Resin sheet and building material laminate
The resin sheet design with a thin cationic water-soluble polymer layer addresses the balance between antibacterial performance and secondary processability, ensuring effective adhesiveness and printability.
Patent Information
- Application Number
- JP2023055994
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-30
AI Technical Summary
Resin sheets face challenges in achieving a balance between functional properties like antibacterial performance and secondary processability, such as adhesiveness and printability, due to the exposure of functional agents on the surface or the need for high agent content in the resin composition.
A resin sheet design with a base material, a first functional layer containing a thermoplastic resin and a functional agent, and a second functional layer with a cationic water-soluble polymer, where the second layer is thin (0.1 μm or less) to maintain functionality without affecting adhesion and printability.
The resin sheet maintains antibacterial properties while enhancing secondary processability, ensuring excellent adhesiveness and printability without compromising environmental stability.
Smart Images

Figure 2024143361000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin sheet and a building material laminate. [Background technology]
[0002] Resin sheets are widely used in various fields such as daily necessities, building materials, agricultural products, etc. Here, as a means for imparting various functions to a resin sheet by using a functional agent having a function corresponding to the intended use of the resin sheet, such as antibacterial properties, a coating method in which a coating layer containing a functional agent is provided on the surface of the resin sheet, and a kneading method in which a functional agent is directly added to the resin constituting the resin sheet and then molded, etc., have been considered.
[0003] The coating method can easily impart functionality even with a small amount of functional agent added, but there is concern that the functional agent is exposed to the surface, resulting in poor environmental stability such as water resistance, moisture resistance, and weather resistance. The kneading method has excellent environmental stability, but on the other hand, it is necessary to increase the amount of additive to exert its function, which may affect secondary processability such as printability and adhesion to other films, making it difficult to achieve a quantitative balance.
[0004] Patent Document 1 describes a resin composition that contains a calcium hydroxide material as an antibacterial agent. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-120763 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the resin sheet produced from the resin composition described in Patent Document 1 has room for improvement in terms of secondary processability such as adhesiveness. An object of the present invention is to provide a resin sheet that is suitable for secondary processability without losing functions such as antibacterial properties. [Means for solving the problem]
[0007] The present invention relates to the following resin sheet. [1] A resin sheet comprising a substrate, a first functional layer provided on one main surface of the substrate and containing a thermoplastic resin and a functional agent, and a second functional layer provided on a surface of the first functional layer and containing a cationic water-soluble polymer, The functional agent includes at least one of calcium hydroxide and a metal carrier, The resin sheet, wherein the second functional layer has a thickness of 0.1 μm or less. Effect of the Invention
[0008] According to the present invention, it is possible to provide a resin sheet that is suitable for secondary processability without losing functions such as antibacterial properties. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a resin sheet according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of a resin sheet according to another embodiment of the present invention. [Diagram 3] FIG. 3 is a cross-sectional view showing an example of a building material laminate according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, a resin sheet and a building material laminate according to an embodiment of the present invention will be described in detail. The following is an example (representative example) of the present invention, and the present invention is not limited thereto.
[0011] <Resin sheet> A cross-sectional view of a resin sheet according to an embodiment of the present invention is shown in Fig. 1. The resin sheet 1 in Fig. 1 has a substrate 10, a first functional layer 11 provided on one main surface of the substrate 10, and a second functional layer 12 provided on a surface of the first functional layer 11.
[0012] A cross-sectional view of a resin sheet according to another embodiment of the present invention is shown in Fig. 2. The resin sheet 1 in Fig. 2 has a substrate 10, a first functional layer 11 provided on one main surface of the substrate 10, a second functional layer 12 provided on the surface of the first functional layer 11, a third functional layer 13 provided on the other main surface of the substrate 10, and a fourth functional layer 14 provided on the surface of the third functional layer 13.
[0013] <Base material> The substrate is used to impart strength to the resin sheet, and is preferably made of a thermoplastic resin film. By using a thermoplastic resin film as the substrate, mechanical strength such as stiffness, water resistance, chemical resistance, and opacity as required can be imparted to the resin sheet or a printed matter using the resin sheet.
[0014] The thermoplastic resin used for the substrate is not particularly limited, and examples thereof include polyolefin resins such as polyethylene resins, polypropylene resins, polybutene, and 4-methyl-1-pentene (co)polymers; functional group-containing olefin resins such as ethylene-vinyl acetate copolymers, ethylene-(meth)acrylic acid copolymers, metal salts (ionomers) of ethylene-(meth)acrylic acid copolymers, ethylene-(meth)acrylic acid alkyl ester copolymers (the alkyl group preferably has 1 to 8 carbon atoms), maleic acid-modified polyethylene, and maleic acid-modified polypropylene; aromatic polyesters (polyethylene terephthalate, polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc., aliphatic polyesters (polybutylene succinate, polylactic acid, etc.); polyamide resins such as nylon-6, nylon-6,6, nylon-6,10, nylon-6,12, etc.; styrene resins such as syndiotactic polystyrene, atactic polystyrene, acrylonitrile-styrene (AS) copolymer, styrene-butadiene (SBR) copolymer, acrylonitrile-butadiene-styrene (ABS) copolymer, etc.; polyvinyl chloride resins; polycarbonate resins; polyphenylene sulfide, etc. These resins may be used in combination of two or more kinds.
[0015] Among these, polyolefin resins or polyester resins are preferred because of their high water resistance and transparency, and among polyolefin resins, polypropylene resins are more preferred, and among polyester resins, polyethylene terephthalate is more preferred.
[0016] The substrate may contain a filler to adjust the stiffness, whiteness and opacity of the substrate. Examples of the filler include inorganic fillers and organic fillers, which may be used alone or in combination. When a substrate containing a filler is stretched, a large number of fine pores with the filler as a nucleus can be formed inside the substrate, which can result in whitening, opacity and weight reduction.
[0017] Examples of inorganic fillers include heavy calcium carbonate, light calcium carbonate, calcined clay, talc, diatomaceous earth, titanium oxide, zinc oxide, barium sulfate, silicon oxide, magnesium oxide, and inorganic particles surface-treated with fatty acid, polymer surfactant, antistatic agent, etc. Among these, heavy calcium carbonate, light calcium carbonate, calcined clay, and talc are preferred because they have good pore formability and are inexpensive. From the viewpoint of improving whiteness and opacity, titanium oxide, zinc oxide, and barium sulfate are preferred.
[0018] The organic filler is not particularly limited, but is preferably an organic particle that is incompatible with the thermoplastic resin, has a melting point or glass transition temperature higher than that of the thermoplastic resin, and is finely dispersed under the melt-kneading conditions of the thermoplastic resin.For example, when the thermoplastic resin is a polyolefin-based resin, the organic filler may be an organic particle such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polystyrene, polyamide, polycarbonate, polyethylene sulfide, polyphenylene sulfide, polyimide, polyether ketone, polyether ether ketone, polymethyl methacrylate, poly-4-methyl-1-pentene, a homopolymer of a cyclic olefin, or a copolymer of a cyclic olefin and ethylene.Fine powder of a thermosetting resin such as a melamine resin may also be used, and it is also preferable to crosslink the thermoplastic resin to make it insoluble. The melting point (° C.) and glass transition temperature (° C.) of the resin can be measured by differential scanning calorimetry (DSC).
[0019] The inorganic filler and the organic filler may be used alone by selecting one from the above, or may be used in combination of two or more. When two or more are combined, the combination may be an inorganic filler and an organic filler.
