Producing method and producing device for fiber-reinforced resin linear material
By stretching and fusing thermoplastic resin yarns through guide holes with a controlled opening area ratio, the method addresses fusion failures and thickness variations in fiber-reinforced resin linear bodies, ensuring stable production and recyclability.
Patent Information
- Application Number
- JP2023056091
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional methods for producing fiber-reinforced thermoplastic resin linear bodies face issues such as fusion failures, splits or tears, and variations in thickness and width, leading to defects in subsequent processes like weaving.
A method involving the stretching and fusing of bundled thermoplastic resin yarns through guide holes with a specific opening area ratio (0.2 to 1.7) under controlled heating conditions, using composite fibers with a sheath-core structure and melting the sheath component to fuse the fibers together.
This approach produces fiber-reinforced resin linear bodies with reduced thickness and width variations, minimizing defects and enhancing process stability while using recyclable materials with low environmental impact.
Smart Images

Figure 2024143421000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method and an apparatus for producing a fiber-reinforced resin linear body in which both the reinforcing fibers and the matrix resin are composed of thermoplastic resin. [Background technology]
[0002] Conventionally, a fiber-reinforced thermoplastic resin linear body has been proposed that aims to reduce the environmental load by forming the reinforcing fibers from a thermoplastic resin without using glass fiber or carbon fiber (see Patent Document 1). The fiber-reinforced thermoplastic resin linear body described in Patent Document 1 has a sheath component and a core component, and is produced by bundling sheath-core type composite spun fibers made of a thermoplastic resin whose melting point is 20°C or more lower than that of the core component, and fusing the sheath component while stretching it at a temperature above the melting point of the sheath component and below the melting point of the core component. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2003-326609 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the conventional manufacturing method described above, poor fusion occurs when the spun fibers are fused together while being stretched, and splits or cracks may occur in the obtained fiber-reinforced resin linear body. In addition, the conventional manufacturing method also has the problem that the thickness and width of the fiber-reinforced resin linear body are likely to vary. If a fiber-reinforced resin linear body having splits or cracks or a fiber-reinforced resin linear body having an inconsistent thickness or width is used to manufacture a product such as a fabric, problems may occur in the subsequent process such as the weaving process, or the product may have a defective appearance.
[0005] Therefore, the present invention aims to provide a manufacturing method and manufacturing apparatus for fiber-reinforced resin linear bodies that suppresses poor fusion between spun fibers and produces fiber-reinforced thermoplastic resin linear bodies with little variation in thickness and width. [Means for solving the problem]
[0006] The method for producing a fiber-reinforced resin linear body according to the present invention includes a draw-fusion process in which a yarn formed by bundling a plurality of spun fibers of one or more types of thermoplastic resin is drawn under heating conditions while the spun fibers are thermally fused to each other, and in the draw-fusion process, the yarn is passed through a guide hole having an opening area ratio (= total cross-sectional area of each spun fiber constituting the yarn / opening area) of 0.2 to 1.7. In the stretch-melting step, the yarn may be passed through a plurality of guide holes. In this case, the opening area of the guide holes may be decreased toward the downstream side in the yarn transport direction. In the method for producing a fiber-reinforced resin linear body of the present invention, for example, the yarn is passed through the guide hole at least once between the start of the stretching and fusing step and the intermediate position. As the spun fiber, for example, a composite fiber obtained by simultaneously extruding two or more thermoplastic resins having different components from a composite nozzle and composite spinning the same can be used. The spun fiber may be a sheath-core type conjugate spun fiber having a sheath component and a core component, the melting point of the sheath component being made of a thermoplastic resin that is 20°C or more lower than the melting point of the core component. In this case, the stretching and fusion step may involve stretching the yarn while melting the sheath component under saturated water vapor pressure at a temperature that is equal to or higher than the melting point of the sheath component and lower than the melting point of the core component, thereby heat-fusing the spun fibers together.
