moved over the printing plate 110, the openings of the printing plate 110 are sucked into a vacuum state, and then the curable resin composition is pressed to fill the openings of the printing plate 110 with the curable resin composition. Thereafter, the printing plate 110 is removed, and the first pattern 11 of the curable resin composition is formed on the first substrate 21 as shown in FIG. 1C and FIG. 1D.

[0027] 4, the pressure printing method may be a pressure printing method using a pressure printing device 100 and a printing plate 110. In this pressure printing method, the pressure printing device 100 is moved over the printing plate 110, and pressure is applied to the curable resin composition to fill the openings of the printing plate 110 with the curable resin composition.

[0028] By using the pressurized printing method in this way, even if the thickness of the printing plate (for example, the emulsion of a screen printing plate) is increased, the filling property of the printing plate can be improved. In addition, the viscosity of the adhesive layer material, i.e., the curable resin composition, can be increased, and the sagging of the adhesive layer when the printing plate is removed can be reduced. Therefore, it is easy to realize a thicker adhesive layer, i.e., a thicker pattern of the curable resin composition.

[0029] The curable resin composition may have thixotropy, which can enhance the filling property into the printing plate and reduce sagging of the adhesive layer when the printing plate is removed.

[0030] The openings of the printing plate 110 may be tapered, which can improve the release of the pattern of the curable resin composition from the plate.

[0031] The surface of the printing plate 110 may be treated to be water-repellent. Examples of the water-repellent treatment include coating with a liquid-repellent material such as a fluororesin or silicone resin. This can improve the release of the pattern of the curable resin composition from the plate and can improve the rectangular shape of the pattern of the curable resin composition.

[0032] Next, the first pattern 11 is molded to further control the pattern shape after printing. For example, as shown in FIG. 2A, the first pattern 11 and the mold 120 are aligned, and as shown in FIG. 2B, the mold 120 is pressed against the first pattern 11 to mold it, and as shown in FIG. 2C, the mold is released to form the second pattern 12. It is preferable that the second pattern 12 has a pattern height equal to or lower than that of the first pattern 11. In addition, from the viewpoint of putting the second pattern 12 inside the mold 120, it is preferable that the width of the mold 120 is wider than that of the first pattern 11. With regard to the width and height of the mold 120, it is preferable that the cross-sectional area of ​​the mold 120 is 1 to 2 times the cross-sectional area of ​​the first pattern 11 from the viewpoint of preventing the resin from leaking out of the mold.

[0033] The material constituting the mold is not particularly limited, and examples thereof include metals such as stainless steel, inorganic substances such as glass, and organic substances such as rubber and resin, and two or more of these may be used in combination. In addition, the mold may be surface-treated to improve releasability and durability. Examples of surface treatments include organic coatings such as fluororesins, silicone resins, and PEEK, and metal coatings such as cemented carbide, hard chrome, and DLC.

[0034] The arithmetic mean roughness Ra of the bottom surface of the mold is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. After the shape of the mold is transferred using a RepliSet (manufactured by Struers), the arithmetic mean roughness Ra of the bottom surface of the mold can be measured using a 3D measuring laser microscope.

[0035] Furthermore, mold 120 and substrate 21 may be heated from before mold 120 is pressed against substrate 21 until mold release. The heating temperature is preferably 40° C. to 300° C., and more preferably 40° C. to 150° C. from the viewpoints of removing the solvent and adjusting the physical properties of the cured product.

[0036] When the curable resin composition used as the adhesive layer is a photosensitive resin, it is preferable to further include a step of exposing the first pattern 11 or the second pattern 12 to light. The exposure may be performed after the formation of the first pattern, after the formation of the second pattern, or both, and if the exposure is performed after the formation of the second pattern, it may be performed before or after demolding. By including an exposure step, it is possible to suppress changes in the pattern shape over time.

[0037] As a light source for photocuring (exposing) the curable resin composition, a light source that emits light with the absorption wavelength of the polymerization initiator and sensitizer used may be used, and a light source having a wavelength in the range of 200 nm to 450 nm (e.g., a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a high-power metal halide lamp, a xenon lamp, a carbon arc lamp, or a light-emitting diode) can usually be used.

[0038] In addition, for the purpose of removing the solvent and adjusting the physical properties of the cured product of the curable resin composition, heat may be applied before or after photocuring to a degree that does not reduce the adhesiveness of the cured product of the curable resin composition, so as to perform pre-baking and after-baking. The heating temperature can be appropriately set, but is preferably 40°C to 300°C, more preferably 40°C to 150°C.

