Flux-cored wire for self-sealed arc welding

A flux-cored wire with optimized C, Mn, Al, Si, S, Mg, Ni, SiO2, and metal fluorides/carbonates composition stabilizes arcs, reduces spatter, and enhances strength and toughness, addressing the limitations of existing self-shielded arc welding for high-strength steels.

JP2024144036APending Publication Date: 2024-10-11NIPPON STEEL WELDING & ENGINEERING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023184703
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-10-27
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing flux-cored wires for self-shielded arc welding of high-strength steels face issues with poor welding workability, including unstable arcs, excessive spatter, and porosity defects such as pits and blowholes, while also struggling to achieve the necessary strength and toughness for high-strength steel applications.

Method used

A flux-cored wire composition with specific ranges of C, Mn, Al, Si, S, Mg, Ni, SiO2, metal fluorides, and metal carbonates, along with iron powder, is used to stabilize the arc, reduce spatter, and enhance the strength and toughness of weld metal, while minimizing porosity defects.

Benefits of technology

The wire achieves weld metals with strength ranging from 490 MPa to 670 MPa and excellent toughness, with stable arcs, low spatter, and no porosity defects, improving overall welding workability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144036000001
    Figure 2024144036000001
  • Figure 2024144036000002
    Figure 2024144036000002
  • Figure 2024144036000003
    Figure 2024144036000003
Patent Text Reader

Abstract

To provide a flux-cored wire for self-sealed arc welding which enables the yield of weld metal with high strength and excellent in tenacity, enables the suppression of welding defects, and has favorable welding workability.SOLUTION: A flux-cored wire for self-sealed arc welding is characterized by containing 0.04 to 0.12% of C, 1.0 to 2.5% of Mn, 1.0 to 3.0% of Al, 0.5% or less of Si, and 0.016 to 0.04% of S by mass% to the whole mass of the wire, in the total of a steel-made outer shell and flux, where the flux contains 1.0 to 3.0% of Mg, 0.1 to 3.0 of Ni, 0.5% or less of the total of SiO2 conversion value, 1.5 to 5.0% of the total of F conversion value, 0.2 to 2.0% of the total of one or two or more kinds of metal carbonates, and 30 to 60% of iron powder by mass% to the whole mass of the flux.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a flux-cored wire for self-shielded arc welding of 490 MPa to 670 MPa class high tensile steel, which can provide a weld metal with high strength and excellent toughness, does not cause welding defects such as pits or blowholes, and has good welding workability. [Background technology]

[0002] The flux-cored wire for self-shielded arc welding is a welding method in which a gas generating agent such as a metal fluoride or a metal carbonate is added to the welding wire, and the metal fluoride and the metal carbonate are decomposed by the arc heat during welding to generate a shielding gas, which covers the molten pool and allows welding to be performed without using a shielding gas and by blocking the atmosphere. This welding method does not require equipment such as a cylinder or piping for delivering the shielding gas, so the welding equipment has a simple structure and is easy to carry, and is widely used in civil engineering and construction fields. For example, Patent Document 1 discloses a flux-cored wire for self-shielded arc welding that allows all-position welding.

[0003] However, the flux-cored wire for self-shielded arc welding disclosed in Patent Document 1 has problems such as poor welding workability due to an unstable arc and a large amount of spatter generation, a tendency to develop porosity defects such as pits and blowholes, and poor mechanical properties of the weld metal, compared to general flux-cored wires for gas-shielded arc welding.

[0004] As a means for solving this problem, Patent Document 2 discloses a flux-cored wire for self-shielded arc welding, which improves shielding resistance and prevents porosity defects such as pits and blowholes by adding appropriate amounts of Al, which has the effect of fixing N in the molten metal and improving porosity resistance, Mg, which has the effect of shielding the welded part, metal fluorides, and metal carbonates to the welding wire, and which has good welding workability such as stabilizing the arc and reducing the amount of spatter. However, although the use of the flux-cored wire for self-shielded arc welding disclosed in Patent Document 2 can suppress porosity defects such as pits and blowholes, stabilize the arc, and reduce the amount of spatter, there is a problem that the microstructure of the weld metal is easily coarsened because a large amount of Al is added, making it difficult to obtain a weld metal with excellent mechanical properties, and in particular, it is difficult to obtain sufficient toughness of the weld metal.

