Cylindrical member for exhaust gas treatment device and exhaust gas treatment device

The cylindrical component for exhaust gas treatment devices addresses the issue of carrier retention and thermal stability by using an insulating layer with controlled roughness and crystalline glass composition, enhancing the performance of exhaust gas treatment systems.

JP2024143856AInactive Publication Date: 2024-10-11NGK INSULATORS LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023056770
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing exhaust gas treatment devices face challenges in maintaining the position of electrically heated carriers due to insufficient frictional force and thermal shock resistance, particularly in plug-in hybrid and hybrid vehicles where catalyst temperature is low at engine startup, leading to inadequate exhaust gas purification.

Method used

A cylindrical component for an exhaust gas treatment device is designed with an insulating layer on its inner surface, featuring specific arithmetic mean roughness (Ra) and ten-point average roughness (Rzjis94) ranges, along with a crystalline glass composition containing silicon, boron, and magnesium, to enhance both canning properties and thermal shock resistance.

Benefits of technology

The solution provides a cylindrical component with improved holding capability and thermal stability, ensuring effective exhaust gas treatment by maintaining the position of electrically heated carriers and withstanding high-temperature exhaust gases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143856000001_ABST
    Figure 2024143856000001_ABST
Patent Text Reader

Abstract

To provide a cylindrical member for an exhaust gas treatment device excellent in canning property and thermal shock resistance.SOLUTION: A cylindrical member for an exhaust gas treatment device includes a cylindrical metallic member, and an insulation layer provided on an inner peripheral surface of the cylindrical metallic member. Arithmetic average roughness Ra of an external surface of the insulation layer measured along a circumferential direction of the cylindrical metallic member according to JIS B0601:2013 is 0.5 μm or more and 10.0 μm or less, and ten-point average roughness Rzjis94 is 1.0 μm or more and 25.0 μm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a tubular part for an exhaust gas treatment device, and also to an exhaust gas treatment device including a tubular part for an exhaust gas treatment device and an electrically heated carrier accommodated therein. [Background technology]

[0002] Conventionally, a columnar honeycomb structure carrying a catalyst has been used to purify harmful substances such as HC, CO, and NOx contained in exhaust gas emitted from engines of vehicles. When treating exhaust gas with a catalyst carried on a honeycomb structure, the catalyst needs to be heated to its activation temperature. However, when the engine is started, the catalyst does not reach its activation temperature, so there is a problem that exhaust gas is not sufficiently purified. In particular, plug-in hybrid vehicles (PHEVs) and hybrid vehicles (HVs) include driving using only the motor, so the engine is started less frequently and the catalyst temperature at engine start is low, so the exhaust gas purification performance is likely to decrease immediately after the engine is started.

[0003] In response to this, an electrically heated catalyst (EHC) has been proposed, in which an electrically heated carrier (for example, an electrically heated honeycomb structure) is provided with a pair of electrodes and an electric current is passed through it to heat the electrically heated carrier. This electrically heated catalyst is used in a state in which the electrically heated carrier is housed in a metallic cylindrical part (cylindrical container). The electrically heated catalyst generates heat when electricity is passed through it, but when a voltage is applied to the electrically heated catalyst, electricity also flows through the cylindrical part, causing electricity to flow throughout the entire vehicle.

[0004] Therefore, a technology is known in which the inner circumferential surface of a cylindrical part is protected with an insulating layer for the purpose of electrically protecting the cylindrical part (Patent Publication No. 5408341, Patent Publication No. 5864213, JP 2022-131300, JP 2022-132045). The electrically heated carrier housed in the cylindrical member is held by friction between the inner circumferential surface of the cylindrical part, but the contact area of ​​the electrically heated carrier with the cylindrical part is likely to decrease due to the presence of the electrodes, and the insulating layer tends to have a small friction coefficient, so the friction between the cylindrical part and the electrically heated carrier decreases, and the electrically heated carrier may come off the cylindrical part due to external forces such as exhaust gas pressure and vehicle vibration, or the position of the electrically heated carrier may be displaced due to vibration. Therefore, there is a demand to increase the friction between the cylindrical part and the electrically heated carrier.

[0005] In this regard, WO 2021 / 176767 proposes a cylindrical member for an exhaust gas treatment device, which comprises a cylindrical metal member and an insulating layer provided on the inner circumferential surface of the cylindrical metal member, and the surface of the insulating layer has an uneven portion and a static friction coefficient of 0.30 or more. In order to obtain a surface with a static friction coefficient of 0.30 or more, the WO 2021 / 176767 discloses that the height difference of the uneven portion (the height difference between the lowest part and the highest part in a cross-sectional view of the insulating layer parallel to the flow direction of the exhaust gas) is preferably 300 μm or less, and that the surface of the insulating layer preferably has an uneven portion of 30% or more.

[0006] The examples of the international publication also describe how an insulating layer was formed by applying an insulating layer-forming slurry to the inner circumferential surface of a cylindrical metal member to form a dried coating layer, pressing a mold having convex portions against the surface of the dried coating layer to form concave portions of a predetermined groove shape, and then heating the layer to form an insulating layer. The obtained insulating layer in Example 1 had a thickness of 300 μm, a porosity of 9%, a height difference between the concave and convex portions of 23 μm, a ratio of the concave and convex portions of 66%, and a static friction coefficient of 0.33, while the thickness of the insulating layer in Example 2 was 300 μm, a porosity of 5%, a height difference between the concave and convex portions of 23 μm, a ratio of the concave and convex portions of 80%, and a static friction coefficient of 0.35. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 5408341 [Patent Document 2] Patent No. 5864213 [Patent Document 3] Patent Publication No. 2022-131300 [Patent Document 4] JP 2022-132045 A [Patent Document 5] International Publication No. 2021 / 176767 Summary of the Invention [Problem to be solved by the invention]

[0008] Increasing the frictional force between the cylindrical part and the electrically heated carrier is important in order to improve the function (canning ability) of holding the electrically heated carrier at a specified place inside the cylindrical part. However, there is a limit to increasing the friction coefficient of the insulating layer by simply specifying the height difference of the uneven parts as described in Patent Document 5. In addition, Patent Document 5 does not consider the thermal shock resistance of the insulating layer, but it is desirable for the insulating layer to have thermal shock resistance that can withstand high-temperature exhaust gas.

[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide, in one embodiment, a tubular part for an exhaust gas treatment device that includes an insulating layer that can achieve both excellent canning properties and excellent thermal shock resistance. In another embodiment, the present invention is to provide an exhaust gas treatment device that includes such a tubular part for an exhaust gas treatment device. [Means for solving the problem]

[0010] The present inventors have conducted extensive research to solve the above problems and have found that it is advantageous for an insulating layer to have a predetermined range of arithmetic mean roughness Ra and ten-point mean roughness Rzjis94 measured along the circumferential direction of a cylindrical metal member. The height difference of the unevenness described in Patent Document 5 is considered to be similar to the maximum height Rz, but in order to achieve both excellent canning properties and excellent thermal shock resistance, it is more important to control both the arithmetic mean roughness Ra and the ten-point mean roughness Rzjis94 within appropriate ranges. The present invention was completed based on this knowledge and is exemplified below.

