Metal carbide-coated carbon material
By controlling the chlorine concentration, thickness, and surface properties of the metal carbide coating on carbon materials, the yield of semiconductor single crystals is improved, addressing the issue of crystal polymorphism and extending the product life of growth components.
Patent Information
- Application Number
- JP2023055681
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
SiC single crystals grown using metal carbide-coated carbon materials as crucibles and guide members exhibit lower yield due to crystal polymorphism, which is caused by high chlorine concentration in the metal carbide coating film.
A metal carbide-coated carbon material with a chlorine concentration in the coating film of 25000 ppm μm or less, a thickness of 10 μm to 100 μm, and a specific surface roughness and thermal expansion coefficient is used to suppress crystal polymorphism, thereby improving yield.
The yield of semiconductor single crystals is enhanced by reducing chlorine concentration in the metal carbide coating film, leading to improved product life and reduced occurrence of crystal polymorphism during growth.
Smart Images

Figure 2024143155000003 
Figure 2024143155000004 
Figure 2024143155000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal carbide-coated carbon material in which the surface of a carbon substrate is coated with a metal carbide coating film. [Background technology]
[0002] Carbides such as tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide, and tungsten carbide have a high melting point and are excellent in chemical stability, strength, toughness, and corrosion resistance. Therefore, by coating a carbon substrate with a carbide, the properties of the carbon substrate, such as heat resistance, chemical stability, strength, toughness, and corrosion resistance, can be improved. Carbide-coated carbon materials, in which a carbide film is coated on the surface of a carbon substrate, particularly tantalum carbide-coated carbon materials, are used as components of semiconductor single crystal manufacturing equipment for Si (silicon), SiC (silicon carbide), GaN (gallium nitride), and the like.
[0003] The sublimation recrystallization method (modified Lely process) is widely known as a method for producing bulk single crystals of SiC. In this method, the inside of a crucible is filled with SiC raw material, and a SiC seed crystal is placed on top of it. A cylindrical guide member is also installed around the SiC seed crystal. The sublimation gas generated by heating the SiC raw material rises along the inner wall of the guide member, and the SiC single crystal grows on the SiC seed crystal.
[0004] Also, SiC single crystal substrates used in semiconductor devices and the like are manufactured by epitaxially growing SiC single crystals on SiC substrates made of bulk single crystals. Known methods for epitaxially growing SiC single crystals include liquid phase epitaxy (LPE), vapor phase epitaxy (VPE), and chemical vapor deposition (CVD). Usually, the method for epitaxially growing SiC single crystals is the CVD method. In the epitaxial growth method using the CVD method, the SiC substrate is placed on a susceptor in the equipment and raw material gas is supplied at a high temperature of 1500°C or higher to grow the SiC single crystal.
[0005] In such a method for producing a SiC single crystal, in order to obtain a higher quality crystal, Patent Document 1 discloses a method using a crucible whose graphite base has an inner surface coated with tantalum carbide, and Patent Document 2 discloses a method using a guide member whose inner wall is coated with tantalum carbide. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2019-99453 A [Patent Document 2] JP 2019-108611 A Summary of the Invention [Problem to be solved by the invention]
[0007] It is known that SiC single crystals grown using a metal carbide-coated carbon material as a crucible or guide member have a higher crystal growth yield than those grown using uncoated carbon material. However, even when a metal carbide-coated carbon material is used, further yield improvement is required. The main causes of yield reduction include point defects, extended defects (dislocations, stacking faults), and crystal polymorphism (polytype). Among these, the present invention attempts to improve the yield of semiconductor single crystals by focusing on suppressing crystal polymorphism.
