Resin composition, molded product, wire coating material, construction material and metal composite material

Biomass-derived ethylene-unsaturated carboxylic acid copolymers and ethylene-based polymers are formulated into resin compositions, addressing environmental concerns by maintaining metal adhesion and mechanical properties comparable to fossil fuel-derived resins.

JP2024143110AInactive Publication Date: 2024-10-11DOW MITSUI POLYCHEMICALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023055616
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional ethylene-unsaturated carboxylic acid copolymer resins used in automobile interior and exterior materials, building materials, films, and sheets are derived from fossil fuels, posing environmental concerns due to depletion risks and high carbon dioxide emissions, and there is a need for more environmentally friendly alternatives with equivalent metal adhesion properties.

Method used

Development of ethylene-unsaturated carboxylic acid copolymers and ethylene-based polymers using biomass-derived raw materials, formulated into resin compositions with specific content ratios to achieve improved environmental friendliness and metal adhesion comparable to fossil fuel-derived resins.

Benefits of technology

The resin composition exhibits equivalent metal adhesion properties to conventional fossil fuel-derived resins while reducing environmental impact by utilizing biomass-derived components, offering improved heat resistance and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143110000001
    Figure 2024143110000001
Patent Text Reader

Abstract

To provide a resin composition with improved environmental consideration, while having metal adhesion properties comparable to those of conventional resin compositions produced using only resins obtained from fossil fuels.SOLUTION: A resin composition includes an ethylene-unsaturated carboxylic acid copolymer (A) and an ethylenic polymer (B) (excluding those corresponding to the ethylene-unsaturated carboxylic acid copolymer (A)), where the biomass level of the entire resin composition is more than 0 mass% and 100 mass% or less as measured in accordance with ASTM D6866.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a molded article, an electric wire covering material, a building material, and a metal composite material. [Background technology]

[0002] Ethylene-unsaturated carboxylic acid copolymers are used in a variety of applications, including automobile interior and exterior materials, building materials such as wallpaper and flooring, and films and sheets for miscellaneous goods, due to their excellent adhesion to metal and glass, transparency, mechanical strength, flexibility, elongation, and recovery, etc. Patent documents 1 and 2 are cited as examples of documents related to resins containing ethylene-unsaturated carboxylic acid copolymers used in such fields.

[0003] Patent Document 1 describes a laminate film for metal deposition, characterized in that (1) at least one side of a base layer has a layer for deposition made of a resin composition containing (I) 10 to 95% by weight of one or more ethylene copolymers selected from ethylene-(meth)acrylic acid ester copolymers, ethylene-(meth)acrylic acid copolymers, ethylene-unsaturated glycidyl monomer copolymers, and ethylene-unsaturated dicarboxylic anhydride-(meth)acrylic acid ester terpolymers, each containing 50 to 95% by weight of an ethylene component, and (II) 5 to 90% by weight of a crystalline polyolefin having a melting point of 110° C. or higher. The document describes that the laminate film for metal deposition can provide a laminate film having a layer for metal deposition (hereinafter referred to as a deposition layer) made of a polyolefin composition in which the adhesion of the metal deposition film is greatly improved without impairing the inherent characteristics of the polyolefin film, such as gloss.

[0004] Patent Document 2 describes a foamed wallpaper having a paper base material, a resin layer, and a picture pattern layer, characterized in that (1) the resin layer contains at least one selected from the group consisting of ethylene-vinyl acetate copolymer and ethylene-unsaturated carboxylic acid copolymer as a resin component, and (2) the picture pattern layer is formed from a water-based ink containing a urethane resin emulsion and is formed on the resin layer. It also describes that the foamed wallpaper can provide a foamed wallpaper with good adhesion of the picture pattern layer and good surface rubbing properties. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 2-39931 [Patent Document 2] JP 2007-196590 A Summary of the Invention [Problem to be solved by the invention]

[0006] On the other hand, resins containing ethylene-unsaturated carboxylic acid copolymers for use in automotive interior and exterior materials, building materials, films, and sheets are generally derived from fossil fuels. However, there are concerns that petroleum, a fossil fuel, will soon be exhausted, and it emits a large amount of carbon dioxide during the manufacturing process and disposal process after the product is made, raising concerns about its impact on global warming.

[0007] The present invention has been made in consideration of the above circumstances, and provides a resin composition that has metal adhesion equivalent to that of resin compositions produced using only conventional resins obtained from fossil fuels, while being more environmentally friendly. [Means for solving the problem]

[0008] The present inventors have found that, in a resin composition containing an ethylene-unsaturated carboxylic acid copolymer (A) and an ethylene-based polymer (B) (excluding those corresponding to the above-mentioned ethylene-unsaturated carboxylic acid copolymer (A)), by using components produced using raw materials derived from biomass for at least a part of each component, it is possible to obtain a resin composition having metal adhesion equivalent to that of a resin composition produced only using raw materials derived from conventional fossil fuels, while being improved in environmental friendliness.

[0009] The present invention provides the following resin composition, molded article, electric wire covering material, building material, and metal composite material.

[0010] [1] An ethylene-unsaturated carboxylic acid copolymer (A), An ethylene-based polymer (B) (excluding those corresponding to the ethylene-unsaturated carboxylic acid-based copolymer (A)), A resin composition comprising: The resin composition has a biomass content of more than 0 mass % and not more than 100 mass % as measured in accordance with ASTM D6866 for the entire resin composition. [2] When the total resin component of the resin composition is 100 mass%, The resin composition according to [1], wherein the content of the ethylene-unsaturated carboxylic acid copolymer (A) is from 1% by mass to 99% by mass. [3] When the total resin component of the resin composition is 100 mass%, The resin composition according to [1] or [2], wherein the content of the ethylene polymer (B) is from 1% by mass to 99% by mass. [4] The resin composition according to any one of [1] to [3], wherein the content of structural units derived from an unsaturated carboxylic acid in the ethylene-unsaturated carboxylic acid copolymer (A) is 1 mass% or more and 49 mass% or less, when the entire ethylene-unsaturated carboxylic acid copolymer (A) is taken as 100 mass%. [5] The resin composition according to any one of [1] to [4], wherein the ethylene-based polymer (B) contains a low-density polyethylene. [6] The resin composition according to any one of [1] to [5], wherein the ethylene-based polymer (B) comprises a biomass ethylene-based polymer obtained by polymerizing a monomer containing ethylene derived from biomass. [7] The resin composition according to any one of [1] to [6], wherein a total content of the ethylene-unsaturated carboxylic acid copolymer (A) and the ethylene polymer (B) is 2 mass% or more and 100 mass% or less, when the entire resin composition is taken as 100 mass%. [8] The resin composition according to any one of [1] to [7], wherein the ethylene-unsaturated carboxylic acid-based copolymer (A) contains a biomass ethylene-unsaturated carboxylic acid-based copolymer obtained by polymerizing a monomer containing ethylene derived from biomass. [9] The resin composition according to any one of [1] to [8], wherein the unsaturated carboxylic acid of the ethylene-unsaturated carboxylic acid copolymer (A) includes at least one selected from the group consisting of acrylic acid and methacrylic acid.

