Solid-state battery and manufacturing method of solid-state battery

By incorporating a Li-Mg-X layer on the surface of the solid electrolyte layer, the solid-state battery achieves enhanced charging and discharging efficiency through reduced interfacial resistance and improved lithium ion diffusion.

JP2024143042AInactive Publication Date: 2024-10-11TOYOTA JIDOSHA KK

Patent Information

Application Number
JP2023055517
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing solid-state batteries have room for improvement in charging and discharging efficiency, specifically in the ratio of discharge capacity to charge capacity.

Method used

The solid-state battery is configured with a negative electrode active material layer comprising a Li-Mg-X alloy, where X is In or Ag, and a Li-Mg-X layer is formed on the surface of the solid electrolyte layer, preventing the formation of a resistance layer during charging and enhancing lithium ion diffusion.

Benefits of technology

The configuration results in higher charging and discharging efficiency by minimizing reductive decomposition of the solid electrolyte layer and maintaining a stable interface, thereby improving battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143042000001
    Figure 2024143042000001
Patent Text Reader

Abstract

To provide a solid-state battery with high charging and discharging efficiency.SOLUTION: A solid-state battery according to the present disclosure includes a positive electrode layer, a negative electrode layer including a negative electrode active material layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer. When the solid-state battery is fully charged, the negative electrode active material layer has a Li-Mg-X layer, and X is at least one selected from the group consisting of In and Ag. The Li-Mg-X layer is formed on a surface of the solid electrolyte layer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a solid-state battery and a method for manufacturing a solid-state battery. [Background technology]

[0002] 2. Description of the Related Art Conventionally, solid-state batteries have been known as lithium-ion secondary batteries having excellent safety. Patent Document 1 discloses an all-solid-state battery (hereinafter, also referred to as a "solid-state battery"). The solid-state battery disclosed in Patent Document 1 utilizes a deposition-dissolution reaction of metallic lithium as a reaction at the negative electrode. The solid-state battery includes a positive electrode including a positive electrode layer, a negative electrode including a negative electrode current collector and a negative electrode layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer. The negative electrode layer includes a β single-phase alloy of metallic lithium and metallic magnesium as a negative electrode active material. When the all-solid-state battery is fully charged, the element ratio of lithium element in the alloy is 81.80 atomic% or more and 99.97 atomic% or less. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-184513 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, from the viewpoint of improving the practicality of solid-state batteries, there is room for improvement in the charge / discharge efficiency of the solid-state battery of Patent Document 1. "Charge / discharge efficiency" refers to the ratio of the discharge capacity to the charge capacity.

[0005] The present disclosure has been made in consideration of the above circumstances. An object of one embodiment of the present disclosure is to provide a solid-state battery with high charge / discharge efficiency and a method for manufacturing the solid-state battery. [Means for solving the problem]

[0006] Means for solving the above problems include the following embodiments. <1> A solid-state battery comprising: a positive electrode layer, a negative electrode layer including a negative electrode active material layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, wherein when the solid-state battery is fully charged, the negative electrode active material layer has a Li-Mg-X layer, where X is at least one selected from the group consisting of In and Ag, and the Li-Mg-X layer is formed on a surface of the solid electrolyte layer. <2> When the solid-state battery is fully charged, the negative electrode active material layer is the Li-Mg-In layer. <1> The solid-state battery according to claim 1, <3> When the solid-state battery is fully charged, the negative electrode active material layer is the Li-Mg-Ag layer. <1> or <2> The solid-state battery according to claim 1, <4> 1. A method for producing a solid-state battery including a positive electrode layer, a negative electrode layer including a negative electrode current collector, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, the method comprising the steps of: forming an X layer on a surface of the solid electrolyte layer facing the negative electrode layer; and forming an Mg layer on a surface of the negative electrode current collector facing the solid electrolyte layer, wherein the X is at least one selected from the group consisting of In and Ag. <5> The X is In or Ag. <4> A method for producing the solid-state battery according to claim 1. Effect of the Invention

[0007] According to the present disclosure, a solid-state battery having high charge / discharge efficiency and a method for manufacturing the solid-state battery are provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In the present disclosure, a numerical range indicated using "~" means a range including the numerical values ​​described before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in stages in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with the upper limit or lower limit of another numerical range described in stages. In the numerical ranges described in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with a value shown in the examples. In the present disclosure, a combination of two or more preferred embodiments is a more preferred embodiment. In the present disclosure, the amount of each component means the total amount of the multiple substances, unless otherwise specified, when there are multiple substances corresponding to each component. In the present disclosure, the term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.

