Composition for bonded magnet, bonded magnet, and integrally-molded component
A bonded magnet composition with a unique microstructure of Sm-Fe-N particles surrounded by polyamide resin and embedded in polyamide elastomer matrix addresses thermal shock issues, ensuring high resistance and adhesion with metal parts.
Patent Information
- Application Number
- JP2023055371
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Bonded magnets used in combination with metal parts often fail thermal shock tests due to differences in linear expansion coefficients, leading to cracking or separation at the adhesive interface.
A bonded magnet composition containing samarium-iron-nitrogen magnet powder and a thermoplastic resin binder, comprising a polyamide elastomer and polyamide resin, with a specific microstructure where Sm-Fe-N particles are surrounded by a polyamide resin layer and embedded in a polyamide elastomer matrix, enhancing cold and thermal shock resistance.
The composition achieves high thermal shock resistance, preventing cracking and separation, while maintaining excellent magnetic properties and mechanical strength, suitable for integrally molded parts with metal components.
Smart Images

Figure 2024142948000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a bonded magnet composition, a bonded magnet, and a unitarily molded part. [Background technology]
[0002] Bonded magnets are produced by heating and kneading a composition containing magnet powder and binder components such as organic resin in a kneading machine such as an extruder, processing it into a shape such as pellets, and then hot molding it using a technique such as injection molding, compression molding, or extrusion molding.
[0003] Compared to sintered magnets, such bonded magnets have the advantage that they have high dimensional accuracy and are easy to produce in complex shapes. They also have high uniformity in quality and performance, good yields, and good machinability. In particular, magnets manufactured by injection molding using thermoplastic resins as binder resins have the advantage of high dimensional accuracy and no need for post-processing, reducing the manufacturing costs of the magnets. Furthermore, bonded magnets containing rare earth magnet powder have excellent magnetic properties (residual magnetic flux density Br, coercive force iHc, and maximum energy product (BH)max) and strong magnetic force. As a result, they can be made smaller and have higher properties, making them useful for applications such as small motors and sensors.
[0004] Thermoplastic resin binders such as polyamide resin and polyphenylene sulfide (PSS) resin are widely used as binder components for bonded magnets, and among these, polyamide resin is considered to be particularly preferable in terms of mechanical strength, weather resistance, etc. On the other hand, the use of a resin composition containing a polyamide elastomer and a polyamide resin has also been proposed.
[0005] For example, Patent Document 1 discloses a nylon resin composition consisting of 80 to 95% by weight of magnetic powder and 20 to 5% by weight of binder resin, in which the binder resin is 80 to 95% by weight of a resin composition and 20 to 5% by weight of a plasticizer, and the resin composition is 0 to 100% by weight (excluding 0% by weight) of a polyamide-based elastomer and 0 to 100% by weight (excluding 100% by weight) of a polyamide (Claim 1 of Patent Document 1).
[0006] Patent Document 2 discloses a resin composition characterized by including a polyamide-based elastomer containing 50% by weight or more of a polyetheramide elastomer (X) obtained by polymerizing a component containing a specific diamine compound (A), a polyamide-forming monomer (B), and a dicarboxylic acid compound (C), and containing, as coexisting components, (a) a thermoplastic resin, and (b) at least one of a flame retardant and a magnetic powder (C) (Claim 1 of Patent Document 2). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2004-352792 A [Patent Document 2] International Publication No. 2008 / 123450 Summary of the Invention [Problem to be solved by the invention]
[0008] Bonded magnets are often used as integrally molded parts by combining them with metal parts. Specifically, bonded magnets are combined with metal parts by adhesive bonding or insert molding to create integrally molded parts, and are used in this form. However, bonded magnets and metal parts have different linear expansion coefficients. Therefore, when integrally molded parts are subjected to thermal shock tests, problems such as cracks occurring in the bonded magnet or the adhesive peeling off and the bonded magnet and metal part becoming separated are likely to occur. For this reason, bonded magnets are desired to have excellent durability (resistance to thermal shock) in thermal shock tests.
[0009] In the past, improvements have been made to bonded magnets and compositions for bonded magnets used in the manufacture of these bonded magnets in order to improve their resistance to thermal shocks. However, conventional bonded magnets and compositions for bonded magnets have had limitations in meeting this demand.
[0010] The present inventors have conducted extensive research in light of these problems, and as a result have discovered that in a bonded magnet composition containing samarium-iron-nitrogen magnet powder and a thermoplastic resin binder, by using a polyamide elastomer and a polyamide resin as the thermoplastic resin binder, and by controlling the distribution of the magnet powder, the polyamide elastomer, and the polyamide resin, and imparting a unique microstructure to the bonded magnet composition, it is possible to obtain a bonded magnet that is particularly excellent in resistance to cold and thermal shocks.
[0011] The present invention was completed based on such findings, and aims to provide a bonded magnet composition that can produce a bonded magnet with particularly excellent resistance to cold and thermal shocks. Another aim of the present invention is to provide a bonded magnet having a molded body of the bonded magnet composition, and an integrally molded part having the bonded magnet. [Means for solving the problem]
[0012] The present invention encompasses the following aspects (1) to (12). In this specification, the expression "to" includes both ends of the expression. In other words, "X to Y" is synonymous with "X or more and Y or less."
[0013] (1) A magnet containing samarium-iron-nitrogen magnet powder and a thermoplastic resin binder; the thermoplastic resin binder comprises a polyamide elastomer and a polyamide resin; a ratio of the amount of polyamide elastomer to the total amount of polyamide elastomer and polyamide resin contained in the thermoplastic resin binder is 50% by mass or more and 80% by mass or less; A composition for bonded magnets, in which at least some of the particles constituting the samarium-iron-nitrogen based magnet powder are surrounded by a resin layer mainly composed of polyamide resin, and a matrix resin mainly composed of polyamide elastomer is present in the gaps between the particles surrounded by the resin layer.
[0014] (2) The composition for bonded magnets according to (1) above, wherein the ratio of the amount of polyamide elastomer to the total amount of polyamide elastomer and polyamide resin contained in the thermoplastic resin binder is 70% by mass or more and 80% by mass or less.
