Liquid crystal polymer composition

A liquid crystal polymer composition with a wholly aromatic liquid crystal polymer, reinforcing fibers, and a carbodiimide compound maintains mechanical strength and improves hydrogen gas barrier properties, addressing the issue of gas permeability in reinforced polymers.

JP2024143269APending Publication Date: 2024-10-11UENO PHARMA CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023055851
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Liquid crystal polymers with added reinforcing fibers lose their gas barrier properties, making them unsuitable for hydrogen gas containers, necessitating improvements in both hydrogen gas barrier properties and mechanical strength.

Method used

A liquid crystal polymer composition containing a wholly aromatic liquid crystal polymer, reinforcing fibers, and a carbodiimide group-containing compound is developed, which maintains mechanical properties like bending strength while enhancing hydrogen gas barrier properties.

Benefits of technology

The composition achieves excellent mechanical properties and hydrogen gas barrier properties, suitable for applications such as liquid hydrogen tanks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143269000001
    Figure 2024143269000001
  • Figure 2024143269000002
    Figure 2024143269000002
  • Figure 2024143269000003
    Figure 2024143269000003
Patent Text Reader

Abstract

To provide a liquid crystal polymer composition capable of forming an article such as a molded product having improved hydrogen gas barrier properties while maintaining mechanical properties such as flexural strength.SOLUTION: There is provided a liquid crystal polymer composition which comprises 100 pts.mass of a wholly aromatic liquid crystal polymer having a crystal melting temperature of 210 to 250°C, 1 to 100 pts.mass of a reinforcing fiber and 0.01 to 10 pts.mass of a carbodiimide group-containing compound.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid crystalline polymer composition capable of forming articles, such as molded articles, having improved hydrogen gas barrier properties while maintaining mechanical properties, such as flexural strength. [Background technology]

[0002] Fiber reinforced plastics (FRP) are composite materials consisting of a matrix resin, such as a thermosetting resin such as unsaturated polyester resin, epoxy resin, or polyimide resin, or a thermoplastic resin such as polyethylene, polypropylene, polyamide, polysulfone, polyethersulfone, or polyetheretherketone, and a fiber reinforcement such as carbon fiber, glass fiber, or aramid fiber. These composite materials are molded, for example, through a molding and processing process such as heating and pressing from a prepreg, which is an intermediate product in which a fiber reinforcement is impregnated with a matrix resin. In particular, composite materials using carbon fiber as a fiber reinforcement are lightweight and have excellent mechanical properties such as high strength, and therefore have been widely used in recent years as components for aircraft, automobiles, etc.

[0003] In addition, in an era when hydrogen, a clean fuel, is used instead of hydrocarbon fuels, and in a situation where a so-called hydrogen energy society is coming, there is an increasing demand for lightweight hydrogen storage containers in consideration of ease of handling. For this purpose, it is considered effective to use carbon fiber reinforced plastics, which are lighter than conventionally used metal materials such as stainless steel and aluminum and have excellent specific strength. However, organic plastics generally have poor gas barrier properties, and hydrogen gas, which has an extremely small molecular diameter, easily passes through them, making it difficult to use carbon fiber reinforced plastics as hydrogen containers as they are. Therefore, it has been proposed to use a liquid crystal polymer with excellent gas barrier properties as a hydrogen container (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2005-126651 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, although liquid crystal polymers have excellent gas barrier properties, when reinforcing fibers are added to them to produce molded articles, the gas barrier properties decrease, making them unsuitable as containers for hydrogen gas, and further improvements were therefore required.

[0006] An object of the present invention is to provide a liquid crystalline polymer composition capable of forming an article such as a molded article having improved hydrogen gas barrier properties while maintaining mechanical properties such as bending strength, etc. Another object of the present invention is to provide a liquid hydrogen tank using the molded article. [Means for solving the problem]

[0007] As a result of intensive research to solve the above problems, the present inventors have discovered that by further blending a carbodiimide group-containing compound with a composition containing a liquid crystal polymer and reinforcing fibers, the hydrogen gas barrier properties of an article such as a molded product can be improved while maintaining mechanical properties such as bending strength, and have thus completed the present invention.

[0008] That is, the present invention includes the following preferred embodiments. [1] A liquid crystal polymer composition comprising 100 parts by mass of a wholly aromatic liquid crystal polymer having a crystalline melting temperature of 210 to 250°C, 1 to 100 parts by mass of a reinforcing fiber, and 0.01 to 10 parts by mass of a carbodiimide group-containing compound. [2] The liquid crystal polymer composition according to [1], wherein the wholly aromatic liquid crystal polymer has a crystalline melting temperature of 215 to 245°C. [3] The wholly aromatic liquid crystal polymer is represented by the formulas (I) to (IV) [ka] [In the formula, Ar1 and Ar2 each represent one or more divalent aromatic groups, and p, q, r and s each represent the composition ratio (mol %) of each repeating unit in the wholly aromatic liquid crystal polyester, and satisfy the following condition: 0.5≦p / q≦2.5 2≦r≦15, and 2≦s≦15] The liquid crystal polymer composition according to [1] or [2], which is a wholly aromatic liquid crystal polyester containing a repeating unit represented by the following formula: [4] In the formula (III) and / or formula (IV), Ar1 and Ar2 are each independently represented by any one of the formulas (1) to (4). [ka] The liquid crystal polymer composition according to [3], comprising one or more repeating units which are aromatic groups selected from the group consisting of: [5] The liquid crystal polymer composition according to any one of [1] to [4], wherein the reinforcing fiber is a carbon fiber. [6] The liquid crystal polymer composition according to any one of [1] to [5], wherein the carbodiimide group-containing compound is a polycarbodiimide compound. [7] A molded article made of the liquid crystal polymer composition according to any one of [1] to [6]. [8] The molded article according to [7], which is a liquid hydrogen tank. Effect of the Invention

