Evaluation method for amount of attached polymer, and manufacturing method for base material with polymer
Infrared spectroscopy with a calibration curve is used to quantify polymer adhesion, addressing the lack of quantitative methods in existing technologies and ensuring stable polymer coating production.
Patent Information
- Application Number
- JP2023055960
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for evaluating polymer attachment to a base material do not provide a quantitative measure of the amount of polymer attached.
A method using infrared spectroscopy to determine the adhesion amount of a polymer by correlating the peak area of a functional group in the polymer's molecule with the amount of polymer attached, utilizing a calibration curve to quantify the polymer adhesion.
Enables accurate quantification of polymer adhesion, improving measurement stability and allowing for consistent production of polymer-coated substrates.
Smart Images

Figure 2024143338000004 
Figure 2024143338000005 
Figure 2024143338000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for evaluating the amount of polymer adhesion and a method for producing a substrate with a polymer. [Background technology]
[0002] Various evaluation methods for polymers using infrared spectroscopy have been developed so far. For example, the technique described in Patent Document 1 is known as this type of technique. Patent Document 1 describes an evaluation method characterized by evaluating the thickness of a chemical on the surface of a polymer test piece and / or evaluating the degree of discoloration of the surface of the polymer test piece (Table 1 of Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-085067 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the polymer evaluation method described in Patent Document 1, no specific consideration is given to a method for quantifying the amount of polymer adhered to a substrate. [Means for solving the problem]
[0005] As a result of further investigation, the inventors have found that in the infrared absorption spectrum (AS) of a polymer-attached substrate measured using infrared spectroscopy, in addition to the absorption peaks originating from the material constituting the substrate, an absorption peak originating from at least one type of functional group that the polymer has in its molecule is also detected. As a result of further intensive research based on this finding, it was found that in the infrared absorption spectrum (AS) of a substrate with a polymer measured by infrared spectroscopy, there is a correlation between the peak area (S) of an absorption peak derived from one of the functional groups contained in the polymer molecule and the amount (W) of the polymer attached to the substrate, which led to the completion of the present invention.
[0006] According to one aspect of the present invention, there is provided the following method for evaluating the amount of polymer adhesion and method for producing a substrate with a polymer. 1. A method for producing a substrate having a polymer, the polymer having one or more functional groups in the molecule formed on at least a part of the surface of the substrate, comprising a quantitative determination step of quantifying the amount of the polymer attached thereto by infrared spectroscopy; The quantitative step is a method for evaluating the amount of polymer adhesion, which comprises calculating a peak area (S) of an absorption peak derived from one of the functional groups in the polymer from an infrared absorption spectrum (AS) of the polymer-attached substrate obtained by infrared spectroscopy, and quantifying the amount of polymer adhesion (W) based on the peak area (S). 2. The method for evaluating the amount of polymer adhesion according to 1., The method for evaluating the amount of polymer attached, in the quantitative step, calculates the amount of polymer attached (W) from the peak area (S) derived from one of the functional groups in the polymer using a calibration curve showing the correlation between the amount of polymer attached (w) and the peak area (s) of an absorption peak derived from one of the functional groups. 3. The method for evaluating the amount of polymer adhesion according to 1. or 2., The method for evaluating a polymer adhesion amount, wherein in the quantitative determination step, the peak area (S) is calculated from the infrared absorption spectrum (AS) normalized using a peak intensity derived from the substrate. 4. A method for evaluating a polymer adhesion amount according to any one of 1. to 3., The method for evaluating the amount of attached polymer, wherein in the quantitative determination step, the peak area (S) is calculated from the infrared absorption spectrum (AS) that has been subjected to waveform separation processing. 5. A method for evaluating a polymer adhesion amount according to any one of 1. to 4., In the quantitative step, the infrared absorption spectrum (AS) is normalized using the peak intensity of an absorption peak of an overtone of an aromatic ring derived from the base material, and the peak area (S) derived from the functional group having C=O absorption is calculated from the normalized infrared absorption spectrum (AS). 