Method for producing catalyst for production of unsaturated aldehydes and unsaturated carboxylic acids
By controlling storage conditions such as temperature, light shielding, and moisture impermeability, the catalyst composition is stabilized, improving yield and selectivity in the production of unsaturated aldehydes and unsaturated carboxylic acids.
Patent Information
- Application Number
- JP2024006491
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-01-19
- Publication Date
- 2024-10-11
AI Technical Summary
Existing methods for producing unsaturated aldehydes and unsaturated carboxylic acids face challenges in achieving high yield and selectivity, with catalysts deteriorating due to inadequate storage conditions of ammonium molybdate, leading to increased production costs and reduced catalyst life.
Controlled storage conditions for ammonium molybdate, including temperature, light shielding, moisture impermeability, and humidity, to stabilize the catalyst composition and improve yield and selectivity.
The method enhances catalyst performance in gas-phase catalytic oxidation reactions, particularly for producing unsaturated aldehydes and unsaturated carboxylic acids, by maintaining catalyst stability and efficiency.
Smart Images

Figure 2024144109000001 
Figure 2024144109000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel catalyst which can obtain a target product in high yield, and in particular which can realize a high yield when an unsaturated aldehyde or an unsaturated carboxylic acid is oxidatively produced. [Background technology]
[0002] Methods for producing the corresponding unsaturated aldehydes and unsaturated carboxylic acids using propylene, isobutylene, t-butyl alcohol, etc. as raw materials are widely used industrially, and many reports have been made on means for improving the yield and catalytic activity (e.g., Patent Document 1, etc.).
[0003] For example, Patent Document 2 focuses on a specific property of the catalyst, specifically, it describes that a catalyst with high yield and high selectivity can be obtained by controlling the ratio Ri=Pi / Ph of the intensity Pi of the diffraction peak (i) of β-Bi2Mo2O9 appearing at 2θ=27.76±0.1° to the intensity Ph of the diffraction peak (h) of CoMoO4 appearing at 2θ=26.5±0.1° in the X-ray diffraction pattern using Cu-Kα radiation of the catalytically active component within the range of 0.4 to 2.0. Similarly, Patent Document 3 describes that the catalytic performance such as catalytic activity and selectivity can be improved by controlling the crystallinity T in the range of 2θ=5° to 90° measured by X-ray diffraction analysis using Cu-Kα radiation of the catalytically active component within the range of 4% to 18%.
[0004] Patent Document 4 discloses a method for improving the yield of a catalyst produced by using an aqueous solution of ammonium heptamolybdate (sometimes abbreviated as ammonium molybdate or molyan in this specification) used as a raw material by adjusting the turbidity of the solution to a specific range. Patent Document 5 discloses a method for improving the yield of a catalyst by selecting and using a raw material molybdate that exhibits specific physical properties.
[0005] Even though the above-mentioned measures have been improved, there is a demand for further improvement in yield and catalytic activity in the production of corresponding unsaturated aldehydes and / or unsaturated carboxylic acids by partial oxidation of propylene, isobutylene, t-butyl alcohol, etc. For example, the yield of the target product determines the amount of propylene, isobutylene, t-butyl alcohol, butenes, etc. required for production, and has a significant impact on the production cost. In addition, the catalytic activity determines the reaction bath temperature when producing the target product, and when a catalyst with low activity is used, the reaction bath temperature must be increased to maintain the yield of the target product. This causes the catalyst to be thermally stressed, causing a decrease in selectivity and yield, and also shortening the catalyst life. Furthermore, as a raw material used in catalysts, although there was a certain amount of knowledge regarding the properties of molyammonium chloride and the performance of catalysts manufactured using this molyammonium chloride as described in the above-mentioned Patent Document 5, this method is not suitable as a manufacturing method for industrial catalysts. This is because the manufacturing method described in Patent Document 5 means that molyammonium chloride that does not exhibit a specific physical property is excluded and not used, which is inefficient because it incurs the cost of disposing of molyammonium chloride that does not exhibit a specific physical property, and the cost of changing the manufacturing schedule if it is found that molyammonium chloride does not exhibit a specific physical property just before manufacturing. In other words, rather than selecting the optimal molyammonium chloride as described in conventional publicly known documents, it was potentially necessary to clarify the storage conditions of molyammonium chloride and to comply with these. As for the storage conditions of molyammonium chloride, the SDS states, as with general industrial raw materials or reagents, "The storage area should be equipped with lighting and ventilation equipment necessary for storing or handling dangerous and harmful substances. Store in a cool, dark place away from direct sunlight." (Non-Patent Document 2). However, there are the following improvements to these conventional storage conditions. First, it was unclear to those skilled in the art which of the factors of the above storage conditions (illuminance of lighting, storage temperature, ventilation volume of the surrounding environment, storage humidity, and the relationship between these factors and the storage period) was important, and further, how to quantitatively control the numerical range of each of these factors to produce a catalyst without deteriorating its performance and / or stably. Furthermore, from the viewpoint of the production cost of an industrial catalyst, it is not preferable to improve the storage conditions more than necessary. For example, it was thought that if Moriyan was stored in a cool and dark place, Moriyan would not deteriorate and the performance of the catalyst as a final product would not be a problem, based on the description in the above SDS, but the present inventors have made it clear for the first time that such storage conditions lead to an increase in the catalyst cost as a final product, and that it is not preferable because Moriyan deteriorates if the storage temperature is too low, as described below. Thus, the storage conditions described in conventional SDS alone were insufficient for the industrial use of catalytic ammonium phosphate. However, the inventors have identified important storage condition factors (storage temperature and storage period parameters, storage absolute humidity and storage period parameters, and cumulative global solar radiation) and further discovered the numerical ranges for which these should be controlled, thereby creating the present invention. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2016 / 136882 [Patent Document 2] JP 2017-024009 A [Patent Document 3] International Publication No. 2010 / 038677 [Patent Document 4] JP 2015-147188 A [Patent Document 5] Japanese Patent No. 7024194 [Non-patent literature]
[0007] [Non-Patent Document 1] Hort Science,No.18,6 P818-822 (1983) [Non-Patent Document 2] Ministry of Health, Labor and Welfare. "Safety Data Sheet Ammonium Molybdate". Workplace Safety Site. 2019 / 03 / 15. https: / / anzeninfo.mhlw.go.jp / anzen / gmsds / 12027-67-7.html Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention proposes a method for producing a catalyst used in a process for producing corresponding unsaturated aldehydes and unsaturated carboxylic acids using propylene, isobutylene, t-butyl alcohol, etc. as raw materials, which has high selectivity for the target compound, high yield, and is stable. [Means for solving the problem]
[0009] According to the research of the present inventors, by controlling the storage of ammonium molybdate used as a molybdenum raw material under specific conditions, it has been discovered that the performance of the final catalyst, particularly the selectivity and yield, is improved, and it has further been found that the catalyst can be manufactured more stably, and thus the present invention has been completed.