[0009] The liquid crystal polymer composition of the present invention is excellent in mechanical properties such as bending strength and hydrogen gas barrier properties, and therefore can be suitably used in various applications such as containers requiring hydrogen gas barrier properties, such as liquid hydrogen tanks. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The wholly aromatic liquid crystal polymer used in the liquid crystal polymer composition of the present invention is a wholly aromatic liquid crystal polyester or a wholly aromatic liquid crystal polyester amide which forms an anisotropic molten phase and is called a thermotropic liquid crystal polymer by those skilled in the art.

[0011] The anisotropic melt phase properties of the wholly aromatic liquid crystal polymer can be confirmed by a conventional polarimetric inspection method using cross polarizers, that is, by observing a sample placed on a hot stage under a nitrogen atmosphere.

[0012] Examples of the repeating units constituting the wholly aromatic liquid crystal polymer used in the present invention include aromatic oxycarbonyl repeating units, aromatic dicarbonyl repeating units, aromatic dioxy repeating units, aromatic aminooxy repeating units, aromatic diamino repeating units, aromatic aminocarbonyl repeating units, and combinations thereof.

[0013] Specific examples of monomers that provide aromatic oxycarbonyl repeating units include aromatic hydroxycarboxylic acids such as 4-hydroxybenzoic acid, 3-hydroxybenzoic acid, 2-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 5-hydroxy-2-naphthoic acid, 3-hydroxy-2-naphthoic acid, 4'-hydroxyphenyl-4-benzoic acid, 3'-hydroxyphenyl-4-benzoic acid, 4'-hydroxyphenyl-3-benzoic acid, and the like, as well as their alkyl, alkoxy, or halogen-substituted derivatives, and their acylated derivatives, ester derivatives, acid halides, and other ester-forming derivatives. Among these, 4-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid are preferred because they are easy to adjust the mechanical properties, heat resistance, crystal melting temperature, and moldability of the resulting wholly aromatic liquid crystal polymer to appropriate levels.

[0014] Specific examples of monomers that provide aromatic dicarbonyl repeating units include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 1,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, and 4,4'-dicarboxybiphenyl, as well as their alkyl, alkoxy, or halogen-substituted derivatives, and their ester-forming derivatives such as ester derivatives and acid halides. Among these, terephthalic acid and 2,6-naphthalenedicarboxylic acid are preferred because they are easy to adjust the mechanical properties, heat resistance, crystal melting temperature, and moldability of the resulting wholly aromatic liquid crystal polymer to appropriate levels.

[0015] Specific examples of the monomer that gives the aromatic dioxy repeating unit include aromatic diols such as hydroquinone, resorcinol, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 4,4'-dihydroxybiphenyl, 3,3'-dihydroxybiphenyl, 3,4'-dihydroxybiphenyl, 4,4'-dihydroxybiphenyl ether, and their alkyl, alkoxy or halogen-substituted derivatives, as well as their acylated derivatives and other ester-forming derivatives. Among these, hydroquinone and 4,4'-dihydroxybiphenyl are preferred because they are easy to adjust the reactivity during polymerization, the mechanical properties, heat resistance, crystal melting temperature and moldability of the resulting wholly aromatic liquid crystal polymer to an appropriate level.

[0016] Monomers which provide the aromatic aminooxy repeating unit, aromatic diamino repeating unit and aromatic aminocarbonyl repeating unit include aromatic hydroxyamines, aromatic diamines and aromatic aminocarboxylic acids.

[0017] The wholly aromatic liquid crystal polymer used in the present invention may contain an aromatic oxydicarbonyl repeating unit or a thioester bond, provided that the object of the present invention is not impaired. Examples of monomers that give thioester bonds include mercaptoaromatic carboxylic acids, aromatic dithiols, and hydroxyaromatic thiols. The amount of these monomers used is preferably 10 mol% or less based on the total amount of the aromatic oxycarbonyl repeating unit, aromatic dicarbonyl repeating unit, aromatic dioxy repeating unit, aromatic aminooxy repeating unit, aromatic diamino repeating unit, and monomers that give aromatic aminocarbonyl repeating units.

