Workpiece processing protective sheet and method for manufacturing workpiece individualized piece

A protective sheet with controlled thermal deformability addresses the chipping issue in thin semiconductor devices by minimizing deformation during multiple thermal cycles, ensuring high-yield production of singulated workpieces.

JP2024143342APending Publication Date: 2024-10-11LINTEC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023055968
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

As semiconductor devices become thinner, the issue of chipping during the backside grinding process of workpieces, such as semiconductor wafers, increases due to multiple thermal cycles of the workpiece processing protection sheets, leading to contact between singulated workpieces.

Method used

A workpiece processing protective sheet with controlled thermal deformability, comprising a base material, buffer layer, and adhesive layer, designed to minimize deformation during multiple thermal cycles, ensuring minimal contact between singulated workpieces.

Benefits of technology

The protective sheet maintains a small amount of deformation within a certain range, preventing chipping and allowing for high-yield production of singulated workpieces even after multiple thermal cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143342000001_ABST
    Figure 2024143342000001_ABST
Patent Text Reader

Abstract

To provide a workpiece processing protective sheet having less deformation amount even when receiving thermal histories many times and having the deformation amount in a fixed range.SOLUTION: A workpiece processing protective sheet includes a base material 10; a buffer layer 20 provided on the side of at least one surface of the base material; and an adhesive layer 30 provided on the side of the other surface of the base material. When thermomechanically analyzing the workpiece processing protective sheet, a deformation ratio Df1 at the time of first heating at 50°C is within 0.67%; and the absolute value of a difference between the deformation ratio Df1 at the time of the first heating and a deformation ratio Df2 at the time of second heating at 50°C is within 0.067%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a protective sheet for workpiece processing and a method for manufacturing a workpiece singulated product. In particular, the present invention relates to a protective sheet for workpiece processing suitable for use in a method for grinding the back surface of a workpiece and singulating the workpiece by the resulting stress, and a method for manufacturing a workpiece singulated product using the protective sheet for workpiece processing. [Background technology]

[0002] As various electronic devices become smaller and more multifunctional, the semiconductor chips mounted on them are also required to be smaller and thinner. In order to thin the chips, the backside of the semiconductor wafer is generally ground to adjust the thickness. In addition, to obtain thinned chips, a method called Dicing Before Grinding (DBG) is sometimes used, in which a groove of a specified depth is formed on the front side of the wafer with a dicing blade, and then the wafer is ground from the backside, and the ground surface reaches the groove or the vicinity of the groove to separate the wafer and obtain chips. In DBG, the backside grinding of the wafer and the wafer separation can be performed simultaneously, so that thin chips can be efficiently manufactured.

[0003] In addition, in recent years, a method has been proposed as a variation of the pre-dicing method, in which a modified region is provided inside the wafer by a laser, and the wafer is divided into individual pieces by stress during grinding the back surface of the wafer. Hereinafter, this method may be referred to as LDBG (Laser Dicing Before Grinding). In LDBG, the wafer is cut in the crystal direction starting from the modified region, so that the occurrence of chipping can be reduced more than in the pre-dicing method using a dicing blade. As a result, chips with excellent bending strength can be obtained, and the chips can be further thinned. Furthermore, compared to DBG, in which a groove of a predetermined depth is formed on the wafer surface by a dicing blade, there is no region where the wafer is scraped off by the dicing blade, that is, the kerf width is extremely small, so that the chip yield is excellent.

[0004] Conventionally, when grinding the back surface of a workpiece such as a semiconductor wafer or when dividing the workpiece by DBG or LDBG, a workpiece processing protective sheet called a back grinding sheet is generally attached to the workpiece in order to protect the workpiece and the divided pieces and to hold the workpiece and the divided pieces. After back grinding, an adhesive tape having an adhesive layer is attached to the grinding surface, or a protective film forming tape is attached to form a protective film. Thereafter, the workpiece processing protective sheet attached to the surface of the workpiece is peeled off after its adhesive force is reduced by irradiating it with energy rays such as ultraviolet rays. By such a process, an adhesive layer or a protective film forming layer is formed on the divided pieces of the workpiece.

[0005] As the protective sheet for workpiece processing, a laminated protective sheet including a base material, an adhesive layer, and a buffer layer may be used. Specific examples of such protective sheets for workpiece processing are described in, for example, Patent Document 1 (JP Patent Publication 2015-183008 A). The buffer layer is provided to absorb vibrations generated during grinding of the workpiece and to reduce unevenness caused by foreign matter, thereby stably holding the workpiece flat. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2015-183008 A Summary of the Invention [Problem to be solved by the invention]

[0007] As semiconductor devices become smaller, the final thickness of individual workpieces such as chips tends to become thinner. However, as the individual workpieces become thinner, the phenomenon called "chipping", in which the individual workpieces are damaged, has increased. After intensively investigating the cause of this phenomenon, the present inventors have obtained the following findings.

[0008] When grinding the backside of a workpiece, a protective sheet for workpiece processing is temporarily attached to the circuit surface of the workpiece, and the backside of the workpiece (the side opposite the circuit surface) is ground while spraying water. Spraying water removes the frictional heat generated during backside grinding, and also washes away the grinding chips of the workpiece and the chips of the grinding wheel generated during grinding. Hereinafter, the grinding chips of the workpiece and the chips of the grinding wheel may be collectively referred to as "grinding chips." Additionally, the water sprayed during grinding may be referred to as "grinding water."

[0009] When attaching a protective sheet for workpiece processing to the back surface of a workpiece such as a semiconductor wafer having a large difference in surface unevenness, the protective sheet for workpiece processing may be heated to soften the adhesive layer, and then the protective sheet for workpiece processing may be heated and attached to the surface of the workpiece. By heating the protective sheet for workpiece processing, the adhesive layer softens and deforms to follow the difference in surface unevenness of the workpiece, filling in the surface unevenness, and reliably preventing the grinding water from penetrating the circuit surface.

[0010] In addition, after grinding the backside of the workpiece, a further polishing process called dry polishing may be performed. Dry polishing refers to the process of mirror-finishing the backside of the individual chips with a dry grindstone. Through this process, the fracture layer on the backside of the chips is reduced and the flexural strength is increased. Since water is not sprayed during this process, frictional heat is generated on the grinding surface of the workpiece, which heats up the protective sheet for workpiece processing.

[0011] When grinding the back surface of a workpiece having a large unevenness difference on the surface, the protective sheet for workpiece processing is heated at least twice as described above. Therefore, the protective sheet for workpiece processing is subjected to a thermal history at least twice. When the protective sheet for workpiece processing is heated, it generally softens and deforms. According to the DBG method and LDBG method described above, a group of chips is obtained on the protective sheet for workpiece processing in a form in which the kerf width (chip spacing) is extremely narrow. In particular, according to the LDBG method, the kerf width is substantially 0 (zero).

[0012] When the protective sheet for workpiece processing is heated and attached to the workpiece by heat, the workpiece is divided into individual pieces, and when the temperature returns to room temperature, the protective sheet for workpiece processing tries to return to its shape and size before heating. At this time, if the kerf width is narrow, the chips may come into contact with each other, causing chipping.

[0013] Furthermore, when the workpiece processing protection sheet is heated in the dry polishing process, the workpiece processing protection sheet is deformed again, causing the chip spacing to change, and chipping also occurs at this time.

[0014] If the protection sheet for workpiece processing is subjected to multiple heat histories, the possibility of chipping increases.

[0015] For this reason, it is required that the amount of deformation of the protection sheet for workpiece processing is small even when it is subjected to multiple heat histories, and that the amount of deformation remains within a certain range. [Means for solving the problem]

[0016] The gist of the present invention, which aims to solve such problems, is as follows. (1) A protective sheet for work processing having a substrate, a buffer layer provided on at least one surface of the substrate, and an adhesive layer provided on the other surface of the substrate, When thermomechanical analysis of the protective sheet for workpiece processing is performed under the following conditions, the deformation rate Df1 during the first heating is within 0.67%, and the absolute value of the difference between the deformation rate Df1 during the first heating and the deformation rate Df2 during the second heating is within 0.067%. Thermomechanical analysis conditions Sample size: length 20mm, width 4.5mm Chuck spacing: 15mm The temperature is raised from 23°C to 50°C with a load of 10g and a heating rate of 3°C / min, then allowed to cool to 23°C, and the temperature is raised again to 50°C with a load of 10g and a heating rate of 3°C / min. The deformation rate Df1 (%) when 50°C is reached for the first time, and the deformation rate Df2 (%) when 50°C is reached for the second time are measured. Df1 and Df2 are calculated using the following formulas. Df1 = 100 × (S1-S0) / S0 Df2 = 100 × (S2-S0) / S0 Here, S0 is the chuck interval before the test, S1 is the chuck interval when the temperature reached 50°C for the first time, and S2 is the chuck interval when the temperature reached 50°C for the second time. (2) The protective sheet for workpiece processing according to (1), in which the deformation ratio Df2 (%) when the second temperature reaches 50°C is 0.67% or less. (3) The protective sheet for workpiece processing according to (1), wherein the buffer layer is a cured product of a buffer layer-forming composition containing an energy ray-polymerizable compound. (4) A protective sheet for workpiece processing as described in (1) which is attached to the surface of a workpiece in a process for dividing a workpiece into individual workpieces by grinding the back surface of the workpiece having a groove formed on its surface or a modified region formed inside. (5) A protective sheet for workpiece processing as described in (1) having a substrate, buffer layers provided on both sides of the substrate, and an adhesive layer provided on the surface of one of the buffer layers. (6) The protective sheet for workpiece processing according to (5), wherein the buffer layers provided on both sides of the substrate are both polyolefin-based resin films. (7) A step of heat-attaching the workpiece processing protection sheet according to any one of (1) to (6) above to a surface of the workpiece; A step of forming a groove from the front surface side of the workpiece, or forming a modified region inside the workpiece from the front surface or rear surface of the workpiece; A step of grinding the workpiece having the protective sheet attached to the surface and the groove or the modified region formed thereon from the back side to separate the workpiece into a plurality of workpiece pieces starting from the groove or the modified region; A manufacturing method for a work piece segmented product, comprising a step of performing dry polishing after segmentation. Effect of the Invention

[0017] In the protective sheet for workpiece processing according to the present invention, even if the protective sheet for workpiece processing is subjected to a thermal history many times, the deformation amount is small and within a certain range. Therefore, even if the protective sheet for workpiece processing is subjected to a thermal history many times, there is no contact between the individual workpieces, and individual workpieces can be obtained with a high yield. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a protection sheet for workpiece processing according to this embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing a state in which the protection sheet for workpiece processing according to this embodiment is attached to the surface of a semiconductor wafer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The protective sheet for workpiece processing according to the present invention will be specifically described below. First, the main terms used in this specification will be described.