[0005] In recent years, the strength of welded structures has been increasing in the civil engineering and architectural fields, and high-strength steels such as 590 MPa class steels are widely used. When welding such high-strength steels, the weld metal is also required to have a considerable strength, so elements that improve the strength of the weld metal, such as Mo, are sometimes added to the welding wire used in self-shielded arc welding. However, when Mo or the like is contained in the weld metal, it becomes even more difficult to obtain the toughness of the weld metal.

[0006] As a means for solving these problems, Patent Document 3 discloses a flux-cored wire for self-shielded arc welding, which contains an appropriate amount of Al, BaF2, and Sr composite oxide to stabilize the arc, thereby reducing the amount of spatter generation, and improving welding workability by suppressing pore defects such as pits and blowholes, and also contains appropriate amounts of C, Mn, Ni, and Mo to improve the strength and toughness of the weld metal. However, the flux-cored wire for self-shielded arc welding disclosed in Patent Document 3 has a problem that the strength of the weld metal is excessively high because the amounts of C, Mn, Ni, and Mo added are increased, although good welding workability can be obtained by stabilizing the arc, reducing the amount of spatter generation, and suppressing pore defects such as pits and blowholes. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 62-238097 [Patent Document 2] Japanese Patent Application Publication No. 3-118993 [Patent Document 3] JP 2009-119497 A Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been devised in view of the above-mentioned problems, and aims to provide a flux-cored wire for self-shielded arc welding of 490 MPa to 670 MPa class high tensile steel, which can provide a weld metal with high strength and excellent toughness, can suppress porosity defects such as pits and blowholes, and has good welding workability. [Means for solving the problem]

[0009] In order to solve the above-mentioned problems, the flux-cored wire for self-shielded arc welding according to the present invention is a flux-cored wire for self-shielded arc welding in which a steel sheath is filled with flux, and the flux and the steel sheath together contain, in mass % relative to the total mass of the wire, 0.04 to 0.12% C, 1.0 to 2.5% Mn, 1.0 to 3.0% Al, 0.5% or less Si, and 0.016 to 0.04% S, and further contain, in mass % relative to the total mass of the wire, 1.0 to 3.0% Mg, 0.1 to 3.0% Ni, SiO of an oxide of Si, and 2 The flux is characterized in that it contains, in mass % relative to the total mass of the flux, 30 to 60% iron powder, with the remainder consisting of the Fe content of the steel sheath, the Fe content of the iron alloy powder, and impurities. Effect of the Invention

[0010] According to the flux-cored wire for self-shielded arc welding of the present invention, a weld metal having high strength of 490 MPa to 670 MPa and excellent toughness can be obtained, and a flux-cored wire for self-shielded arc welding can be provided that is free from porosity defects such as pits and blowholes and has good welding workability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In order to solve the above-mentioned problems, the present inventors conducted detailed studies on the component composition of a flux-cored wire for self-shielded arc welding that can produce a weld metal with high strength of 490 MPa to 670 MPa and excellent toughness, and that has excellent welding workability such as no generation of porosity defects such as pits or blowholes, a stable arc, and a small amount of spatter.

[0012] As a result, it was found that by adding an appropriate amount of Al to the flux-cored wire for self-shielded arc welding, N in the molten metal can be fixed as AlN to suppress the occurrence of porosity defects such as pits and blowholes, but Al can coarsen the microstructure of the weld metal and reduce the toughness of the weld metal. Therefore, as a result of examining various methods for improving the strength of the weld metal while suppressing the coarsening of the microstructure, it was found that by adding a large amount of metal fluorides, metal carbonates, and Mg that generate gas to the flux-cored wire for self-shielded arc welding, it is possible to improve the shielding properties and reduce the amount of Al added, and it is possible to suppress the coarsening of the microstructure, and it is also possible to improve the strength and toughness of the weld metal by adding appropriate amounts of C and Mn. However, it was found that if the amount of metal carbonate added is excessive, large spatters are likely to be generated. It was also found that if the amount of Mn added is increased to obtain the necessary toughness of the weld metal, the strength of the weld metal becomes too high.

[0013] As a result of further investigations into obtaining a weld metal that suppresses the occurrence of porosity defects such as pits and blowholes, has a strength of 490MPa to 670MPa, and has good toughness, it was found that by reducing the amount of metal carbonate added to suppress the amount of slag generation, by keeping the amount of Al added to a minimum and increasing the amounts of Si, Mg, and metal fluorides added to suppress the occurrence of porosity defects such as pits and blowholes, and by keeping the amount of Mn added low and adjusting the amount of C added, a weld metal with a strength of 490MPa to 670MPa and good toughness can be obtained. Furthermore, it was found that the addition of appropriate amounts of Cu and Ni can suppress the coarsening of the ferrite structure and improve the toughness of the weld metal.