[0018] Among copolymers combining these repeating units, some form an anisotropic molten phase and some do not, depending on the monomer composition and composition ratio, and the sequence distribution of each repeating unit in the copolymer. However, the wholly aromatic liquid crystal polymer used in the present invention is limited to copolymers that form an anisotropic molten phase.

[0019] The wholly aromatic liquid crystal polymer used in the present invention may be a blend of two or more liquid crystal polymers.

[0020] The crystalline melting temperature of the wholly aromatic liquid crystal polymer used in the present invention, measured by a differential scanning calorimeter, is 210 to 250°C, preferably 212 to 248°C, and more preferably 215 to 245°C.

[0021] When the crystalline melting temperature of the wholly aromatic liquid crystal polymer is within the above range, the reinforcing fibers are easily dispersed uniformly in the composition, and mechanical properties such as bending strength are improved.

[0022] In the present specification and claims, the "crystalline melting temperature" is determined from the crystalline melting peak temperature measured at a heating rate of 20°C / min using a differential scanning calorimeter (hereinafter abbreviated as DSC). More specifically, after observing the endothermic peak temperature (Tm1) observed when a sample of a wholly aromatic liquid crystal polymer is measured under a heating condition of 20°C / min from room temperature, the sample is held at a temperature 20 to 50°C higher than Tm1 for 10 minutes, and then cooled to room temperature under a heating condition of 20°C / min, and then measured again under a heating condition of 20°C / min. The temperature showing the peak top is taken as the crystalline melting temperature of the wholly aromatic liquid crystal polymer. For example, Exstar6000 manufactured by Seiko Instruments Inc. can be used as a measuring instrument.

[0023] As the wholly aromatic liquid crystal polymer used in the present invention, wholly aromatic liquid crystal polyesters containing repeating units represented by formulae (I) to (IV) are suitably used. [ka]

[0024] [In the formula, Ar1 and Ar2 each represent one or more divalent aromatic groups, and p, q, r and s each represent the composition ratio (mol %) of each repeating unit in the wholly aromatic liquid crystal polyester, and satisfy the following condition: 0.5≦p / q≦2.5 2≦r≦15, and 2≦s≦15.]

[0025] The molar ratio (p / q) of the composition ratio p (mol %) according to the above formula (I) to the composition ratio q (mol %) according to the above formula (II) is more preferably from 0.6 to 1.8, and further preferably from 0.8 to 1.6.

[0026] In the above-mentioned wholly aromatic liquid crystal polyesters which are suitably used, the total composition ratio of p and q is preferably from 70 to 96 mol %, and more preferably from 76 to 90 mol %.

[0027] In the above-mentioned wholly aromatic liquid crystal polyesters which are preferably used, the composition ratio p in formula (I) and the composition ratio q in formula (II) are each preferably 32 to 54 mol %, more preferably 36 to 52 mol %.

[0028] In the wholly aromatic liquid crystal polyester preferably used in the present invention, by containing the repeating units represented by formula (I) and formula (II) at least in the above-mentioned molar ratio (p / q), and optionally in the above-mentioned total composition ratio of p and q and / or each of p and q in the above-mentioned composition ratio (mol %), a wholly aromatic liquid crystal polyester exhibiting a crystalline melting temperature of 210°C to 250°C can be preferably obtained.

[0029] In the wholly aromatic liquid crystal polyester preferably used in the present invention, the composition ratio r of formula (III) and the composition ratio s of formula (IV) are each preferably 2 to 15 mol %, more preferably 5 to 12 mol %. r and s are preferably equimolar amounts.

[0030] In the above repeating units, for example, Ar1 (or Ar2) represents two or more kinds of divalent aromatic groups means that the wholly aromatic liquid crystal polyester contains two or more kinds of repeating units represented by formula (III) (or (IV)) according to the type of divalent aromatic group. In this case, the composition ratio r of formula (III) (or the composition ratio s of formula (IV)) represents the total composition ratio of two or more kinds of repeating units.

[0031] Specific examples of monomers which provide the repeating unit represented by formula (I) include 4-hydroxybenzoic acid and its ester-forming derivatives such as acylation products, ester derivatives and acid halides.

[0032] Specific examples of monomers which provide the repeating unit represented by formula (II) include 6-hydroxy-2-naphthoic acid and its ester-forming derivatives such as acylation products, ester derivatives and acid halides.

[0033] Specific examples of monomers that provide the repeating unit represented by formula (III) include aromatic diols such as hydroquinone, resorcinol, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 4,4'-dihydroxybiphenyl, 3,3'-dihydroxybiphenyl, 3,4'-dihydroxybiphenyl, 4,4'-dihydroxybiphenyl ether, and ester-forming derivatives thereof, such as alkyl, alkoxy or halogen substituted products, and acylated products thereof.

[0034] Specific examples of monomers that provide the repeating unit represented by formula (IV) include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 1,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 4,4'-dicarboxybiphenyl, and the like, as well as alkyl, alkoxy, or halogen-substituted derivatives thereof, and ester-forming derivatives thereof such as ester derivatives and acid halides.