[0015] (3) The bonded magnet composition according to (1) or (2) above, wherein the samarium-iron-nitrogen based magnet powder has an average particle size of 1.8 μm or more and 3.3 μm or less.
[0016] (4) A composition for a bonded magnet according to any one of (1) to (3) above, wherein the content of samarium-iron-nitrogen based magnet powder contained in said composition for a bonded magnet is 88.0% by mass or more and 91.0% by mass or less.
[0017] (5) A composition for a bonded magnet according to any one of the above (1) to (4), wherein the polyamide elastomer has a tensile breaking elongation of 400% or more and a flexural modulus of elasticity of 100 MPa or more.
[0018] (6) A composition for a bonded magnet according to any one of the above (1) to (5), wherein the polyamide resin is a polyamide 12 resin.
[0019] (7) A composition for a bonded magnet according to any one of (1) to (6) above, wherein the polyamide resin has a weight average molecular weight Mw of 4,500 or more and 7,500 or less, as determined by molecular weight distribution measurement.
[0020] (8) A composition for a bonded magnet according to any one of (1) to (7) above, further comprising carbon fibers.
[0021] (9) A composition for a bonded magnet according to any one of (1) to (8) above, further comprising a carboxylate ester.
[0022] (10) The samarium-iron-nitrogen magnet powder is SmFe 17 A composition for a bonded magnet according to any one of the above (1) to (9), having a composition represented by N3.
[0023] (11) A bonded magnet comprising a molded article of the bonded magnet composition according to any one of (1) to (10) above.
[0024] (12) An integrally molded part comprising the bonded magnet of (11) above and a metal part. Effect of the Invention
[0025] According to the present invention, there is provided a bonded magnet composition capable of producing a bonded magnet having particularly excellent resistance to thermal shock. Also, according to the present invention, there is provided a bonded magnet having a molded body of the bonded magnet composition, and an integrally molded part having the bonded magnet. [Brief description of the drawings]
[0026] [Figure 1] An AFM image of a cross section of a bonded magnet is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] A specific embodiment of the present invention (hereinafter, referred to as the present embodiment) will be described. Note that the present invention is not limited to the following embodiment, and various modifications are possible within the scope of the present invention.
[0028] <<1. Bonded magnet composition The bonded magnet composition of this embodiment includes a samarium-iron-nitrogen magnet powder and a thermoplastic resin binder. The thermoplastic resin binder includes a polyamide elastomer and a polyamide resin, and the ratio of the amount of polyamide elastomer to the total amount of the polyamide elastomer and polyamide resin contained in the thermoplastic resin binder is 50% by mass or more and 80% by mass or less. Furthermore, at least some of the particles constituting the samarium-iron-nitrogen magnet powder are surrounded by a resin layer mainly composed of polyamide resin, and a matrix resin mainly composed of polyamide elastomer is present in the gaps between the particles surrounded by the resin layer.
[0029] A bonded magnet composition (hereinafter sometimes simply referred to as "composition") is a precursor of a bonded magnet. That is, the composition is molded under heating using a method such as injection molding or extrusion molding to produce a bonded magnet. The bonded magnet may be anisotropic or isotropic. If a magnetic field is applied to the composition during molding, an anisotropic magnet can be produced, and if a magnetic field is not applied, an isotropic magnet can be obtained.
[0030] [1] Magnet powder The bonded magnet composition of this embodiment contains samarium-iron-nitrogen (Sm-Fe-N; SFN) based magnet powder (hereinafter sometimes simply referred to as "magnet powder"). The magnet powder is the powder that is the main component of the magnetic properties of the bonded magnet. Sm-Fe-N based magnet powder is a type of rare earth transition metal based magnet powder, and is known as a high-performance, inexpensive magnet powder. Sm-Fe-N based magnet powder is composed of Sm2Fe 17 N x When x=3, that is, Sm2Fe 17 The saturation magnetization is maximized when the composition is Sm2FeN3. This makes it possible to increase the magnetic flux density of the resulting bonded magnet. Therefore, the Sm-Fe-N magnet powder is 17It is preferable that the composition has a composition represented by N3. Note that the powder refers to an aggregate of a plurality of particles that exhibits fluidity as a whole. It can also be said that a plurality of particles that exhibit fluidity as a whole constitutes a powder.
[0031] The average particle size of the Sm-Fe-N magnet powder is not limited. However, the average particle size is preferably 1.8 μm or more and 3.3 μm or less. By increasing the average particle size to 1.8 μm or more, the decrease in the fluidity and moldability of the composition can be suppressed, and the oxidation of the magnet powder and the associated risk of fire can be reduced. In addition, the Sm-Fe-N magnet powder has a nucleation-type coercive force generation mechanism. By decreasing the average particle size to 3.3 μm or less, the coercive force can be improved.
[0032] The average particle size can be determined by observing the magnet powder with a scanning electron microscope (SEM). The magnet powder can be determined by treating the bonded magnet composition or the bonded magnet with a solvent such as hexafluoroisopropanol to dissolve and remove the resin, and then removing the reinforcing agent by magnetic separation. Alternatively, the magnet powder used to manufacture the bonded magnet composition can be directly subjected to SEM observation. More specifically, this can be performed in accordance with the method in the examples described below.
[0033] The content of Sm-Fe-N magnet powder in the bonded magnet composition is not limited. However, the content is preferably 88.0% by mass or more and 91.0% by mass or less. By increasing the content to 88.0% by mass or more, the magnetic properties of the obtained bonded magnet, especially the magnetic flux density, are further improved. In addition, the resin content is reduced, so the linear expansion coefficient of the bonded magnet is reduced. Therefore, when the bonded magnet is applied to an integrally molded part, the difference in the linear expansion coefficient with the metal part is suppressed, and as a result, the cold and thermal shock resistance is further improved. On the other hand, by suppressing the content to 91.0% by mass or less, it is possible to increase the fluidity of the bonded magnet. The moldability of the bonded magnet is improved, and problems such as the bonded magnet being unable to be molded or the molded body (bonded magnet) having poor appearance such as welds can be suppressed. The content of Sm-Fe-N magnet powder is more preferably 88.0% by mass or more and 90.0% by mass or less.