[0020] The average particle size of the inorganic filler and the organic filler is preferably large from the viewpoint of ease of mixing with the thermoplastic resin. In addition, the average particle size of the inorganic filler and the organic filler is preferably small from the viewpoint of preventing troubles such as sheet breakage and strength reduction of the substrate during stretching when voids are generated inside by stretching to improve opacity and printability. Specifically, the average particle size of the inorganic filler and the organic filler is preferably 0.01 μm or more, more preferably 0.1 μm or more, and even more preferably 0.5 μm or more. In addition, the average particle size of the inorganic filler and the organic filler is preferably 30 μm or less, more preferably 20 μm or less, and even more preferably 15 μm or less.
[0021] The average particle size of the inorganic filler and the organic filler can be determined by observing a cut surface of the substrate with an electron microscope, measuring the maximum diameters of at least 10 particles, and calculating the average value as the average dispersed particle size when dispersed in a thermoplastic resin by melt kneading and dispersion.
[0022] The content of the filler in the substrate is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, from the viewpoint of imparting opacity to the substrate. From the viewpoint of imparting rigidity to the substrate and improving the handleability of the resin sheet, the filler content in the substrate is preferably 45% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less.
[0023] The substrate may contain any of the known additives as necessary, such as antioxidants, light stabilizers, ultraviolet absorbers, crystal nucleating agents, plasticizers, dispersants for fillers, slip agents such as fatty acid amides, antiblocking agents, dyes, pigments, release agents, and flame retardants.
[0024] The substrate may have a single layer structure or a multi-layer structure. The thickness of the substrate is preferably 30 μm or more, more preferably 50 μm or more, because sufficient mechanical strength is easily obtained, and is preferably 500 μm or less, more preferably 300 μm or less, because the weight of the resin sheet is reduced and the handleability is easily improved.
[0025] When the substrate has internal pores, the porosity, which represents the proportion of pores in the substrate, is preferably 10% or more, more preferably 12% or more, even more preferably 15% or more, and particularly preferably 20% or more from the viewpoint of obtaining opacity. From the viewpoint of maintaining mechanical strength, the porosity is preferably 45% or less, more preferably 44% or less, even more preferably 42% or less, and particularly preferably 40% or less.
[0026] The porosity can be measured by the area ratio of pores in a certain region of the cross section of the substrate observed with an electron microscope. Specifically, an arbitrary part of the substrate is cut out, embedded in epoxy resin and solidified, then cut perpendicularly to the surface direction of the substrate using a microtome, and attached to an observation sample stage so that the cut surface becomes the observation surface. Gold or gold-palladium, etc. is evaporated on the observation surface, and the pores are observed at an arbitrary magnification (for example, 500 to 3000 times magnification) that is easy to observe with an electron microscope, and the observed region is captured as image data. The obtained image data is subjected to image processing with an image analyzer to determine the area ratio (%) of the pore portion, which can be used as the porosity (%). In this case, the porosity can be determined by averaging the measured values in observations of arbitrary 10 or more points.
[0027] <First functional layer> In the resin sheet according to the embodiment of the present invention, the first functional layer is provided on one main surface of the substrate and contains a thermoplastic resin and a functional agent. By having the resin sheet have the first functional layer containing the functional agent, various functions such as antibacterial properties can be imparted to the resin sheet. In addition, by including the functional agent in the resin (kneading the functional agent into the resin), the environmental stability of the resin sheet can be improved. In addition, since the second functional layer described later is provided on the surface of the first functional layer, even if the content of the functional agent in the first functional layer is increased to improve functionality, the functional agent can be prevented from affecting the adhesiveness and printability of the resin sheet, and a resin sheet with excellent secondary processability can be obtained.
[0028] The thermoplastic resin constituting the first functional layer is not particularly limited as long as it does not impair the effects of the present invention, and the same thermoplastic resin as that of the substrate can be used. Among the thermoplastic resins, polyolefin resins or functional group-containing olefin resins are preferred from the viewpoints of excellent processability and water resistance, and polyolefin resins are more preferred. Among the polyolefin resins, polyethylene resins or polypropylene resins are preferred from the viewpoints of chemical resistance, processability, and low cost.
[0029] Examples of polyolefin resins include polyethylene resins (low density polyethylene, medium density polyethylene, high density polyethylene, linear low density polyethylene, low crystalline or amorphous ethylene-α-olefin copolymer, ethylene-cyclic olefin copolymer, etc.), polypropylene resins (crystalline polypropylene, low crystalline polypropylene, amorphous polypropylene, propylene-ethylene copolymer (random copolymer or block copolymer, etc.), propylene-α-olefin copolymer, propylene-ethylene-α-olefin copolymer, etc.), polybutene, 4-methyl-1-pentene (co)polymers (poly(4-methyl-1-pentene), 4-methyl-1-pentene-α-olefin copolymer, etc.). The α-olefin is not particularly limited as long as it is copolymerizable with ethylene, propylene, and 4-methyl-1-pentene, and examples thereof include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, and 1-octene. Examples of functional group-containing olefin resins include ethylene-ethyl (meth)acrylate copolymers, ethylene-methyl (meth)acrylate copolymers, ethylene-n-butyl (meth)acrylate copolymers, ethylene-vinyl acetate copolymers, maleic acid modified polyethylene, and maleic acid modified polypropylene. These may be used alone or in combination.
[0030] The thickness of the first functional layer is preferably 1 μm or more, more preferably 2 μm or more, from the viewpoint of effectively obtaining the function of the first functional layer, and is preferably 200 μm or less, from the viewpoint of reducing the weight of the resin sheet itself and improving the handleability. By making the first functional layer thin, it is possible to provide a resin sheet that is less likely to impair the functionality of the substrate (such as opacity) and can be adjusted to have qualities such as thickness and stiffness suitable for label applications and secondary processing suitability.
[0031] <Functional Agent> The functional agent is not limited as long as it has the property of imparting various functions to the resin sheet, and is preferably, for example, a functional agent having one or more functions selected from antibacterial, antifungal, and antiviral properties. In addition, the functional agent may be used alone or in combination of two or more kinds. As used herein, "antibacterial" refers to, for example, killing, damaging, or preventing the growth of bacteria and fungi. "Anti-fungal" refers to, for example, preventing the occurrence or growth of mold. "Anti-viral" refers to, for example, inactivating viruses.
[0032] The functional agent includes at least one of calcium hydroxide and a metal carrier. The functional agent may be used alone or in combination with two or more kinds. Calcium hydroxide and the metal carrier have antibacterial, antifungal, and antiviral properties.
[0033] From the viewpoint of making the first functional layer a porous layer, the calcium hydroxide is preferably a calcium hydroxide support, and examples of the calcium hydroxide support include shell powder and calcined shell powder.
[0034] The metal carrier is composed of a metal and a carrier that supports the metal. Examples of the metal include gold, silver, copper, mercury, zinc, iron, lead, bismuth, titanium, tin, and nickel. The form of the metal is not particularly limited, and examples include metal particles, metal ions, and metal salts (including metal complexes). Among them, from the viewpoint of obtaining better antibacterial, antiviral, or antifungal properties, it is preferable that the metal contains gold, silver, or copper. Examples of the carrier include inorganic oxides (e.g., zeolite (crystalline aluminosilicate), silica gel, silicates such as clay minerals, glass (including water-soluble glass), zirconium phosphate, calcium phosphate, etc.), activated carbon, metal carriers, and organic metals. From the viewpoint of obtaining better antibacterial, antiviral, or antifungal properties, it is preferable that the metal carrier is a silver carrier. Specifically, the silver in the silver carrier is preferably a silver salt such as silver nitrate, silver chloride, silver sulfate, silver lactate, or silver acetate; a silver complex such as a silver ammonia complex, a silver chloro complex, or a silver thiosulfate complex; silver particles; or a silver ion.