[0039] Next, the first substrate 21 and the second substrate 22 are bonded together via the second patterns 12. For example, as shown in FIG. 3A, the first substrate 21 and the second substrate 22 on which the plurality of second patterns 12 are formed are pressure-bonded to obtain a substrate laminate. The pressure-bonding temperature is usually 25°C to 350°C, preferably 60°C to 300°C, and more preferably 80°C to 250°C. The pressure-bonding conditions are usually 0MPa to 50MPa, preferably 0MPa to 40MPa, and more preferably 0MPa to 30MPa. From the viewpoint of improving the adhesive strength, it is preferable to cure the substrate at 80°C to 350°C after pressure-bonding. Then, each pattern is diced to separate the substrate into individual pieces to obtain the substrate laminate shown in FIG. 3B.

[0040] In the above description, an example is described in which the first substrate 21 on which a plurality of patterns are formed and the second substrate 22 are pressure-bonded, but the present invention is not limited to this method. For example, after forming a plurality of second patterns on the first substrate, the individual pieces of the first substrate on which the patterns are formed by dicing may be individually bonded to the second substrate which has been previously diced, or the first substrate which has been previously diced may be rearranged to form a plurality of second patterns, and then the first substrate may be bonded to the second substrate either collectively or individually.

[0041] 2A to 2C may be omitted. In this case, the first substrate 21 and the second substrate 22 may be bonded together via the first substrate 11 in FIG. 3A and FIG. 3B.

[0042] [Curable resin composition] The curable resin composition is a composition containing a curable resin, and the curable resin may be a thermosetting and / or photocurable resin. When the curable resin is a photosensitive resin that is cured by light, it can be brought into a B-stage (semi-cured) state by a photoreaction, and is therefore preferred because it can be easily used as an adhesive layer that constitutes a substrate laminate.

[0043] As the curable resin, a compound having a cationic polymerizable functional group such as an epoxy group, an oxetane group, or a vinyl ether group can be used. Specific examples of the curable resin include novolac phenol type epoxy resin, biphenyl type epoxy resin, dicyclopentadiene type epoxy resin, cyclohexyl epoxy group-containing polyorganosiloxane (cyclic or linear), glycidyl group-containing polyorganosiloxane (cyclic or linear), bisphenol F diglycidyl ether, bisphenol A diglycidyl ether, 2,2'-bis(4-glycidyloxycyclohexyl)propane, 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, vinylcyclohexene dioxide, 2-(3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, vinylcyclohexene dioxide, 2-(3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, vinylcyclohexene dioxide, 2-(3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, vinylcyclohexene dioxide ... bis(3,4-epoxycyclohexane)-5,5-spiro-(3,4-epoxycyclohexyl)adipate, 1,2-cyclopropanedicarboxylic acid bisglycidyl ester, triglycidyl isocyanurate, monoallyl diglycidyl isocyanurate, diallyl monoglycidyl isocyanurate, 1,4-bis{(3-ethyl-3-oxetanyl)methoxy}methyl}benzene, bis{1-ethyl(3-oxetanyl)}methyl ether, 3-ethyl-3-(phenoxymethyl)oxetane, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, and the like.

[0044] From the viewpoint of stability, the cationic polymerizable functional group is preferably an epoxy group, more preferably a glycidyl group and / or an alicyclic epoxy group, and even more preferably an alicyclic epoxy group. The curable resin preferably has two or more cationic polymerizable functional groups, more preferably three or more. When the curable resin has three or more cationic polymerizable functional groups, a cured product having high crosslink density and excellent heat resistance can be obtained. The multiple cationic polymerizable functional groups of the curable resin may be the same or different. The content of the cationic polymerizable group in the solid content of the curable resin composition is preferably 1% by weight or more and 99% by weight or less, more preferably 5% by weight or more and 90% by weight or less.

[0045] The curable resin is preferably a polysiloxane compound from the viewpoints of heat resistance during reflow and reduction of outgassing. The polysiloxane compound has a siloxane bond (-Si-O-), but has a T unit (XSiO 3 / 2 ) or Q units with four oxygen atoms bonded to a silicon atom (SiO 4 / 2 The higher the content of XSiO, the harder the cured product will be and the more reliable its heat resistance will be. Polysiloxane compounds also contain M units (XSiO 1 / 2 ) or D units with two oxygen atoms bonded to a silicon atom (XSiO 2 / 2 The higher the content of ), the softer and less stressed the cured product will be. From the viewpoint of compatibility with other components, it is preferable that the polysiloxane compound has a cationically polymerizable group.