[0034] Known methods for manufacturing Sm-Fe-N magnet powder include the melting method and the reduction diffusion method. In the melting method, metal powder containing iron (Fe) and samarium (Sm) is used as the raw material, which is heated and melted at a temperature of 1500°C or higher in a furnace such as a high-frequency furnace or an arc furnace. The resulting product is then crushed and further heat-treated to homogenize the composition to produce an Sm-Fe master alloy. The resulting master alloy is then nitrided to produce magnet powder.
[0035] In contrast, in the reduction diffusion method, a mixture of samarium oxide (Sm2O3), iron raw materials (Fe, Fe2O3, etc.), and a reducing agent (Ca, etc.) is heated to obtain a master alloy, which is then nitrided to produce magnet powder. Sm-Fe-N magnet powder has a nucleation-type coercive force generation mechanism. To obtain high coercive force, it is desirable to make the particles fine. Therefore, it is desirable to prepare fine Sm-Fe-N magnet powder by finely grinding the nitrided master alloy or by using fine raw materials.
[0036] Preferably, the Sm-Fe-N magnet powder is produced by a reduction-diffusion method. The reduction-diffusion method, which uses inexpensive oxide raw materials (such as Sm2O3), has the advantage of reducing raw material costs. In addition, magnet powder with fewer impurities can be obtained compared to the melting method. In contrast, the melting method involves extremely complicated steps. In addition, since the product is exposed to the air between each step, there is a risk of impurities being generated on the product surface due to oxidation. If the product surface is oxidized, nitriding will not proceed uniformly, and the properties of the resulting magnet powder, particularly magnetic properties such as saturation magnetization, coercive force, and / or squareness, will deteriorate, and the maximum energy product of the bonded magnet obtained as a result may decrease.
[0037] In the reduction diffusion method, a samarium raw material (Sm2O3), an iron raw material (Fe, etc.), and a reducing agent (Ca, etc.) are first reduced to obtain a reduction product containing a Sm-Fe alloy. Next, this reduction product is subjected to a wet treatment to remove by-products derived from the reducing agent contained in the reduction product (CaO, Ca(OH)2, etc.). The resulting Sm-Fe alloy is then nitrided in a mixed gas flow containing ammonia and hydrogen. The resulting nitride is crushed and dried to obtain Sm-Fe-N magnet powder.
[0038] Sm-Fe-N magnet powder is Sm2Fe 17 In the case of the N3 alloy, it is preferable to pulverize the coarse powder. That is, since the magnetic alloy coarse powder having an average particle size exceeding 20 μm has low magnetic properties, it is preferable to pulverize it in an organic solvent. During or after pulverization, the magnet powder may be put into a solution containing a surface treatment agent such as phosphoric acid and stirred to provide a coating such as a composite phosphate coating on the magnet powder surface. For pulverization, a known pulverizing device applicable to magnet powder pulverization may be used. Among these, a wet pulverizing device such as a media stirring mill or a bead mill is particularly suitable because it is easy to obtain a uniform powder composition and particle size. In addition, organic solvents such as isopropyl alcohol, ethanol, toluene, methanol, and hexane are preferable as the pulverization solvent. After pulverization, the pulverization may be filtered and dried using a filter with a predetermined opening.
[0039] The Sm-Fe-N magnet powder may be surface-treated with a coupling agent, such as a silane-based coupling agent, a titanium-based coupling agent, or an aluminum-based coupling agent, and is particularly preferably surface-treated with a silane-based coupling agent.
[0040] [2] Thermoplastic resin binder The bonded magnet composition of this embodiment contains a thermoplastic resin binder. The thermoplastic resin binder contains a polyamide elastomer and a polyamide resin. When the thermoplastic binder is heated during kneading or molding, it plasticizes and gives the composition fluidity. When cooled after molding, it solidifies. Therefore, it functions to bind the magnet powder and maintain the shape retention of the bonded magnet.
[0041] The content of the thermoplastic resin binder contained in the bonded magnet composition is not limited. However, the content is preferably 7.0% by mass or more and 11.0% by mass or less. By increasing the content to 7.0% by mass or more, it is possible to increase the fluidity of the bonded magnet composition. On the other hand, by keeping the content to 11.0% by mass or less, the linear expansion coefficient of the resulting bonded magnet is reduced, further improving the resistance to cold and thermal shock.
[0042] (A) Polyamide elastomer The polyamide elastomer may have a polyamide segment and a polyether segment. The polyamide elastomer preferably has a tensile elongation at break of 400% or more and a flexural modulus of 100 MPa or more. By using a polyamide elastomer having such a tensile elongation at break and flexural modulus, the flowability of the bonded magnet composition is improved and the thermal shock resistance is further improved. The tensile elongation at break is measured by the method specified in ISO527. The flexural modulus is measured by the method specified in ISO178.
[0043] (B) Polyamide resin As the polyamide resin, various resins such as polyamide 12 resin, polyamide 11 resin, polyamide 6 resin, etc. can be used. Among these, it is preferable that the polyamide resin is polyamide 12 resin. By using polyamide 12 resin, the flowability of the bonded magnet composition becomes good and the moldability becomes particularly high. In addition, by using polyamide 12 resin, the strength of the obtained bonded magnet is further increased.
[0044] The polyamide resin preferably has a weight average molecular weight Mw of 4500 or more and 7500 or less, as measured by molecular weight distribution. By increasing Mw to 4500 or more, the mechanical strength of the resulting bonded magnet is further increased. On the other hand, by keeping Mw to 7500 or less, the fluidity of the bonded magnet composition is improved. Mw is more preferably 5000 or more and 6000 or less. The weight average molecular weight Mw is determined by molecular weight distribution measurement under conditions similar to those in the examples.
