Transparent conductive film

A transparent conductive film with an amorphous layer thicker than a crystalline layer, optimized for low resistance and flexibility, addresses the trade-off by ensuring both properties are met through specific layer thickness and composition.

JP2024143151AInactive Publication Date: 2024-10-11NITTO DENKO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023055676
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Transparent conductive films face a trade-off between low resistance and flexibility, with crystalline layers offering low resistance but poor flexibility, and amorphous layers providing flexibility but high resistance.

Method used

A transparent conductive film with a structure comprising an amorphous layer thicker than a crystalline layer, where the amorphous layer is formed first and has a higher tin oxide content than the crystalline layer, ensuring a total thickness of 100 nm or more.

Benefits of technology

The film achieves both low resistance and flexibility by maintaining the amorphous layer's thickness to ensure flexibility while the crystalline layer provides stress relief, resulting in a balanced performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143151000001_ABST
    Figure 2024143151000001_ABST
Patent Text Reader

Abstract

To provide a transparent conductive film suitable for achieving both low resistance and flexibility in a transparent conductive layer.SOLUTION: A transparent conductive film X includes a transparent substrate 10 and a transparent conductive layer 20 in a thickness direction H in that order. The transparent conductive layer 20 is 100 nm or more in thickness. The transparent conductive layer 20 includes an amorphous layer 21 and a crystalline layer 22 in that order from the transparent substrate 10 side. The amorphous layer 21 is thicker than the crystalline layer 22.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a transparent conductive film. [Background technology]

[0002] Conventionally, a transparent conductive film is known that includes a resin transparent substrate and a transparent conductive layer in that order in the thickness direction. The transparent conductive layer is used as a conductive film for forming a transparent electrode in various devices such as a display panel, a touch panel, and a solar cell. The transparent conductive layer is formed as a crystalline or amorphous conductive oxide layer by forming a conductive oxide film on the transparent substrate by a sputtering method, for example. The technology related to such a transparent conductive film is described, for example, in Patent Document 1 below. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-157021 A Summary of the Invention [Problem to be solved by the invention]

[0004] The transparent conductive layer of the transparent conductive film is required to have low resistance. This requirement is particularly strong for transparent conductive films for transparent electrodes. From the viewpoint of low resistance, it is better for the transparent conductive layer to be crystalline rather than amorphous. On the other hand, it is also required for the transparent conductive layer of the transparent conductive film to be less likely to crack when bent (flexibility). In particular, transparent conductive films for devices that are repeatedly folded (foldable devices) are required to have excellent flexibility. From the viewpoint of flexibility, it is better for the transparent conductive layer to be amorphous rather than crystalline. There is such a trade-off relationship between the low resistance and flexibility of the transparent conductive layer.

[0005] The present invention provides a transparent conductive film suitable for achieving both low resistance and flexibility of a transparent conductive layer. [Means for solving the problem]

[0006] The present invention [1] includes a transparent conductive film comprising a transparent substrate and a transparent conductive layer in that order in a thickness direction, wherein the transparent conductive layer has a thickness of 100 nm or more, and the transparent conductive layer has an amorphous layer and a crystalline layer in that order from the transparent substrate side, and the amorphous layer is thicker than the crystalline layer.

[0007] The present invention [2] includes the transparent conductive film according to the above [1], in which the ratio of the thickness of the amorphous layer to the thickness of the crystalline layer is 1.2 or more.

[0008] The present invention [3] includes the transparent conductive film according to the above [1] or [2], wherein the ratio of the thickness of the amorphous layer to the thickness of the crystalline layer is 5 or less.

[0009] The present invention [4] includes the transparent conductive film according to any one of the above [1] to [3], wherein the transparent conductive layer is an indium tin composite oxide layer.

[0010] The present invention [5] includes the transparent conductive film according to the above [4], wherein the tin oxide ratio in the amorphous layer is higher than the tin oxide ratio in the crystalline layer. Effect of the Invention

[0011] In the transparent conductive film of the present invention, as described above, the transparent conductive layer has a thickness of 100 nm or more, and the transparent conductive layer has an amorphous layer and a crystalline layer in this order from the transparent substrate side, and the amorphous layer is thicker than the crystalline layer. The transparent conductive layer having a thickness of 100 nm or more is suitable for ensuring low resistance of the transparent conductive layer. In a transparent conductive layer having a thickness of 100 nm or more, the amorphous layer being thicker than the crystalline layer is suitable for ensuring flexibility of the transparent conductive layer. The transparent conductive layer having an amorphous layer and a crystalline layer in this order from the transparent substrate side is suitable for achieving both low resistance and flexibility of the transparent conductive layer. Such a transparent conductive film is suitable for achieving both low resistance and flexibility of the transparent conductive layer. [Brief description of the drawings]

[0012] [Figure 1] 1 is a schematic cross-sectional view of one embodiment of a transparent conductive film of the present invention. [Diagram 2] 2 shows an example of a method for producing the transparent conductive film shown in Fig. 1. Fig. 2A shows a preparation step, Fig. 2B shows a first layer forming step, Fig. 2C shows a second layer forming step, and Fig. 2D shows a heating step. [Diagram 3] This illustrates a case where the transparent conductive layer in the transparent conductive film shown in FIG. 1 is patterned. [Figure 4] 4 shows a bending test of the transparent conductive films of Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] A transparent conductive film X according to one embodiment of the present invention includes a transparent substrate 10 and a transparent conductive layer 20 in this order in a thickness direction H. The transparent conductive film X has a sheet shape that spreads in a direction (plane direction) perpendicular to the thickness direction H. The transparent conductive film X is an element included in, for example, a touch sensor device, a light control element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, an image display device, and the like.

