Welding method and welding device
The described welding method for aluminum-based materials uses dual-wavelength laser beams and wobbling to stabilize the molten pool, reducing blowholes and spatter, resulting in high-quality welds.
Patent Information
- Application Number
- JP2023056490
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Welding aluminum-based materials poses challenges due to increased likelihood of blowholes and spatter formation, necessitating an improved welding method and apparatus.
A welding method using a combination of laser beams with specific wavelengths (800-1200 nm and 550 nm or less) and wobbling technique, along with a beam shaper to form multiple spots, maintains a keyhole in an open state, and adjusts power ratios and wobbling parameters to enhance weld quality.
The method effectively reduces blowholes and spatter, ensuring strong and conductive welds in aluminum-based materials by maintaining a stable molten pool and facilitating air bubble escape.
Smart Images

Figure 2024143700000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a welding method and a welding apparatus. [Background technology]
[0002] 2. Description of the Related Art Conventionally, there has been known a welding method in which a laser beam is scanned and irradiated onto the surfaces of a plurality of members made of an aluminum-based material to weld the plurality of members (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2018 / 181724 Summary of the Invention [Problem to be solved by the invention]
[0004] In this type of welding, it is important not only to secure the required joint strength, but also to prevent welding defects such as spatters and blowholes. Through extensive research by the inventors, it was discovered that blowholes are more likely to occur in aluminum-based materials than in other materials.
[0005] Therefore, one object of the present invention is to provide a new and improved welding method and welding apparatus capable of welding a plurality of components, for example, made of an aluminum-based material, by scanning a laser beam over the surface of the workpiece to be processed and welding the plurality of components. [Means for solving the problem]
[0006] The welding method of the present invention is a welding method for welding a plurality of components, for example, made of an aluminum-based material, by scanning a surface of a workpiece to be processed with a laser beam, the surface including the components being processed, the laser beam including a first laser beam having a wavelength of 800 nm or more and 1200 nm or less, and a second laser beam having a wavelength of 550 nm or less, the laser beam being irradiated onto the surface while being wobbled.
[0007] In the welding method, the second laser light may have a wavelength of not less than 380 [nm] and not more than 500 [nm].
[0008] In the welding method, the first laser light may be split into a plurality of beams to form a plurality of spots on the surface.
[0009] In the welding method, the first laser beam may be split into a plurality of beams using a beam shaper.
[0010] In the welding method, the beam shaper may be a diffractive optical element.
[0011] In the welding method, the first laser light may include a central laser light and peripheral laser light surrounding the central laser light, and a ratio of a power of the central laser light to a power of the peripheral laser light may be 1 / 4 or more and 7 / 3 or less.
[0012] In the welding method, the moving speed of the wobbling center of the laser light may be 100 mm / s or less.
[0013] In the welding method, a wobbling frequency of the laser light may be 300 Hz or more.
[0014] In the welding method, a wobbling speed of the laser beam may be 100 [mm / s] or less, and a wobbling frequency of the laser beam may be 300 [Hz] or more.
[0015] In the welding method, the overlap rate R of the wobbling is calculated by the following formula (1): R = 2 × (Ae - Aw) / Ae (1) Here, when Aw is defined as the area of a region which is the sum of a first ellipse whose major axis is the distance between the position where the scanning path for one wobbling rotation is first located on the movement path of the wobbling center and the position where the scanning path for one wobbling rotation next is located on said movement path and the minor axis is the wobbling diameter, and a second ellipse whose major axis is the distance between the position where the scanning path for the next one wobbling rotation is first located on said movement path and the position where the scanning path for one wobbling rotation next is located on said movement path and the minor axis is the wobbling diameter, and Ae is defined as the sum of the area of the first ellipse and the area of the second ellipse, R may be greater than or equal to 0.51.
[0016] In the welding method, a keyhole may be formed in a molten pool formed by irradiation of the laser light, and the keyhole may be maintained in an open state without being intermittently closed.