[0035] Furthermore, among the wholly aromatic liquid crystal polyesters preferably used in the present invention, wholly aromatic liquid crystal polyesters in which Ar1 and Ar2 relating to the repeating units represented by formulas (III) and (IV) each independently contain one or more types selected from the group consisting of aromatic groups represented by formulas (1) to (4) are more preferably used. [ka]

[0036] Among these, as the repeating unit represented by formula (III), it is particularly preferred to use aromatic groups represented by formulas (1) and (3), i.e., hydroquinone and 4,4'-dihydroxybiphenyl and their ester-forming derivatives as monomers that give these repeating units, because this makes it easy to adjust the reactivity during polymerization and the mechanical properties, heat resistance, crystalline melting temperature and molding processability of the resulting wholly aromatic liquid crystal polyester to appropriate levels.

[0037] As the repeating unit represented by formula (IV), it is particularly preferred to use aromatic groups represented by formulas (1) and (4), i.e., terephthalic acid and 2,6-naphthalenedicarboxylic acid and their ester-forming derivatives as monomers that give these repeating units, since this makes it easy to adjust the mechanical properties, heat resistance, crystalline melting temperature and molding processability of the resulting wholly aromatic liquid crystal polyester to appropriate levels.

[0038] In the above repeating unit, for example, Ar1 (or Ar2) containing two or more aromatic groups means that the wholly aromatic liquid crystal polyester contains two or more types of repeating units represented by formula (III) (or (IV)) according to the type of divalent aromatic group. That is, the wholly aromatic liquid crystal polyester of formula (III) and / or formula (IV) is preferably a wholly aromatic liquid crystal polyester containing one or more types of repeating units in which Ar1 and Ar2 are each independently an aromatic group selected from the group consisting of formulas (1) to (4). In this case, the composition ratio r according to formula (III) (or the composition ratio s according to formula (IV)) represents the composition ratio of the two or more types of repeating units in total.

[0039] In the wholly aromatic liquid crystal polyester preferably used in the present invention, the total composition ratio of the repeating units [p+q+r+s] is preferably 100 mol %, but other repeating units may be further contained within a range that does not impair the object of the present invention.

[0040] Examples of monomers which provide other repeating units constituting the wholly aromatic liquid crystal polyester preferably used in the present invention include other aromatic hydroxycarboxylic acids, aromatic hydroxyamines, aromatic diamines, aromatic aminocarboxylic acids, aromatic hydroxydicarboxylic acids, aromatic mercaptocarboxylic acids, aromatic dithiols, aromatic mercaptophenols, and combinations thereof.

[0041] Specific examples of other aromatic hydroxycarboxylic acids include 3-hydroxybenzoic acid, 2-hydroxybenzoic acid, 5-hydroxy-2-naphthoic acid, 3-hydroxy-2-naphthoic acid, 4'-hydroxyphenyl-4-benzoic acid, 3'-hydroxyphenyl-4-benzoic acid, 4'-hydroxyphenyl-3-benzoic acid, and alkyl, alkoxy or halogen substituted derivatives thereof, as well as ester-forming derivatives thereof such as acylation products, ester derivatives and acid halides.

[0042] The total composition ratio of the repeating units provided by these other monomer components is preferably 10 mol % or less based on the total repeating units.

[0043] The method for producing the wholly aromatic liquid crystal polymer used in the present invention will now be described.

[0044] The method for producing the wholly aromatic liquid crystal polymer used in the present invention is not particularly limited, and any known polycondensation method for forming an ester bond or an amide bond from a combination of the above-mentioned monomers, such as a molten acidolysis method or a slurry polymerization method, can be used.

[0045] The melt acidolysis method is a preferred method for preparing the wholly aromatic liquid crystal polymer used in the present invention, in which the monomers are first heated to form a melt of reactants, and then the reaction is continued to obtain a molten polymer. A vacuum may be applied to facilitate removal of volatile by-products (e.g., acetic acid, water, etc.) produced in the final stage of condensation.

[0046] A slurry polymerization process is a process in which the reaction is carried out in the presence of a heat exchange fluid, and a solid product is obtained in suspension in the heat exchange medium.

[0047] In both the melt acidolysis method and the slurry polymerization method, the polymerizable monomer components used in producing the wholly aromatic liquid crystal polymer can be subjected to the reaction at room temperature in a modified form in which the hydroxyl group and / or amino group is acylated, that is, as a lower acylated product. The lower acyl group preferably has 2 to 5 carbon atoms, more preferably has 2 or 3 carbon atoms. Particularly preferred is a method in which an acetylated product of the monomer is used in the reaction.

[0048] The acylated monomer may be one that has been previously synthesized by separate acylation, or may be produced in the reaction system by adding an acylating agent such as acetic anhydride to the monomer during the production of the wholly aromatic liquid crystal polymer.

[0049] In either the molten acidolysis method or the slurry polymerization method, a catalyst may be used in the reaction, if necessary.

[0050] Specific examples of catalysts include organotin compounds (dialkyltin oxides such as dibutyltin oxide, diaryltin oxides, etc.), titanium dioxide, antimony trioxide, organotitanium compounds (alkoxytitanium silicates, titanium alkoxides, etc.), alkali and alkaline earth metal salts of carboxylic acids (potassium acetate, sodium acetate, etc.), Lewis acids (BF3, etc.), gaseous acid catalysts such as hydrogen halides (HCl, etc.), and the like.