[0014] The transparent substrate 10 is an element that ensures the strength of the transparent conductive film X. The transparent substrate 10 has a first surface 11 and a second surface 12 opposite to the first surface 11.

[0015] The transparent substrate 10 is, for example, a transparent resin film having flexibility. Examples of the material of the resin film include polyester resin, polyolefin resin, acrylic resin, polycarbonate resin, polyethersulfone resin, polyarylate resin, melamine resin, polyamide resin, polyimide resin, cellulose resin, and polystyrene resin. Examples of the polyester resin include polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate. Examples of the polyolefin resin include polyethylene, polypropylene, and cycloolefin polymer. Examples of the acrylic resin include polymethacrylate. From the viewpoints of transparency and strength, the material of the resin film is preferably polyester resin, and more preferably PET.

[0016] The transparent substrate 10 may have a multi-layer structure in which a cured resin layer (not shown) is formed on one or both sides of a resin film. Examples of the cured resin layer include a hard coat layer and an anti-blocking layer. The cured resin layer is a cured product of a curable resin composition. The curable resin composition contains a curable resin. Examples of the curable resin include polyester resin, acrylic urethane resin, acrylic resin (excluding acrylic urethane resin), urethane resin (excluding acrylic urethane resin), amide resin, silicone resin, epoxy resin, and melamine resin. These curable resins may be used alone or in combination of two or more kinds. Examples of the curable resin include ultraviolet-curable resin and thermosetting resin.

[0017] The curable resin composition may contain particles. Examples of the particles include inorganic oxide particles and organic particles. Examples of the inorganic oxide particle material include silica, alumina, titania, zirconia, calcium oxide, tin oxide, indium oxide, cadmium oxide, and antimony oxide. Examples of the organic particle material include polymethyl methacrylate, polystyrene, polyurethane, acrylic-styrene copolymer, benzoguanamine, melamine, and polycarbonate.

[0018] The thickness of the cured resin layer is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more, from the viewpoint of exhibiting the function of the cured resin layer in the transparent conductive film X. The thickness of the cured resin layer is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less, from the viewpoint of ensuring the transparency of the transparent conductive film X.

[0019] The first surface 11 (the surface on the transparent conductive layer 20 side) of the transparent substrate 10 may be subjected to a surface modification treatment. Examples of the surface modification treatment include a corona treatment, a plasma treatment, an ozone treatment, a primer treatment, a glow treatment, and a coupling agent treatment.

[0020] The thickness of the transparent substrate 10 is preferably 1 μm or more, more preferably 10 μm or more, even more preferably 50 μm or more, still more preferably 80 μm or more, and even more preferably 90 μm or more, from the viewpoint of ensuring the strength of the transparent conductive film X. The thickness of the transparent substrate 10 is preferably 500 μm or less, more preferably 300 μm or less, even more preferably 200 μm or less, and even more preferably 150 μm or less, from the viewpoint of ensuring the handleability of the transparent substrate 10 in the roll-to-roll system.

[0021] The total light transmittance (JIS K 7375-2008) of the transparent substrate 10 is preferably 80% or more, more preferably 85% or more, and even more preferably 88% or more, from the viewpoint of ensuring the transparency of the transparent substrate 10. The total light transmittance of the transparent substrate 10 is, for example, 100% or less.

[0022] The transparent conductive layer 20 is a film having both optical transparency and electrical conductivity. In this embodiment, the transparent conductive layer 20 is disposed on the transparent substrate 10. Specifically, the transparent conductive layer 20 contacts the first surface 11 of the transparent substrate 10. The transparent conductive layer 20 also has an amorphous layer 21 as a first layer and a crystalline layer 22 as a second layer, in this order from the transparent substrate 10 side. In this embodiment, the amorphous layer 21 contacts the transparent substrate 10. The crystalline layer 22 is disposed on the opposite side of the amorphous layer 21 from the transparent substrate 10. In this embodiment, the crystalline layer 22 contacts the amorphous layer 21. It is preferable that the crystalline layer 22 is disposed on the opposite side of the amorphous layer 21 from the transparent substrate 10 and contacts the amorphous layer 21 from the viewpoint of stress relaxation of the crystalline layer 22 when the transparent conductive film X is bent. The stress relaxation of the crystalline layer 22 during bending helps to suppress the occurrence of cracks in the transparent conductive layer 20 during bending.