[0009] (1) Solid state battery The solid-state battery of the present disclosure includes a positive electrode layer, a negative electrode layer including a negative electrode active material layer, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer. When the solid-state battery is fully charged, the negative electrode active material layer has a Li (lithium)-Mg (magnesium)-X layer. The X (hereinafter, also referred to as "metal element X") is at least one selected from the group consisting of In (indium) and Ag (silver). The Li-Mg-X layer is formed on the surface of the solid electrolyte layer.

[0010] In this disclosure, "when the solid-state battery is fully charged" refers to the time when the state of charge (SOC) of the solid-state battery is 100%. SOC indicates the ratio of the charge capacity to the fully charged capacity of the solid-state battery. At the fully charged capacity, the SOC is 100%. The term "Li-Mg-X layer" refers to an alloy layer mainly composed of lithium, magnesium, and metal element X. More specifically, the term "Li-Mg-X layer" refers to a layer in which the ratio of lithium is 45 atomic% or more, the ratio of magnesium is 0.3 atomic% or more, and the ratio of metal element X is 0.1 atomic% or more, relative to the total amount of all elements constituting the layer. The ratio of lithium may be 45 atomic% to 99.6 atomic%. The ratio of magnesium may be 0.3 atomic% to 45 atomic%. The ratio of metal element X may be 0.1 atomic% to 5 atomic%. "The Li-Mg-X layer is formed on the surface of the solid electrolyte layer" means that no Li layer is interposed between the Li-Mg-X layer and the solid electrolyte layer when the solid battery is fully charged. "Li layer" means a metal layer containing lithium element as a main component. More specifically, "Li layer" means a layer in which the ratio of lithium element is 98 atomic % or more relative to the total amount of all elements constituting the layer.

[0011] The solid-state battery of the present disclosure has the above-described configuration and therefore has high charge / discharge efficiency. This effect is believed to be due to, but not limited to, the following reasons. It is known that when the solid electrolyte layer and metallic lithium come into physical contact with each other during charging and discharging of a solid-state battery, a reductive decomposition reaction of the solid electrolyte layer proceeds. When the reductive decomposition reaction of the solid electrolyte layer proceeds, a layer (hereinafter also referred to as a "resistance layer") that acts as an interface resistance may be formed between the solid electrolyte layer and the negative electrode layer. As a result, the charge and discharge efficiency of the solid-state battery may decrease. In the present disclosure, the Li-Mg-X layer is formed on the surface of the solid electrolyte layer. In other words, no Li layer is interposed between the Li-Mg-X layer and the solid electrolyte layer during charging of the solid battery. That is, the reductive decomposition reaction of the solid electrolyte layer is unlikely to proceed. As a result, a resistance layer is unlikely to be formed. Furthermore, in the present disclosure, during charging and discharging of the solid battery, lithium ions are more likely to diffuse at the interface between the solid electrolyte layer and the negative electrode layer than when the Li-Mg-X layer is not formed on the surface of the solid electrolyte layer. As a result, it is presumed that the charge and discharge efficiency of the solid battery of the present disclosure is higher than that of the conventional battery due to the synergistic effect of the combination of the metal element Li, the metal element Mg, and the metal element X.

[0012] (1.1)Battery structure The structure of the solid-state battery is a laminated structure of a positive electrode layer / anode layer / solid electrolyte layer. The solid-state battery includes a so-called all-solid-state battery using a solid electrolyte as an electrolyte, and the solid electrolyte may contain an electrolytic solution of less than 10 mass% with respect to the total amount of the electrolyte. The solid electrolyte may be a composite solid electrolyte containing an inorganic solid electrolyte and a polymer electrolyte.

[0013] The solid-state battery may be configured by sealing the end faces (side faces) of the laminated structure of the positive electrode layer / solid electrolyte layer / negative electrode layer with a resin. The shape of the solid-state battery is not particularly limited, and may be, for example, a coin type, a cylindrical type, a square type, a sheet type, a button type, a flat type, or a laminate type.