[0011] [Aspect 1] A cylindrical metal member; an insulating layer provided on an inner peripheral surface of the cylindrical metal member; Equipped with The outer surface of the insulating layer has an arithmetic mean roughness Ra of 0.5 μm or more and 10.0 μm or less, and a ten-point mean roughness Rzjis94 of 1.0 μm or more and 25.0 μm or less, as specified in JIS B0601:2013, measured along the circumferential direction of the cylindrical metal member. Cylindrical parts for exhaust gas treatment equipment. [Aspect 2] The outer surface of the insulating layer has an arithmetic mean roughness Ra of 1.0 μm or more and 4.0 μm or less, and a ten-point mean roughness Rzjis94 of 2.0 μm or more and 10.0 μm or less, as specified in JIS B0601:2013, measured along the circumferential direction of the cylindrical metal member. The cylindrical part for an exhaust gas treatment device according to embodiment 1. [Aspect 3] The cylindrical part for an exhaust gas treatment device according to embodiment 1 or 2, wherein the insulating layer comprises a glass containing a crystalline substance, the glass comprising silicon, boron and magnesium, the silicon content in the glass being 20 mol% or less, the magnesium content being 10 mol% or more, and the boron content being 40 mol% or less. [Aspect 4] 4. The tubular part for an exhaust gas treatment device according to embodiment 3, wherein the glass further contains barium, and lanthanum, zinc, or a combination thereof. [Aspect 5] 5. The cylindrical part for an exhaust gas treatment device according to any one of aspects 1 to 4, wherein the insulating layer has a thickness of 30 μm to 800 μm. [Aspect 6] 6. The tubular part for an exhaust gas treatment device according to any one of aspects 1 to 5, wherein the static friction coefficient of the outer surface of the insulating layer is 0.5 to 4.0. [Aspect 7] A columnar electrically heated carrier capable of generating heat when electricity is applied thereto; A tubular part for an exhaust gas treatment device according to any one of aspects 1 to 6, which houses the electrically heated carrier; An exhaust gas treatment device comprising: [Aspect 8] 8. The exhaust gas treatment device according to embodiment 7, further comprising a mat material between the electrically heated carrier and the tubular part for an exhaust gas treatment device. Effect of the Invention

[0012] According to one embodiment of the present invention, a tubular part for an exhaust gas treatment device can be provided that has an insulating layer that is excellent in both canning property and thermal shock resistance. Therefore, by using this tubular part for an exhaust gas treatment device, it is possible to provide a high-quality exhaust gas treatment device. [Brief description of the drawings]

[0013] [Figure 1] 1 is a schematic cross-sectional view of a tubular part for an exhaust gas treatment device according to one embodiment of the present invention, observed in a direction perpendicular to the flow direction of exhaust gas. [Diagram 2] 1 is a schematic cross-sectional view of an exhaust gas treatment device according to one embodiment of the present invention, observed from a direction perpendicular to the flow direction of exhaust gas. [Diagram 3] 3 is a schematic cross-sectional view taken along line bb' in the exhaust gas treatment device shown in FIG. 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Next, the embodiments of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiments, and that appropriate changes and improvements in the design may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.

[0015] (1. Cylindrical parts for exhaust gas treatment equipment) FIG. 1 shows a schematic cross-sectional view of a tubular part for an exhaust gas treatment device according to one embodiment of the present invention, when observed from a direction perpendicular to the flow direction of exhaust gas. The tubular part for an exhaust gas treatment device 100 according to one embodiment of the present invention shown in FIG. 1 includes a tubular metal member 10 and an insulating layer 20 provided on the inner peripheral surface of the tubular metal member 10. A hollow portion 30 is formed on the inner peripheral side of the insulating layer 20, and an exhaust gas treatment device can be configured by accommodating an electrically heated carrier in the hollow portion 30. Note that, although the tubular part 100 shown in FIG. 1 is cylindrical, the shape of the tubular part 100 can be appropriately designed depending on the purpose.

[0016] [1-1. Cylindrical metal parts] The cylindrical metal member 10 can accommodate a columnar electrically heated carrier. The axial direction of the cylindrical metal member 10 coincides with the axial direction of the columnar electrically heated carrier (the same as the flow direction of the exhaust gas), and the central axis O of the cylindrical metal member 10 preferably coincides with the central axis of the columnar electrically heated carrier. In addition, the central position of the cylindrical metal member 10 in the axial direction preferably coincides with the central position of the columnar electrically heated carrier in the axial direction. Furthermore, the cylindrical metal member 10 may be uniform along the axial direction, but at least a part of it (for example, both axial ends, etc.) may have a reduced or increased diameter.

[0017] The inner peripheral surface of the cylindrical metal member before the insulating layer is provided is not particularly limited, but the arithmetic mean roughness Ra measured along the circumferential direction of the cylindrical metal member is preferably 10.0 μm or less, more preferably 7.0 μm or less, and even more preferably 5.0 μm or less. By controlling the arithmetic mean roughness Ra within such a range, the insulating layer can be uniformly formed on the inner peripheral surface of the cylindrical metal member. Moreover, this arithmetic mean roughness Ra is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1.0 μm or more. By controlling the arithmetic mean roughness Ra within such a range, the adhesive force of the insulating layer to the inner peripheral surface of the cylindrical metal member can be increased by the anchor effect. Therefore, the inner peripheral surface of the cylindrical metal member before the insulating layer is provided is preferably, for example, 0.1 μm or more and 10.0 μm or less, more preferably 0.5 μm or more and 7.0 μm or less, and even more preferably 1.0 μm or more and 5.0 μm or less, in terms of arithmetic mean roughness Ra measured along the circumferential direction of the cylindrical metal member. Setting the inner circumferential surface of the tubular metal member before the insulating layer is provided within such a range is also advantageous in terms of setting the surface roughness of the insulating layer to an appropriate range, which will be described later. The arithmetic mean roughness Ra can be adjusted by subjecting the inner circumferential surface of the tubular metal member to a surface treatment. Although not limited thereto, a representative example of the surface treatment is a roughening treatment such as blasting. In this specification, the "arithmetic mean roughness Ra" of the inner circumferential surface of the cylindrical metal member is measured by a stylus-type surface roughness measuring instrument in accordance with JIS B0601:2013.