[10] The resin composition according to any one of [1] to [9], having a melt mass flow rate (MFR) of 0.1 g / 10 min or more and 300 g / 10 min or less, measured in accordance with JIS K 7210:1999 at 190°C under a load of 2160 g.

[11] The resin composition according to any one of [1] to

[10] , wherein a laminate of a press sheet of the resin composition obtained according to the following <Preparation of Press Sheet> and <Preparation of Laminate> and a copper plate, a titanium plate, or a zinc-plated plate has an adhesion to a copper plate, a titanium plate, or a zinc-plated plate of 70 N / 15 mm or more, as measured according to the following <Evaluation of Adhesion>. <Press sheet production> The resin composition was heated at 160°C for 4 minutes, during which degassing was performed 5 times, and then subjected to a pressure of 9.8 MPa (100 kg / cm) at 160°C for 4 minutes. 2) conditions, then press molded at 20°C, 3 minutes, 14.7 MPa (150 kg / cm 2 ) and produce a pressed sheet with a thickness of 1.0 mm. <Preparation of Laminate> The press sheet is laminated onto a 1.0 mm thick copper plate, a 1.0 mm thick titanium plate, or a 1.0 mm thick hot-dip zinc-aluminum-magnesium alloy plated steel plate, and the sheets are bonded together using a vacuum heating laminator under conditions of a temperature of 180°C, a pressure of 0 MPa (gauge pressure), and a sealing time of 2 minutes, and then bonded again under conditions of a temperature of 180°C, a pressure of 0.5 MPa (gauge pressure), and a sealing time of 6 minutes to obtain a laminate, which is then left to stand in the air and slowly cooled by natural cooling. <Evaluation of Adhesion> A test piece 75 mm long and 15 mm wide was cut out from the laminate and stored for one day in an environment of 23°C and 50% RH. Using a tensile tester in accordance with JIS K 7161-1:2014, the press sheet of the test piece was peeled off at 180° from the 1.0 mm thick copper plate, 1.0 mm thick titanium plate, or 1.0 mm thick hot-dip zinc-aluminum-magnesium alloy plated steel plate at a tensile speed of 100 mm / min, and the adhesive strength (N / 15 mm) was determined.

[12] A molded article obtained by molding the resin composition according to any one of [1] to

[11] .

[13] A wire covering material comprising the resin composition according to any one of [1] to

[11] or the molded article according to

[12] .

[14] A building material comprising the resin composition according to any one of [1] to

[11] or the molded article according to

[12] .

[15] A metal composite material comprising the resin composition according to any one of [1] to

[11] or the molded article according to

[12] . Effect of the Invention

[0011] According to the present invention, it is possible to provide a resin composition that has metal adhesion equivalent to that of conventional resin compositions produced using only fossil fuel-derived resins, while being more environmentally friendly. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, embodiments of the present invention will be described with reference to the drawings. In this specification, "A to B" indicating a range of values ​​means A or more and B or less unless otherwise specified. In addition, in this embodiment, metal adhesion refers to the interlayer adhesion strength between a copper plate, a titanium plate, or a zinc-plated plate and a press sheet of the resin composition of this embodiment in a laminate produced by laminating a press sheet of the resin composition of this embodiment to a copper plate, a titanium plate, or a zinc-plated plate.

[0013] 1.Resin composition The resin composition according to the present embodiment includes an ethylene-unsaturated carboxylic acid copolymer (A) and an ethylene-based polymer (B) (excluding those corresponding to the above-mentioned ethylene-unsaturated carboxylic acid copolymer (A)), and the biomass degree of the entire resin composition, as measured in accordance with ASTM D6866, is more than 0 mass% and 100 mass% or less.

[0014] According to the resin composition of this embodiment, it is possible to provide a resin composition which contains an ethylene-unsaturated carboxylic acid copolymer (A) and an ethylene polymer (B), and which uses components produced using raw materials derived from biomass for at least a portion of each component, thereby providing a resin composition which has metal adhesion equivalent to that of conventional resin compositions produced using only raw materials derived from fossil fuels, while being improved in environmental friendliness.

[0015] In the resin composition according to this embodiment, when the entire resin components of the resin composition are taken as 100% by mass, the content of the ethylene-unsaturated carboxylic acid copolymer (A) is, from the viewpoint of further improving metal adhesion, preferably 1% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, even more preferably 30% by mass or more, even more preferably 40% by mass or more, and even more preferably 45% by mass or more, and from the viewpoint of improving heat resistance, preferably 99% by mass or less, more preferably 90% by mass or less, even more preferably 80% by mass or less, even more preferably 70% by mass or less, even more preferably 60% by mass or less, and even more preferably 55% by mass or less.

[0016] In the resin composition according to this embodiment, when the entire resin components of the resin composition are taken as 100% by mass, the content of the ethylene-based polymer (B) is, from the viewpoint of further improving the performance balance between metal adhesion and heat resistance, preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, even more preferably 15% by mass or more, and even more preferably 20% by mass or more, and from the viewpoint of further improving metal adhesion, is preferably 99% by mass or less, more preferably 90% by mass or less, even more preferably 70% by mass or less, even more preferably 50% by mass or less, and even more preferably 35% by mass or less.

[0017] In the resin composition according to the present embodiment, when the entire resin components of the resin composition are taken as 100% by mass, the total content of the ethylene-unsaturated carboxylic acid-based copolymer (A) and the ethylene-based polymer (B) is, from the viewpoint of further improving metal adhesion, preferably 2% by mass or more, more preferably 10% by mass or more, even more preferably 30% by mass or more, even more preferably 50% by mass or more, even more preferably 60% by mass or more, even more preferably 65% ​​by mass or more, and even more preferably 70% by mass or more. There is no upper limit for the total content of the ethylene-unsaturated carboxylic acid-based copolymer (A) and the ethylene-based polymer (B), but it is, for example, 100% by mass or less.

[0018] <Ethylene-unsaturated carboxylic acid copolymer (A)> The ethylene-unsaturated carboxylic acid copolymer (A) is a copolymer of ethylene and an unsaturated carboxylic acid. The ethylene-unsaturated carboxylic acid copolymer (A) may be in the form of a block copolymer, a random copolymer or a graft copolymer. Taking into consideration suitability for extrusion lamination processing, however, it is preferable to use a binary random copolymer, a ternary random copolymer, a graft copolymer of a binary random copolymer or a graft copolymer of a ternary random copolymer, and more preferably a binary random copolymer or a ternary random copolymer.

[0019] The unsaturated carboxylic acid in the ethylene-unsaturated carboxylic acid copolymer (A) may be at least one selected from the group consisting of acrylic acid, methacrylic acid, 2-ethylacrylic acid, crotonic acid, maleic acid, fumaric acid, itaconic acid, maleic anhydride, fumaric anhydride, itaconic anhydride, monomethyl maleate, monoethyl maleate, and monoethyl maleate. Among these, the unsaturated carboxylic acid preferably includes at least one selected from the group consisting of acrylic acid and methacrylic acid, from the viewpoint of further improving the flexibility of the resulting molded article.