[0035] The content of the functional agent in the first functional layer is preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 3% by mass or more, and particularly preferably 5% by mass or more. The content of the functional agent in the first functional layer is preferably 30% by mass or less, more preferably 28% by mass or less, and even more preferably 25% by mass or less. When the content of the functional agent is 1% by mass or more, the function such as antibacterial property of the first functional layer is easily exhibited even on the second functional layer. In addition, when the content of the functional agent is 30% by mass or less, dispersibility in the thermoplastic resin is improved, which is preferable.
[0036] When calcium hydroxide is used as the functional agent, the content of calcium hydroxide in the first functional layer is preferably 1% by mass or more, more preferably 2% by mass or more, particularly preferably 5% by mass or more, and preferably 30% by mass or less, more preferably 20% by mass or less, particularly preferably 15% by mass or less. In the case of a calcium hydroxide support, the value converted into the content of calcium hydroxide itself is preferably within the above range. When a metal carrier is used as the functional agent, the content of the metal carrier in the first functional layer is preferably 1 mass% or more, more preferably 2 mass% or more, particularly preferably 3 mass% or more, and preferably 10 mass% or less, more preferably 8 mass% or less, particularly preferably 7 mass% or less.
[0037] The first functional layer is preferably a stretched layer. When the first functional layer is a stretched layer containing the functional agent, in some cases, the stretched layer further contains at least one of an inorganic filler and an organic filler in addition to the functional agent, and thus can be a stretched porous layer. When the first functional layer has a porous structure, the functional agent is easily exposed to the surface of the first functional layer, and the effect of the functional agent is easily exerted, which is preferable. In addition, when the first functional layer is a stretched layer, the surface is roughened and the contact area of the functional agent is increased, so that the function such as antibacterial property is effectively expressed.
[0038] The inorganic filler and the organic filler are preferably the same as those in the above-mentioned base material.
[0039] When the first functional layer contains an inorganic filler or an organic filler, the content of these is preferably 10 to 60 mass%, more preferably 15 to 50 mass%. Note that when the functional agent is a calcium hydroxide carrier or a metal carrier and the first functional layer contains an inorganic filler in addition to the functional agent, the content of the inorganic filler refers to the total content of the calcium hydroxide carrier and the metal carrier.
[0040] The first functional layer may contain other components within the range that does not impair the effects of the present invention. Examples of other components include the additives exemplified for the substrate.
[0041] <Second functional layer> In the resin sheet according to the embodiment of the present invention, the second functional layer is provided on the surface of the first functional layer, contains a cationic water-soluble polymer, and has a thickness of 0.1 μm or less. Due to the nature of the function such as antibacterial properties, the first functional layer is usually provided on the outermost surface of the resin sheet. However, in the resin sheet according to the embodiment of the present invention, the first functional layer is covered with the second functional layer and is not provided on the outermost surface of the resin sheet. However, by making the second functional layer contain a cationic water-soluble polymer and suppressing the thickness to a certain level or less, even if the first functional layer is not on the outermost surface, the expression of the function such as antibacterial properties is not inhibited, and further, the surface performance of the second functional layer, i.e., secondary processability, can be imparted to the resin sheet.
[0042] <Cationic Water-Soluble Polymer> By including a cationic water-soluble polymer in the second functional layer, the expression of functions such as antibacterial properties by the first functional layer is less likely to be inhibited. The water solubility of the cationic water-soluble polymer is sufficient if it is such that the aqueous medium containing the cationic water-soluble polymer is in a solution state when preparing the coating liquid for forming the second functional layer.
[0043] Examples of cationic water-soluble polymers include (meth)acrylic polymers or ethyleneimine polymers having an amino group or an ammonium salt structure, water-soluble polymers having a phosphonium salt structure, and vinyl polymers obtained by cationizing water-soluble polymers such as polyvinylpyrrolidone and polyvinyl alcohol through modification, and one of these can be used alone or two or more can be used in combination. Among these, (meth)acrylic polymers or ethyleneimine polymers having an amino group or an ammonium salt structure are preferred from the viewpoint of transferability and adhesion of ink or toner to the second functional layer, and (meth)acrylic polymers or ethyleneimine polymers having an amino group are more preferred.
[0044] From the viewpoint of safety, the (meth)acrylic polymer or ethyleneimine polymer having an amino group or an ammonium salt structure preferably has a primary to tertiary amino group or a primary to tertiary ammonium salt structure, more preferably has a secondary to tertiary amino group or a secondary to tertiary ammonium salt structure, and even more preferably has a tertiary amino group or a tertiary ammonium salt structure. In addition, from the viewpoint of obtaining a resin with a high degree of crosslinking by reaction with a silane coupling agent described later and obtaining high adhesion between the ink or toner and the second functional layer, a primary to tertiary amino group or a primary to tertiary ammonium salt structure is preferred, a primary to secondary amino group or a primary to secondary ammonium salt structure is more preferred, and a primary amino group or a primary ammonium salt structure is even more preferred.
[0045] Among these, ethyleneimine-based polymers are preferred because they have high affinity with inks or toners used in various printing methods, particularly ultraviolet-curable inks used in flexographic printing methods, thereby improving adhesion between the second functional layer and the ink. Examples of the ethyleneimine-based polymer include polyethyleneimine, poly(ethyleneimine-urea), ethyleneimine adducts of polyamine polyamides, their alkyl-modified products, cycloalkyl-modified products, aryl-modified products, allyl-modified products, aralkyl-modified products, benzyl-modified products, cyclopentyl-modified products, cyclic aliphatic hydrocarbon-modified products, glycidol-modified products, and hydroxides thereof. Examples of the modifier for obtaining the modified products include methyl chloride, methyl bromide, n-butyl chloride, lauryl chloride, stearyl iodide, oleyl chloride, cyclohexyl chloride, benzyl chloride, allyl chloride, cyclopentyl chloride, and the like.
[0046] From the viewpoint of improving adhesion to the first functional layer and to ink, etc., the weight average molecular weight of the cationic water-soluble polymer is preferably 1,000 or more, more preferably 10,000 or more, even more preferably 20,000 or more, and particularly preferably 25,000 or more, while the weight average molecular weight is preferably 1,000,000 or less, and more preferably 500,000 or less. The weight average molecular weight and number average molecular weight of the polymer can be obtained by converting values measured by GPC (Gel Permeation Chromatography) into polystyrene equivalent values.
[0047] The second functional layer preferably contains a resin which is a reaction product of a cationic water-soluble polymer and a silane coupling agent. By reacting with the silane coupling agent, the adhesion to the first functional layer can be improved. The silane coupling agent has a functional group which is highly reactive with an organic material, and it is presumed that this functional group crosslinks the thermoplastic resin of the first functional layer with the cationic water-soluble polymer to improve the adhesion to the first functional layer and prevent the intrusion of moisture between the first functional layer and the second functional layer. It is presumed that this suppresses the peeling of the second functional layer and, in turn, the peeling of the ink or toner from the printed matter, thereby improving the abrasion resistance. In addition, it is presumed that the silane coupling agent crosslinks the cationic water-soluble polymers to form a network structure, and that this network structure improves the transferability and adhesion of the ink or toner. Furthermore, it is presumed that the silane coupling agent crosslinks with the cationic water-soluble polymer to increase the molecular weight of the hydrophilic component (polar resin component) of the cationic water-soluble polymer, thereby improving the water resistance. In addition, even when the second functional layer contains a reaction product of a cationic water-soluble polymer and a silane coupling agent, it may contain cationic water-soluble polymer as an unreacted component.