[0023] In this embodiment, the amorphous layer 21 is formed of an amorphous conductive oxide. Examples of the conductive oxide include an indium-containing conductive oxide and an antimony-containing conductive oxide. Examples of the indium-containing conductive oxide include an indium tin composite oxide (ITO), an indium zinc composite oxide (IZO), an indium gallium composite oxide (IGO), and an indium gallium zinc composite oxide (IGZO). Examples of the antimony-containing conductive oxide include an antimony tin composite oxide (ATO). From the viewpoint of realizing high transparency and good electrical conductivity of the transparent conductive layer 20, the conductive oxide is preferably an indium-containing conductive oxide, and more preferably ITO. ITO may contain a metal or semimetal other than In and Sn in an amount less than the respective contents of In and Sn.

[0024] The ratio of the amount of tin oxide to the total amount of indium oxide (In2O3) and tin oxide (SnO2) in the ITO in the amorphous layer 21 (tin oxide ratio R1) is preferably 11 mass% or more, more preferably 12 mass% or more, even more preferably 12.5 mass% or more, from the viewpoint of ensuring the amorphousness of the amorphous layer 21, and is preferably 15 mass% or less, more preferably 14 mass% or less, even more preferably 13 mass% or less. From the viewpoint of ensuring the amorphousness of the amorphous layer 21, the tin oxide ratio R1 is preferably higher than the tin oxide ratio R2 of the crystalline layer 22 described below.

[0025] The tin oxide ratio in ITO can be identified, for example, as follows. First, the abundance ratio of indium atoms (In) and tin atoms (Sn) in ITO, which is the object to be measured, is determined by X-ray photoelectron spectroscopy. From the abundance ratios of In and Sn in ITO, the ratio of the number of Sn atoms to the number of In atoms in ITO is determined. This gives the tin oxide ratio in ITO. The tin oxide ratio in ITO can also be determined from the tin oxide (SnO2) content of the ITO target used during sputtering film formation.

[0026] Whether a film such as the amorphous layer 21 is an amorphous film can be determined by observing the cross section of the film (target film) with a field emission transmission electron microscope (FE-TEM). When no crystal grains are observed but an amorphous region is observed in the cross section of the target film with FE-TEM, the target film can be determined to be an amorphous film.

[0027] In this embodiment, the crystalline layer 22 is formed of a crystalline conductive oxide. Examples of the conductive oxide include the conductive oxide layer described above for the amorphous layer 21. From the viewpoint of realizing high transparency and good electrical conductivity of the transparent conductive layer 20, the conductive oxide is preferably an indium-containing conductive oxide, more preferably ITO. The material of the crystalline layer 22 and the material of the amorphous layer 21 may be different types, but are preferably the same type. The transparent conductive layer 20 having the amorphous layer 21 and the crystalline layer 22 is preferably an indium-containing conductive oxide layer, more preferably an indium tin composite oxide layer.

[0028] The ratio of the amount of tin oxide to the total amount of indium oxide and tin oxide in the ITO in the crystalline layer 22 (tin oxide ratio R2) is, from the viewpoint of ensuring the crystallinity of the crystalline layer 22, preferably 1 mass% or more, more preferably 3 mass% or more, even more preferably 5 mass% or more, and is preferably less than 11 mass%, more preferably 10.5 mass% or less, even more preferably 10 mass% or less.

[0029] Whether a film such as the crystalline layer 22 is a crystalline film can be determined by observing the cross section of the film (target film) with a field emission transmission electron microscope (FE-TEM). When no amorphous regions are identified but crystal grains are identified in the cross section of the target film with FE-TEM, the target film can be determined to be a crystalline film.

[0030] The thickness (total thickness) of the transparent conductive layer 20 is 100 nm or more. A transparent conductive layer 20 having a thickness of 100 nm or more is suitable for reducing the resistance of the transparent conductive layer 20. From the viewpoint of reducing the resistance of the transparent conductive layer 20, the thickness of the transparent conductive layer 20 is preferably 110 nm or more, more preferably 120 nm or more, and even more preferably 125 nm or more. From the viewpoint of suppressing the occurrence of cracks in the transparent conductive layer 20 when the transparent conductive film X is bent (from the viewpoint of the flexibility of the transparent conductive layer 20), the thickness of the transparent conductive layer 20 is preferably 300 nm or less, more preferably 200 nm or less, and even more preferably 150 nm or less.

[0031] The amorphous layer 21 is thicker than the crystalline layer 22. Such a configuration is suitable for ensuring the flexibility of the transparent conductive layer 20. The ratio (T1 / T2) of the thickness T1 of the amorphous layer 21 to the thickness T2 of the crystalline layer 22 is preferably 1.2 or more, and more preferably 1.5 or more, from the viewpoint of the flexibility of the transparent conductive layer 20. From the viewpoint of reducing the resistance of the transparent conductive layer 20, the ratio (T1 / T2) is preferably 5 or less, and more preferably 4 or less.