[0008] Therefore, an object of the present invention is to suppress the crystal polymorphism of semiconductor single crystals and improve the yield by using a metal carbide-coated carbon material. [Means for solving the problem]
[0009] As a result of intensive research, the present inventors discovered that by setting the chlorine concentration in the metal carbide coating film of a metal carbide-coated carbon material to 25,000 ppm μm or less, it is possible to suppress the crystal polymorphism of the semiconductor single crystal and improve the yield of the semiconductor single crystal, and thus completed the present invention. [1] A metal carbide-coated carbon material comprising a carbon substrate containing carbon as a main component and a metal carbide coating film coating at least a portion of the carbon substrate, wherein the metal carbide coating film is at least one metal carbide selected from the group consisting of tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide and tungsten carbide, and the chlorine concentration in the metal carbide coating film is 25,000 ppm μm or less. [2] The metal carbide-coated carbon material according to the above [1], wherein the metal carbide coating film has a thickness of 10 μm or more and 100 μm or less. [3] The metal carbide-coated carbon material according to the above [1] or [2], wherein the metal carbide coating film has a surface having an arithmetic mean roughness Ra of 0.1 μm or more and 9.5 μm or less. [4] The metal carbide coated carbon material according to any one of the above [1] to [3], wherein the arithmetic mean roughness Ra of the surface of the carbon substrate is 0.1 μm or more and 10.0 μm or less. [5] The linear thermal expansion coefficient of the carbon substrate is 3.5 × 10 -6 / ℃ or more, 8.2×10 -6 The metal carbide-coated carbon material according to any one of the above [1] to [4], wherein the temperature is 0.1 to 1.5° C. / ° C. or lower. [6] The metal carbide-coated carbon material according to any one of the above [1] to [5], wherein the metal carbide constituting at least the surface of the metal carbide coating film is tantalum carbide. [7] The metal carbide-coated carbon material according to any one of the above [1] to [6], wherein the metal carbide constituting the metal carbide coating film is tantalum carbide. Effect of the Invention
[0010] According to the present invention, the occurrence of crystal polymorphism during crystal growth and epitaxial growth of a semiconductor single crystal can be suppressed, thereby improving the yield of the semiconductor single crystal. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic diagram of an external heat type reduced pressure CVD apparatus according to an embodiment of the present invention. [Diagram 2]FIG. 1 is a schematic diagram of a reduced pressure heating furnace for growing semiconductor single crystals according to an embodiment of the present invention. [Diagram 3] 1 is a schematic diagram of a semiconductor single crystal epitaxial growth apparatus according to an embodiment of the present invention. [Figure 4] 1 shows the results of a GDMS analysis of the tantalum carbide-coated carbon material of Example 1. [Diagram 5] 1 shows the results of cross-sectional SEM observation of the tantalum carbide-coated carbon material of Example 1. [Figure 6] 1 shows the results of SEM observation of the surface of the tantalum carbide-coated carbon material of Example 1. [Figure 7] FIG. 2 is a diagram for explaining a method for measuring the adhesion strength of a tantalum carbide coating film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The metal carbide-coated carbon material of the present invention will be described using a tantalum carbide-coated carbon material as an example.
[0013] [Tantalum carbide coated carbon material] A tantalum carbide-coated carbon material according to one embodiment of the present invention comprises a carbon substrate containing carbon as a main component, and a tantalum carbide coating film coating at least a portion of the carbon substrate, and the chlorine concentration in the tantalum carbide coating film is 25,000 ppm·μm or less.
[0014] (Carbon substrate) The carbon substrate in the tantalum carbide-coated carbon material according to one embodiment of the present invention is a substrate mainly composed of carbon. The carbon substrate may further contain chlorine. Examples of the carbon substrate material include isotropic graphite, extruded graphite, pyrolytic graphite, and carbon fiber-reinforced carbon composite material (C / C composite). The shape and characteristics of the carbon substrate are not particularly limited, and the carbon substrate may be processed into any shape depending on the application.
[0015] <Arithmetic surface roughness Ra> The arithmetic mean roughness Ra of the surface of the carbon substrate affects the semiconductor single crystal growth and epitaxial growth. The larger the arithmetic mean roughness Ra of the surface of the carbon substrate, the greater the peel strength between the carbon substrate and the tantalum carbide coating film, so the arithmetic mean roughness Ra of the surface of the carbon substrate is preferably 0.1 μm or more. On the other hand, if the arithmetic mean roughness Ra of the surface of the carbon substrate is too large, the specific surface area of the carbon substrate increases, and the tantalum carbide coating film is likely to crack or peel off. As a result, when the tantalum carbide-coated carbon material is used as a member for semiconductor single crystal growth or epitaxial growth, the product life of the member may be shortened. Therefore, from the viewpoint of the product life of the tantalum carbide-coated carbon material, the arithmetic mean roughness Ra of the surface of the carbon substrate is preferably 10.0 μm or less.
[0016] Considering the occurrence rate of cracks and peeling of the tantalum carbide coating film, the arithmetic mean roughness Ra of the surface of the carbon substrate is preferably 0.1 μm or more and 10.0 μm or less, and more preferably 2.0 μm or more and 6.0 μm or less. By making the arithmetic mean roughness Ra of the surface of the carbon substrate within the above range, the peel strength between the carbon substrate and the tantalum carbide coating film can be 10 MPa or more, and the product life of the member when the tantalum carbide-coated carbon material is used as a member for semiconductor single crystal growth and epitaxial growth can be extended. The arithmetic mean roughness Ra of the surface of the carbon substrate is a value measured based on JIS B 0633:2001 (ISO 4288:1996).
[0017] <Linear thermal expansion coefficient> The linear thermal expansion coefficient of the carbon substrate is preferably 3.5×10 -6 / ℃ or more, 8.2×10 -6 / ℃ or less. The linear thermal expansion coefficient of the carbon substrate is 3.5×10 -6 / ℃ or more, 8.2×10 -6 When the linear thermal expansion coefficient of the carbon substrate is less than 0.5.0×10 / °C, the occurrence of microcracks in the tantalum carbide coating film can be further suppressed. From this viewpoint, the linear thermal expansion coefficient of the carbon substrate is more preferably less than 0.5.0×10 / °C. -6 ~7.5×10-6 / ℃. The linear thermal expansion coefficient of the tantalum carbide coating is approximately 6.3×10 -6 / °C. The linear thermal expansion coefficient of the carbon substrate can be measured in accordance with JIS R 1618.