[0020] The ethylene-unsaturated carboxylic acid copolymer (A) is a copolymer in which at least ethylene and an unsaturated carboxylic acid are copolymerized, and may be a ternary or higher multicomponent copolymer in which a third copolymer component is further copolymerized. Examples of the third copolymerization component include unsaturated carboxylates (e.g., (meth)acrylic acid alkyl esters such as methyl acrylate, ethyl acrylate, isobutyl acrylate, n-butyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, isobutyl methacrylate, n-butyl methacrylate, isooctyl methacrylate, 2-ethylhexyl methacrylate, dimethyl maleate, and diethyl maleate), vinyl esters (e.g., vinyl acetate, vinyl propionate, and the like), unsaturated hydrocarbons (e.g., propylene, butene, 1,3-butadiene, pentene, 1,3-pentadiene, 1-hexene, and the like), oxides such as vinyl sulfate and vinyl nitrate, halogen compounds (e.g., vinyl chloride, vinyl fluoride, and the like), vinyl group-containing primary and secondary amine compounds, carbon monoxide, and sulfur dioxide. Among these, from the viewpoint of further improving flexibility, the third copolymerization component is preferably an unsaturated carboxylic acid ester, more preferably a (meth)acrylic acid alkyl ester (the alkyl moiety preferably has 1 to 4 carbon atoms). These other copolymerization components may be used alone or in combination of two or more.

[0021] The ethylene-unsaturated carboxylic acid copolymer (A) preferably contains an ethylene-unsaturated carboxylic acid copolymer obtained by polymerizing a monomer containing ethylene derived from biomass. From the viewpoint of further improving environmental friendliness, the biomass degree of the ethylene-unsaturated carboxylic acid copolymer (A) is preferably more than 0 mass%, more preferably 0.01 mass% or more, even more preferably 0.1 mass% or more, even more preferably 1 mass% or more, even more preferably 5 mass% or more, even more preferably 10 mass% or more, even more preferably 20 mass% or more, even more preferably 30 mass% or more, even more preferably 40 mass% or more, even more preferably 50 mass% or more, even more preferably 60 mass% or more, even more preferably 70 mass% or more, even more preferably 80 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, and there is no upper limit for the biomass degree of the ethylene-unsaturated carboxylic acid copolymer (A), but it is preferably 100 mass% or less. The method for producing ethylene derived from biomass and the biomass content will be described later.

[0022] The content of structural units derived from ethylene in the ethylene-unsaturated carboxylic acid copolymer (A), when the entire ethylene-unsaturated carboxylic acid copolymer (A) is taken as 100 mass%, is preferably 50 mass% or more, more preferably 55 mass% or more, even more preferably 60 mass% or more, even more preferably 65 mass% or more, even more preferably 70 mass% or more, and even more preferably 75 mass% or more from the viewpoint of further improving heat resistance, mechanical strength, etc., and is preferably 99 mass% or less, more preferably 96 mass% or less, even more preferably 93 mass% or less, and even more preferably 90 mass% or less from the viewpoint of further improving transparency.

[0023] The content of structural units derived from unsaturated carboxylic acids in the ethylene-unsaturated carboxylic acid copolymer (A), when the entire ethylene-unsaturated carboxylic acid copolymer (A) is taken as 100% by mass, is preferably 1% by mass or more, more preferably 3% by mass or more, even more preferably 5% by mass or more, and even more preferably 8% by mass or more from the viewpoint of further improving the flexibility of the obtained molded body, and is preferably 49% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and even more preferably 20% by mass or less, from the viewpoint of further improving the performance balance of processability and heat resistance.

[0024] The content of structural units derived from monomers other than ethylene and unsaturated carboxylic acid in the ethylene-unsaturated carboxylic acid copolymer (A) is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 15% by mass or less, and even more preferably 12% by mass or less, from the viewpoint of improving heat resistance, when the entire ethylene-unsaturated carboxylic acid copolymer (A) is taken as 100% by mass. There is no lower limit for the content of structural units derived from monomers other than ethylene and unsaturated carboxylic acid in the ethylene-unsaturated carboxylic acid copolymer (A), but it may be 0% by mass or more, 1% by mass or more, 5% by mass or more, or 8% by mass or more.

[0025] Here, the content of constituent units derived from ethylene, the content of constituent units derived from unsaturated carboxylic acid, and the content of constituent units derived from monomers other than ethylene and unsaturated carboxylic acid in the ethylene-unsaturated carboxylic acid copolymer (A) can be measured, for example, by Fourier transform infrared absorption spectroscopy (FT-IR).

[0026] Ethylene-unsaturated carboxylic acid copolymers can be obtained by radical polymerization of each polymer component under high temperature and pressure. Moreover, the ethylene-unsaturated carboxylic acid copolymer may be a commercially available product.

[0027] The density of the ethylene-unsaturated carboxylic acid copolymer (A), as measured in accordance with JIS K 7112:1999, is preferably 900 kg / m from the viewpoint of improving mechanical strength. 3 More preferably, it is 920 kg / m or more. 3 More preferably, 930 kg / m 3 From the viewpoint of improving extrusion lamination processability and flexibility, it is preferably 980 kg / m 3 Less than or equal to 960 kg / m 3 More preferably, 950 kg / m or less 3 The following is the result.

[0028] The melting point of the ethylene-unsaturated carboxylic acid copolymer (A), as measured by a differential scanning calorimeter (DSC), is preferably 70°C or higher, and more preferably 80°C or higher, from the viewpoint of improving heat resistance, and is preferably 130°C or lower, more preferably 120°C or lower, even more preferably 110°C or lower, and even more preferably 100°C or lower, from the viewpoint of improving metal adhesion. The melt mass flow rate (MFR) of the ethylene-unsaturated carboxylic acid copolymer (A), as measured according to JIS K 7210:1999 under conditions of 190°C and a load of 2160 g, is preferably 0.01 g / 10 min or more, more preferably 0.1 g / 10 min or more, even more preferably 1 g / 10 min or more, even more preferably 5 g / 10 min or more, even more preferably 10 g / 10 min or more, and even more preferably 20 g / 10 min or more, from the viewpoint of further improving moldability and processing stability, and is preferably 100 g / 10 min or less, more preferably 80 g / 10 min or less, even more preferably 60 g / 10 min or less, even more preferably 50 g / 10 min or less, and even more preferably 40 g / 10 min or less, from the viewpoint of further improving heat resistance, mechanical strength, and the like.

[0029] <Ethylene-based polymer (B)> The ethylene-based polymer (B) is polyethylene or a copolymer of ethylene and a polar monomer. However, the ethylene-based polymer (B) does not include those corresponding to the above-mentioned ethylene-unsaturated carboxylic acid-based copolymer (A). From the viewpoint of further improving the metal adhesion, the ethylene-based polymer (B) preferably contains polyethylene.