[0010] That is, the present invention relates to the following 1) to 6). 1) The composition of the catalyst active component is represented by the following general formula (1A) or (1B), Mo a1 Bi b1 Ni c1 Co d1 Fe e1 X f1 Y g1 Z h1 O i1 ···(1A) (In the formula, Mo, Bi, Ni, Co, and Fe each represent molybdenum, bismuth, nickel, cobalt, and iron, X represents at least one element selected from tungsten, antimony, tin, zinc, chromium, manganese, magnesium, silicon, aluminum, cerium, and titanium, Y represents at least one element selected from sodium, potassium, cesium, rubidium, and thallium, Z belongs to Groups 1 to 16 of the periodic table and means at least one element selected from elements other than the above Mo, Bi, Ni, Co, Fe, X, and Y, and a1, b1, c1, d1, e1, f1, g1, h1, and i1 each represent the number of atoms of molybdenum, bismuth, nickel, cobalt, iron, X, Y, Z, and oxygen, and when a1 = 12, 0 < b1 ≤ 7, 0 ≤ c1 ≤ 10, 0 < d1 ≤ 10, 0 < c1 + d1 ≤ 20, 0 < e1 ≤ 5, 0 ≤ f1 ≤ 2, 0 ≤ g1 ≤ 3, 0 ≤ h1 ≤ 5, and i1 is a value determined by the oxidation state of each element), Mo 12 V a W b Cu c Sb d X e Y f Z g O h ···(1B) (In the formula, Mo, V, W, Cu, Sb, and O represent molybdenum, vanadium, tungsten, copper, antimony, and oxygen, respectively; X represents at least one element selected from the group consisting of alkali metals and thallium; Y represents at least one element selected from the group consisting of magnesium, calcium, strontium, barium, and zinc; Z represents at least one element selected from the group consisting of bismuth, tellurium, silver, selenium, silicon, aluminum, boron, niobium, cerium, tin, chromium, manganese, iron, cobalt, nickel, samarium, germanium, zirconium, titanium, chromium, tantalum, lead, indium, sulfur, palladium, gallium, lanthanum, and arsenic. Also, a, b, c, d, e, f, g, and h represent the atomic ratios of the respective elements. With respect to 12 molybdenum atoms, 0 < a ≤ 10.0, 0 ≤ b ≤ 10.0, 0 < c ≤ 6.0, 0 ≤ d ≤ 10.0, 0 ≤ e ≤ 0.50, 0 ≤ f ≤ 1.0, 0 ≤ g < 6.0. Further, h is the number of oxygen atoms necessary to satisfy the valences of the respective components.) A method for producing a catalyst for producing an unsaturated aldehyde and / or an unsaturated carboxylic acid, wherein the storage conditions of ammonium heptamolybdate used as a molybdenum raw material include the following Condition 1. Condition 1: Stored in a light-shielding and moisture-impermeable container, and satisfying the following formula (2) during the entire storage period history exp (保管温度[℃]-50) × number of storage days [days] ≤ 5200 ··· (2) However, the light-shielding container is a container having a light-shielding rate (measured by a method according to JIS L 1055) of visible light and / or ultraviolet light of 95% or more, and the moisture-impermeable container is a container having a moisture permeation amount (moisture permeability) of less than 5 g / (m 2 ·24 hours) per 24 hours. Also, the storage temperature is the average temperature of the stored ammonium molybdate itself during the storage period. 2) The composition of the catalyst active component is represented by the following general formula (1A) or (1B), Mo a1 Bi b1 Ni c1 Co d1 Fee1 X f1 Y g1 Z h1 O i1 ···(1A) (wherein Mo, Bi, Ni, Co and Fe represent molybdenum, bismuth, nickel, cobalt and iron respectively, X represents at least one element selected from tungsten, antimony, tin, zinc, chromium, manganese, magnesium, silicon, aluminum, cerium and titanium, Y represents at least one element selected from sodium, potassium, cesium, rubidium, and thallium, Z belongs to Groups 1 to 16 of the periodic table and means at least one element selected from elements other than the above Mo, Bi, Ni, Co, Fe, X, and Y, and a1, b1, c1, d1, e1, f1, g1, h1, and i1 represent the number of atoms of molybdenum, bismuth, nickel, cobalt, iron, X, Y, Z and oxygen respectively, when a1 = 12, 0 < b1 ≦ 7, 0 ≦ c1 ≦ 10, 0 < d1 ≦ 10, 0 < c1 + d1 ≦ 20, 0 < e1 ≦ 5, 0 ≦ f1 ≦ 2, 0 ≦ g1 ≦ 3, 0 ≦ h1 ≦ 5, and i1 = a value determined by the oxidation state of each element), Mo 12 V a W b Cu c Sb d X e Y f Z g O h ···(1B) (In the formula, Mo, V, W, Cu, Sb, and O represent molybdenum, vanadium, tungsten, copper, antimony, and oxygen, respectively; X represents at least one element selected from the group consisting of alkali metals and thallium; Y represents at least one element selected from the group consisting of magnesium, calcium, strontium, barium, and zinc; Z represents at least one element selected from the group consisting of bismuth, tellurium, silver, selenium, silicon, aluminum, boron, niobium, cerium, tin, chromium, manganese, iron, cobalt, nickel, samarium, germanium, zirconium, titanium, chromium, tantalum, lead, indium, sulfur, palladium, gallium, lanthanum, and arsenic. Also, a, b, c, d, e, f, g, and h represent the atomic ratios of the respective elements. With respect to 12 molybdenum atoms, a satisfies 0 < a ≤ 10.0, b satisfies 0 ≤ b ≤ 10.0, c satisfies 0 < c ≤ 6.0, d satisfies 0 ≤ d ≤ 10.0, e satisfies 0 ≤ e ≤ 0.50, f satisfies 0 ≤ f ≤ 1.0, g satisfies 0 ≤ g < 6.0. Further, h is the number of oxygen atoms required to satisfy the valences of the respective components.) A method for producing a catalyst for producing an unsaturated aldehyde and / or an unsaturated carboxylic acid, wherein the storage conditions of ammonium heptamolybdate used as a molybdenum raw material include the following Condition 2. Condition 2: The storage temperature during the period is 45°C or lower and it is stored in a moisture-impermeable container, and satisfies the following formula (3) among the histories of all storage periods The cumulative total daily solar radiation amount [MJ / m 2 ≤ 345 ··· (3) 3) The composition of the catalyst active component is represented by the following general formula (1A) or (1B), Mo a1 Bi b1 Ni c1 Co d1 Fe e1 X f1 Y g1 Z h1 O i1 ··· (1A) (wherein Mo, Bi, Ni, Co, and Fe represent molybdenum, bismuth, nickel, cobalt, and iron respectively, X represents at least one element selected from tungsten, antimony, tin, zinc, chromium, manganese, magnesium, silicon, aluminum, cerium, and titanium, Y represents at least one element selected from sodium, potassium, cesium, rubidium, and thallium, Z belongs to Groups 1 to 16 of the periodic table and means at least one element selected from elements other than the above Mo, Bi, Ni, Co, Fe, X, and Y, and a1, b1, c1, d1, e1, f1, g1, h1, and i1 represent the number of atoms of molybdenum, bismuth, nickel, cobalt, iron, X, Y, Z, and oxygen respectively, and when a1 = 12, 0 < b1 ≦ 7, 0 ≦ c1 ≦ 10, 0 < d1 ≦ 10, 0 < c1 + d1 ≦ 20, 0 < e1 ≦ 5, 0 ≦ f1 ≦ 2, 0 ≦ g1 ≦ 3, 0 ≦ h1 ≦ 5, and i1 is a value determined by the oxidation state of each element), Mo 12 V a W b Cu c Sb d X e Y f Z g O h ···(1B) (In the formula, Mo, V, W, Cu, Sb, and O represent molybdenum, vanadium, tungsten, copper, antimony, and oxygen, respectively; X represents at least one element selected from the group consisting of alkali metals and thallium; Y represents at least one element selected from the group consisting of magnesium, calcium, strontium, barium, and zinc; Z represents at least one element selected from the group consisting of bismuth, tellurium, silver, selenium, silicon, aluminum, boron, niobium, cerium, tin, chromium, manganese, iron, cobalt, nickel, samarium, germanium, zirconium, titanium, chromium, tantalum, lead, indium, sulfur, palladium, gallium, lanthanum, and arsenic. Also, a, b, c, d, e, f, g, and h represent the atomic ratios of the respective elements. With respect to 12 molybdenum atoms, 0 < a ≤ 10.0, 0 ≤ b ≤ 10.0, 0 < c ≤ 6.0, 0 ≤ d ≤ 10.0, 0 ≤ e ≤ 0.50, 0 ≤ f ≤ 1.0, 0 ≤ g < 6.0. Further, h is the number of oxygen atoms necessary to satisfy the valences of the respective components.) A method for producing a catalyst for producing an unsaturated aldehyde and / or an unsaturated carboxylic acid, wherein the storage conditions of ammonium heptamolybdate used as a molybdenum raw material include the following Condition 3. Condition 3: Stored in a light-shielding container and satisfying the following formula (4) during the history of all storage periods Storage absolute humidity [g / m 3 × number of storage days [days] ≤ 12.0 ··· (4) 4) A method for producing a catalyst in which ammonium heptamolybdate used as a molybdenum raw material is stored under storage conditions including two or more of the above Conditions 1 to 3, and the method for producing a catalyst for producing an unsaturated aldehyde and / or an unsaturated carboxylic acid according to any one of the above 1) to 3) satisfying the following formula (5). exp (保管温度[℃]-50) × number of storage days [days] / 5200 + cumulative total daily solar radiation amount [MJ / m 2 / 345 + storage absolute humidity [g / m 3 × number of storage days [days] / 12.0 ≤ 1.0 ··· (5) 5) A method for producing a catalyst for producing an unsaturated aldehyde and / or an unsaturated carboxylic acid, comprising the steps of: preparing a mixture of ammonium heptamolybdate stored under the storage conditions described in any one of 1) to 3) above and water; adding other raw materials; and obtaining an aqueous solution or aqueous slurry. 