[0007] The manufacturing apparatus for fiber-reinforced resin linear bodies according to the present invention comprises a heating and stretching section which heats and stretches a yarn formed by bundling a plurality of spun fibers made of a thermoplastic resin, and one or more guide members which are installed within the heating and stretching section and have holes for passing the yarn, and the holes of the guide members have an opening area ratio (= total cross-sectional area of each spun fiber constituting the yarn / opening area) of 0.2 to 1.7. Effect of the Invention
[0008] According to the present invention, it is possible to produce a fiber-reinforced thermoplastic resin linear body having little variation in thickness and width while suppressing poor fusion between spun fibers. [Brief description of the drawings]
[0009] [Figure 1] 1 is a flowchart showing a method for producing a fiber-reinforced resin linear body according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram showing a configuration example of a manufacturing apparatus for a fiber-reinforced resin linear body according to an embodiment of the present invention. [Diagram 3] A to C are cross-sectional views showing examples of composite fiber structures, where A is a sheath-core type, B is an eccentric sheath-core type, and C is a side-by-side type. [Figure 4] 1A to 1C are schematic diagrams showing configuration examples of a guide member. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. Note that the present invention is not limited to the following preferred embodiments.
[0011] A method for producing a fiber-reinforced resin linear body according to an embodiment of the present invention is a method for producing a fiber-reinforced thermoplastic resin linear body in which both the reinforcing fibers and the matrix resin are thermoplastic resins, and the thread is passed through a guide hole having an opening area ratio within a specific range when the thread is stretched and fused. The method for producing a fiber-reinforced resin linear body according to the present embodiment can be carried out, for example, by an apparatus for producing a fiber-reinforced resin linear body having a heating and stretching section that heats and stretches a thread formed by bundling a plurality of spun fibers made of a thermoplastic resin, and one or more guide members that are installed in the heating and stretching section and have holes for inserting the thread.
[0012] Fig. 1 is a flow chart showing a method for producing a fiber-reinforced resin linear body according to this embodiment, and Fig. 2 is a diagram showing a configuration example of a manufacturing apparatus for a fiber-reinforced resin linear body for carrying out the manufacturing method shown in Fig. 1. In the manufacturing method for a fiber-reinforced resin linear body according to this embodiment, for example, the melt spinning step S1, the bundling step S2, the stretching and fusing step S3, and the winding step S4 shown in Fig. 1 are carried out by the manufacturing apparatus shown in Fig. 2 to produce a fiber-reinforced thermoplastic resin linear body.
[0013] [Melt spinning process S1] In the melt spinning step S1, a thermoplastic resin is melt-spun using a melt spinning nozzle 1 to obtain a spun fiber 10. The conditions for melt spinning are not particularly limited and can be appropriately selected depending on the type of thermoplastic resin. Here, the thermoplastic resin forming the spun fiber 10 is not particularly limited, but examples that can be used include crystalline polyesters such as polypropylene (PP), polyethylene (PE), polyethylene terephthalate (PET) and polybutylene terephthalate (PBT), and polyamide (PA).
[0014] The structure of the spun fiber 10 is not particularly limited, and may be a single fiber formed of one type of thermoplastic resin, or may be a composite fiber obtained by extruding two or more types of thermoplastic resins from a composite nozzle at the same time and compositely spinning them. Figures 3A to 3C are cross-sectional views showing examples of the composite fiber structure. For example, when the spun fiber 10 is a sheath-core type composite fiber 11 shown in Figure 3A or an eccentric sheath-core type composite fiber 12 shown in Figure 3B, it is preferable to use a resin having a melting point 20°C or more lower for the sheath component (first thermoplastic resin 11a, 12a) than that of the core component (second thermoplastic resin 11b, 12b). When the spun fiber 10 is a side-by-side type composite fiber 13 shown in Figure 3C, it is preferable to use a resin having a melting point 20°C or more lower for the component on one side (first thermoplastic resin 13a) than that of the component on the other side (second thermoplastic resin 13b).
[0015] Here, the first thermoplastic resin 11a, 12a, 13a constituting the composite fibers 11 to 13 may have a melting point lower than that of the second thermoplastic resin 11b, 12b, 13b, and may be, for example, a resin mainly composed of an olefin-based polymer. Examples of the olefin-based polymer include ethylene-based polymers such as high-density, medium-density, and low-density polyethylenes and linear low-density polyethylenes, copolymers of propylene and other α-olefins, specifically propylene-butene-1 random copolymers, propylene-ethylene-butene-1 random copolymers, non-crystalline propylene-based polymers such as soft polypropylene, poly4-methylpentene-1, and the like. In particular, high-density polyethylene is preferable in terms of fiber properties. These olefin-based polymers may be used alone or in combination of two or more.
