Method of producing sintered ore

By separately producing granules A and B with controlled alumina and limestone blending, the method optimizes melt assimilation and air permeability, addressing the challenges of raw material variability in sintered ore production, enhancing strength and productivity.

JP2024143107AActive Publication Date: 2024-10-11KOBE STEEL LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023055612
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Existing methods for producing sintered ore face challenges in controlling the melt assimilation between granules due to varying raw material properties, leading to issues with air permeability, productivity, and strength of the sintered ore, as the composition of the adhesion layer is not adequately designed, particularly concerning alumina and calcium oxide content.

Method used

The method involves separately producing granules A and B with specific composition constraints, including a blending ratio of low alumina ore ≤30 mass% and a weighted average [C/F] ≧0.115, and using gradient blending of limestone and high-crystalline water ore to optimize the adhesion layer properties, ensuring appropriate melt generation and assimilation during sintering.

Benefits of technology

This approach enhances the strength and productivity of sintered ore by promoting melt assimilation and maintaining air permeability within the sintering machine, resulting in improved sintering quality and yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143107000001_ABST
    Figure 2024143107000001_ABST
Patent Text Reader

Abstract

To provide a method of producing a sintered ore, which can improve strength and productivity of the sintered ore by designing appropriate granule components in a granulating step that produces multiple types of granules differently, taking into consideration characteristics of raw materials used.SOLUTION: In operating a sintering process that produces a sintered ore by differently producing granules A and B in each of which an adhesion layer 3 surrounds a core particle 2 and then mixing and firing these granules A and B, granules A and B are produced by meeting the following conditions: a proportion of low-alumina ore blended in each of granules A and B is ≤30 mass%; and a weighted average [C / F] in the adhesion layers of the granules A and B is ≥0.115, performing gradient blending of low-alumina ore to the granule A, performing gradient blending of limestone 4 to the granule A so that [C / F] in the adhesion layer 3 of the granule B is ≥0.08, and performing gradient blending of high crystallization water ore to the granule A so that a crystallization water component in the adhesion layer 3 of the granule A is ≤4.0 mass%.SELECTED DRAWING: Figure 8
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing sintered ore by mixing iron ore and auxiliary materials, granulating the mixture, and baking the granulated mixture. [Background technology]

[0002] Generally, in the sintering process (the process of producing sintered ore), iron ore and auxiliary materials (limestone, etc.) are first mixed in a granulator and carbon material, which serves as a heat source, is added to produce granules that will serve as the sintering raw material.The granules are then loaded into the sintering machine and fired to produce the finished sintered ore.

[0003] Among these, in the granulation process, the raw material charged into the granulator from the raw material hopper is rolled while adding water, so that fine ore, limestone, etc. adhere to the core ore to form an adhesion layer. In this way, a granulated material with an adhesion layer is produced. As for the granulator, a method using a drum mixer or a pan pelletizer is generally used. The granulated material is fired in a sintering machine to produce sintered ore. Technologies for producing such sintered ore are disclosed in, for example, Patent Documents 1 to 3.

[0004] Patent Document 1 aims to stably and reliably improve the yield and productivity of sintered ore in a sintered ore manufacturing method without changing the chemical components of the sintered ore that affect blast furnace operation.

[0005] Specifically, various fine ores to be mixed as sinter raw materials are classified into two series (high Al2O3 content side = first series (A) and low Al2O3 content side = second series (B)) according to the Al2O3 content, and the CaO source (4A, 4B) and powder fuel (7A, 7B) are mixed with the fine ores of each of the classified series (A, B). The mixtures of each series (A, B) are mixed and granulated (8A, 8B), and then the granulated products of each series are mixed. (9) to obtain all sintered raw materials, and then firing (10) the all sintered raw materials to produce sintered ore, the basicity (mass ratio CaO / SiO2) of the fine powder portion of 0.5 mm or less in the mixture of the first series (A) is set to a range of 4.4 to 7.3, and the mixing ratio of the mixture of the first series (A) (excluding return ore and pulverized fuel) to the mixture of the second series (B) (excluding pulverized fuel) is set to a range of 2:8 to 8:2 by mass.

[0006] Patent Document 2 aims to make it possible to improve the productivity and strength of sintered ore when a large amount of fine ore (pellet feed) is blended in a sintered ore manufacturing method.

[0007] Specifically, the method for producing sintered ore comprises a main granulation process and a secondary granulation process in parallel, in which the sintering raw material is divided into a main sintering raw material and a secondary sintering raw material, and these are mixed and granulated, the granulated products produced in the main granulation process and the secondary granulation process are combined, and the combined granulated products are fired. In the secondary granulation process, the ratio of fine ore and fine ore, which are part of the secondary sintering raw material, is 1.5 / 1 or more and less than 3 / 1, the binder is quicklime and crushed ore, and the amount of the crushed ore is 3% by mass or more and less than 7% by mass of the secondary sintering raw material.

[0008] The object of Patent Document 3 is to suppress the production of strip-shaped CaF with poor reducibility, while promoting the production of amorphous slag with excellent room-temperature strength and resistance to reduction disintegration, thereby enabling the production of sintered ore with excellent room-temperature strength, reduction disintegration resistance, and reducibility with good yield.

[0009] Specifically, in the pretreatment method for sintering raw materials, the {average Al2O3 weight content / (average Al2O3 weight content+average Fe2O3 weight content)} value and the average SiO2 weight content value of all the fine ores are calculated from the chemical components and blending ratios of various fine ores to be blended as the sintering raw materials, various fine ores are classified based on these average values, and for fine ores having an {Al2O3 weight content / (Al2O3 weight content+Fe2O3 weight content)} value lower than the average value and an SiO2 weight content value higher than the average value, a CaO source to be blended as a flux is blended so that the CaO weight content / SiO2 weight content value is higher than the average value of all the sintering raw materials, and this blend is mixed and granulated prior to mixing and granulation of all the sintering raw materials. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2009-114485 A [Patent Document 2] JP 2016-191122 A [Patent Document 3] Japanese Patent Application Publication No. 63-076825 Summary of the Invention [Problem to be solved by the invention]

[0011] Now, Fig. 1 shows a schematic outline of the sintering process in which raw material 1 is granulated to produce sintered ore. As shown in Fig. 1, when producing sintered ore, raw material 1 (hereinafter referred to as granulated material 1) that has been pre-processed in granulation equipment 7 such as a drum mixer 8 is fed to a pallet cart on a sintering machine 10, and the surface of the raw material packed bed containing carbonaceous material is ignited, and gas is sucked in from below to propagate the combustion. During the combustion, the granulated materials 1 are melted and assimilated between each other and solidified to produce the finished sintered ore.