[0018] (Tantalum carbide coating) The tantalum carbide coating film is mainly composed of tantalum carbide, and the chlorine concentration in the tantalum carbide coating film is 25000 ppm·μm or less. The tantalum carbide coating film may cover a part of the carbon substrate, or may cover the entire carbon substrate. In this specification, the chlorine concentration is based on mass.
[0019] <Chlorine concentration> In one embodiment of the present invention, the tantalum carbide coating film of the tantalum carbide-coated carbon material has a chlorine concentration of 25,000 ppm μm or less. If the chlorine concentration in the tantalum carbide coating film is greater than 25,000 ppm μm, crystal polymorphism occurs in the semiconductor single crystal during crystal growth and epitaxial growth of the semiconductor single crystal, resulting in a decrease in the yield of the semiconductor single crystal. From this viewpoint, the chlorine concentration in the tantalum carbide coating film is preferably 10000 ppm·μm or less, more preferably 5000 ppm·μm or less, even more preferably 4000 ppm·μm or less, even more preferably 3000 ppm·μm or less, even more preferably 1000 ppm·μm or less, even more preferably 300 ppm·μm or less, even more preferably 200 ppm·μm or less, even more preferably 150 ppm·μm or less, even more preferably 100 ppm·μm or less, even more preferably 50 ppm·μm or less, and particularly preferably 30 ppm·μm or less. The lower limit of the range of the chlorine concentration in the tantalum carbide coating film is not particularly limited, but is usually 0.1 ppm·μm or more, or 1 ppm·μm. The chlorine concentration in the tantalum carbide coating film can be measured by the method described in the Examples below.
[0020] <Explanation of the mechanism of the decrease in the rate of crystal polymorphism due to the decrease in the chlorine concentration in the tantalum carbide coating film> Next, the mechanism by which the rate of crystal polymorphism is reduced by reducing the chlorine concentration in the tantalum carbide coating film will be explained, but this explanation does not limit the present invention in any way. The growth and epitaxial growth of semiconductor single crystals are carried out in high-temperature environments. The tantalum carbide-coated carbon material used as a component is also exposed to high-temperature environments. Therefore, the chlorine component contained in the tantalum carbide coating film is either released from the tantalum carbide coating film by itself due to heat, or reacts with impurity atoms contained in the tantalum carbide coating film and the carbon substrate to become a halide and release it from the tantalum carbon coating film. When the source gas is highly supersaturated in the single crystal growth environment, the chlorine component or halide adheres or adsorbs to the facets of the growing semiconductor single crystal. When a crystal nucleus is formed starting from the adhesion or adsorption point, the orientation of the nucleus is selected randomly. Therefore, it is considered that the probability of the occurrence of a crystal polymorph having a crystal face different from the crystal face growing from the step increases.
[0021] <Method for measuring chlorine concentration in tantalum carbide coating> The chlorine concentration in the tantalum carbide coating film can be measured, for example, by glow discharge mass spectrometry (GDMS) using a glow discharge mass spectrometer (product name "VG9000") manufactured by VG Elemental under the following measurement conditions. (Measurement conditions) Discharge Gas: Ar(7N) Insulator: Ceramic ·Secondary Electrode:In Orifice ·Cell:Flat Cell Assembly Nomakization: 1kV, 1.6mA Ion Current: Ta ~1.2×E-11 A ·Detectors:Faraday cup:160msec Daly-multiplier: 500msec
[0022] The measured data is a value obtained by correcting the ion intensity ratio (IBR (Ion Beam Ratio)) with the relative sensitivity factor (RSF). The RSF used here is a standard value built into the software. The RSF varies depending on the measurement conditions and the shape of the discharge cell, but the value corrected with the RSF built into the software (RSF corrected value) is considered to be closer to the mass concentration than the IBR. As an example of the measured data, the results of Example 1 described below are shown in FIG. 4. The vertical axis indicates the concentration (weight ppm) and the horizontal axis indicates the depth (μm). The depth is calculated based on the actual measured value of the crater depth after analysis, assuming that the sputtering rate during the analysis is constant. Note that, since there are irregularities of several μm on the crater bottom after analysis, it is considered that there is an error of about 10% in the depth resolution.
[0023] The definition of "in the metal carbide coating film" is that part where the carbon concentration fluctuates in the GDMS analysis within a range where the actual film thickness measured by cross-sectional observation using a scanning electron microscope (SEM) or the like can be correlated with the interface between the tantalum carbide coating film and the carbon substrate. For example, in Example 1 described below, the film thickness is found to be 30 μm by cross-sectional observation using a SEM, and the measurement data shown in FIG. 4 shows an increase in carbon concentration near 30 μm. Therefore, for example, in the measurement data shown in FIG. 4, the part from a depth of 0 μm to a depth of 30 μm where the carbon concentration increases rapidly is defined as "in the metal carbide coating film."