[0018] The material of the cylindrical metal member is preferably a metal from the viewpoint of manufacturability, and examples of such materials include stainless steel, titanium alloy, copper alloy, aluminum alloy, brass, etc. Among these, stainless steel is preferred because of its high durability, reliability, and low cost.

[0019] The thickness of the tubular metal member is not particularly limited, but is preferably 0.1 mm or more, more preferably 0.3 mm or more, and even more preferably 0.5 mm or more. By controlling the thickness of the tubular metal member within such a range, durability and reliability can be ensured. Furthermore, the thickness of the tubular metal member is preferably 10.0 mm or less, more preferably 5.0 mm or less, and even more preferably 3.0 mm or less. By controlling the thickness of the tubular metal member within such a range, the weight of the tubular metal member can be reduced. Therefore, the thickness of the tubular metal member is preferably 0.1 mm or more and 10.0 mm or less, more preferably 0.3 mm or more and 5.0 mm or less, and even more preferably 0.5 mm or more and 3.0 mm or less.

[0020] The axial length of the cylindrical metal member can be appropriately set depending on the purpose, the length of the electrically heated carrier, etc. The length of the cylindrical metal member can be, for example, 30 mm to 600 mm, 40 mm to 500 mm, or 50 mm to 400 mm. Preferably, the axial length of the cylindrical metal member is greater than the length of the electrically heated carrier. In this case, the electrically heated carrier can be disposed so as not to be exposed from the cylindrical metal member.

[0021] The inner diameter (hydraulic diameter) of the tubular metal member and its cross-sectional shape perpendicular to the flow direction of the exhaust gas may be set so as to obtain the desired gripping pressure according to the outer diameter and outer peripheral shape of the electrically heated carrier to be housed, as well as the thickness of the insulating layer.

[0022] [1-2. Insulating layer] 1 again, the outer surface 21 of the insulating layer 20 provided on the inner peripheral surface of the tubular metal member 10 has an arithmetic mean roughness Ra measured along the circumferential direction of the tubular metal member 10 of 0.5 μm to 10.0 μm, and a ten-point mean roughness Rzjis94 measured along the circumferential direction of the tubular metal member 10 of 1.0 μm to 25.0 μm. In a preferred embodiment, the arithmetic mean roughness Ra is 1.0 μm to 4.0 μm, and the ten-point mean roughness Rzjis94 is 2.0 μm to 10.0 μm. In a more preferred embodiment, the arithmetic mean roughness Ra is 1.0 μm to 3.0 μm, and the ten-point mean roughness Rzjis94 is 2.0 μm to 5.0 μm.

[0023] By controlling the arithmetic mean roughness Ra and ten-point mean roughness Rzjis94 of the outer surface of the insulating layer 20 within such ranges, an insulating layer having both excellent canning properties and thermal shock resistance can be obtained. If the arithmetic mean roughness Ra is too small or too large, the canning properties will deteriorate. Even if the arithmetic mean roughness Ra is within an appropriate range, if there are large localized irregularities, they can become the starting points of cracks and cause a decrease in thermal shock resistance. For this reason, it is important to control both the arithmetic mean roughness Ra and the ten-point mean roughness Rzjis94 within appropriate ranges. In this specification, the "arithmetic mean roughness Ra" of the outer surface of the insulating layer is measured with a stylus-type surface roughness measuring instrument at a reference length of 3 mm in accordance with JIS B0601:2013. In this specification, the "ten-point average roughness Rzjis94" of the outer surface of the insulating layer is measured with a stylus-type surface roughness measuring instrument at a reference length of 3 mm in accordance with JIS B0601:2013.

[0024] The thickness of the insulating layer is not particularly limited, but is preferably 800 μm or less, more preferably 600 μm or less, and even more preferably 450 μm or less. By controlling the thickness within such a range, it is possible to make it difficult for the insulating layer to peel off from the inner surface of the cylindrical metal member. In addition, the thickness of the insulating layer is preferably 30 μm or more, more preferably 50 μm or more, and even more preferably 100 μm or more. Therefore, the thickness of the insulating layer is preferably 30 to 800 μm, more preferably 50 to 600 μm, and even more preferably 100 to 450 μm. By controlling the thickness of the insulating layer within such a range, it is possible to stably ensure the insulation between the columnar electrically heated carrier and the cylindrical metal member. In this specification, the "thickness" of the insulating layer is measured by the following method. An arbitrary cross section passing through the central axis O of the cylindrical part for an exhaust gas treatment device and parallel to the flow direction of the exhaust gas is cut out. In the cross section, the total length L of the inner circumferential surface of the cylindrical metal member on which the insulating layer is provided is measured. In addition, the total area S of the insulating layer is measured in the cross section. The "thickness" T of the insulating layer is given by T=S / L.

[0025] The static friction coefficient of the outer surface of the insulating layer is preferably 0.5 to 4.0, more preferably 0.6 to 2.0, and even more preferably 0.6 to 1.5. By controlling the static friction coefficient within such a range, it is possible to ensure a frictional force capable of suppressing the displacement (movement in the exhaust gas flow direction) of the electrically heated carrier caused by external forces due to exhaust gas pressure and vehicle vibration. In this specification, the "static friction coefficient" of the outer surface of the insulating layer is measured in accordance with JIS K7125:1999.

[0026] The material of the insulating layer is not particularly limited, but preferably contains glass containing crystalline matter. When the glass contains crystalline matter, an insulating layer that is difficult to soften and deform even at high temperatures (e.g., 750°C or higher) can be formed. Furthermore, when the glass contains crystalline matter, an insulating layer that has excellent adhesion to the cylindrical metal member can be formed. This is because the difference in thermal expansion coefficient with the cylindrical metal member can be reduced, and the thermal stress generated during heating can be reduced. The presence or absence of crystalline matter (crystals) can be confirmed by X-ray diffraction.

[0027] The glass preferably contains silicon, boron, and magnesium. This allows for the formation of a highly uniform insulating layer that is not easily softened or deformed even at high temperatures (e.g., 750°C or higher). Silicon may be contained in the glass in the form of, for example, SiO2. Boron may be contained in the glass in the form of, for example, B2O3. Magnesium may be contained in the glass in the form of, for example, MgO. Thus, the glass may be, for example, a SiO2-B2O3-MgO-based glass.

[0028] Silicon (substantially, SiO2) is a component that forms the skeleton of glass. More specifically, silicon is a component for precipitating crystals by heat treatment, and is a component that widens the vitrification range to facilitate vitrification and improves water resistance and heat resistance. The content of silicon in glass is preferably 20 mol% or less, more preferably 17 mol% or less, even more preferably 5 mol% to 15 mol%, and particularly preferably 10 mol% to 15 mol%. Boron (substantially, B2O3) is a component that enhances meltability and fluidity as well as devitrification resistance. The content of boron in glass is not particularly limited, but is preferably 40 mol% or less, more preferably 20 mol% to 40 mol%, even more preferably 25 mol% to 37 mol%, and particularly preferably 28 mol% to 35 mol%. Magnesium (substantially, MgO) is a component that is a constituent of crystals and is a component that reduces high-temperature viscosity to enhance meltability and fluidity. By including magnesium in the glass, it is possible to form an insulating layer that is resistant to softening and deformation even at high temperatures and has a high uniformity. The magnesium content in the glass is preferably 10 mol% or more, more preferably 15 mol% or more and 55 mol% or less, and even more preferably 25 mol% or more and 52 mol% or less.