[0014] (1.2) Negative electrode layer The solid-state battery includes a negative electrode layer, which includes a known negative electrode current collector and a negative electrode active material layer.

[0015] (1.2.1) Negative electrode active material layer The negative electrode layer has a negative electrode active material layer. In a fully charged state, the negative electrode active material layer has a Li-Mg-X layer. The metal element X is at least one selected from the group consisting of In and Ag. The Li-Mg-X layer is formed on the surface of the solid electrolyte layer. The layer structure of the negative electrode active material layer was determined in the same manner as described in the Examples.

[0016] The metal element X may be one selected from the group consisting of In and Ag. When the metal element X is In or Ag, the negative electrode active material layer at full charge tends to be a Li-Mg-X layer, and does not include each of the Li-Mg layer, Li-X layer, Mg-X layer, and Li layer. This is presumed to be due to the following reason. That is, during charging (Li deposition), Li first reacts with X (In or Ag) to form a Li-X layer. Then, the deposited Li and Mg diffuse mutually, and the concentration difference becomes the driving force to form a Li-Mg-X layer. Each of X and Mg is a metal with a wide solid solution region with Li (= high solid solubility). Therefore, X does not remain at the interface even during charging and discharging, and the Li-Mg-X layer distributed in the negative electrode can be maintained.

[0017] In terms of increasing the charge / discharge efficiency of the solid-state battery, the ratio of the metal element X, the ratio of Li, and the ratio of Mg at full charge are preferably within the following ranges. That is, the ratio of the metal element X is preferably 0.05 atomic% to 15.0 atomic%, more preferably 0.12 atomic% to 2.0 atomic%, and even more preferably 0.3 atomic% to 1.0 atomic%, based on the total amount of the negative electrode active material layer. The ratio of Li is not particularly limited, and is preferably 85.0 atomic% to 99.5 atomic%, more preferably 98.0 atomic% to 99.88 atomic%, and even more preferably 99.0 atomic% to 99.7 atomic%, based on the total amount of the negative electrode active material layer. The proportion of Mg is not particularly limited, and is preferably 0.1 atomic % to 25.0 atomic %, more preferably 0.3 atomic % to 20.0 atomic %, and further preferably 0.8 atomic % to 6.0 atomic %, relative to the total amount of the negative electrode active material layer.

[0018] The ratio is calculated by removing the negative electrode layer from a fully charged all-solid-state battery, performing an ICP (Inductively Coupled Plasma) analysis on the negative electrode layer, and calculating the element ratio of the alloy contained in the negative electrode layer.

[0019] When the solid-state battery is fully charged, the thickness of the Li-Mg-X layer is not particularly limited and may be 1 μm to 30 μm.

[0020] When the solid-state battery is fully charged, the negative electrode active material layer is preferably a Li-Mg-In layer. This increases the charge / discharge efficiency of the solid electrolyte. In this case, the Li-Mg-In layer is in contact with the surface of the solid electrolyte layer and the surface of the negative electrode current collector.

[0021] When the solid-state battery is fully charged, the negative electrode active material layer is preferably a Li-Mg-Ag layer. This allows the charge / discharge efficiency of the solid electrolyte to be higher than when the negative electrode active material layer is a Li-Mg-In layer when the solid-state battery is fully charged. In this case, the Li-Mg-Ag layer is in contact with the surface of the solid electrolyte layer and the surface of the negative electrode current collector.

[0022] When the solid-state battery is being discharged (eg, SOC: 0%), the negative electrode active material layer does not need to have a Li layer.

[0023] (1.3) Solid electrolyte layer The solid-state battery includes a solid electrolyte layer. The solid electrolyte layer may include a solid electrolyte. The solid electrolyte preferably includes at least one selected from a group of solid electrolytes consisting of a known sulfide solid electrolyte, a known oxide solid electrolyte, and a known halide solid electrolyte. The solid electrolyte layer may have a single layer structure or a multilayer structure of two or more layers. The solid electrolyte layer may include a known binder.