6) A method for producing a catalyst for producing an unsaturated aldehyde and / or an unsaturated carboxylic acid, comprising subjecting the aqueous solution or aqueous slurry described in 5) above to the following steps (a) to (c): (a) drying the aqueous solution or aqueous slurry to obtain a dry product; (b) forming the dried slurry obtained in step (a) into a formed product; (c) A step of firing the molded product obtained in step (b) in an atmosphere having a controlled oxygen concentration. Effect of the Invention
[0011] The catalyst produced by the production method of the present invention is extremely effective in improving the catalytic performance, particularly the yield and selectivity, in gas-phase catalytic oxidation reactions, and is particularly useful as an oxidation catalyst for producing the corresponding unsaturated aldehydes and unsaturated carboxylic acids using propylene, isobutylene, t-butyl alcohol, etc. as raw materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] [Storage conditions for ammonium heptamolybdate] The ammonium heptamolybdate used in the production of the catalyst of the present invention is characterized in that it has been stored so as to include the following condition 1. Here, the term "include" means that the material stored substantially under condition 1 falls within the technical scope of the present invention, and does not fall outside the technical scope even if it has been temporarily placed under conditions other than condition 1. Similarly, it is also preferable that the material has been stored so as to include condition 2 or 3.
[0013] <Condition 1> Condition 1 relates to the temperature surrounding the Moriyasu, and is a condition in which the product is stored in a light-proof, moisture-tight container and the following formula (2) is satisfied throughout the entire storage period. [Formula (2)] exp (保管温度[℃]-50) × number of storage days [days]≦5200···(2) Catalysts manufactured using molybdenum that meets these conditions are very effective in improving the catalytic performance, especially the yield and selectivity, in gas-phase catalytic oxidation reactions. Equation (2) was obtained empirically, and the detailed mechanism is unknown, but exp (保管温度[℃]-50) The term can also be interpreted as the form of the reaction rate of deterioration of Morian. In other words, if the temperature of the storage environment is high, the deterioration will be exponentially faster, and the longer the storage period in that environment, the more linear the deterioration will progress, and Morian should be stored to avoid these. In this invention, the storage temperature refers to the temperature of the stored Morian itself, averaged over the storage period. For example, if the average temperature in the environment in which Morian is stored is 50°C, but the temperature of the Morian itself stored in a light-proof, moisture-impermeable container is 25°C on average over the storage period, the storage temperature to be entered into formula (2) is 25°C. Such storage temperatures are measured by thermocouples or temperature loggers installed in Morian, or simply by stickers or paints that record thermal history. However, as an exception to the above calculation, if the maximum temperature of Morian during the storage period exceeds 50°C, the storage temperature in formula (2) is defined as the average temperature of Morian itself during the storage period when it exceeded 50°C, and the number of storage days in formula (2) is defined as the storage period when the temperature of Morian itself exceeded 50°C. (exp (保管温度[℃]-50) The upper limit of the storage period is 5200 days, but the preferred range is 5000 days, 4600 days, 4300 days, 4000 days, 3700 days, 3300 days, 3500 days, 3000 days, 2700 days, 2500 days, 2300 days, 2000 days, 1700 days, 1500 days, and 1300 days, with 1000 days being particularly preferred, and 100 days being most preferred. The lower limit is 0 days, i.e., storage at a temperature lower than 50°C. The storage temperature has a lower limit, preferably 0°C. The lower limit is preferably 1°C, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C, 9°C, and most preferably 10°C. Conventionally, storage in a cool and dark place was a well-known storage condition for Morian, but as a result of the study by the inventors, it became clear that even if the conditions for cool and dark storage were met, if the storage temperature was too low, Morian would deteriorate and the performance of the catalyst produced using this Morian would also deteriorate. If the storage temperature is set lower than necessary, the storage cost of Morian would increase, and as a result, the production cost of the catalyst would also increase, so a lower limit should be set for the storage temperature. This lower limit of the storage temperature is also applied to Condition 2 and Condition 3 described below. In this specification, the storage period means the period from when the catalyst raw material to be stored is manufactured to when it is transported, received, stored, and used in the manufacturing process as a catalyst raw material. In addition, in this specification, "Meeting condition ○ during the entire storage period history" means that the conditions (conditions 1 to 3) indicated with ○ are met during all or part of the storage period, and the calculation of condition ○ includes the cumulative value during the storage period. In other words, taking the above condition 1 as an example, during the entire storage period of Moriyasu, at time A, it was stored in a light-proof and moisture-impermeable container at a storage temperature of 55°C for 13.5 days (i.e., 10 days after exp under condition 1 at time A). (保管温度[℃]-50) × storage period is 2004 days), then the temperature is controlled at a temperature lower than 50°C, and then in period B, the storage temperature is 56°C for 10 days in a light-proof and moisture-impermeable container (i.e., exp (保管温度[℃]-50) × 4034 days), the cumulative exp (保管温度[℃]-50) × The number of storage days is 6038 days, which means that it is determined that it does not meet condition 1. The same concept applies to conditions 2 and 3 below. From formula (2), it can be understood by numerical calculation that, although it depends on the storage period, if the storage temperature of molasses is less than 50°C, it will not affect the catalytic performance, and that it is not essential to store it in a cool, dark place as described in the SDS, and for example, it is not necessary to store it refrigerated at 5°C (and therefore there is no need to incur refrigeration costs). In this way, from the viewpoint of catalytic performance, the critical value of the storage temperature within the range of realistic storage costs for an industrial catalyst is clarified for the first time by the present invention.