[0016] On the other hand, as the second thermoplastic resins 11b, 12b, and 13b, for example, polypropylene, polyethylene terephthalate, nylon, etc. can be used, but isotactic polypropylene is preferable from the viewpoints of stretchability, fiber properties, and suppression of thermal shrinkage. These resins may be used alone or in combination of two or more kinds.
[0017] [Focusing process S2] In the bundling step S2, a plurality of spun fibers 10 obtained in the melt spinning step S1 described above are bundled by rod-shaped bundling guides 2 made of ceramic or the like arranged at a predetermined interval to form a thread 20. The thread 20 may be composed of one type of spun fiber 10, but may also be composed of two or more types of spun fibers 10 mixed in a predetermined ratio.
[0018] [Stretch fusion process S3] In the draw-melting step S3, the yarn 20 formed in the bundling step S2 described above is introduced, for example, via an introduction roller 3 into a heating and drawing section 4 equipped with a drawing tank capable of heating the inside with steam or the like, and while drawing under heated conditions, the spun fibers 10 are heat-melted and integrated to obtain a linear body 30. This draw-melting step S3 may be performed under normal pressure, or may be performed under pressurized conditions by pressurizing the inside of the drawing tank.
[0019] In the manufacturing method of the fiber-reinforced resin linear body of the present embodiment, for example, one or more guide members 5 having holes for inserting the yarn 20 are installed in the heat stretching section 4, and the yarn 20 is passed through the holes (guide holes) of the guide members 5 in the stretching and fusing step S3. FIGS. 4A to 4C are schematic diagrams showing configuration examples of the guide members. The configuration of the guide member 5 is not particularly limited, and in addition to the guide member 51 shown in FIG. 4A in which rods 51b are assembled in a lattice pattern and have a rectangular opening (guide hole 51a) in a plan view, a guide member 52 shown in FIG. 4B in which an elliptical or circular opening (guide hole 52a) in a plan view is formed in a plate member 52b, and a guide member 53 shown in FIG. 4C in which a rectangular opening (guide hole 53a) in a plan view is formed in a plate member 53b, can be used.
[0020] In addition, the shape of the guide hole is not limited to the above-mentioned shape, and various shapes such as a rhombus, a trapezoid, a triangle, a polygon, etc. can be adopted in a plan view. If the guide hole has a corner shape in a plan view, it is preferable that the corner is rounded (the corner of the hole is formed with a curved surface).
[0021] Here, the guide holes 51a, 52a, 53a have an opening area ratio R (=total cross-sectional area of each spun fiber 10 constituting the yarn 20 / opening area) of 0.2 to 1.7. If the opening area ratio of the guide holes 51a, 52a, 53a is less than 0.2, the size of the guide holes 51a, 52a, 53a becomes excessively large compared to the thickness of the yarn 20, making it difficult to stably obtain the bundling effect, and making the linear body 30 more likely to split or tear. On the other hand, if the opening area ratio R exceeds 1.7, the size of the guide holes 51a, 52a, 53a becomes excessively small relative to the yarn 20 passing therethrough, increasing the resistance during passage and making it more likely to cause yarn breakage. From the viewpoint of suppressing the oscillation of the traveling yarn 20, the opening area ratio R of the guide holes 51a, 52a, 53a is preferably 0.25 to 1.0.
[0022] The guide member 5 can be made of, for example, ceramic materials such as alumina, metal materials such as stainless steel, copper, zinc, and brass, or metal materials plated with nickel plating on the surface, or various composite materials, but is not limited thereto, and may be made of a material that does not melt or dissolve due to heat or moisture applied in the stretch fusion process. The surface roughness of the guide member 5 is also not particularly limited, but if there are sharp protrusions such as needles in the guide hole, there is a risk that the fibers that come into contact with them will be torn or cut, so it is preferable that there are no such protrusions.
[0023] In the manufacturing method of the fiber-reinforced resin linear body of this embodiment, multiple guide members 5 may be installed in the heating and stretching section 4, and the yarn 20 may be passed through the guide hole multiple times in the stretching and fusing step S3. In this case, it is preferable that the opening area of the guide hole is made smaller toward the downstream side in the yarn transport direction. This reduces the load applied to each fiber during bundling, and can increase the degree of bundling while suppressing fiber breakage.