[0012] Figure 2 shows a schematic overview of the granulated material 1. As shown in Figure 2, most granulated materials 1 have a shape in which a core ore 2 of +1 mm is covered with limestone 4 and fine ore 5 (or auxiliary raw material) of -1 mm. In other words, the granulated material 1 has an adhesion layer 3 formed around it, and is also called a pseudo-particle.

[0013] When granules melt in a sintering machine, the part where the granules start to melt is the adhesion layer with a large specific surface area, and the molten calcium ferrite (CF) generated from the molten adhesion layer engulfs and assimilates the surrounding granules, and the sintering reaction proceeds. At this time, the better the melting and assimilation between the granules, the stronger the bond structure becomes, and the stronger the sintered ore product will be.

[0014] The melt assimilation between the granulated materials depends on the amount and viscosity of the generated melt, which are influenced by the components of the adhesion layer, i.e., the properties of the raw material used during granulation. For example, when iron ore with a high fine powder content is used, the iron content in the adhesion layer of the granulated material becomes relatively high, while the CaO content of the melt component becomes relatively low, which reduces the amount of melt generated. Also, when ore with a high alumina content is used, even if the amount of melt generated is sufficient, the viscosity of the melt increases, resulting in poor assimilation and a fragile structure.

[0015] Furthermore, the productivity of sintered ore is dominated by the yield in the sintering machine and the permeability of the raw material packed bed. If the permeability of the raw material packed bed is good, the sintering time can be shortened, and the production volume can be improved. In order to ensure the permeability in the sintering machine, it is necessary to increase the void ratio of the raw material packed bed (reduce the density).

[0016] If a highly viscous molten liquid is generated from the granulated material, it becomes difficult for the gas to flow when it is sucked in from below the sintering machine, preventing the formation of a gas path and reducing air permeability, lowering the productivity of sintered ore. Also, if the amount of molten liquid is small, unburned ore will occur, which will lead to a decrease in the yield in the sintering machine and a decrease in the productivity of sintered ore. Conversely, if the amount of molten liquid is too large, it will hinder the gas flow and cause uneven sintering.

[0017] That is, to improve the air permeability in the sintering machine, it is important to have an appropriate amount of melt and viscosity of the melt. For the above-mentioned melt control during sintering, it is important to appropriately design the adhesion layer components of the granulated material by selecting the raw materials used in granulation. However, the properties of the ore are generally fixed, and it is difficult to control the selection and amount of raw materials due to the supply and demand constraints of the ore.

[0018] Patent Document 1 does not specify the blending of high water of crystallization ore. In other words, the upper limit of the water of crystallization component in the adhesion layer is unknown. In addition, Patent Documents 2 and 3 do not specify the value of [C / F] (=CaO / Fe2O3) in the adhesion layer of the granulated material. In other words, Patent Documents 2 and 3 make it difficult to design the appropriate composition of the granulated material.

[0019] In view of the above problems, the present invention aims to provide a method for producing sintered ore that can improve the strength, productivity, etc. of sintered ore by appropriately designing the components of the granulated materials in consideration of the characteristics of the raw materials used in the granulation process in which a plurality of granulated materials are produced separately. [Means for solving the problem]

[0020] In order to achieve the above object, the present invention provides the following technical solutions.

[0021] The method for producing sintered ore according to the present invention comprises producing granulated material A and granulated material B, each of which has an adhesion layer formed around the outer periphery of a core particle, and mixing and firing the granulated material A and the granulated material B to produce sintered ore. The sintering process is characterized in that granulated material A and granulated material B that satisfy the following (1) and (2) are produced during the operation of the sintering process.

[0022] (1) The blending ratio of low alumina ore in each of granulated material A and granulated material B is ≦30 mass% (2) Weighted average [C / F] in the adhesion layer of granulated material A and granulated material B ≧ 0.115 Note that [C / F] refers to CaO (mass%) / Fe2O3 (mass%).

[0023] Preferably, when producing granulated material A and granulated material B by "gradient blending of raw materials" in which the amount of a specific raw material charged to each granulator is changed and blended, the low alumina ore is blended in a gradient manner into granulated material A so that a larger amount of low alumina ore is blended into granulated material A.

[0024] Preferably, the limestone is blended into the granulated material A at an inclination so that a larger amount of limestone is blended into the granulated material A, and the adhesion layer of the granulated material B has a ratio [C / F] of ≧0.08.

[0025] Preferably, the ore with high water of crystallization is blended into the granulated material A at an inclination so that the ore with high water of crystallization is blended in a large amount into the granulated material A, and the crystal water content in the adhesion layer of the granulated material A is ≦4.0 mass%. Effect of the Invention

[0026] According to the method for producing sintered ore of the present invention, in the granulation process in which a plurality of granules are separately produced, the strength, productivity, etc. of the sintered ore can be improved by appropriately designing the components of the granules taking into account the characteristics of the raw materials used. [Brief description of the drawings]

[0027] [Figure 1] FIG. 1 is a diagram showing a schematic outline of a sintering process for producing sintered ore. [Diagram 2] FIG. 2 is a schematic diagram showing an outline of a granulated material produced by a sintering process. [Diagram 3] FIG. 2 is a diagram showing a schematic outline of the granulation step (granulation equipment) of the present embodiment. [Figure 4] FIG. 2 is a diagram showing an example of a separate granulation method in a granulation step. [Diagram 5] FIG. 1 is a graph showing the relationship between the [C / F] of the adhesion layer of granulated material in a single granulation and the sintering rotation strength. [Figure 6] FIG. 1 is a graph showing the relationship between Canadian concentrate blends (low alumina ores) and granulation properties. [Figure 7]FIG. 13 is a diagram showing the relationship between crystal water in an adhesion layer and the variation in sintering rotation strength. [Figure 8] FIG. 1 is a schematic diagram showing an outline of an even limestone mix and a graded limestone mix. [Figure 9] FIG. 1 is a graph showing the relationship between the [C / F] of the adhesion layer of granulated material B produced by separate granulation and the sintering rotation strength. [Figure 10] FIG. 1 is a diagram showing the influence in a sintering machine when raw materials such as Canadian concentrate (low alumina ore) and Australian ore (high crystal water ore) are unevenly distributed in the granulated material 1 on one side. [Figure 11] FIG. 13 is a diagram showing the evaluation results of sinter strength and sintered ore productivity by a square pot test. [Figure 12] FIG. 1 is a flow chart showing the steps of a method for producing sintered ore according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] Hereinafter, an embodiment of the method for producing sintered ore according to the present invention will be described with reference to the drawings. Note that the embodiment described below is an example of the present invention, and the configuration of the present invention is not limited to this specific example.