[0046] From the viewpoint of adjusting workability, reactivity, adhesiveness, and strength of the cured product, the curable resin composition preferably further contains a crosslinking agent having two or more photopolymerizable functional groups other than cationic polymerizable functional groups. The crosslinking agent is not particularly limited, but examples thereof include an alkoxysilane compound and a (meth)acrylate compound.

[0047] The curable resin composition preferably further comprises a photoacid generator. The photoacid generator is not particularly limited as long as it is a compound capable of generating an acid capable of curing the curable resin by irradiation with active energy rays. The pKa of the acid generated by the photoacid generator is not particularly limited, but is, for example, less than 3, preferably less than 1.

[0048] The photoacid generator is not particularly limited, and a known photoacid generator can be used (for example, see JP-A-2000-1648, JP-T-2001-515533, and WO-2002 / 83764). Among these, sulfonate esters, carboxylate esters, and onium salts are preferred, and onium salts are more preferred.

[0049] Examples of the sulfonate esters include disulfones, disulfonyldiazomethanes, disulfonylmethanes, sulfonylbenzoylmethanes, imide sulfonates such as trifluoromethylsulfonate derivatives, benzoin sulfonates, sulfonates of 1-oxy-2-hydroxy-3-propyl alcohol, pyrogallol trisulfonates, and benzyl sulfonates, and two or more of these may be used in combination.

[0050] Carboxylic acid esters can also be used in the same manner as sulfonate esters.

[0051] In general, sulfonate esters and carboxylate esters may require a heating step, for example to a temperature of from 50° C. to 100° C., in order to liberate the acid.

[0052] The onium salt is not particularly limited, but examples thereof include sulfonium salts, iodonium salts, etc. Among these, aromatic sulfonium salts are preferred from the viewpoint of absorption wavelength.

[0053] The counter ion of the onium salt is, for example, tetrafluoroborate (BF4 - ), hexafluorophosphate (PF6 - ), hexafluoroantimonate (SbF6 - ), hexafluoroarsenate (AsF6 - ), hexachloroantimonate (SbCl6 - ), tetraphenylborate, tetrakis(trifluoromethylphenyl)borate, tetrakis(pentafluoromethylphenyl)borate, fluoroalkyl fluorophosphate, perchlorate ion (ClO4 - ), trifluoromethanesulfonate ion (CF3SO3 - ), fluorosulfonate ion (FSO3 - ), toluenesulfonate ion, trinitrobenzenesulfonate ion, trinitrotoluenesulfonate ion, etc.

[0054] The content of the photoacid generator in the curable resin composition is not particularly limited, but from the viewpoint of the balance between the curing speed and the physical properties of the cured product, it is preferably 0.1 parts by weight or more and 20 parts by weight or less, and more preferably 0.5 parts by weight or more and 10 parts by weight or less, relative to 100 parts by weight of the curable resin. When the content of the photoacid generator in the curable resin composition is 0.1 parts by weight or more relative to 100 parts by weight of the curable resin, the curing time is shortened and a sufficiently cured cured product is obtained, and when it is 20 parts by weight or less, coloration of the cured product is suppressed and the heat resistance or light resistance of the cured product is improved.

[0055] The curable resin composition may further contain a basic compound from the viewpoint of controlling the curing rate and improving storage stability.

[0056] The curable resin composition may further contain a sensitizer. This improves the sensitivity of the curable resin composition to light such as visible light. In addition, a curable resin composition having sensitivity to light of long wavelengths such as g-line (436 nm), h-line (405 nm) and i-line (365 nm) can be obtained. The curability of the curable resin composition can be adjusted by using a sensitizer and a photoacid generator in combination.

[0057] The sensitizer is not particularly limited, but examples thereof include anthracene-based compounds and thioxanthone-based compounds, and two or more of these may be used in combination.

[0058] The curable resin composition may further contain an adhesion improver. Examples of the adhesion improver include adhesives and coupling agents, and two or more of these may be used in combination.

[0059] The adhesive is not particularly limited, but examples thereof include epoxy compounds, oxetane compounds, phenolic resins, coumarone-indene resins, rosin ester resins, terpene-phenolic resins, α-methylstyrene-vinyl toluene copolymers, polyethylmethylstyrene, aromatic polyisocyanates, and the like.