6. A method for evaluating a polymer adhesion amount according to any one of 1. to 5., The method for evaluating a polymer adhesion amount, wherein the substrate is an organic particle or an inorganic particle. 7. A method for producing a substrate with a polymer, comprising the steps of: a surface modification step of forming a polymer on at least a portion of the surface of the substrate; and a quality assessment step of determining whether the amount of polymer adhesion is within a predetermined range based on the method for evaluating the amount of polymer adhesion according to any one of 1. to 6. Method for producing a substrate with a polymer. Effect of the Invention
[0007] According to the present invention, there are provided an evaluation method capable of quantitatively determining the amount of polymer attached to a substrate, and a method for producing a polymer-attached substrate using the same. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a diagram showing an infrared absorption spectrum of a substrate alone sample. [Diagram 2] FIG. 2 is a diagram showing an infrared absorption spectrum of a sample for FT-IR measurement. [Diagram 3] FIG. 1 is a diagram showing the relationship between the polymer concentration and the peak area corresponding to the absorption peak of each functional group derived from the polymer. [Figure 4] FIG. 1 is a diagram showing a calibration curve for calculating the amount of attached polymer.
[0009] The method for evaluating the amount of polymer adhesion according to this embodiment will be outlined below.
[0010] The method for evaluating the amount of polymer adhesion of this embodiment includes a quantitative step of quantifying the amount of polymer adhesion in a polymer-attached substrate, in which a polymer having one or more functional groups in the molecule is formed on at least a part of the surface of the substrate, by using infrared spectroscopy. In this quantitative step, the peak area (S) of an absorption peak derived from one of the functional groups in the polymer is calculated from the infrared absorption spectrum (AS) of the polymer-attached substrate obtained by infrared spectroscopy, and the amount of polymer adhesion (W) is quantified based on the peak area (S).
[0011] According to the findings of the present inventors, it has been found that in the infrared absorption spectrum (AS) of a substrate with a polymer measured by infrared spectroscopy, the peak area (S) of an absorption peak derived from one of the functional groups contained in the polymer molecule is correlated with the amount (W) of the polymer attached to the substrate. Therefore, the amount (W) of the polymer attached to the substrate can be quantified by the index of the peak area (S) of the absorption peak derived from the functional group in the polymer.
[0012] In addition, a calibration curve showing the correlation between the peak area (s) of the absorption peak derived from the functional group of the polymer and the amount of polymer attached (w) is created using multiple samples with different amounts of polymer attached. By using such a calibration curve, it becomes possible to quantify the amount of unknown polymer attached (W) in the polymer-attached substrate using an index called polymer mass. Note that this index is not limited to polymer mass, and an index obtained by modifying the polymer mass, such as an index obtained by dividing the polymer mass by the polymer molecular weight or the substrate mass, can also be used.
[0013] In addition, by using the waveform separation technique, it is possible to stably obtain the peak area (S) corresponding to the absorption peak derived from the functional group of the polymer from the infrared absorption spectrum (AS) of the polymer-attached substrate measured by infrared spectroscopy. This reduces measurement variability in the method for evaluating the amount of polymer attached, thereby improving measurement stability. This technique can also be used when creating the above-mentioned calibration curve.
[0014] Hereinafter, each component of the method for evaluating the amount of polymer adhesion according to this embodiment will be described in detail.
[0015] The substrate may be one whose surface is at least partially or entirely covered with a polymer, and is not particularly limited as long as it is a base (support) that serves as a scaffold for the polymer.
[0016] The shape of the substrate is not particularly limited, and may be any of a spherical shape, a plate shape, or various shapes according to the application. When the substrate is spherical, it may be a perfect sphere, a nearly spherical shape other than a perfect sphere, an elliptical shape, or the like. At least a part of the surface of the substrate may be a smooth surface, or may be composed of a non-smooth surface, for example, an uneven surface.