[0032] The ratio of the thickness T1 of the amorphous layer 21 to the thickness (total thickness) of the transparent conductive layer 20 is preferably more than 50%, more preferably 55% or more, and even more preferably 60% or more, from the viewpoint of the flexibility of the transparent conductive layer 20. The ratio is preferably 90% or less, more preferably 85% or less, and even more preferably 80% or less, from the viewpoint of ensuring the low resistance of the transparent conductive layer 20. Moreover, the thickness T1 of the amorphous layer 21 is preferably more than 50 nm, more preferably 60 nm or more, and even more preferably 70 nm or more, from the viewpoint of the flexibility of the transparent conductive layer 20. The thickness T1 is preferably 200 nm or less, more preferably 150 nm or less, and even more preferably 100 nm or less, from the viewpoint of ensuring the low resistance of the transparent conductive layer 20.

[0033] The ratio of the thickness T2 of the crystalline layer 22 to the thickness (total thickness) of the transparent conductive layer 20 is preferably 10% or more, more preferably 15% or more, and even more preferably 20% or more, from the viewpoint of ensuring low resistance of the transparent conductive layer 20. From the viewpoint of flexibility of the transparent conductive layer 20, the ratio is preferably less than 50%, more preferably 45% or less, and even more preferably 40% or less. Moreover, from the viewpoint of low resistance of the transparent conductive layer 20, the thickness T2 of the crystalline layer 22 is preferably 15 nm or more, more preferably 25 nm or more, even more preferably 40 nm or more, and even more preferably 50 nm or more. From the viewpoint of flexibility of the transparent conductive layer 20, the thickness T2 is preferably 70 nm or less, more preferably 65 nm or less, and even more preferably 60 nm or less.

[0034] The total light transmittance (JIS K 7375-2008) of the transparent conductive layer 20 is preferably 80% or more, more preferably 85% or more, and even more preferably 88% or more, from the viewpoint of ensuring the transparency of the transparent conductive layer 20. The total light transmittance of the transparent conductive layer 20 is, for example, 100% or less.

[0035] From the viewpoint of reducing the resistance of the transparent conductive layer 20, the specific resistance of the transparent conductive layer 20 is preferably 3.5×10 -4 Ω cm or less, preferably 3.2×10 -4 Ω cm or less, more preferably 3.0×10 -4 Ω·cm or less, more preferably 2.8×10 -4 The specific resistance of the transparent conductive layer 20 is, for example, 0.5×10 -4 Ω cm or more, 1.0×10 -4 Ω cm or more, 2.0×10 -4 The resistivity is Ω·cm or more. The method for measuring the resistivity is as described later in the Examples.

[0036] The total light transmittance (JIS K 7375-2008) of the transparent conductive film X is preferably 80% or more, more preferably 85% or more, and even more preferably 88% or more. Such a configuration is suitable for ensuring the transparency required of the transparent conductive film X when the transparent conductive film X is provided in a touch sensor device, a light control element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, an image display device, and the like. The total light transmittance of the transparent conductive film X is, for example, 100% or less. The method for measuring the total light transmittance is as described below in the examples.

[0037] The transparent conductive film X is produced, for example, as follows.

[0038] First, as shown in FIG. 2A, a transparent substrate 10 is prepared (preparation step).

[0039] Next, as shown in FIG. 2B, a first layer 21' is formed on the transparent substrate 10 (first layer formation step). The first layer 21' is an amorphous first conductive oxide layer. This first conductive oxide layer is a layer that maintains its amorphous nature after a heating step (FIG. 2D) described later. Specifically, in this step, a conductive oxide film is formed on the first surface 11 of the transparent substrate 10 by a sputtering method to form the amorphous first conductive oxide layer (first layer 21').

[0040] In the sputtering method, it is preferable to use a sputtering deposition apparatus capable of performing a film formation process by a roll-to-roll method. When a sputtering deposition apparatus of the roll-to-roll method is used in the first layer formation step, a long transparent substrate 10 as a work film is run from a pay-out roll to a take-up roll provided in the apparatus, and a material is deposited on the work film to form the first layer 21'. The running speed of the work film is, for example, 0.5 to 5 m / min. In addition, in the sputtering method, a sputtering deposition apparatus having one deposition chamber may be used, or a sputtering deposition apparatus having multiple deposition chambers arranged in order along the running path of the transparent substrate 10 may be used (the same applies to the second layer formation step described later).

[0041] In the sputtering method, specifically, a sputtering gas (inert gas) is introduced under vacuum conditions into a film-forming chamber equipped with a sputtering film-forming apparatus, while a negative voltage is applied to a target arranged on a cathode in the film-forming chamber. This generates a glow discharge to ionize gas atoms, and the gas ions collide with the target surface at high speed to eject target material from the target surface, and the ejected target material is deposited on the work film (transparent substrate 10). For example, the sintered body of the conductive oxide described above for the amorphous layer 21 is used as the target material. For example, the sputtering gas includes argon, krypton, xenon, and a mixture of these gases. The sputtering method is preferably a reactive sputtering method. In the reactive sputtering method, for example, oxygen as a reactive gas in addition to the sputtering gas is introduced into the film-forming chamber.