[0030] From the viewpoint of further improving the mechanical strength of the resulting molded article, the ethylene-based polymer (B) preferably contains polyethylene, more preferably contains at least one selected from the group consisting of low-density polyethylene (LDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE), and even more preferably contains low-density polyethylene (LDPE). The ethylene polymer (B) is produced by a high pressure process, a medium pressure process or a low pressure process, preferably by a high pressure process. The ethylene polymer (B) may be a single polymer or a mixture of two or more kinds of ethylene polymers.

[0031] Copolymers of ethylene and polar monomers include ethylene-vinyl acetate copolymers.

[0032] The ethylene polymer (B) preferably includes a biomass ethylene polymer obtained by polymerizing a monomer containing ethylene derived from biomass. From the viewpoint of further improving environmental friendliness, the biomass degree of the ethylene-based polymer (B) is preferably more than 0 mass%, more preferably 10 mass% or more, even more preferably 20 mass% or more, even more preferably 30 mass% or more, even more preferably 40 mass% or more, even more preferably 50 mass% or more, even more preferably 60 mass% or more, even more preferably 70 mass% or more, even more preferably 80 mass% or more, even more preferably 90 mass% or more, even more preferably 93 mass% or more, and there is no upper limit for the biomass degree of the ethylene-based polymer (B), but it is preferably 100 mass% or less. The method for producing ethylene derived from biomass and the biomass content will be described later.

[0033] The density of the ethylene polymer (B), as measured in accordance with JIS K 7112:1999, is preferably 900 kg / m from the viewpoint of further improving the mechanical strength. 3 More preferably, 905 kg / m 3 More preferably, 910 kg / m 3 More preferably, 915 kg / m 3 From the viewpoint of further improving the balance between metal adhesion and flexibility, it is preferably 940 kg / m 3 Less than or equal to 930 kg / m 3 More preferably, 925 kg / m 3 More preferably, 920 kg / m or less 3or less, i.e., in the range of low density polyethylene.

[0034] The melt mass flow rate (MFR) of the ethylene polymer (B), measured according to JIS K 7210:1999 under conditions of 190°C and a load of 2160 g, is not limited as long as it can be mixed with the ethylene-unsaturated carboxylic acid copolymer (A) and molded, but is preferably 0.01 g / 10 min or more, more preferably 0.1 g / 10 min or more, even more preferably 1 g / 10 min or more, even more preferably 3 g / 10 min or more, even more preferably 5 g / 10 min or more, and is preferably 100 g / 10 min or less, more preferably 70 g / 10 min or less, even more preferably 50 g / 10 min or less, even more preferably 30 g / 10 min or less, and even more preferably 10 g / 10 min or less.

[0035] <Biomass-derived ethylene> The method for producing biomass-derived ethylene according to the present embodiment is not limited, and a known method can be used. Examples of the method for producing biomass-derived ethylene are given below.

[0036] "Biomass" refers to organic resources that are primarily derived from plants and animals, excluding fossil fuels. Methods for producing biomass-derived ethylene include, for example, a method in which plant raw materials are fermented by microorganisms to produce biomass-derived ethanol (bioethanol) and then dehydrated, and a method in which ethylene is extracted from biomass naphtha, which is produced using vegetable oil waste and residual oil as raw materials. The former raw materials include non-edible raw materials and edible raw materials. Examples of non-edible raw materials include cellulosic crops such as pulp, kenaf, and rice straw, waste paper, papermaking residues, wood, charcoal, compost, natural rubber, cotton, factory flue gas, waste gas, etc. Examples of edible raw materials include carbohydrate crops such as sugarcane, soybean pulp, corn, potatoes, wheat, and rice, buckwheat, and soybeans. As the former raw materials, one or more types selected from the group consisting of these can be used. As the latter raw material, various waste materials, unused resources, resource crops, etc. can be used. Specifically, oils and fats such as rapeseed oil and soybean oil, essential oils such as eucalyptus oil, vegetable oil cakes, etc. can be used. From the viewpoint of reducing the amount of carbon dioxide generated in the life cycle from the raw material to the disposal of the plastic product, it is preferable to use ethylene extracted from biomass naphtha.

[0037] Ethylene can be extracted from biomass naphtha by known methods such as heating, cracking, distillation, and purification, in the same manner as extraction from naphtha derived from fossil fuels.

[0038] The method for producing bioethanol is not limited, and for example, ethanol can be produced by contacting edible biomass raw materials such as sugarcane and corn with ethanol-producing microorganisms, such as yeast, or products derived from their crushed products to ferment sugar, and then purifying the ethanol. Ethanol can be purified by conventional methods such as distillation, membrane separation, and extraction. As a production method using non-edible raw materials as biomass raw materials, for example, ethanol can be obtained by using synthetic gas (gas mainly composed of carbon monoxide and hydrogen) generated by burning non-edible raw materials that are waste resources such as used paper and papermaking residues, and flue gas and waste gas emitted from factories, etc. as carbon sources and fermenting them with microorganisms.

[0039] The ethanol obtained as described above can be dehydrated to obtain biomass-derived ethylene. The dehydration reaction requires certain conditions, such as the type of catalyst, heating temperature, and pressure, but any of the conventional methods can be used.

[0040] In the process of producing the biomass ethylene obtained in this way, higher alcohol and higher alkene impurities may be produced during the ethanol fermentation and dehydration steps, and therefore these by-products can be removed before or after the dehydration of the ethanol.

[0041] <Biomass ratio> In the resin composition according to this embodiment, the biomass degree of the entire resin composition, measured in accordance with ASTM D6866, exceeds 0% by mass, from the viewpoint of improving environmental friendliness, and is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, even more preferably 20% by mass or more, and even more preferably 25% by mass or more. There is no upper limit for the biomass degree of the entire resin composition, but it may be 100% by mass or less, or may be 90% by mass or less, 70% by mass or less, or may be 50% by mass or less. In ASTM D6866, radiocarbon from biomass ( 14 The biomass ratio is calculated by measuring the carbon concentration of fossil fuels. 14 C) shows a constant value, making it possible to distinguish it from biomass-derived carbon. For example, when polyethylene has a biomass content of more than 0 mass% but less than 100 mass%, it can be said to contain both biomass-derived ethylene and fossil fuel-derived ethylene.

[0042] In the present embodiment, the polymerization method for the ethylene-unsaturated carboxylic acid copolymer (A) containing biomass-derived ethylene and the ethylene polymer (B) containing biomass-derived ethylene is not limited, and a conventionally known method similar to that in the case where fossil fuel-derived ethylene is used as the raw material can be used.

[0043] <Other ingredients> The resin composition according to the present embodiment may contain various additives within the scope of the present invention. Examples of such additives include one or more additives selected from the group consisting of inorganic fillers such as silica and talc, antioxidants, weathering stabilizers, wavelength conversion materials, antistatic agents, antifogging agents, antiblocking agents, slip agents, pigments, etc. Furthermore, the resin composition according to this embodiment may contain resins other than the ethylene-unsaturated carboxylic acid copolymer (A) and the ethylene polymer (B) within the scope of the invention.