[0014] <Condition 2> Condition 2 concerns the amount of light received by Moriyasu, and requires that the storage temperature during the storage period be below 45°C and that it be stored in a moisture-impermeable container, and that the following formula (3) be satisfied throughout the entire storage period history. [Formula (3)] Accumulative total solar radiation during storage period [MJ / m 2 ]≦345 (3) Catalysts manufactured using molyammonium hydroxide that meets these conditions are extremely effective in improving the catalytic performance, especially the yield and selectivity, in gas-phase catalytic oxidation reactions. Equation (3) was obtained empirically, and the detailed mechanism is unknown, but it is believed that a high cumulative amount of global solar radiation during storage will promote the decomposition of molyammonium hydroxide due to high temperatures and / or ultraviolet rays during the day, and due to the temperature difference between daytime and nighttime, and molyammonium hydroxide should be stored in a way that avoids this. The upper limit of (cumulative global solar radiation during storage) is 345MJ / m 2 However, the preferred order is 320MJ / m 2 , 300MJ / m 2 , 280MJ / m 2 , 260MJ / m 2 , 240MJ / m 2 , 220MJ / m 2 , 200MJ / m 2 , 180MJ / m 2 , 160MJ / m 2 , 140MJ / m 2 , 120MJ / m 2 , 100MJ / m 2 , 75MJ / m 2 , 50MJ / m2 and most preferably 50MJ / m 2 The lower limit is 10MJ / m 2 In other words, the storage conditions should be such that the container is almost completely shielded from light, as described above. Here, the unit of global solar radiation is MJ / m 2 However, the case where the unit is appropriately converted is also included in the present application. In other words, when converting to the time integral value of the photon flux density according to Non-Patent Document 1, the global solar radiation [MJ / m 2 ] is multiplied by 4.57 to get the unit mol / m 2 When converted to the time integral value of illuminance, it is expressed as the total solar radiation [MJ / m 2 ] is divided by 54 to obtain the time integral value of illuminance in Mlux s. From equation (3), even if Moriyasu is stored for two full years at an illuminance of, for example, about 0.1 lux (night sky under a full moon), the total solar radiation is 341 MJ / m 2 According to the present invention, the catalyst performance is not affected and the catalyst can be stably produced. That is, although it is necessary to store the catalyst in a cool and dark place as described in the SDS, it is not necessarily necessary to store the catalyst in a completely dark room. It can be understood from numerical calculations that storage in a metal steel drum or aluminum pouch and fiber drum, which are both practical for industrial catalyst raw materials, is sufficient. In this way, the critical value of the amount of global solar radiation within the range of practical storage costs for industrial catalysts from the viewpoint of catalyst performance is clarified for the first time by the present invention.
[0015] <Condition 3> Condition 3 concerns the temperature and humidity surrounding Moriyasu, and is a condition in which the product is stored in a light-proof container and the following formula (4) is satisfied throughout the entire storage period. [Formula (4)] Storage absolute humidity [g / m 3 ] × number of storage days [days]≦12.0···(4) Catalysts manufactured using molyammonium hydroxide that satisfies these conditions are extremely effective in improving the catalytic performance, particularly the yield and selectivity, in gas-phase catalytic oxidation reactions. Equation (4) was obtained empirically, and the detailed mechanism is unknown, but it is believed that a high storage absolute humidity will promote the decomposition of molyammonium hydroxide due to its moisture absorption and due to the independent contribution of condition 1 mentioned above, and molyammonium hydroxide should be stored in a manner that avoids this. In this invention, the storage absolute humidity refers to the absolute humidity in the immediate vicinity of the stored molyammonium hydroxide, averaged over the storage period, and if the molyammonium hydroxide is placed in a container, it refers to the absolute humidity inside the container. For example, if the average absolute humidity in the environment in which the molyammonium hydroxide is stored is 10 g / m 3 However, when Moriyasu was stored in a light-shielding container, the absolute humidity inside the container averaged 1.0 g / m 3 In this case, the storage absolute humidity to be entered into formula (4) is 1.0 g / m 3 This average absolute humidity is measured by a humidity logger installed in the container or at Moriyasu, or more simply, by a sticker or paint that records the humidity history. [Storage absolute humidity [g / m 3 The upper limit for [days] × storage period is 12.0 g / m 3 ・days, but the preferred order is 11.0g / m 3 ·day, 10.0g / m 3 ·day, 9.0g / m 3 g / m 3 ·day, 8.0g / m 3 ·day, 7.0g / m 3 ·day, 6.0g / m 3 ·day, 5.0g / m 3 ·day, 4.0g / m 3 ·day, 3.0g / m 3 10 g / m 3 ·days. The lower limit is 1.0 g / m 3 A few days will be fine. From equation (4), although it depends on the storage period, the realistic storage conditions for molybdenum are as follows: if molybdenum is placed in a moisture-impermeable container and the dead volume (space not filled with molybdenum) in the container is sufficiently small, the absolute temperature in the container will be 1.0 g / m on average during the storage period. 3It can be seen from numerical calculations that the absolute humidity in storage is about the same as that in the conventional catalysts, and does not affect the catalyst performance, i.e., storage in a room with controlled humidity is not necessarily required (hence, there is no need to incur storage costs). In this way, the critical value of the absolute humidity for storage within the range of realistic storage costs for industrial catalysts from the viewpoint of catalyst performance is clarified for the first time by the present invention.