[0042] The conditions for film formation by sputtering (sputter film formation) in the first layer formation process (first sputter film formation conditions) are as follows, from the viewpoint of properly forming a first conductive oxide layer that maintains its amorphous nature after the heating process (Figure 2D) described below.

[0043] The ultimate vacuum in the deposition chamber before sputtering is preferably 0.9×10 -4 Pa or less. In the reactive sputtering method, the ratio of the amount of oxygen introduced to the total amount of sputtering gas and oxygen introduced into the film formation chamber is preferably 1 flow % or more, more preferably 2 flow % or more, and also preferably 8 flow % or less, more preferably 5 flow % or less. The film formation temperature (the temperature of the transparent substrate 10 on which the first layer 21' is formed) is preferably -50°C or more, more preferably -25°C or more, and also preferably 20°C or less, more preferably 0.0°C or less. By adjusting the ultimate vacuum in the first layer formation step, the oxygen introduction ratio, the film formation temperature, and the air pressure during film formation, it is possible to form a first conductive oxide layer that maintains its amorphous nature after the heating step (FIG. 2D).

[0044] In the first layer forming process, examples of the power source for applying a voltage to the target include a DC power source, an AC power source, an MF power source, and an RF power source. The power source may be a combination of a DC power source and an RF power source. The absolute value of the discharge voltage during sputtering is, for example, 50 V or more and, for example, 500 V or less. The horizontal magnetic field strength on the target is, for example, 10 mT or more and, for example, 100 mT or less.

[0045] Next, as shown in FIG. 2C, a second layer 22' is formed on the first layer 21' (second layer forming step). The second layer 22' is an amorphous second conductive oxide layer. This second conductive oxide layer is a layer that is crystallized by a heating step (FIG. 2D) described later. In this step, specifically, a conductive oxide is formed on the first layer 21' by a sputtering method to form an amorphous second conductive oxide layer (second layer 22'). The first layer 21' and the second layer 22' form an amorphous transparent conductive layer 20'.

[0046] In the sputtering method, it is preferable to use a sputtering deposition apparatus capable of performing a deposition process by a roll-to-roll method. When a roll-to-roll sputtering deposition apparatus is used in the second layer forming step, a long transparent substrate 10 with a first layer 21' is run as a work film from a pay-out roll to a take-up roll provided in the apparatus, and a material is deposited on the work film to form the second layer 22'. The method of performing the sputtering method and the fact that a reactive sputtering method is preferable as the sputtering method are the same as those described above for the first layer forming step.

[0047] The conditions for sputtering in the second layer forming step (second sputtering conditions) are as follows, from the viewpoint of appropriately forming the second conductive oxide layer that is crystallized in the heating step (FIG. 2D) described later.

[0048] The ultimate vacuum in the deposition chamber before sputtering is preferably 5.0×10 -4 Pa or less. In the reactive sputtering method, the ratio of the amount of oxygen introduced to the total amount of sputtering gas and oxygen introduced into the film formation chamber is preferably 1 flow% or more, more preferably 1.5 flow% or more, and also preferably 6 flow% or less, more preferably 3 flow% or less. The film formation temperature (the temperature of the workpiece film on which the second layer 22' is formed) is preferably -50°C or more, more preferably -25°C or more, and also preferably 20°C or less, more preferably 0.0°C or less. By adjusting the ultimate vacuum in the second layer formation process, the oxygen introduction ratio, the film formation temperature, and the air pressure during film formation, the second conductive oxide layer that is crystallized by the heating process (FIG. 2D) can be formed.

[0049] In the second layer forming step, the power supply for applying a voltage to the target, the absolute value of the discharge voltage during sputtering deposition, and the horizontal magnetic field strength above the target are the same as those described above for the first layer forming step.

[0050] In this manufacturing method, next, as shown in FIG. 2D, the second layer 22' is heated to crystallize it to form the crystalline layer 22 (heating step). Examples of heating means include an infrared heater and an oven. Examples of heating ovens include a heat medium heating oven and a hot air heating oven. The environment during heating may be either a vacuum environment or an atmospheric environment. Preferably, heating is performed in the presence of oxygen. From the viewpoint of ensuring a high crystallization rate, the heating temperature is preferably 100° C. or higher, more preferably 120° C. or higher. From the viewpoint of suppressing the influence of heating on the transparent substrate 10, the heating temperature is preferably 180° C. or lower, more preferably 160° C. or lower. From the viewpoint of sufficient crystallization of the crystalline layer 22, the heating time is preferably 5 minutes or more, preferably 10 minutes or more, and more preferably 20 minutes or more. From the viewpoint of shortening the tact time in this step, the heating time is preferably 200 minutes or less, more preferably 100 minutes or less, and more preferably 80 minutes or less.