[0017] The material of the substrate is not particularly limited, but at least one of an organic material and an inorganic material is used. In this case, the substrate may be a core particle composed of either an organic particle or an inorganic particle.
[0018] As the organic material, for example, an organic polymer is used. Examples of organic polymers include synthetic resins such as polystyrene, polyvinyl chloride, polypropylene, (meth)acrylic resins, polymethyl methacrylate, and silicone rubber, cellulose derivatives such as nitrocellulose, cellulose, and methylcellulose, phenolic resins, polylactic acid, polyethylene, and melamine phenol, copolymers containing one of these as a main component (for example, copolymers containing styrene as a main component), and copolymers containing two or more of these. These may be used alone or in combination of two or more.
[0019] As the inorganic particles, particles made of an inorganic substance can be used. Examples of inorganic substances include inorganic materials such as metals, ceramics, and glass. Specific examples of inorganic substances include silica. These may be used alone or in combination of two or more. In addition, inorganic materials having magnetic properties may be used as inorganic substances. In this way, the inorganic particles may be non-magnetic particles or magnetic particles.
[0020] Here, the method for evaluating the polymer adhesion amount of this embodiment will be described using an example in which latex particles are used as a substrate. The latex particles are core particles composed of an organic polymer such as polystyrene. In other words, the evaluation method of the present embodiment can quantify the amount of polymer attached to a substrate having a polymer formed on the surface of a latex particle. However, the substrate is not limited to the latex particles.
[0021] One embodiment of the method for evaluating the amount of polymer attached includes a quantitative step of calculating the amount of polymer attached to the substrate with the polymer based on the peak area (S) derived from the functional group in the polymer obtained by infrared spectroscopy using a calibration curve (hereinafter referred to as the "calibration curve (sw)") showing a correlation between the peak area (s) of an absorption peak derived from a specific functional group in the polymer and the amount of polymer attached (w).
[0022] First, the procedure for preparing the calibration curve (sw) will be described. The calibration curve (sw) can be created, for example, by following steps i and ii below using multiple n samples of polymer-attached substrates with different amounts of polymer attached (w) (where n is not particularly limited as long as it is a natural number of 2 or more, but may be 3 or more, or 5 or more). Step i: By infrared spectroscopy, a plurality of infrared absorption spectrum data (as1, as2, . . . asn) corresponding to a plurality of samples is obtained. Step ii: In each of the obtained infrared absorption spectrum data, a plurality of peak area data (s1, s2, . . . sn) for an absorption peak originating from a predetermined functional group (f1) in the polymer is obtained. Step iii: The above calibration curve (sw) is created based on the correlation between the multiple peak area data (s1, s2, . . . sn) and the multiple polymer adhesion amount data (w1, w2, . . . wn).
[0023] (Calibration curve creation process i) The infrared spectroscopy that can be used is Fourier transform infrared spectroscopy (FIIR). The preparation (pretreatment) of the measurement samples (multiple samples) used in infrared spectroscopy is not particularly limited, and known solid sample preparation methods using transmission methods such as the tablet method or plate method or reflection methods such as the ATR method can be used. From the viewpoint of spectral accuracy, the tablet method is preferable. For the tablet method, a material that becomes transparent in the infrared region when pressure is applied can be used, for example, an alkali halide such as potassium bromide (KBr).
[0024] The procedure for preparing a measurement sample using the KBr tablet method is shown below, but is not limited to this. First, the dispersion of latex particles is vacuum-dried at a predetermined temperature to obtain a substrate sample. For example, 10 μL of a 10% by mass aqueous dispersion of latex particles is placed in a mortar and vacuum-dried at 40° C. overnight. Next, a polymer solution containing a polymer is added to the substrate sample so that the polymer concentration, expressed as (polymer mass / substrate sample mass) x 100, is w1 (mass %), w2 (mass %), ... wn (mass %), and the solvent is evaporated to obtain multiple composite samples. For example, a methanol solution of a polymer is dropped onto the substrate sample so that the polymer concentration is 0, 1, 5, 10, 15, ... 20 mass %, and the methanol is evaporated at room temperature to obtain multiple composite samples. Next, multiple samples (solid measurement samples) with different polymer concentrations are prepared by the KBr tablet method. In the KBr tablet method, for example, KBr powder and a composite sample are mixed and pressed to obtain multiple tablets (multiple samples) with different polymer concentrations. When using a measurement sample using the KBr pellet method, it is advisable to perform background measurement using KBr alone before measuring the infrared absorption spectrum.