[0029] If the silicon and magnesium contents are within these ranges, the above-mentioned effect (formation of an insulating layer that is highly uniform and does not easily soften or deform even at high temperatures) becomes significant. Furthermore, if the boron content is appropriate, the above-mentioned effect becomes even more significant. In this specification, the element content in glass is the molar ratio of the atoms of the element when the amount of all atoms in the glass excluding oxygen atoms is taken as 100 mol%. The element contents of silicon, boron, magnesium, etc. in glass can be measured by inductively coupled plasma (ICP) atomic emission spectrometry.

[0030] The glass may further contain barium. In this case, the glass may further contain lanthanum, zinc, or a combination thereof. Barium may be contained in the glass in the form of BaO, for example. Lanthanum may be contained in the glass in the form of La2O3, for example. Zinc may be contained in the glass in the form of ZnO, for example. Barium (substantially BaO) and zinc (substantially ZnO) are each a constituent component of a crystal. Lanthanum (substantially La2O3) is a component for improving fluidity. By containing barium in the glass and, if necessary, further containing lanthanum, zinc, or a combination thereof, an insulating layer having extremely excellent adhesion to the cylindrical metal member can be formed. When barium is contained in the glass, the content of barium in the glass is preferably 20 mol% or less, more preferably 2 mol% or more and 20 mol% or less. In one embodiment, the content of barium in the glass may be 2 mol% or more and 6 mol% or less, and in another embodiment, it may be 6 mol% or more and 18 mol% or less. When lanthanum is contained in the glass, the content of lanthanum in the glass is preferably 20 mol% or less, more preferably 2 mol% or more and 20 mol% or less, and even more preferably 2 mol% or more and 17 mol% or less. When zinc is contained in the glass, the content of zinc in the glass is preferably 20 mol% or less, more preferably 2 mol% or more and 10 mol% or less, and even more preferably 3 mol% or more and 8 mol% or less. In one embodiment, the total content of lanthanum and zinc in the glass can be 4 mol% or more and 20 mol% or less, and in another embodiment, it can be 8 mol% or more and 20 mol% or less. The amount of barium, lanthanum and zinc atoms in the glass can be measured by inductively coupled plasma (ICP) emission spectrometry.

[0031] The glass may further contain other metal elements. Examples of such metal elements include aluminum, calcium, and strontium. These metal elements may be contained in the glass alone or in combination of two or more. The other metal elements may also be contained in the glass in the form of metal oxides (e.g., Al2O3, CaO, SrO) like the above elements. Aluminum (substantially Al2O3) is a component that forms the skeleton of the glass, increases the strain point, adjusts the viscosity, and further suppresses phase separation. Calcium (substantially CaO) is a component that widens the vitrification range to facilitate vitrification, and is a component that lowers the high-temperature viscosity without lowering the strain point to enhance melting and fluidity. Strontium (substantially SrO) is a component that widens the vitrification range to facilitate vitrification, and is a component that suppresses phase separation and enhances devitrification resistance.

[0032] When aluminum is contained in the glass, the content of aluminum in the glass can be, for example, 15 mol% or less, can be 5 mol% or more and 15 mol% or less, and can be 5 mol% or more and 10 mol% or less. When calcium is contained in the glass, the content of calcium in the glass can be, for example, 7 mol% or less, can be 3 mol% or more and 7 mol% or less. When strontium is contained in the glass, the content of strontium in the glass can be, for example, 12 mol% or less, can be 8 mol% or more and 12 mol% or less. The amount of atoms of other metals such as aluminum, calcium, and strontium in the glass can be measured by inductively coupled plasma (ICP) atomic emission spectrometry.

[0033] The content of the alkali metal element in the glass may be, for example, 1000 ppm by mass or less. That is, the glass may be a so-called alkali-free glass. The content of the alkali metal element in the glass is preferably 800 ppm by mass or less, more preferably 500 ppm by mass or less, even more preferably 200 ppm by mass or less, and particularly preferably 100 ppm by mass or less. The content of the alkali metal element is preferably as small as possible, and may be, for example, substantially zero (below the detection limit). By making the content of the alkali metal element in the glass very small, it is possible to realize a cylindrical part for an exhaust gas treatment device in which the generation of environmental load substances can be suppressed even at high temperatures. In this specification, the "content of the alkali metal element in the glass" means the total amount of the alkali metal element contained in the glass. Examples of the alkali metal include lithium, sodium, potassium, rubidium, cesium, and francium. The alkali metal element contained in the glass may be, for example, sodium, potassium, or a combination thereof. The alkali metal element contained in the glass may be, for example, sodium. The content of the alkali metal element can be measured by inductively coupled plasma (ICP) emission spectrometry.

[0034] The insulating layer may be formed by any appropriate method. Typically, the insulating layer is formed by applying and drying a slurry (dispersion) containing a glass source to form a coating film, and then firing the coating film. The slurry may contain raw materials as the glass source, or may contain glass frit. Below, as a representative example, a method of forming an insulating layer using a slurry containing glass frit as the glass source will be described.

[0035] In one embodiment, a method for forming an insulating layer includes the steps of producing glass frit from a glass source (raw material), preparing a raw material slurry containing the glass frit, forming a coating of the slurry on the inner surface of a tubular metal member, and firing the coating to form an insulating layer containing glass.

[0036] Specific examples of raw materials include silica sand (silicon source), dolomite (magnesium and calcium source), boron oxide, alumina (aluminum source), barium oxide, lanthanum oxide, zinc oxide (zinc oxide), and strontium oxide. The raw materials are not limited to oxides, and may be, for example, carbonates or hydroxides. Glass frit can typically be produced by synthesizing glass from glass raw materials and pulverizing the obtained glass (for example, pulverizing in two stages of coarse pulverization and fine pulverization). When synthesizing glass, melting is performed for a long time at high temperatures (typically 1200° C. or higher).

[0037] The lower limit of the median diameter of the glass frit is preferably 20 μm or more, more preferably 24 μm or more, and even more preferably 28 μm or more, from the viewpoint of ensuring the surface roughness of the insulating layer. The upper limit of the median diameter of the glass frit is preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 35 μm or less, from the viewpoint of suppressing the variation in the thickness of the insulating film. Therefore, the median diameter of the glass frit is, for example, preferably 20 to 50 μm, more preferably 24 to 40 μm, and even more preferably 28 to 35 μm. The median diameter of the glass frit is calculated by measuring the volume-based particle size distribution in accordance with JIS Z8825:2013 "Particle size analysis - laser diffraction and scattering method".