[0048] The silane coupling agent may be contained in the second functional layer as an unreacted portion that does not constitute a reaction product with the cationic polymer. Specific examples of the silane coupling agent that can be used include epoxy-based silane coupling agents, vinyl-based silane coupling agents, (meth)acrylic-based silane coupling agents, amino-based silane coupling agents, ureido-based silane coupling agents, mercapto-based silane coupling agents, and isocyanate-based silane coupling agents.
[0049] The content of the cationic water-soluble polymer component in the second functional layer (total amount of unreacted portion and reacted portion with the silane coupling agent) is preferably 30 to 100 mass%. The content of the cationic water-soluble polymer component in the second functional layer (total amount of unreacted portion and reacted portion with the silane coupling agent) is preferably 50 mass% or more, more preferably 60 mass% or more, even more preferably 75 mass% or more, and preferably 100 mass% or less, more preferably 95 mass% or less, even more preferably 90 mass% or less, particularly preferably 80 mass% or less. When the content of the cationic water-soluble polymer is 30% by mass or more, the first functional layer can easily provide functions such as antifungal properties.
[0050] When the second functional layer contains an ethyleneimine-based polymer, the content of the ethyleneimine-based polymer component (total amount of unreacted portion and reacted portion with the silane coupling agent) is preferably 30 to 100% by mass. The content of the ethyleneimine-based polymer component in the second functional layer (total amount of unreacted portion and reacted portion with the silane coupling agent) is preferably 30% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, and preferably 100% by mass or less, more preferably 80% by mass or less, even more preferably 60% by mass or less, particularly preferably 50% by mass or less. When the content of the ethyleneimine-based polymer is 30% by mass or more, the adhesion between the second functional layer and the ink is likely to be improved.
[0051] When the second functional layer contains a silane coupling agent, the content of the silane coupling agent component (total amount of unreacted and reacted) is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 20 parts by mass or more, per 100 parts by mass of the cationic polymer component (total amount of unreacted and reacted) in the second functional layer. The content of the silane coupling agent component (total amount of unreacted and reacted) in the second functional layer is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 30 parts by mass or less, per 100 parts by mass of the cationic polymer component (total amount of unreacted and reacted) in the second functional layer.
[0052] In addition, when the second functional layer contains a silane coupling agent, the content of the silane coupling agent component (total amount of unreacted and reacted) is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 3% by mass or more, based on the total mass of the second functional layer. In addition, the content of the silane coupling agent component (total amount of unreacted and reacted) in the second functional layer is preferably 20% by mass or less, more preferably 18% by mass or less, and even more preferably 15% by mass or less, based on the total mass of the second functional layer.
[0053] The amount of silane coupling agent contained in the second functional layer is within the above range, so that the amount of unreacted silane coupling agent remaining in the second functional layer can be suppressed. This makes the hardness of the second functional layer moderate, so that it can follow the bending of the resin sheet, and can prevent the second functional layer from cracking. In addition, the amount of silane coupling agent is within the above range, so that the amount of unreacted cationic polymer remaining can be suppressed, so that the water resistance of the second functional layer is excellent.
[0054] <Antistatic agent> The second functional layer preferably contains an antistatic agent, from the viewpoint of improving the surface resistivity and making it easier to obtain antistatic properties. Among the antistatic agents, polymer-type antistatic agents are preferred from the viewpoint of reducing surface contamination due to bleed-out. The polymer-type antistatic agent is not particularly limited, and cationic, anionic, amphoteric or nonionic antistatic agents can be used, which can be used alone or in combination of two or more. When the second functional layer contains a cationic polymer-type antistatic agent, the antistatic agent is contained as a cationic water-soluble polymer.
[0055] Examples of cationic antistatic agents include antistatic agents having an ammonium salt structure, a phosphonium salt structure, etc. Examples of anionic antistatic agents include antistatic agents having an alkali metal salt (lithium salt, sodium salt, potassium salt, etc.) structure of sulfonic acid, phosphoric acid, carboxylic acid, etc. The anionic antistatic agent may be an antistatic agent having an alkali metal salt structure of acrylic acid, methacrylic acid, (anhydrous) maleic acid, etc. in its molecular structure.
[0056] Examples of amphoteric antistatic agents include antistatic agents that contain both cationic and anionic antistatic agent structures in the same molecule. Examples of amphoteric antistatic agents include betaine antistatic agents. Examples of nonionic antistatic agents include ethylene oxide polymers having an alkylene oxide structure, polymers having ethylene oxide polymerization components in the molecular chain, and the like. Other examples of antistatic agents include polymer-type antistatic agents that have boron in the molecular structure.
[0057] Among these, as the polymer-type antistatic agent, a cationic antistatic agent is preferable, a nitrogen-containing polymer-type antistatic agent is more preferable, an antistatic agent having a quaternary ammonium salt structure is further preferable, and an acrylic resin having a quaternary ammonium salt structure is particularly preferable. As the polymer-type antistatic agent, commercially available products such as Saftomer ST-1000, ST-1100, and ST-3200 (trade names) manufactured by Mitsubishi Chemical Corporation can be used. As the polymer-type antistatic agent, a compound that reacts with a silane coupling agent or a compound that does not react with a silane coupling agent may be used. However, from the viewpoint of ease of manifesting antistatic performance, a compound that does not react with a silane coupling agent is preferred.
[0058] When the second functional layer contains an antistatic agent, the content of the antistatic agent is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, based on the total mass of the second functional layer. The content of the antistatic agent in the second functional layer is preferably 80% by mass or less, more preferably 60% by mass or less, even more preferably 40% by mass or less, and particularly preferably 30% by mass or less, based on the total mass of the second functional layer.
[0059] If necessary, the second functional layer may contain other auxiliary components such as a crosslinking promoter, an antiblocking agent, a pH adjuster, an antifoaming agent, etc. Examples of the crosslinking promoter include phosphoric acid, sulfuric acid, citric acid, and succinic acid.
[0060] <Inorganic filler> The content of the inorganic filler in the second functional layer is 9 parts by mass or less relative to 100 parts by mass of the cationic water-soluble polymer. That is, the second functional layer does not contain an inorganic filler, or if it does contain an inorganic filler, the content is 9 parts by mass or less. By containing the inorganic filler in an amount of 9 parts by mass or less, blank spots in the printed portion due to the unevenness of the second functional layer caused by the inorganic filler are prevented, and a high ink transfer rate is easily obtained. From the same viewpoint, the content of the inorganic filler in the second functional layer is more preferably 5 parts by mass or less, and even more preferably 3 parts by mass or less relative to 100 parts by mass of the cationic water-soluble polymer.
[0061] <Thermoplastic resin particles> The second functional layer preferably does not contain thermoplastic resin particles. Thermoplastic resin particles refer to particles derived from an emulsion of a thermoplastic resin such as an olefin copolymer, which is dispersed in a dispersion medium in a coating liquid for forming a second functional layer. Since the second functional layer does not contain thermoplastic resin particles, a recording paper having excellent appearance such as gloss and transparency can be obtained. From the same viewpoint, the content of the thermoplastic resin particles in the second functional layer is more preferably 5 parts by mass or less, and even more preferably 3 parts by mass or less, relative to 100 parts by mass of the cationic water-soluble polymer.