[0025] (Calibration curve creation process ii) In this embodiment, it is preferable to perform waveform separation processing on the infrared absorption spectrum (as) of the sample obtained by infrared spectroscopy, which makes it possible to stably obtain the peak area (s) corresponding to the absorption peak derived from the functional group of the polymer.
[0026] The waveform separation process is generally performed by normalizing the infrared absorption spectrum (as) using a specific absorption peak derived from the substrate, and then waveform separating the normalized infrared absorption spectrum (as) using the absorption derived from the functional groups of the polymer.
[0027] A specific example of the waveform separation process is a method based on the following steps 1 to 4. However, the method is not limited to these steps. Step 1: Normalize the peak intensity in the infrared absorption spectrum (as) using a specific absorption peak derived from the substrate. Step 2: If necessary, subtract the infrared absorption spectrum (peak area) of the substrate alone from the infrared absorption spectrum (as). Note that the infrared absorption spectrum of the substrate alone to be used should also be normalized in advance using a specific absorption peak derived from the substrate. Step 3: Using the absorption due to the functional groups of the polymer, the normalized infrared absorption spectrum (as) is subjected to waveform separation. Step 4: After waveform separation, the peak area (s) corresponding to the absorption peak due to the functional group (f) of the polymer is obtained. The infrared absorption spectrum measured is, for example, 1400 to 2000 cm -1 In the above measurement wavenumber range, a measurement sample that has been baseline corrected so that the base is horizontal can be used.
[0028] In the above step 1, a process is performed to normalize the peak intensity of the infrared absorption spectrum (as) of the sample obtained in the calibration curve creation step i. A predetermined absorption peak derived from the substrate can be used as the standard for normalization, but when the substrate is an organic material (latex particles, etc.), for example, an absorption peak of an aromatic ring overtone can be used. When the substrate is an inorganic material, for example, an absorption peak derived from an oxide such as SiO2, TiO2, Al2O3, Fe2O3, Fe3O4, MgO, ZnO, ZrO2, or CuO can be used.
[0029] In the above step 2, when the absorption peak originating from the substrate overlaps or partially overlaps with the absorption peak originating from the functional group of the polymer used in step 3, it is preferable to subtract the infrared absorption spectrum (peak area) of the substrate alone from the infrared absorption spectrum (as) in advance. However, when no overlap is observed or the overlap is small enough to be acceptable, step 2 does not have to be carried out. The infrared absorption spectrum of the substrate alone is obtained by using the substrate alone (e.g., latex particles) as a measurement sample for the KBr tablet method described in the calibration curve creation step I. When the substrate is an organic material, the infrared absorption spectrum of the substrate alone is normalized using the absorption peak of the overtone of the aromatic ring.
[0030] In the above step 3, waveform separation processing is performed on the normalized infrared absorption spectrum (as). Absorption from the functional group of the polymer is not particularly limited as long as a peak can be observed, and examples include C=O, CH, C=C, COC, NH, CN, NO2, SO2, etc. Among these, it is preferable to use the absorption of C=O, which has strong absorption, since it can be clearly observed even in small amounts. In addition, taking into consideration that aromatic ring absorption originating from the substrate exists in the portion overlapping with C=O, it is preferable to fix the aromatic ring absorption originating from the substrate at the peak (center position, half width, height) obtained by the waveform separation result of the substrate alone, and fit the peaks originating from various functional groups having C=O absorption (unsaturated ester group, saturated ester group, carboxylic acid group, cyclic anhydride group, etc.) with a Gaussian function (waveform separation processing). Fitting may be performed with a Lorentzian function or a Voigt function other than the Gaussian function. In addition, when the substrate is an organic material, the peak obtained by the waveform separation result of the substrate alone means a peak corresponding to an aromatic overtone among the infrared absorption spectrum of the substrate alone after normalization, which is fitted by a similar method such as a Gaussian function.