[0029] The method for producing sintered ore according to the present invention was developed through the study of the points described below, and it was discovered that the strength and productivity of sintered ore can be improved by appropriately designing the components of granulated materials A and B taking into account the characteristics of the raw materials used in the granulation process in which multiple granulated materials 1 (in this embodiment, granulated materials A and B) that serve as sintering raw materials are produced separately.

[0030] That is, the method for producing sintered ore of the present invention is characterized in that, when a sintering process is carried out in which granulated material A and granulated material B, each having an adhesion layer 3 formed around the outer periphery of a core particle 2, are separately produced, and then these granulated materials A and B are mixed and fired to produce sintered ore, the following (1) and (2) are satisfied, and the granulated material A and granulated material B are produced.

[0031] (1) The blending ratio of low alumina ore in each of granulated material A and granulated material B is ≦30 mass% (2) Weighted average [C / F] in the adhesion layer of granulated material A and granulated material B ≧ 0.115 Note that [C / F] refers to CaO (mass%) / Fe2O3 (mass%).

[0032] More preferably, when producing granulated material A and granulated material B by "inclined blending of raw materials" in which the amount of specified raw materials charged to each granulator (in this embodiment, drum mixers 8 and 9) is changed and blended, the low-alumina ore is blended in an inclined manner into granulated material A so that a larger amount of low-alumina ore is blended into granulated material A.

[0033] More preferably, the limestone 4 is blended into the granulated material A at an inclination so that a larger amount of the limestone 4 is blended into the granulated material A, and the adhesion layer of the granulated material B has a [C / F] of 0.08 or more.

[0034] More preferably, the ore with high water of crystallization is blended into the granulated material A at an inclination so that the ore with high water of crystallization is blended in a large amount into the granulated material A, and the crystal water content in the adhesion layer of the granulated material A is ≦4.0 mass%.

[0035] The method for producing sintered ore according to the present invention will be described in more detail below.

[0036] When manufacturing the granulated material 1, the overall properties of the granulated material 1 are largely determined by the ores and auxiliary materials used. For example, when a single (one type) granulated material 1 is manufactured, all the granulated materials 1 show almost the same melting behavior, so that it is not possible to control the melting and assimilation state.

[0037] Therefore, by providing multiple granulation systems to produce different granulated materials 1 and assigning functions to each granulated material 1, melting and assimilation are promoted and the sintering strength and air permeability of the raw material packed bed are improved, that is, productivity is improved.

[0038] Specifically, one of the multiple granulated materials 1 (hereinafter referred to as granulated material A) is preferentially mixed (more than the other granulated material 1 (hereinafter referred to as granulated material B)) with auxiliary raw materials such as limestone, low alumina ore, and high crystal water ore to produce an easily meltable granulated material A. Granulated material A, which is mixed with a large amount of low alumina ore, produces a low-viscosity and large amount of melt liquid, so that the remaining difficult-to-melt granulated material B is drawn in during sintering and assimilated, forming a strong sintered body (sintered ore).

[0039] An outline of the sintering process for producing sintered ore is shown typically in Fig. 1. Fig. 2 shows an outline of a granulated material 1 produced in the sintering process (granulation step).

[0040] Generally, in the sintering process, iron ore is mixed with auxiliary materials (limestone 4, etc.), carbonaceous material as a heat source is added, and granulated material 1 as the sintering raw material is produced in a granulator (drum mixer 8, 9). The granulated material 1 is then loaded into a sintering machine 10 and fired to produce sintered ore as the finished product.

[0041] In the granulation process, as shown in Fig. 1, the raw materials charged into the granulator from a raw material layer 6 (raw material hopper 6) are rolled while adding water, so that limestone 4, fine ore 5, etc. adhere to the core ore 2 to form an adhesion layer 3, as shown in Fig. 2. In this way, a granulated material 1 with an adhesion layer 3 formed thereon is produced. Note that, as for the granulator, a method using, for example, a drum mixer 8 or a pan pelletizer 11 is generally used. The granulated material 1 is fired in a sintering machine 10 to produce sintered ore.

[0042] In this embodiment, in the sintering process of mixing and firing, a plurality of granulators (drum mixers 8, 9) are used to separately produce a plurality of granulated materials 1 (granulated material A, granulated material B) which are the raw material for sintered ore.

[0043] FIG. 3 shows a schematic overview of the granulation step (granulation equipment 7) of this embodiment.

[0044] As shown in Fig. 3, in this embodiment, raw materials discharged from a raw material process equipped with multiple lines are used in a granulation facility 7 equipped with two parallel lines to produce two types of granulated materials 1. Specifically, granulated material A, which is easy to melt, is granulated in a drum mixer 8 of line II, and granulated material B, which is difficult to melt, is granulated in a drum mixer 9 of line I. These granulated materials A and B are mixed and fired in a sintering machine 10 to produce sintered ore.

[0045] FIG. 4 shows an example of the separate granulation method in the granulation step.

[0046] As shown in FIG. 4, in the granulation process, raw materials extracted from a raw material process (raw material layers 6a, 6b) equipped with multiple systems are processed into separate granules 1 in multiple granulation equipment 7 (drum mixer 8, pan pelletizer 11, etc.), and each granule 1 is mixed and fed into a sintering machine 10 (the so-called separate granulation method).

[0047] In the example of Fig. 4, one type of granulated material 1 is granulated in a drum mixer 8, the other type of granulated material 1 is granulated in a pan pelletizer 11, and the two types of granulated materials 1 are mixed and fired in a sintering machine 10 to produce sintered ore. Note that the present invention is also applicable to the example of Fig. 4.

[0048] Such a separate granulation method is known as a technology that aims to improve air permeability by changing the melting behavior between multiple granulated materials 1 in the sintering machine 10. The granulated materials 1 granulated by the separate granulation method are divided into a granulated material 1 on the melt supply side (in this embodiment, granulated material A) that melts easily when fired and plays a role in assimilating the surrounding granulated materials 1 while drawing them in, and a granulated material 1 on the melt receiving side (in this embodiment, granulated material B). In other words, it is important to design the granulated material A on the melt sharing side so that it has low viscosity and generates a large amount of molten liquid. In other words, it is necessary to granulate the granulated material A that melts easily and the granulated material B that melts less easily.