[0014] Regarding other welding workability, it was found that adding appropriate amounts of iron powder, S, sodium oxide and potassium oxide is effective in stabilizing the arc and reducing the amount of spatter.

[0015] Furthermore, they found that by adding an appropriate amount of silicon oxide, the viscosity of the molten slag can be adjusted, and the slag encapsulation of the weld bead and the bead shape can be improved.

[0016] The flux-cored wire for self-shielded arc welding to which the present invention is applied has been made possible by the synergistic effect of each component composition alone or by the coexistence of each component, and the reasons for adding and limiting each component composition will be described below. Note that, in the following, the chemical components of the flux-cored wire for self-shielded welding will be expressed as mass% which is the ratio to the total mass of the wire or mass% to the total mass of the flux, and the description regarding mass% will be simply written as %.

[0017] [The total mass of the steel sheath and flux is C: 0.04 to 0.12%] C has the effect of improving the strength of the weld metal through solid solution strengthening. C also reduces the CO and CO generated during welding. 2 C has the effect of blocking the atmosphere from the molten pool, improving shielding properties, and suppressing the occurrence of welding defects such as pits and blowholes. If C is less than 0.04%, the effect is not sufficiently obtained, and the strength of the weld metal is not obtained. If C is less than 0.04%, the shielding properties are not sufficiently ensured, and welding defects such as pits and blowholes are likely to occur. On the other hand, if C exceeds 0.12%, the strength of the weld metal becomes excessively high and the toughness decreases. Therefore, the total C content of the steel sheath and the flux is set to 0.04 to 0.12%. Note that C can be added from the flux as metal powder, alloy powder, etc., in addition to being a component contained in the steel sheath.

[0018] [Mn: 1.0-2.5% by mass (total mass of steel sheath and flux) relative to total mass of wire] Mn acts as a deoxidizer for the weld metal and has the effect of improving the strength and toughness of the weld metal. If the Mn content is less than 1.0%, the effect is not sufficiently obtained, and the strength and toughness of the weld metal decrease. On the other hand, if the Mn content exceeds 2.5%, the strength of the weld metal becomes excessively high, and the toughness decreases. Therefore, the total Mn content of the steel sheath and the flux is set to 1.0 to 2.5%. Note that Mn can be added from the flux as an alloy powder of metal Mn, Fe-Mn, Fe-Si-Mn, etc., in addition to being a component contained in the steel sheath.

[0019] [The total mass of the steel sheath and flux is 1.0 to 3.0% Al by mass percentage relative to the total mass of the wire] Al acts as a deoxidizer to improve the toughness of the weld metal, and also has the effect of forming AlN in the molten metal to fix the N that has entered, thereby suppressing the occurrence of welding defects such as pits and blowholes. If Al is less than 1.0%, the effect is not sufficiently obtained, and welding defects such as pits and blowholes are likely to occur. On the other hand, if Al exceeds 3.0%, the Al in the weld metal is excessively retained, the microstructure becomes coarse, and the toughness of the weld metal decreases. Therefore, the total Al content of the steel sheath and the flux is set to 1.0 to 3.0%. In addition to the components contained in the steel sheath, Al can be added from the flux as alloy powder such as metallic Al, Fe-Al, and Al-Mg.

[0020] [Si: 0.5% or less (total mass of steel sheath and flux) in terms of mass% of total wire mass] Silicon acts as a deoxidizer and has the effect of suppressing the occurrence of welding defects such as pits and blowholes and improving the mechanical properties of the weld metal, but if it is excessively contained in the weld metal, the strength of the weld metal becomes excessively high and the toughness decreases, so the total amount of silicon in the steel sheath and flux is set to 0.5% or less. From the viewpoint of suppressing the occurrence of welding defects such as pits and blowholes and ensuring the toughness of the weld metal, it is more preferable that the amount of silicon is 0.1 to 0.5%. In addition to being a component contained in the steel sheath, silicon can be added from the flux as alloy powder such as metal silicon, Fe-Si, Fe-Si-Mn, and Al-Si.