[0017] The welding apparatus of the present invention is a welding method for welding a surface of a workpiece, for example including a plurality of components made of an aluminum-based material, by irradiating and scanning a laser beam onto the surface of the workpiece to weld the plurality of components, the laser beam including a first laser beam having a wavelength of 800 nm or more and 1200 nm or less and a second laser beam having a wavelength of 550 nm or less, the laser beam being irradiated onto the surface while being wobbled, the welding apparatus having an optical head for outputting the laser beam toward the surface, the optical head having a laser scanner. Effect of the Invention
[0018] According to the present invention, it is possible to obtain a new and improved welding method and welding apparatus capable of welding a plurality of components, for example, made of an aluminum-based material, by scanning the surface of the workpiece while irradiating the surface with a laser beam and welding the plurality of components. [Brief description of the drawings]
[0019] [Figure 1]FIG. 1 is an exemplary schematic configuration diagram of a laser welding device according to an embodiment. [Diagram 2] FIG. 2 is an explanatory diagram showing the concept of the principle of the diffractive optical element included in the laser welding apparatus of the embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing an example of a laser beam spot formed on the surface of the processing object by the laser welding apparatus of the embodiment. [Figure 4] FIG. 4 is a cross-sectional view (photographic image) of an example of a processed object on which a weld is formed by the laser welding device of the reference example. [Diagram 5] FIG. 5 is a cross-sectional view (photographic image) of an example of a processed object on which a weld is formed by the laser welding device of the embodiment. [Figure 6] FIG. 6 is an explanatory diagram of a wobbling operation on the surface of a processing object by the laser welding device of the embodiment. [Figure 7] FIG. 7 is a schematic diagram showing an example of a scanning path of a laser light spot on the surface of an object to be processed by the laser welding device of the reference example. [Figure 8] FIG. 8 is a schematic diagram showing an example of a scanning path of a laser light spot on the surface of an object to be processed by the laser welding apparatus of the embodiment. [Figure 9] FIG. 9 is a diagram illustrating the overlap rate of the wobbling on the surface of the object to be processed by the laser welding device of the embodiment. [Figure 10] FIG. 10 is an explanatory diagram showing an example of a welding result corresponding to a moving speed of the wobbling center and a numerical range of the wobbling frequency in the wobbling operation of the laser welding device of the embodiment. [Figure 11] FIG. 11 is a schematic diagram showing an example of a laser light spot formed on the surface of an object to be processed by the laser welding apparatus of the embodiment. [Figure 12] FIG. 12 is a schematic diagram showing an example of a laser light spot formed on the surface of the processing object by the laser welding apparatus of the embodiment. [Figure 13]FIG. 13 is a schematic diagram showing an example of a laser light spot formed on the surface of the processing object by the laser welding apparatus of the embodiment. [Figure 14] FIG. 14 is a graph showing an example of power density distribution on a line passing through the center and extending in the width direction of a laser beam spot formed on the surface of an object to be processed by the laser welding device of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Exemplary embodiments of the present invention are disclosed below. The configurations of the embodiments shown below, and the actions and results (effects) brought about by the configurations are merely examples. The present invention can be realized by configurations other than those disclosed in the following embodiments. Furthermore, according to the present invention, it is possible to obtain at least one of the various effects (including derivative effects) obtained by the configurations.
[0021] In this specification, ordinal numbers may be given for convenience to distinguish directions, members, parts, laser beams, shapes, etc. Note that ordinal numbers do not indicate a priority order or sequence, and do not specify a number.
[0022] In this specification, ordinal numbers may be given for convenience to distinguish between parts, members, parts, laser beams, directions, etc. Note that ordinal numbers do not indicate a priority or order, and do not specify a number.