[0020] The work refers to a plate-shaped body to which the protective sheet for work processing according to this embodiment is attached and then cut into individual pieces. Examples of the work include a circular wafer (including a case having an orientation flat), a rectangular panel level package, and a strip (rectangular substrate) sealed with molded resin. Among them, a wafer is preferable from the viewpoint of easily obtaining the effect of the present invention. The wafer may be, for example, a semiconductor wafer such as a silicon wafer, a gallium arsenide wafer, a silicon carbide wafer, a gallium nitride wafer, or an indium phosphide wafer, or an insulating wafer such as a glass wafer, a lithium tantalate wafer, or a lithium niobate wafer, or may be a reconstructed wafer made of a resin and a semiconductor used for producing a fan-out package or the like. From the viewpoint of easily obtaining the effect of the present invention, a semiconductor wafer or an insulating wafer is preferable, and a semiconductor wafer is more preferable.

[0021] The protective sheet for workpiece processing means a laminate including a substrate, a buffer layer provided on at least one side of the substrate, and an adhesive layer provided on the other side of the substrate, and does not preclude the inclusion of other constituent layers other than these. For example, a primer layer may be formed on the substrate surface on the adhesive layer side, and a release sheet for protecting the adhesive layer until use may be laminated on the surface of the adhesive layer. The buffer layer may be provided on both sides of the substrate, and in this case, the adhesive layer is formed on the surface of one of the buffer layers. The buffer layer may be formed directly on the surface of the substrate, or may be formed via another layer such as an easy-adhesion layer. The same applies when a buffer layer is provided on both sides of the substrate and an adhesive layer is provided on the surface of the one of the buffer layers, and a primer layer may be formed on the surface of the buffer layer on which the adhesive layer is provided. The protective sheet for workpiece processing may also have a constituent layer having antistatic properties. Furthermore, the substrate may be a single layer or may be a multilayer. The same applies to the buffer layer and the adhesive layer.

[0022] A protective sheet for semiconductor processing is an example of a protective sheet for workpiece processing, and "for semiconductor processing" means that it can be used in each process such as transporting semiconductor wafers, back grinding, dicing, and picking up semiconductor chips.

[0023] The singulation of a workpiece refers to dividing the workpiece into individual circuits to obtain individual workpieces. For example, if the workpiece is a semiconductor wafer, the individual workpieces are semiconductor chips, and if the workpiece is a panel level package or a strip (rectangular substrate) sealed with molded resin, the individual workpieces are semiconductor packages.

[0024] The "front surface" of a workpiece refers to the surface on which circuits, electrodes, etc. are formed, and the "back surface" of a workpiece refers to the surface on which no circuits, etc. are formed. The electrodes may be convex electrodes such as bumps.

[0025] DBG (Dicing Before Grinding) is a method in which grooves of a specified depth are formed on the front side of a workpiece (e.g., a wafer), and then the workpiece is ground from the back side to separate the workpiece by grinding. The grooves formed on the front side of the workpiece are formed by methods such as blade dicing, laser dicing, and plasma dicing.

[0026] In addition, LDBG (Laser Dicing Before Grinding) is a modified version of DBG, in which a modified region is created inside a workpiece (e.g., a wafer) using a laser, and the workpiece is divided into individual pieces by stress, etc., generated when grinding the back surface of the workpiece.

[0027] The term "group of individualized workpieces" refers to a plurality of individualized workpieces held on the protective sheet for workpiece processing according to the present invention after the workpiece is singulated. These individualized workpieces, as a whole, form a shape similar to that of the workpiece. The term "group of chips" is an example of a "group of individualized workpieces" and refers to a plurality of chips held on the protective sheet for workpiece processing according to the present embodiment after the wafer is singulated. These chips, as a whole, form a shape similar to that of the wafer. For example, the group of semiconductor chips refers to a plurality of semiconductor chips held on the protective sheet for semiconductor processing after the semiconductor wafer is singulated, and these semiconductor chips, as a whole, form a shape similar to that of the semiconductor wafer.

[0028] "(Meth)acrylate" is used as the term to refer to both "acrylate" and "methacrylate," and similar terms.

[0029] The "energy rays" refer to ultraviolet rays, electron beams, etc., and are preferably ultraviolet rays.

[0030] Unless otherwise specified, the "weight average molecular weight" is a polystyrene equivalent value measured by gel permeation chromatography (GPC). Measurements by such a method are performed, for example, using a high-speed GPC device "HLC-8120GPC" manufactured by Tosoh Corporation with a high-speed column "TSK guard column HXL -H", "TSK Gel GMH XL ", "TSK Gel G2000 H XL (All of the above are manufactured by Tosoh Corporation) connected in the above order, the column temperature was 40° C., the liquid flow rate was 1.0 mL / min, and the detector was a differential refractometer.

[0031] The release sheet is a sheet that supports the pressure-sensitive adhesive layer in a releasable manner. The term "sheet" is not limited to a specific thickness, and is used to include a film.

[0032] The mass ratios in the explanations of compositions such as the pressure-sensitive adhesive layer composition are based on the active ingredient (solid content), and do not include the solvent unless otherwise specified.

[0033] Next, the configuration of each member of the protective sheet for workpiece processing according to the present invention will be described in more detail. Note that the protective sheet for workpiece processing according to the present invention may be simply referred to as a "protective sheet".

[0034] (1. Protective sheet for workpiece processing) The workpiece processing protective sheet 1 according to this embodiment has a substrate 10, a buffer layer 20 provided on at least one surface of the substrate 10, and an adhesive layer 30 provided on the other surface of the substrate 10. A specific example thereof, as shown in FIG. 1, has a substrate 10, a buffer layer 20 formed on one surface of the substrate, and an adhesive layer 30 formed on the other surface of the substrate. Alternatively, the protective sheet 1 may have a structure having a substrate 10, a buffer layer 20 formed on both surfaces of the substrate, and an adhesive layer 30 formed on the surface of one of the buffer layers 20. The protective sheet 1 for workpiece processing may have other layers as long as the effects of the present invention can be obtained. That is, as long as the protective sheet for workpiece processing has a substrate, a buffer layer, and an adhesive layer, for example, another layer may be formed between the substrate and the buffer layer, or another layer may be formed between the substrate and the adhesive layer.

[0035] As shown in Figure 2, an adhesive layer 30 is attached to the circuit surface of a workpiece (e.g., a semiconductor wafer) 100 as an adherend, i.e., the surface 100a of the workpiece (e.g., a semiconductor wafer) 100, so that the protective sheet for workpiece processing (specifically, the protective sheet for semiconductor processing) 1 of this embodiment protects the surface 100a of the semiconductor wafer 100 when the back surface 100b of the semiconductor wafer 100 is ground.

[0036] The components of the protection sheet for workpiece processing will be described in detail below.

[0037] (2. Base material) The substrate 10 is not limited as long as it is made of a material capable of supporting a workpiece such as a wafer before back grinding and holding the workpiece or a group of individual pieces of the workpiece after back grinding. For example, various resin films used as substrates for back grinding sheets are exemplified as the substrate. The substrate may be made of a single layer film made of one resin film, or may be made of a multi-layer film in which multiple resin films are laminated.

[0038] (2.1 Physical properties of the substrate) In this embodiment, the substrate preferably has high rigidity. The high rigidity of the substrate can suppress vibration during back grinding, and as a result, the support and holding performance of the wafer etc. is improved, and damage and cracks of the wafer etc. are further reduced. In addition, it is possible to reduce the stress when peeling the workpiece processing protective sheet from the wafer etc., and damage and cracks of the wafer etc. caused during peeling are further reduced. Furthermore, the workability when attaching the workpiece processing protective sheet to the wafer etc. is also improved. Specifically, the Young's modulus of the substrate at 23°C is preferably 1000 MPa or more, more preferably 2000 MPa or more. The upper limit of the Young's modulus is not particularly limited, but from the viewpoint of ease of handling, it is preferably 10000 MPa or less, more preferably 6000 MPa or less, and particularly preferably 5000 MPa or less.

[0039] In this embodiment, the thickness of the substrate is preferably 20 μm to 800 μm, more preferably 30 μm to 100 μm, and particularly preferably 40 μm to 80 μm. When the thickness of the substrate is within the above range, the wafer or the like can be securely held during back grinding, and the occurrence of cracks can be further suppressed.

[0040] (2.2 Substrate material) The material of the substrate may be selected so that the Young's modulus of the substrate falls within the above range. In this embodiment, examples of the substrate include polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polyester such as fully aromatic polyester, polyimide, polyamide, polycarbonate, polyacetal, modified polyphenylene oxide, polyphenylene sulfide, polysulfone, polyether ketone, biaxially oriented polypropylene, etc. Among these, it is preferable to use one or more selected from polyester, polyamide, polyimide, and biaxially oriented polypropylene, more preferably polyester, and even more preferably polyethylene terephthalate.

[0041] Furthermore, the substrate may contain a plasticizer, a lubricant, an infrared absorbing agent, an ultraviolet absorbing agent, a filler, a colorant, an antistatic agent, an antioxidant, a catalyst, etc., within the scope of not impairing the effects of the present invention. Furthermore, the substrate may be transparent or opaque, and may be colored or vapor-deposited as desired.

[0042] At least one of the main surfaces of the substrate may be subjected to an adhesion treatment such as a corona treatment in order to improve adhesion with other layers. At least one of the main surfaces of the substrate may have a thin primer layer in order to improve adhesion with a buffer layer formed on the main surface.

[0043] The primer layer-forming composition for forming the primer layer is not particularly limited, and examples thereof include compositions containing polyester resins, urethane resins, polyester urethane resins, acrylic resins, etc. The primer layer-forming composition may contain a crosslinking agent, a photopolymerization initiator, an antioxidant, a softener (plasticizer), a filler, a rust inhibitor, a pigment, a dye, etc., as necessary.

[0044] The thickness of the primer layer is preferably 0.01 to 10 μm, more preferably 0.03 to 5 μm. Since the material of the primer layer is soft, the influence on the rigidity of the substrate is small, and for example, the tensile load of the substrate and the tensile load of the substrate with the primer layer are substantially the same.

[0045] For example, the Young's modulus of the substrate can be controlled by selecting the resin composition, adding a plasticizer, or adjusting the stretching conditions during production of the resin film.

[0046] (3. Adhesive Layer) The adhesive layer 30 is attached to the circuit surface of the workpiece, and protects the circuit surface and supports the workpiece or the individual pieces of the workpiece until it is peeled off from the circuit surface. The adhesive layer may be composed of one layer (single layer), or may be composed of two or more layers. By making the adhesive layer a single layer, costs can be reduced, and delamination within the adhesive layer can be prevented when the protective sheet for workpiece processing is peeled off. When the adhesive layer has multiple layers, these multiple layers may be the same or different from each other, and the combination of layers constituting these multiple layers is not particularly limited.

[0047] The thickness of the adhesive layer is not particularly limited, but is preferably 3 μm to 200 μm, more preferably 5 μm to 100 μm, even more preferably 10 μm to 70 μm, and particularly preferably 15 μm to 45 μm. By keeping the thickness of the adhesive layer within the above range, cracking of the workpiece and movement of the individual pieces of the workpiece can be suppressed.