[0024] The chlorine concentration is calculated as the integral value of the chlorine concentration in the range of "in the metal carbide coating film." For example, in the measurement data shown in Figure 4, the integral value of the chlorine concentration from a depth of 0 μm to a depth of 30 μm is defined as the "chlorine concentration." In the measurement data shown in Figure 4, the chlorine concentration value is 27.5 ppm μm.
[0025] <Other atoms> The tantalum carbide coating film contains tantalum carbide as the main component and chlorine at a concentration of 25000 ppm μm or less, but may contain trace amounts of atoms other than carbon, tantalum, and chlorine as long as the effects of the present invention are not impaired. For example, the tantalum carbide coating film may contain impurity elements or doping elements other than carbon, tantalum, and chlorine at a concentration of 10000 ppm μm or less.
[0026] <Method of manufacturing tantalum carbide coated carbon material> The tantalum carbide coated carbon material according to one embodiment of the present invention can be produced by forming a tantalum carbide layer on the surface of a carbon substrate. The tantalum carbide coating film can be formed on the surface of the carbon substrate by, for example, a chemical vapor deposition (CVD) method, a sintering method, a carbonization method, or the like. Among these, the CVD method is preferred as a method for forming a tantalum carbide coating film, since it can form a uniform and dense tantalum carbide coating film.
[0027] Further, the CVD method includes a thermal CVD method, a photo-CVD method, a plasma CVD method, and the like, and for example, a thermal CVD method can be used to form a tantalum carbide layer. The thermal CVD method has advantages such as a relatively simple apparatus configuration and no damage to the carbon substrate by plasma. For example, an externally heated low-pressure CVD apparatus 10 as shown in FIG. 1 can be used to form a tantalum carbide coating film by the thermal CVD method. In the externally heated low-pressure CVD apparatus 10, a carbon substrate 14 is supported by a support means 15 in a reaction chamber 12 equipped with a heater 13, a raw material supply unit 16, an exhaust unit 17, and the like.
[0028] A method for producing a tantalum carbide-coated carbon material according to one embodiment of the present invention will be described with reference to FIG. First, the carbon substrate 14 is placed in the reaction chamber 12 of the externally heated low-pressure CVD apparatus 10. The carbon substrate 14 is supported by a supporting means 15 having three supporting portions each having a pointed tip.
[0029] Next, the reaction chamber 12 is heated. For example, the reaction chamber 12 is heated under conditions of an atmospheric pressure of 10 to 1000 Pa and a temperature of 800 to 2200°C.
[0030] Next, a tantalum carbide coating film is formed on the surface of the carbon substrate 14. As raw material gases, a gas of a compound containing carbon atoms such as methane (CH4), hydrogen (H2) gas, and a tantalum halide gas such as tantalum pentachloride (TaCl5) are supplied from the raw material supply unit 16 to the reaction chamber 12. The tantalum halide gas can be generated, for example, by a method of heating and vaporizing tantalum halide, or a method of reacting tantalum metal with a halogen gas. Next, the raw material gas supplied from the raw material supply unit 16 is subjected to a thermal CVD reaction at a high temperature and reduced pressure of a temperature of 800 to 2200°C and a pressure of 1 to 1000 Pa, to form a tantalum carbide coating film on the carbon substrate 14.
[0031] <Method for controlling chlorine concentration in tantalum carbide coating film> Supplying hydrogen (H2) gas when supplying the source gas promotes the reaction in which chlorine is released from the tantalum halide gas, making it possible to reduce the chlorine concentration in the tantalum carbide layer to 25,000 ppm·μm or less. In addition, it is preferable that the molar ratio of tantalum atoms contained in the tantalum halide gas and hydrogen atoms contained in the hydrogen gas in the source gas satisfies the following formula: Tantalum atom (Ta):Hydrogen atom (H) = 1:x (4≦x<16) In addition, when the value of x is 16 or more, the chlorine is released from the tantalum halide gas, but a tantalum carbide coating film containing an excess amount of Ta is formed, which is not a 1:1 molar ratio of Ta:C like Ta2C or Ta metal. Here, the molar ratio of tantalum atoms contained in the tantalum halide gas and hydrogen atoms contained in the hydrogen gas in the source gas can be calculated from the volumetric flow rates of the tantalum halide gas and hydrogen gas in their standard states. For example, when tantalum pentachloride is used as the tantalum halide gas, 1 mole of tantalum halide gas contains 1 mole of tantalum atoms. On the other hand, 1 mole of hydrogen gas contains 2 moles of hydrogen atoms.