[0023] In each figure, the X direction is represented by an arrow X, the Y direction is represented by an arrow Y, and the Z direction is represented by an arrow Z. The X direction, Y direction, and Z direction intersect with each other and are perpendicular to each other. The scanning direction SD of the laser light spot is represented by an arrow SD, and the width direction WD perpendicular to the scanning direction is represented by an arrow WD.
[0024] [Embodiment] Fig. 1 is a schematic configuration diagram of a laser welding apparatus 100 according to an embodiment. As shown in Fig. 1, the laser welding apparatus 100 includes a laser device 111, a laser device 112, an optical head 120, an optical fiber 130, and a movement mechanism 140. The laser welding apparatus 100 is an example of a welding apparatus.
[0025] As shown in FIG. 1, the workpiece W is a metal member 11 made of an aluminum-based material and a metal member 12 made of an aluminum-based material stacked in the Z direction. The laser welding device 100 irradiates a surface Wa of the workpiece W facing the Z direction with a laser beam L approximately along the opposite direction of the Z direction, thereby forming a welded portion 14 that penetrates the metal member 11 from the surface Wa in the opposite direction of the Z direction to the metal member 12. This results in a joined body 10 in which the metal members 11 and 12 are joined via the welded portion 14. That is, the joined body 10 has the metal members 11, 12, and the welded portion 14. In addition, when the metal members 11 and 12 are conductors, the metal members 11 and 12 are electrically connected via the welded portion 14 in the joined body 10.
[0026] The laser devices 111 and 112 each have a laser oscillator and are configured to be able to output laser light with a power of, for example, several kW. The laser devices 111 and 112 emit laser light with a wavelength of 380 [nm] or more and 1200 [nm] or less. The laser devices 111 and 112 each have a laser light source therein, such as a fiber laser, a semiconductor laser (element), a YAG laser, or a disk laser. The laser devices 111 and 112 may be configured to output multi-mode laser light with a power of several kW as the sum of the outputs of the multiple light sources.
[0027] The laser device 111 outputs a first laser beam having a wavelength of 800 nm or more and 1200 nm or less. The laser device 111 is an example of a first laser device. As an example, the laser device 111 has a fiber laser or a semiconductor laser (element) as a laser light source. The first laser beam mainly contributes to forming a keyhole in the molten pool.
[0028] On the other hand, the laser device 112 outputs a second laser light having a wavelength of 550 [nm] or less. The laser device 112 is an example of a second laser device. As an example, the laser device 112 has a semiconductor laser (element) as a laser light source. The laser device 112 preferably outputs a second laser light having a wavelength of 380 [nm] or more and 500 [nm] or less. The second laser light having a shorter wavelength than the first laser light has a higher absorption rate for the metal members 11, 12 than the first laser light, and accordingly, the metal members 11, 12 can be heated more efficiently. Therefore, by irradiating the second laser light together with the first laser light, it is possible to obtain an effect that the temperature change depending on the location in the molten pool and its surrounding area can be mitigated and the movement of the molten pool can be suppressed and stabilized, compared to the case where the first laser light is irradiated alone.
[0029] The optical fibers 130 guide the laser beams output from the laser devices 111 and 112 to the optical head 120 .
[0030] The optical head 120 is an optical device for irradiating the laser light input from the laser devices 111 and 112 toward the processing object W. The optical head 120 includes a collimator lens 121, a condenser lens 122, a mirror 123, a dichroic mirror 124, and a DOE 125. The collimator lens 121, the condenser lens 122, the mirror 123, the dichroic mirror 124, and the DOE 125 may also be referred to as optical components.
[0031] The optical head 120 is configured to be able to change its relative position with respect to the workpiece W in order to scan the laser light L while irradiating the laser light L on the surface Wa of the workpiece W. The relative movement between the optical head 120 and the workpiece W can be achieved by moving the optical head 120 by the moving mechanism 140, moving the workpiece W by a moving stage (not shown) or the like, or moving both the optical head 120 by the moving mechanism 140 and the workpiece W by a moving stage or the like. The moving mechanism 140 and the moving stage can also be referred to as a scanning mechanism.