[0016] In addition, when two or more of conditions 1 to 3 are used in combination during the entire storage period history, the technical scope shall be judged by converting the percentage to the upper limit. For example, if storage is performed under condition 1 such that the value of formula (2) is 2600 days, and then / or during the same period, storage is performed under condition 3 such that the value of formula (4) is 6.0 g / day m 3 If stored as follows, the result would be 2600 days / 5200 days + 6.0g / m 3 Days / 12.0g / m 3 As a similar example, if the storage temperature is 60°C and the storage is in a non-light-shielding container, and the value of formula (2) is 2600 days, and the value of formula (3) is 172 MJ / m during the same period, 2 If stored as follows, the rate is 2600 days / 5200 days + 172 MJ / m 2 / 345MJ / m 2 = 1.0, which means that the storage falls within the technical scope of the present invention. By quantifying the degree of deterioration of molasses under various storage conditions as in the present invention, if it is discovered that molasses has been transported under high temperature conditions, for example, further deterioration of molasses can be suppressed by taking precautions in the subsequent storage process to ensure that the storage temperature and total solar radiation amount fall within the ranges of the present invention, which is also something that was not present in conventional knowledge. As for the storage conditions of Moriyasu, the SDS states that "The storage area should be equipped with lighting and ventilation facilities necessary for storing or handling hazardous or harmful materials. Store in a cool, dark place away from direct sunlight," just like general industrial raw materials or reagents. However, it can be said that the conditions for storing Moriyasu (storage in the present invention) throughout the entire process from when it is manufactured as a raw material to when it is used, as well as the storage from when it is received as a raw material until it is used, are important. However, it has remained unclear to those skilled in the art which of these storage condition factors (illuminance of lighting, storage temperature, ventilation volume of the surrounding environment, storage humidity) is important, and furthermore, what the critical numerical ranges are for these important factors that affect the performance of the catalyst as a final product. In addition, from the viewpoint of the manufacturing cost and the specifications of the manufacturing equipment as an industrial catalyst, it is not desirable to improve the storage conditions more than necessary. That is, the essence of this application is to provide storage conditions for Moriyan that can ensure the catalyst performance at a realistic cost as an industrial catalyst raw material. In other words, the specifications of the storage container, factors that should be specified during storage (storage temperature, illuminance received by Moriyan during storage (cumulative total solar radiation during the storage period), and humidity received by Moriyan during storage (storage absolute humidity)), and further, the numerical ranges of these factors are specified and provided within realistic ranges suitable for industrial catalysts. According to the findings of the present inventors, even if a catalyst manufacturer receives moriyan and stores it in a cool, dark place, if the moriyan is temporarily exposed to high temperatures during the process before or after, i.e., before transportation or preparation, the catalyst using the moriyan may have insufficient performance or problems may occur during preparation. In other words, it is necessary to consider the storage conditions (= storage conditions in this invention) of moriyan not only during the storage from when it is received as a raw material until it is used in catalyst production, but also during the entire process from when it is manufactured as a raw material until it is used. As for the publicly known storage conditions of Moriyasu, the SDS states that, like general industrial raw materials or reagents, "the storage area should be provided with lighting and ventilation equipment necessary for storing or handling hazardous or harmful materials. Store in a cool, dark place away from direct sunlight" (Non-Patent Document 2). However, under such conventional storage conditions, it is unclear which of the factors in the storage conditions (illuminance of lighting, storage temperature, ventilation volume of the surrounding environment, storage humidity) is important, and it is unclear to those skilled in the art how to control the quantitative thresholds of the parameters that take into account the storage period and each of the above factors, so that the catalyst can be produced stably and / or without deteriorating the performance of the catalyst. In response to this, the present inventors have diligently studied and found important storage condition factors (parameters of storage temperature and storage period, parameters of storage absolute humidity and storage period, and cumulative total solar radiation), and further found the numerical ranges to be controlled for these, leading to the creation of the present invention. In addition, as another aspect that has been revealed for the first time as a result of the inventors' studies, it can be mentioned that they have found appropriate storage conditions from the viewpoint of production costs as an industrial catalyst. That is, as mentioned above, it is not the case that a low storage temperature is good, but rather that too low a storage temperature is undesirable because it deteriorates molyammonium salt. Thus, the conventional storage conditions described in the SDS alone were insufficient for industrial use of molyammonium salt for the catalyst of the present invention, but the present inventors quantitatively discovered new parameters, including time, as storage conditions for molyammonium salt, and the numerical range to be controlled, leading to the creation of the present invention.
[0017] The containers in the above conditions 1 to 3 are described below. In the present invention, a light-shielding container is a container with a visible light and / or ultraviolet light shielding rate (measured by a method conforming to JISL 1055) of 95% or more, specifically, a plastic bag with metal vapor deposition such as an aluminum pouch, various metal drums such as steel drums and stainless steel drums, and various colored plastics (for example, high-density polyethylene) with a thickness of 3 mm or more, wood, enamel, and ceramics, and all containers are included in the present application regardless of their shape and color as long as they do not have gaps of 1 mm or more that allow light to enter. As a special example of a light-shielding container, a plastic bag and a container that are partially or entirely lined with a black material inside the container so that ambient light can be absorbed even if it enters the container are also included in the category of the light-shielding container of the present invention. Furthermore, storage in a non-light-shielding container in an environment without windows and where visible light and / or ultraviolet light does not enter from the surroundings is also included in storage in a light-shielding container. That is, storage in a light-shielding container in the present invention includes storage of the molten metal in an environment that is almost free of visible light and / or ultraviolet light. In the present invention, a moisture-impermeable container is a container having a moisture permeability of 5 g / (m 224 hours), and the material is, for example, acrylic resin, polystyrene, PET, AS resin, polyvinyl chloride, polyethylene, polypropylene, ABS resin, phenolic resin, or aluminum-pouched one of these, preferably polyethylene or aluminum-pouched polyethylene, and the thickness of the plastic bag is not limited as long as it satisfies the above-mentioned moisture permeability, but is preferably 0.01 mm or more and 0.1 mm or less, and its shape is not limited. In addition, plastic bags and containers equipped with a gas adsorbent or desiccant that can remove the surrounding atmosphere, especially moisture, even if it is mixed into the container, also belong to the category of containers of the present invention. Similarly, when storing in an environment where a gas adsorption device or desiccant device is installed to remove moisture, it is considered to be stored in a moisture-impermeable container regardless of the type of container the molten metal is put into. In other words, storage in a moisture-impermeable container in the present invention includes storage of the molten metal in a low-humidity environment.
[0018] [Catalyst composition of formula (1A)] The catalyst for producing an unsaturated aldehyde produced by the production method of the present invention has a composition of catalytically active components represented by the following formula (1A). [Formula (1A)] Mo a1 Bi b1 Ni c1 Co d1 Fe e1 X f1 Y g1 Z h1 O i1 (1A) (In the formula, Mo, Bi, Ni, Co, and Fe represent molybdenum, bismuth, nickel, cobalt, and iron respectively, X represents at least one element selected from tungsten, antimony, tin, zinc, chromium, manganese, magnesium, silicon, aluminum, cerium, and titanium, Y represents at least one element selected from sodium, potassium, cesium, rubidium, and thallium, Z belongs to Group 1 to Group 16 of the periodic table and means at least one element selected from elements other than the above Mo, Bi, Ni, Co, Fe, X, and Y, and a1, b1, c1, d1, e1, f1, g1, h1, and i1 represent the number of atoms of molybdenum, bismuth, nickel, cobalt, iron, X, Y, Z, and oxygen respectively. When a1 = 12, 0 < b1 ≦ 7, 0 ≦ c1 ≦ 10, 0 < d1 ≦ 10, 0 < c1 + d1 ≦ 20, 0 < e1 ≦ 5, 0 ≦ f1 ≦ 2, 0 ≦ g1 ≦ 3, 0 ≦ h1 ≦ 5, and i1 is a value determined by the oxidation state of each element.)
[0019] In the above formula (1A), when a1 = 12, the preferable ranges of b1 to h1 are as follows. The lower limits of b1 are preferably 0.1, 0.2, 0.3, 0.4, 0.5 in this order, and the upper limits are preferably 6, 5, 4, 3, 2 in this order. That is, the most preferable range of b1 is 0.5 or more and 2 or less. The lower limits of c1 are preferably 0.2, 0.5, 0.8, 1.0, 1.5, 1.8, 2.0, 2.5 in this order, and the upper limits are preferably 8, 7, 6, 5, 4, 3.5 in this order. That is, the most preferable range of c1 is 2.5 or more and 3.5 or less. The lower limits of d1 are preferably 1, 2, 3, 4, 5, 6 in this order, and the upper limits are preferably 9.5, 9, 8.5, 8, 7.5, 7 in this order. That is, the most preferable range of d1 is 6 or more and 7 or less. The lower limit of c1+d1 is preferably 1.2, 2.0, 4.0, 6.0, 8.0, and 8.3, and the upper limit is preferably 20.0, 15.0, 12.5, 11.0, 10.0, and 9.0. That is, the range of c1+d1 is preferably 1.2 or more and 20.0 or less, 2.0 or more and 15.0 or less, 4.0 or more and 12.5 or less, 6.0 or more and 11.0 or less, and 8.0 or more and 10.0 or less, and the most preferable range is 8.3 or more and 9.0 or less. The lower limit of c1+d1 is preferably 1.2, 2.0, 4.0, 6.0, 8.0, and 8.3, and the upper limit is preferably 20.0, 15.0, 12.5, 11.0, 10.0, and 9.0. That is, the range of c1+d1 is preferably 1.2 or more and 20.0 or less, 2.0 or more and 15.0 or less, 4.0 or more and 12.5 or less, 6.0 or more and 11.0 or less, and 8.0 or more and 10.0 or less, and the most preferable range is 8.3 or more and 9.0 or less. The lower limit of e1 is preferably 0.1, 0.2, 0.5, 0.8, 1.0, and 1.5, and the upper limit is preferably 4.5, 4, 3.5, 3, 2.5, 2, and 2.5. In other words, the most preferable range for e1 is 1.5 or more and 2.5 or less. The upper limit of f1 is preferably 1.8, 1.5, 1.0, 0.8, and 0.5, and the lower limit is preferably 0. That is, the more preferable range for f1 is 0 or more and 0.5 or less, and 0 is most preferable. The lower limit of g1 is preferably 0.01, 0.015, and 0.02, and the upper limit is preferably 2, 1, 0.5, 0.4, 0.3, 0.2, 0.1, and 0.05. That is, the most preferable range for g1 is 0.02 or more and 0.05 or less. The upper limit of h1 is preferably 4, 3, 2, 1.8, 1.5, 1.0, 0.8, and 0.5, and the lower limit is preferably 0. That is, a more preferable range for h1 is 0 or more and 0.5 or less, and 0 is most preferable.