[0024] It is also preferable that at least one guide member 5 is provided in the first half of the heating and drawing section 4 (upstream in the conveying direction from the intermediate position between the yarn inlet and the yarn outlet). That is, in the draw-melting step S3, it is preferable that the yarn is passed through the guide hole at least once between the start and the intermediate position. This makes it easier for the spun fibers 10 constituting the yarn 20 to be fused together. Furthermore, the heating and drawing section 4 may be provided with multiple draw tanks to perform drawing or draw-melting in multiple stages, in which case it is preferable that the guide member 5 is provided in the draw tank in which the spun fibers 10 are fused together.
[0025] On the other hand, when the spun fibers 10 constituting the thread 20 are sheath-core composite fibers, the draw-fusion step S3 preferably involves melting the sheath component while drawing the thread 20 under saturated water vapor pressure at a temperature equal to or higher than the melting point of the sheath component and lower than the melting point of the core component, thereby heat-fusing the spun fibers 10 together. This allows the sheath component to be melted without melting the core component, thereby ensuring that the spun fibers 10 are reliably fused together.
[0026] [Winding process S4] The linear body 30 formed in the stretch-melting step S3 is drawn out by, for example, a drawing roller 6 and wound up by a winder 7.
[0027] As described above in detail, in the method for producing a fiber-reinforced resin linear body of this embodiment, when the yarn is stretched and melted, the yarn is passed through a guide hole having an opening area ratio of 0.2 to 1.7, so that the degree of bundling of the yarn is improved, the spun fibers can be reliably fused to each other, and the resulting linear body can be prevented from having variations in thickness and width. This makes it possible to produce a fiber-reinforced thermoplastic resin linear body that is free of splits or cracks due to poor fusion of the spun fibers and has little variation in thickness and width.
[0028] By using the fiber-reinforced thermoplastic resin linear body manufactured according to this embodiment, it is possible to manufacture products that are less prone to problems in later processes such as the weaving process and that also have a good appearance. Furthermore, the fiber-reinforced thermoplastic resin linear body manufactured according to this embodiment is easy to recycle and has a small environmental impact because both the reinforcing fibers and the matrix resin are made of thermoplastic resin and no glass fiber or carbon fiber is used. EXAMPLES
[0029] The effects of the present invention will be specifically described below with reference to examples and comparative examples. In these examples, the fiber-reinforced resin linear bodies of the examples and comparative examples were produced by the following method using the production apparatus shown in Fig. 2, and the variations in thickness and width were evaluated.
[0030] Specifically, first, a core component was made of polypropylene with a melt flow rate (MFR) of 18 g / 10 min at 230°C, and a sheath component was made of linear low density polyethylene (LLDPE) with a MFR of 6.3 g / 10 min at 230°C. Using a conventional conjugate spinning apparatus and a core-sheath conjugate spinning nozzle (number of holes: 480), a sheath-core conjugate fiber with the structure shown in FIG. 3A was melt-spun. The spinning temperature was 250°C, and the core-sheath ratio was 65 / 35 in cross-sectional ratio. The obtained spun fibers (sheath-core conjugate fibers) were bundled into a yarn, which was then stretched and fused in the heating and stretching section 4 to produce a fiber-reinforced linear body 30 with a fineness of about 1850 dtex.
[0031] <Example 1> 4A were installed at three locations: a front portion within 2 m from the yarn inlet of the heating and drawing section 4, a central portion within 1 m from the midpoint between the inlet and the outlet, and a rear portion within 2 m from the outlet, and the yarn was passed through the guide holes three times in the drawing and melt-bonding process to produce a fiber-reinforced linear body. At that time, the total length of the heating and drawing section 4 was 10 m, and the opening area ratio R of each guide member 51 was 1.7.
[0032] <Example 2> A fiber-reinforced linear body was produced in the same manner and under the same conditions as in Example 1 described above, except that the opening area ratio R of the guide member 51 installed in the front portion was changed to 0.25 and the guide member 51 in the rear portion was removed.
[0033] <Example 3> A fiber-reinforced linear body was produced in the same manner and under the same conditions as in Example 1 described above, except that the guide member 51 in the front portion was removed and the yarn was passed through guide holes in the central and rear portions.