[0032] The collimating lenses 121 (121-1, 121-2) each collimate the laser light input via the optical fiber 130. The collimated laser light becomes parallel light.
[0033] Mirror 123 reflects the first laser light that has been collimated by collimator lens 121-1. The first laser light reflected by mirror 123 travels in the opposite direction to the X direction toward dichroic mirror 124. Note that in a configuration in which the first laser light is input to optical head 120 so as to travel in the opposite direction to the X direction, mirror 123 is not necessary.
[0034] The DOE 125 can appropriately shape the beam shape of the first laser light, and therefore can appropriately shape the arrangement and shape of the spots on the surface Wa. As conceptually illustrated in FIG. 2, the DOE 125 has a configuration in which, for example, a plurality of diffraction gratings 125a with different periods are superimposed. The DOE 125 can shape the beam shape by bending the parallel light in a direction influenced by each diffraction grating 125a or by superimposing the diffraction gratings 125a. The DOE 125 is an example of a beam shaper.
[0035] The optical head 120 may have a beam shaper provided after the collimator lens 121-2 to adjust the beam shape of the second laser light, or a beam shaper provided after the dichroic mirror 124 to adjust the beam shapes of both the first laser light and the second laser light. By appropriately adjusting the beam shape of the laser light L with the beam shaper, the occurrence of spatters and blowholes during welding can be further suppressed.
[0036] The dichroic mirror 124 is a high-pass filter that transmits the first laser light and reflects but does not transmit the second laser light. The first laser light passes through the dichroic mirror 124 and travels in the opposite direction of the X direction toward the galvano scanner 126. On the other hand, the dichroic mirror 124 reflects the second laser light that has been collimated by the collimator lens 121-2. The second laser light reflected by the dichroic mirror 124 travels in the opposite direction of the X direction toward the galvano scanner 126.
[0037] The galvano scanner 126 has two mirrors 126a and 126b, and is a device that can move the irradiation position of the laser light L and scan the laser light L without moving the optical head 120 by controlling the angles of the two mirrors 126a and 126b. The angles of the mirrors 126a and 126b are changed by, for example, a motor (not shown). The galvano scanner 126 is an example of a laser scanner and can also be called a scanning mechanism. Note that the laser scanner is not limited to the galvano scanner 126.
[0038] The condenser lens 122 condenses the first laser light and the second laser light as parallel light, and irradiates the object W to be processed with the condensed light as laser light L (output light).
[0039] Fig. 3 is a plan view showing an example of a spot S formed on a surface Wa by irradiation with a laser beam L. The spot S including a plurality of spots S1 and S2 shown in Fig. 3 is formed by a DOE 125. In the example of Fig. 3, a beam of a first laser beam is split into a plurality of beams via the DOE 125, and a single spot S11 located on the optical axis of the laser beam L and a plurality of spots S12 arranged at approximately equal intervals in a ring shape around the optical axis are formed on the surface Wa by the plurality of beams. The laser beam forming the spot S1 is referred to as a central laser beam of the first laser beam, and the laser beam forming the spot S12 is referred to as a peripheral laser beam of the first laser beam.
[0040] The beam forming spot S1 and the beam forming spot S2 each have, for example, a Gaussian shape, a flat-top shape, or other shapes (power distribution) in the radial direction of a cross section perpendicular to the optical axis direction of the beam. Note that in each diagram, as in Figure 3, in which the spots S1 and S2 of each beam are represented by circles on the surface Wa, the diameter of the circle representing the spots S1 and S2 is the spot diameter. Each spot diameter includes the peak of the spot and is 1 / e of the peak intensity. 2 It can be defined as the diameter of the region with an intensity of 1 / e of the peak intensity in the case of a non-circular spot, which is not shown in the figure. 2 The length of the region having the above intensity in the width direction WD that intersects with and is perpendicular to the Z direction and the scanning direction SD can be defined as the spot width.