[0048] The thickness of the adhesive layer means the thickness of the entire adhesive layer. For example, the thickness of an adhesive layer composed of multiple layers means the total thickness of all layers constituting the adhesive layer.

[0049] (3.1 Composition of Adhesive Layer) The composition of the adhesive layer is not particularly limited as long as the adhesive layer has enough adhesiveness to protect the circuit surface of the work. In this embodiment, the adhesive layer is preferably composed of an acrylic adhesive layer composition, a urethane adhesive layer composition, a rubber adhesive layer composition, a silicone adhesive layer composition, or the like, and contains a polymer (adhesive polymer) capable of exhibiting adhesiveness. From the viewpoint of efficiently controlling the adhesiveness to the work, the adhesive layer is more preferably composed of an acrylic adhesive layer composition. The acrylic adhesive layer composition contains an acrylic polymer as an adhesive polymer.

[0050] The pressure-sensitive adhesive layer is preferably composed of an energy ray-curable composition for a pressure-sensitive adhesive layer, which allows the pressure-sensitive adhesive layer to protect the circuit surface with sufficient adhesive strength before curing by energy ray irradiation and to be easily peeled off after curing.

[0051] (3.2 Composition for adhesive layer) In the following, the adhesive layer composition constituting the adhesive layer will be described in detail using an example in which the adhesive layer is energy ray curable, but these are non-limiting examples, and the adhesive layer may be composed of a non-energy ray curable acrylic adhesive layer composition, a urethane adhesive layer composition, a rubber adhesive layer composition, a silicone adhesive layer composition, etc.

[0052] The energy ray curable composition for the adhesive layer may contain an adhesive polymer and an energy ray curable compound separately from the adhesive polymer, or the adhesive polymer itself may have energy ray curability. When the adhesive polymer itself has energy ray curability, an energy ray curable group is introduced into the adhesive polymer, and the energy ray curable group is preferably introduced into the main chain or side chain of the adhesive polymer.

[0053] In addition, when an energy ray curable compound is blended separately from the adhesive polymer, a monomer or oligomer having an energy ray curable group is used as the energy ray curable compound.Specific examples of the energy ray curable compound include polyvalent (meth)acrylate monomers such as trimethylolpropane tri(meth)acrylate, pentaerythritol (meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, and 1,6-hexanediol (meth)acrylate, and oligomers such as urethane (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, and epoxy (meth)acrylate.The oligomer is an oligomer having a weight average molecular weight (Mw) of less than 10,000, and among these, urethane (meth)acrylate oligomers are preferred.

[0054] In this embodiment, the content of the energy ray-curable compound in the composition for the adhesive layer is preferably 0.1 to 300 parts by mass, more preferably 1 to 100 parts by mass, and even more preferably 5 to 50 parts by mass, relative to 100 parts by mass of the adhesive polymer, from the viewpoint of controlling the amount of energy ray-curable carbon-carbon double bonds.

[0055] Hereinafter, the case where the energy ray-curable adhesive polymer contained in the composition for adhesive layer is an energy ray-curable acrylic polymer (hereinafter also referred to as "acrylic polymer (A)") will be described in more detail.

[0056] (3.2.1 Acrylic polymer (A)) The acrylic polymer (A) is an acrylic polymer having an energy ray curable group introduced therein and a structural unit derived from a (meth)acrylate. The energy ray curable group is preferably introduced into a side chain of the acrylic polymer.

[0057] The acrylic polymer (A) is preferably a reaction product obtained by reacting an acrylic copolymer (A0) having a structural unit derived from an alkyl (meth)acrylate (a1) and a structural unit derived from a functional group-containing monomer (a2) with an energy ray-curable substance (Xa) having an energy ray-curable group.

[0058] As the alkyl(meth)acrylate (a1), an alkyl(meth)acrylate having an alkyl group with a carbon number of 1 to 18 is used. Specific examples include methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, n-butyl(meth)acrylate, n-pentyl(meth)acrylate, n-hexyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, and the like.

[0059] From the viewpoint of improving the adhesive strength of the pressure-sensitive adhesive layer to be formed, the content of the structural units derived from the alkyl (meth)acrylate (a1) in the acrylic copolymer (A0) is preferably 40 to 98 mass%, more preferably 45 to 95 mass%, and even more preferably 50 to 90 mass%, relative to all structural units (100 mass%) of the acrylic copolymer (A0).

[0060] The functional group-containing monomer (a2) is a monomer having a functional group such as a hydroxy group, a carboxy group, an epoxy group, an amino group, a cyano group, a nitrogen atom-containing cyclic group, an alkoxysilyl group, etc. Among the above, the functional group-containing monomer (a2) is preferably at least one selected from the group consisting of a hydroxy group-containing monomer, a carboxy group-containing monomer, and an epoxy group-containing monomer, and from the viewpoint of facilitating the reaction of the acrylic copolymer (A0) with the energy ray-curable substance (Xa), a hydroxy group-containing monomer is more preferred.

[0061] Examples of hydroxy group-containing monomers include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and unsaturated alcohols such as vinyl alcohol and allyl alcohol.

[0062] The functional group-containing monomer (a2) may be used alone or in combination of two or more kinds.

[0063] The content of the structural units derived from the functional group-containing monomer (a2) in the acrylic copolymer (A0) is preferably 1 to 35 mass%, more preferably 3 to 32 mass%, and even more preferably 6 to 30 mass%, based on the total structural units (100 mass%) of the acrylic copolymer (A0).

[0064] If the content is 1% by mass or more, a certain amount of functional groups that become reaction sites with the energy ray curable material (Xa) can be secured. Therefore, the pressure-sensitive adhesive layer can be appropriately cured by irradiation with energy rays, so that the adhesive strength after irradiation with energy rays can be reduced. In addition, if the content is 30% by mass or less, a sufficient pot life of the coating agent can be secured when the coating agent of the pressure-sensitive adhesive layer composition is applied to form the pressure-sensitive adhesive layer.

[0065] The acrylic copolymer (A0) may be a copolymer of an alkyl (meth)acrylate (a1) and a functional group-containing monomer (a2), or may be a copolymer of the (a1) component, the (a2) component, and a monomer (a3) ​​other than the (a1) and (a2) components.

[0066] Examples of the other monomers (a3) ​​include (meth)acrylates having a cyclic structure such as cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate, as well as vinyl acetate and styrene. The other monomers (a3) ​​may be used alone or in combination of two or more.

[0067] The energy ray-curable substance (Xa) is a compound having an energy ray-curable group and a substituent (hereinafter also simply referred to as a "reactive substituent") capable of reacting with a functional group in the structural unit derived from the component (a2) of the acrylic copolymer (A0).

[0068] The energy ray-curable group may be any group containing an energy ray-curable carbon-carbon double bond, and examples thereof include a (meth)acryloyl group and a vinyl group, with a (meth)acryloyl group being preferred.

[0069] The reactive substituent in the energy ray curable substance (Xa) may be appropriately changed depending on the functional group possessed by the functional group-containing monomer (a2), and may be, for example, an isocyanate group, a carboxyl group, an epoxy group, etc., with the isocyanate group being preferred from the viewpoint of reactivity, etc. When the energy ray curable substance (Xa) has an isocyanate group, for example, when the functional group of the functional group-containing monomer (a2) is a hydroxyl group, it becomes possible for the substance to easily react with the acrylic copolymer (A0).

[0070] Specific examples of the energy ray curable substance (Xa) include (meth)acryloyloxyethyl isocyanate, meta-isopropenyl-α,α-dimethylbenzyl isocyanate, (meth)acryloyl isocyanate, allyl isocyanate, glycidyl (meth)acrylate, (meth)acrylic acid, etc. These energy ray curable substances (Xa) may be used alone or in combination of two or more kinds.

[0071] From the viewpoint of controlling the amount of energy ray-curable carbon-carbon double bonds, the energy ray-curable substance (Xa) is reacted with the functional groups in an amount of preferably 50 to 98 equivalents, more preferably 55 to 93 equivalents, of the total amount (100 equivalents) of functional groups derived from the functional group-containing monomer (a2) in the acrylic copolymer (A0).

[0072] The weight average molecular weight (Mw) of the acrylic polymer (A) is preferably from 300,000 to 1,600,000, and more preferably from 400,000 to 1,400,000. By having such an Mw, it is possible to impart appropriate adhesiveness to the pressure-sensitive adhesive layer.

[0073] Even when the adhesive polymer has energy ray curability, it is preferable that the composition for adhesive layer contains the above-mentioned energy ray curable compound other than the adhesive polymer.

[0074] 3.2.2 Crosslinking Agents The adhesive layer composition preferably further contains a crosslinking agent. The adhesive layer composition crosslinks, for example, by a reaction between an adhesive polymer having a functional group such as a hydroxyl group and a functional group in the crosslinking agent. The adhesive layer is more likely to function as an adhesive layer by crosslinking the adhesive polymer with the crosslinking agent.

[0075] Examples of the crosslinking agent include an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, an aziridine-based crosslinking agent, and a chelate-based crosslinking agent, and among these, an isocyanate-based crosslinking agent is preferred. The crosslinking agents may be used alone or in combination of two or more kinds.

[0076] Examples of the isocyanate crosslinking agent include tolylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, and adducts of these diisocyanates with polyhydric alcohols (eg, trimethylolpropane, etc.).

[0077] The content of the crosslinking agent is preferably 0.01 to 10 parts by mass, and more preferably 0.03 to 7 parts by mass, based on 100 parts by mass of the adhesive polymer.

[0078] (3.2.3 Photoinitiators) The pressure-sensitive adhesive layer composition preferably further contains a photopolymerization initiator. When the pressure-sensitive adhesive layer composition contains a photopolymerization initiator, energy ray curing of the pressure-sensitive adhesive layer composition by ultraviolet light or the like is facilitated.

[0079] Examples of the photopolymerization initiator include acetophenone, 2,2-diethoxybenzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, Michler's ketone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzyl diphenylsulfide, tetramethylthiuram monosulfide, benzyl dimethyl ketal, dibenzyl, diacetyl, 1-chloroanthraquinone, 2-chloroanthraquinone, 2-ethylanthraquinone, 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxycyclohexylphenyl ketone, and the like. Examples of the photopolymerization initiator include low molecular weight polymerization initiators such as 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropanone-1,2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,2-hydroxy-2-methyl-1-phenyl-propan-1-one, diethylthioxanthone, isopropylthioxanthone, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and 2,4,6-trimethylbenzoyldiphenyl-phosphine oxide, and oligomerized polymerization initiators such as oligo{2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone}. The photopolymerization initiator may be used alone or in combination of two or more kinds.

[0080] The content of the photopolymerization initiator is preferably 0.01 to 10 parts by mass, more preferably 0.03 to 7 parts by mass, and further preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the adhesive polymer.

[0081] The adhesive layer composition may contain other additives within the range that does not impair the effects of the present invention. Examples of other additives include tackifiers, antioxidants, softeners (plasticizers), fillers, rust inhibitors, pigments, dyes, etc. When these additives are contained, the content of each additive is preferably 0.01 to 6 parts by mass, more preferably 0.02 to 2 parts by mass, based on 100 parts by mass of the adhesive polymer.