[0062] The thickness of the second functional layer is 0.1 μm or less, preferably 0.09 μm or less, more preferably 0.08 μm or less. The thickness of the second functional layer is very thin, 0.1 μm or less, and does not inhibit the function of the first functional layer, so that the function is easily expressed and the secondary processability of the resin sheet is easily obtained. From the viewpoint of stably forming a uniform second functional layer, the thickness of the second functional layer is preferably 0.01 μm or more, more preferably 0.02 μm or more, and even more preferably 0.03 μm or more.
[0063] <Third functional layer> The resin sheet according to the embodiment of the present invention may have a third functional layer on the other main surface of the substrate. The third functional layer is preferably the same as the first functional layer described above. By having a layer containing a functional agent on the other main surface, it is useful in applications where antibacterial properties or the like are required on the other main surface side as well. For example, when the resin sheet according to an embodiment of the present invention is used in a building material laminate described below, it is sufficient for the resin sheet to have antibacterial or other functions on one main surface side (the first functional layer side), and there is little need to impart functions to the other main surface side (the third functional layer side) because the resin sheet is adhered to the building material board and is not exposed on the surface. On the other hand, when the resin sheet according to the embodiment of the present invention is used, for example, as a reflective sheet for a plant factory, it is desirable for both sides to have a function such as antibacterial properties, and therefore it is preferable for it to have a third functional layer.
[0064] The configuration of the third functional layer is preferably the same as the configuration of the first functional layer, including the preferred aspects.
[0065] <Fourth functional layer> The resin sheet according to the embodiment of the present invention may have a fourth functional layer on the surface of the third functional layer. The fourth functional layer is preferably the same as the above-mentioned second functional layer. When the resin sheet according to the embodiment of the present invention is used in a building material laminate described below, the inclusion of the fourth functional layer makes it easier to obtain adhesion to the building material board. When the resin sheet according to the embodiment of the present invention is used, for example, as a reflective sheet for a plant factory, the inclusion of the fourth functional layer makes it easier to obtain antistatic properties and printability, similar to the second functional layer.
[0066] The configuration of the fourth functional layer is preferably the same as the configuration of the second functional layer, including the preferred embodiment.
[0067] <Method of manufacturing resin sheet> <Methods of manufacturing the substrate, the first functional layer, and the third functional layer> The substrate in the resin sheet according to the embodiment of the present invention can be obtained by mixing the material constituting the substrate and other components as necessary, and then molding the mixture. The first functional layer can be obtained by mixing a thermoplastic resin, a functional agent, and other components as necessary, and then molding the mixture. The third functional layer can also be obtained in the same manner as the first functional layer. The molding method is not particularly limited, and various known molding methods can be used alone or in combination. For example, the resin can be molded into a film by cast molding, which is a method of extruding a molten resin into a sheet using a single-layer or multi-layer T-die, I-die, or the like connected to a screw-type extruder, calendar molding, rolling molding, inflation molding, or the like. The substrate, the first functional layer, or the third functional layer may be molded by casting or calendar molding a mixture of a thermoplastic resin and an organic solvent or oil, and then removing the solvent or oil.
[0068] The substrate, the first functional layer, and the third functional layer may be molded separately and then laminated, or the substrate and the first functional layer, or the first functional layer, the substrate, and the third functional layer may be molded together. For example, a laminate in which the substrate and the first functional layer or the third functional layer are laminated together can be obtained by using a molding method such as co-extrusion.
[0069] Examples of molding methods for laminating the substrate with the first functional layer and the third functional layer include a multi-layer die method using a feed block or a multi-manifold, and an extrusion lamination method using multiple dies, and each method can also be combined.
[0070] The substrate, the first functional layer, and the third functional layer may each be a non-stretched film or a stretched film. Examples of the stretching method include a longitudinal stretching method using the difference in peripheral speed between rolls, a transverse stretching method using a tenter oven, a sequential biaxial stretching method combining these, a rolling method, a simultaneous biaxial stretching method using a combination of a tenter oven and a pantograph, a simultaneous biaxial stretching method using a combination of a tenter oven and a linear motor, etc. Also usable is a simultaneous biaxial stretching (inflation molding) method in which a molten resin is extruded into a tube shape using a circular die connected to a screw-type extruder, and then air is blown into the extruded resin.
[0071] From the viewpoint of imparting appropriate stiffness to the resin sheet and adjusting the water vapor transmission coefficient by being porous, it is preferable that at least one of the substrate and the first functional layer is stretched. When the substrate has a multi-layer structure, it is preferable that at least one of the layers is stretched. When multiple layers are stretched, each layer may be stretched individually before lamination, or may be stretched collectively after lamination, or a stretched layer may be stretched again after lamination.
[0072] The stretching temperature during stretching is preferably in the range of the glass transition temperature of the thermoplastic resin or higher when the thermoplastic resin is a non-crystalline resin, and is preferably in the range of the glass transition temperature of the non-crystalline part of the thermoplastic resin or higher and the melting point of the crystalline part of the thermoplastic resin or lower when the thermoplastic resin is a crystalline resin, specifically, the temperature is preferably 2 to 60°C lower than the melting point of the thermoplastic resin.
[0073] The stretching speed when stretching is not particularly limited, but from the viewpoint of stable stretch forming, it is preferably within the range of 20 to 350 m / min.
[0074] The stretching ratio when stretching can also be appropriately determined in consideration of the properties of the thermoplastic resin used. For example, when a thermoplastic resin film containing a propylene homopolymer or a copolymer thereof is stretched in one direction, the stretching ratio is usually about 1.2 times or more, preferably 2 times or more, and usually 12 times or less, preferably 10 times or less. On the other hand, when biaxially stretching, the stretching ratio is usually 1.5 times or more, preferably 10 times or more, and usually 60 times or less, preferably 50 times or less, in terms of area stretching ratio.
[0075] When a thermoplastic resin film containing a polyester resin is stretched in one direction, the stretching ratio is usually 1.2 times or more, preferably 2 times or more, and usually 10 times or less, preferably 5 times or less. When biaxially stretched, the stretching ratio is, in terms of area stretching ratio, usually 1.5 times or more, preferably 4 times or more, and usually 20 times or less, preferably 12 times or less. For example, when the substrate contains a filler, if the stretching ratio is within the above range, the desired porosity is obtained and the opacity is improved. In addition, the substrate is less likely to break, and stable stretch molding tends to be possible.
[0076] By the above, a resin laminate of first functional layer / substrate or a resin laminate of first functional layer / substrate / third functional layer can be obtained.
[0077] <Surface treatment> The first functional layer and / or the third functional layer are preferably subjected to a surface treatment. By subjecting the first functional layer and / or the third functional layer to a surface treatment such as a corona treatment, the surface free energy is likely to be within a desired range. By activating the surface of the first functional layer and / or the third functional layer, the adhesion with the second functional layer and / or the fourth functional layer can be improved.
[0078] Examples of the surface treatment include corona discharge treatment, frame treatment, plasma treatment, glow discharge treatment, ozone treatment, etc., and these treatments can be combined. Among these, corona discharge treatment or frame treatment is preferred, and corona treatment is more preferred.
[0079] When performing corona discharge treatment, the discharge amount is preferably 600 J / m 2 (10W min / m 2 ) or more, and more preferably 1,200 J / m 2 (20W min / m 2 ) or more. The discharge amount is preferably 12,000 J / m 2 (200W min / m 2 ) or less, and more preferably 10,800 J / m 2 (180W min / m 2 The discharge amount when carrying out the flame treatment is preferably 8,000 J / m 2 More preferably, 20,000 J / m 2 The discharge amount is preferably 200,000 J / m or more. 2 or less, more preferably 100,000 J / m 2 The following is the result.