[0032] The tantalum carbide-coated carbon material according to the embodiment of the present invention is an example of the metal carbide-coated carbon material according to the present invention, and the metal carbide-coated carbon material according to the present invention is not limited to the tantalum carbide-coated carbon material according to the embodiment of the present invention. In the metal carbide-coated carbon material according to the present invention, the metal carbide constituting the metal carbide coating film that coats the carbon substrate is not limited to tantalum carbide. For example, carbides such as niobium carbide, zirconium carbide, hafnium carbide and tungsten carbide can be used as the metal carbide constituting the metal carbide coating film that coats the carbon substrate. In addition, a combination of two or more metal carbides selected from the group consisting of tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide and tungsten carbide may be used as the metal carbide constituting the metal carbide coating film that coats the carbon substrate. Among tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide and tungsten carbide, tantalum carbide is preferred because it has the highest melting point and is excellent in chemical stability, strength and corrosion resistance.
[0033] When tantalum carbide is used for the metal carbide coating film, the entire metal carbide coating film does not need to be made of tantalum carbide, but at least the surface of the metal carbide coating film needs to be made of tantalum carbide. EXAMPLES
[0034] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.
[0035] The metal carbide coated carbon materials of Examples 1 to 21 and Comparative Example 1 were produced as follows. Example 1 2 and 3, isotropic graphite was processed into a bottomed cylindrical shape (crucible 21), a truncated conical cylindrical shape (guide member 22), a disk shape (susceptor 31), and a cylindrical shape (inner wall member 38), which were used as carbon substrates (see reference numeral 14 in FIG. 1). The arithmetic mean roughness Ra of the surface of the carbon substrate 14 was 6.0 μm, and the linear thermal expansion coefficient of the carbon substrate 14 was 7.0×10 -6 / °C. The linear thermal expansion coefficient of the carbon substrate was measured using a thermomechanical analyzer (TMA7300) manufactured by Yamato Scientific Co., Ltd., and the thermal expansion coefficient in the temperature range from 200°C to 1200°C was used.
[0036] Next, the carbon substrate 14 was placed in the reaction chamber 12 of the externally heated reduced pressure CVD apparatus 10 shown in Fig. 1. The carbon substrate 14 was supported by a support means 15 having three support parts each having a pointed tip. At this time, the tip of the support part was in contact with the outer surface of the truncated cone-shaped carbon substrate 14, the outer surface of the carbon substrate 14 of the bottomed cylindrical carbon substrate 14, the lower surface of the disk-shaped carbon substrate 14, and the outer surface of the cylindrical carbon substrate 14.
[0037] Next, 0.25 SLM of methane (CH4) gas, 1.0 SLM of argon (Ar) gas and 0.125 SLM of hydrogen (H2) gas as carrier gases, and 0.25 SLM of tantalum pentachloride (TaCl5) vaporized by heating to a temperature of 220°C were supplied from the raw material supply unit 16 into the reaction chamber 12, and the raw material gases were reacted in the reaction chamber 12 under conditions of an atmospheric pressure of 100 Pa and a temperature of 1250°C, to form a tantalum carbide coating film on the entire surface of the carbon substrate 14.
[0038] The carbon substrate 14 coated with the tantalum carbide coating film was removed from the reaction chamber 12, and a crucible 21 (see FIG. 2), a guide member 22 (see FIG. 2), a susceptor 31 (see FIG. 3), and an inner wall member 38 (see FIG. 3) made of a tantalum carbide-coated carbon material were completed. From the cross-sectional observation of the tantalum carbide coating film by a scanning electron microscope (SEM), the film thickness was calculated to be 30 μm. SEM photographs of the cross-section of the tantalum carbide coating film in the tantalum carbide-coated carbon material of Example 1 are shown in Figs. The arithmetic mean roughness Ra of the tantalum carbide coating film surface was measured using a surface roughness measuring instrument (manufactured by Mitutoyo Corporation, product name "Surftest SJ-210"), and the result was that the arithmetic mean roughness Ra of the tantalum carbide coating film surface was 5.5 μm.
[0039] Furthermore, the chlorine concentration in the tantalum carbide coating was measured by the glow discharge mass spectrometry (GDMS) method described in this specification. The measurement data is shown in Figure 4. As a result, it was found that the chlorine concentration in the tantalum carbide coating was 27.5 ppm μm.
[0040] The adhesion strength of the tantalum carbide coating was measured and found to be 19.6 MPa. The adhesion strength of the tantalum carbide coating was measured by the following method. The adhesion strength of the tantalum carbide coating film was measured, for example, using a thin film adhesion strength measuring device (manufactured by Quad Group, product name "Romulus"), by adhering the tantalum carbide coating film 41 and a pin 46 with adhesive 45, pressing down with a pressing jig 44 and pulling the pin 46, as shown in Fig. 7, to measure the stress when the tantalum carbide coating film 41 peeled off. Five measurements were made, and the average of the five calculations was regarded as the adhesion strength of the tantalum carbide coating film.