[0021] [S: 0.016~0.04% by mass (total mass of steel sheath and flux) S reduces the viscosity and surface tension of droplets when the wire melts, facilitating droplet transfer, reducing the size of spatter and improving welding workability. In addition, S is a low melting point compound, so it aggregates at the interface between the weld metal and slag, improving slag removal. If S is less than 0.016%, spatter increases and slag removal becomes difficult. On the other hand, if S exceeds 0.04%, cracks are more likely to occur in the weld metal. Therefore, the total S content of the steel sheath and flux should be 0.016 to 0.04%. In addition to being a component contained in the steel sheath, S can be added to the flux as alloy powder such as FeS.

[0022] [Mg in flux by mass% relative to the total wire mass: 1.0-3.0%] Mg acts as a deoxidizer, promoting the deoxidation of the weld metal, suppressing the occurrence of welding defects such as pits and blowholes, and improving the toughness of the weld metal. If the Mg content is less than 1.0%, the effect is not sufficiently obtained, welding defects such as pits and blowholes are more likely to occur, and the toughness of the weld metal is reduced. On the other hand, if the Mg content exceeds 3.0%, the arc becomes excessively strong and unstable, and the amount of spatter generated increases. Therefore, the Mg content in the flux is set to 1.0 to 3.0%. Note that Mg can be added to the flux as metallic Mg, alloy powder such as Al-Mg, etc.

[0023] [Ni in flux by mass% relative to the total wire mass: 0.1-3.0%] Ni, like Mn, is an austenite stabilizing element and has the effect of suppressing the coarsening of ferrite structure. However, when Ni is less than 0.1%, the effect of suppressing the coarsening of ferrite is too small, and the toughness of the weld metal decreases. Also, when Ni exceeds 3.0%, the strength becomes excessive and the toughness also decreases. Therefore, Ni in the flux is set to 0.1 to 3.0%. Ni can be added from the flux as metallic Ni, Fe-Ni, or other alloy powder.

[0024] [The mass percent of silicon oxide in the flux relative to the total mass of the wire is SiO 2 Total conversion value: 0.5% or less Silicon oxide has the effect of adjusting the viscosity and melting point of the molten slag, improving the encapsulation of the slag, and improving the bead shape, so it is better to add an appropriate amount. However, the SiO 2 If the total of the converted values ​​exceeds 0.5%, the basicity of the molten slag decreases, the oxygen content of the weld metal increases, and the toughness of the weld metal decreases. Therefore, the SiO 2 The total of the converted values ​​must be 0.5% or less. Silicon oxide can be added from the flux as silica sand, potash glass, fluorite, etc.

[0025] [The total F-equivalent value of metal fluorides in the flux in mass% relative to the total wire mass: 1.5 to 5.0%] The metal fluoride acts as a gas generating agent, and has the effect of increasing the shielding effect of the molten pool from the atmosphere and concentrating and stabilizing the arc. If the total F-converted value of the metal fluoride is less than 1.5%, the effect is not sufficiently obtained, the shielding effect is insufficient, welding defects such as pits and blowholes are likely to occur, the arc becomes unstable, and the amount of spatter generation increases. On the other hand, if the total F-converted value of the metal fluoride exceeds 5.0%, the arc becomes excessively strong and unstable, and the amount of spatter generation increases. Therefore, the total F-converted value of the metal fluoride contained in the flux is 1.5 to 5.0%. The metal fluoride can be added from the flux as fluorite, sodium fluoride, lithium fluoride, magnesium fluoride, potassium silicofluoride, cryolite, aluminum fluoride, etc.

[0026] [The total of one or more metal carbonates in the flux in mass% relative to the total mass of the wire: 0.2 to 2.0%] Metal carbonates act as gas generators and are decomposed by the arc heat during welding to produce CO 2It has the effect of generating gas, isolating the molten pool from the atmosphere to improve shielding, suppressing the occurrence of welding defects such as pits and blowholes, and improving the mechanical properties of the weld metal, but it also increases the amount of slag produced, which causes welding defects such as slag inclusion, so it is important to properly manage the amount added. If the total amount of one or more metal fluorine carbonates is less than 0.2%, the effect is not sufficient and welding defects such as pits and blowholes are likely to occur. On the other hand, if the total amount of one or more metal carbonates exceeds 2.0%, the arc becomes excessively strong and unstable, the amount of spatter generation increases, and the amount of slag generation increases, making it easy for slag inclusion defects to occur. Therefore, the total amount of one or more metal carbonates in the flux is 0.2 to 2.0%. The metal carbonates can be added from the flux as calcium carbonate, barium carbonate, manganese carbonate, lithium carbonate, magnesium carbonate, etc.