[0031] In the above step 4, after waveform separation, the peak area (s) corresponding to the absorption peak derived from the functional group (f) of the polymer is obtained. Examples of the functional groups (f1 to f4) of the polymer having C=O include unsaturated ester groups, saturated ester groups, carboxylic acid groups, cyclic anhydride groups (maleic anhydride groups), etc. For any functional group, a peak area (s) can be obtained.
[0032] (Calibration curve creation process iii) An approximation line is created as a calibration curve (sw) that represents the correlation between the peak area (s) obtained in the calibration curve creation step ii and the amount of polymer attached (w). The approximation line may be any line that represents a monotonic relationship, and may be, for example, any of a linear function, a quadratic or cubic function, an exponential function, a logarithmic function, and the like. For example, a plurality of plots representing a plurality of peak area data and a plurality of polymer adhesion amount data can be approximated by a known method such as the least squares method, and an approximate straight line can be used as the calibration curve (sw).
[0033] The data on the amount of polymer adhesion (w1, w2, ... wn) can be calculated, for example, using the amounts of polymers charged for each of the samples. When all of the polymers react and adhere to the surface of the substrate, the charged amount can be considered as the amount of polymer adhesion. Alternatively, the amount of polymer remaining in the reaction solution of the polymer and the substrate can be obtained, and the amount of polymer adhesion can be calculated by subtracting the remaining amount from the charged amount. Here, the amount of polymer attached can be the dry mass (g) measured after the polymer is dried.
[0034] The inventors have examined the calibration curve (sw) created in the calibration curve creation step iii and found that an approximation line showing a proportional relationship between the peak area (s) and the amount of polymer attached (w) can be obtained in all cases of an unsaturated ester group, a saturated ester group, a carboxylic acid group, and a cyclic anhydride group (maleic anhydride group). As a result of further investigation, it was found that when latex particles are used as the base material, the saturated ester group and carboxylic acid group overlap with the absorption of substances other than the polymer, and the maleic anhydride group opens its ring in water and may change over time. From the standpoint of accuracy and stability, therefore, it is preferable to use an unsaturated ester group (f1) as the functional group (f) of the polymer having C=O.
[0035] Next, using the above-mentioned calibration curve (sw) prepared in advance, the amount of polymer attached to the polymer-attached substrate (W) is calculated based on the peak area (S) derived from the functional group (f) in the polymer obtained by infrared spectroscopy.
[0036] To obtain the peak area (S) derived from the functional group (f) in the polymer, a method similar to the method used to obtain the peak area (s) described above can be used. An example of a specific method is as follows, but is not limited to this. First, a measurement sample is prepared by the KBr pellet method, and the infrared absorption spectrum (AS) of the polymer-attached substrate is measured by Fourier transform infrared spectroscopy (FIIR). Next, the infrared absorption spectrum (AS) is normalized using a predetermined absorption peak derived from the substrate. Next, the peak area (S) attributable to the functional group (f) in the polymer is obtained from the normalized infrared absorption spectrum (AS). Regarding the functional group (f) in the polymer, from the viewpoints of accuracy and stability, the functional group (f) of the polymer having C═O may be an unsaturated ester group. If necessary, the infrared absorption spectrum (peak area) of the substrate alone may be subtracted from the normalized infrared absorption spectrum (AS). Moreover, the infrared absorption spectrum (AS) may be subjected to waveform separation processing using a Gaussian function as described above.
[0037] By substituting the peak area (S) derived from the functional group (f) in the polymer obtained above into the calibration curve (sw), the amount of polymer attached to the polymer-attached substrate (W) can be calculated.