[0038] The glass frit and the solvent are mixed to prepare a raw material slurry (dispersion). In order to ensure the surface roughness of the insulating layer, the lower limit of the viscosity of the raw material slurry measured at 20°C using a coaxial double cylindrical rotational viscometer of the inner cylinder constant speed type in accordance with JIS Z8803:2011 is preferably 50 mPa·s or more, more preferably 100 mPa·s or more. In addition, in order to suppress the variation in the coating amount per unit time, the upper limit of the viscosity of the raw material slurry measured at 20°C using a coaxial double cylindrical rotational viscometer of the inner cylinder constant speed type in accordance with JIS Z8803:2011 is preferably 1000 mPa·s or less, more preferably 500 mPa·s or less. Therefore, the viscosity of the raw material slurry is, for example, preferably 50 to 1000 mPa·s, more preferably 100 to 500 mPa·s.

[0039] The solvent may be water or an organic solvent. The solvent is preferably water or a water-soluble organic solvent, more preferably water. The solvent may be mixed at a ratio of preferably 50 to 300 parts by mass, more preferably 80 to 200 parts by mass, per 100 parts by mass of the glass frit. When preparing the raw material slurry, a slurry aid (e.g., a resin, a plasticizer, a dispersant, a thickener, various additives) may be further mixed. The type, number, combination, amount, etc. of the slurry aid may be appropriately set depending on the purpose. In this specification, the term "solvent" refers to a liquid medium contained in the raw material slurry, and is a concept that includes a solvent and a dispersion medium.

[0040] Next, the raw material slurry is applied to the inner peripheral surface of the cylindrical metal member and dried to form a coating film. Any appropriate method can be used as the coating method. Specific examples of the coating method include spraying, immersion with the cylindrical metal member masked except for the portion where the insulating layer is to be formed, and bar coating. The coating thickness can be adjusted according to the desired thickness of the insulating layer. The drying temperature is, for example, 40°C to 120°C, or, for example, 50°C to 110°C. The drying time is, for example, 1 minute to 60 minutes, or, for example, 10 minutes to 30 minutes.

[0041] Finally, the coating film is baked to form an insulating layer. The baking temperature is preferably 1100° C. or lower, more preferably 600° C. to 1100° C., and further preferably 700° C. to 1050° C. The baking time is, for example, 5 minutes to 30 minutes, or, for example, 8 minutes to 15 minutes.

[0042] (2. Exhaust gas treatment equipment) Fig. 2 shows a schematic cross-sectional view of an exhaust gas treatment device according to one embodiment of the present invention when observed from a direction perpendicular to the flow direction of exhaust gas. Fig. 3 shows a schematic cross-sectional view of the line b-b' in the exhaust gas treatment device shown in Fig. 2. As shown in Figs. 2 and 3, the exhaust gas treatment device 200 includes a columnar electrically heated support 50 capable of generating heat when electricity is applied thereto, and a cylindrical part for an exhaust gas treatment device 100 that houses the electrically heated support 50.

[0043] In the exhaust gas treatment device 200, the gripping pressure applied from the tubular part 100 for an exhaust gas treatment device to the outer peripheral surface of the electrically heated carrier 50 in a direction perpendicular to the exhaust gas flow direction is preferably 0.2 to 2.0 MPa, and more preferably 0.5 to 1.0 MPa. By controlling the gripping pressure within this range, it is possible to stably suppress the displacement (movement in the exhaust gas flow direction) of the electrically heated carrier 50 caused by external forces due to the exhaust gas pressure and vehicle vibration. Here, the gripping pressure can be determined by using a thin sensor sheet to measure the pressure applied to the outer peripheral surface of the electrically heated carrier 50 at room temperature (25° C.). Specifically, the gripping pressure is determined by wrapping a tactile sensor around the outer peripheral surface of the electrically heated carrier 50 and housing it in the tubular part 100 for an exhaust gas treatment device, and measuring the pressure applied to the outer peripheral surface of the electrically heated carrier 50 from the pressure read by the tactile sensor.

[0044] The electrically heated carrier 50 is not particularly limited, but is preferably a honeycomb structure having an outer peripheral wall 51 and partition walls 55 disposed inside the outer peripheral wall 51 and defining a plurality of cells 54 forming flow paths from a first end face 52 to a second end face 53. The cells 54 may penetrate from the first end face 52 to the second end face 53 and be open on both sides, or a plugged portion may be formed at the end of the cells 54 on either the first end face 52 side or the second end face 53 side.

[0045] The external shape of the electrically heated carrier 50 is not particularly limited, and may be, for example, a cylinder whose end face is round, such as a circular, oval, elliptical, racetrack, or oval shape, a cylinder whose end face is polygonal, such as a triangular or rectangular shape, or a cylinder whose end face has other irregular shapes. The electrically heated carrier 50 shown in the figure has a circular end face shape and is cylindrical as a whole.

[0046] The material of the electrically heated carrier 50 (the outer peripheral wall 51 and the partition wall 55) is not particularly limited as long as it can generate heat by Joule heat when electricity is applied, and metals, ceramics, etc. can be used. When ceramics is used as the material of the electrically heated carrier 50, at least one ceramic selected from the group consisting of oxide ceramics such as alumina, mullite, zirconia, and cordierite, and non-oxide ceramics such as silicon carbide, silicon nitride, and aluminum nitride can be used. In addition, silicon carbide-metal silicon composite material and silicon carbide / graphite composite material can also be used. Among these, from the viewpoint of achieving both heat resistance and electrical conductivity, it is preferable that the material of the electrically heated carrier 50 contains a silicon-silicon carbide composite material or a ceramic mainly composed of silicon carbide. When the material of the electrically heated carrier 50 is mainly composed of a silicon-silicon carbide composite material, it means that the electrically heated carrier 50 contains 90 mass% or more of the silicon-silicon carbide composite material (total mass) of the entirety. Here, the silicon-silicon carbide composite material contains silicon carbide particles as aggregates and silicon as a binder for binding the silicon carbide particles, and it is preferable that a plurality of silicon carbide particles are bound by silicon so as to form pores between the silicon carbide particles. When the material of the electrically heated carrier 50 is said to be mainly composed of silicon carbide, it means that the electrically heated carrier 50 contains silicon carbide (total mass) in an amount of 90 mass% or more of the total.