[0020] In the formula (1A), X is preferably tungsten, antimony, zinc, magnesium, calcium or cerium, and particularly preferably antimony or zinc. In the formula (1A), Y is preferably sodium, potassium or cesium, more preferably potassium or cesium. In the formula (1A), Z is preferably vanadium, copper, niobium, zirconium, calcium, beryllium, strontium, barium, lead, or phosphorus.
[0021] [Regarding the production method of the catalyst having the composition described in formula (1A)] Hereinafter, a method for preparing a catalyst having the composition described in formula (1A) will be described. In the method for producing the catalyst of the present invention, it is preferable to first prepare a mixture (mixture) of the above-mentioned ammonium molybdate and water, add a raw material for the bismuth component and a raw material for the iron component, and obtain an aqueous solution or aqueous slurry. The starting materials for each element are not particularly limited except for those related to ammonium molybdate, but for example, the following can be used:
[0022] As the bismuth component raw material, bismuth salts such as bismuth nitrate, bismuth subcarbonate, bismuth sulfate, bismuth acetate, bismuth trioxide, metal bismuth, etc. can be used, but bismuth nitrate is more preferable, and when it is used, a high-performance catalyst can be obtained. As the raw materials of iron, cobalt, nickel and other elements, oxides or nitrates, carbonates, organic acid salts, hydroxides, etc. that can be turned into oxides by ignition, or mixtures thereof can be used. For example, the iron component raw material and the cobalt component raw material and / or the nickel component raw material are dissolved and mixed in water at a desired ratio under a condition of 10 to 80°C, mixed with a separately prepared molybdenum component raw material and Z component raw material aqueous solution or slurry under a condition of 20 to 90°C, heated and stirred for about 1 hour under a condition of 20 to 90°C, and then an aqueous solution in which the bismuth component raw material is dissolved and, if necessary, an X component raw material and a Y component raw material are added to obtain an aqueous solution or slurry containing the catalyst components. Hereinafter, both are collectively referred to as the prepared liquid (A).
[0023] Here, the preparation liquid (A) does not necessarily contain all the catalytically active component elements, and some of the elements or some of the amounts may be added in a subsequent step. In addition, when preparing the preparation liquid (A), if the amount of water in which each component raw material is dissolved or an acid such as sulfuric acid, nitric acid, hydrochloric acid, tartaric acid, or acetic acid is added for dissolution, the acid concentration in the aqueous solution sufficient to dissolve the raw materials is not suitable for preparation, for example, in the range of 5% by mass to 99% by mass, and the form of the preparation liquid (A) may become a clay-like mass. In this case, an excellent catalyst cannot be obtained. The form of the preparation liquid (A) is preferably an aqueous solution or a slurry, because an excellent catalyst can be obtained.
[0024] The preparation liquid (A) can be obtained by uniformly mixing each active ingredient-containing compound and water. The amount of water used in the preparation liquid (A) is not particularly limited as long as it can completely dissolve all the compounds used or can be uniformly mixed. The amount of water used may be appropriately determined taking into consideration the drying method and drying conditions. Usually, the amount of water is 100 parts by mass or more and 2000 parts by mass or less with respect to 100 parts by mass of the total mass of the compounds for preparing the slurry. The amount of water is preferably large, but if there is too much water, there are many disadvantages such as high energy costs in the drying process and incomplete drying. Alternatively, the amount of water used in the slurry liquid is 3.0 to 4.5 times, preferably 3.4 to 4.2 times, in mass ratio, assuming that the amount of ammonium molybdate used is 1. In addition, the water temperature when ammonium molybdate is added is preferably 70°C or more, more preferably 75°C or more, and most preferably 80°C or more.
[0025] The above-mentioned preparation liquid (A) of the source compounds of each of the component elements is preferably prepared by (a) mixing the above-mentioned source compounds all at once, (b) mixing them all at once and then aging them, (c) mixing them stepwise, (d) repeating mixing and aging them stepwise, or a combination of (a) to (d). Here, the above-mentioned aging refers to "processing industrial raw materials or semi-finished products under specific conditions such as a certain time and a certain temperature to obtain or increase the required physical or chemical properties or to advance a predetermined reaction." In the present invention, the above-mentioned certain time refers to a range of 5 minutes to 24 hours, and the above-mentioned certain temperature refers to a range above room temperature and below the boiling point of the aqueous solution or aqueous dispersion. Among these, the method (c) of mixing stepwise is preferable in terms of the activity and yield of the finally obtained catalyst, and the more preferable method is a method in which each raw material to be mixed stepwise into the mother liquor is a solution in which it is completely dissolved, and the most preferable method is a method in which an alkali metal solution and various mixtures of nitrates are mixed into a mother liquor in which a molybdenum raw material is prepared as a preparation liquid or an aqueous slurry. However, it is not always necessary to mix all of the catalyst constituent elements in this step, and some of the elements or some amounts of the elements may be added in a subsequent step.
[0026] In the present invention, the shape of the stirring blades of the stirrer used when mixing the essential active ingredients is not particularly limited, and any stirring blade such as a propeller blade, turbine blade, paddle blade, inclined paddle blade, screw blade, anchor blade, ribbon blade, large lattice blade, etc. can be used in one stage or in two or more stages of the same or different blades in the vertical direction. In addition, a baffle (baffle plate) may be installed in the reaction tank as necessary.
[0027] In a preferred production method, the thus obtained preparation liquid (A) is converted into a catalyst through the following steps (a) to (c).