[0049] In the sintering machine 10, ignition occurs from the surface of the raw material packed bed containing carbonaceous material, and the air is sucked in from below to spread the combustion. When the combustion spreads to the packed granulated material 1, a part of the granulated material 1 melts, and a calcium ferrite (CF) molten liquid is generated by the combustion heat generated when the fine coke is burned, and the molten liquid flows downward along with the flow of the sucked gas, agglomerating the fine ores with slag bonding by the molten liquid, and assimilating the other granulated material 1. The molten and assimilated granulated material 1 is cooled to obtain a sintered body (sintered ore).

[0050] At this time, the melting and assimilating characteristics between the granulated materials 1 change depending on the properties of the melt generated from the granulated material 1. For example, when a high-alumina raw material is used for the granulated material 1, the viscosity of the generated melt increases, and the highly viscous melt is difficult to flow downward, making it difficult to assimilate other granulated materials 1. In addition, the melt acts like a wall, hindering the gas flow and possibly causing a deterioration in the air permeability of the raw material packed bed. In other words, this leads to a decrease in productivity. In addition, when a difficult-to-melt raw material is used, the amount of generated melt is insufficient, resulting in poor assimilation (i.e., the occurrence of unburned parts), which leads to a decrease in productivity.

[0051] In this way, in the process of producing sintered ore, it is necessary to ensure the ventilation of the raw material packed bed in the sintering machine 10 and stably supply the air required for combustion to the raw material packed bed. For this purpose, it is necessary to appropriately mix and granulate raw materials such as iron ore and limestone 4 in the granulation process, which is a pretreatment process for sintering, to produce pseudo-particled granulated material 1.

[0052] Therefore, in the present invention, limestone 4 and fine ore 5 such as low alumina ore and high water of crystallization ore are blended in a gradient manner (blended in a larger amount than in granulated material B) in one of the granulated materials A. The "gradient blending" of the auxiliary raw materials (limestone 4 and fine ore 5 such as low alumina ore and high water of crystallization ore) when producing the granulated materials A and B will be described in detail later.

[0053] Table 1 shows the definitions of the parameters used in this embodiment.

[0054] [Table 1]

[0055] For example, as shown in Table 1, the "low alumina ore" used in this embodiment is iron ore with a low alumina content of less than 1.0 mass%. A representative example of this low alumina ore is Canadian concentrate, which is characterized by its fine particle size (-1 mm fineness rate is about 90%). However, since the alumina content is low, the viscosity of the molten liquid generated is low, but compared to other ores, In comparison, the particle size range of -1 mm, which is the adhesion layer 3, is relatively large, so the reactivity is poor and there is a lot of residue left undissolved. In addition, the ore surface is smooth and does not have good granulation properties.

[0056] The particle size is measured by sieving, with -1mm being "1mm under, passing through a sieve with 1mm openings" and +1mm being "1mm over, unable to pass through a sieve with 1mm openings."

[0057] In addition, the "high water of crystallization ore" in this embodiment is iron ore with a high water of crystallization content of 10.0 mass% or more. A representative example of high water of crystallization ore is Australian ore, which has a wide particle size distribution. However, since high water of crystallization ore contains a lot of micro-order powder, it has good melting properties and produces a large amount of melt, but the structural viscosity of the melt is high because the crystal water becomes bubbles when liberated and remains in the melt.

[0058] In this embodiment, the weighted average [C / F] (=CaO / Fe2O3) in the adhesion layer 3 of all the granulated materials 1 (granulated materials A and granulated materials B) is set to be 0.115 or more. This will be described in detail below.

[0059] The weighted average [C / F] in the adhesion layer 3 of each of the granulated material A and the granulated material B can be calculated by the following formula.

[0060] Weighted average [C / F] of granulated material A and granulated material B = weight of granulated material A / (weight of granulated material A + weight of granulated material B) × [C / F] of adhesive layer 3 of granulated material A + weight of granulated material B / (weight of granulated material A + weight of granulated material B) × [C / F] of adhesive layer 3 of granulated material B The melting starting point of the granulated material 1 during sintering is the adhesion layer 3 with a large specific surface area. The properties of the melt generated during sintering are determined by controlling the components of this adhesion layer 3 during granulation. Note that the adhesion layer 3 in this embodiment refers to an aggregate of adhesion powder composed of fine particles of -1 mm.

[0061] An index showing the melting and assimilation properties of the pseudo-particled granulated material 1 is the mass ratio of CaO to Fe2O3 in the adhesive layer 3, [C / F] (=CaO (mass%) / Fe2O3 (mass%). The higher the weighted average [C / F] value of the adhesive layer 3, the greater the relative amount of molten liquid generated, and therefore the better the melting properties. On the other hand, if the weighted average [C / F] value of the adhesive layer 3 is low, the amount of molten liquid is small, and therefore it can be determined that the melting properties are poor.

[0062] Here, the strength effect of the weighted average [C / F] of the adhesion layer 3 of the granulated material 1 was investigated by a small pot test. The test method and conditions are described in the implementation conditions section (Experiment 1) in Tables 2 and 3. In this test example, granulation was performed using a single granulation method, and the suction air volume during sintering was kept constant, so that the method can investigate the average component effect of the granulated material 1.

[0063] Table 2 shows the conditions for carrying out the small sintering pot tests (Experiment 1 and Experiment 2).

[0064] [Table 2]

[0065] Table 3 shows the raw material blending conditions during the single granulation test (Experiment 1).

[0066] [Table 3]

[0067] FIG. 5 shows the weighted average [C / F] of the adhesion layer 3 of the granulated material 1 in a single granulation and the sintering rotational strength.

[0068] As shown in Fig. 5, when the weighted average [C / F] of the adhesion layer 3 falls below 0.115, the amount of melt is insufficient, melt assimilation between each granule 1 does not progress, and the rotational strength of the sintered ore product drops sharply. In other words, the weighted average [C / F] of the average adhesion layer 3 of the granule 1 required to improve melt assimilation is ] must be 0.115 or greater.

[0069] For this reason, in the present invention, the weighted average [C / F] in the adhesive layer 3 of each of the granulated material A and the granulated material B is set to satisfy ≧0.115.

[0070] In this embodiment, when low alumina ore is charged into a granulator (drum mixer 8) for granulating a specific granulated material 1 (granulated material A), the blending ratio of the low alumina ore is set to an upper limit of 30 mass%, and the low alumina ore is blended at a gradient. This will be described in detail below.