[0045] In the bonded magnet composition of this embodiment, at least some of the particles (Sm-Fe-N particles) constituting the Sm-Fe-N magnetic powder are surrounded by a resin layer mainly composed of polyamide resin. Also, a matrix resin mainly composed of polyamide elastomer is present in the gaps between the particles (coated particles) surrounded by the resin layer. That is, the resin layer mainly composed of polyamide resin surrounds the Sm-Fe-N particles, which are in turn surrounded by a matrix resin mainly composed of polyamide elastomer. Alternatively, it can be said that the composition has a sea-island structure in which the matrix resin constitutes the sea portion and the coated particles constitute the island portion.
[0046] By imparting such a unique microstructure to the bonded magnet composition, the thermal shock resistance of the resulting bonded magnet is significantly improved. Although not limited to the above, the following points are considered as the mechanism. That is, polyamide elastomer has a small Young's modulus and a large fracture strain. Therefore, it has viscoelastic properties. By dispersing Sm-Fe-N particles in the polyamide elastomer having viscoelastic properties, it is expected that the stress is relieved and the thermal shock resistance is improved. However, the adhesion between the Sm-Fe-N particles and the polyamide elastomer is low. Therefore, in a system consisting of only polyamide elastomer and Sm-Fe-N particles, when an impact is applied, separation occurs at the interface between the Sm-Fe-N particles and the polyamide elastomer, and the mechanical strength of the entire bonded magnet is reduced. Therefore, it is not possible to actually improve the thermal shock resistance.
[0047] In contrast, polyamide resin has a strong adhesive force to both Sm-Fe-N particles and polyamide elastomer. By interposing polyamide resin between Sm-Fe-N particles and polyamide elastomer, it is possible to utilize the stress relaxation function of polyamide elastomer without causing a decrease in mechanical strength due to interfacial separation. As a result, it is believed that the cold and thermal shock resistance is significantly improved.
[0048] The matrix resin has a stress relaxation function. The matrix resin is mainly composed of a polyamide elastomer. That is, the component that occupies the largest mass ratio in the matrix resin is the polyamide elastomer. As long as the matrix resin is mainly composed of a polyamide elastomer, it does not exclude the inclusion of other components, for example, polyamide resin. However, in order to fully exert the stress relaxation function, it is preferable that the ratio of polyamide elastomer contained in the matrix resin is high.
[0049] On the other hand, the resin layer acts as an interface bonding layer connecting the Sm-Fe-N particles and the matrix resin (resin mainly composed of polyamide elastomer). The resin layer is mainly composed of polyamide resin. That is, the component that occupies the largest mass ratio in the resin layer is polyamide resin. As long as the resin layer is mainly composed of polyamide resin, it does not exclude the inclusion of other components, such as polyamide elastomer. However, in order to fully exert the function as an interface bonding layer, it is preferable that the proportion of polyamide resin contained in the resin layer is high.
[0050] It is sufficient that at least a part of the Sm-Fe-N particles is surrounded by the resin layer. However, from the viewpoint of utilizing the function of the resin layer as an interface bonding layer, the higher the ratio of particles surrounded by the resin layer, the better. The ratio of particles surrounded by the resin layer is preferably 50% by number or more, more preferably 70% by number or more, and even more preferably 90% by number or more.
[0051] In the bonded magnet composition of the present embodiment, the ratio of the polyamide elastomer to the total amount of the polyamide elastomer and polyamide resin contained in the thermoplastic resin binder (elastomer ratio) is 50% by mass or more and 80% by mass or less. By limiting the elastomer ratio within such a range, the formation of the above-mentioned fine structure (sea-island structure) can be promoted. If the elastomer ratio is less than 50% by mass, the ratio of the matrix resin (sea portion) is too small, so that the bonding between the coated particles (island portion) progresses. Therefore, the stress relaxation function based on the matrix resin does not work sufficiently, and the thermal shock resistance decreases. In addition, the fluidity of the composition decreases, and moldability may be impaired. On the other hand, if the elastomer ratio is more than 80% by mass, the ratio of the resin layer is too small, so that the problem of poor adhesion between the Sm-Fe-N particles and the matrix resin occurs, and the thermal shock resistance also decreases. From the viewpoint of improving the fluidity while maintaining excellent thermal shock resistance, the elastomer ratio is preferably 60% by mass or more and 80% by mass or less, and more preferably 70% by mass or more and 80% by mass or less.
[0052] The thermoplastic resin binder may be composed of only polyamide elastomer and polyamide resin, or may contain other resin components. However, in order to fully utilize the stress relaxation function and the function of the interface bonding layer possessed by the polyamide elastomer and polyamide resin, the higher the proportion of the polyamide elastomer and polyamide resin, the more preferable. The proportion of the polyamide elastomer and polyamide resin in the thermoplastic resin binder is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more.
[0053] [3] Strengthener The bonded magnet composition may contain carbon fiber as a reinforcing agent. Generally, various reinforcing agents such as carbon flakes and glass fibers are known. However, by using carbon fiber, the tensile strength of the resulting bonded magnet can be effectively increased. In the bonded magnet composition of this embodiment, it is preferable to use carbon fiber with a fiber diameter of 5 μm or more and 12 μm or less. By including carbon fiber with such a fiber diameter, it is possible to increase the strength of the bonded magnet, increase the fluidity of the composition, and improve moldability. From the viewpoint of increasing the strength, the fiber diameter of the carbon fiber is more preferably 5 μm or more and 8 μm or less.
[0054] The carbon fiber (reinforcing agent) content in the bonded magnet composition is preferably 0.5% by mass or more and 2.0% by mass or less. By increasing the content to 0.5% by mass or more, the strength of the bonded magnet increases, and it becomes possible to further improve resistance to cold and thermal shocks. From the viewpoint of improving resistance to cold and thermal shocks, the content is more preferably 0.7% by mass or more. On the other hand, by keeping the content to 2.0% by mass or less, the fluidity of the bonded magnet composition is further increased. From the viewpoint of improving fluidity, the content is more preferably 1.5% by mass or less.