[0082] The adhesive strength of the adhesive layer can be adjusted, for example, by the type and amount of monomers constituting the adhesive polymer (e.g., acrylic polymer (A)), the amount of energy ray curable groups introduced into the adhesive polymer, etc. For example, increasing the amount of energy ray curable groups tends to decrease the adhesive strength after curing. However, the adhesive strength of the adhesive layer can also be adjusted by factors other than the above factors. For example, it can be appropriately adjusted by the amount of crosslinking agent and the amount of photopolymerization initiator blended in the adhesive layer composition, etc.

[0083] (4.Buffer layer) As shown in FIG. 1, the buffer layer 20 is formed on the main surface of the substrate opposite to the main surface on which the adhesive layer is formed. Alternatively, the buffer layer 20 may be formed on both sides of the substrate 10, and an adhesive layer may be formed on the surface of one of the buffer layers. The buffer layer 20 is a soft layer compared to the substrate, and relieves vibration and stress during back grinding of a work such as a wafer, thereby preventing cracks and chips from occurring in the work. In addition, the work to which the protective sheet for work processing is attached is placed on the suction table via the protective sheet for work processing during back grinding, and the buffer layer as a constituent layer of the protective sheet for work processing makes it easier for the work to be properly held on the suction table. In addition, even if there is a foreign object on the suction table, the unevenness of the foreign object can be absorbed by the deformation of the buffer layer, and the work can be ground to a smooth and uniform thickness.

[0084] The thickness of the buffer layer is preferably 15 to 80 μm, and more preferably 20 to 70 μm. By setting the thickness of the buffer layer within the above range, the buffer layer can appropriately relieve stress during back grinding.

[0085] The buffer layer may be a layer formed from a composition for a buffer layer containing an energy ray-curable compound, or may be a polyolefin-based resin film.

[0086] <Polyolefin resin film> Polyolefin resin film with a density of 900 kg / m 3 It is preferable that the material is made of a polyolefin resin having a density of 930 kg / m or more. 3 More preferably, the material is made of a polyolefin resin having a density of 950 kg / m or more. 3 It is particularly preferable that the film is made of the above polyolefin resin. Examples of the film made of such a polyolefin resin include LDPE film, LLDPE film, HDPE film, etc., and among them, a film having a density of 920 to 942 kg / m 3 LDPE film, density 942~980kg / m 3 In particular, when the buffer layer is made of a polyolefin-based resin film, it is preferable that the buffer layer 20 is formed on both sides of the substrate 10 and a pressure-sensitive adhesive layer is formed on the surface of one of the buffer layers.

[0087] The buffer layer may be entirely made of the polyethylene (PE) film, or may be a laminated film.

[0088] <Layer formed from a buffer layer-forming composition containing an energy ray-polymerizable compound> The buffer layer-forming composition containing the energy ray-polymerizable compound can be cured by being irradiated with energy rays.

[0089] More specifically, the buffer layer forming composition containing the energy ray polymerizable compound preferably contains urethane (meth)acrylate (a1). The buffer layer forming composition more preferably contains, in addition to the above (a1), a polymerizable compound (a2) having an alicyclic group or heterocyclic group having 6 to 20 ring atoms and / or a polymerizable compound (a3) ​​having a functional group. The buffer layer forming composition preferably contains, in addition to the above components (a1) to (a3), a multifunctional polymerizable compound (a4). Furthermore, the buffer layer forming composition preferably contains a photopolymerization initiator, and may contain other additives and resin components within the range that does not impair the effects of the present invention.

[0090] Hereinafter, each component contained in the buffer layer forming composition containing the energy ray-polymerizable compound will be described in detail.

[0091] (Urethane (meth)acrylate (a1)) The urethane (meth)acrylate (a1) is a compound having at least a (meth)acryloyl group and a urethane bond, and has the property of being polymerized and cured by irradiation with energy rays. The urethane (meth)acrylate (a1) is an oligomer or polymer.

[0092] The weight average molecular weight (Mw) of component (a1) is preferably 1,000 to 100,000, more preferably 2,000 to 60,000, and even more preferably 10,000 to 30,000. The number of (meth)acryloyl groups (hereinafter also referred to as "functionality") in component (a1) may be monofunctional, bifunctional, or trifunctional or higher, but is preferably monofunctional or bifunctional.

[0093] Component (a1) can be obtained, for example, by reacting a polyol compound with a polyisocyanate compound to obtain a terminal isocyanate urethane prepolymer, and then reacting the resulting prepolymer with a (meth)acrylate having a hydroxyl group. Component (a1) may be used alone or in combination of two or more kinds.

[0094] The polyol compound that is the raw material of component (a1) is not particularly limited as long as it is a compound having two or more hydroxyl groups. Specific examples of polyol compounds include alkylene diols, polyether polyols, polyester polyols, polycarbonate polyols, etc. Among these, polyester polyols or polycarbonate polyols are preferred.

[0095] The polyol compound may be any of a difunctional diol, a trifunctional triol, and a polyol having 4 or more functional groups. A difunctional diol is preferable, and a polyester type diol or a polycarbonate type diol is more preferable.

[0096] Examples of the polyisocyanate compound include aliphatic polyisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, and trimethylhexamethylene diisocyanate; alicyclic diisocyanates such as isophorone diisocyanate, norbornane diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, dicyclohexylmethane-2,4'-diisocyanate, and ω,ω'-diisocyanate dimethylcyclohexane; and aromatic diisocyanates such as 4,4'-diphenylmethane diisocyanate, tolylene diisocyanate, xylylene diisocyanate, tolidine diisocyanate, tetramethylene xylylene diisocyanate, and naphthalene-1,5-diisocyanate. Among these, isophorone diisocyanate, hexamethylene diisocyanate, and xylylene diisocyanate are preferred.

[0097] The above-mentioned polyol compound is reacted with a polyisocyanate compound to give a terminal isocyanate urethane prepolymer, and then a hydroxyl group-containing (meth)acrylate is reacted with the urethane (meth)acrylate (a1). The hydroxyl group-containing (meth)acrylate is not particularly limited as long as it is a compound having a hydroxyl group and a (meth)acryloyl group in at least one molecule.

[0098] Specific examples of (meth)acrylates having a hydroxy group include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 4-hydroxycyclohexyl (meth)acrylate, 5-hydroxycyclooctyl (meth)acrylate, 2-hydroxy-3-phenyloxypropyl (meth)acrylate, pentaerythritol tri(meth)acrylate, polyethylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate; hydroxy group-containing (meth)acrylamides such as N-methylol (meth)acrylamide; and reaction products obtained by reacting a diglycidyl ester of vinyl alcohol, vinylphenol, or bisphenol A with (meth)acrylic acid; and the like. Among these, hydroxyalkyl (meth)acrylate is preferred, and 2-hydroxyethyl (meth)acrylate is more preferred.

[0099] The conditions for reacting the isocyanate-terminated urethane prepolymer and the (meth)acrylate having a hydroxyl group are preferably such that the reaction is carried out at 60 to 100° C. for 1 to 4 hours in the presence of a solvent and a catalyst, which are added as necessary.

[0100] The content of component (a1) in the buffer layer forming composition is preferably 10 to 70 parts by mass, and more preferably 20 to 60 parts by mass, based on the total amount (100 parts by mass) of the buffer layer forming composition.

[0101] (Polymerizable Compound (a2) Having an Alicyclic Group or a Heterocyclic Group with 6 to 20 Ring Atoms) Component (a2) is a polymerizable compound having an alicyclic group or a heterocyclic group with 6 to 20 ring atoms, and is preferably a compound having at least one (meth)acryloyl group, more preferably a compound having one (meth)acryloyl group. By using component (a2), the film formability of the obtained buffer layer forming composition can be improved.

[0102] Although the definition of component (a2) overlaps with the definition of component (a3) ​​described later, the overlapping portion is included in component (a3). For example, a compound having at least one (meth)acryloyl group, an alicyclic group or heterocyclic group having 6 to 20 ring atoms, and a functional group such as a hydroxyl group, an epoxy group, an amide group, or an amino group is included in the definitions of both component (a2) and component (a3), but in the present invention, the compound is included in component (a3).

[0103] The number of ring-forming atoms in the alicyclic group or heterocyclic group contained in component (a2) is preferably 6 to 20, more preferably 6 to 18, further preferably 6 to 16, and particularly preferably 7 to 12. Examples of atoms forming the ring structure of the heterocyclic group include carbon atoms, nitrogen atoms, oxygen atoms, and sulfur atoms.

[0104] The number of ring atoms refers to the number of atoms constituting the ring itself of a compound having a structure in which atoms are bonded in a ring, and does not include atoms that do not constitute the ring (for example, hydrogen atoms bonded to atoms constituting the ring) or atoms contained in the substituent when the ring is substituted with a substituent.

[0105] Specific examples of the component (a2) include alicyclic group-containing (meth)acrylates such as isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxy (meth)acrylate, cyclohexyl (meth)acrylate, and adamantane (meth)acrylate; and heterocyclic group-containing (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate, morpholine (meth)acrylate, and cyclic trimethylolpropane formal acrylate.

[0106] The component (a2) may be used alone or in combination of two or more kinds. Of the alicyclic group-containing (meth)acrylates, isobornyl (meth)acrylate is preferred.

[0107] The content of component (a2) in the buffer layer forming composition is preferably 0 to 80 parts by mass, and more preferably 0 to 70 parts by mass, based on the total amount (100 parts by mass) of the buffer layer forming composition.

[0108] (Polymerizable compound having a functional group (a3)) Component (a3) ​​is a polymerizable compound containing a functional group such as a hydroxyl group, an epoxy group, an amide group, or an amino group, and is preferably a compound having at least one (meth)acryloyl group, more preferably a compound having one (meth)acryloyl group.

[0109] The component (a3) ​​has good compatibility with the component (a1), and the viscosity of the buffer layer-forming composition can be easily adjusted to an appropriate range. In addition, the buffer layer has good buffer performance even if it is relatively thin.

[0110] Examples of the component (a3) ​​include hydroxyl group-containing (meth)acrylates, epoxy group-containing compounds, amide group-containing compounds, and amino group-containing (meth)acrylates.

[0111] Examples of hydroxyl group-containing (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, phenylhydroxypropyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl acrylate.

[0112] Examples of epoxy group-containing compounds include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, and allyl glycidyl ether. Of these, epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate and methyl glycidyl (meth)acrylate are preferred.

[0113] Examples of amide group-containing compounds include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylolpropane(meth)acrylamide, N-methoxymethyl(meth)acrylamide, and N-butoxymethyl(meth)acrylamide.

[0114] Examples of the amino group-containing (meth)acrylate include primary amino group-containing (meth)acrylate, secondary amino group-containing (meth)acrylate, and tertiary amino group-containing (meth)acrylate.

[0115] Among these, hydroxyl group-containing (meth)acrylates are preferred, and hydroxyl group-containing (meth)acrylates having an aromatic ring, such as phenylhydroxypropyl (meth)acrylate, are more preferred. The component (a3) ​​may be used alone or in combination of two or more kinds.