[0080] <Manufacture of the second functional layer and the fourth functional layer> The second functional layer can be formed by applying an aqueous solution (hereinafter also referred to as "coating liquid for forming the second functional layer") containing a cationic water-soluble polymer and an aqueous solvent, and optionally containing a silane coupling agent, an antistatic agent, etc., to the surface of the first functional layer, and then drying. The fourth functional layer can also be formed by applying an aqueous solution (hereinafter also referred to as "coating liquid for forming the fourth functional layer") containing a cationic water-soluble polymer and an aqueous solvent, and optionally containing a silane coupling agent, an antistatic agent, etc., to the surface of the third functional layer, and then drying.
[0081] The aqueous solvent may be water, or may contain water as the main component and a water-soluble organic solvent such as methyl alcohol, ethyl alcohol, isopropyl alcohol, acetone, methyl ethyl ketone, ethyl acetate, toluene, xylene, etc. The main component of water means that 50 mass% or more of the total is water. The use of an aqueous solvent makes process management easier and is also preferable from the viewpoint of safety.
[0082] The amount of cationic water-soluble polymer contained in the coating liquid for forming the second functional layer or the coating liquid for forming the fourth functional layer (hereinafter collectively referred to as "coating liquid") is preferably 50 mass% or more, more preferably 60 mass% or more, even more preferably 75 mass% or more, based on the mass of all components other than the aqueous medium of the coating liquid, and is preferably 100 mass% or less, more preferably 95 mass% or less, even more preferably 90 mass% or less, and particularly preferably 80 mass% or less.
[0083] When a silane coupling agent is used, the content of the silane coupling agent is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 20 parts by mass or more, based on 100 parts by mass of the cationic polymer in the coating liquid. The content of the silane coupling agent in the coating liquid is preferably 100 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 30 parts by mass or less, based on 100 parts by mass of the cationic polymer in the coating liquid. The content of the silane coupling agent is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 3% by mass or more, based on the mass of all components other than the aqueous medium of the coating liquid. The content of the silane coupling agent in the coating liquid is preferably 20% by mass or less, more preferably 18% by mass or less, and even more preferably 15% by mass or less, based on the mass of all components other than the aqueous medium of the coating liquid.
[0084] When an antistatic agent is used, the amount of the antistatic agent contained in the coating liquid is preferably 80 mass % or less, more preferably 60 mass % or less, even more preferably 40 mass % or less, and particularly preferably 30 mass % or less, based on the mass of all components of the coating liquid other than the aqueous medium.
[0085] The coating liquid may contain other auxiliary components such as a crosslinking accelerator, an antiblocking agent, a pH adjuster, and a defoaming agent, as necessary.
[0086] The coating liquid can be applied using a coating device such as a die coater, a bar coater, a roll coater, a lip coater, a gravure coater, a spray coater, a blade coater, a reverse coater, or an air knife coater. The amount of the coating liquid to be applied can be appropriately adjusted taking into consideration the thickness of the second functional layer or the fourth functional layer after drying, the concentration of the components contained therein, and the like. The application of the coating liquid and the drying of the coating film may be carried out in-line in accordance with the molding of the laminated resin film, or may be carried out off-line.
[0087] The coating film can be dried using a drying device such as a hot air blower or an infrared dryer. When the coating solution contains a silane coupling agent, it is presumed that drying the coating film advances a dehydration condensation reaction of the silane coupling agent in the coating film, producing a resin that is a reaction product of the silane coupling agent and the cationic water-soluble polymer.
[0088] By the above, a resin sheet according to an embodiment of the present invention having a configuration of second functional layer / first functional layer / substrate, or a resin sheet according to an embodiment of the present invention having a configuration of second functional layer / first functional layer / substrate / third functional layer / fourth functional layer can be obtained.
[0089] <Surface resistivity of resin sheet> In the resin sheet according to the embodiment of the present invention, the surface resistivity of the second functional layer side is preferably 1×10 -1 ~9×10 12 This makes it possible to prevent problems such as blocking between sheets when storing the resin sheets in a rolled or stacked state. The surface resistivity of the second functional layer side is preferably 1×10 11 Ω / sq. or less, more preferably 1×10 10 Ω / sq. or less. In order to adjust the surface resistivity to a desired range, for example, the second functional layer may contain an antistatic agent. In addition, when the resin sheet has a fourth functional layer, it is preferable that the surface resistivity on the fourth functional layer side is also within the above range. The surface resistivity of the resin sheet can be measured in accordance with JIS K6911:1995.
[0090] <Surface free energy of resin sheet> The resin sheet according to the embodiment of the present invention preferably has a surface free energy of 34 to 80 mN / m on the second functional layer side. High surface free energy enhances affinity (wettability) with water, improves the functional expression of the functional agent, and makes it easier to obtain antibacterial and other effects. Furthermore, if the surface free energy on the second functional layer side is within the above range, the second functional layer is more likely to be formed stably. Furthermore, when a printing layer is further provided on the surface of the second functional layer, adhesion to the printing layer is improved. Furthermore, the second functional layer is more likely to be formed stably. In order to adjust the surface free energy to a desired range, for example, the first functional layer may be subjected to a surface treatment such as a corona treatment. In addition, when the resin sheet has a fourth functional layer, it is preferable that the surface free energy on the fourth functional layer side is also within the above range. The surface free energy of the resin sheet can be measured in accordance with JIS K6768:1999.
[0091] <Water vapor permeability coefficient of resin sheet> The resin sheet according to the embodiment of the present invention preferably has a water vapor permeability coefficient of 0.01 to 2.5 gmm / (m 2 ·24hr), and more preferably 0.05 to 2.4 gmm / (m 2 ·24hr), and more preferably 0.1 to 2.3 gmm / (m 2 ·24hr), and particularly preferably 0.5 to 2.2 gmm / (m 2 With a water vapor transmission coefficient in the above range, for example, when the resin sheet is used in a building material laminate described later, it can prevent indoor air from leaking out to the outside in winter and prevent warm, humid air from entering the room in summer, making it easier to maintain a comfortable indoor space without the need for special energy such as air conditioning. In order to set the water vapor transmission coefficient within the desired range, for example, a resin sheet made of a molded thermoplastic resin rather than fibers or the like may be used, or the porosity of the resin sheet may be controlled. The water vapor transmission coefficient of a resin sheet is, for example, measured by the cup method in accordance with JIS-Z-0208:1976 under conditions of a temperature of 40°C and a relative humidity of 90% (g / m2 The thermal expansion coefficient can be calculated by measuring the thermal expansion coefficient (T / 24 hr) and converting it into the thickness of the resin sheet (mm).
[0092] <Applications of resin sheets> INDUSTRIAL APPLICABILITY The resin sheet according to the embodiment of the present invention can fully exhibit functions such as antibacterial properties and also has excellent secondary processability, and is therefore useful as a component of a building material laminate, a reflective sheet for a plant factory, and the like.
[0093] <Building material laminate> Fig. 3 shows a cross-sectional view of a building material laminate according to an embodiment of the present invention. The building material laminate 2 in Fig. 3 has a building material board 20 and a resin sheet 1 according to an embodiment of the present invention provided on one main surface of the building material board 20. As shown in Fig. 3, the second functional layer 12 is placed so as to be the outermost surface. Although not shown, the resin sheet 1 may also be provided on the other main surface of the building material board 20, and in that case, the second functional layer is also placed so as to be the outermost surface.
[0094] Examples of building boards include non-combustible building boards and wood-based building boards. Examples of non-combustible building boards include fiber-reinforced cement boards and metal boards. Examples of fiber-reinforced cement boards include gypsum boards, slag gypsum boards, calcium silicate boards, and flexible boards. Examples of metal boards include galvalume steel plates and aluminum spandrels. Examples of wood-based building boards include plywood boards. The thickness of the building board is preferably about 3 to 20 mm.