[0047] The manufacturing method of the electrically heated carrier 50 is not particularly limited, and can be performed according to a method known in the art. As an example, a method of manufacturing a honeycomb structure as the electrically heated carrier 50 will be described. First, a forming raw material is prepared by adding metal silicon powder (metal silicon), a binder, a surfactant, a pore former, water, etc. to silicon carbide powder (silicon carbide). Next, the obtained forming raw material is kneaded to form a clay, and the clay is extruded to prepare a honeycomb molded body. In the extrusion molding, a die having a desired overall shape, cell shape, partition wall thickness, cell density, etc. can be used. Next, the obtained honeycomb molded body is dried and then fired to prepare a honeycomb structure.

[0048] A pair of electrode parts 61 is preferably provided on the outer peripheral wall 51 of the electrically heated carrier 50. The pair of electrode parts 61 are provided in a band shape extending in the flow direction of the exhaust gas on the outer peripheral surface of the electrically heated carrier 50, sandwiching the central axis of the electrically heated carrier 50. By providing the pair of electrode parts 61, the uniformity of the heat distribution of the electrically heated carrier 50 when a voltage is applied between the pair of electrode parts 61 is increased.

[0049] The material of the electrode portion 61 is not particularly limited, and metals and conductive ceramics can be used. Examples of metals include Ag, Cu, Ni, Au, Pd, Cr, Fe, Co, Ni, Si, or Ti, or alloys containing at least one metal selected from the group consisting of these metals. Examples of conductive ceramics include metal compounds such as silicon carbide (SiC) and metal silicides such as tantalum silicide (TaSi2) and chromium silicide (CrSi2). In addition, composite materials (cermets) consisting of a combination of one or more of the conductive ceramics and one or more of the metals may be used. Specific examples of the cermets include composite materials of metal silicon and silicon carbide, composite materials of metal silicides such as tantalum silicide and chromium silicide, metal silicon and silicon carbide, and composite materials in which one or more of the insulating ceramics such as alumina, mullite, zirconia, cordierite, silicon nitride, and aluminum nitride are added to one or more of the above metals from the viewpoint of reducing thermal expansion. As the material for the electrode portion 61, among the various metals and conductive ceramics mentioned above, a combination of a metal silicide such as tantalum silicide or chromium silicide and a composite material of metal silicon and silicon carbide is preferred because it can be fired simultaneously with the electrically heated carrier 50, which contributes to simplifying the manufacturing process.

[0050] The electrical resistivity of the electrode portion 61 is preferably lower than that of the electrically heated carrier 50. With such a configuration, electricity flows preferentially through the electrode portion 61, and electricity spreads easily in the flow path direction and circumferential direction of the cell 54 when electricity is applied. The electrical resistivity of the electrode portion 61 is preferably 1 / 10 or less of the electrical resistivity of the electrically heated carrier 50, more preferably 1 / 20 or less, and even more preferably 1 / 30 or less. However, if the difference in electrical resistivity between the two becomes too large, current will concentrate between the ends of the opposing electrode portions 61, and the heat generated by the electrically heated carrier 50 will be biased. Therefore, the electrical resistivity of the electrode portion 61 is preferably 1 / 200 or more of the electrical resistivity of the electrically heated carrier 50, more preferably 1 / 150 or more, and even more preferably 1 / 100 or more. In the present invention, the electrical resistivity of the electrode portion 61 is a value measured at 25°C by a four-terminal method.

[0051] The method for forming the electrode portion 61 is not particularly limited, and can be performed according to a method known in the art. For example, a paste or slurry for forming the electrode portion may be applied to the outer peripheral surface of the electrically heated carrier 50 by a method such as screen printing, and then fired. The paste or slurry for forming the electrode portion may be fired simultaneously with the firing of the honeycomb molded body.

[0052] A metal terminal 60 can be joined to each of the pair of electrode parts 61. The metal terminal 60 can be directly or indirectly joined to the outer surface of each of the pair of electrode parts 61. Therefore, the cylindrical metal member 10 and the insulating layer 20 of the cylindrical part for exhaust gas treatment device 100 can be provided with a through hole for allowing the metal terminal 60 to be joined to the electrode part 61. When a voltage is applied to the electrically heated carrier 50 via the metal terminal 60, it is possible to pass electricity and cause the electrically heated carrier 50 to heat up by Joule heat. As a result, for example, the catalyst supported on the electrically heated carrier 50 can be heated to the active temperature of the catalyst before or at the time of engine start. As a result, exhaust gas can be sufficiently treated (representatively, purified) even at the time of engine start.

[0053] One metal terminal 60 can be connected to the positive pole of a power source (e.g., a battery), and the other metal terminal 60 can be connected to the negative pole of the power source (e.g., a battery). A gap may be provided around the metal terminal 60 to insulate the cylindrical metal member 10 from the metal terminal 60, or a cover 62 made of an insulating material may be provided.

[0054] The electrically heated carrier 50 is typically coaxially housed in the hollow portion 30 of the tubular part 100. The electrically heated carrier 50 may be housed directly in the tubular part 100 (i.e., without any other member therebetween), or may be housed via a mat material (not shown). When the electrically heated carrier 50 is housed directly in the tubular part 100, the electrically heated carrier 50 is fixed to the tubular part 100 by, for example, fitting.

[0055] The mat material functions as a buffer material, and therefore can suppress damage to the electrically heated carrier 50. In addition, if the mat material is insulating, it can suppress the flow of electricity to the cylindrical metal member 10 when the electrically heated carrier 50 is energized. The mat material is not particularly limited, but preferably contains inorganic fibers such as ceramic fibers. The ceramic fibers preferably contain one type selected from the group consisting of alumina, mullite, silicon carbide, silicon nitride, zirconia, and titania, or a composite thereof. The mat material typically covers the entire outer circumferential surface of the electrically heated carrier 50, and the cylindrical part 100 can hold the electrically heated carrier 50 via the mat material.

[0056] By supporting a catalyst on the electrically heated carrier 50, the electrically heated carrier 50 can be used as a catalyst body. When the electrically heated carrier 50 is a honeycomb structure, the partition walls 55 can support a catalyst. By supporting a catalyst on the partition walls 55, it is possible to convert CO, NOx, hydrocarbons, etc. in the exhaust gas passing through the cells 54 into harmless substances through a catalytic reaction. Examples of the catalyst include precious metal catalysts and other catalysts. Precious metal catalysts include three-way catalysts or oxidation catalysts in which precious metals such as platinum (Pt), palladium (Pd), and rhodium (Rh) are supported on the surface of alumina pores and contain co-catalysts such as ceria and zirconia, or alkaline earth metals and platinum are used to reduce nitrogen oxides (NO x ) as a storage component of NO x Examples of catalysts that do not use precious metals include NOx storage reduction catalysts (LNT catalysts). x Examples include selective catalytic reduction catalysts (SCR catalysts). Two or more catalysts selected from these catalysts may be used. There is no particular limitation on the method of supporting the catalyst, and any known supporting method may be used. EXAMPLES

[0057] The following examples are provided to better understand the present invention and its advantages, but the present invention is not limited to these examples.