[0038] The manufacturing method of the polymer-attached substrate of this embodiment includes a surface modification step of forming a polymer on at least a portion of the surface of the substrate, and a quality assessment step of determining whether the amount of polymer adhesion is within a predetermined range based on the above-mentioned polymer adhesion amount evaluation method.
[0039] As an example, the above-mentioned polymer-attached substrate can be used as particles for an agglutination method used in detecting a target substance by an agglutination method. The agglutination method is a method in which a sample containing a target substance (e.g., an antigen) is contacted in a dispersion medium with a polymer-attached substrate carrying a ligand (e.g., an antibody) that specifically recognizes (binds to) the target substance, causing the ligand to bind to the target substance, forming a complex between the target substance, the ligand, and the polymer-attached particles, and selectively agglutinating the polymer-attached substrate. One type of agglutination method, the immune agglutination method (also called immune turbidimetry), utilizes an antigen-antibody reaction to react an antigen with an antibody present on the surface of the polymer-attached substrate, thereby agglutinating the polymer-attached substrate. In a method for detecting a target substance using an agglutination method, the degree of agglutination of the polymer-attached substrate can be characterized and quantified by optical measurement such as absorbance, scattered light intensity, or transmitted light intensity. The polymer-attached substrate used in such an aggregation method can be suitably used as an in vitro diagnostic agent or the like. However, it was necessary to consider the conditions for immobilizing the ligand (antibody) every time the lot of the raw material latex particles was changed, because it was expected that the surface of the latex particles would change with each lot. Therefore, in the manufacturing method of a polymer-attached substrate, a quality assessment process based on the above-mentioned polymer adhesion amount evaluation method is performed, whereby the polymer adhesion amount as the surface condition of the particles can be kept within a predetermined range, thereby suppressing lot-to-lot variation of the polymer-attached substrate.
[0040] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES
[0041] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.
[0042] <Polymer synthesis> Norbornene and maleic anhydride were reacted by radical polymerization at a predetermined ratio using an azo compound (polymerization initiator), to obtain polymer precursor A. Subsequently, various functional monomers having the following functional groups 1 to 3 were subjected to a ring-opening reaction with alcohol in the functional monomer at a predetermined ratio, and introduced into the side chains (ring-opened maleic anhydride groups) of each polymer precursor A, followed by reprecipitation with hexane or diethyl ether to obtain maleic anhydride-based polymers (polymers A1 to A4 shown in Table 1).
[0043] [Table 1]
[0044] [ka] [ka]
[0045] <Preparation of calibration curve> (1) Preparation of samples for FT-IR measurement 10 μL of a dispersion of latex particles (polystyrene latex particles, manufactured by JSR, product name: IMMUNTEX, average particle diameter: 351 nm, solid content: 10% by mass) was placed in a mortar and dried in vacuum at 40° C. overnight to obtain a “substrate alone sample.” Next, a methanol solution containing the polymer A1 synthesized above was added to the above substrate alone sample so that the polymer concentrations were 0, 1, 2.5, 5, 7.1, 8.5, 10, 11.5, 12.5, 13, 15, 17.5, and 20 mass%, and the methanol was evaporated at room temperature to obtain multiple "composite samples" with different polymer concentrations. The polymer concentration was calculated from (mass of polymer / mass of the base material alone sample)×100. Next, the KBr powder and the composite sample were mixed and pressed to prepare tablets with different polymer concentrations (samples for FT-IR measurement).
[0046] (ii) FI-IR measurement Using a Fourier transform infrared spectrophotometer (manufactured by JASCO Corporation, product name: FT-IR6100), infrared absorption spectra (as) were obtained for the multiple samples for FT-IR measurement obtained above according to the following steps 1 to 4. Based on the obtained infrared absorption spectrum (as), the peak area (s) corresponding to the absorption peak derived from the functional group of the polymer was obtained.