[0024] (1.4) Positive electrode layer The solid-state battery includes a positive electrode layer. The positive electrode layer may include a known positive electrode collector and a positive electrode active material layer. The positive electrode active material layer is laminated on a main surface of the positive electrode collector on the solid electrolyte layer side. The positive electrode active material layer may contain a known positive electrode active material. The positive electrode active material preferably contains a lithium composite oxide. The positive electrode layer may include a known solid electrolyte, a known conductive assistant, a known binder, and other components (e.g., a thickener, a surfactant, a dispersant, a wetting agent, an antifoaming agent, etc.).

[0025] (2) Manufacturing method of solid-state batteries The method for producing a solid-state battery according to the present disclosure is a method for producing a solid-state battery including a positive electrode layer, a negative electrode layer including a negative electrode current collector, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer. The method includes a step of forming an X layer on the surface of the solid electrolyte layer facing the negative electrode layer (hereinafter also referred to as an "X layer forming step"), and a step of forming an Mg layer on the surface of the negative electrode current collector facing the solid electrolyte layer (hereinafter also referred to as an "Mg layer forming step"). The X is at least one selected from the group consisting of In and Ag.

[0026] In the present disclosure, an "X layer" refers to a metal layer containing metal element X as a main component. In the "X layer", the ratio of metal element X to the total amount of all elements constituting the X layer may be 100 atomic %. In the present disclosure, the term "Mg layer" refers to a metal layer containing the metal element Mg as a main component. In the "Mg layer", the ratio of the metal element Mg to the total amount of all elements constituting the Mg layer may be 100 atomic %. The "X layer" and the "Mg layer" are precursors of the "Li-Mg-X layer" in the present disclosure. Specifically, each of the X layer and the Mg layer incorporates lithium ions upon charging the solid-state battery, becoming one Li-Mg-X layer.

[0027] Since the manufacturing method of the solid-state battery according to the present disclosure has the above configuration, the solid-state battery according to the present disclosure can be produced.

[0028] (2.1)X layer formation process The solid-state battery of the present disclosure includes an X-layer forming step. In the X-layer forming step, an X-layer is formed on the surface of the solid electrolyte layer on the negative electrode layer side. This produces a solid electrolyte layer with an X-layer. The solid electrolyte layer with an X-layer has a solid electrolyte layer and an X-layer formed on the surface of the solid electrolyte layer on the negative electrode layer side.

[0029] The method for preparing the solid electrolyte layer may be a known method.

[0030] The method for forming the X-layer is not particularly limited and may be any known method, including a dry process and a wet process. In the dry process, the X-layer is formed by treatment in a gas phase or vacuum. Specifically, examples of the dry process include physical vapor deposition (e.g., vacuum deposition, ion plating, sputtering, etc.), chemical vapor deposition (e.g., thermal CVD (Chemical Vapor Deposition), plasma CVD, plasma CVD, etc.), and thermal spraying (e.g., flame spraying, arc spraying, plasma spraying, etc.). In the wet process, the X-film is formed using a solution. Specifically, examples of the wet process include plating (e.g., electroplating, electroless plating, electroforming, etc.), and electrolytic polymerization, etc.

[0031] Among them, the physical vapor deposition method or the chemical vapor deposition method is preferable as the method for forming the X layer. This method provides better uniformity of the initial X layer and better adhesion between the X layer and the solid electrolyte layer than the method for forming the X layer using the pressing method or the fine particle coating method. As a result, a solid battery with higher charge / discharge efficiency is obtained. This is presumably due to the following reasons. In the physical vapor deposition method or chemical vapor deposition method, the X layer is formed thinner and with a uniform thickness that follows the uneven shape of the interface of the solid electrolyte. In addition, the adhesive strength between the solid electrolyte and the X layer is strong. Therefore, voids are unlikely to form at the interface between the solid electrolyte layer and the X layer. As a result, the battery performance of the solid battery is unlikely to deteriorate. On the other hand, in the pressing method or the fine particle coating method, the X layer is likely to be formed with an uneven thickness depending on the location of the solid electrolyte interface. For example, the X layer may be embedded in the uneven shape of the solid electrolyte layer interface, or may accumulate in a large amount in the recesses of the solid electrolyte interface. This may cause unevenness in the progress of the Li deposition reaction, resulting in the presence of voids at the interface between the X layer and the solid electrolyte layer. In addition, due to the uneven thickness of the X layer and the weak adhesive strength between the X layer and the solid electrolyte layer, there may be places where the solid electrolyte layer is partially exposed. From there, a reaction of the solid electrolyte (for example, a reduction decomposition reaction) may proceed. As a result, the battery performance of the solid battery may deteriorate.