[0055] [4] Additives The bonded magnet composition may contain a carboxylic acid ester as an additive. Examples of the carboxylic acid ester include sebacic acid ester and / or adipic acid ester. In order to increase the fluidity during molding, additives such as lubricants such as hydrocarbons or fatty acids and plasticizers such as various esters are generally used. However, when these additives are used, it may be difficult to obtain high adhesive strength when the resulting bonded magnet and metal parts are bonded together with an adhesive such as an epoxy adhesive. In contrast, when a carboxylic acid ester such as sebacic acid ester or adipic acid ester is used, high adhesive strength can be ensured.
[0056] The content of the carboxylic acid ester (additive) in the bonded magnet composition is preferably 0.3% by mass or more and 1.0% by mass or less. By increasing the content to 0.3% by mass or more, it is possible to sufficiently increase the adhesive strength between the bonded magnet and metal parts, etc., although the mechanism is not clear. From the viewpoint of improving the adhesive strength, the content of the carboxylic acid ester is more preferably 0.5% by mass or more. On the other hand, by keeping the content to 1.0% by mass or less, it is possible to further increase the resistance to cold and thermal shocks. From the viewpoint of increasing the resistance to cold and thermal shocks, the content of the carboxylic acid ester is more preferably 0.8% by mass or less.
[0057] [5] Other ingredients The bonded magnet composition of this embodiment may contain only magnet powder, thermoplastic resin binder (polyamide elastomer and polyamide resin), carbon fiber, and carboxylic acid ester, or may contain other components. Examples of other components include antioxidants, stabilizers, pigments, and / or compatibilizers. The bonded magnet composition may contain these components as necessary to the extent that the effects of the composition are not impaired.
[0058] [6] Liquidity The flowability (Q value) of the bonded magnet composition of this embodiment is 1.5 cm 3 / sec or more is preferable. Here, the fluidity (Q value) is a value measured using a flow tester under the conditions of a capillary temperature of 250°C, a load of 588N, an orifice diameter of 1mm, an orifice length of 1mm, and a preheating time of 300°C. By increasing the fluidity of the bonded magnet composition, the molding processability is improved. Therefore, it is possible to easily manufacture thin or complex shaped bonded magnets without the need for post-processing. In addition, the amount of magnet powder in the composition can be increased while maintaining a high dispersion state, and even if the content is the same, the orientation of the magnet powder can be improved. Furthermore, there is no need to perform molding at high temperatures to increase the fluidity. Since low-temperature molding is possible, the deterioration of the magnetic properties of the magnet powder can be suppressed. As a result of these combined effects, it is possible to manufacture bonded magnets, especially anisotropic bonded magnets, with excellent magnetic properties. It is desirable to have high fluidity, and it is preferable to have a flow rate of 2.0 cm or less. 3 / sec or more is more preferable. On the other hand, compositions with excessively high fluidity are difficult to manufacture. 3 / sec or less.
[0059] The bonded magnet composition of this embodiment can impart excellent thermal shock resistance to the bonded magnet obtained by molding it. Therefore, it is extremely useful as a composition for manufacturing bonded magnets. The bonded magnet obtained from this bonded magnet composition can be used for small, flat, complex-shaped products, including motor parts for electronic components. In addition, this bonded magnet has the characteristics that it can be mass-produced, does not require post-processing, and can be insert-molded. Therefore, it is particularly suitable for use in the manufacture of integrally molded parts combined with metal parts.
[0060] <<2. Manufacturing method of the composition for bonded magnets>> In the manufacturing method for the bonded magnet composition of this embodiment, Sm-Fe-N magnet powder, polyamide elastomer and polyamide resin as thermoplastic resin binder, and, if necessary, carbon fiber, carboxylic acid ester, antioxidant, and other components are weighed in predetermined amounts, mixed in a mixer such as a stirring mixer, and then kneaded using a kneading device. The details of the magnet powder, thermoplastic resin binder, and other components are as described above.
[0061] When the raw materials are mixed, the mixing ratio of the polyamide elastomer to the total amount of the polyamide elastomer and the polyamide resin in the thermoplastic resin binder is set to 50% by mass or more and 80% by mass or less. Also, the mixing ratio of the magnet powder in the raw materials is preferably set to 88.0% by mass or more and 91.0% by mass or less.
[0062] The shape of the thermoplastic resin binder (polyamide elastomer and polyamide resin) added during mixing and kneading is not particularly limited. For example, various shapes such as powder, beads, pellets, etc. can be used. Among them, the powder shape is preferable from the viewpoint of uniform mixing with the magnet powder.
[0063] The mixing and kneading of the raw materials may be carried out by a known method. The kneading device is not particularly limited, and for example, a batch kneader or a continuous extruder can be used. During kneading, it is preferable to control the shear force applied to the composition being kneaded in the kneading device. For example, when a kneader is used, the shear force can be controlled by adjusting conditions such as temperature, the amount of raw materials fed into the mixing tank, the kneading blade rotation speed, or the kneading time. In addition, when a continuous extruder is used, the shear force can be controlled by adjusting conditions such as temperature distribution, raw material feeding speed, screw segment shape, screw rotation speed, and die hole diameter.
[0064] It is desirable to mix and knead the raw materials, such as the magnet powder, the thermoplastic resin binder, and the additives, so that they are dispersed uniformly. When mixing and kneading are performed in a batch manner, the dispersion state can be visually confirmed. Furthermore, if the kneading is performed for an extremely long time, the composition may thicken excessively. Therefore, it is desirable to complete the kneading within a range where the thickening does not proceed excessively.
[0065] The kneading is preferably carried out at a temperature between the melting point of the thermoplastic resin binder and 250°C. If the kneading temperature is lower than the melting point, the fluidity of the composition decreases, making it difficult to uniformly disperse the raw materials. If the kneading temperature is too high, the polyamide elastomer and the polyamide resin become miscible with each other, making it difficult to obtain the desired microstructure. Furthermore, there is also the problem that the magnet powder is oxidized, leading to a decrease in magnetic properties. The kneading temperature is more preferably between 180°C and 220°C.