[0047] Step 1: The peak intensity in the infrared absorption spectrum (as) of each FT-IR measurement sample was normalized using the absorption peak of the overtone of the aromatic ring derived from the latex particles (base material).
[0048] Step 2: The infrared absorption spectrum (peak area) of the latex particles (base material alone) was subtracted from the infrared absorption spectrum (as) of each FT-IR measurement sample. However, for the infrared absorption spectrum of the base material alone used, the measurement sample was prepared using the KBr tablet method, and the peak intensity was standardized in advance using the absorption peak of the aromatic ring overtone. However, the infrared absorption spectrum measured was from 1400 to 2000 cm -1 The baseline was corrected so that the base was horizontal in the measurement wave number range of 1000, 1000, 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000, 10000, 11000, 12000, 13000, 14000, 15000, 16000, 17000, 18000, 19000, 20000, 210000, 22000, 23000, 24000, 25000, 26000, 27000, 28000, 29000, 30000, 310000, 32000, 33000, Here, the infrared absorption spectrum of the latex particles (base material alone) is shown in FIG. 1, and the infrared absorption spectrum (as) of one of the samples for FT-IR measurement is shown in FIG.
[0049] Step 3: Considering that the aromatic ring absorption of the latex particle (base material alone) exists in the area overlapping with C=O, the aromatic ring absorption from the base material was fixed to the peak (center position, half width, height) obtained from the waveform separation of the base material alone, and the peaks from various functional groups with C=O absorption (unsaturated ester group, saturated ester group, carboxylic acid group, cyclic anhydride group, etc.) were each fitted with a Gaussian function (waveform separation processing). Note that the peaks obtained from the waveform separation of the base material alone refer to the peaks corresponding to aromatic overtones among the infrared absorption spectrum of the base material alone after normalization, which is fitted with a Gaussian function.
[0050] Step 4: After waveform separation, the peak areas (s) of the functional groups (f1 to f4) of the polymer having C=O, i.e., unsaturated ester groups, saturated ester groups, carboxylic acid groups, and cyclic anhydride groups (maleic anhydride groups), were obtained.
[0051] By the FT-IR measurement based on the above steps 1 to 4, the peak areas (s) corresponding to the absorption peaks of each functional group derived from polymer A (unsaturated ester group, saturated ester group, carboxylic acid group, cyclic anhydride group) were obtained for each of the multiple FT-IR measurement samples (samples containing polymer A1 and base material).
[0052] (iii) Preparation of a calibration curve The horizontal axis is the polymer concentration, and the vertical axis is the peak areas corresponding to the absorption peaks of unsaturated ester groups, saturated ester groups, carboxylic acid groups, and cyclic anhydride groups. The relationship between the polymer concentration and the peak areas corresponding to the absorption peaks of each functional group derived from the polymer is shown in Figure 3. From Figure 3, it was shown that the polymer concentration and peak area of all the above four functional groups show a proportional relationship. Among them, from the viewpoint of measurement stability, a calibration curve was created by the least squares method using the proportional relationship between the polymer concentration and peak area of the unsaturated ester group. The calibration curve for calculating the amount of attached polymer is shown in Figure 4.
[0053] Based on the calibration curve prepared above, the formula polymer concentration = (mass of polymer / mass of substrate sample alone) × 100 was transformed to derive a function for calculating the "amount of polymer attached (mg) per 100 mg of latex particles (substrate)" using the peak area (s) as a variable. Then, by measuring the infrared absorption spectrum (AS) of the substrate with the polymer and calculating the peak area (S) corresponding to the absorption peak of the functional group of the polymer, such as an unsaturated ester group, and introducing this value into the above equation, it became possible to quantify the amount of the unsaturated ester group polymer attached.
[0054] <Quantitative determination of the amount of polymer attached to a substrate with polymer> (Preparation of calibration curves for other polymers A2 to A4) In addition, using the above polymers A2 to A4, samples for FT-IR measurement were prepared in the same manner as for polymer A1, and a calibration curve was created using the peak area (s) of the absorption peak of the unsaturated ester group, and a function for calculating the amount of attached polymer was derived from the calibration curve.