[0032] The thickness of the X layer is not particularly limited and may be from 1 nm to 1000 nm.

[0033] X is preferably In or Ag. This improves the charge / discharge efficiency of the resulting solid-state battery compared to when X is In and Ag. X is more preferably Ag. This improves the charge / discharge efficiency of the resulting solid-state battery compared to when X is In.

[0034] (2.2) Mg layer formation process The method for manufacturing a solid-state battery according to the present disclosure includes a Mg layer forming step. In the Mg layer forming step, a Mg layer is formed on the surface of the negative electrode current collector facing the solid electrolyte layer. This produces a negative electrode current collector with a Mg layer. The negative electrode current collector with a Mg layer has a negative electrode current collector and a Mg layer formed on the surface of the negative electrode current collector facing the solid electrolyte layer.

[0035] The negative electrode current collector may be prepared by a known method.

[0036] The method for forming the Mg layer is not particularly limited, and may be the same as the method exemplified for forming layer X. Among them, the method for forming the Mg layer is preferably a physical vapor deposition method or a chemical vapor deposition method.

[0037] The thickness of the Mg layer is not particularly limited and may be from 30 nm to 3000 nm.

[0038] (2.3) Lamination process The method for producing a solid-state battery of the present disclosure may include a lamination step. In the lamination step, a negative electrode current collector with an Mg layer, a solid electrolyte layer with an X layer, and a positive electrode layer are laminated in this order to form a battery precursor. The battery precursor is formed by laminating a negative electrode current collector, an Mg layer, an X layer, a solid electrolyte layer, and a positive electrode layer in this order.

[0039] The positive electrode layer may be prepared by any known method.

[0040] The lamination method may be, for example, a pressing method. A slurry may be used when forming the positive electrode layer. The pressing method may be a roll press, a cold isostatic press (CIP), or the like. The pressing pressure is usually 1 MPa to 600 MPa.

[0041] (2.4) Charging process The method for producing a solid-state battery of the present disclosure may include a charging step, in which the battery precursor is charged to produce a solid-state battery.

[0042] When the charging process is performed, lithium ions move from the positive electrode layer to the negative electrode layer. The lithium ions are taken into the Mg layer and the X layer, respectively, to form one Li-Mg-X layer. At this time, no Li layer is formed between the solid electrolyte layer and the negative electrode current collector. This is presumably because the precipitated Li and Mg diffuse into each other, and the concentration difference becomes the driving force to form the Li-Mg-X layer.

[0043] The charging conditions for the charging step are not particularly limited and may be appropriately selected depending on the thickness of the Mg layer and the thickness of the X layer, etc. EXAMPLES

[0044] The present disclosure will be described in more detail below with reference to examples, but the invention of the present disclosure is not limited to these examples.

[0045] [1] Examples and Comparative Examples [1.1] Example 1 [1.1.1] Solid state battery LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 The positive electrode mixture containing the binder and the solvent was applied onto one surface of an Al current collector foil to obtain a positive electrode layer. Li containing LiBr and LiI as sulfide-based solid electrolytes 2 SP 2 S 5A mixture of the electrolyte, binder, and solvent was prepared. This mixture was applied onto a resin film to produce a thin solid electrolyte film. The thin solid electrolyte film was formed at a density of 7 ton / cm. 2 The solid electrolyte layer was obtained by pressing the substrate at a pressure of 100 MPa. An In material was prepared as a raw material for the modification layer. Using the In material and a magnetron sputtering device, In was deposited on one surface of the solid electrolyte layer to form an In layer (ie, a modification layer) having a thickness of 100 nm. Using an electron beam deposition apparatus, Mg was deposited on one surface of a Ni foil serving as a negative electrode current collector to form a 1000 nm-thick Mg layer. A Ni current collector foil having an Mg layer on one side was placed on the side of the solid electrolyte layer where the In layer was placed. A positive electrode layer was placed on the side opposite to the side where the In layer was placed, so that the solid electrolyte layer and the positive electrode layer were in contact with each other. These were cold isostatically pressed (CIP) at 4 ton / cm. 2 The solid-state battery was obtained by pressing the positive electrode current collector at a pressure of 1000 MPa. The solid-state battery had a positive electrode current collector, a positive electrode layer, a solid electrolyte layer, an In layer, an Mg layer, and a negative electrode current collector in this order.