[0051] The heating in this process crystallizes the second layer 22' while maintaining the amorphous nature of the first layer 21', thereby forming the transparent conductive layer 20 (amorphous layer 21, crystalline layer 22). In this process, methods for crystallizing the second layer 22' while maintaining the amorphous nature of the first layer 21' include increasing the tin oxide ratio or Sn concentration of the first layer 21' compared to the second layer 22', and increasing the amount of oxygen introduced during the first sputtering deposition compared to the second sputtering deposition (the higher the tin oxide ratio or Sn concentration of the first layer 21', the more difficult it is for the first layer 21' to crystallize when heated).

[0052] In this manner, the transparent conductive film X is produced.

[0053] The transparent conductive layer 20 in the transparent conductive film X may be patterned as shown in Fig. 3. The transparent conductive layer 20 can be patterned by etching the transparent conductive layer 20 through a predetermined etching mask. The patterned transparent conductive layer 20 is, for example, a wiring pattern.

[0054] In the transparent conductive film X, as described above, the transparent conductive layer 20 has a thickness of 100 nm or more, and the transparent conductive layer 20 has an amorphous layer 21 and a crystalline layer 22 in this order from the transparent substrate side, with the amorphous layer 21 being thicker than the crystalline layer 22. The transparent conductive layer 20 having a thickness of 100 nm or more is suitable for ensuring low resistance of the transparent conductive layer 20. In the transparent conductive layer 20 having a thickness of 100 nm or more, the amorphous layer 21 being thicker than the crystalline layer 22 is suitable for ensuring flexibility of the transparent conductive layer 20. The transparent conductive layer 20 having the amorphous layer 21 and the crystalline layer 22 in this order from the transparent substrate 10 side is suitable for achieving both low resistance and flexibility of the transparent conductive layer 20.

[0055] Therefore, the transparent conductive film X is suitable for achieving both low resistance and flexibility of the transparent conductive layer 20. Specific examples are as shown below in Examples and Comparative Examples. EXAMPLES

[0056] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the examples. In addition, the specific numerical values ​​of the blending amounts (contents), physical property values, parameters, etc. described below can be replaced with the upper limit (a numerical value defined as "equal to or less than") or lower limit (a numerical value defined as "equal to or more than") of the blending amounts (contents), physical property values, parameters, etc. corresponding to those described in the above-mentioned "Form for carrying out the invention".

[0057] Example 1 First, a long polyethylene terephthalate (PET) film (product name "GC100-JBN", thickness 100 μm, manufactured by Mitsubishi Chemical Corporation) was prepared as a transparent substrate.

[0058] Next, a conductive oxide film was formed on one side (first side) of the transparent substrate by reactive sputtering to form an amorphous first conductive oxide layer having a thickness T1 of 100 nm as the first layer (first layer 21' in FIG. 2B) (first layer formation process). In this process, a first sputtering deposition apparatus (DC magnetron sputtering deposition apparatus) of the roll-to-roll method was used. This apparatus is equipped with a deposition chamber in which the deposition process can be carried out while running the work film by the roll-to-roll method. The sputtering deposition conditions in this process (first sputtering deposition conditions) are as follows:

[0059] The ultimate vacuum in the deposition chamber of the first sputter deposition device was 0.9×10 -4 After evacuation to 100 Pa, argon as a sputtering gas and oxygen as a reactive gas were introduced into the deposition chamber, and the pressure in the deposition chamber was set to 0.2 Pa. The ratio of the amount of oxygen introduced to the total amount of argon and oxygen introduced into the deposition chamber was about 3.2 flow rate %. As the target, a sintered body of indium oxide and tin oxide was used, with a tin oxide ratio of 12.5 mass %. As the power source for applying voltage to the target, a DC power source was used. The horizontal magnetic field strength above the target was 30 mT. The deposition temperature (the temperature of the transparent substrate on which the first layer is formed) was -8°C. The running speed of the PET film as the work film was 2.7 m / min.

[0060] Next, a conductive oxide was deposited on the first layer on the transparent substrate by reactive sputtering to form an amorphous second conductive oxide layer having a thickness T2 of 25 nm as the second layer (second layer 22' in FIG. 2C) (second layer formation process). As a result, an amorphous transparent conductive layer (transparent conductive layer 20' in FIG. 2C) was formed on the transparent substrate. In this process, a second sputter deposition apparatus (DC magnetron sputter deposition apparatus) of the roll-to-roll method was used. This apparatus is equipped with a deposition chamber in which the deposition process can be performed while running the work film by the roll-to-roll method. The sputter deposition conditions in this process (second sputter deposition conditions) are as follows:

[0061] The ultimate vacuum in the deposition chamber of the second sputter deposition device was 5.0×10-4 After evacuation to 100 Pa, argon as a sputtering gas and oxygen as a reactive gas were introduced into the deposition chamber, and the pressure in the deposition chamber was set to 0.2 Pa. The ratio of the amount of oxygen introduced to the total amount of argon and oxygen introduced into the deposition chamber was about 1.5 flow rate %. As the target, a sintered body of indium oxide and tin oxide was used, with a tin oxide ratio of 10.0 mass %. As the power source for applying voltage to the target, a DC power source was used. The horizontal magnetic field strength above the target was 90 mT. The deposition temperature (the temperature of the work film on which the second layer is formed) was -5°C. The running speed of the PET film as the work film was 2.7 m / min.