[0041] In the example of FIG. 3, the spot S2 formed by the beam of the second laser light is formed such that the multiple spots S1 based on the first laser light are positioned inside the outer edge of the spot S2.
[0042] [Welding method] In welding using the laser welding device 100, first, the workpiece W having the metal members 11 and 12 is set (temporarily fixed) on a support device (not shown) or the like so that the workpiece W is in a position and posture where the laser light L is irradiated onto the surface Wa. Then, while the laser light L is irradiated onto the surface Wa, the scanning mechanism is operated to relatively move the laser light L and the workpiece W in a direction intersecting the Z direction. As a result, the laser light L moves (scans) on the surface Wa in the scanning direction SD while being irradiated onto the surface Wa. A molten pool is formed in the portion of the workpiece W irradiated with the laser light L. Thereafter, the molten pool solidifies as the temperature decreases, and the metal members 11 and 12 are welded together, and a joint 10 is obtained.
[0043] [Weld cross section] Fig. 4 is a cross-sectional view along the Z direction and the scanning direction SD of a reference example workpiece W on which a weld 14 is formed. As shown in Fig. 4, it was found that when the metal members 11 and 12 are made of an aluminum-based material, blowholes H are more likely to occur at a relatively deep position in the weld 14 than when the metal members 11 and 12 are made of a copper-based material, and a large number of blowholes H are formed if the welding conditions are not set appropriately. It was also confirmed that in such a case, the amount of spatter scattering during welding also increases.
[0044] 5 is a cross-sectional view along the Z direction and the scanning direction SD of the workpiece W in the embodiment in which a weld 14 is formed. Through intensive research by the inventors, it has been found that even when the metal members 11 and 12 are made of an aluminum-based material, a preferable joined body 10 with few blowholes H in the weld 14 can be obtained by appropriately setting the welding conditions. It has also been confirmed that in such a case, the scattering of spatter during welding can be significantly reduced.
[0045] The following describes welding conditions that make it possible to obtain a favorable weld 14 and joint 10 as shown in Fig. 5. The quality of the joint 10 can be determined based on, for example, the number of blowholes H per unit length in the scanning direction SD of the weld 14.
[0046] [Wobbling overlap rate] The inventors have found through extensive research that the wobbling action of the spot S on the surface Wa is highly effective.
[0047] FIG. 6 shows a scanning path Pc of the spot S (see FIG. 3) formed by irradiation of the laser light L on the surface Wa in a coordinate system fixed to the optical head 120 when the spot S is scanned while being wobbled. The spot S of the laser light L is scanned on a circumference of a wobbling radius Rw and a wobbling diameter Dw by a substantially uniform circular motion around the wobbling center Cw by the operation of the galvano scanner 126. That is, the scanning path Pc is circular. Also, by the operation of a scanning mechanism such as the moving mechanism 140, the wobbling center Cw moves at a moving speed Vc along a moving path Ptc along the surface Wa. Note that the moving path Ptc has a linear shape in the example of FIG. 6, but is not limited to a linear shape. The moving path Ptc determines the shape of the bead of the weld 14 formed on the surface Wa.
[0048] FIG. 7 is a plan view showing a scanning path Pt of the spot S on the surface Wa of the workpiece W of the reference example. FIG. 8 is a plan view showing a scanning path Pt of the spot S on the surface Wa of the workpiece W of the embodiment. Due to the rotational motion of the spot S and the translational motion of the wobbling center Cw as shown in FIG. 6, the spot S is scanned in a spiral shape on the surface Wa as shown in FIGS. 7 and 8. In other words, the scanning path Pt of the spot S has a spiral shape. The scanning direction SD is the moving direction of the wobbling center Cw, in other words, the extension direction of the moving path Ptc of the wobbling center Cw.