[0071] The blending ratio of the low alumina ore can be calculated by the following formula.

[0072] Low alumina ore blending ratio = (amount of low alumina ore in granulated material A / total amount of raw materials in granulated material A) x 100 (mass%) Now, low alumina ore is ore with an alumina content of less than 1.0 mass%. A typical example of this low alumina ore is Canadian concentrate, which is characterized by fine particle size (-1 mm fineness rate is about 90%). Because it is low alumina, the viscosity of the molten liquid generated is low, but compared to other ores, the particle size is relatively large in the -1 mm particle size range that forms the adhesion layer 3, so the reactivity is poor and there is a lot of undissolved material. The surface is smooth and the granulation properties are poor. In this embodiment, Canadian concentrate is used as the low alumina ore. However, Canadian concentrate is just one example.

[0073] In addition, "gradient blending" refers to the process of producing multiple granulated materials 1 (in this embodiment, granulated material A and granulated material B) by making the blending ratio of a specific raw material in the granulated material 1 (in this embodiment, granulated material A) higher than that of the other granulated material 1 (granulated material B).

[0074] Specifically, the "gradient blending" of the auxiliary raw materials (limestone 4, and fine ores 5 such as low alumina ore and high crystal water ore) is a method of blending the amounts of the auxiliary raw materials in each of the granulation equipment 7 (drum mixers 8 and 9 in this embodiment) arranged in parallel, while keeping the total amount of the auxiliary raw materials constant (without changing the overall amount of the auxiliary raw materials), by changing the amounts of the auxiliary raw materials for each of the drum mixers 8 and 9.

[0075] For example, a large amount of auxiliary raw materials is mixed into the drum mixer 8 on one side (system A), and a small amount of auxiliary raw materials is mixed into the drum mixer 9 on the other side (system B). By mixing the auxiliary raw materials in a "tilted" manner (changing the amount of auxiliary raw materials) relative to the drum mixers 8 and 9 in this way, it is possible to simultaneously produce granulated material A with a large amount of auxiliary raw materials (highly soluble in solvent) and granulated material B with a small amount of auxiliary raw materials (lower in solvent and less soluble) (see Table 1).

[0076] In the following explanation, mixing the amounts of the auxiliary materials in each drum mixer 8 and 9 will be referred to as "graded mixing" of the auxiliary materials. For example, mixing a large amount of low-alumina ore in the granulated material A produced by the drum mixer 8 will be referred to as "graded mixing" of the low-alumina ore.

[0077] In other words, in the drum mixers 8 and 9, the amount of low alumina ore in each mixer is not the same but is varied, which is called "gradient blending of low alumina ore."

[0078] Low alumina ore generates a large amount of melt because the viscosity of the melt is low, but high water of crystallization ore generates a large amount of melt, although the viscosity of the melt is high. When low alumina ore is blended with a specific granulated material 1 (granulated material A in this embodiment) at a gradient, the melting property of the granulated material A becomes good.

[0079] Granulated material A functions as a melt donor to granulated material 1 (granulated material B) on the other side. In other words, by blending low alumina ore in the order of granulated material A > granulated material B (gradient blending), the viscosity of granulated material A on the melt supply side is reduced.

[0080] However, a typical example of low-alumina ore is Canadian concentrate, which has a fine particle size and is characterized by a high -1 mm fineness rate (about 90%). When the low-alumina ore is Canadian concentrate, most of it exists as an adhesion layer 3 in the granulated material 1.

[0081] Therefore, when the amount of low alumina ore from Canadian concentrate is increased, the iron content in the adhesion layer 3 increases and the [C / F] of the adhesion layer 3 decreases, resulting in poor melting properties. Furthermore, the thickness of the adhesion layer 3 also increases, making the fine low alumina ore that adheres in the drying zone in the sintering machine 10 more likely to peel off, which causes poor ventilation in the sintering machine 10.

[0082] Figure 6 shows the relationship between the blending of Canadian concentrate and granulation properties. Note that Canadian concentrate is shown as an example of low alumina ore.

[0083] As shown in Figure 6, Canadian concentrate has a smooth surface and good wettability, so it has poor granulation properties. Therefore, if the blending amount of Canadian concentrate in the granulator (drum mixer 8, 9) exceeds 30 mass%, the amount of ungranulated powder increases and granulation fails. For this reason, the upper limit of the blending amount of Canadian concentrate (low alumina ore) in the granulator (drum mixer 8, 9) is set to 30 mass%.

[0084] That is, in the present invention, the blending ratio of the low alumina ore in the granulated material A is set to ≦30 mass%. Also, the low alumina ore is blended in the granulated material A at a gradient so that the low alumina ore is blended in a large amount in the granulated material A.

[0085] That is, the alumina concentration in the adhesion layer 3 of the granulated material A, which is a gradient blend of low-alumina ore with an alumina content of 1.0 mass% or less, is set to be lower than the alumina concentration in the adhesion layer 3 of the other granulated material B. Also, the upper limit of the blending amount of the low-alumina ore in the granulated material A is set to 30 mass%. That is, in the granulated material A, the low-alumina ore is preferentially blended so as to maximize the blending ratio of the low-alumina ore ≦30 mass%.

[0086] In this embodiment, the ore with high water of crystallization is blended at a gradient such that the water of crystallization component in the adhesion layer 3 of the granulated material A does not exceed 4.0 mass %. This will be described in detail below.

[0087] The crystal water content in the adhesive layer 3 of the granulated material A can be calculated by the following formula. The crystal water content is based on the adhesive layer 3.

[0088] Crystal water content = the proportion of crystal water contained in the adhesion layer 3 of granulated material A (mass%) A typical example of high water of crystallization ore is Australian ore, and in this embodiment, ore with a water of crystallization content of 10 mass% or more is referred to as high water of crystallization ore. Australian ore has a wider particle size distribution and a higher water of crystallization content than Canadian concentrate (low alumina ore). High water of crystallization ore (Australian ore) contains ultrafine particles, so it has a large surface area and is easily melted. High water of crystallization ore contains a lot of micro-order powder, so it has good melting properties and produces a large amount of melt, but when the water of crystallization is released, it becomes bubbles and remains in the melt, so the structural viscosity of the melt is high.

[0089] In other words, Australian ore has a large amount of melt. However, on the other hand, the decomposition reaction of the crystal water component is an endothermic reaction, and this endothermic reaction inhibits the formation of melt. This decomposition reaction of the crystal water causes bubbles to form in the melt, and the structural viscosity of the melt is high.