[0027] [Iron powder in flux as a percentage by mass relative to the total mass of the flux: 30-60%] Iron powder is contained in the flux to adjust the flux filling rate, and has the effect of improving the fluidity of the flux and stabilizing the flux filling rate. In addition, iron powder has good thermal conductivity, so it has the effect of stabilizing the arc during welding. If the iron powder is less than 30%, the flux filling rate is not stable, and the conductivity in the flux decreases, making the arc unstable and increasing the amount of spatter generation. On the other hand, if the iron powder exceeds 60%, the flux filling rate increases, causing wire breakage during the wire drawing process during manufacturing. Therefore, the iron powder in the flux is set to 30 to 60% by mass relative to the total mass of the flux. The iron powder is not particularly limited, but it is more preferable to use hydrogen-reduced iron powder or atomized iron powder from the viewpoint of ensuring the toughness of the weld metal.

[0028] [The total mass of the steel sheath and flux is Cu: 0.05 to 1.0%] Like Mn and Ni, Cu is an austenite stabilizing element, and has the effect of suppressing the coarsening of the ferrite structure and improving toughness. However, if Cu is less than 0.05%, the above effect cannot be obtained. On the other hand, if Cu exceeds 1.0%, the strength becomes excessive and the toughness decreases. Therefore, the total Cu content of the steel sheath and flux is set to 0.05 to 1.0%. Cu can be added from the flux as metallic Cu, Fe-Cu, etc.

[0029] [Li in flux in mass percent relative to total wire mass: 0.05-0.3%] Li has the effect of suppressing the occurrence of welding defects such as pits and blowholes. If Li is less than 0.05%, the above effect cannot be obtained. On the other hand, if Li exceeds 0.3%, the arc becomes unstable and the amount of spatter increases. Therefore, the Li content in the flux is set to 0.05 to 0.3%. Li can be added to the flux as lithium fluoride, lithium carbonate, etc.

[0030] [The percentage of Na oxide and K oxide in the flux in mass% relative to the total mass of the wire] 2 O conversion value and K 2 Total of type 1 or type 2 O conversion value: 0.02 to 0.15% Na oxide and K oxide have the effect of stabilizing the arc and suppressing the increase in the amount of spatter. 2 O conversion value and K 2 If the total of one or both of the O-equivalents is less than 0.02%, the above-mentioned effects cannot be obtained. 2 O conversion value and K 2 If the total of type 1 or type 2 O conversion value exceeds 0.15%, the arc length becomes extremely long, the penetration becomes shallow, slag inclusion occurs, and the arc becomes extremely unstable. Therefore, the Na oxide and K oxide in the flux 2 O conversion value and K 2 The total of type 1 or type 2 is 0.02 to 0.15% converted into O. Na oxide and K oxide can be added from the flux as powder of potash glass, soda glass, etc.

[0031] The balance of the flux-cored wire for self-shielded arc welding of the present invention is the Fe content of the steel sheath, the Fe content of the iron alloy powder such as Fe-Si, Fe-Mn, Fe-Si-Mn, Fe-Al alloy, etc., and impurities. There is no particular limitation on the impurities, but from the viewpoint of preventing hot cracking, it is preferable that P is 0.010% or less.

[0032] The flux-cored wire for self-shielded arc welding of the present invention has a structure in which flux is filled inside a steel sheath, and can be roughly divided into a seamless type in which a pipe-shaped steel sheath is filled with flux or filled with flux and then the seam of the steel sheath is welded, and a seam type in which the seam of the steel sheath is crimped without welding, and either type may be used. The flux filling rate is not particularly limited, but is preferably 10 to 30% of the total mass of the wire from the viewpoint of productivity. The outer diameter of the flux-cored wire of this embodiment is not particularly limited, but is preferably 1.6 to 3.2 mm from the viewpoint of wire production volume. EXAMPLES

[0033] The effects of the present invention will now be described in more detail with reference to examples.

[0034] A steel sheath (C: 0.001-0.10%, Si: 0.05% or less, Mn: 0.1-0.6%, P: 0.05% or less, S: 0.05% or less) was used, the steel sheath was formed into a U-shape, and filled with flux at a filling rate of 15-25%, to produce a flux-cored wire with a mass percentage relative to the total mass of the wire as shown in Table 1. The wire diameter was 2.4 mm. The flux used was dried before filling.