[0066] The bonded magnet composition of this embodiment can be manufactured by mixing and kneading the raw materials at once, although this is not limited thereto. That is, it can be manufactured by mixing and kneading the magnet powder and the thermoplastic resin binder (polyamide elastomer, polyamide resin) all at once. Therefore, it is not necessary to perform multiple kneading operations, such as kneading the magnet powder and the polyamide elastomer, then adding the polyamide resin and kneading again. Even if the composition is mixed and kneaded all at once, a composition with excellent fluidity and resistance to cold and thermal shock can be obtained. However, kneading may be performed multiple times depending on the necessity of the manufacturing operation.
[0067] <<3. Bonded magnets>> The bonded magnet of this embodiment includes a molded body of the bonded magnet composition described above. That is, the bonded magnet is produced by molding the bonded magnet composition. Specifically, the bonded magnet composition is heated and melted at a temperature equal to or higher than the melting point of the resin binder, which is a component of the bonded magnet composition, and the resulting melt is molded to produce the bonded magnet. Molding may be performed by a known method such as injection molding, extrusion molding, or compression molding. If the composition is molded in a magnetic field, an anisotropic bonded magnet can be obtained, and if the composition is molded in a non-magnetic field, an isotropic bonded magnet can be obtained. When polyamide 12 resin is used, the heat melting temperature is preferably in the range of 180°C to 250°C, more preferably 200°C to 220°C.
[0068] Among the above-mentioned molding methods, it is particularly preferable to mold the bonded magnets by injection molding. Injection molding allows for a large degree of freedom in the shape of the molded bonded magnet, and also results in bonded magnets with excellent surface properties and magnetic properties. Therefore, the obtained bonded magnets can be directly incorporated as part of electronic components. The above-mentioned bonded magnet compositions have good fluidity and excellent moldability in injection molding, making it easy to mold bonded magnets. Furthermore, the occurrence of external appearance defects such as welds during injection molding can be effectively prevented.
[0069] The bonded magnet of this embodiment has a microstructure derived from the composition. That is, at least a portion of the particles constituting the samarium-iron-nitrogen magnetic powder contained in the bonded magnet are surrounded by a resin layer mainly composed of polyamide resin, and matrix resin mainly composed of polyamide elastomer is present in the gaps between the particles surrounded by this resin layer. Bonded magnets with such a unique microstructure (sea-island structure) are characterized by their excellent resistance to thermal shocks, due to their structure.
[0070] The bonded magnet of this embodiment has excellent magnetic properties, excellent resistance to cold and thermal shock, and is less likely to crack. Therefore, it has excellent mechanical strength. This bonded magnet is used for small, flat, complex-shaped products such as motor parts for electronic devices. It also has features such as mass production, no need for post-processing, and insert molding. Such bonded magnets are particularly suitable for use in integrally molded parts with metal materials.
[0071] It is desirable to magnetize the obtained bonded magnet before use. For magnetization, an electromagnet that generates a static magnetic field or a capacitor magnetizer that generates a pulsed magnetic field is used. The magnetizing magnetic field, i.e., the magnetic field strength during magnetization, differs slightly depending on the type of magnet powder, so it cannot be determined in general terms. For example, it should be 1200 kA / m (15 kOe) or more, and preferably 2400 kA / m (30 kOe) or more.
[0072] Furthermore, the bonded magnet may be composed only of a molded body of a bonded magnet composition, or may include other components such as a surface layer.
[0073] <<4. Integral molding parts>> The integrally molded part of this embodiment includes the above-mentioned bonded magnet and a metal part. The above-mentioned bonded magnet can be combined and integrated with a metal part by adhesion via an adhesive or insert molding, thereby producing an integrally molded part. The integrally molded part can be produced by a known method. For example, it can be produced by applying a predetermined adhesive to the bonding surfaces of the bonded magnet and the metal part, pressing them together, and holding them at room temperature for 12 to 24 hours.
[0074] A typical bonded magnet material has a different linear expansion coefficient from that of a metal part. Therefore, when an integrally molded part is manufactured using this bonded magnet material and subjected to a thermal shock test, the bonded magnet is likely to crack. In contrast, the bonded magnet of this embodiment has high mechanical strength and excellent thermal shock resistance, so that the bonded magnet in the integrally molded part can be effectively prevented from cracking. Furthermore, when the bonded magnet of this embodiment is bonded to a metal part using an adhesive such as an epoxy adhesive, the adhesive strength is not weakened and the bonded magnet can be provided with excellent adhesive strength to the metal part. EXAMPLES
[0075] The present invention will be described in more detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples.
[0076] (1) Preparation of bonded magnet composition and bonded magnet [Example 1] As the magnet powder, 90.0 mass% of samarium-iron-nitrogen (Sm-Fe-N; SFN) magnet powder (manufactured by Sumitomo Metal Mining Co., Ltd.) having an average particle size of 2.3 μm, 8.2 mass% of a resin binder composed of polyamide elastomer and polyamide 12 resin, 1.0 mass% of carbon fiber (C fiber) having a fiber diameter of 11 μm as a reinforcing agent, and 0.8 mass% of sebacic acid ester as an additive were weighed out, and then mixed in a stirring mixer, and further kneaded at 200 ° C. using a continuous extruder to prepare a bonded magnet composition. The polyamide elastomer had a tensile breaking elongation of 530% and a flexural modulus of elasticity of 130 MPa. The polyamide 12 resin had a weight average molecular weight Mw of 5300. The ratio of polyamide elastomer in the resin binder (elastomer ratio) was 65 mass%.
[0077] The average particle size of the magnet powder was measured as follows. First, the magnet powder was observed using a scanning electron microscope (JEOL Ltd., JSM-IT200; SEM) to obtain an SEM image. The observation was performed at a magnification of 2000 times or more. Next, image analysis was performed on 1000 particles in the obtained SEM image to determine the particle size distribution based on volume. The cumulative 50% diameter (xd50) was then calculated as the average particle size from the obtained particle size distribution.