[0090] However, since the amount of melt of high water of crystallization ore is relatively large, by combining Australian ore with granulated material A, which is a gradient blend of Canadian concentrate, a low alumina ore, as mentioned above, a large amount of melt with low viscosity is generated, which can function sufficiently as a melt donor. From this, it is thought that Australian ore (high water of crystallization ore) has a melting promotion effect.

[0091] In other words, by blending the high water of crystallization ore in the order of granulated material A > granulated material B (inclined blending), the amount of melt generated by granulated material A, which is the melt supplying side, is increased. The definition of inclined blending is as described above, and it means that the blending ratio of a specific raw material in granulated material A is made higher than that of other granulated material B. In other words, a large amount of high water of crystallization ore is blended into granulated material A granulated by the drum mixer 8.

[0092] In this embodiment, the high crystal water ore is the Australian ore as described above. However, the Australian ore is only one example.

[0093] FIG. 7 shows the relationship between the crystal water in the adhesion layer 3 and the variation in sintering rotation strength.

[0094] As shown in Figure 7, Tables 2 and 3, the results of the single granulation pot test (Experiment 1) showed that when the crystal water content in the adhesion layer 3 exceeds 4.0 mass%, strength variations occur, so the upper limit for the crystal water content in the adhesion layer 3 is 4.0 mass%.

[0095] That is, in the present invention, the crystal water content in the adhesion layer of the granulated material A is set to ≦4.0 mass%. Also, limestone 4 is blended into the granulated material A at an inclination so that the limestone 4 is blended in a large amount into the granulated material A.

[0096] In other words, the concentration of water of crystallization in the adhesion layer 3 of the granulated material A, which is a gradient blend of high water of crystallization ore with a water of crystallization content of 10 mass% or more, is set to be higher than the concentration of water of crystallization in the adhesion layer 3 of another granulated material B. In addition, the upper limit of the water of crystallization component in the adhesion layer 3 of one granulated material A is 4.0 mass%.

[0097] In this embodiment, limestone 4 is gradiently blended with granulated material A within a range in which [C / F] in the adhesion layer 3 of granulated material 1 other than granulated material A, i.e., granulated material B, does not fall below 0.08. This will be described in detail below.

[0098] The [C / F] of the granulated material B in the adhesive layer 3 can be calculated by the following formula. However, the standard for [C / F] of the granulated material B is based on the adhesive layer 3.

[0099] [C / F] of granulated material B = CaO ratio in adhesion layer 3 of granulated material B / Fe2O3 ratio in adhesion layer 3 of granulated material B (-) FIG. 8 shows a schematic outline of a uniform mix of limestone 4 and a gradient mix of limestone 4 according to the present invention.

[0100] As shown in Figure 8, the gradient blending of limestone 4 is a technology that aims to achieve both the breathability of the raw material packed bed and sintering strength by placing limestone 4 near specific granulated material A (gradient blending of more limestone 4 near granulated material A) compared to the normal even blending of limestone 4. The highly fluid molten liquid generated from granulated material A that melts preferentially engulfs the surrounding granulated material B as the molten liquid flows, promoting melting and assimilation.

[0101] In other words, since limestone 4 is dominant in the melting property of granulated material 1, the blending of limestone 4 is set to granulated material A > granulated material B (gradient blending) to improve the melting property of granulated material A on the melt supply side.

[0102] As mentioned above, the granulated material A, which is a low-alumina ore made in Canada, has a low [C / F] value in the adhesion layer 3 and poor melting properties. By adding limestone 4 to the granulated material A, the [C / F] value in the adhesion layer 3 can be increased, and the melting properties of the granulated material A can be ensured.

[0103] The effect of [C / F] of the adhesion layer 3 in the separate granulation method was investigated by a small pan test. The test method and conditions are described in the items of implementation conditions (Experiment 2) in Tables 2 and 4.

[0104] Table 4 shows the raw material blending conditions during the parallel granulation test (Experiment 2). In this embodiment, the granulation equipment 7 has two systems, system I and system II, and the granulation method is a drum mixer system (two systems of drum mixers 8 and 9) (see FIG. 3). In addition, the total amount in system I:total amount in system II=65:35.

[0105] [Table 4]

[0106] In this test example, two types of granulated material A and granulated material B were produced. Granulated material 1 on one side is granulated material A, which is easily soluble, with a high [C / F] value in the adhesive layer 3. Granulated material 1 on the other side is granulated material B, which is less soluble, with a low [C / F] value in the adhesive layer 3. Here, the strength effect of granulated material B (granulated material 1 with low [C / F]) was investigated. Note that the total amount of raw material used under each condition was the same, and only the distribution ratio of granulated material A / granulated material B was changed.

[0107] FIG. 9 shows the relationship between the [C / F] of the adhesion layer 3 of the granulated material B obtained by separate granulation and the sintering rotation strength.

[0108] As shown in Fig. 9, when the [C / F] of the adhesive layer 3 of the granulated material B falls below 0.08, the sintering rotation strength decreases. In other words, while maintaining the weighted average [C / F] of the average adhesive layer 3 of the granulated material A / granulated material B > 0.115, the sintering strength can be maintained as long as the [C / F] of the adhesive layer 3 of the granulated material B > 0.08.

[0109] The reason why the lower limit of the weighted average [C / F] on the granulated material B side could be relaxed from 0.115 is the effect of the separate granulation method. When the Canadian concentrate (low alumina ore) and limestone 4 are graded and mixed with the granulated material A, the [C / F] value of the adhesion layer 3 of the granulated material B is designed not to fall below 0.08.

[0110] That is, in the present invention, the adhesion layer of the granulated material B satisfies [CaO / Fe2O3]≧0.08. In addition, the high crystal water ore is blended in the granulated material A at an inclination so that the high crystal water ore is blended in a large amount in the granulated material A.

[0111] In other words, the limestone 4 is mixed according to the [C / F] of the adhesion layer 3 of the granulated materials A and B. The ratio is adjusted. Also, the value of [C / F] of the adhesion layer 3 of the granulated material B on the side where the limestone 4 is not mixed in a gradient is set so as not to fall below 0.08.

[0112] Granulated material A and granulated material B, which have been granulated while satisfying the above-mentioned constraints, are mixed and fired to produce sintered ore.

[0113] The granulated material B may be the granulated material 1 produced in a granulation facility 7 equipped with a plurality of systems (which may be arranged in parallel).