[0044] The resin composition according to the present embodiment can be prepared, for example, by simultaneously or continuously mixing the ethylene-unsaturated carboxylic acid copolymer (A), the ethylene polymer (B) and any additives, and the mixing order is not limited. As a preparation method, it is preferable to melt mix them using a single screw extruder, a twin screw extruder, a Banbury mixer, a roll, various kneaders, etc.

[0045] Hereinafter, the physical properties of the resin composition according to this embodiment will be described.

[0046] In the resin composition according to the present embodiment, the melt mass flow rate (MFR), measured in accordance with JIS K 7210:1999 under conditions of 190°C and a load of 2160g, is, from the viewpoint of further improving moldability and processability, preferably 0.1 g / 10 min or more, more preferably 1.0 g / 10 min or more, even more preferably 3.0 g / 10 min or more, even more preferably 5.0 g / 10 min or more, even more preferably 10.0 g / 10 min or more, even more preferably 13.0 g / 10 min or more, and is preferably 300 g / 10 min or less, more preferably 200 g / 10 min or less, even more preferably 100 g / 10 min or less, even more preferably 50 g / 10 min or less, and even more preferably 30 g / 10 min or less.

[0047] In the resin composition according to the present embodiment, the density measured in accordance with JIS K 7112:1999 is preferably 910 kg / m from the viewpoint of further improving the performance balance of metal adhesion and processability. 3 More preferably, 915 kg / m 3 More preferably, 920 kg / m 3 More preferably, 925 kg / m 3 From the viewpoint of further improving processability, it is preferably 950 kg / m 3 Less than or equal to 945 kg / m 3 More preferably, 940 kg / m 3 The following is the result.

[0048] In the resin composition according to the present embodiment, the melting point is preferably 70° C. or higher, more preferably 75° C. or higher, even more preferably 80° C. or higher, and even more preferably 85° C. or higher from the viewpoint of improving the balance of flexibility and processability, and is preferably 130° C. or lower, more preferably 120° C. or lower, even more preferably 110° C. or lower, and even more preferably 100° C. or lower from the viewpoint of further improving the performance balance of flexibility and processability. The melting point is measured, for example, by a differential scanning calorimeter (DSC) or the like.

[0049] In the resin composition according to the present embodiment, from the viewpoint of further improving the balance of performance among metal adhesion, processability, and heat resistance, the freezing point is preferably 60° C. or higher, more preferably 65° C. or higher, and even more preferably 68° C. or higher, and is preferably 100° C. or lower, more preferably 90° C. or lower, and even more preferably 80° C. or lower. The freezing point is measured, for example, by a differential scanning calorimeter (DSC) or the like.

[0050] In the resin composition according to the present embodiment, the latent heat of fusion is preferably 60 J / g or more, more preferably 65 J / g or more, even more preferably 70 J / g or more, even more preferably 75 J / g or more, and is preferably 130 J / g or less, more preferably 120 J / g or less, even more preferably 110 J / g or less, from the viewpoint of further improving the performance balance of metal adhesion, processability, and heat resistance. The latent heat of fusion is measured, for example, by a differential scanning calorimeter (DSC) or the like.

[0051] In the resin composition according to this embodiment, the stress at break measured in accordance with JIS K 7161-1:2014 is preferably 8 MPa or more, more preferably 10 MPa or more, and even more preferably 13 MPa or more, from the viewpoint of further improving mechanical strength such as toughness. In the resin composition according to this embodiment, the upper limit of the stress at break measured in accordance with JIS K 7161-1:2014 is not limited, but may be, for example, 30 MPa or less, or 25 MPa or less.

[0052] In the resin composition according to this embodiment, the elongation at break measured in accordance with JIS K 7161-2:2014 is, from the viewpoint of further improving flexibility, preferably 450% or more, more preferably 480% or more, even more preferably 500% or more, and even more preferably 520% ​​or more, and from the viewpoint of further improving the performance balance of mechanical strength and heat resistance, is preferably 750% or less, more preferably 730% or less, even more preferably 700% or less, and even more preferably 680% or less.

[0053] The stress at break (based on JIS K 7161-1:2014) and the elongation at break (based on JIS K 7161-2:2014) of the resin composition according to the present embodiment are measured using a tensile tester. The measurement can be performed by cutting a 3 mm thick press sheet of the resin composition according to the present embodiment into a dumbbell shape according to the above JIS standard to prepare a test piece, and pulling it under the conditions of a chuck distance of 90 mm, a pulling speed of 50 mm / min, 23°C, and a relative humidity of 50% RH. The elongation at break represents the elongation of the test piece just before break between the designated gauge points in the tensile test. The stress at break is the value obtained by dividing the tensile force at the break point by the initial cross-sectional area of ​​the test piece when the test piece breaks in the tensile test.

[0054] In the resin composition according to this embodiment, the flexural modulus at 23° C., measured in accordance with JIS K 7106:1995, is preferably 30 MPa or more, more preferably 35 MPa or more, even more preferably 40 MPa or more, and even more preferably 45 MPa or more, from the viewpoint of further improving the performance balance of heat resistance and mechanical properties, and is preferably 150 MPa or less, more preferably 140 MPa or less, even more preferably 130 MPa or less, and even more preferably 120 MPa or less, from the viewpoint of further improving the performance balance of flexibility, conformability, processability, and handleability.

[0055] In the resin composition according to this embodiment, the Shore A hardness, measured in accordance with JIS K 7215:1986, is preferably 70 or more, more preferably 75 or more, even more preferably 80 or more, and even more preferably 85 or more, from the viewpoint of further improving the performance balance of moldability and flexibility, and is preferably 120 or less, more preferably 110 or less, and even more preferably 100 or less, from the viewpoint of further improving the performance balance of moldability and flexibility.

[0056] In the resin composition according to this embodiment, the Shore D hardness, measured in accordance with JIS K 7215:1986, is preferably 30 or more, more preferably 35 or more, and even more preferably 40 or more from the viewpoint of improving heat resistance, and is preferably 70 or less, more preferably 65 or less, and even more preferably 60 or less, from the viewpoint of further improving flexibility and processability.

[0057] The Shore A hardness and the Shore D hardness are measured using a type D durometer in accordance with JIS K 7215:1986.

[0058] In the resin composition according to this embodiment, the Vicat softening point measured in accordance with JIS K 7206:2016 is preferably 40°C or higher, more preferably 45°C or higher, and even more preferably 50°C or higher, from the viewpoint of further improving the performance balance of heat resistance, flexibility, processability, and handleability, and is preferably 100°C or lower, more preferably 90°C or lower, and even more preferably 80°C or lower.