[0062] Next, the transparent conductive layer (first layer / second layer) on the transparent substrate was heated in a hot air heating oven (heating step). In this step, the heating temperature was 140° C., and the heating time was 1 hour. This step maintained the amorphous nature of the first layer while crystallizing the second layer to form a transparent conductive layer (transparent conductive layer 20 in FIG. 2D). This transparent conductive layer has an amorphous layer (amorphous layer 21 in FIG. 2D) as the first layer after heating, and a crystalline layer (crystalline layer 22 in FIG. 2D) derived from the second layer that has been crystallized by heating.

[0063] In this manner, a transparent conductive film of Example 1 was produced. The transparent conductive layer of the transparent conductive film of Example 1 had an amorphous indium tin composite oxide layer (thickness T1 100 nm, tin oxide ratio 12.5 mass%) and a crystalline indium tin composite oxide layer (thickness T2 25 nm, tin oxide ratio 10.0 mass%), in this order from the transparent substrate side.

[0064] Example 2 The transparent conductive film of Example 2 was produced in the same manner as the transparent conductive film of Example 1, except for the following: In the first layer forming step, the first layer was formed to a thickness (T1) of 75 nm, and in the second layer forming step, the second layer was formed to a thickness (T2) of 50 nm.

[0065] [Comparative Examples 1 to 4] Each of the transparent conductive films of Comparative Examples 1 to 5 was produced in the same manner as the transparent conductive film of Example 1, except for the following: The thickness T1 of the first layer in the first layer forming step and the thickness T2 of the second layer in the second layer forming step were set to the thicknesses shown in Table 1 (the second layer was not formed in Comparative Example 1, and the first layer was not formed in Comparative Example 4).

[0066] Comparative Example 5 The transparent conductive film of Comparative Example 5 was produced in the same manner as the transparent conductive film of Comparative Example 2, except for the following. The second layer forming step and the first layer forming step were carried out in this order. In the second layer forming step, a second layer having a thickness (T2) of 75 nm was formed on the transparent substrate. In the first layer forming step, a first layer having a thickness (T1) of 50 nm was formed on the second layer.

[0067] <Layer thickness> The thickness (total thickness) of the transparent conductive layer of each of the transparent conductive films in Examples 1 and 2 and Comparative Examples 1 to 5 was measured by observation with a field emission transmission electron microscope (FE-TEM). Specifically, first, a cross-sectional observation sample of each of the transparent conductive layers in Examples 1 and 2 and Comparative Examples 1 to 5 was prepared by FIB microsampling. In the FIB microsampling method, an FIB device (product name "FB2200", manufactured by Hitachi) was used, and the acceleration voltage was set to 10 kV. Next, the cross-section of the transparent conductive layer in the cross-sectional observation sample was observed by FE-TEM, and the thickness of the transparent conductive layer was measured in the observed image. In the observation, an FE-TEM device (product name "JEM-2800", manufactured by JEOL) was used, and the acceleration voltage was set to 200 kV.

[0068] The thickness T1 of the amorphous layer (first layer) in Examples 1 and 2 and Comparative Examples 2 and 3 was measured by FE-TEM observation of a cross-sectional observation sample prepared from an intermediate product before the second layer was formed on the first layer. The thickness T2 of the crystalline layer (second layer) of each transparent conductive layer in Examples 1 and 2 and Comparative Examples 2 and 3 was determined by subtracting the thickness T1 of the first layer from the total thickness of the transparent conductive layer.

[0069] The thickness T2 of the crystalline layer (second layer) in Comparative Example 5 was measured by FE-TEM observation of a cross-sectional observation sample prepared from an intermediate product before the first layer was formed on the second layer. The thickness T1 of the amorphous layer (first layer) of the transparent conductive layer in Comparative Example 5 was determined by subtracting the thickness of the second layer from the total thickness of the transparent conductive layer.

[0070] <Crystalline> The crystallinity (amorphous, crystalline) of the first and second layers of each of the transparent conductive layers in Examples 1 and 2 and Comparative Examples 1 to 5 was examined as follows.