[0060] The coupling agent is not particularly limited, but may be, for example, a silane coupling agent. The silane coupling agent is not particularly limited as long as it is a compound having at least one functional group reactive to an organic group and at least one silicon atom-containing group having hydrolysis. As the group reactive to an organic group, from the viewpoint of handling, an epoxy group, a methacryl group, an acrylic group, an isocyanate group, an isocyanurate group, a vinyl group, and a carbamate group are preferred, and from the viewpoint of curing and adhesion, an epoxy group, a methacryl group, and an acrylic group are particularly preferred. As the silicon atom-containing group having hydrolysis, from the viewpoint of handling, an alkoxysilyl group is preferred, and from the viewpoint of reactivity, a methoxysilyl group and an ethoxysilyl group are particularly preferred.

[0061] The content of the adhesion improver in the curable resin composition is preferably 0.1 parts by weight or more and 20 parts by weight or less, more preferably 0.3 parts by weight or more and 10 parts by weight or less, and even more preferably 0.5 parts by weight or more and 5 parts by weight or less, relative to 100 parts by weight of the curable resin. When the content of the adhesion improver in the curable resin composition is 0.1 parts by weight or more relative to 100 parts by weight of the curable resin, the effect of the adhesion improver is obtained, and when it is 20 parts by weight or less, the curability of the curable resin composition and the physical properties of the cured product are improved.

[0062] The curable resin composition may further contain a thermoplastic resin.

[0063] The thermoplastic resin is not particularly limited, and examples thereof include polymethyl methacrylate-based resins such as homopolymers of methyl methacrylate, random, block or graft polymers of methyl methacrylate and other monomers (e.g., Optretz (Hitachi Chemical Co., Ltd.)), acrylic resins such as polybutyl acrylate-based resins such as homopolymers of butyl acrylate, random, block or graft polymers of butyl acrylate and other monomers, polycarbonate-based resins such as polycarbonates having a structure derived from monomers such as bisphenol A and 3,3,5-trimethylcyclohexylidene bisphenol (e.g., APEC (Teijin Co., Ltd.)), homopolymers or copolymers of norbornene derivatives, vinyl monomers, and cycloolefin-based resins such as resins obtained by ring-opening metathesis polymerization of norbornene derivatives or hydrogenated products thereof (e.g., APEL (Teijin Co., Ltd.)). Examples of the resin include olefin-maleimide resins such as copolymers of ethylene and maleimide (e.g., TIPAS (manufactured by Tosoh Corporation)), polyester resins such as polyesters obtained by polycondensation of bisphenols (e.g., bisphenol A, bis(4-(2-hydroxyethoxy)phenyl)fluorene, etc.) or diols (e.g., diethylene glycol, etc.) with phthalic acids (e.g., terephthalic acid, isophthalic acid, etc.) or aliphatic dicarboxylic acids (e.g., O-PET (manufactured by Kanebo Corporation)), polyethersulfone resins, polyarylate resins, polyvinyl acetal resins, polyethylene resins, polypropylene resins, polystyrene resins, polyamide resins, silicone resins, fluororesins, natural rubber, rubber-like resins such as EPDM, and the like, and two or more of these may be used in combination.

[0064] The thermoplastic resin may have a crosslinkable group. The crosslinkable group is not particularly limited, but may be, for example, an epoxy group, an amino group, a radically polymerizable unsaturated group, a carboxyl group, an isocyanate group, a hydroxyl group, or an alkoxysilyl group. From the viewpoint of the heat resistance of the cured product, it is preferable that the thermoplastic resin has an average of one or more crosslinkable groups.

[0065] From the viewpoint of compatibility with the polysiloxane compound, the number average molecular weight of the thermoplastic resin is preferably 10,000 or less, more preferably 5,000 or less. On the other hand, from the viewpoint of toughness of the cured product, the number average molecular weight of the thermoplastic resin is preferably 10,000 or more, more preferably 100,000 or more. From the viewpoint of viscosity and moldability of the curable resin composition, the molecular weight distribution of the thermoplastic resin is preferably 3 or less, more preferably 2 or less, and even more preferably 1.5 or less.

[0066] The content of the thermoplastic resin in the curable resin composition is preferably 5% by weight or more and 50% by weight or less, and more preferably 10% by weight or more and 30% by weight or less. When the content of the thermoplastic resin in the curable resin composition is 5% by weight or more, the toughness of the cured product is improved, and when it is 50% by weight or less, the heat resistance (elastic modulus at high temperatures) of the cured product is improved.

[0067] The curable resin composition may further contain a filler, an antioxidant, a radical polymerization inhibitor, a solvent, and the like, as necessary.