[0059] The Vicat softening point is determined as follows. Using the resin composition according to this embodiment, a thermal deformation tester is used in accordance with JIS K 7206:2016. A needle indenter is placed at the top center of a test piece obtained from a 3 mm-thick press sheet of the resin composition so that the test piece is in contact with the test piece. While applying a load of 10 N, the temperature of the heat transfer medium, silicone oil, is increased from 20°C at a heating rate of 50°C / h, and the temperature of the heat transfer medium is measured when the needle indenter penetrates 1 mm from the surface of the test piece.

[0060] The adhesion of the resin composition according to this embodiment to a copper plate is preferably 70 N / 15 mm or more, more preferably 75 N / 15 mm or more, even more preferably 80 N / 15 mm or more, even more preferably 85 N / 15 mm or more, and even more preferably 90 N / 15 mm or more. There is no upper limit to the adhesion of the resin composition according to this embodiment to a copper plate, but it may be, for example, 130 N / 15 mm or less, or 120 N / 15 mm or less.

[0061] The adhesion of the resin composition according to this embodiment to a titanium plate is preferably 70 N / 15 mm or more, more preferably 75 N / 15 mm or more, even more preferably 80 N / 15 mm or more, even more preferably 85 N / 15 mm or more, and even more preferably 90 N / 15 mm or more. There is no upper limit to the adhesion of the resin composition according to this embodiment to the titanium plate, but it may be, for example, 150 N / 15 mm or less, or 140 N / 15 mm or less.

[0062] The adhesion of the resin composition according to this embodiment to a zinc-plated plate is preferably 70 N / 15 mm or more, more preferably 75 N / 15 mm or more, even more preferably 80 N / 15 mm or more, even more preferably 85 N / 15 mm or more, even more preferably 90 N / 15 mm or more, and even more preferably 100 N / 15 mm or more. There is no upper limit to the adhesion of the resin composition according to this embodiment to a zinc-plated sheet, but it may be, for example, 180 N / 15 mm or less, or 170 N / 15 mm or less.

[0063] The adhesion of the resin composition according to this embodiment to a copper plate, a titanium plate, or a zinc-plated plate is measured as follows. (Press sheet creation) The resin composition of this embodiment is heated at 160°C for 4 minutes, during which degassing is performed 5 times, and then subjected to a compressive test at 160°C for 4 minutes under 9.8 MPa (100 kg / cm 2 ) conditions, then press molded at 20°C, 3 minutes, 14.7 MPa (150 kg / cm 2) and produce a pressed sheet with a thickness of 1.0 mm. (Preparation of Laminate) The obtained press sheet is laminated to a 1.0 mm thick copper plate, a 1.0 mm thick titanium plate, or a 1.0 mm thick hot-dip zinc-aluminum-magnesium alloy plated steel plate, and the plates are laminated using a vacuum heating laminator at a temperature of 180°C, a pressure of 0 MPa (gauge pressure), and a sealing time of 2 minutes, and then laminated at a temperature of 180°C, a pressure of 0.5 MPa (gauge pressure), and a sealing time of 6 minutes to obtain a laminate. The obtained laminate is left in the air and slowly cooled by natural cooling. The metal plates are used as they are without any processing. (Evaluation of Adhesion) Next, a test piece with a length of 75 mm and a width of 15 mm is cut out from the obtained laminate. The obtained test piece is stored for one day under an environment of 23°C and 50% RH. In accordance with JIS K 7161-1:2014, the press sheet of the test piece is peeled off at 180° from the copper plate having a thickness of 1.0 mm, the titanium plate having a thickness of 1.0 mm, or the hot-dip zinc-aluminum-magnesium alloy-plated steel plate having a thickness of 1.0 mm at a tensile speed of 100 mm / min using a tensile tester to determine the adhesive strength (N / 15 mm).

[0064] 2. Molded body The molded article of the present embodiment is obtained by molding the resin composition of the present embodiment. The molding method is not limited, and known molding methods such as extrusion molding, injection molding, compression molding, and blow molding can be used, and the molded article can be obtained by molding into various shapes such as a sheet shape, a film shape, a plate shape, and other three-dimensional shapes. The molded article of the present embodiment may be made only of the resin composition of the present embodiment, or may be made of the resin composition of the present embodiment and other components. The molded article of the present embodiment may be a part or the whole of a member.

[0065] Furthermore, the surface of the molded article of the present embodiment may be subjected to a frame treatment, a corona treatment, a plasma treatment, a hard coat treatment with an inorganic or organic compound, an antistatic treatment, an antireflection treatment, an electromagnetic shielding treatment, etc., within the scope of not impairing the effects of the present invention. These treatments can be performed on the surface of the molded article by deposition, sputtering, dipping, thermal transfer, etc.

[0066] The molded article of the present embodiment can be used in a wide range of fields, including, but not limited to, optical materials, interior or exterior parts of electric and electronic devices, trays for electronic parts, automotive materials, various machine parts, housing and building materials, pipes, tubes, toys, and daily necessities.

[0067] 3.Wire sheathing material The wire covering material of the present embodiment includes the resin composition of the present embodiment or the molded article of the present embodiment. The wire covering material of the present embodiment is a material for protecting the surface of an electric wire, which is a conductor. The wire covering material may contain a filler, a flame retardant, and the like from the viewpoint of further improving the balance of performance among insulation properties, flame retardancy, and heat dissipation properties. The wire covering material of the present embodiment may contain components contained in conventionally known wire covering materials. In addition, the wire coating material may be directly applied to the outer circumference of the conductor, or other intermediate members, such as a shield conductor or other insulators, may be interposed between the conductor and the wire coating material.

[0068] The material and diameter of the conductor are not particularly limited and can be appropriately determined depending on the application. The thickness of the wire coating is also not particularly limited and can be appropriately determined taking into account the conductor diameter, etc.

[0069] The wire covering material can be produced by, for example, extrusion coating the outer periphery of a conductor using a conventionally known extrusion molding machine after melt-kneading the resin composition according to the present embodiment using a conventionally known kneading machine such as a Banbury mixer, a pressure kneader, or a roll.

[0070] 4. Building materials The building material of the present embodiment includes the resin composition of the present embodiment or the molded article of the present embodiment. The building material of the present embodiment is not limited to being a building material, and for example, the resin composition of the present embodiment or the molded article of the present embodiment can be molded into films, tubes, hoses, tapes, sheets, etc., which can be used for, for example, flooring, wallpaper, handrails, windows, partitions, doors, etc.

[0071] 5.Metal composite materials The metal composite material of the present embodiment includes the resin composition of the present embodiment or the molded article of the present embodiment. The metal composite material of the present embodiment includes a metal material, a resin material containing the resin composition of the present embodiment, and a carbon material having a metal bonding group. The carbon material is present at the interface between the metal material and the resin material and functions as a bonding material. The method for producing the metal composite material of the present embodiment is not particularly limited, but the material can be produced by immobilizing a carbon material having a metal-binding group on the surface of a metal material, and then contacting a molten resin with the surface of the metal material on which the carbon material is immobilized, thereby bonding the metal material and the resin material.