[0035] [Table 1]

[0036] Using the prototype flux-cored wire for self-shielded arc welding, self-shielded arc welding was performed, and a weld metal test and a welding workability evaluation were performed.

[0037] The weld metal test was conducted in accordance with JIS Z 3111:2005 and JIS Z 3313:2009 under the welding conditions shown in Table 2. The steel plate used was JIS G 3106:2020 SM490A (plate thickness 20 mm). A0 tensile test pieces and V-notch impact test pieces were taken from the center of the plate thickness of the weld metal of the obtained test specimens and used for tensile tests and impact tests, respectively.

[0038] The criteria for judging the tensile properties of the weld metal were as follows: a tensile strength in the range of 490 to 670 MPa was rated as good, and an average absorbed energy value of 3 pieces at 20°C of 27 J or more was rated as good.

[0039] In addition, after preparing the test specimens for the weld metal test, the excess metal and backing metal were ground down to the steel plate surface to make it smooth, and then an X-ray examination was carried out in accordance with JIS Z 3104:1995 to check for the presence or absence of welding defects. The results are summarized in Table 3.

[0040] The welding workability was evaluated based on the arc stability during welding in the weld metal test, the amount of spatter generated, and the quality of slag removability. Productivity was also evaluated.

[0041] (Arc stability) When the arc was stable during welding and the droplet transfer was uniform and stable, the result was rated as good, and when the droplet transfer was unstable and large spatter occurred, the result was rated as poor.

[0042] (Amount of spatter generated) It is preferable that the amount of spatter generated during welding is small. Specifically, a copper collection box was used to measure the weight of spatter generated during 1 minute of welding to determine the value per unit time (g / min). The spatter was measured five times under the welding conditions shown in Table 4, and the average value was calculated. A value of 5.0 g / min or less was considered good.

[0043] (Slag removability) It is desirable that the slag on the weld bead surface can be easily removed after welding. When removing the slag, the case where the slag can be easily removed by tapping it lightly and the case where the slag adhered to the bead surface can be easily removed with a wire brush were rated as "good", and the case where the slag remaining on the bead surface could not be easily removed even with a wire brush were rated as "bad".

[0044] (Productivity) After filling the inside of the steel sheath with flux, a wire that broke less than once during the wire drawing process was rated as good, and a wire that broke once or more was rated as poor.

[0045] [Table 2]

[0046] [Table 3]

[0047] [Table 4]

[0048] In Tables 1 and 3, wire symbols 1 to 26 are examples of the present invention, and wire symbols 27 to 38 are comparative examples. Wire symbols 1 to 26, which are examples of the present invention, have appropriate C, Mn, Al, Si, and S in the flux-cored wire for self-shielded arc welding, and the SiO of Mg, Ni, and Si oxide in the flux. 2Since the total of the F-converted values ​​of the metal fluorides, the total of one or more types of metal carbonates, and the iron powder are appropriate, productivity is good, no cracks occur in the weld metal, the arc is stable and the amount of spatter is small, slag removability is good, no welding defects such as pits, blowholes, slag inclusion, or weld metal cracks occur, and the tensile strength and absorbed energy of the weld metal are both good.

[0049] In the comparative example, wire number 27 had a high C content, so the tensile strength of the weld metal was high and the absorbed energy was low. In addition, there was a lot of iron powder, so there were many breaks during production. 2 O conversion value and K 2 The total O equivalent value was appropriate, so the arc was stable and there was little spatter. However, the Cu content was low, so the effect of improving toughness was not obtained.

[0050] Wire No. 28 had low C content, so the tensile strength of the weld metal was low and blowholes occurred in the weld. In addition, because it had a high Li content, the arc became unstable and a large amount of spatter was generated.

[0051] Wire No. 29 had a low Li content, so it was not effective in suppressing the occurrence of welding defects such as pits and blowholes. It had a high Mn content, so the tensile strength of the weld metal was high and the absorbed energy was low. Also, it had a low Al content, so blowholes occurred in the weld.

[0052] Wire No. 30 had a low Mn content, so the tensile strength and absorbed energy of the weld metal were low. 2 O conversion value and K 2 Because the total O equivalent value was high, the arc became unstable, a large amount of spatter was generated, and slag was included in the weld.

[0053] Wire No. 31 had a high Si content, so the tensile strength of the weld metal was high and the absorbed energy was low. Because it had a high Mg content, the arc was strong and unstable, and a large amount of spatter was generated.