[0114] From the above, if the Canadian concentrate (low alumina ore) is unevenly distributed in the granulated material 1 on one side, the [C / F] value of the adhesion layer 3 decreases, causing a localized lack of melt in the sintering machine 10. In addition, there is a risk that the collapse of the granulated material 1 will cause a deterioration in the air permeability of the raw material packed bed.

[0115] In addition, if Australian ore (ore with high crystal water content) is unevenly distributed in the granulated material 1 on one side or the other, a highly viscous molten liquid may be generated locally, which may cause uneven burning during sintering or obstruct gas flow, resulting in a decrease in the air permeability of the raw material packed bed.

[0116] FIG. 10 shows the influence in the sintering machine 10 when Canadian concentrate (low alumina ore) or Australian ore (high crystal water ore) is unevenly distributed in the granulated material 1 on one side.

[0117] As shown in Figure 10, when the Canadian concentrate is biased (there is a bias in the raw material distribution), the fine low-alumina ore that adheres in the drying zone is more likely to peel off than when the raw material distribution is uniform. When this happens, the voids in the sintering tank (raw material packed bed) of the sintering machine 10 are filled, and the air permeability of the raw material packed bed deteriorates. This is thought to cause a decrease in the productivity of sintered ore.

[0118] In addition, in the combustion zone, a decrease in [C / F] of the adhesion layer 3 of the granulated material 1 and an increase in the crystal water content cause a localized lack of melt and an increase in the viscosity of the melt in the combustion zone. By distributing the raw materials of granulated material A / granulated material B in a way that satisfies the above-mentioned constraints on granulation and sintering, it is possible to improve sintering strength and productivity.

[0119] In a large-scale pan test, the effects of the gradient blending of limestone 4 and the preferential blending of low alumina ore and high crystal water ore were investigated. The test method and conditions are described in the item on implementation conditions in Table 5 (Experiment 3) below.

[0120] Table 5 shows the conditions for the large sintering pot test (Experiment 3).

[0121] [Table 5]

[0122] In this experimental example, the suction pressure was kept constant during sintering. The large pot test was conducted to simulate an actual sintering machine 10, and the sintering strength and productivity were also evaluated.

[0123] Examples and comparative examples carried out according to the method for producing sintered ore of the present invention are shown in Tables 6 and 7. Note that Table 6 is a continuous table, but is divided and arranged above and below for ease of viewing.

[0124] [Table 6]

[0125] [Table 7]

[0126] Figure 11 shows the results and evaluation of sinter strength and sintered ore productivity in a square pot test.

[0127] As shown in FIG. 11, Table 6, and Table 7, for condition a, the amount of limestone 4 was adjusted so that the [C / F] of the adhesion layer 3 on the I system side (granulated material B) was less than 0.08. For conditions b and c, the amount of limestone 4 was adjusted to make the [C / F] of the adhesion layer 3 of the granulated material 1 in the I system / II system, etc., equivalent. For condition d, the limestone 4 was mixed in equal amounts, and the [C / F] of the adhesion layer 3 of the granulated material 1 in the I system / II system, etc. was equivalent. In addition, for conditions e, d', and f, the limestone 4 was mixed at a gradient with respect to the II system. However, the [C / F] of the adhesion layer 3 of the granulated material 1 in the I system / II system, etc. in conditions b to d was the same.

[0128] Here, the above-mentioned granulated material B was granulated in the drum mixer 9 on the I-line side, and the granulated material A was granulated in the drum mixer 8 on the II-line side. When granulation was performed under condition a, which did not comply with the constraint of [C / F] of the adhesion layer 3 of the granulated material B on the I-line side ([C / F] of the adhesion layer 3 of the granulated material B granulated in the drum mixer 9 of the I-line side ≒ 0.07), both the sintering strength and productivity were low.

[0129] Therefore, when granulation was performed under condition b, which respected the constraints of [C / F] in the adhesion layer 3, the sintered strength improved. When Canadian concentrate, a low-alumina ore with a lot of fine powder, was used, productivity improved when it was changed from condition a and b, which biased the blending toward system I, to condition c, then to condition d, which prioritized the blending toward system II.

[0130] In this embodiment, the preferential blending means distributing the blending to the maximum extent possible to satisfy the granulation constraints (upper blending limit of Canadian concentrate (low alumina ore): 30 mass%). For example, the blending rate of low alumina ore is set close to 30 mass%, such as 29 mass%.

[0131] By using a gradient blend of limestone 4 and preferentially blending Australian ore (high crystal water ore) containing a lot of crystal water into granulated material A on the II system side, the melting promotion effect described above was obtained, and both productivity and sintered strength were maximized. Details of the blending conditions are listed in the experimental condition tables such as Tables 6 and 7 shown above.

[0132] Here, the present embodiment and a comparative example will be described.

[0133] As shown in Table 6, in the condition a of the comparative example, the blending ratio of low alumina ore in the granulated material B (I series) is 32.2 mass%, which does not satisfy the blending condition regulations, and the [C / F] of the adhesion layer 3 of the granulated material B is 0.07, which does not satisfy the component condition regulations, so the productivity and rotational strength are low. As a result, the desired results are not obtained in the overall evaluation.

[0134] In the comparative example, the mixing ratio of low alumina ore in the granulated material B (I series) is 30.7 mass%, which does not satisfy the prescribed mixing conditions, and therefore the productivity and rotational strength are low. As a result, the desired results are not obtained in the overall evaluation.

[0135] The condition c of the comparative example does not meet the requirements for the blending conditions, and therefore the desired results are not obtained in the overall evaluation. In this experimental example, the base condition is the condition c of the comparative example, in which the blending amounts of low alumina ore in the granulated material B (I series) and the granulated material A (II series) and the [C / F] of the adhesion layer 3 are the same.

[0136] Condition d of the comparative example has a smaller gradient of [C / F] of the adhesive layer 3 than condition f (this embodiment). In other words, the difference in [C / F] of the adhesive layer 3 between granulated material B (I series) and granulated material A (II series) is small at 0.01, and if the difference is at least 0.02 or more, a significant effect cannot be obtained, considering the fluctuation of the actual process. As a result, the rotation strength is low, and the desired result is not obtained as an overall evaluation.

[0137] In the comparative example, condition e, the mixing ratio of high crystal water ore in the granulated material B (I system) is 0, which does not satisfy the prescribed mixing conditions, so the rotation strength is low. As a result, the desired result is not obtained in the overall evaluation.