[0116] The content of component (a3) ​​in the buffer layer forming composition is preferably 0 to 40 parts by mass, more preferably 0 to 35 parts by mass, and even more preferably 0 to 30 parts by mass, relative to the total amount (100 parts by mass) of the buffer layer forming composition.

[0117] (Polyfunctional polymerizable compound (a4)) The polyfunctional polymerizable compound refers to a compound having two or more photopolymerizable unsaturated groups. The photopolymerizable unsaturated group is a functional group containing a carbon-carbon double bond, such as a (meth)acryloyl group, a vinyl group, an allyl group, and a vinylbenzyl group. Two or more types of photopolymerizable unsaturated groups may be combined. A three-dimensional network structure (crosslinked structure) is formed by reacting a photopolymerizable unsaturated group in the polyfunctional polymerizable compound with a (meth)acryloyl group in component (a1) or by reacting photopolymerizable unsaturated groups in component (a4) with each other. When a polyfunctional polymerizable compound is used, the number of crosslinked structures formed by energy ray irradiation is more likely to increase compared to when a compound containing only one photopolymerizable unsaturated group is used.

[0118] The definition of component (a4) overlaps with the definitions of components (a2) and (a3) ​​described above, but the overlapping parts are included in component (a4). For example, a compound having an alicyclic group or heterocyclic group with 6 to 20 ring atoms and having two or more (meth)acryloyl groups is included in the definitions of both components (a4) and (a2), but in the present invention, the compound is included in component (a4). In addition, a compound containing a functional group such as a hydroxyl group, an epoxy group, an amide group, or an amino group and having two or more (meth)acryloyl groups is included in the definitions of both components (a4) and (a3), but in the present invention, the compound is included in component (a4).

[0119] From the above viewpoints, the number of photopolymerizable unsaturated groups (number of functional groups) in the polyfunctional polymerizable compound is preferably 2 to 10, and more preferably 3 to 6.

[0120] The weight average molecular weight of the component (a4) is preferably 30-40,000, more preferably 100-10,000, and even more preferably 200-1,000.

[0121] Specific examples of the component (a4) include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate having 200 to 800 repeating units derived from glycol, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, divinylbenzene, vinyl (meth)acrylate, divinyl adipate, and N,N'-methylenebis(meth)acrylamide. Polyethylene glycol di(meth)acrylate generally has the number of glycol units expressed in parentheses; for example, if the number of glycol units is 600, it is expressed as polyethylene glycol (600) diacrylate. The component (a4) may be used alone or in combination of two or more kinds. Among these, polyethylene glycol diacrylate and neopentyl glycol di(meth)acrylate are preferable.

[0122] The content of component (a4) in the buffer layer forming composition is preferably 2 to 40 parts by mass, more preferably 3 to 20 parts by mass, and even more preferably 5 to 15 parts by mass, relative to the total amount (100 parts by mass) of the buffer layer forming composition.

[0123] (Polymerizable compound (a5) other than components (a1) to (a4)) The buffer layer-forming composition may contain a polymerizable compound (a5) other than the above components (a1) to (a4) within the range that does not impair the effects of the present invention.

[0124] Examples of the component (a5) include alkyl (meth)acrylates having an alkyl group having 1 to 20 carbon atoms, vinyl compounds such as styrene, hydroxyethyl vinyl ether, hydroxybutyl vinyl ether, N-vinyl formamide, N-vinyl pyrrolidone, and N-vinyl caprolactam, etc. The component (a5) may be used alone or in combination of two or more kinds.

[0125] The content of component (a5) in the buffer layer-forming composition is preferably 0 to 20 parts by mass, more preferably 0 to 10 parts by mass, even more preferably 0 to 5 parts by mass, and particularly preferably 0 to 2 parts by mass, relative to the total amount (100 parts by mass) of the buffer layer-forming composition.

[0126] (Photopolymerization initiator) It is preferable that the buffer layer-forming composition further contains a photopolymerization initiator from the viewpoints of shortening the polymerization time by light irradiation and reducing the amount of light irradiation when forming the buffer layer.

[0127] Examples of the photopolymerization initiator include benzoin compounds, acetophenone compounds, acylphosphinoxide compounds, titanocene compounds, thioxanthone compounds, peroxide compounds, and further photosensitizers such as amines and quinones. More specific examples include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzyl phenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyronitrile, dibenzyl, diacetyl, 8-chloroanthraquinone, and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.

[0128] These photopolymerization initiators can be used alone or in combination of two or more kinds.

[0129] The content of the photopolymerization initiator in the composition for forming the buffer layer is preferably 0.05 to 15 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.3 to 5 parts by mass, relative to 100 parts by mass of the total amount of the energy ray-polymerizable compounds.

[0130] (Other additives) The buffer layer forming composition may contain other additives within the range that does not impair the effects of the present invention. Examples of other additives include antistatic agents, antioxidants, softeners (plasticizers), fillers, rust inhibitors, pigments, dyes, etc. When these additives are blended, the content of each additive in the buffer layer forming composition is preferably 0.01 to 6 parts by mass, more preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the total amount of the energy ray polymerizable compounds.

[0131] (Resin component) The buffer layer-forming composition may contain a resin component within the range that does not impair the effects of the present invention. Examples of the resin component include polyene-thiol-based resins, polyolefin-based resins such as polybutene, polybutadiene, and polymethylpentene, and thermoplastic resins such as styrene-based copolymers.

[0132] The content of these resin components in the composition for forming a buffer layer is preferably 0 to 20 parts by mass, more preferably 0 to 10 parts by mass, even more preferably 0 to 5 parts by mass, and particularly preferably 0 to 2 parts by mass, relative to the total amount (100 parts by mass) of the composition for forming a buffer layer.

[0133] The buffer layer formed from the buffer layer-forming composition containing the energy ray-polymerizable compound is obtained by polymerizing and curing the buffer layer-forming composition having the above-mentioned composition by energy ray irradiation. In other words, the buffer layer is a cured product of the buffer layer-forming composition.

[0134] Therefore, the buffer layer contains polymerization units derived from component (a1). The buffer layer may also contain polymerization units derived from component (a2), polymerization units derived from component (a3), polymerization units derived from component (a4), and / or polymerization units derived from component (a5). The content ratio of each polymerization unit in the buffer layer usually corresponds to the ratio (feed ratio) of each component constituting the buffer layer forming composition. For example, when the content of component (a1) in the buffer layer forming composition is 10 to 70 parts by mass with respect to the total amount (100 parts by mass) of the buffer layer forming composition, the buffer layer contains 10 to 70 parts by mass of polymerization units derived from component (a1). When the content of component (a2) in the buffer layer forming composition is 10 to 80 parts by mass with respect to the total amount (100 parts by mass) of the buffer layer forming composition, the buffer layer contains 10 to 80 parts by mass of polymerization units derived from component (a2). The same applies to components (a3) ​​to (a5).

[0135] (5. Thermal deformation of protective sheets for workpiece processing) As shown in Fig. 1, the protective sheet for workpiece processing 1 has a substrate 10, a buffer layer 20, and an adhesive layer 30. The greatest feature of the present invention is that the thermal deformation property of the protective sheet for workpiece processing is controlled within a specific range.

[0136] In other words, when a thermomechanical analysis of the protective sheet for workpiece processing 1 was performed under conditions involving two temperature changes, the deformation rate Df1 during the first heating was within 0.67%, and the absolute value of the difference between the deformation rate Df1 during the first heating and the deformation rate Df2 during the second heating was within 0.067%.

[0137] The thermomechanical analysis was carried out using a sample of 20 mm in length and 4.5 mm in width cut out from the workpiece processing protection sheet, with the sample having the same thickness as the workpiece processing protection sheet.

[0138] The above sample is held with a chuck distance of 15 mm, a load of 10 g is applied, and the temperature is raised and lowered twice, and the deformation rate of the sample is determined from the change in the chuck distance during this process. In the first heating run, the temperature is raised from 23°C to 50°C at a rate of 3°C / min, and then allowed to cool to 23°C. In the second heating run, a load of 10 g is again applied, and the temperature is raised to 50°C at a rate of 3°C / min.

[0139] The deformation rate Df1 (%) when the temperature reaches 50°C for the first time, and the deformation rate Df2 (%) when the temperature reaches 50°C for the second time are measured. Df1 and Df2 are calculated using the following formulas. Df1 = 100 × (S1-S0) / S0 Df2 = 100 × (S2-S0) / S0

[0140] Here, S0 is the chuck interval before the test, S1 is the chuck interval when the temperature reached 50°C for the first time, and S2 is the chuck interval when the temperature reached 50°C for the second time.

[0141] As described above, the deformation ratio Df1 during the first heating is within 0.67%, preferably within 0.33%, more preferably within 0.17%, and particularly preferably within 0.13%.

[0142] Furthermore, as described above, the absolute value of the difference between the deformation rate Df1 during the first heating and the deformation rate Df2 during the second heating is within 0.067%, preferably within 0.033%, more preferably within 0.020%, and particularly preferably within 0.0067%.

[0143] Furthermore, the deformation ratio Df2 during the second heating is preferably within 0.67%, more preferably within 0.33%, even more preferably within 0.17%, and particularly preferably within 0.13%.

[0144] The thermal deformation property of the protection sheet for workpiece processing can be controlled by appropriately setting the Young's modulus of the substrate and the structure of the buffer layer.

[0145] For example, by setting the Young's modulus of the substrate to be large, Df1 and Df2 can be lowered, and the absolute value of their difference can also be reduced. By increasing the thickness of the substrate, Df1 and Df2 can be lowered, and the absolute value of their difference can also be reduced.

[0146] In addition, when the buffer layer is a cured product of a buffer layer-forming composition containing an energy ray polymerizable compound, if the cured product contains a large amount of three-dimensional network structure (crosslinked structure), Df1 and Df2 can be reduced, and the absolute value of the difference between them can also be reduced. A three-dimensional network structure (crosslinked structure) is formed by reacting a photopolymerizable unsaturated group in the functional polymerizable compound constituting the buffer layer with a (meth)acryloyl group in component (a1) or by reacting photopolymerizable unsaturated groups in component (a4) with each other. When a multifunctional polymerizable compound is used, the crosslinked structure formed by energy ray irradiation is more likely to increase compared to when a compound containing only one photopolymerizable unsaturated group is used.

[0147] For example, if the number of (meth)acryloyl groups in the urethane (meth)acrylate (a1) is large, the number of crosslinked structures in the buffer layer increases, the buffer layer becomes harder, Df1 and Df2 can be lowered, and the absolute value of the difference between them can also be lowered. Therefore, by adjusting the amount of components involved in the formation of the crosslinked structure, the thermal deformation property of the protective sheet for workpiece processing can be controlled within an appropriate range. Examples of components involved in the formation of the crosslinked structure include the (meth)acryloyl group in the urethane (meth)acrylate (a1) and the polyfunctional polymerizable compound (a4). In particular, the polyfunctional polymerizable compound (a4) is easy to use and is a useful component for forming the crosslinked structure.