[0041] The prepared crucible 21 and guide member 22 were placed in a reduced pressure heating furnace 20 as shown in Fig. 2, and a SiC single crystal was grown by a sublimation recrystallization method. A SiC raw material 25 was placed in the crucible 21, and a SiC seed crystal 24 having a diameter of 2 inches was placed on the upper part of the crucible 21. Argon gas was flowed into the reduced pressure heating furnace 20 at a flow rate of 10 to 30 SLM, and the SiC raw material 25 was sublimated under conditions of an atmospheric pressure of 500 to 1000 Pa and a temperature of 2000 to 2500°C, to grow a SiC single crystal having a thickness of 5 mm on the SiC seed crystal 24.
[0042] The production of SiC single crystals was repeated several times to confirm the number of times the crucible 21 and the guide member 22 had been repeatedly used. As a result, after 24 uses, peeling of the tantalum carbide coating film was confirmed on the crucible 21, making it necessary to replace it with a new member.
[0043] The fabricated susceptor 31 and inner wall member 38 were placed in a CVD apparatus 30 as shown in Fig. 3, and a SiC single crystal was epitaxially grown by the CVD method. A SiC single crystal substrate 34, which had been processed from a bulk single crystal into a substrate shape, was placed on the susceptor 31. Monosilane (SiH4) gas was flowed into the CVD apparatus at 30 sccm and propane (C3H8) gas at 70 sccm, and the pressure was set to 45 Torr and the temperature to 1550°C, and a SiC single crystal was epitaxially grown on the SiC single crystal substrate.
[0044] The production of SiC single crystals was repeated several times to confirm the number of times the susceptor 31 and the inner wall member 38 could be repeatedly used. As a result, peeling of the tantalum carbide coating film was confirmed after 96 uses, and it became necessary to replace the members with new ones.
[0045] In addition, the polymorphism occurrence rate of the obtained single crystal was examined, and the polymorphism occurrence rate of the SiC single crystal produced by the sublimation recrystallization method and the polymorphism occurrence rate of the SiC single crystal produced by epitaxial growth were both 0%. The polymorphism occurrence rate was measured as follows. The grown SiC single crystal was irradiated with ultraviolet (UV) light and its appearance was examined. If even the slightest crystal disorder was observed, this was deemed to be the occurrence of crystal polymorphism.
[0046] Example 2 Except for changing the flow rate of hydrogen (H2) gas from 0.125 SLM to 0.2 SLM, the crucible 12, the guide member 19, the susceptor 31, and the inner wall member 38 were manufactured and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0047] Example 3 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the flow rate of hydrogen (H2) gas was changed from 0.125 SLM to 0.15 SLM and the flow rate of tantalum pentachloride (TaCl5) was changed from 0.25 SLM to 0.3 SLM. The results are shown in Table 2.
[0048] Example 4 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the flow rate of hydrogen (H2) gas was changed from 0.125 SLM to 0.2 SLM and the flow rate of tantalum pentachloride (TaCl5) was changed from 0.25 SLM to 0.4 SLM. The results are shown in Table 2.
[0049] Example 5 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the flow rate of hydrogen (H2) gas was changed from 0.125 SLM to 0.25 SLM and the flow rate of tantalum pentachloride (TaCl5) was changed from 0.25 SLM to 0.5 SLM. The results are shown in Table 2.
[0050] Example 6 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the flow rate of hydrogen (H2) gas was changed from 0.125 SLM to 0.15 SLM, the flow rate of tantalum pentachloride (TaCl5) was changed from 0.25 SLM to 0.3 SLM, and the film thickness was changed from 30 μm to 10 μm by shortening the film formation time. The results are shown in Table 2.
[0051] Example 7 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the flow rate of hydrogen (H2) gas was changed from 0.125 SLM to 0.15 SLM and the film thickness was changed from 30 μm to 50 μm by extending the film formation time. The results are shown in Table 2.
[0052] Example 8 The crucible 12, the guide member 19, the susceptor 31, and the inner wall member 38 were produced and evaluated in the same manner as in Example 1, except that the arithmetic mean roughness Ra of the surface of the carbon base material 14 was changed from 6.0 μm to 0.1 μm. The results are shown in Table 2.
[0053] Example 9 The crucible 12, the guide member 19, the susceptor 31, and the inner wall member 38 were produced and evaluated in the same manner as in Example 1, except that the arithmetic mean roughness Ra of the surface of the carbon base material 14 was changed from 6.0 μm to 10 μm. The results are shown in Table 2.
[0054] Example 10 The thermal expansion coefficient of the carbon substrate 14 is 7.0×10 -6 / ℃ to 3.5×10 -6 / ° C., crucible 12, guide member 19, susceptor 31, and inner wall member 38 were produced and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0055] Example 11 The thermal expansion coefficient of the carbon substrate 14 is 7.0×10 -6 / ℃ to 8.2×10 -6 / ° C., crucible 12, guide member 19, susceptor 31, and inner wall member 38 were produced and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0056] Example 12 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were manufactured and evaluated in the same manner as in Example 1, except that the metal chloride gas was changed from tantalum pentachloride (TaCl5) to niobium pentachloride (NbCl5) without changing the flow rate of the metal chloride gas (0.25 SLM). The results are shown in Table 2.