[0072] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Furthermore, the present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES

[0073] Hereinafter, the present embodiment will be described in detail with reference to examples, etc. However, the present embodiment is not limited to the description of these examples.

[0074] [material] The following components were used. The melt flow rate (MFR) was measured at 190°C and a load of 2160g in accordance with JIS K 7210:1999. The density was measured in accordance with JIS K 7112:1999. The biomass degree was measured in accordance with ASTM D6866. The melting point was measured by differential scanning calorimetry (DSC).

[0075] <Ethylene-unsaturated carboxylic acid copolymer (A)> Ethylene-methacrylic acid copolymer 1 (content of ethylene-derived structural units: 85% by mass, content of methacrylic acid-derived structural units: 15% by mass, MFR (190°C, 2160g load): 25g / 10min, density: 940kg / m 3 , melting point: 93°C, biomass content: 0% by mass Ethylene-methacrylic acid copolymer 2 (content of structural units derived from ethylene: 80% by mass, content of structural units derived from methacrylic acid: 10% by mass, content of structural units derived from isobutyl acrylate: 10% by mass, MFR (190°C, 2160g load): 36g / 10min, density: 940kg / m 3 , melting point: 86°C, biomass content: 0% by mass

[0076] <Ethylene-based polymer (B)> Low-density polyethylene 1: Low-density polyethylene (Braskem, SBC818, MFR (190°C, 2160g load): 8.3g / 10min, density: 918kg / m 3 , Biomass content: 95%) Low-density polyethylene 2: Low-density polyethylene (manufactured by Mitsui Dow Polychemicals, MFR (190°C, 2160g load): 7.2g / 10min, density: 918kg / m 3 , Biomass content: 0%)

[0077] [Examples 1 to 6 and Comparative Examples 1 to 6] <Preparation of resin composition (P)> The materials were mixed in advance in the proportions shown in Table 1, fed into a twin-screw extruder with a screw diameter of 30 mmφ, melt-kneaded under the following extrusion conditions or melt-kneading conditions, and granulated to prepare pellets of resin composition (P).

[0078] The extrusion conditions and melt-kneading conditions in the twin-screw extruder are as follows. Screw effective length L / D: 35 ·Extruder setting temperature (℃): C1 (110), C2 (160), C3 (180), C4 (180), C5 (180), H (180), D (180) Screw speed: 200 rpm Screen mesh: 60 / 120 / 60 Output: 15kg / h

[0079] [Biomass content of resin composition (P)] The biomass degree (mass%) of the resin composition (P) obtained in each example was calculated from the biomass degree of the low-density polyethylene 1 used as the raw material and the content of the low-density polyethylene 1 when the entire resin composition (P) was taken as 100 mass%.

[0080] [Content of structural units derived from unsaturated carboxylic acid in resin composition (P)] The content (mass%) of constituent units derived from unsaturated carboxylic acid in the resin composition (P) obtained in each example was calculated from the content of constituent units derived from unsaturated carboxylic acid in the ethylene-unsaturated carboxylic acid copolymer (A) used as the raw material and the content of the ethylene-unsaturated carboxylic acid copolymer (A) when the entire resin composition (P) was taken as 100 mass%.

[0081] [MFR of resin composition (P)] The MFR (g / 10 min) of the resin composition (P) obtained in each example was measured under conditions of 190° C. and a load of 2160 g in accordance with JIS K 7210:1999.

[0082] [Density of resin composition (P)] The density (kg / cm) of the resin composition (P) obtained in each example 3 ) was measured in accordance with JIS K 7112:1999.

[0083] [Melting point, freezing point and latent heat of fusion of resin composition (P)] The melting point (° C.), solidification point (° C.) and latent heat of fusion (J / g) of the resin composition (P) obtained in each example were measured using a differential scanning calorimeter (DSC).

[0084] <Press sheet production> The resin composition (P) obtained in each example was heated at 160°C for 4 minutes, during which time it was degassed 5 times, and then it was heated at 160°C for 4 minutes and compressed under 9.8 MPa (100 kg / cm 2 ) conditions, then press molded at 20°C, 3 minutes, 14.7 MPa (150 kg / cm 2 ) and press sheets with thicknesses of 3 mm and 1.0 mm were produced.

[0085] The obtained press sheets were evaluated for stress at break, elongation at break, bending stiffness, Shore A hardness, Shore D hardness, Vicat softening point and metal adhesion according to the following methods.

[0086] [Stress at break and elongation at break] The stress at break (based on JIS K 7161-1:2014) and elongation at break (based on JIS K 7161-2:2014) of the 3 mm thick pressed sheets obtained in each example were measured using a tensile tester. The pressed sheets were cut into dumbbell test pieces conforming to the JIS standard, and measurements were made by pulling them under the conditions of chuck distance: 90 mm, tensile speed: 50 mm / min, 23°C, and relative humidity of 50% RH. The elongation at break represents the elongation of the test piece just before break between the designated gauge points in the tensile test. The stress at break is the value obtained by dividing the tensile force at the break point by the initial cross-sectional area of ​​the test piece when it breaks in the tensile test.

[0087] [Flexural rigidity] The flexural modulus (MPa) of the 3 mm thick press sheet obtained in each example was measured in accordance with JIS K 7106: 1995. The press sheet was cut into a test piece having a length of 100 mm, a width of 20 mm, and a thickness of 3 mm, and the test piece was measured at 23°C using an automatic reading type "Olsen type stiffness tester" manufactured by Toyo Seiki Seisakusho.

[0088] [Shore A hardness and Shore D hardness] The Shore A hardness and Shore D hardness of the 3 mm thick press sheet obtained in each example were measured in accordance with JIS K 7215: 1986. The press sheet was cut into a size of 100 mm in length, 20 mm in width, and 3 mm in thickness to prepare a test piece, and two of the test pieces were stacked together and measured at 23°C using a type D durometer.

[0089] [Vicat softening point] The Vicat softening point (°C) of the 3 mm thick press sheet obtained in each example was measured in accordance with JIS K 7206: 2016. Using a thermal deformation tester, a needle indenter was placed at the center of the top of the press sheet so that it was in contact with the press sheet, and while applying a load of 10 N, the temperature of the heat transfer medium, silicon oil, was increased from 20°C at a heating rate of 50°C / h, and the temperature of the heat transfer medium was measured when the needle indenter penetrated 1 mm from the surface of the test piece.

[0090] <Evaluation of adhesion to metal plate> The press sheet having a thickness of 1.0 mm obtained in each example was laminated on a copper plate (Standard Test Piece C1020P (1 / 2H), thickness: 1.0 mm), a titanium plate (Standard Test Piece TP340, thickness: 1.0 mm) or a hot-dip zinc-aluminum-magnesium alloy-plated steel plate (Nissin Steel, ZAM (registered trademark) MSM-CC-ZC90, thickness: 1.0 mm), and laminated using a vacuum heating lamination machine (NPC double vacuum chamber lamination machine, LM-50 × 50S) at a temperature of 180 ° C, a pressure of 0 MPa (gauge pressure), a sealing time of 2 minutes, and a temperature of 180 ° C, a pressure of 0.5 MPa (gauge pressure), and a sealing time of 6 minutes to produce a laminate. The obtained laminate was left in the air and slowly cooled by natural cooling. The metal plates were used as they were without any treatment.