[0049] In the scanning path Pt in Figure 7, many blowholes H occurred and a lot of spattering occurred, as shown in the cross section of Figure 4. In contrast, in the scanning path Pt in Figure 8, there were fewer blowholes H and less spattering, as shown in the cross section of Figure 5. This is presumably because, compared to the scanning path Pt in Figure 7, the degree of overlap between one wobbling revolution and the next is higher in the scanning path Pt in Figure 8, and the molten state of the molten pool is maintained for a longer period of time, making it easier for bubbles to escape.
[0050] FIG. 9 is a plan view for explaining the overlap rate between one rotation of wobbling and the next rotation of wobbling. Here, for simplicity, the scanning path Pt of the spot S for two consecutive rotations of wobbling is replaced with two ellipses (a first ellipse E1 and a second ellipse E2). The first ellipse E1 is an ellipse whose major axis is the distance D1 between a position P11 where the scanning path Pt for one rotation of wobbling is first located on the moving path Ptc of the wobbling center Cw and a position P12 where the scanning path Pt for one rotation of wobbling is next located on the moving path Ptc, and whose minor axis is the wobbling diameter Dw. The second ellipse E2 is an ellipse whose major axis is the distance D2 between a position P21 where the scanning path Pt for the next rotation of wobbling is first located on the moving path Ptc and a position P22 where the scanning path Pt for one rotation of wobbling is next located on the moving path Ptc, and whose minor axis is the wobbling diameter Dw. Then, the overlap rate R of the wobbling is calculated by the following formula (1). R = 2 × (Ae - Aw) / Ae (1) Here, Aw is the area of the sum of the first ellipse E1 and the second ellipse E2 (the hatched area in FIG. 9), and Ae is the sum of the area of the first ellipse E1 and the area of the second ellipse E2.
[0051] According to the experimental analysis by the inventors, when the overlap rate R of the wobbling is defined as in the formula (1), when R≧0.51, it is found that a state close to the cross section in Fig. 5, i.e., a preferable joint 10 with few blowholes H in the welded part 14 and satisfying the predetermined conditions of mechanical strength and electrical conductivity, can be obtained, and spatter is also reduced to a level that satisfies the predetermined conditions for not affecting the surroundings. It was also found that when R≧0.82, it is found that the state of the cross section in Fig. 5, i.e., the best state with almost no blowholes H in the welded part 14 and extremely little scattering of spatter, can be obtained.
[0052] [Wobbling center movement speed and wobbling frequency] 10 is a graph showing welding results corresponding to the moving speed Vc of the wobbling center Cw and the numerical range of the wobbling frequency. Here, the wobbling frequency is 1 / tw, where tw is the time required for one wobbling rotation of the spot S, that is, one rotation of the scanning path Pc in FIG. 6.
[0053] The inventors' experimental analysis revealed that, as shown in Fig. 10, it is preferable (good) for the moving speed Vc of the wobbling center Cw to be 100 [mm / s] or less, and it is preferable (good) for the wobbling frequency to be 300 [Hz] or more. This is presumably because the lower the moving speed Vc, the larger the overlap rate R, and the higher the wobbling frequency, the larger the overlap rate R. This allows the molten state of the molten pool to be maintained for a longer period of time, which makes it easier for bubbles to escape. It was also found that, as shown in Fig. 10, it is even more preferable (best) for the moving speed Vc of the wobbling center Cw to be 100 [mm / s] or less and the wobbling frequency to be 300 [Hz] or more.
[0054] [Spot shape] 11 to 13 are plan views illustrating patterns of the spots S of the laser light L on the surface Wa. It has been found that, in addition to the pattern shown in FIG. 3, the patterns shown in FIGS. 11 to 13 also provide a preferable joint 10 with few blowholes H in the welded portion 14. As shown in FIGS. 11 to 13, the shape of the spot S2 by the second laser light can be various shapes such as a circle, a square, an ellipse, and an oval (not shown). In addition, the shape, arrangement, number, and other specifications of the spots S1 by the first laser light and the spots S2 by the second laser light can be changed in various ways. In any case, the size (diameter, width, area) of the spot S2 is preferably larger than the size (diameter, width, area) of the spot S1.