[0057] Example 13 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the metal chloride gas was changed from tantalum pentachloride (TaCl5) to hafnium tetrachloride (HfCl4) without changing the flow rate of the metal chloride gas (0.25 SLM). The results are shown in Table 2.
[0058] Example 14 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the metal chloride gas was changed from tantalum pentachloride (TaCl5) to zirconium tetrachloride (ZrCl4) without changing the flow rate of the metal chloride gas (0.25 SLM). The results are shown in Table 2.
[0059] Example 15 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the metal chloride gas was changed from tantalum pentachloride (TaCl5) to tungsten pentachloride (WCl5) without changing the flow rate of the metal chloride gas (0.25 SLM). The results are shown in Table 2.
[0060] (Example 16) The flow rate (0.25 SLM) of the metal chloride gas was not changed, and the metal chloride gas was changed from tantalum pentachloride (TaCl5) to a mixed gas of tantalum pentachloride (TaCl5) and niobium pentachloride (NbCl5) (TaCl5:NbCl5=100:1). The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were manufactured and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0061] (Example 17) The flow rate (0.25 SLM) of the metal chloride gas was not changed, and the metal chloride gas was changed from tantalum pentachloride (TaCl5) to a mixed gas of tantalum pentachloride (TaCl5) and tungsten pentachloride (WCl5) (TaCl5:WCl5=100:1). The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were manufactured and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0062] (Example 18) Except for shortening the film formation time and changing the film thickness from 30 μm to 2 μm, the crucible 12, the guide member 19, the susceptor 31, and the inner wall member 38 were fabricated and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0063] (Example 19) The crucible 12, the guide member 19, the susceptor 31, and the inner wall member 38 were produced and evaluated in the same manner as in Example 1, except that the arithmetic mean roughness Ra of the surface of the carbon base material 14 was changed from 6.0 μm to 32 μm. The results are shown in Table 2.
[0064] (Example 20) The crucible 12, the guide member 19, the susceptor 31, and the inner wall member 38 were produced and evaluated in the same manner as in Example 1, except that the arithmetic mean roughness Ra of the surface of the carbon base material 14 was changed from 6.0 μm to 0.05 μm. The results are shown in Table 2.
[0065] Example 21 The thermal expansion coefficient of the carbon substrate 14 is 7.0×10 -6 / ℃ to 1.9 × 10 -6 / ° C., crucible 12, guide member 19, susceptor 31, and inner wall member 38 were produced and evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0066] Comparative Example 1 The crucible 12, guide member 19, susceptor 31, and inner wall member 38 were fabricated and evaluated in the same manner as in Example 1, except that the flow rate of hydrogen (H2) gas was changed from 0.125 SLM to 0 SLM and the flow rate of tantalum pentachloride (TaCl5) was changed from 0.25 SLM to 0.5 SLM. The results are shown in Table 2.
[0067] The production conditions for Examples 1 to 21 and Comparative Example 1 are shown in Table 1. [Table 1]
[0068] The evaluation results of Examples 1 to 21 and Comparative Example 1 are shown in Table 2. [Table 2]
[0069] Comparing the results of Examples 1 to 21 with the result of Comparative Example 1, it was found that by setting the chlorine concentration in the metal carbide coating film to 25,000 ppm μm or less, it is possible to suppress the crystal growth of the semiconductor single crystal and the occurrence of crystal polymorphism during epitaxial growth.
[0070] Comparing the results of Examples 1 to 5 and Comparative Example 1, it was found that when the chlorine concentration in the tantalum carbide coating film was in the range of 25,000 ppm μm or less, the metal carbide-coated carbon material had a long product life and suppressed the occurrence of crystal polymorphism during crystal growth and epitaxial growth of the semiconductor single crystal. Note that the repeated use of the tantalum carbide-coated carbon material in Comparative Example 1 was discontinued before the tantalum carbide-coated carbon material became unusable due to peeling of the tantalum carbide coating film, etc., due to the occurrence of crystal polymorphism.
[0071] Comparing the results of Example 1, Example 6, Example 7 and Example 18, when the thickness of the tantalum carbide coating film is 10 μm or more and 100 μm or less, the product life of the metal carbide-coated carbon material is long, and the occurrence of crystal polymorphism during the crystal growth and epitaxial growth of the semiconductor single crystal is suppressed. When the thickness of the tantalum carbide coating film is 10 μm or less, the occurrence of crystal polymorphism during the crystal growth and epitaxial growth of the single crystal semiconductor is confirmed. In addition, the repeated use of the tantalum carbide-coated carbon material in Example 18 was discontinued before the tantalum carbide-coated carbon material became unusable due to the peeling of the tantalum carbide coating film, etc., because crystal polymorphism occurred. In addition, when the thickness of the tantalum carbide coating film exceeds 100 μm, the film formation time increases, and the film formation cost increases, which is not preferable. Therefore, the thickness of the tantalum carbide coating film is preferably 10 μm or more and 100 μm or less.