[0068] The filler is not particularly limited, but examples thereof include silica-based fillers (e.g., quartz, fume silica, precipitated silica, silicic anhydride, fused silica, crystalline silica, ultrafine amorphous silica, etc.), silicon nitride, silver powder, alumina, aluminum hydroxide, titanium oxide, glass fiber, carbon fiber, mica, carbon black, graphite, diatomaceous earth, clay, talc, calcium carbonate, magnesium carbonate, barium sulfate, inorganic fillers such as inorganic balloons, epoxy-based fillers, and the like.

[0069] The antioxidant is not particularly limited, but examples thereof include hindered phenol-based antioxidants, citric acid, phosphoric acid, and sulfur-based antioxidants, and two or more of these may be used in combination.

[0070] The radical polymerization inhibitor is not particularly limited, but examples thereof include phenolic radical inhibitors such as 2,6-di-t-butyl-3-methylphenol (BHT), 2,2'-methylene-bis(4-methyl-6-t-butylphenol), and tetrakis(methylene-3(3,5-di-t-butyl-4-hydroxyphenyl)propionate)methane; and amine radical inhibitors such as phenyl-β-naphthylamine, α-naphthylamine, N,N'-sec-butyl-p-phenylenediamine, phenothiazine, and N,N'-diphenyl-p-phenylenediamine; and two or more of these may be used in combination.

[0071] The solvent is not particularly limited, but examples thereof include hydrocarbon solvents such as benzene, toluene, hexane, and heptane; ether solvents such as tetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, and diethyl ether; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; glycol solvents such as propylene glycol-1-monomethyl ether-2-acetate (PGMEA), ethylene glycol diethyl ether, and diethylene glycol diethyl ether; halogen-based solvents such as chloroform, methylene chloride, and 1,2-dichloroethane; ester solvents such as butyl acetate and isobutyl isobutyrate; and lactone solvents such as γ-butyrolactone, ε-caprolactone, and δ-valerolactone, and two or more of these may be used in combination.

[0072] The content of the solvent in the curable resin composition is not particularly limited, but is, for example, 0.001 mL or more and 10 mL or less per 1 g of the solid content of the curable resin composition.

[0073] The curable resin composition may further contain a colorant, a release agent, a flame retardant, a flame retardant auxiliary, a surfactant, an antifoaming agent, an emulsifier, a leveling agent, an anti-repellent agent, an ion trapping agent (antimony-bismuth, etc.), a thixotropy imparting agent, a tackifier, a storage stability improving agent, an ozone degradation inhibitor, a light stabilizer, a thickener, a plasticizer, a reactive diluent, an antioxidant, a heat stabilizer, an electrical conductivity imparting agent, an antistatic agent, a radiation shielding agent, a nucleating agent, a phosphorus-based peroxide decomposer, a lubricant, a pigment, a metal deactivator, a thermal conductivity imparting agent, a physical property adjusting agent, and the like.

[0074] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and the above embodiment may be modified as appropriate within the scope of the spirit of the present invention. [Explanation of symbols]

[0075] 11 First Pattern 12 Second Pattern 21 First board 22 Second board 100 Pressure printing device (vacuum pressure printing device) 110 Print Edition 120 Mold

Claims

1. forming a first pattern of a curable resin composition on a first substrate using a pressure printing method; bonding the first substrate and the second substrate together via the first pattern; A method for manufacturing a substrate laminate, comprising:

2. The method further includes forming a second pattern by molding the first pattern using a mold after the step of forming the first pattern, The bonding step includes bonding the first substrate and the second substrate via the second pattern. A method for producing the substrate laminate according to claim 1 .

3. The method for manufacturing a substrate laminate according to claim 1 or 2, wherein the pressure printing method is a vacuum pressure printing method.

4. one of the first substrate and the second substrate is a semiconductor device substrate, The other of the first substrate and the second substrate is a transparent substrate. A method for producing the substrate laminate according to claim 1 or 2.

5. The method for producing a substrate laminate according to claim 1 , wherein the curable resin composition contains at least one of a glycidyl group and an alicyclic epoxy group.

6. The method for producing a substrate laminate according to claim 1 , wherein the curable resin composition contains a polysiloxane compound.

7. The method for producing a substrate laminate according to claim 1 , wherein the curable resin composition contains a photosensitive resin.

8. The method for manufacturing a substrate laminate according to claim 1 , further comprising the step of exposing to the first pattern.

9. The method for manufacturing a substrate laminate according to claim 2 , further comprising the step of exposing to the second pattern.

Citation Information

Patent Citations

  • Wafer sealing method for CMOS image sensor

    JP2013115104A