[0055] Further, according to an experimental analysis by the inventors, regarding the ratio of the power of the central laser light of the first laser light forming the spot S11 illustrated in FIG. 3 to the power of the peripheral laser light of the first laser light forming the spot S12 illustrated in FIG. 3 (hereinafter referred to as the power ratio), (1) If the power ratio is too high, a deep molten pool can be formed, but the amount of melt around it decreases, so there is not enough time for the blowhole to escape from the molten pool. (2) If the power ratio is too low, it is difficult to form a deep molten pool, and it can only be applied to thin workpieces. From this viewpoint, the inventors have found that the power ratio is preferably 1 / 4 or more and 7 / 3 or less. Note that the spot pattern of the central laser light and the peripheral laser light is not limited to the example of FIG.
[0056] [Intensity distribution within the spot] Fig. 14 is a graph showing an example of the power density distribution on a line passing through the center C1 and extending in the width direction of the spot S of the laser light L formed on the surface Wa. The inventors' experimental analysis revealed that it is preferable for the power density to have a peak at the center and a so-called flat-top distribution in which there is little change with position in the width direction around it, as shown in Fig. 14. This is presumably because the central peak ensures the depth of the molten pool and therefore the weld, while the peripheral area stabilizes the molten pool by reducing the change in power density with location, thereby suppressing the occurrence of blowholes H and spatters associated with the movement of the molten pool.
[0057] [Opening and closing the keyhole during welding] Furthermore, the inventors' experimental analysis has revealed that a preferable joint 10 with few blowholes H in the welded part 14 can be obtained when the keyhole formed in the molten pool mainly by the action of the first laser light in the welding process is maintained in an open state without closing intermittently. This is presumably because, when the keyhole closes during welding, a recess formed in the molten pool by the keyhole remains as a blowhole H in the welded part 14. The above-mentioned conditions such as the wobbling parameters, spot shape, power ratio, and power density distribution are also conditions for the keyhole to be maintained in an open state without closing intermittently.
[0058] As described above, in the welding method for welding a surface Wa of a workpiece W including a plurality of metal members 11, 12 made of an aluminum-based material by irradiating the surface Wa with a laser beam L and scanning the surface Wa, a preferable joint 10 with few blowholes H in the welded portion 14 can be obtained by irradiating the laser beam L including a first laser beam and a second laser beam onto the surface Wa while appropriately wobbing the laser beam L, as in the present embodiment.
[0059] Although the embodiment of the present invention has been illustrated above, the above embodiment is merely an example and is not intended to limit the scope of the invention. The above embodiment can be implemented in various other forms, and various omissions, substitutions, combinations, and modifications can be made without departing from the gist of the invention. In addition, the specifications of each configuration, shape, and the like (structure, type, direction, model, size, length, width, thickness, height, number, arrangement, position, material, etc.) can be appropriately changed and implemented.