[0091] Next, a test piece was cut out from the obtained laminate with a length of 75 mm and a width of 15 mm. The obtained test piece was stored for one day under an environment of 23°C and 50% RH. In accordance with JIS K 7161-1:2014, a tensile tester (Shimadzu Corporation, EZ-SX, 100N) was used to determine the adhesive strength (N / 15mm) when the press sheet of the test piece was peeled off at 180° from the copper plate having a thickness of 1.0 mm, the titanium plate having a thickness of 1.0 mm, or the hot-dip zinc-aluminum-magnesium alloy-plated steel plate having a thickness of 1.0 mm at a tensile speed of 100 mm / min.

[0092] The adhesion to the copper plate, titanium plate and zinc-plated plate was evaluated according to the following criteria. The results are shown in Table 1. (standard) A (Good): Adhesive strength is 70N / 15mm or more B (Poor): Adhesive strength is less than 70N / 15mm

[0093] [Table 1]

[0094] As is clear from Table 1, although the resin composition (P) of Example 1 contained raw materials derived from biomass, the adhesion to copper plate, titanium plate, and zinc-plated plate all had performance equivalent to that of the resin composition (P) (Comparative Example 1) that used only raw materials derived from fossil fuels. In addition, the resin composition (P) of Example 1 had an MFR, density, melting point, freezing point, latent heat of fusion, stress at break, elongation at break, flexural modulus, Shore A hardness, Shore D hardness and Vicat softening point that were all equivalent to those of the resin composition (P) using only raw materials derived from fossil fuels (Comparative Example 1). The same was true in comparisons between Example 2 and Comparative Example 2, Example 3 and Comparative Example 3, Example 4 and Comparative Example 4, Example 5 and Comparative Example 5, and Example 6 and Comparative Example 6.

Claims

1. An ethylene-unsaturated carboxylic acid copolymer (A), An ethylene-based polymer (B) (excluding those corresponding to the ethylene-unsaturated carboxylic acid-based copolymer (A)), A resin composition comprising: The resin composition has a biomass content of more than 0 mass% and not more than 100 mass%, as measured in accordance with ASTM D6866 for the entire resin composition.

2. When the total resin component of the resin composition is 100 mass%, The resin composition according to claim 1, wherein the content of the ethylene-unsaturated carboxylic acid copolymer (A) is 1% by mass or more and 99% by mass or less.

3. When the total resin component of the resin composition is 100 mass%, The resin composition according to claim 1 or 2, wherein the content of the ethylene polymer (B) is from 1% by mass to 99% by mass.

4. The resin composition according to any one of claims 1 to 3, wherein the content of structural units derived from unsaturated carboxylic acids in the ethylene-unsaturated carboxylic acid copolymer (A) is 1 mass% or more and 49 mass% or less, when the entire ethylene-unsaturated carboxylic acid copolymer (A) is 100 mass%.

5. The resin composition according to any one of claims 1 to 4, wherein the ethylene-based polymer (B) contains a low-density polyethylene.

6. The resin composition according to any one of claims 1 to 5, wherein the ethylene-based polymer (B) comprises a biomass ethylene-based polymer obtained by polymerizing a monomer containing ethylene derived from biomass.

7. The resin composition according to any one of claims 1 to 6, wherein a total content of the ethylene-unsaturated carboxylic acid copolymer (A) and the ethylene polymer (B) is 2 mass% or more and 100 mass% or less, when the entire resin composition is taken as 100 mass%.

8. The ethylene-unsaturated carboxylic acid copolymer (A) comprises a biomass ethylene-unsaturated carboxylic acid copolymer obtained by polymerizing a monomer containing ethylene derived from biomass. The resin composition according to any one of claims 1 to 7.

9. The resin composition according to any one of claims 1 to 8, wherein the unsaturated carboxylic acid of the ethylene-unsaturated carboxylic acid copolymer (A) comprises at least one selected from the group consisting of acrylic acid and methacrylic acid.

10. The resin composition according to any one of claims 1 to 9, wherein the melt mass flow rate (MFR) measured in accordance with JIS K 7210:1999 under conditions of 190 ° C. and a load of 2160 g is 0.1 g / 10 min or more and 300 g / 10 min or less.

11. The resin composition according to any one of claims 1 to 10, wherein a laminate of a press sheet of the resin composition obtained according to the following <Preparation of Press Sheet> and <Preparation of Laminate> and a copper plate, a titanium plate, or a zinc-plated plate has an adhesion to a copper plate, a titanium plate, or a zinc-plated plate of 70 N / 15 mm or more, as measured according to the following <Evaluation of Adhesion>. <Press sheet production> The resin composition was heated at 160° C. for 4 minutes, during which degassing was performed five times, and then subjected to a compression test at 160° C. for 4 minutes under 9.8 MPa (100 kg / cm 2 ) conditions, and then press-molded at 20°C, 3 minutes, and 14.7 MPa (150 kg / cm 2 ) to prepare a pressed sheet having a thickness of 1.0 mm. <Preparation of Laminate> The press sheet is laminated onto a copper plate having a thickness of 1.0 mm, a titanium plate having a thickness of 1.0 mm, or a hot-dip zinc-aluminum-magnesium alloy plated steel plate having a thickness of 1.0 mm, and the laminate is bonded using a vacuum heating laminator under conditions of a temperature of 180° C., a pressure of 0 MPa (gauge pressure), and a sealing time of 2 minutes, and then bonded under conditions of a temperature of 180° C., a pressure of 0.5 MPa (gauge pressure), and a sealing time of 6 minutes to obtain a laminate, which is then left to stand in the air and slowly cooled by natural cooling. <Evaluation of Adhesion> A test piece having a length of 75 mm and a width of 15 mm was cut out from the laminate and stored for one day under an environment of 23° C. and 50% RH. The press sheet of the test piece was peeled at 180° from the 1.0 mm-thick copper plate, 1.0 mm-thick titanium plate, or 1.0 mm-thick hot-dip zinc-aluminum-magnesium alloy-plated steel plate of the test piece at a tensile speed of 100 mm / min using a tensile tester in accordance with JIS K 7161-1:2014 to determine the adhesive strength (N / 15 mm).

12. A molded article obtained by molding the resin composition according to any one of claims 1 to 11.

13. A wire covering material comprising the resin composition according to any one of claims 1 to 11 or the molded article according to claim 12.

14. A building material comprising the resin composition according to any one of claims 1 to 11 or the molded article according to claim 12.

15. A metal composite material comprising the resin composition according to any one of claims 1 to 11 or the molded article according to claim 12.

Citation Information

Patent Citations

  • Laminated film for metal deposition

    JP1990039931A

  • Expanded wallpaper

    JP2007196590A