[0058] <1. Manufacturing of cylindrical parts for exhaust gas treatment equipment> Example 1 The inner surface of a cylindrical metal tube made of SUS430 with a wall thickness of 3 mm was subjected to sandblasting treatment using #24 alumina abrasive grains. The treatment time was 1 minute. The arithmetic mean roughness Ra of the inner surface of the metal tube after sandblasting treatment was measured along the circumferential direction of the metal tube using a Mitutoyo SJ-210 stylus surface roughness tester in accordance with JIS B0601:2013, and was found to be 0.6 μm.

[0059] On the other hand, raw materials containing a prescribed amount of silica sand (Si source), B2O3, Mg(OH)2, and BaCO3 were melted to prepare glass frit. The obtained glass frit was pulverized by a wet ball mill method and classified to obtain glass frit with a median diameter of 20 μm. The median diameter of the glass frit was calculated in accordance with JIS Z8825:2013 "Particle size analysis - laser diffraction and scattering method". 100 parts by mass of this glass frit was added to 100 parts by mass of water and wet mixed in a ball mill processor to prepare a glass raw material dispersion (slurry). The viscosity of the obtained slurry at 20°C was measured by the above-mentioned method using a viscometer (VT-06 manufactured by Rion Co., Ltd.). The results are shown in Table 1.

[0060] The glass raw material dispersion was sprayed onto the entire inner circumferential surface of the sandblasted metal pipe obtained above to form a coating film, which was then dried at 50° C. The metal pipe on which the dried coating film was formed was then fired in a heating furnace at 860° C. to form an insulating layer, thereby producing a tubular part for an exhaust gas treatment device. The tubular part for an exhaust gas treatment device was produced in the number required for the following tests.

[0061] Example 2 The Ra of the inner surface of the cylindrical metal tube was changed to 0.9 μm by changing the sandblasting conditions, the median diameter of the glass frit was changed to 30 μm by changing the classification conditions, and the water mixing ratio in the slurry was changed so that the viscosity of the slurry was approximately the same as in Example 1. Except for this, the same procedure as in Example 1 was used to manufacture the cylindrical parts for exhaust gas treatment equipment in the number required for the following tests.

[0062] Example 3 The Ra of the inner surface of the cylindrical metal tube was changed to 1.8 μm by changing the sandblasting conditions, the median diameter of the glass frit was changed to 30 μm by changing the classification conditions, and the water blending ratio in the slurry was changed so that the viscosity of the slurry was within the range shown in Table 1. Except for this, the same procedure as in Example 1 was used to manufacture the cylindrical parts for exhaust gas treatment equipment in the number required for the following tests.

[0063] Example 4 The Ra of the inner surface of the cylindrical metal tube was changed to 4.5 μm by changing the sandblasting conditions, the median diameter of the glass frit was changed to 40 μm by changing the classification conditions, and the water blending ratio in the slurry was changed so that the viscosity of the slurry was within the range shown in Table 1. Except for this, the same procedure as in Example 1 was used to manufacture the cylindrical parts for exhaust gas treatment equipment in the number required for the following tests.

[0064] Example 5 The Ra of the inner surface of the cylindrical metal tube was changed to 7.2 μm by changing the sandblasting conditions, the median diameter of the glass frit was changed to 50 μm by changing the classification conditions, and the water blending ratio in the slurry was changed so that the viscosity of the slurry was within the range shown in Table 1. Except for this, the same procedure as in Example 1 was used to manufacture the cylindrical parts for exhaust gas treatment equipment in the number required for the following tests.

[0065] Comparative Example 1 The Ra of the inner surface of the cylindrical metal tube was changed to 0.1 μm by changing the sandblasting conditions, the median diameter of the glass frit was changed to 5 μm by changing the classification conditions, and the water blending ratio in the slurry was changed so that the viscosity of the slurry was within the range shown in Table 1. Except for this, the same procedure as in Example 1 was used to manufacture the cylindrical parts for exhaust gas treatment equipment in the number required for the following tests.

[0066] Comparative Example 2 The Ra of the inner surface of the cylindrical metal tube was changed to 12.0 μm by changing the sandblasting conditions, the median diameter of the glass frit was changed to 60 μm by changing the classification conditions, and the water blending ratio in the slurry was changed so that the viscosity of the slurry was within the range shown in Table 1. Except for this, the same procedure as in Example 1 was used to manufacture the cylindrical parts for exhaust gas treatment equipment in the number required for the following tests.

[0067] Comparative Example 3 The inner surface of a cylindrical metal tube made of SUS430 with a wall thickness of 3 mm was subjected to sandblasting treatment using alumina abrasive grains of #24 to #60. The treatment time was 1 minute. The arithmetic mean roughness Ra of the inner surface of the metal tube after sandblasting treatment was measured along the circumferential direction of the metal tube using a Mitutoyo Corporation SJ-210 stylus surface roughness tester in accordance with JIS B0601:2013, and was found to be 2.0 μm.

[0068] Next, 100 parts by mass of water was added to 100 parts by mass of glass frit prepared in Example 1, the median diameter of which was changed to 30 μm by changing the classification conditions, and the mixture was wet-mixed in a ball mill to obtain a glass raw material dispersion (slurry).

[0069] The glass raw material dispersion was sprayed onto the entire inner surface of the sandblasted metal tube obtained above to form a coating film, and then dried at 50 ° C. for 60 minutes. Next, in order to form groove-shaped recesses as shown in Figures 2 and 3 of WO 2021 / 176767, a mold having a convex portion corresponding to the recessed portion was pressed against the dried coating film, and the metal tube was baked in a heating furnace at 860 ° C. for 10 minutes to form an insulating layer with a height difference of 23.0 μm between the convex and concave portions, thereby producing a cylindrical part for an exhaust gas treatment device. The number of cylindrical parts for exhaust gas treatment devices required for the following tests was produced.

[0070] <2. Characteristics of cylindrical parts for exhaust gas treatment equipment>

[0071] (2-1. Thickness of the insulating layer) The thickness of the insulating layer of each of the tubular parts for exhaust gas treatment equipment obtained above was measured by the measurement method described above on a cross section cut out from the tubular part for exhaust gas treatment equipment, which was parallel to the flow direction of the exhaust gas and passed through the central axis O of the tubular part for exhaust gas treatment equipment. The results are shown in Table 1.

[0072] (2-2. Surface roughness of the insulating layer) The outer surface of the insulating layer of each of the tubular parts for exhaust gas treatment equipment obtained above was measured for arithmetic mean roughness Ra and ten-point mean roughness Rzjis94 in accordance with JIS B0601:2013 along the circumferential direction of the metal tube using a Mitutoyo Corporation SJ-210 stylus-type surface roughness tester. The results are shown in Table 1.