[0060] For example, in the embodiment, the workpiece has a configuration in which two metal members made of an aluminum-based material are stacked on top of each other, but the workpiece is not limited to this, and the present invention is also applicable to other types of workpieces, such as a workpiece having three or more metal members made of an aluminum-based material, or a workpiece having metal members whose ends are butted against each other to form a boundary. [Explanation of symbols]
[0061] 10...Zygote 11, 12...Metal parts 14…Welded section 100...Laser welding device (welding device) 111...Laser device 112...Laser device 120...Optical head 121, 121-1, 121-2...Collimating lenses 122...Condenser lens 123…Mirror 124…Dichroic mirror 125...DOE (diffractive optical element) 125a...Diffraction grating 126...Galvanometer scanner (laser scanner) 126a, 126b…Mirror 130...Optical fiber 140...Movement mechanism Ae…The sum of the areas of the first and second ellipses Aw: Area of the combined region of the first and second ellipses C1…center Cw…Mainly wobbling D1,D2…distance Dw…Wobbling diameter E1…First ellipse E2: Second ellipse H...Blowhole L: Laser light P11, P12, P21, P22…Location Pc…Scanning path Pt…scanning path Ptc…Movement path Rw…Wobbling radius S, S1, S11, S12, S2... Spot SD: Scanning direction Vc…Movement speed W…Processing target Wa…Surface WD: Width direction X…direction Y...Direction Z…direction
Claims
1. A welding method for welding a plurality of members made of an aluminum-based material by scanning a surface of the object to be processed with a laser beam while irradiating the surface with the laser beam, the plurality of members being welded together, the method comprising the steps of: the laser light includes a first laser light having a wavelength of 800 nm or more and 1200 nm or less, and a second laser light having a wavelength of 550 nm or less, The welding method further comprises irradiating the surface with the laser light while wobbling the laser light.
2. 2. The welding method according to claim 1, wherein the second laser light has a wavelength of 380 nm or more and 500 nm or less.
3. The method of claim 1 , wherein the first laser light is split into multiple beams to form multiple spots on the surface.
4. The welding method according to claim 3 , wherein the first laser beam is split into a plurality of beams using a beam shaper.
5. The method of claim 4 , wherein the beam shaper is a diffractive optical element.
6. the first laser beam includes a central laser beam and a peripheral laser beam surrounding the central laser beam, The welding method according to claim 4 , wherein a ratio of a power of the central laser beam to a power of the peripheral laser beam is equal to or greater than 1 / 4 and equal to or less than 7 / 3.
7. 2. The welding method according to claim 1, wherein the moving speed of the wobbling center of the laser light is 100 mm / s or less.
8. 2. The welding method according to claim 1, wherein the wobbling frequency of the laser light is 300 Hz or more.
9. 2. The welding method according to claim 1, wherein a wobbling speed of the laser beam is 100 mm / s or less, and a wobbling frequency of the laser beam is 300 Hz or more.
10. The overlap rate R of the wobbling is expressed by the following formula (1): R=2×(Ae-Aw) / Ae... (1) Here, Aw is the area of a region which is the sum of a first ellipse whose major axis is the distance between the position where the scanning path for one wobbling rotation is first located on the movement path of the wobbling center and the position where the scanning path for one wobbling rotation next lies on the movement path and the wobbling diameter is the minor axis, and a second ellipse whose major axis is the distance between the position where the scanning path for the next one wobbling rotation is first located on the movement path and the position where the scanning path for one wobbling rotation next lies on the movement path and the wobbling diameter is the minor axis, and Ae is the sum of the areas of the first ellipse and the second ellipse.
2. The welding method according to claim 1, wherein R≧0.51 when defined as follows:
11. A keyhole is formed in the molten pool formed by the irradiation of the laser light, The method of any one of claims 1 to 10, wherein the keyhole is maintained open without closing intermittently.
12. A welding method for welding a plurality of members made of an aluminum-based material by scanning a laser beam on a surface of a processing object including the plurality of members, the method comprising the steps of: the laser light includes a first laser light having a wavelength of 800 nm or more and 1200 nm or less, and a second laser light having a wavelength of 550 nm or less, A welding apparatus for performing a welding method, comprising: irradiating the surface with the laser light while wobbling the laser light, an optical head for outputting the laser light toward the surface; The welding apparatus, wherein the optical head includes a laser scanner.
Citation Information
Patent Citations
Welding method and welding device
JP2021159931A
Welding method and laser welding system
JP2023029489A
Laser welding method, laser welding conditions determining method, and laser welding system
WO2016194322A1
Welding method and welding apparatus
WO2021193855A1
Laser keyhole welding structure of aluminum material and laser keyhole welding method
WO2018181724A1