[0138] In the condition d' of the comparative example, the gradient of the blending ratio of high crystal water ore is smaller than that of the condition f (this embodiment), and the crystal water content of the adhesion layer is higher in the granulated material B (I series). In other words, the difference in the blending ratio of high crystal water ore between the granulated material B (I series) and the granulated material A (II series) is small. As a result, the rotation strength is low, and the desired result is not obtained as an overall evaluation. If the crystal water content of the adhesion layer is higher on the granulated material A (II series) side, the same effect as that of the condition f of this embodiment can be obtained.

[0139] In the present embodiment, the condition f satisfies the requirements for the blending conditions for the gradient blending of low alumina ore, high crystal water ore, and limestone 4 for the granulated material A (II series), and has a sufficient blending difference with respect to the granulated material B (I series). As a result, the productivity and rotational strength were improved. As a result, the desired good results were obtained as an overall evaluation.

[0140] In the sintering process (granulation step) in which multiple granulated materials A and B are produced, the composition design of granulated materials A and B taking into account the characteristics of the raw materials used (such as setting an upper limit (≦30 mass%) for the blending ratio of a specific raw material (low alumina ore) and setting upper and lower limit ranges for the [C / F] of the adhesion layer 3 (weighted average [C / F] of the adhesion layer 3 of all granulated materials 1 ≧0.115, crystal water content of the adhesion layer 3 of granulated material A ≦4.0 mass%, [C / F] of the adhesion layer 3 of granulated material B ≧0.08)) can be set to improve the melting and assimilation between each granulated material A and B during sintering, thereby improving the quality and productivity of the finished product (sintered ore).

[0141] Here, the concept of granulation design when granulating the granulated product 1 will be described below.

[0142] At least one of the multiple granulated materials 1 is mixed with Canadian concentrate (low alumina ore), limestone 4, and Australian ore (high crystal water ore) in a gradient manner. The reason is that by producing granulated material A with low alumina and a high [C / F] value of the adhesion layer 3, this granulated material A can function as a melt donor.

[0143] The upper limit of the blending amount of Canadian concentrate (low alumina ore) in each granulator (drum mixers 8 and 9 in this embodiment) is 30 mass%. The reason is that the granulation property deteriorates when the blending rate of low alumina ore is 30 mass% or more.

[0144] The upper limit of the crystal water content in the adhesion layer 3 of each granule 1 is set to 4.0 mass %. The reason for this is that localized generation of a highly viscous melt may cause uneven firing.

[0145] FIG. 12 shows the procedure of the method for producing sintered ore according to the present invention.

[0146] 12, first, it is confirmed that the weighted average [C / F] of the adhesive layer 3 of the average granulated product 1 produced from the raw material used is 0.115 or more, and that the crystal water content of the adhesive layer 3 is less than 4.0 mass%. In other words, when the weighted average [C / F] of the adhesive layer 3 is less than 0.115, or when the crystal water content of the adhesive layer 3 is 4.0 mass% or more, the present invention is not applicable, so it is confirmed.

[0147] (i) The low alumina ore is preferentially blended into one of the granules 1 (granule A). At this time, the blending ratio of the low alumina ore in the granule A is set to the maximum possible extent so as not to exceed 30 mass%.

[0148] (ii) A granulated material A, which is a mixture of low alumina ore, is mixed with high water of crystallization ore. The crystal water content of the adhesion layer 3 is set so as not to become 4.0 mass %.

[0149] (iii) Limestone 4 is added to the granulator (the drum mixer 8 on the II line side in this embodiment) that has added the low alumina ore at an inclination. At this time, the [C / F] of the adhesion layer 3 of the remaining granulated material B is set to the maximum possible value so as not to fall below 0.08.

[0150] According to the method for producing sintered ore of the present invention, in the granulation process in which multiple granulated materials A and B are produced separately, the strength and productivity of the sintered ore can be improved by appropriately designing the components of the granulated materials A and B in consideration of the characteristics of the raw materials used.

[0151] It should be noted that the embodiments disclosed herein are illustrative in all respects and should not be considered as limiting. In particular, in the embodiments disclosed herein, matters not explicitly stated, such as operating conditions, operating conditions, various parameters, dimensions, weights, volumes of components, etc., do not deviate from the scope of ordinary practice by a person skilled in the art, and values ​​that can be easily assumed by a person skilled in the art are used.

[0152] In addition, the granulated material A and the granulated material B described in detail in this embodiment are named for convenience in the description, and the naming method for them is arbitrary. That is, for the granulated material 1, A may be called B, and B may be called A. Similarly, for the granulation equipment 7 having a plurality of systems, the names I and II are named for convenience in the description, and the naming method is arbitrary. [Explanation of symbols]

[0153] 1 Granulated materials A Granules B Granules 2 nuclear particle 3. Adhesion layer 4 limestone 5. Fine ore 6 Raw material layer (raw material hopper) 7 Granulation equipment 8 Drum Mixer (II Series) 9 Drum Mixer (I System) 10 Sintering machine 11 Bread Pelletizer

Claims

1. A method for producing sintered ore, comprising the steps of producing granulated material A and granulated material B, each having an adhesion layer formed around the outer periphery of a core particle, mixing and firing the granulated material A and granulated material B to produce sintered ore, the method being characterized in that the method produces granulated material A and granulated material B that satisfy the following (1) and (2): (1) The blending ratio of low alumina ore in each of granulated material A and granulated material B is ≦30 mass% (2) Weighted average [C / F] in the adhesion layer of granulated material A and granulated material B ≧ 0.115 [C / F] is CaO (mass%) / Fe 2 O 3 (mass%).

2. When making granulated material A and granulated material B by "gradient blending of raw materials" in which the amount of the specified raw materials charged to each granulator is changed and blended, The low alumina ore is blended into the granulated material A at an inclination so that the low alumina ore is blended in a large amount into the granulated material A. The method for producing sintered ore according to claim 1 .

3. In order to mix a large amount of limestone in granulated material A, the limestone is mixed in granulated material A at an inclination, and the adhesion layer of granulated material B has a [C / F] of ≧0.

08. The method for producing sintered ore according to claim 2 .

4. In order to mix a large amount of high water of crystallization ore in the granulated material A, the high water of crystallization ore is mixed in the granulated material A at an inclination, and the water of crystallization content in the adhesion layer of the granulated material A is set to ≦4.0 mass%. The method for producing sintered ore according to claim 3 .

Citation Information

Patent Citations

  • Method for producing sintered ore for blast furnace

    JP2002105542A

  • Method for manufacturing sintered ore with little slag

    JP2003313614A

  • Method for using steel slag in sintering

    JP2020158848A

  • Method of sintered ore