[0148] By adding the polyfunctional polymerizable compound (a4), the movement of molecules inside the cured product is inhibited, and the stress relaxation property is reduced, and Df1 and Df2 can be reduced, and the absolute value of the difference between them can also be designed to be low. In other words, by increasing the amount of the polyfunctional polymerizable compound (a4) added, it becomes easier to achieve the above physical properties. The urethane (meth)acrylate (a1) and components involved in the formation of a long chain structure play a role in mitigating the brittleness of the buffer layer due to the decrease in the stress relaxation rate.

[0149] When the buffer layer is composed of a polyolefin film, the thermal deformation property of the workpiece processing protection sheet can be controlled by appropriately setting the melt flow rate (MFR), glass transition temperature (Tg), melting point (mp), etc. of the polyolefin resin that constitutes the polyolefin film.

[0150] For example, if the MFR of the polyolefin resin is decreased, Df1 and Df2 can be decreased, and the absolute value of the difference between them can also be decreased. Also, if the Tg and mp of the polyolefin resin are increased, Df1 and Df2 can be decreased, and the absolute value of the difference between them can also be decreased.

[0151] When the pressure-sensitive adhesive layer is energy ray-curable, the above-mentioned thermomechanical analysis is performed on the protection sheet for workpiece processing before it is irradiated with energy rays.

[0152] (6. Release Sheet) A release sheet may be attached to the surface of the workpiece processing protective sheet. Specifically, the release sheet is attached to the surface of the adhesive layer of the workpiece processing protective sheet. The release sheet is attached to the surface of the adhesive layer to protect the adhesive layer during transportation and storage. The release sheet is releasably attached to the workpiece processing protective sheet, and is peeled off and removed from the workpiece processing protective sheet before the workpiece processing protective sheet is used (i.e., before the workpiece is attached).

[0153] The release sheet used is a release sheet having at least one surface that has been subjected to a release treatment, and specifically, examples thereof include a release sheet having a release agent applied onto the surface of a release sheet substrate.

[0154] The substrate for the release sheet is preferably a resin film, and examples of the resin constituting the resin film include polyester resin films such as polyethylene terephthalate resin, polybutylene terephthalate resin, and polyethylene naphthalate resin, polyolefin resins such as polypropylene resin and polyethylene resin, etc. Examples of the release agent include silicone-based release agents, alkyd-based release agents, and fluorine-based release agents.

[0155] The thickness of the release sheet is not particularly limited, but is preferably 10 to 200 μm, and more preferably 20 to 150 μm.

[0156] (7. Manufacturing method of protective sheet for workpiece processing) The method for producing the protective sheet for workpiece processing according to the present embodiment is not particularly limited, and any known method may be used. The method for producing the protective sheet for workpiece processing shown in FIG. 1 will be described below.

[0157] First, as a coating agent for a composition for a pressure-sensitive adhesive layer for forming a pressure-sensitive adhesive layer, for example, a composition for a pressure-sensitive adhesive layer containing the above-mentioned components or a composition obtained by diluting the composition for a pressure-sensitive adhesive layer with a solvent, etc. is prepared. Similarly, as a buffer layer, for example, the above-mentioned PE film is prepared.

[0158] Examples of the solvent include organic solvents such as methyl ethyl ketone, acetone, ethyl acetate, tetrahydrofuran, dioxane, cyclohexane, n-hexane, toluene, xylene, n-propanol, and isopropanol.

[0159] The substrate and the PE film are then bonded together. The lamination may be, for example, a dry lamination method using a primer layer, or may be thermocompression bonding.

[0160] In addition, the adhesive layer composition is applied to the release-treated surface of the release sheet by a known method such as spin coating, spray coating, bar coating, knife coating, roll coating, blade coating, die coating, gravure coating, etc., and dried as necessary to form an adhesive layer.Then, the adhesive layer on the release sheet and the substrate are laminated together to obtain a workpiece processing protective sheet in which the adhesive layer is formed in this order on one main surface of the substrate and the buffer layer is formed on the other main surface of the substrate.The release sheet may be removed when the workpiece processing protective sheet is used.

[0161] When the buffer layer is formed from a buffer layer-forming composition containing an energy ray-polymerizable compound, the buffer layer is formed by coating and curing the buffer layer-forming composition on a release sheet, and then laminating the buffer layer to the substrate and removing the release sheet to obtain a laminate of the buffer layer and the substrate.

[0162] The adhesive layer provided on the release sheet is then attached to the substrate side of the laminate to produce a protective sheet for workpiece processing in which the release sheet is attached to the surface of the adhesive layer. The release sheet attached to the surface of the adhesive layer may be appropriately peeled off and removed before use of the protective sheet for workpiece processing.

[0163] The method of forming the adhesive layer on the release sheet is as described above. As a method of forming a buffer layer on the release sheet, the buffer layer can be formed by directly applying the buffer layer forming composition on the release sheet by a known application method to form a coating film, and irradiating this coating film with energy rays. Alternatively, the buffer layer can be formed by directly applying the buffer layer forming composition on one side of the substrate, and drying by heating or irradiating the coating film with energy rays.

[0164] Examples of methods for applying the buffer layer-forming composition include spin coating, spray coating, bar coating, knife coating, roll coating, blade coating, die coating, gravure coating, etc. In order to improve the coatability, an organic solvent may be added to the buffer layer-forming composition, and the composition may be applied onto the release sheet in the form of a solution.

[0165] When the buffer layer forming composition contains an energy ray polymerizable compound, it is preferable to irradiate the coating film of the buffer layer forming composition with energy rays to harden it and form a buffer layer. The buffer layer may be hardened in one hardening process or in multiple hardening processes. For example, the coating film on the release sheet may be completely hardened to form a buffer layer, and then the buffer layer may be laminated to a substrate, or the coating film may not be completely hardened, but a buffer layer forming film in a semi-hardened state may be formed, and the buffer layer forming film may be laminated to a substrate, and then the buffer layer may be completely hardened by irradiating the energy rays again to form a buffer layer. The energy rays irradiated in the hardening process are preferably ultraviolet rays. In addition, when hardening, the coating film of the buffer layer forming composition may be exposed, but it is preferable to harden the coating film by irradiating the energy rays in a state where the coating film is covered with a release sheet or a substrate and the coating film is not exposed.

[0166] A method for producing a protective sheet having buffer layers on both sides of a substrate can, for example, be to obtain a laminate in which a buffer layer, a substrate, and a buffer layer are laminated in this order by the method described above, and then to form a pressure-sensitive adhesive layer on one of the buffer layer sides.

[0167] (7. Method for manufacturing workpieces) The protective sheet for workpiece processing according to the present invention is used to temporarily hold a workpiece such as a semiconductor wafer, a semiconductor chip, glass, or ceramic during processing of the workpiece. The processing of the workpiece includes, for example, cutting, polishing, etc., but is not limited thereto. Among these uses, the protective sheet for workpiece processing according to the present invention is particularly preferably used in a method for manufacturing individual pieces of workpieces such as semiconductor chips by attaching the protective sheet to the surface of the workpiece such as a semiconductor wafer and grinding the backside of the workpiece. More preferably, the protective sheet for workpiece processing according to the present invention is preferably used in DBG in which backside grinding of the workpiece such as a semiconductor wafer and individualization of the workpiece are performed simultaneously. Particularly preferably, the protective sheet for workpiece processing according to the present invention is preferably used in LDBG in which a group of chips with a small kerf width is obtained when the semiconductor wafer is individualized.

[0168] As a non-limiting example of the use of the protection sheet for workpiece processing, a method for manufacturing a semiconductor device will be described in more detail below.

[0169] Specifically, the method for producing the workpiece individual pieces includes at least the following steps 1 to 4. Step 1: The above-mentioned protective sheet for workpiece processing is heated and attached to the surface of the workpiece. Step 2: A step of forming a groove from the front surface side of the workpiece, or forming a modified region inside the workpiece from the front or back surface of the workpiece. Step 3: A step of grinding the workpiece having the protective sheet for workpiece processing attached to its surface and the grooves or modified regions formed therein from its back surface to separate the workpiece into a plurality of chips starting from the grooves or modified regions. Step 4: A step of dry polishing the back surface of the individual workpieces.

[0170] After the above steps, the workpiece processing protection sheet is peeled off from the plurality of individual workpieces (that is, the group of individual workpieces).

[0171] Below, each step of the manufacturing method for the above-mentioned workpiece singulated with resin sheet is described in detail for the case where the workpiece processing protective sheet is a semiconductor processing protective sheet, the workpiece is a semiconductor wafer, and the workpiece singulated is a semiconductor chip.

[0172] In step 1, as shown in Fig. 2, the adhesive layer 30 of the protective sheet for semiconductor processing 1 according to this embodiment is heat-attached to the surface 100a of the semiconductor wafer 100. By heat-attaching the protective sheet for semiconductor processing to the surface of the semiconductor wafer, the surface of the semiconductor wafer is sufficiently protected. If the protective sheet for semiconductor processing is larger than the shape of the semiconductor wafer after heat-attaching to the semiconductor wafer, the protective sheet for semiconductor processing may be cut to fit the shape of the semiconductor wafer and the excess portion may be removed, as necessary.

[0173] This step may be performed before or after step 2, which will be described later. For example, when forming a modified region in a semiconductor wafer, it is preferable to perform step 1 before step 2. On the other hand, when forming grooves on the semiconductor wafer surface by dicing or the like, step 1 is performed after step 2. That is, in this step 1, a protective sheet for semiconductor processing is attached to the surface of the wafer having the grooves formed in step 2, which will be described later.

[0174] The conditions for heat attachment of the protective sheet for semiconductor processing 1 are not particularly limited, but it is sufficient to apply pressure by a roll or the like that allows the adhesive layer of the protective sheet for semiconductor processing 1 to be appropriately softened and does not damage the circuits on the surface of the semiconductor wafer. The heating temperature may be, for example, about 40 to 80°C.

[0175] The thickness of the semiconductor wafer before grinding is not particularly limited, but is usually about 500 to 1000 μm. Also, the semiconductor wafer usually has a circuit formed on its surface. The formation of the circuit on the wafer surface can be performed by various methods including conventionally widely used methods such as an etching method and a lift-off method.

[0176] (Process 2) In step 2, a groove is formed from the front surface side of the semiconductor wafer, or a modified region is formed inside the semiconductor wafer from the front surface or rear surface of the semiconductor wafer.

[0177] The grooves formed in this step are shallower than the thickness of the semiconductor wafer. The grooves can be formed by dicing using a conventionally known wafer dicing device or the like. In step 3 described below, the semiconductor wafer is divided into a plurality of semiconductor chips along the grooves.

[0178] The modified region is an embrittled portion of the semiconductor wafer, and is a region that becomes a starting point for breaking the modified region of the semiconductor wafer and dicing into semiconductor chips due to the thinning of the semiconductor wafer caused by grinding in the grinding process or the application of grinding force. That is, the grooves and modified region in step 2 are formed so as to follow the dividing lines that will be formed when the semiconductor wafer is divided and diced into semiconductor chips in step 3 described below.