[0051] The catalyst is used in an amount of usually 1 to 1000 ppm, preferably 2 to 100 ppm, based on the total amount of monomers.

[0052] The wholly aromatic liquid crystal polymer thus obtained through the polycondensation reaction is withdrawn in a molten state from the polymerization reaction vessel and then processed into pellets, flakes, or powder.

[0053] The liquid crystal polymer composition of the present invention has improved gas barrier properties by containing reinforcing fibers and a carbodiimide group-containing compound in addition to the wholly aromatic liquid crystal polymer described above.

[0054] Examples of the reinforcing fibers contained in the liquid crystal polymer composition of the present invention include carbon fibers, glass fibers, silica alumina fibers, alumina fibers, potassium titanate fibers, aluminum borate fibers, and aramid fibers. Among these, carbon fibers are particularly preferred because of their excellent mechanical properties. These reinforcing fibers may be used alone or in combination of two or more kinds, but it is preferred to use the carbon fibers in such a way that the proportion of the total reinforcing fibers is 80 mass% or more.

[0055] The carbon fiber preferably used as the reinforcing fiber contained in the liquid crystal polymer composition of the present invention is a general carbon fiber obtained by baking a precursor called a precursor. More specifically, the precursor is first flame-retarded in an oxidizing atmosphere, and then the obtained flame-retarded fiber is baked at about 800 to 2000 ° C. in an inert gas atmosphere. If necessary, it is further baked in an inert gas at a higher temperature. Carbon fibers are usually known to have a sizing agent applied to their surface.

[0056] The type of carbon fiber contained in the liquid crystal polymer composition of the present invention is not particularly limited, but examples include polyacrylonitrile-based (hereinafter sometimes referred to as "PAN-based"), petroleum / coal pitch-based (hereinafter sometimes referred to as "pitch-based"), rayon-based, and lignin-based.

[0057] Examples of PAN-based carbon fibers include "TORAYCA (registered trademark)" manufactured by Toray Industries, Inc., "PYROFIL (registered trademark)" manufactured by Mitsubishi Chemical Corporation, and "Tenax (registered trademark)" manufactured by Teijin Ltd. Examples of pitch-based carbon fibers include "DIALEAD (registered trademark)" manufactured by Mitsubishi Chemical Corporation, "DONACARBO (registered trademark)" manufactured by Osaka Gas Chemicals Co., Ltd., and "KURECA (registered trademark)" manufactured by Kureha Corporation.

[0058] The carbon fiber contained in the liquid crystal polymer composition of the present invention is not particularly limited, but is preferably a carbon fiber bundle in which a plurality of single fibers are bundled or a chopped carbon fiber bundle, and more preferably a carbon fiber bundle from the viewpoint of productivity.

[0059] The number average fiber diameter of the carbon fibers contained in the liquid crystal polymer composition of the present invention is not particularly limited, but is from 1 μm to 10 μm, and preferably from 5 μm to 8 μm. The number average fiber diameter of the carbon fibers means the number average value of the fiber diameters measured for 50 carbon fibers by observing the carbon fibers with a scanning electron microscope (1000x).

[0060] When the number average fiber diameter of the carbon fibers is 1 μm or more, the carbon fibers are easily dispersed in the wholly aromatic liquid crystal polymer. In addition, the carbon fibers are easy to handle during the production of the liquid crystal polymer composition. In addition, when the number average fiber diameter of the carbon fibers is 10 μm or less, the wholly aromatic liquid crystal polymer is efficiently reinforced by the carbon fibers. Therefore, excellent mechanical strength can be imparted to a molded article molded from the liquid crystal polymer composition of the present invention.

[0061] The number of fibers in the carbon fiber bundle contained in the liquid crystal polymer composition of the present invention is not particularly limited, but is preferably 3000 or more, more preferably 12000 or more. When the number of fibers in the carbon fiber bundle is 3000 or more, the content of carbon fibers in the liquid crystal polymer composition is sufficient in terms of excellent mechanical strength when formed into a molded article. In addition, the number of fibers in the carbon fiber bundle is preferably 60000 or less, more preferably 18000 or less. When the number of fibers in the carbon fiber bundle is 60000 or less, the carbon fibers are easily dispersed in the wholly aromatic liquid crystal polymer. In addition, the carbon fibers are easy to handle during the production of the liquid crystal polymer composition.

[0062] The content of the reinforcing fiber contained in the liquid crystal polymer composition of the present invention is 1 to 100 parts by mass, preferably 2 to 80 parts by mass, more preferably 3 to 70 parts by mass, and further preferably 5 to 60 parts by mass, relative to 100 parts by mass of the wholly aromatic liquid crystal polymer. By having the content of the reinforcing fiber within the above range, a molded product having excellent mechanical properties such as bending strength can be formed.