[0054] Wire No. 32 had a high Al content, so the absorbed energy of the deposited metal was low. Also, the total F-converted value of the metal fluorides was low, so the arc was unstable, there was a lot of spatter, and blowholes occurred in the weld. In addition, the Na oxide and K oxide Na 2 O conversion value and K 2 Since the total O equivalent value was small, the effect of stabilizing the arc and suppressing the increase in the amount of spatter generation was not obtained.

[0055] Wire No. 33 had a low Mg content, so blowholes occurred in the weld and the absorbed energy of the weld metal was low. 2 O conversion value and K 2 The total O equivalent value was appropriate, so the arc was stable and there was little spatter.

[0056] Wire No. 34 had a high Ni content, so the tensile strength of the weld metal was high and the absorbed energy was low. In addition, the total amount of metal carbonates was high, so the arc was unstable, there was a lot of spatter, and slag was included in the weld.

[0057] Wire No. 35 had low Ni content, so the absorbed energy of the deposited metal was low. Also, because it had low S content, spatter increased and slag removability was poor.

[0058] Wire symbol 36 is silicon oxide (SiO 2 Because the total converted value was large, the absorbed energy of the deposited metal was low. Also, because there was little iron powder, the arc became unstable and the amount of spatter increased.

[0059] Wire No. 37 had a high total F-converted value of metal fluorides, which resulted in an unstable arc and a large amount of spatter. In addition, because it contained a lot of Cu, the tensile strength of the weld metal was high and the absorbed energy was low.

[0060] Wire number 38 had a high S content, which caused cracks in the weld. Also, the total amount of metal carbonate was low, which caused blowholes. Also, the appropriate amount of Cu caused the absorbed energy of the weld metal to be high.

Claims

1. In a flux-cored wire for self-shielded arc welding, which is made by filling a steel sheath with flux, the total mass of the steel sheath and the flux is, in mass %, C: 0.04-0.12%, Mn: 1.0 to 2.5%, Al: 1.0-3.0%, Si: 0.5% or less, S: 0.016 to 0.04%; Furthermore, in the flux, the mass percentage relative to the total mass of the wire is: Mg: 1.0-3.0%, Ni: 0.1 to 3.0%, Silicon oxide SiO 2 Total of conversion values: 0.5% or less, Total F-converted value of metal fluorides: 1.5 to 5.0%, Contains one or more metal carbonates in total: 0.2 to 2.0%; Furthermore, in terms of mass% relative to the total mass of the flux, Iron powder: contains 30-60% A flux-cored wire for self-shielded arc welding, the balance of which consists of the Fe content of the steel sheath, the Fe content of the iron alloy powder, and impurities.

2. The total mass of the wire is calculated by the mass percentage of the steelmaking sheath and flux. Cu: 0.05-1.0% 2. The flux-cored wire for self-shielded arc welding according to claim 1, further comprising:

3. The total of one or more of the metal fluorides and metal carbonates in the flux in terms of Li, expressed as a percentage by mass relative to the total mass of the wire. Li: 0.05-0.3% 3. The flux-cored wire for self-shielded arc welding according to claim 1, further comprising:

4. The Na content of Na oxide and K oxide in the flux in mass% relative to the total mass of the wire 2 O conversion value and K 2 The flux-cored wire for self-shielded arc welding according to claim 1 or 2, further comprising one or two types of O in total: 0.02 to 0.15% in terms of O.

5. The total of one or more of the metal fluorides and metal carbonates in the flux converted into Li, expressed as a percentage by mass relative to the total mass of the wire, is Li: 0.05 to 0.3%; and the total of one or more of the metal fluorides and metal carbonates in the flux converted into Li, expressed as a percentage by mass relative to the total mass of the wire, is Na: 0.05 to 0.3%. 2 O conversion value and K 2 The flux-cored wire for self-shielded arc welding according to claim 1 or 2, further comprising one or two types of O in total: 0.02 to 0.15% in terms of O.

Citation Information

Patent Citations

  • Flux cored wire for self-shielded arc welding

    JP1990075495A

  • Flux-cored wire

    JP2017196651A

  • Flux-cored wire for self-shielded arc welding

    JP2021167019A

  • Self-shielded flux cored electrode for fracture critical applications

    US20060096966A1

  • Flux-cored wire for self-shielded arc welding

    JP1987238097A