[0179] The modified region is formed by irradiating a laser focused on the inside of the semiconductor wafer, and the modified region is formed inside the semiconductor wafer. The laser may be irradiated from the front side or the back side of the semiconductor wafer. In the embodiment in which the modified region is formed, when the step 2 is performed after the step 1 and the laser is irradiated from the front side of the wafer, the laser is irradiated to the semiconductor wafer through the semiconductor processing protective sheet.

[0180] The semiconductor wafer with the protective sheet for semiconductor processing attached and the grooves or modified regions formed thereon is placed on the suction table and is adsorbed and held on the suction table. At this time, the front side of the semiconductor wafer is placed on the table side and is adsorbed via the protective sheet for semiconductor processing.

[0181] (Step 3) After steps 1 and 2, the back surface 100b of the semiconductor wafer on the suction table is ground to separate the semiconductor wafer into a plurality of semiconductor chips, thereby obtaining a group of chips.

[0182] Here, when grooves are formed in the semiconductor wafer, the back grinding is performed so as to thin the semiconductor wafer at least to a position that reaches the bottom of the groove. By this back grinding, the grooves become cuts that penetrate the wafer, and the semiconductor wafer is divided by the cuts and singulated into individual semiconductor chips.

[0183] On the other hand, when a modified region is formed, the grinding surface (wafer back surface) may reach the modified region by grinding, but it does not have to reach the modified region strictly. That is, it is sufficient to grind to a position close to the modified region so that the semiconductor wafer is broken and divided into semiconductor chips starting from the modified region. In addition, when the division is insufficient, for example, the division may be advanced by attaching a pick-up tape described later and then stretching the pick-up tape.

[0184] The shape of the individual semiconductor chips may be square or elongated, such as rectangular. The thickness of the individual semiconductor chips is not particularly limited, but is preferably about 5 to 100 μm, and more preferably 10 to 45 μm. According to LDBG, which provides a modified region inside the wafer with a laser and divides the wafer into individual chips by stress during wafer back grinding, it is easy to make the thickness of the individual semiconductor chips 50 μm or less, and more preferably 10 to 45 μm. The size of the individual semiconductor chips is not particularly limited, but the chip size is preferably 600 mm or less. 2 Less than 400mm, more preferably 2 Less than 120mm, more preferably 2 is less than.

[0185] (Step 4) Next, the backside of the individual semiconductor chip is dry polished. Dry polishing refers to a process of polishing with a polishing puff without using water or abrasive slurry. Various general-purpose polishing puffs can be used as the polishing puff, and commercially available products include, but are not limited to, Disco's polishing wheels "Gettering DP" and "DP08 SERIES." Damaged parts of the chip, i.e., grinding marks, are removed by dry polishing.

[0186] Since no water is used during dry polishing, the backside of the chips is heated by friction, and the protective sheet for workpiece processing is also heated to about 60° C. If dry polishing is continued in this state, the protective sheet for workpiece processing may deform and the chips may collide with each other, but according to the protective sheet for workpiece processing of the present invention, since thermal deformation is suppressed, even if the temperature of the protective sheet for workpiece processing changes during dry polishing or by subsequent cooling, the shape of the sheet does not deform, chips do not collide with each other, and chipping can be suppressed.

[0187] Through the above steps, a workpiece is obtained on the protective sheet for work processing, and if the workpiece is a semiconductor wafer, a plurality of semiconductor chips aligned in the shape of the wafer before cutting are obtained. The protective sheet for work processing with the workpiece singulated thereon is removed from the suction table and transferred to the next step.

[0188] After the dry polishing is completed, a film adhesive or a protective film (or its precursor film) to be used in the subsequent die bonding process may be applied to the ground surface. When forming the film adhesive or protective film, the resin film that will become the adhesive or protective film is pressed onto the back surface of the chip.

[0189] The protective sheet for workpiece processing of the present invention has a unique thermal deformation property as described above, so that even if the protective sheet for workpiece processing is subjected to a thermal history many times, the deformation amount is small and within a certain range. Therefore, even if the protective sheet for workpiece processing is subjected to a thermal history many times, there is no contact between the individual pieces of the workpiece, and the individual pieces of the workpiece can be obtained with a high yield.

[0190] Next, the protective sheet for workpiece processing is peeled off from the individualized workpieces (i.e., a plurality of individual workpieces). This step is performed, for example, by the following method.

[0191] First, when the adhesive layer of the workpiece processing protective sheet is formed from an energy ray curable adhesive, the adhesive layer is cured by irradiating it with energy rays. Next, a pick-up tape is attached to the back side of the individualized workpiece, and the position and direction are adjusted so that the workpiece can be picked up. At this time, a ring frame arranged on the outer periphery of the workpiece is also attached to the pick-up tape, and the outer periphery of the pick-up tape is fixed to the ring frame. The workpiece and the ring frame may be attached to the pick-up tape at the same time, or may be attached at different times. Next, the workpiece processing protective sheet is peeled off from the multiple workpieces held on the pick-up tape.

[0192] Then, the plurality of workpieces are picked up from the pickup tape. If the workpieces are semiconductor chips, they are fixed onto a substrate or the like for a semiconductor device to manufacture a semiconductor device.

[0193] The pickup tape is not particularly limited, but may be, for example, an adhesive tape including a substrate and an adhesive layer provided on at least one surface of the substrate.

[0194] Also, instead of the pick-up tape, an adhesive tape can be used. Examples of the adhesive tape include a laminate of a film-like adhesive and a release sheet, a laminate of a dicing tape and a film-like adhesive, and a dicing-die bonding tape consisting of an adhesive layer and a release sheet having the functions of both a dicing tape and a die bonding tape. That is, in this embodiment, a step of attaching a dicing-die bonding tape to the back surface of the workpiece may be included. Also, before attaching the pick-up tape, a film-like adhesive may be attached to the back surface side of the individualized workpiece. When a film-like adhesive is used, the film-like adhesive may be the same shape as the wafer.

[0195] When using an adhesive tape or when a film-like adhesive is applied to the back side of the singulated work before the pick-up tape is applied, the plurality of workpiece singulations on the adhesive tape or pick-up tape are picked up together with the adhesive layer divided into the same shape as the workpiece singulations. The workpiece singulations are then fixed onto a substrate or the like via the adhesive layer, and a semiconductor device is manufactured. The adhesive layer is divided by a laser or an expander. Also, instead of the adhesive tape, a protective film forming tape for forming a protective film on the back side of the chip may be used.

[0196] The above describes an example of the protective sheet for work processing according to the present invention, which is used in a method for dividing a workpiece by DBG or LDBG, but the protective sheet for work processing according to the present invention can also be used for normal back grinding, and can also be used to temporarily hold a workpiece when processing glass, ceramics, etc. It can also be used as various types of re-peelable protective sheets. EXAMPLES

[0197] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.

[0198] The measurement and evaluation methods are described below. In the following evaluations, the release films on the buffer layer and the pressure-sensitive adhesive layer were appropriately peeled off before the measurements.

[0199] [Thermal deformation] The test was carried out using samples of 20 mm length and 4.5 mm width obtained by cutting out the protective sheets for workpiece processing prepared in the examples and comparative examples. The thickness of the samples was the same as that of the protective sheets for workpiece processing.

[0200] The above sample is held with a chuck distance of 15 mm, a load of 10 g is applied, and the temperature is raised and lowered twice, and the deformation rate of the sample is determined from the change in the chuck distance during this process. In the first heating run, the temperature is raised from 23°C to 50°C at a rate of 3°C / min, and then allowed to cool to 23°C. In the second heating run, a load of 10 g is again applied, and the temperature is raised to 50°C at a rate of 3°C / min.

[0201] The deformation rate Df1 (%) when the temperature reaches 50°C for the first time, and the deformation rate Df2 (%) when the temperature reaches 50°C for the second time are measured.

[0202] Df1 and Df2 are calculated using the following formulas. Df1 = 100 × (S1-S0) / S0 Df2 = 100 × (S2-S0) / S0

[0203] Here, S0 is the chuck interval before the test, S1 is the chuck interval when the temperature reached 50°C for the first time, and S2 is the chuck interval when the temperature reached 50°C for the second time.

[0204] [Crack evaluation] The protective sheets for workpiece processing manufactured in the examples and comparative examples were attached to a silicon wafer with a diameter of 12 inches and a thickness of 775 μm while the table temperature of a backgrinding tape laminator (manufactured by Lintec, device name "RAD3510F / 12") was heated to 50°C. A lattice-shaped modified region was formed on the wafer using a laser saw (manufactured by Disco, device name "DFL7361"). The lattice size was 10 mm x 10 mm.

[0205] Next, the wafer was ground (including dry polishing) to a thickness of 30 μm using a back grinding machine (manufactured by Disco, machine name "DGP8761"), and singulated into a plurality of chips. After the grinding process, energy rays (ultraviolet rays) were irradiated, and a dicing tape (manufactured by Lintec, Adwill D-175D) was affixed to the opposite side of the workpiece processing protective sheet, and the adhesive tape for semiconductor processing was peeled off. The singulated chips were then observed under a digital microscope, and the number of chips with cracks was counted and classified according to the following criteria for each crack size. The crack size (μm) was determined by comparing the length (μm) of the crack along the vertical direction of the chip with the length (μm) of the crack along the horizontal direction of the chip, and the larger value was used.

[0206] (standard) Large crack: Crack size is over 20μm Medium crack: Crack size is between 10μm and 20μm Small crack: Crack size is less than 10μm

[0207] The crack occurrence rate (%) was calculated based on the following formula. Crack occurrence rate (%) = Number of chips with cracks / Total number of chips x 100 A sample was rated as "good" if the crack occurrence rate was 2.0% or less, the number of large cracks was 0, the number of medium cracks was 10 or less, and the number of small cracks was 20 or less, and all other cases were rated as "poor".

[0208] In the following examples and comparative examples, all parts by weight are calculated on a solid content basis. (Preparation of composition for adhesive layer and preparation of release sheet with adhesive layer) An energy ray-curable acrylic copolymer (Mw: 500,000) was obtained by reacting 2-methacryloyloxyethyl isocyanate (MOI) with an acrylic polymer obtained by copolymerizing 50 parts by mass of n-butyl acrylate (BA), 20 parts by mass of methyl methacrylate (MMA), and 30 parts by mass of 2-hydroxyethyl acrylate (2HEA) so that 80 equivalents of the hydroxyl groups of the total hydroxyl groups (100 equivalents) of the acrylic polymer were added.