[0063] The carbodiimide group-containing compound used in the liquid crystal polymer composition of the present invention is a compound having a carbodiimide group (-N=C=N-), and is not particularly limited as long as it is a compound having at least one carbodiimide group.

[0064] Examples of the carbodiimide group-containing compound include polycarbodiimide compounds having two or more carbodiimide groups in the molecule and monocarbodiimide compounds having one carbodiimide group in the molecule.

[0065] Specific examples of the polycarbodiimide compound include aromatic polycarbodiimides such as poly(4,4'-diphenylmethanecarbodiimide), poly(p-phenylenecarbodiimide), poly(m-phenylenecarbodiimide), poly(diisopropylphenylcarbodiimide), and poly(triisopropylphenylcarbodiimide); and alicyclic polycarbodiimides such as poly(dicyclohexylmethanecarbodiimide).

[0066] Examples of the monocarbodiimide compound include aromatic monocarbodiimide compounds such as diphenylcarbodiimide, di-2,6-dimethylphenylcarbodiimide, di-2,6-diethylphenylcarbodiimide, di-2,6-diisopropylphenylcarbodiimide, di-2,6-ditert-butylphenylcarbodiimide, di-o-tolylcarbodiimide, di-p-tolylcarbodiimide, di-2,4,6-trimethylphenylcarbodiimide, di-2,4,6-triisopropylphenylcarbodiimide, and di-2,4,6-triisobutylphenylcarbodiimide; alicyclic monocarbodiimide compounds such as di-cyclohexylcarbodiimide and di-cyclohexylmethanecarbodiimide; and aliphatic monocarbodiimide compounds such as di-isopropylcarbodiimide and di-octadecylcarbodiimide.

[0067] The carbodiimide group-containing compound may be used alone or in combination of two or more. Among these, preferred specific compounds are polycarbodiimide compounds, particularly preferred are aliphatic polycarbodiimide compounds, and examples of commercially available products thereof include Carbodilite (registered trademark) HMV-8CA and Carbodilite (registered trademark) LA-1 manufactured by Nisshinbo Chemical Inc.

[0068] The content of the carbodiimide group-containing compound in the liquid crystal polymer composition of the present invention is 0.01 to 10 parts by mass, preferably 0.02 to 5 parts by mass, more preferably 0.03 to 3 parts by mass, further preferably 0.05 to 1.5 parts by mass, and particularly preferably 0.07 to 1 part by mass, relative to 100 parts by mass of the wholly aromatic liquid crystal polymer. By having the content of the carbodiimide group-containing compound within the above range, the hydrogen gas barrier property of the liquid crystal polymer composition is improved.

[0069] The liquid crystal polymer composition of the present invention is characterized in that the crystalline melting temperature of the wholly aromatic liquid crystal polymer used is 210 to 250°C, and therefore the reinforcing fibers and the carbodiimide group-containing compound are uniformly dispersed in the wholly aromatic liquid crystal polymer, which is the matrix resin, and can be blended by melt kneading at a low temperature.

[0070] The liquid crystal polymer composition of the present invention may contain, as an optional component, inorganic and / or organic fillers other than the reinforcing fibers described above.

[0071] Specific examples of inorganic and / or organic fillers that may be contained in the liquid crystal polymer composition of the present invention include talc, mica, graphite, wollastonite, dolomite, clay, glass flakes, glass beads, glass balloons, calcium carbonate, barium sulfate, titanium oxide, etc. These may be used alone or in combination of two or more. Among these, talc is preferred because it has a good balance between physical properties and cost.

[0072] When an inorganic and / or organic filler is blended, the content thereof is preferably 1 to 150 parts by mass, and more preferably 10 to 100 parts by mass, based on 100 parts by mass of the wholly aromatic liquid crystal polymer.

[0073] If the content of the inorganic and / or organic filler is less than 1 part by mass, it is difficult to obtain the effect of improving the mechanical strength and heat resistance of the liquid crystal polymer composition due to the inorganic and / or organic filler, and if it exceeds 150 parts by mass, the fluidity tends to decrease. In the present invention, it is preferable that the liquid crystal polymer composition does not contain an inorganic and / or organic filler.

[0074] In addition to the wholly aromatic liquid crystal polymer, reinforcing fiber and carbodiimide group-containing compound, other additives and resin components may be added to the liquid crystal polymer composition of the present invention, as long as the object of the present invention is not impaired.

[0075] Specific examples of other additives include, for example, lubricants such as higher fatty acids, higher fatty acid esters, higher fatty acid amides, and higher fatty acid metal salts (here, higher fatty acids refer to those having 10 to 25 carbon atoms), release agents such as polysiloxanes and fluororesins, colorants such as dyes, pigments, and carbon black, flame retardants, antistatic agents, surfactants, nucleating agents such as talc, organic phosphates, and sorbitols, antiblocking agents, antioxidants such as phosphorus-based antioxidants, phenol-based antioxidants, and sulfur-based antioxidants, weather resistance agents, heat stabilizers, and neutralizing agents. These additives can be used alone or in combination of two or more.

[0076] The total amount of other additives in the liquid crystal polymer composition is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the wholly aromatic liquid crystal polymer.