[0073] (2-3. Static friction coefficient of insulating layer) The static friction coefficient of the outer surface of the insulating layer of each of the cylindrical parts for exhaust gas treatment equipment obtained above was measured in accordance with JIS K7125: 1999. The results are shown in Table 1.

[0074] (2-4. Crystallinity of the insulating layer) The insulating layer of each of the cylindrical parts for exhaust gas treatment equipment obtained above was judged to be crystalline or amorphous by X-ray diffraction (XRD). If a crystal diffraction peak was obtained in the diffraction line, it was judged to be crystallized (crystalline), and if the diffraction line was a halo and no diffraction peak was obtained, it was judged to be amorphous. The results are shown in Table 1.

[0075] (2-5. Composition of the insulating layer) The element contents, excluding oxygen atoms, in the glass constituting the insulating layer of each of the cylindrical parts for exhaust gas treatment equipment obtained above were measured by inductively coupled plasma (ICP) emission spectrometry. The results are shown in Table 1.

[0076] (2-6. Canning ability) A cylindrical honeycomb structure manufactured by NGK Insulators with an outer shape of 80 mm in diameter and 65 mm in length was produced in a conventional manner. This honeycomb structure was inserted into the hollow portion of each of the cylindrical parts for exhaust gas treatment equipment obtained above and gripped. The gripping pressure was measured with a tactile sensor and found to be 0.5 MPa. Thereafter, the honeycomb structure was punched out at a temperature of 600°C and a punching speed of 1 mm / min, and the maximum load (N) was measured and used as an index of canning property. The canning property was evaluated according to the following criteria. The results are shown in Table 1. ○(Good): Maximum load is 450N or more △ (Acceptable): Maximum load is 250N or more and less than 450N × (Failure): Maximum load is less than 250N

[0077] (2-7. Thermal shock resistance) Each of the cylindrical parts for exhaust gas treatment equipment obtained above was placed in a heating furnace with an atmospheric temperature of 900°C for 30 minutes, and then immediately placed in a heating furnace with an atmospheric temperature of 150°C for 5 minutes. After that, it was removed from the heating furnace and visually checked for the presence or absence of cracks in the insulating layer. This was counted as one cycle, and the number of cycles until cracks appeared in the insulating layer was counted, and the thermal shock resistance was evaluated according to the following criteria. ○ (Good): No cracks occurred even after 9 or more cycles (stopped after 10 cycles) △ (Acceptable): Cracks occur after 5 to 8 cycles × (Failure): Cracks occur within 1 to 4 cycles

[0078] [Table 1]

[0079] <3. Consideration> In Comparative Example 1, the arithmetic mean roughness Ra and ten-point mean roughness Rzjis94 of the outer surface of the insulating layer of the tubular part for exhaust gas treatment equipment were too small, and the canning property was poor. In Comparative Example 2, the arithmetic mean roughness Ra and ten-point mean roughness Rzjis94 of the outer surface of the insulating layer of the tubular part for exhaust gas treatment equipment were too large, and both the canning property and the thermal shock resistance were poor. In Comparative Example 3, the arithmetic mean roughness Ra of the outer surface of the insulating layer of the tubular part for exhaust gas treatment equipment was too large, and the thermal shock resistance was poor. On the other hand, in Examples 1 to 5, both the arithmetic mean roughness Ra and the ten-point mean roughness Rzjis94 of the outer surface of the insulating layer of the tubular part for exhaust gas treatment equipment were adjusted to appropriate ranges, and thus a tubular part for exhaust gas treatment equipment with excellent canning property and thermal shock resistance was obtained. [Explanation of symbols]

[0080] 10: Cylindrical metal member 20: Insulating layer 21 :Outer surface 30: Hollow part 50: Electrically heated carrier 51 :Outer wall 52: 1st end surface 53: 2nd end face 54: Cell 55: Bulkhead 60: Metal terminal 61: Electrode part 62: Cover 100: Cylindrical parts for exhaust gas treatment equipment 200: Exhaust gas treatment equipment

Claims

1. A cylindrical metal member; an insulating layer provided on an inner peripheral surface of the cylindrical metal member; Equipped with The outer surface of the insulating layer has an arithmetic mean roughness Ra of 0.5 μm or more and 10.0 μm or less, and a ten-point mean roughness Rzjis94 of 1.0 μm or more and 25.0 μm or less, as specified in JIS B0601:2013, measured along the circumferential direction of the cylindrical metal member. Cylindrical parts for exhaust gas treatment equipment.

2. The outer surface of the insulating layer has an arithmetic mean roughness Ra of 1.0 μm or more and 4.0 μm or less, and a ten-point mean roughness Rzjis94 of 2.0 μm or more and 10.0 μm or less, as specified in JIS B0601:2013, measured along the circumferential direction of the cylindrical metal member. The tubular part for an exhaust gas treatment device according to claim 1 .

3. 3. The cylindrical part for an exhaust gas treatment device according to claim 1 or 2, wherein the insulating layer comprises glass containing crystalline matter, the glass comprising silicon, boron and magnesium, the silicon content in the glass being 20 mol% or less, the magnesium content being 10 mol% or more, and the boron content being 40 mol% or less.

4. 4. The tubular part for an exhaust gas treatment device according to claim 3, wherein the glass further contains barium, and lanthanum, zinc, or a combination thereof.

5. 3. The cylindrical part for an exhaust gas treatment device according to claim 1, wherein the insulating layer has a thickness of 30 μm to 800 μm.

6. 3. The tubular part for an exhaust gas treatment device according to claim 1, wherein the static friction coefficient of the outer surface of the insulating layer is 0.5 to 4.

0.

7. A columnar electrically heated carrier capable of generating heat when electricity is applied thereto; The cylindrical part for an exhaust gas treatment device according to claim 1 or 2, which houses the electrically heated carrier; An exhaust gas treatment device comprising:

8. The exhaust gas treatment device according to claim 7, further comprising a mat material between the electrically heated carrier and the tubular part for the exhaust gas treatment device.

Citation Information

Patent Citations

  • Nonnstage speed change gear

    JP1979008341A

  • Gallium- and / or indium-containing zeolites, manufacture and use

    JP1983064213A

  • Cylindrical member for exhaust gas treatment device, exhaust gas treatment device using cylindrical member, and insulation layer used in cylindrical member

    JP2022131300A

  • Cylindrical member for exhaust gas treatment device, exhaust gas treatment device using cylindrical member, and insulation layer used in cylindrical member

    JP2022132045A

  • Cylindrical member for exhaust gas treatment device, electric heating type member for exhaust gas treatment device, and exhaust gas treatment device

    WO2021176767A1