[0046] [1.1.2] Negative electrode active material layer of a solid-state battery when fully charged The cross section of the solid-state battery in a fully charged state was processed, and the negative electrode active material layer was observed with a secondary electron microscope (SEM). The thickness of the layer that appeared to be a Li layer was confirmed. The type and concentration of the contained metal species and the thickness of the Li-Mg-In layer were estimated from element mapping and spectrum analysis of each layer with an energy dispersive X-ray analyzer (EDX). This revealed that the negative electrode active material layer of Example 1 was a Li-Mg-In layer when the solid-state battery was fully charged.

[0047] [1.1.3] Negative electrode active material layer of a solid-state battery at full discharge The cross section of the solid-state battery in the fully discharged state was processed, and the negative electrode active material layer was analyzed in the same manner as the analysis of the negative electrode active material layer of the solid-state battery in the fully charged state. This revealed that the negative electrode active material layer of Example 1 was an Mg-In layer (the ratio of Li in the Mg-In layer: 88.0 atomic % or less) when the solid-state battery was fully discharged.

[0048] [1.2] Example 2 [1.2.1] Solid state battery Except for changing the In material to an Ag material, a solid-state battery was obtained in the same manner as in Example 1. The solid-state battery had a positive electrode current collector, a positive electrode layer, a solid electrolyte layer, an Ag layer, an Mg layer, and a negative electrode current collector, in this order.

[0049] [1.2.2] Negative electrode active material layer of a solid-state battery when fully charged The cross section of the solid-state battery in a fully charged state was processed, and the negative electrode active material layer was analyzed in the same manner as in Example 1. This revealed that the negative electrode active material layer of Example 2 was a Li-Mg-Ag layer when the solid-state battery was fully charged.

[0050] [1.2.3] Negative electrode active material layer of a solid-state battery at full discharge The cross section of the solid-state battery in a fully discharged state was processed, and the negative electrode active material layer was analyzed in the same manner as in Example 1. This revealed that the negative electrode active material layer of Example 2 was an Mg-Ag layer (ratio of Li in the Mg-Ag layer: 88.0 atomic % or less) when the solid-state battery was fully discharged.

[0051] [1.3] Comparative Example 1 [1.3.1] Solid state battery In the same manner as in Example 1, a positive electrode layer and a solid electrolyte layer were obtained. Using an electron beam deposition apparatus, Mg was deposited on one surface of a Ni foil serving as a negative electrode current collector to form a 1000 nm-thick Mg layer. A Ni current collector foil having an Mg layer on one side was placed on one side of the solid electrolyte layer. A positive electrode layer was placed on the side of the solid electrolyte layer opposite to the side on which the Mg layer was placed, so that the solid electrolyte layer and the positive electrode layer were in contact with each other. These were cold isostatically pressed (CIP) at 4 ton / cm. 2 The solid-state battery had a positive electrode current collector, a positive electrode layer, a solid electrolyte layer, an Mg layer, and a negative electrode current collector, in this order.

[0052] [1.3.2] Negative electrode active material layer of a fully charged solid-state battery The cross section of the charged solid-state battery was processed, and the negative electrode active material layer was analyzed in the same manner as in Example 1. This revealed that the negative electrode active material layer of Comparative Example 1 was a Li-Mg layer when the solid-state battery was fully charged.

[0053] [1.3.3] Negative electrode active material layer of a solid-state battery at full discharge The cross section of the solid-state battery in a fully discharged state was processed, and the negative electrode active material layer was analyzed in the same manner as in Example 1. This revealed that the negative electrode active material layer of Comparative Example 1 was an Mg layer (ratio of Li in the Mg layer: 98.5 atomic % or less) when the solid-state battery was fully discharged.