[0055] (Preparation of substrate with polymer) Diamine was mixed into the dispersion of latex particles used above, and the carboxy groups of the polystyrene latex particles were reacted with the diamine to introduce primary amino groups, followed by purification (amino treatment). Next, the above polymers A1 to A4 were added to a solution containing polystyrene latex particles having primary amino groups, and mixed at a predetermined mixing ratio to react the primary amino groups with the maleic anhydride groups. The resulting mixture was purified to obtain a dispersion containing core particles (substrates with polymer) having a polymer introduced onto their surfaces (polymer introduction treatment). For each of the obtained polymer-attached substrates, an infrared absorption spectrum (AS) was obtained according to the procedure described above in <Preparation of calibration curve>, and the peak area (S) corresponding to the absorption peak of the unsaturated ester group was calculated. This peak area (S) was calculated for each of the polymers A1 to A4 for each amount of the polymers.
[0056] The amount of polymer attached was calculated by inserting the obtained peak area (S) into the function derived above. The relationship between the amount of polymer attached calculated from the function and the amount of polymer added in the above (preparation of substrate with polymer) was evaluated, and it was confirmed that there was a correlation between the two in all of the cases of polymers A1 to A4. Therefore, it was confirmed that the amount of polymer attached can be quantified by the method of the embodiment.
Claims
1. The method includes a quantitative determination step of quantifying an adhesion amount of a polymer on a substrate having a polymer having one or more functional groups in a molecule formed on at least a part of a surface of the substrate, using infrared spectroscopy; The quantitative step is a method for evaluating the amount of attached polymer, which comprises calculating a peak area (S) of an absorption peak derived from one of the functional groups in the polymer from an infrared absorption spectrum (AS) of the polymer-attached substrate obtained by infrared spectroscopy, and quantifying the amount of attached polymer (W) based on the peak area (S).
2. The method for evaluating a polymer adhesion amount according to claim 1, The method for evaluating a polymer adhesion amount, in the quantitative determination step, calculates the polymer adhesion amount (W) from the peak area (S) derived from one of the functional groups in the polymer using a calibration curve showing a correlation between the polymer adhesion amount (w) and a peak area (s) of an absorption peak derived from one of the functional groups.
3. The method for evaluating a polymer adhesion amount according to claim 1 or 2, The method for evaluating a polymer adhesion amount, wherein in the quantitative determination, the peak area (S) is calculated from the infrared absorption spectrum (AS) normalized using a peak intensity derived from the substrate.
4. The method for evaluating a polymer adhesion amount according to claim 1 or 2, The method for evaluating a polymer adhesion amount, wherein in the quantitative determination step, the peak area (S) is calculated from the infrared absorption spectrum (AS) that has been subjected to waveform separation processing.
5. The method for evaluating a polymer adhesion amount according to claim 1 or 2, In the quantitative step, the infrared absorption spectrum (AS) is normalized using a peak intensity of an absorption peak of an overtone of an aromatic ring derived from the base material, and the peak area (S) derived from the functional group having C═O absorption is calculated from the normalized infrared absorption spectrum (AS).
6. The method for evaluating a polymer adhesion amount according to claim 1 or 2, The method for evaluating a polymer adhesion amount, wherein the substrate is an organic particle or an inorganic particle.
7. A method for producing a substrate with a polymer, comprising the steps of: a surface modification step of forming a polymer on at least a portion of the surface of the substrate; and a quality assessment step of determining whether the amount of polymer adhesion is within a predetermined range based on the method for evaluating the amount of polymer adhesion according to claim 1 or 2. Method for producing a substrate with a polymer.
Citation Information
Patent Citations
Method for evaluating thickness of chemical on polymer test piece surface, and method for evaluating discoloration degree of polymer test piece surface
JP2016085067A