[0034] <Example 4> A fiber-reinforced linear body was produced in the same manner and under the same conditions as in Example 1 described above, except that the guide members 51 in the front and rear portions were removed and the yarn was passed through the guide hole only in the central portion.
[0035] <Example 5> A fiber-reinforced linear body was produced in the same manner and under the same conditions as in Example 1 described above, except that the opening area ratio R of the guide member 51 installed in the front portion was changed to 0.2 and the guide member 51 in the central portion was removed.
[0036] <Example 6> A fiber-reinforced linear body was produced in the same manner and under the same conditions as in Example 1 described above, except that the guide members 51 in the central and rear portions were removed and the yarn was passed through the guide hole only in the front portion.
[0037] <Example 7> A fiber-reinforced linear body was produced in the same manner and under the same conditions as in Example 1 described above, except that the guide members 51 in the front and central portions were removed and the yarn was passed through the guide hole only in the rear portion.
[0038] <Comparative Example 1> A fiber-reinforced linear body was produced in the same manner and under the same conditions as in Example 1 described above, except that the opening area ratios R of the guide members 51 installed in the front, center, and rear portions were all set to 0.1.
[0039] <Comparative Example 2> A fiber-reinforced linear body was produced in the same manner and under the same conditions as in Example 1 described above, except that the opening area ratios R of the guide members 51 installed in the front, center, and rear portions were all set to 2.0.
[0040] <Comparative Example 3> A fiber-reinforced linear body was produced in the same manner and under the same conditions as in Comparative Example 2 described above, except that the guide member 51 in the rear portion was removed and the yarn was passed through the guide holes in the front and central portions.
[0041] <Comparative Example 4> A fiber-reinforced linear body was produced in the same manner and under the same conditions as in Comparative Example 2 described above, except that the guide member 51 in the front portion was removed and the yarn was passed through guide holes in the central and rear portions.
[0042] <Comparative Example 5> A fiber-reinforced linear body was produced in the same manner and under the same conditions as in Example 1 described above, except that the guide member 51 was not provided and the stretching and melting were carried out.
[0043] [evaluation] The thread width of the linear bodies produced in the examples and comparative examples was measured with a vernier caliper. The number of evaluations per test piece was 30, and the number of test pieces used for evaluation was 2 or more. The standard deviation of the thread width was calculated based on the measured values. As a result, those with a maximum value of 0.25 or less were evaluated as ○ (pass), and those with a maximum value of more than 0.25 were evaluated as × (fail).
[0044] The results are shown in Tables 1 and 2 below.
[0045] [Table 1]
[0046] [Table 2]
[0047] As shown in Table 2 above, in Comparative Example 1, in which the opening area ratio of the guide hole was less than 0.2, and in Comparative Example 5, in which the yarn was not passed through the guide hole, the maximum standard deviation of the yarn width of the produced linear bodies was 0.3 or more, and the width variation was large. In addition, in Comparative Examples 2 to 4, in which the opening area ratio of the guide hole exceeded 1.7, yarn breakage occurred and linear bodies could not be produced. In contrast, the linear bodies of Examples 1 to 7 produced within the scope of the present invention had small variation in yarn width and did not suffer from splits or tears.
[0048] From the above results, it was confirmed that according to the present invention, poor fusion between spun fibers can be suppressed and a fiber-reinforced thermoplastic resin linear body with little variation in thickness and width can be obtained.