[0078] The tensile elongation at break of the polyamide elastomer was measured by the method specified in ISO 527, and the flexural modulus was measured by the method specified in ISO 178. The weight average molecular weight Mw of the polyamide 12 resin was measured using an RI detector of an analyzer: GPC-104 (manufactured by Shoko Scientific Co., Ltd.). Specifically, the value measured using the analyzer with hexafluoroisopropanol as the eluent was converted into the value of polymethyl methacrylate to obtain the weight average molecular weight.
[0079] The bonded magnet composition was then injection molded to produce a ring-shaped bonded magnet. The injection molding was performed at a molding temperature of 220°C and with four pinpoint gates. The resulting bonded magnet had an outer diameter of 32 mm, an inner diameter of 30 mm, and a height of 20 mm.
[0080] [Example 2] The blending ratio of the resin binder (polyamide elastomer and polyamide 12 resin) was changed to 7.2 mass%, and the blending ratio of the reinforcing agent (carbon fiber with a transition diameter of 11 μm) was changed to 2.0 mass%. Otherwise, a bonded magnet composition and a bonded magnet were produced in the same manner as in Example 1.
[0081] [Example 3] The blending ratio of the resin binder (polyamide elastomer and polyamide 12 resin) was changed to 8.7 mass%, and the blending ratio of the reinforcing agent (carbon fiber with a transition diameter of 11 μm) was changed to 0.5 mass%. Otherwise, a bonded magnet composition and a bonded magnet were produced in the same manner as in Example 1.
[0082] [Example 4] The blending ratio of the resin binder (polyamide elastomer and polyamide 12 resin) was changed to 8.0 mass %, and the blending ratio of the additive (sebacic acid ester) was changed to 1.0 mass %. Otherwise, a bonded magnet composition and a bonded magnet were produced in the same manner as in Example 1.
[0083] [Example 5] The blending ratio of the resin binder (polyamide elastomer and polyamide 12 resin) was changed to 8.7 mass%, and the blending ratio of the additive (sebacic acid ester) was changed to 0.3 mass%. Otherwise, a bonded magnet composition and a bonded magnet were produced in the same manner as in Example 1.
[0084] [Example 6] The blending ratio of the magnet powder (SFN magnet powder with an average particle size of 2.3 μm) was changed to 91.0 mass %, and the blending ratio of the resin binder (polyamide elastomer and polyamide 12 resin) was changed to 7.2 mass %. Otherwise, a bonded magnet composition and a bonded magnet were produced in the same manner as in Example 1.
[0085] [Example 7] The blending ratio of the magnet powder (SFN magnet powder with an average particle size of 2.3 μm) was changed to 88.0 mass %, and the blending ratio of the resin binder (polyamide elastomer and polyamide 12 resin) was changed to 10.2 mass %. Otherwise, a bonded magnet composition and a bonded magnet were produced in the same manner as in Example 1.
[0086] [Example 8] The magnet powder used was SFN magnet powder with an average particle size of 1.8 μm (manufactured by Sumitomo Metal Mining Co., Ltd.) Except for this, a bonded magnet composition and a bonded magnet were produced in the same manner as in Example 1.
[0087] [Example 9] The magnet powder used was SFN magnet powder with an average particle size of 3.3 μm (manufactured by Sumitomo Metal Mining Co., Ltd.) Except for this, a bonded magnet composition and a bonded magnet were produced in the same manner as in Example 1.
[0088] [Example 10] The ratio of polyamide elastomer (elastomer ratio) in the resin binder (polyamide elastomer and polyamide 12 resin) was changed to 57 mass %. Aside from that, a bonded magnet composition and a bonded magnet were produced in the same manner as in Example 1.
[0089] [Example 11] The ratio of polyamide elastomer (elastomer ratio) in the resin binder (polyamide elastomer and polyamide 12 resin) was changed to 74 mass %. Otherwise, a bonded magnet composition and a bonded magnet were produced in the same manner as in Example 1.
[0090] [Comparative Example 1] The resin binder was composed of only polyamide elastomer. In other words, the ratio of polyamide elastomer (elastomer ratio) in the resin binder (polyamide elastomer and polyamide 12 resin) was changed to 100 mass %. A bonded magnet composition and a bonded magnet were produced in the same manner as in Example 1.
[0091] [Comparative Example 2] The ratio (elastomer ratio) of the polyamide elastomer in the resin binder (polyamide elastomer and polyamide 12 resin) was changed to 85% by mass. Otherwise, a bonded magnet composition and a bonded magnet were produced in the same procedure as in Example 1.
[0092] [Comparative Example 3] The ratio (elastomer ratio) of the polyamide elastomer in the resin binder (polyamide elastomer and polyamide 12 resin) was changed to 25% by mass. Otherwise, a bonded magnet composition and a bonded magnet were produced in the same procedure as in Example 1. [Comparative Example 4] The resin binder was composed of only polyamide 12 resin. That is, the ratio (elastomer ratio) of the polyamide elastomer in the resin binder (polyamide elastomer and polyamide 12 resin) was changed to 0% by mass. Otherwise, a bonded magnet composition and a bonded magnet were produced in the same procedure as in Example 1.
[0093] (2) Evaluation For the bonded magnet compositions obtained in Examples 1 to 11 and Comparative Examples 1 to 4, evaluations of various properties were carried out as follows.
[0094] <Flowability> The flowability (Q value) of the bonded magnet composition was measured using a melt indexer flow tester (Shimadzu Corporation, CTF-100D). The measurement was carried out under the conditions of a capillary temperature of 250°C, a load of 588 N, an orifice diameter of 1 mm, an orifice length of 1 mm, and a preheating time of 300 seconds.
[0095] <AFM Observation> The cross section of the bonded magnet was observed with an atomic force microscope (AFM) to evaluate the microstructure. Specifically, the bonded magnet was first subjected to cross-section processing by Ar ion etching using a cross-section polisher. The cross section obtained was then observed with an AFM to obtain an elastic modulus image (AFM image). In this case, the measurement range was 10 μm x 10 μm, the number of measurement points was 512 x 512, and the measurement was performed in peak force tapping mode. The presence or absence of a sea-island structure was confirmed from the obtained elastic modulus image, and it was judged according to the following criteria.