[0054] [1.4] Comparative Example 2 [1.4.1] Solid state battery In the same manner as in Example 1, a positive electrode layer and a solid electrolyte layer were obtained. An In material was prepared as a raw material for the modification layer. Using the In material and a magnetron sputtering device, In was deposited on one surface of the solid electrolyte layer to form an In layer (i.e., a modification layer) having a thickness of 100 nm. A Ni current collector was placed as a negative electrode current collector on the surface of the solid electrolyte layer on which the In layer was placed. A positive electrode layer was placed on the surface of the solid electrolyte layer opposite to the surface on which the In layer was placed, so that the solid electrolyte layer and the positive electrode layer were in contact with each other. These were cold isostatically pressed (CIP) at 4 ton / cm. 2 The solid-state battery had a positive electrode current collector, a positive electrode layer, a solid electrolyte layer, an In layer, and a negative electrode current collector, in this order.

[0055] [1.4.2] Negative electrode active material layer of a fully charged solid-state battery The cross section of the charged solid-state battery was processed, and the negative electrode active material layer was analyzed in the same manner as in Example 1. This revealed that the negative electrode active material layer of Comparative Example 2 was a Li-In layer when the solid-state battery was fully charged.

[0056] [1.4.3] Negative electrode active material layer in a solid-state battery at full discharge The cross section of the solid-state battery in a fully discharged state was processed, and the negative electrode active material layer was analyzed in the same manner as in Example 1. This revealed that the negative electrode active material layer of Comparative Example 2 was an In layer (ratio of Li in the In layer: 98.5 atomic % or less) when the solid-state battery was fully discharged.

[0057] [2] Measurement of charge / discharge efficiency The charge / discharge efficiency was calculated according to the following formula (1) using the charge capacity and discharge capacity after 30 cycles of charging and discharging an uncharged solid-state battery. Equation (1): Charge / discharge efficiency (%) = (discharge capacity after 30 cycles / charge capacity after 30 cycles) x 100 The measurement results of the charge / discharge efficiency are shown in Table 1.

[0058] [Table 1]

[0059] In Table 1, in "negative electrode active material layer," "-" indicates that there is no layer. "CC side" in "uncharged" indicates a layer formed on the surface of the negative electrode current collector. "SE side" in "uncharged" indicates a layer formed on the surface of the solid electrolyte layer.

[0060] The negative electrode active material layer of Example 1 had a Li-Mg-In layer. The Li-Mg-In layer was formed on the surface of the solid electrolyte layer. The negative electrode active material layer of Example 2 had a Li-Mg-Ag layer. The Li-Mg-Ag layer was formed on the surface of the solid electrolyte layer. Therefore, it was found that the solid batteries of Examples 1 and 2 had higher charge / discharge efficiency than the solid batteries of Comparative Examples 1 and 2.

Claims

1. A solid-state battery comprising: a positive electrode layer; a negative electrode layer including a negative electrode active material layer; and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, When the solid-state battery is fully charged, the negative electrode active material layer has a Li—Mg—X layer, The X is at least one selected from the group consisting of In and Ag, The Li—Mg—X layer is formed on the surface of the solid electrolyte layer.

2. 2. The solid-state battery according to claim 1, wherein the negative electrode active material layer is the Li-Mg-In layer when the solid-state battery is fully charged.

3. 2. The solid-state battery according to claim 1, wherein the negative electrode active material layer is the Li-Mg-Ag layer when the solid-state battery is fully charged.

4. A method for manufacturing a solid-state battery including a positive electrode layer, a negative electrode layer including a negative electrode current collector, and a solid electrolyte layer disposed between the positive electrode layer and the negative electrode layer, comprising: forming an X layer on a surface of the solid electrolyte layer on the negative electrode layer side; forming an Mg layer on a surface of the negative electrode current collector facing the solid electrolyte layer; Including, The method for producing a solid-state battery, wherein X is at least one selected from the group consisting of In and Ag.

5. The method for producing a solid-state battery according to claim 4 , wherein X is In or Ag.

Citation Information

Patent Citations

  • Water-based ink composition for ballpoint pen and ballpoint pen with built-in the same

    JP2018184513A

Cited By

  • Battery and manufacturing method thereof

    JP2025044755A

  • Battery and manufacturing method thereof

    JP7800521B2