[0077] If the total amount of other additives is less than 0.01 parts by mass, it is difficult for the additives to realize their functions, whereas if it exceeds 5 parts by mass, the thermal stability of the liquid crystal polymer composition during molding tends to deteriorate.

[0078] Furthermore, when additives such as lubricants, release agents, and antiblocking agents are used among the other additives, they may be added when preparing the liquid crystal polymer composition, or may be attached to the pellet surface of the liquid crystal polymer composition during molding.

[0079] Specific examples of other resin components include thermoplastic resins such as polyamide, polyester, polyacetal, polyphenylene ether and modified products thereof, polysulfone, polyethersulfone, polyetherimide, polyamideimide, etc., and thermosetting resins such as phenol resin, epoxy resin, polyimide resin, etc. These resin components may be used alone or in combination of two or more kinds.

[0080] When other resin components are contained, the content thereof is preferably 100 parts by mass or less, and more preferably 80 parts by mass or less, per 100 parts by mass of the wholly aromatic liquid crystal polymer.

[0081] The liquid crystal polymer composition of the present invention can be obtained by blending the above-mentioned wholly aromatic liquid crystal polymer, reinforcing fiber and carbodiimide group-containing compound with the above-mentioned inorganic filler and / or organic filler, other additives and other resin components, etc., as desired, in a predetermined composition, and melt-kneading them using a Banbury mixer, a kneader, a single-screw or twin-screw extruder, etc. The liquid crystal polymer composition of the present invention can also be obtained by dry-blending the wholly aromatic liquid crystal polymer, reinforcing fiber and carbodiimide group-containing compound, and melt-kneading them in a molding machine.

[0082] The liquid crystal polymer composition of the present invention thus obtained can be processed into a molded article by a known molding method such as injection molding, compression molding, extrusion molding, or blow molding.

[0083] The molded article made of the liquid crystal polymer composition of the present invention has improved hydrogen gas barrier properties while maintaining mechanical properties such as bending strength, and is therefore suitable for use as packaging containers such as bottles, films, containers, tanks, etc. It is particularly useful as a liquid hydrogen tank. EXAMPLES

[0084] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the examples, bending strength and hydrogen gas permeability tests were performed according to the methods described below.

[0085] <Flexural strength and flexural modulus> Using an injection molding machine (UH1000-110 manufactured by Nissei Plastics Co., Ltd.), injection molding was performed at a cylinder temperature of 20 to 40°C above the crystal melting temperature and a mold temperature of 70°C to obtain rectangular bending test pieces (length 127 mm x width 12.7 mm x thickness 3.2 mm). The bending test was a three-point bending test using an autograph AGX-V manufactured by Shimadzu Corporation in accordance with ASTM D790, with a span distance of 50.0 mm and a compression speed of 1.3 mm / min.

[0086] Tensile strength and tensile modulus Dumbbell-shaped tensile test pieces (ASTM No. 4, thickness 3.2 mm) were obtained under the same conditions as the molded pieces used for measuring bending strength and bending modulus. The tensile test was performed using an autograph AG-X plus made by Shimadzu Corporation in accordance with ASTM D638, with a span distance of 64.0 mm and a tensile speed of 5 mm / min.

[0087] <Hydrogen gas permeability> Using an injection molding machine (UH1000-110, manufactured by Nissei Plastic Industrial Co., Ltd.), rectangular test pieces (100 mm × 100 mm × 0.8 mm thick) were molded, which were then machined into circles with a diameter of 60 mm. These were then used to perform measurements at 23°C in a dry state in accordance with JIS K7126-1, and the hydrogen gas permeability coefficient was calculated.

[0088] In the examples and comparative examples, the following abbreviations represent the following compounds. LCP: Fully aromatic liquid crystal polymer CF: Carbon fiber CI: Carbodiimide group-containing compounds IP: Imine modified polyolefin POB: 4-hydroxybenzoic acid BON6: 6-hydroxy-2-naphthoic acid HQ: Hydroquinone TPA: Terephthalic acid

[0089] (Synthesis of Liquid Crystal Polymer) [Synthesis example 1 (LCP-1)] A reaction vessel equipped with a stirrer with a torque meter and a distillation tube was charged with 349.3 g (40 mol%) of POB, 476.0 g (40 mol%) of BON6, 69.7 g (10 mol%) of HQ, and 105.0 g (10 mol%) of TPA, and further charged with 1.03 times the moles of acetic anhydride relative to the amount (mol) of hydroxyl groups in the total monomers, and deacetic acid polymerization was carried out under the following conditions.

[0090] The temperature was raised from room temperature to 145°C in 1 hour under a nitrogen gas atmosphere, and the temperature was maintained for 30 minutes. Next, the temperature was raised to 330°C over 7 hours while distilling off the by-product acetic acid, and then the pressure was reduced to 10 mmHg over 80 minutes. The polymerization reaction was terminated when a predetermined torque was reached, the contents were removed from the reaction vessel, and pellets of a wholly aromatic liquid crystal polyester resin were obtained using a pulverizer. The amount of acetic acid distilled during polymerization was almost the theoretical value. The crystal melting temperature (Tm) of the obtained LCP pellets measured by DSC was 218°C.