[0095] The building material laminate can be produced by bonding the resin sheet according to the embodiment of the present invention to at least one surface of a building material board, for example, via an adhesive. The adhesive can be a protein-based adhesive, a carbohydrate-based adhesive, a synthetic resin-based adhesive, a solvent-based adhesive, or the like.
[0096] In the building material laminate, it is preferable that the second functional layer of the resin sheet is located on the outermost surface from the viewpoint of exerting functions such as antibacterial properties and secondary processability such as printability. The building material laminate can be used as an interior material for a wall, and can constitute a wall together with a heat insulating material, an exterior material, etc.
[0097] In addition, the resin sheet according to the embodiment of the present invention can be used as it is for the reflective sheet for the plant factory. At least one surface of the reflective sheet for the plant factory and the surface of the one main surface side (the side opposite to the side where the building board is provided) of the building material laminate may be printed with various methods. Examples of printing methods include various known methods such as offset printing, gravure printing, flexographic printing, letterpress printing, screen printing, inkjet recording, thermal recording, thermal transfer recording, and electrophotographic recording.
[0098] Based on the above, this specification discloses the following resin sheet and building material laminate. [1] A resin sheet comprising a substrate, a first functional layer provided on one main surface of the substrate and containing a thermoplastic resin and a functional agent, and a second functional layer provided on a surface of the first functional layer and containing a cationic water-soluble polymer, The functional agent includes at least one of calcium hydroxide and a metal carrier, The resin sheet, wherein the second functional layer has a thickness of 0.1 μm or less. [2] The resin sheet according to [1], wherein the content of the cationic water-soluble polymer in the second functional layer is 30 to 100 mass %. [3] The resin sheet according to [1] or [2], wherein the cationic water-soluble polymer contains a quaternary ammonium salt. [4] The surface resistivity of the second functional layer side is 1×10 -1 ~9×10 12 The resin sheet according to any one of [1] to [3], having a surface roughness of Ω / sq. [5] The resin sheet according to any one of [1] to [4], wherein the surface free energy on the second functional layer side is 34 to 80 mN / m. [6] The resin sheet according to any one of [1] to [5], wherein the first functional layer contains the functional agent in an amount of 1 to 30 mass %. [7] The resin sheet according to any one of [1] to [6], wherein the first functional layer is an expanded porous layer. [8] Water vapor permeability coefficient is 0.01 to 2.5 gmm / (m 2 The resin sheet according to any one of [1] to [7], wherein the thermal stability is 24 hours. [9] A building material laminate comprising the resin sheet according to any one of [1] to [8] and a building material board, wherein the second functional layer of the resin sheet is located on the outermost surface. EXAMPLES
[0099] The present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the examples can be appropriately changed without departing from the scope of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.
[0100] The materials used are listed below. Propylene homopolymer (Japan Polypropylene Corporation, product name: Novatec PP FY4, MFR (230°C, 2.16 kg load): 5g / 10 min, melting point: 165°C) Heavy calcium carbonate (manufactured by Bihoku Funka Kogyo Co., Ltd., product name: Softon 1800, average particle size: 1.2 μm) Functional agent: metal carrier (manufactured by Ishizuka Glass Co., Ltd., product name: Ion Pure ZAF HS, average particle size: 1.0 μm) Functional agent: Scallop shell powder (manufactured by Nikken Chemical Laboratory Co., Ltd., product name: Shell Nature, average particle size: 3.0 μm, calcium hydroxide 35% by mass) Cationic water-soluble polymer: polyethyleneimine-based polymer containing primary to tertiary amino groups (manufactured by Mitsubishi Chemical Corporation, product name: Saftomer AC-72) Antistatic agent: Polymer-type antistatic agent (product name: Saftomer ST-3200 (manufactured by Mitsubishi Chemical Corporation), solid content concentration: 25% by mass, quaternary ammonium salt) Silane coupling agent: 3-glycidoxypropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-403) Non-cationic water-soluble polymer (acrylic acid-based polymer): sodium polyacrylate (product name: AQUALIC L DL-453 (manufactured by Nippon Shokubai Co., Ltd.), solid content concentration: 35% by mass)
[0101] <Preparation of Resin Compositions for Substrate, First Functional Layer, and Third Functional Layer> The materials shown in Table 1 were mixed in the ratios shown in Table 1 to prepare resin compositions a to h.
[0102] [Table 1]
[0103] <Preparation Examples 1 to 6: Preparation of Coating Fluid for Second Functional Layer or Fourth Functional Layer> An aqueous solution containing materials of the types and amounts (polymers are calculated as solid contents) shown in Table 2 was prepared as a coating liquid.
[0104] [Table 2]
[0105] <Example 1> Resin composition b was melt-kneaded in an extruder set at 230°C, then fed to an extrusion die set at 250°C and extruded into a sheet, which was then cooled to 60°C by a cooling device to obtain an unstretched sheet. This unstretched sheet was heated to 135°C and stretched 5 times in the machine direction by utilizing the difference in peripheral speed between a group of rolls. Next, the resin composition c was melt-kneaded in an extruder set at 250° C., and then extruded into a sheet shape and laminated onto the first surface of the resin layer made of the above-mentioned resin composition b. Next, resin composition g was melt-kneaded in an extruder set at 250° C., and then extruded into a sheet, which was then laminated onto the second surface of the previously formed resin layer made of resin composition b. In this manner, a laminate sheet was obtained in which three layers, a resin layer made of resin composition g, a resin layer made of resin composition b, and a resin layer made of resin composition c, were laminated. Next, this three-layer laminate sheet was cooled to 60°C, heated to about 150°C using a tenter oven and stretched 8.5 times in the transverse direction, and then further heated to 160°C for heat treatment. The resin sheet was then cooled to 60°C and the edges were slit to obtain a resin sheet having a total thickness of 80μm. In the resin sheet, the layers made of the resin compositions (g / b / c) corresponded to the third functional layer, the substrate layer, and the first functional layer, respectively, and had thicknesses (10μm / 60μm / 10μm) and stretching axial numbers (uniaxial / biaxial / uniaxial). The porosity of the substrate was measured and found to be 35%. 30 W·min / m on both sides of resin sheet 2 After subjecting each surface to a corona discharge treatment under the above conditions, the coating solution prepared in Preparation Example 1 was applied to each surface using a roll coater so that the dry thickness was 0.05 μm. The coating film was dried in an oven at 60° C. to form a second functional layer and a fourth functional layer, thereby obtaining a resin sheet.
[0106] <Examples 2 to 10, Comparative Examples 1 to 6> A resin sheet was obtained in the same manner as in Example 1, except that the conditions such as the type of resin composition, the thickness of each layer, the stretching conditions, and the type of coating liquid were changed to those shown in Table 3.