[0071] First, FE-TEM images were taken of the above-mentioned cross-sectional observation sample at a magnification of 2 million times (the sample preparation method and observation method were the same as those described above for the layer thickness measurement). Next, for the first and second layers in the taken images, if lattice fringes (corresponding to the presence of crystal grains) were not observed throughout the layer, the layer was evaluated as amorphous, and if lattice fringes were observed throughout the layer, the layer was evaluated as crystalline. As a result, the following was confirmed. The first layer in Examples 1 and 2 and Comparative Examples 2, 3, and 5 was amorphous, and the second layer in Examples 1 and 2 and Comparative Examples 2, 3, and 5 was crystalline. The transparent conductive layer (first layer) in Comparative Example 1 was amorphous. The transparent conductive layer (second layer) in Comparative Example 4 was crystalline. These confirmation results are shown in Table 1.

[0072] <Specific resistance> The specific resistance of the transparent conductive layer of each of the transparent conductive films of Examples 1 and 2 and Comparative Examples 1 to 5 was measured. Specifically, the measurement was as follows.

[0073] First, a measurement film measuring 100 mm x 50 mm was cut out from the transparent conductive film. Next, the surface resistance of the transparent conductive layer of the measurement film was measured by the four-terminal method in accordance with JIS K 7194 (1994). Next, the surface resistance of the transparent conductive layer was multiplied by the thickness of the transparent conductive layer to calculate the specific resistance (Ω). The values ​​are shown in Table 1.

[0074] <Flexibility> The transparent conductive layer of each of the transparent conductive films of Examples 1 and 2 and Comparative Examples 1 to 5 was examined for flexibility (resistance to cracks when bent) as follows.

[0075] First, a plurality of films (length 20 cm x width 1 cm) were cut out from the transparent conductive film as test samples. Next, as shown in FIG. 4, the test sample 31 was set on a mandrel rod 32 of a predetermined diameter. The sample 31 was bent 180° at the center in the longitudinal direction of the sample 31 so that the transparent conductive layer was located on the outer side of the bend. The ends 31a and 31b in the longitudinal direction of the sample 31 were fixed to a clip device 33. The distance between the ends 31a and 31b was substantially the same as the diameter of the mandrel rod 32. A weight 34 of 1 kg was hung from the clip device 33. The sample 31 was left stationary for 10 seconds in the state shown in FIG. 4 (bending test). Thereafter, the sample 31 was removed from the mandrel rod 32, and the clip device 33 was removed from the sample 31. Then, the transparent conductive layer of the flattened sample 31 was observed with an optical microscope to confirm the presence or absence of cracks in the transparent conductive layer (microscopic observation). Such bending tests and subsequent microscopic observations were performed on multiple samples derived from the same transparent conductive film. That is, multiple bending tests were performed on each transparent conductive film. In the multiple bending tests, the diameter of the mandrel rod 32 was successively reduced by 0.5 mm from 35 mm by replacing the mandrel rod 32. The maximum diameter of the mandrel rod 32 in which no cracks were observed in the microscopic observation is shown in Table 1 as the 180° bend diameter.

[0076] [evaluation] The transparent conductive layer of the transparent conductive film of Comparative Example 1 had a specific resistance of 3.5×10 -4 The transparent conductive layer of the transparent conductive films of Comparative Examples 2 to 5 has a large 180° bending diameter of 20 mm or more. The transparent conductive films of Comparative Examples 1 to 5 do not achieve both low resistance and flexibility of the transparent conductive layer. In contrast, the transparent conductive layer of the transparent conductive films of Examples 1 and 2 has a resistivity of 3.5×10 -4The resistance is small, ie, Ω·cm or less, and the 180° bending diameter is small, ie, less than 20 mm. In the transparent conductive films of Examples 1 and 2, the transparent conductive layer has both low resistance and flexibility.

[0077] [Table 1] [Explanation of symbols]

[0078] X Transparent conductive film H Thickness direction 10 Transparent base material 11 Page 1 12 Side 2 20 Transparent conductive layer 21 Amorphous layer 22 Crystalline Layer

Claims

1. A transparent conductive film having a transparent substrate and a transparent conductive layer in that order in a thickness direction, The transparent conductive layer has a thickness of 100 nm or more, The transparent conductive film, wherein the transparent conductive layer has an amorphous layer and a crystalline layer in this order from the transparent substrate side, and the amorphous layer is thicker than the crystalline layer.

2. The transparent conductive film according to claim 1 , wherein a ratio of a thickness of the amorphous layer to a thickness of the crystalline layer is 1.2 or more.

3. The transparent conductive film according to claim 1 , wherein a ratio of a thickness of the amorphous layer to a thickness of the crystalline layer is 5 or less.

4. The transparent conductive film according to claim 1 , wherein the transparent conductive layer is an indium tin composite oxide layer.

5. The transparent conductive film according to claim 4 , wherein the tin oxide percentage of the amorphous layer is higher than the tin oxide percentage of the crystalline layer.

Citation Information

Patent Citations

  • Transparent conductive film

    JP1996174746A

  • Transparent electrode

    JP1996180748A

  • Photovoltaic device

    JP1998242494A

  • Transparent conductive and touch panel

    JP2010061942A

  • Substrate for solar cell, solar cell, organic thin film solar cell, process for production of substrate for solar cell, and process for production of organic thin film solar cell

    JP2011181904A