[0096] ○: Island structure ×: No sea-island structure
[0097] <Thermal shock test A (heat shock)> The durability of the bonded magnet in thermal shock tests was evaluated. First, a bonded magnet (outer diameter 32 mm, inner diameter 30 mm, height 20 mm) was bonded to the inside of an iron ring with an outer diameter of 34 mm, inner diameter 32 mm, height 22 mm using epoxy resin to create an integrated molded part.
[0098] Next, the obtained integrally molded part was kept at room temperature for 24 hours, and then subjected to a thermal shock test in which one cycle was -40°C for 30 minutes to +100°C for 30 minutes. After 200 cycles, the bonded magnet of the integrally molded part was observed with an optical microscope at 20x magnification to check whether the bonded magnet had any defects such as cracks. Five test samples were evaluated, and the thermal shock test durability (heat shock) was judged according to the following criteria.
[0099] 〇: 0 defects after 200 cycles ×: 1 or more defects after 200 cycles
[0100] <Thermal shock test B (heat shock)> In thermal shock test B, the thermal shock test was carried out under conditions different from those in thermal shock test A. Specifically, an integrally molded part was produced using the same method as in thermal shock test A.
[0101] Next, the obtained integrally molded part was kept at room temperature for 24 hours, and then subjected to a thermal shock test in which one cycle was -40°C for 30 minutes to +90°C for 30 minutes. After 600 cycles, the bonded magnet of the integrally molded part was observed with an optical microscope at 20x magnification to check whether the bonded magnet had any defects such as cracks. Five test samples were evaluated, and the thermal shock test durability (heat shock) was judged according to the following criteria.
[0102] 〇: 0 defects after 600 cycles ×: 1 or more defects after 600 cycles
[0103] (3) Evaluation results The evaluation results obtained for Examples 1 to 11 and Comparative Examples 1 to 4 are shown in the following Tables 1 and 2. In addition, the AFM image obtained in Example 1 is shown in FIG.
[0104] In the samples of Examples 1 to 11, which were produced with an elastomer ratio of 50% by mass or more and 80% by mass or less, AFM images showed a structure in which a resin layer mainly composed of polyamide 12 resin was present on the surface of the particles constituting the SFN powder, and a matrix resin mainly composed of polyamide elastomer was present around the surface, i.e., a sea-island structure. Furthermore, no defects were observed in either thermal shock test A or B, and the samples had excellent thermal shock resistance. Furthermore, the fluidity (Q value) was 1.5 cm 3 / g or more, and had excellent moldability.
[0105] In contrast, no sea-island structure was observed in the samples of Comparative Examples 1 and 2, which were produced with an excessively high elastomer ratio. Furthermore, although no defects occurred in the thermal shock test B, defects occurred in the more severe thermal shock test A. On the other hand, no sea-island structure was observed in the samples of Comparative Examples 3 and 4, which were produced with an excessively low elastomer ratio. Furthermore, defects occurred in the thermal bombardment test A. Furthermore, the fluidity (Q value) was low at less than 1.0.
[0106] From the above results, it was found that the bonded magnet composition of this embodiment makes it possible to obtain a bonded magnet that is particularly excellent in resistance to cold and thermal shocks.
[0107] [Table 1]
[0108] [Table 2] [Explanation of symbols]
[0109] 2 Sm-Fe-N particles 4 Resin layer 6 Matrix Resin
Claims
1. The magnet powder contains samarium-iron-nitrogen magnet powder and a thermoplastic resin binder. the thermoplastic resin binder comprises a polyamide elastomer and a polyamide resin; a ratio of the amount of polyamide elastomer to the total amount of polyamide elastomer and polyamide resin contained in the thermoplastic resin binder is 50% by mass or more and 80% by mass or less; A composition for bonded magnets, in which at least some of the particles constituting the samarium-iron-nitrogen based magnet powder are surrounded by a resin layer mainly composed of polyamide resin, and a matrix resin mainly composed of polyamide elastomer is present in the gaps between the particles surrounded by the resin layer.
2. 2. The bonded magnet composition according to claim 1, wherein the ratio of the amount of polyamide elastomer to the total amount of polyamide elastomer and polyamide resin contained in the thermoplastic resin binder is 70% by mass or more and 80% by mass or less.
3. 3. The bonded magnet composition according to claim 1, wherein the samarium-iron-nitrogen based magnet powder has an average particle size of 1.8 μm or more and 3.3 μm or less.
4. 3. The bonded magnet composition according to claim 1, wherein the content of samarium-iron-nitrogen based magnet powder contained in said bonded magnet composition is 88.0% by mass or more and 91.0% by mass or less.
5. 3. The bonded magnet composition according to claim 1, wherein the polyamide elastomer has a tensile elongation at break of 400% or more and a flexural modulus of elasticity of 100 MPa or more.
6. 3. The bonded magnet composition according to claim 1, wherein the polyamide resin is a polyamide 12 resin.
7. 3. The bonded magnet composition according to claim 1, wherein the polyamide resin has a weight average molecular weight Mw of 4,500 or more and 7,500 or less as determined by molecular weight distribution measurement.
8. 3. The bonded magnet composition according to claim 1, further comprising carbon fibers.
9. 3. The bonded magnet composition according to claim 1, further comprising a carboxylic acid ester.
10. The samarium-iron-nitrogen magnet powder is Sm 2 Fe 17 N 3 3. The bonded magnet composition according to claim 1, having a composition represented by the formula:
11. A bonded magnet comprising a molded body of the bonded magnet composition according to claim 1 or 2.
12. An integrally molded part comprising the bonded magnet according to claim 11 and a metal part.
Citation Information
Patent Citations
Nylon resin composition, resin magnet and resin magnet part
JP2004352792A
Resin composition and molded article
WO2008123450A1