[0028] <(a) Step of drying the prepared liquid (A) to obtain a dried product> The method used in the drying step is not particularly limited as long as it can completely dry the preparation (A), and examples thereof include drum drying, freeze drying, spray drying, and evaporation to dryness. Among these, in the present invention, spray drying is particularly preferred, which can dry the preparation (A) into powder or granules in a short time. The drying temperature of the spray drying varies depending on the concentration of the preparation (A), the liquid sending speed, etc., but generally the temperature at the outlet of the dryer is 70°C or more and 150°C or less, and the inlet temperature is higher than the outlet temperature. In addition, it is preferable to dry the preparation (A) so that the average particle size of the dried product obtained at this time is 10 to 700 μm. In this specification, the dried product may also be expressed as a dry powder. The dried body can be directly used for the coating mixture, but it is preferable to calcinate it in advance since it may improve the moldability (pre-calcination step). The calcination method and conditions are not particularly limited, and known processing methods and conditions can be applied. The optimal conditions for calcination vary depending on the catalyst raw material, catalyst composition, preparation method, etc. used, but the calcination temperature is usually 100 to 350°C, preferably 150 to 300°C, and the calcination time is 1 to 20 hours. The calcination is usually performed in an air atmosphere, but it may be performed in an inert gas atmosphere such as nitrogen, carbon dioxide, helium, or argon, or after calcination in an inert gas atmosphere, it may be further calcined in an air atmosphere as necessary. The calcined solid thus obtained is preferably pulverized before molding. There is no particular limit to the pulverization method, but it is preferable to use a ball mill. Catalyst precursor granules can be obtained by the pre-calcination step and / or the subsequent pulverization step.
[0029] <(b) A step of molding the dried slurry obtained in the step (a) to obtain a molded product> The shape of the catalyst produced by the production method of the present invention is not particularly limited, and it is used after being molded into a columnar, tablet, ring, sphere, etc. in order to reduce the pressure loss of the reaction gas in the oxidation reaction. Among these, it is particularly preferable to support the catalytically active component solid on an inert carrier to form a supported catalyst, since it is expected to improve selectivity and remove reaction heat. This support is preferably performed by the rolling granulation method described below. This method is a method in which, for example, in an apparatus having a flat or uneven disk at the bottom of a fixed container, the disk is rotated at high speed to vigorously stir the carrier in the container by repeating rotation and revolution, and a support mixture containing a binder, a catalytically active component solid, and, if necessary, other additives such as a molding aid and a strength improver is added to these, is supported on the carrier. The method of adding the binder can be arbitrarily selected from the following methods: 1) mixing the binder in advance with the mixture for supporting; 2) adding the binder simultaneously with the mixture for supporting being added to the fixed container; 3) adding the binder after the mixture for supporting being added to the fixed container; 4) adding the binder before the mixture for supporting being added to the fixed container; 5) dividing the mixture for supporting and the binder, and adding the total amount by appropriately combining 2) to 4). In the case of 5), it is preferable to adjust the addition speed using an autofeeder or the like so that a predetermined amount of the mixture for supporting is supported on the carrier without adhesion to the wall of the fixed container or aggregation of the mixture for supporting. Examples of the binder include water, ethanol, polyhydric alcohol, polymeric binder polyvinyl alcohol, celluloses such as crystalline cellulose, methyl cellulose, and ethyl cellulose, and inorganic binder silica sol aqueous solutions. However, celluloses, diols such as ethylene glycol, and triols such as glycerin are preferred, and an aqueous solution of glycerin with a concentration of 5% by mass or more is particularly preferred. The amount of these binders used is usually 2 to 60 parts by mass, and preferably 10 to 50 parts by mass, based on 100 parts by mass of the mixture for supporting.
[0030] Specific examples of the carrier in the above-mentioned support include spherical carriers having a diameter of 1 to 15 mm, preferably 2.5 to 10 mm, such as silicon carbide, alumina, silica alumina, mullite, and alundum. These carriers are usually used with a porosity of 10 to 70%. The ratio of the carrier and the mixture for support is usually such that the mixture for support / (mixture for support+carrier)=10 to 75% by mass, preferably 15 to 60% by mass. When the ratio of the mixture for support is large, the reaction activity of the supported catalyst tends to be high, but the mechanical strength tends to be low. Conversely, when the ratio of the mixture for support is small, the mechanical strength tends to be high, but the reaction activity tends to be low. In the above, examples of the molding aid used if necessary include silica gel, diatomaceous earth, and alumina powder. The amount of the molding aid used is usually 1 to 60 parts by mass with respect to 100 parts by mass of the solid catalytic active component. Furthermore, if necessary, inorganic fibers (e.g., ceramic fibers or whiskers, etc.) inactive to the catalytically active component solid and the reaction gas can be used as a strength improver, which is useful for improving the mechanical strength of the catalyst, and glass fibers are preferred. The amount of these fibers used is usually 1 to 30 parts by mass per 100 parts by mass of the catalytically active component solid. In the first stage of catalyst molding, the molding aid, pore former, and carrier added are not considered as constituent elements of the active component in the present invention, regardless of whether they have activity in the sense of converting the raw materials into some other product. The molded product of the present invention is obtained by the molding step.
[0031] <(c) Step of Firing the Molded Product Obtained in Step (b)> The molded product obtained as described above can be directly used as a catalyst in a gas-phase catalytic oxidation reaction, but calcination is preferable because it may improve the catalytic activity. The calcination method and conditions are not particularly limited, and known treatment methods and conditions can be applied. The optimal conditions for calcination vary depending on the catalyst raw material, catalyst composition, preparation method, etc. used, but the calcination temperature is usually 200 to 600°C, preferably 400 to 600°C, more preferably 500°C to 600°C, and the calcination time is 1 to 20 hours. The calcination is usually performed in an air atmosphere, but may be performed in an inert gas atmosphere such as nitrogen, carbon dioxide, helium, or argon, or may be further calcined in an air atmosphere after calcination in an inert gas atmosphere as necessary.
[0032] <Use of catalyst> The catalyst obtained by the production method of the present invention is used in a reaction for producing the corresponding unsaturated aldehyde or unsaturated carboxylic acid from propylene, isobutylene, t-butyl alcohol, etc. as a raw material. In particular, when the catalyst is used in a reaction for producing acrolein or acrylic acid by gas-phase catalytic oxidation of propylene with molecular oxygen or a molecular oxygen-containing gas, the catalyst can improve the catalytic activity and the yield, and is very effective in improving the price competitiveness of the product compared to known methods. In addition, the catalyst of the present invention is expected to have an improved effect on the process stability of the partial oxidation reaction accompanied by heat generation, such as reducing the hot spot temperature. Furthermore, the catalyst of the present invention is also effective in reducing by-products that have a negative impact on the environment and the quality of the final product, such as carbon monoxide (CO), carbon dioxide (CO2), acetaldehyde, acetic acid, and formaldehyde.
[0033] For example, when propylene is subjected to gas-phase catalytic oxidation with a molecular oxygen-containing gas to produce acrolein and / or acrylic acid, the method of flowing the raw material gas may be a normal single flow method or a recycle method, and may be carried out under generally used conditions and is not particularly limited. For example, a mixed gas consisting of 1 to 10 volume % and preferably 4 to 9 volume % of propylene as a starting raw material substance, 3 to 20 volume % and preferably 4 to 18 volume % of molecular oxygen, 0 to 60 volume % and preferably 4 to 50 volume % of steam, and 20 to 80 volume % and preferably 30 to 60 volume % of an inert gas such as carbon dioxide or nitrogen is filled in a reaction tube and then heated at 250 to 450° C. under a pressure of normal pressure to 10 atm at a space velocity of 300 to 5000 h -1 and the reaction is carried out.