[0107] [Table 3]
[0108] <Antibacterial test> Antibacterial tests were performed on the second functional layer side surfaces of the resin sheets obtained in the Examples and Comparative Examples according to JIS Z2801 using Staphylococcus aureus and Escherichia coli as test strains. The antibacterial properties were evaluated according to the following criteria using the antibacterial activity values obtained for both test strains. 〇: Antibacterial activity value is 3.0 or higher △: Antibacterial activity value is 2.0 or more and less than 3.0 ×: Antibacterial activity value is less than 2.0 (○ or △ is pass)
[0109] <Anti-mold test> A mold resistance test was performed on the second functional layer side surface of the resin sheets obtained in the Examples and Comparative Examples according to JIS Z2911 (Testing method B for plastic products) using Aspergillus niger, Penicillium pinophilum, paecilomyces variotii, Trichoderma virens, and Cheatomium globosum as test molds. For each test mold, the mold growth state after 4 weeks was compared with that of a biaxially oriented polypropylene film (FOS-AQ, non-corona treated surface, manufactured by Futamura Chemical Co., Ltd.), and the mold resistance was evaluated according to the following criteria. ○: No hypha growth observed △: Mycelium growth is within 1 / 3 of the test piece area ×: The growth of hyphae exceeds 1 / 3 of the test piece area. (○ or △ is pass)
[0110] <Antiviral test> An antiviral test according to ISO 21702 was carried out on the second functional layer side surface of the resin sheets obtained in the Examples and Comparative Examples, using Influenza A virus (H3N2): ATCC VR 167 as the virus. The antibacterial properties were evaluated using the obtained antiviral activity values according to the following criteria. 〇: Antiviral activity value is 3.0 or higher △: Antiviral activity value is 2.0 or more and less than 3.0 ×: Antiviral activity value is less than 2.0 (○ or △ is pass)
[0111] <Printability test> Using a color laser printer (manufactured by Casio Corporation, product name: N4-612II), test images were recorded using four color toners, yellow, cyan, magenta, and black, on the second functional layers of the resin sheets obtained in the Examples and Comparative Examples. Next, the resin sheets on which the test images were recorded were immersed in water (ion-exchanged water) filled in a vat so that the image did not float, and the recorded image was rubbed hard with a coin and visually evaluated according to the following evaluation criteria. ○: No change in recorded image △: Peeling occurs in part of the rubbed area of the recorded image. ×: Peeling occurs over the entire surface of the rubbed portion of the recorded image. (○ or △ is pass)
[0112] <Adhesion test> Silicone-treated glassine paper (G7B, Oji Tack Co., Ltd.) was prepared as a release sheet. A mixture of a solvent-based acrylic adhesive (Oribain BPS1109, Toyochem Co., Ltd.), an isocyanate-based crosslinking agent (Oribain BHS8515, Toyochem Co., Ltd.), and toluene in a ratio of 100:3:45 was applied to the silicone-treated surface of the glassine paper, and the resulting sheet had a basis weight of 25 g / m2 after drying. 2 The mixture was then dried to form an adhesive layer. Next, the resin sheets obtained in the examples and comparative examples were laminated so that the adhesive layer and the fourth functional layer were in contact with each other, and pressure-bonded with a pressure roller to form an adhesive layer on the resin sheet. The release sheet of the adhesive label was peeled off, and the adhesive label was attached to a gypsum board (manufactured by Yoshino Gypsum Co., Ltd., product name "Tiger Board"), and this was stored at room temperature for one week. An adhesive tape (manufactured by Nichiban Co., Ltd., product name "Cellotape (registered trademark)", brand name "CT-18") was applied along the entire length of one of the four sides of the resin sheet to make it easy to hold in the hand, and the resin sheet was peeled off from the gypsum board by pulling the peeled part of the resin sheet while maintaining the angle between the gypsum board surface and the peeled part of the resin sheet at about 135°. The peeling propagation state and peeling force of the resin sheet at this time were evaluated according to the following criteria. 〇: Strong peeling power, peels cleanly over the entire surface △: The peeling strength is a little weak, but the entire surface peels off cleanly. ×: Weak peeling strength (○ or △ is pass)
[0113] <Moisture resistance test> The water vapor permeability coefficient of the resin sheets obtained in the Examples and Comparative Examples was measured, and the moisture proofness was evaluated according to the following criteria. 〇: 5.0g mm / (m 2 ·24hr) or less △: 5.0g·mm / (m 2 ·24hr) Super 10.0g·mm / (m 2 ·24hr) or less ×:10.0g mm / (m 2 ·24hr) super (○ or △ is pass)
[0114] The results of each of the above tests are shown in Table 4 below.
[0115] [Table 4]
[0116] From the above results, the resin sheets of Examples 1 to 10 met the pass criteria in all of the functionality tests for antibacterial properties, antifungal properties, and antiviral properties, and the secondary processability tests for adhesion and printability. Comparison between Examples 1 and 2 and comparison between Examples 3 to 6 shows that functions such as antibacterial properties, antifungal properties, and antiviral properties were improved by increasing the content of the functional agent. In Examples 9 and 10, a coating liquid containing no silane coupling agent was used when forming the second functional layer, so that functionality such as antibacterial properties and secondary processability such as adhesion were slightly reduced, but the pass criteria were met. In the resin sheets of Comparative Examples 1 and 2, the first functional layer did not contain a functional agent, and therefore the antibacterial, antifungal, and antiviral functions were not exhibited. The resin sheet of Comparative Example 3 did not exhibit secondary processability such as adhesiveness, printability, and moisture resistance because it did not have a second functional layer. The resin sheet of Comparative Example 4 was not subjected to a corona discharge treatment, and therefore the second functional layer was not formed in a layer shape, and therefore the secondary processability was insufficient. In the resin sheet of Comparative Example 5, the functional agent was not present in the first functional layer but was present on the surface of the resin sheet, so it absorbed moisture and the cohesive strength of the coating film decreased, resulting in poor adhesion and printability. In the resin sheet of Comparative Example 6, the second functional layer did not contain a cationic water-soluble polymer, and therefore the effect of the functional agent was not fully exerted. [Industrial Applicability]
[0117] The resin sheet according to the embodiment of the present invention is suitable for secondary processing without losing its functions such as antibacterial properties, and is useful for daily necessities, building materials, agricultural products, etc. [Explanation of symbols]
[0118] 1...Resin sheet 10...Base material 11...First functional layer 12...Second functional layer 13...Third functional layer 14...Fourth functional layer 2. Building material laminate 20. Building material board
Claims
1. A resin sheet comprising a substrate, a first functional layer provided on one main surface of the substrate and containing a thermoplastic resin and a functional agent, and a second functional layer provided on a surface of the first functional layer and containing a cationic water-soluble polymer, The functional agent includes at least one of calcium hydroxide and a metal carrier, A resin sheet, wherein the second functional layer has a thickness of 0.1 μm or less.
2. The resin sheet according to claim 1, wherein the content of the cationic water-soluble polymer in the second functional layer is 30 to 100 mass %.
3. The resin sheet according to claim 1 , wherein the cationic water-soluble polymer contains a quaternary ammonium salt.
4. The surface resistivity of the second functional layer side is 1×10 -1 ~9×10 12 The resin sheet according to claim 1 or 2, wherein the elastic modulus is Ω / sq.
5. The resin sheet according to claim 1 or 2, wherein the surface free energy on the second functional layer side is 34 to 80 mN / m.
6. The resin sheet according to claim 1 or 2, wherein the first functional layer contains 1 to 30 mass % of the functional agent.
7. The resin sheet according to claim 1 or 2, wherein the first functional layer is an expanded porous layer.
8. Water vapor permeability coefficient is 0.01 to 2.5 gmm / (m 2 The resin sheet according to claim 1 or 2, wherein the heat resistance is 24 hr.
9. A building material laminate comprising the resin sheet according to claim 1 or 2 and a building material board, wherein the second functional layer of the resin sheet is located on the outermost surface.
Citation Information
Patent Citations
Multifunctional PVC decorative film
CN214137705U
Building lmaterial
JP1978094417A
Destaticizing mildewproofing packaging material
JP1991092347A
Antibacterial fancy paper
JP1998058611A
Interior finishing decorative material
JP1999117410A