[0209] 100 parts by mass of this energy ray curable acrylic copolymer was mixed with 10 parts by mass of a multifunctional urethane acrylate ultraviolet curable compound (manufactured by Mitsubishi Chemical Corporation, product name "UT-4332"), 0.375 parts by mass of an isocyanate crosslinking agent (manufactured by Mitsui Chemicals, product name "Takenate D-101E"), and 1 part by mass of bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (manufactured by IGM Resins, product name "Omnirad 819") as a photopolymerization initiator, and diluted with methyl ethyl ketone to prepare a coating liquid of a composition for adhesive layer with a solid content concentration of 34% by mass. The coating liquid of the adhesive composition obtained above was applied to the release-treated surface of a release sheet (manufactured by Lintec Corporation, product name: SP-PET381031) so that the thickness after drying was 20 μm, and the coating was heated and dried to form an adhesive layer on the release sheet, thereby obtaining a release sheet with an adhesive layer.

[0210] [Example 1] (Preparation of Buffer Layer-Forming Composition) A composition for forming a buffer layer was prepared by blending 50 parts of a urethane acrylate oligomer (manufactured by Sartomer, product name "CN8881") and 50 parts of polyethylene glycol (400) diacrylate as ultraviolet-curable compounds, and further blending 2.0 parts by mass of 2-hydroxy-2-methyl-1-phenyl-propan-1-one (manufactured by IGM Resins, product name "Omnirad 1173") as a photopolymerization initiator.

[0211] (Preparation of adhesive sheet) The above-mentioned buffer layer-forming composition was applied to the release-treated surface of a release sheet (manufactured by Lintec Corporation, product name "SP-PET381031", a polyethylene terephthalate (PET) film with silicone release treatment, thickness: 38 μm) to form a coating film. The coating film was then irradiated with ultraviolet light to semi-cure the coating film, forming a buffer layer-forming film with a thickness of 28 μm.

[0212] The above ultraviolet irradiation was performed using a belt conveyor type ultraviolet irradiation device (product name "ECS-401GX" manufactured by iGraphics) and a high pressure mercury lamp (product name "H04-L41" manufactured by iGraphics), with a lamp height of 260 mm, output of 80 W / cm, and illuminance of 70 mW / cm. 2 , irradiation amount 30mW / cm 2 The surface of the buffer layer-forming film thus formed was then bonded to a first easy-adhesion layer of a PET film (thickness: 50 μm, Young's modulus at 23° C.: 4300 MPa) with easy-adhesion layers on both sides, and ultraviolet rays were irradiated again from the release sheet side on the buffer layer-forming film to completely harden the buffer layer-forming film, forming a buffer layer having a thickness of 28 μm.

[0213] The second UV irradiation was performed using the above-mentioned UV irradiation device and high-pressure mercury lamp, with a lamp height of 210 mm, output of 120 W / cm, and illuminance of 155 mW / cm. 2 , irradiation amount 600mW / cm 2 The irradiation conditions were as follows. Next, the adhesive layer of the release sheet with the adhesive layer was attached to the second adhesive layer of the PET film with the adhesive layers on both sides to prepare a protective sheet for processing a workpiece. The results of the thermal deformation amount and crack evaluation are shown in Table 1.

[0214] [Example 2] A protection sheet for workpiece processing was produced in the same manner as in Example 1, except that polyethylene glycol (200) diacrylate was used instead of polyethylene glycol (400) diacrylate in the buffer layer forming composition of Example 1. The results of the thermal deformation amount and crack evaluation are shown in Table 1.

[0215] [Example 3] In the buffer layer forming composition of Example 1, the amount of urethane acrylate oligomer (manufactured by Sartomer, product name "CN8881") was changed to 40 parts, and 10 parts of polyethylene glycol (200) diacrylate and 50 parts of ethoxylated (3) trimethylolpropane triacrylate were added instead of polyethylene glycol (400) diacrylate. A protective sheet for processing a workpiece was produced in the same manner as in Example 1. The results of the thermal deformation amount and crack evaluation are shown in Table 1.

[0216] [Example 4] As a substrate, a PET film (thickness: 50 μm, Young's modulus at 23° C.: 4300 MPa) was prepared. A 2.5 μm thick easy-adhesion layer was provided on both sides of the prepared PET film, and a 25 μm low-density polyethylene (manufactured by Japan Polyethylene Co., Ltd.: "Novatec LD, LF581X") was laminated to both easy-adhesion layers as a buffer layer by dry lamination to obtain a laminate in which a PO-based buffer layer was laminated on both sides of the substrate. Next, the adhesive layer of the release sheet with the adhesive layer was laminated on one of the PO-based buffer layers to produce a protective sheet for work processing. The results of the thermal deformation amount and crack evaluation are shown in Table 1.

[0217] [Example 5] A PET film (thickness: 50 μm, Young's modulus at 23 ° C: 4300 MPa) was prepared as a substrate. A 2.5 μm thick easy-adhesion layer was provided on one side of the prepared PET film, and a 30 μm thick low-density polyethylene (Novatec LD, LF581X, manufactured by Japan Polyethylene Co., Ltd.) was formed as a buffer layer. Next, the adhesive layer of the release sheet with the adhesive layer was attached to the other side of the PET film to prepare a protective sheet for work processing. The results of the thermal deformation amount and crack evaluation are shown in Table 1.

[0218] [Comparative Example 1] Low-density polyethylene (Nippon Polyethylene Co., Ltd.: "Novatec LD, LF607K") was extruded using a small T-die extruder to obtain a film with a thickness of 80 μm. This was used as a substrate, and a protective sheet for work processing was produced in the same manner as in Example 1, except that an easy-adhesion layer and a buffer layer were not provided. The results of the thermal deformation amount and crack evaluation are shown in Table 1.

[0219] [Comparative Example 2] An ethylene-vinyl acetate film (Gunze Co., Ltd., product name "Fanclear LEB", thickness 120 μm) was prepared. A protective sheet for workpiece processing was produced in the same manner as in Comparative Example 1, except that this was used as the substrate. The results of the thermal deformation amount and crack evaluation are shown in Table 1.

[0220] [Comparative Example 3] A bifunctional urethane acrylate oligomer (UA-1) having a mass average molecular weight (Mw) of 5000 was prepared by reacting a polyester diol with an isocyanate-terminated urethane prepolymer obtained by reacting isocyanate with 2-hydroxyethyl acrylate. This oligomer was mixed with isobornyl acrylate (IBXA) and phenyl hydroxypropyl acrylate (HPPA), and further mixed with 2.0 parts by mass of 1-hydroxycyclohexyl phenyl ketone (manufactured by IGM Resins, product name "Omnirad184") and 0.2 parts by mass of a phthalocyanine pigment as a photopolymerization initiator to prepare a coating liquid of a composition for forming a substrate. The coating liquid of the composition for forming a substrate obtained above was applied to the release-treated surface of a release sheet (manufactured by Lintec, product name: SP-PET381031), and the coating film was cured by irradiating ultraviolet light, and a substrate having a thickness of 28 μm and a Young's modulus of 200 MP was prepared on the release sheet. The above ultraviolet irradiation was performed using a belt conveyor type ultraviolet irradiation device (product name "ECS-401GX" manufactured by iGraphics) and a high pressure mercury lamp (product name "H04-L41" manufactured by iGraphics), with a lamp height of 260 mm, output of 80 W / cm, and illuminance of 70 mW / cm. 2 , irradiation amount 30mW / cm 2 The irradiation conditions were as follows:

[0221] Except for using this as the substrate, a protection sheet for workpiece processing was produced in the same manner as in Comparative Example 1. The results of the thermal deformation amount and crack evaluation are shown in Table 1.

[0222] [Comparative Example 4] Ethylene-methacrylic acid copolymer (EMAA; Mitsui DuPont Polychemicals, N0903HC) was extruded using a small T-die extruder, and irradiated with electron beams at a dose of 110 kGy and once to obtain a film with a thickness of 80 μm. A protective sheet for workpiece processing was produced in the same manner as in Comparative Example 1, except that this was used as the substrate. The results of the thermal deformation amount and crack evaluation are shown in Table 1.

[0223] [Table 1]

[0224] In the table, Df1 = 100 × (S1-S0) / S0 Df2 = 100 × (S2-S0) / S0

[0225] From the above results, according to the protective sheet for workpiece processing of the present invention, even if the protective sheet for workpiece processing is subjected to multiple heat histories, the deformation amount is small and within a certain range. Therefore, even if the protective sheet for workpiece processing is subjected to multiple heat histories, there is no contact between the individual workpieces, and the individual workpieces can be obtained with a high yield. [Explanation of symbols]

[0226] 1…Protection sheet for workpiece processing 10...Base material 20…Buffer layer 30...Adhesive layer 100...Semiconductor wafer 100a...circuit surface of semiconductor wafer 100b...Back surface of semiconductor wafer

Claims

1. A protective sheet for work processing having a substrate, a buffer layer provided on at least one surface of the substrate, and an adhesive layer provided on the other surface of the substrate, When the thermomechanical analysis of the workpiece processing protective sheet is performed under the following conditions, the deformation ratio Df1 during the first heating is within 0.67%, and the absolute value of the difference between the deformation ratio Df1 during the first heating and the deformation ratio Df2 during the second heating is within 0.067%. Thermomechanical analysis conditions Sample size: length 20 mm, width 4.5 mm Chuck distance: 15 mm The temperature is raised from 23° C. to 50° C. with a load of 10 g and a heating rate of 3° C. / min, allowed to cool to 23° C., and then heated again to 50° C. with a load of 10 g and a heating rate of 3° C. / min. The deformation rate Df1 (%) when 50° C. is reached for the first time, and the deformation rate Df2 (%) when 50° C. is reached for the second time are measured. Df1 and Df2 are calculated using the following formula. Df1=100×(S1-S0) / S0 Df2=100×(S2-S0) / S0 Here, S0 is the chuck distance before the test, S1 is the chuck distance when the temperature reached 50° C. for the first time, and S2 is the chuck distance when the temperature reached 50° C. for the second time.

2. The protective sheet for workpiece processing according to claim 1, wherein the deformation ratio Df2 (%) when the second temperature reaches 50°C is 0.67% or less.

3. The protection sheet for workpiece processing according to claim 1 , wherein the buffer layer is a cured product of a buffer layer-forming composition containing an energy ray-polymerizable compound.

4. The protective sheet for workpiece processing according to claim 1 is attached to the surface of a workpiece in a process for dividing a workpiece into individual workpieces by grinding the back surface of the workpiece having a groove formed on its surface or a modified region formed inside.

5. 2. The protective sheet for workpiece processing according to claim 1, comprising a substrate, buffer layers provided on both sides of the substrate, and an adhesive layer provided on the surface of one of the buffer layers.

6. 6. The protective sheet for workpiece processing according to claim 5, wherein the buffer layers provided on both sides of the substrate are both polyolefin-based resin films.

7. A step of heat-attaching the workpiece processing protection sheet according to any one of claims 1 to 6 to a surface of the workpiece; A step of forming a groove from the front surface side of the workpiece, or forming a modified region inside the workpiece from the front surface or rear surface of the workpiece; A step of grinding the workpiece having the protective sheet attached to the surface and the groove or the modified region formed thereon from the back side to separate the workpiece into a plurality of workpiece pieces starting from the groove or the modified region; A manufacturing method for a work piece segmented product, comprising a step of performing dry polishing after segmentation.