[0091] The following carbon fibers, carbodiimide group-containing compounds, and imine-modified polyolefins were used.

[0092] Carbon Fiber (CF) Chopped fiber "PYROFIL (registered trademark) TR06U B4J" manufactured by Mitsubishi Chemical Corporation

[0093] Carbodiimide group-containing compounds (CI) "Carbodilite (registered trademark) LA-1" manufactured by Nisshinbo Inc.

[0094] <Imine-modified polyolefin (IP)> "Admer (registered trademark) IP AT3346" manufactured by Mitsui Chemicals, Inc.

[0095] (Examples 1 to 3) LCP-1, carbon fiber, and a carbodiimide group-containing compound (CI) were mixed to the contents shown in Table 1, and melt-kneaded at 250°C using a twin-screw extruder (TEX-30, manufactured by Nippon Steel Corporation) to obtain pellets of a liquid crystal polymer composition. The obtained pellets were used to measure the bending strength, bending modulus, tensile strength, tensile modulus, and hydrogen gas permeability coefficient by the above-mentioned methods. The results are shown in Table 1.

[0096] Comparative Example 1 Pellets of the liquid crystal polymer composition were obtained in the same manner as in Example 1, except that no carbodiimide group-containing compound was used, and the flexural strength, flexural modulus, tensile strength, tensile modulus and hydrogen gas permeability coefficient were measured. The results are shown in Table 1.

[0097] Comparative Example 2 Pellets of the liquid crystal polymer composition were obtained in the same manner as in Example 3, except that no carbodiimide group-containing compound was used, and the flexural strength, flexural modulus, tensile strength, tensile modulus and hydrogen gas permeability coefficient were measured. The results are shown in Table 1.

[0098] Comparative Example 3 Except for using imine-modified polyolefin (IP) instead of the carbodiimide group-containing compound, pellets of the liquid crystal polymer composition were obtained in the same manner as in Example 1, and the bending strength, bending modulus, tensile strength, tensile modulus and hydrogen gas permeability coefficient were measured. The results are shown in Table 1.

[0099] (Reference example 1) Liquid crystal polymer pellets were obtained in the same manner as in Example 1, except that the carbodiimide group-containing compound and carbon fiber were not used, and the bending strength, bending modulus, tensile strength, tensile modulus, and hydrogen gas permeability coefficient were measured. The results are shown in Table 1.

[0100] As shown in Table 1, all of the liquid crystal polymer compositions of Examples 1 to 3 were excellent in mechanical properties such as bending strength, and had improved hydrogen gas barrier properties.

[0101] In contrast, it was confirmed that the compositions of Comparative Examples 1 to 3 had deteriorated hydrogen gas barrier properties compared to Reference Example 1.

[0102] [Table 1]

Claims

1. A liquid crystal polymer composition comprising 100 parts by mass of a wholly aromatic liquid crystal polymer having a crystal melting temperature of 210 to 250° C., 1 to 100 parts by mass of reinforcing fiber, and 0.01 to 10 parts by mass of a carbodiimide group-containing compound.

2. 2. The liquid crystal polymer composition according to claim 1, wherein the wholly aromatic liquid crystal polymer has a crystalline melting temperature of 215 to 245°C.

3. The wholly aromatic liquid crystal polymer is represented by the formulas (I) to (IV): [Formula 1] [In the formula, Ar 1 and Ar 2 each represents one or more kinds of divalent aromatic groups, and p, q, r and s each represent a composition ratio (mol %) of each repeating unit in the wholly aromatic liquid crystal polyester, and satisfy the following condition: 0.5≦p / q≦2.5 2≦r≦15, and 2≦s≦15] 2. The liquid crystal polymer composition according to claim 1, which is a wholly aromatic liquid crystal polyester comprising a repeating unit represented by the following formula:

4. Formula (III) and / or Formula (IV) are Ar 1 and Ar 2 are independently represented by the formulas (1) to (4). [chemical 2] 4. The liquid crystalline polymer composition of claim 3, comprising one or more repeat units which are aromatic groups selected from the group consisting of:

5. 2. The liquid crystalline polymer composition of claim 1, wherein the reinforcing fibers are carbon fibers.

6. 2. The liquid crystalline polymer composition according to claim 1, wherein the carbodiimide group-containing compound is a polycarbodiimide compound.

7. A molded article made of the liquid crystal polymer composition according to any one of claims 1 to 6.

8. 8. The molded article of claim 7, wherein the molded article is a liquid hydrogen tank.

Citation Information

Patent Citations

  • Liquid crystalline resin composition

    JP2008001848A

  • Polybutylene succinate resin composition, and method for producing the same

    JP2012153845A

  • Polybutylene terephthalate resin composition

    JP2015224341A

  • Thermoplastic polyester resin composition and molding thereof

    JP2018053230A

  • Thermoplastic polyester resin composition and molding thereof

    JP2018188547A