[0072] Comparing the results of Examples 1, 8, and 9 with those of Examples 19 and 20, when the arithmetic mean roughness Ra of the surface of the metal carbide coating film is 0.1 μm or more and 9.5 μm or less, or when the arithmetic mean roughness Ra of the surface of the carbon substrate is 0.1 μm or more and 10.0 μm or less, the product life of the metal carbide-coated carbon material is long, and the occurrence of crystal polymorphism during crystal growth and epitaxial growth of the semiconductor single crystal is suppressed. When the arithmetic mean roughness Ra of the surface of the carbon substrate is larger than 10 μm, the product life of the metal carbide-coated carbon material is shortened, and the occurrence of crystal polymorphism during crystal growth and epitaxial growth of the semiconductor single crystal is confirmed. When the arithmetic mean roughness Ra of the carbon substrate surface is smaller than 0.1 μm, the product life of the metal carbide-coated carbon material is shortened.
[0073] Comparing the results of Examples 1, 10, 11 and 21, it is found that the thermal expansion coefficient of the carbon substrate is 3.5×10 -6 / ℃ or more, 8.2×10 -6 / °C or less, the product life of the metal carbide-coated carbon material was long, and the crystal growth of semiconductor single crystals and the occurrence of crystal polymorphism during epitaxial growth were suppressed. -6 When the temperature was lower than 100° C. / ° C., the product life of the metal carbide-coated carbon material was shortened, and the occurrence of crystal polymorphism during crystal growth and epitaxial growth of the semiconductor single crystal was confirmed.
[0074] Comparing the results of Example 1 and Examples 12 to 16, when a metal carbide-coated carbon material in which at least a portion of the surface of a base material mainly composed of carbon is coated with a metal carbide coating film mainly composed of any one of tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide, tungsten carbide, or a combination of two or more of these metal carbides, and the chlorine concentration in the metal carbide coating film is in the range of 25,000 ppm μm or less, the product life of the metal carbide-coated carbon material is long, and the occurrence of crystal polymorphism during crystal growth and epitaxial growth of the semiconductor single crystal is suppressed. [Explanation of symbols]
[0075] 10. Externally heated low-pressure CVD equipment 11 Top Chamber 12 Reaction chamber 13. Heater 14 Carbon Substrate 15 Support means 16 Raw material supply department 17 Exhaust section 20. Decompression heating furnace 21 Crucible 22 Guide member 23 Upper lid 24 SiC seed crystal 25 SiC raw material 30 Epitaxial growth equipment 31 Susceptor 32 Reaction chamber 33 Heater 34 SiC single crystal substrate 35 Exhaust section 36 Raw material supply department 37 Top Chamber 38 Inner wall material 41 Tantalum carbide coating 42 Carbon Substrate 44 Holding jig 45 Adhesive 46 pin
Claims
1. A metal carbide-coated carbon material comprising a carbon substrate containing carbon as a main component and a metal carbide coating film that coats at least a portion of the carbon substrate, the metal carbide constituting the metal carbide coating film is at least one metal carbide selected from the group consisting of tantalum carbide, niobium carbide, zirconium carbide, hafnium carbide, and tungsten carbide; A metal carbide-coated carbon material, wherein the metal carbide coating film has a chlorine concentration of 25,000 ppm·μm or less.
2. 2. The metal carbide coated carbon material according to claim 1, wherein the metal carbide coating film has a thickness of 10 μm or more and 100 μm or less.
3. 2. The metal carbide coated carbon material according to claim 1, wherein the arithmetic mean roughness Ra of the surface of the metal carbide coating film is 0.1 μm or more and 9.5 μm or less.
4. 2. The metal carbide coated carbon material according to claim 1, wherein the arithmetic mean roughness Ra of the surface of the carbon substrate is 0.1 μm or more and 10.0 μm or less.
5. The carbon substrate has a linear thermal expansion coefficient of 3.5×10 -6 / ℃ or more, 8.2 x 10 -6 The metal carbide-coated carbon material according to claim 1, wherein the temperature is 0.1 to 100° C.
6. 2. The metal carbide coated carbon material according to claim 1, wherein the metal carbide constituting at least the surface of the metal carbide coating film is tantalum carbide.
7. 2. The metal carbide coated carbon material according to claim 1, wherein the metal carbide constituting the metal carbide coating film is tantalum carbide.
Citation Information
Patent Citations
Tantalum carbide coating carbon material and method of manufacturing the same, and member for semiconductor single-crystal manufacturing apparatus
JP2019099453A
METHOD OF MANUFACTURING TaC COATING LAYER USING CVD AND PROPERTY OF TaC MANUFACTURED USING THE SAME
JP2019108611A
Tantalum carbide-coated carbon material for heating, production method of tantalum carbide-coated carbon material for heating, silicon carbide epitaxial wafer growth equipment and gallium nitride epitaxial wafer fabrication and growth equipment
JP2022120773A
Carbide-coated carbon material
WO2022009580A1