[0049] The present invention can also have the following configuration. [1] The method includes a stretching and fusing step of stretching a yarn formed by bundling a plurality of spun fibers of one or more types of thermoplastic resin under heating conditions while heat fusing the spun fibers together, A method for producing a fiber-reinforced resin linear body, in which the yarn is passed through a guide hole having an opening area ratio (=total cross-sectional area of each spun fiber constituting the yarn / opening area) of 0.2 to 1.7 in the stretching and fusing step. [2] The method for producing a fiber-reinforced resin linear body according to [1], wherein in the stretching and fusing step, the yarn is passed through a plurality of guide holes. [3] The method for producing a fiber-reinforced resin linear body according to [2], wherein the opening area of the guide hole is made smaller toward the downstream side in the yarn transport direction. [4] The method for producing a fiber-reinforced resin linear body according to any one of [1] to [3], wherein the yarn is passed through the guide hole at least once between the start of the stretching and fusing step and an intermediate position. [5] The method for producing a fiber-reinforced resin linear body according to any one of [1] to [4], wherein the spun fiber is a composite fiber obtained by simultaneously extruding two or more thermoplastic resins having different components from a composite nozzle and subjecting them to composite spinning. [6] The spun fiber is a sheath-core type composite spun fiber having a sheath component and a core component, the melting point of the sheath component being made of a thermoplastic resin that is 20°C or more lower than the melting point of the core component, The method for producing a fiber-reinforced resin linear body according to [5], in the stretch-fusion step, the yarn is stretched while melting the sheath component at a temperature equal to or higher than the melting point of the sheath component and lower than the melting point of the core component under saturated water vapor pressure, thereby heat-fusing the spun fibers together. [7] a heating and drawing section for heating and drawing a yarn formed by bundling a plurality of spun fibers made of a thermoplastic resin; one or more guide members provided in the heating and stretching section and having a hole for inserting the yarn therethrough; The hole of the guide member has an opening area ratio (=total cross-sectional area of each spun fiber constituting the thread / opening area) of 0.2 to 1.7. [8] A plurality of guide members having different opening areas are provided in the heating and stretching section, The manufacturing apparatus for a fiber-reinforced resin linear body described in [7], wherein the multiple guide members are arranged so that the opening area becomes smaller toward the downstream side in the conveying direction. [9] The method for producing a fiber-reinforced resin linear body according to [7] or [8], wherein at least one guide member is disposed in the heating and stretching section upstream in the conveying direction of a midpoint between an inlet and an outlet of the yarn.
[10] The method for producing a fiber-reinforced resin linear body according to any one of [7] to [9], wherein the heating and stretching section is a steam stretching device. [Explanation of symbols]
[0050] 1. Melt spinning nozzle 2. Focusing Guide 3. Introduction roller 4 Heated stretching section 5, 51, 52, 53 Guide members 6 Drawer Rollers 7 Winder 10 Spun fibers 11~13 Composite Fiber 11a, 12a, 13a 1st thermoplastic resin 11b, 12b, 13b Second thermoplastic resin 20 Thread 30 linear body 51a, 52a, 53a Guide holes 51b Bar material 52b, 53b plate material
Claims
1. The method includes a stretch-and-bond process in which a yarn formed by bundling a plurality of spun fibers of one or more types of thermoplastic resin is stretched under heating conditions to thermally bond the spun fibers to each other, In the stretch-fusion step, the yarn is passed through a guide hole having an opening area ratio (=total cross-sectional area of each spun fiber constituting the yarn / opening area) of 0.2 to 1.
7.
2. The method for producing a fiber-reinforced resin linear body according to claim 1 , wherein in the stretch-fusion step, the yarn is passed through a plurality of guide holes.
3. The method for producing a fiber-reinforced resin linear body according to claim 2 , wherein an opening area of the guide hole is decreased toward a downstream side in a yarn transport direction.
4. The method for producing a fiber-reinforced resin linear body according to claim 1 , wherein the yarn is passed through the guide hole at least once during the period from the start of the stretch-fusion step to an intermediate position.
5. 2. The method for producing a fiber-reinforced resin linear body according to claim 1, wherein the spun fiber is a composite fiber obtained by simultaneously extruding two or more thermoplastic resins having different components from a composite nozzle and composite spinning the resins.
6. The spun fiber is a sheath-core type composite spun fiber having a sheath component and a core component, the melting point of the sheath component being made of a thermoplastic resin that is 20° C. or more lower than the melting point of the core component, 6. The method for producing a fiber-reinforced resin linear body according to claim 5, wherein in the stretch-fusion step, the yarn is stretched while melting the sheath component at a temperature equal to or higher than the melting point of the sheath component and lower than the melting point of the core component under saturated water vapor pressure, thereby thermally fusing the spun fibers together.
7. a heating and drawing section for heating and drawing a yarn formed by bundling a plurality of spun fibers made of a thermoplastic resin; one or more guide members provided in the heating and stretching section and having a hole for inserting the yarn therethrough; The hole of the guide member has an opening area ratio (=total cross-sectional area of each spun fiber constituting the yarn / opening area) of 0.2 to 1.7.
Citation Information
Patent Citations
Linear or rod-shaped composite material made of fiber- reinforced thermoplastic resin and its manufacturing method
JP2003326609A