[0034] [Catalyst composition of formula (1B)] As another catalyst composition of the catalyst of the present invention, the catalyst for producing an unsaturated carboxylic acid preferably has a composition represented by the following formula (1B). [Formula (1B)] Mo 12 V a W b Cu c Sb d X e Y f Z g O h (1B) (In the formula, Mo, V, W, Cu, Sb, and O represent molybdenum, vanadium, tungsten, copper, antimony, and oxygen, respectively; X represents at least one element selected from the group consisting of an alkali metal and thallium; Y represents at least one element selected from the group consisting of magnesium, calcium, strontium, barium, and zinc; Z represents at least one element selected from the group consisting of bismuth, tellurium, silver, selenium, silicon, aluminum, boron, niobium, cerium, tin, chromium, manganese, iron, cobalt, nickel, samarium, germanium, zirconium, titanium, chromium, tantalum, lead, indium, sulfur, palladium, gallium, lanthanum, and arsenic. Also, a, b, c, d, e, f, g, and h represent the atomic ratios of the respective elements. With respect to 12 molybdenum atoms, 0 < a ≤ 10.0, 0 ≤ b ≤ 10.0, 0 < c ≤ 6.0, 0 ≤ d ≤ 10.0, 0 ≤ e ≤ 0.50, 0 ≤ f ≤ 1.0, and 0 ≤ g < 6.0. Also, h is the number of oxygen atoms necessary to satisfy the valences of the respective components.)
[0035] In the above formula (1B), the preferable ranges of a to g are as follows. The lower limits of a are, in order of preference, 0.20, 0.50, 0.80, 1.0, 1.5, 2.0, 2.2, 2.5, and most preferably 2.8; the upper limits of a are, in order of preference, 9.0, 8.0, 7.0, 6.0, 5.0, 4.5, 4.0, 3.5, and most preferably 3.2. That is, the most preferable range of a is 2.8 ≤ a ≤ 3.2. The lower limits of b are, in order of preference, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70, 0.80, 0.90, and most preferably 1.0; the upper limits of b are, in order of preference, 9.0, 8.0, 7.0, 6.0, 5.0, 4.0, 3.0, 2.5, 2.0, 1.5, and most preferably 1.4. That is, the most preferable range of a is 1.0 ≤ b ≤ 1.4. The lower limit of c is, in order of desirability, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70, 0.80, 0.90, and most desirably 1.0, and the upper limit of c is, in order of desirability, 5.0, 4.0, 3.0, 2.5, 2.0, 1.5, and most desirably 1.4. That is, the most preferable range of a is 1.0≦c≦1.4. The lower limit of d is, in order of desirability, 0.11, 0.15, 0.18, 0.20, 0.25, 0.30, and 0.35, and is most desirably 0.40, and the upper limit of d is, in order of desirability, 9.0, 8.0, 7.0, 6.0, 5.0, 4.0, 3.0, 2.5, 2.0, 1.5, and 1.0, and is most desirably 0.70. That is, the most preferable range of a is 0.40≦d≦0.70. The upper limit of e is, in order of desirability, 0.40, 0.30, 0.20, and 0.10. That is, the most preferable range of e is 0≦e≦0.10. The upper limit of f is, in order of desirability, 0.80, 0.50, 0.20, 0.15, and most desirably 0.10. That is, the most preferable range of f is 0≦g1≦0.10. The upper limit of g is, in order of desirability, 5.0, 4.0, 3.0, 2.0, 1.0, 0.050, 0.025, and 0.015. That is, the most preferable range of g is 0≦g≦0.015. In a particularly preferred embodiment, e, f and g are 0.
[0036] [Method for producing a catalyst having the composition represented by formula (1B)] Hereinafter, a method for producing a catalyst having the composition described in formula (1B) will be described. Step a) Mixing Generally, when ammonium molybdate is used as the raw material for each element constituting the catalyst, a high performance catalyst can be obtained. As the raw materials of tungsten, vanadium, antimony, copper and other elements, oxides or ammonium salts, carbonates, organic acid salts, hydroxides, etc. that can be converted to oxides by ignition, or mixtures thereof can be used. For example, vanadium component raw material, molybdenum component raw material, and antimony component raw material are mixed in a desired ratio with a separately prepared aqueous solution or slurry of tungsten component raw material and Z component raw material under conditions of 20 to 95 ° C., and heated and stirred for about 1 hour under conditions of 20 to 90 ° C., and then an aqueous solution in which a copper component raw material is dissolved and, if necessary, an X component raw material and a Y component raw material are added to obtain an aqueous solution or slurry containing a catalyst component. Hereinafter, both are collectively referred to as the prepared liquid (A). Herein, the prepared liquid (A) does not necessarily need to contain all the catalyst constituent elements, and some elements or a part of the amount of the elements may be added in a subsequent step. In addition, when preparing the preparation liquid (A), if the amount of water in which each component raw material is dissolved or an acid such as sulfuric acid, nitric acid, hydrochloric acid, tartaric acid, or acetic acid is added for dissolution, the acid concentration in the aqueous solution sufficient to dissolve the raw materials is not suitable, for example, within the range of 5% by mass to 99% by mass, the preparation liquid (A) may become a clay-like lump, which does not become an excellent catalyst. Therefore, the preparation liquid (A) obtained is preferably in the form of an aqueous solution or a slurry, in terms of obtaining an excellent catalyst. In addition, the amount of water used in the slurry liquid is 4.4 to 6.0 times, preferably 4.7 to 5.7 times, in mass ratio, assuming that the amount of ammonium molybdate used is 1. In addition, the water temperature when ammonium molybdate is added is preferably 85°C or higher, more preferably 90°C or higher, and most preferably 95°C or higher.
[0037] Step b) Drying Next, the prepared liquid (A) obtained above is dried to obtain a dry powder. The drying method is not particularly limited as long as it can completely dry the prepared liquid (A), and examples thereof include drum drying, freeze drying, spray drying, and evaporation to dryness. Among these, in the present invention, spray drying is particularly preferred, which can dry the slurry into powder or granules in a short time. The drying temperature of the spray drying varies depending on the concentration of the slurry, the liquid sending speed, etc., but is generally 70 to 150°C at the outlet of the dryer. In addition, it is preferable to dry the mixture so that the average particle size of the dry powder obtained at this time is 20 to 700 μm. In this way, a dry powder (B) is obtained.
[0038] Step c) Pre-firing The resulting dry powder (B) is calcined under air flow at 200°C to 500°C, preferably 300°C to 400°C, which tends to improve the moldability, mechanical strength, and catalytic performance of the catalyst. The calcination time is preferably 1 hour to 12 hours. In this way, a pre-calcined body (C) is obtained.
[0039] Step d) Crushing The obtained pre-calcined body (C) is obtained as a solid (D) in which the dry powder (B) is aggregated by pre-calcination. In order to obtain the pre-calcined powder (E) required in the next molding step, the solid (D) is pulverized. The pulverization method is not particularly limited, and examples thereof include a roller mill, a jet mill, a hammer mill, a rotary mill, and a vibration mill. The average particle size (pre-calcined median size) of the pre-calcined powder (E) obtained at this time is preferably 10 μm or more and 100 μm or less, more preferably 20 μm or more and 80 μm or less, even more preferably 30 μm or more and 50 μm or less, and particularly preferably 35 μm or more and 45 μm or less. In the present specification, the crushed pre-calcined powder (E) is described as a catalyst precursor. However, in the case where there is no agglomeration at the pre-calcined body (C) stage and it can be used without going through a crushing step, the pre-calcined body (C) may be used as a catalyst precursor.
[0040] Process e) Molding There is no particular limitation on the molding method, but when molding into a cylindrical or ring shape, a method using a tablet molding machine, an extrusion molding machine, etc. is preferred. More preferably, when molding into a spherical shape, the pre-sintered powder (E) may be molded into a spherical shape using a molding machine, but a method in which the pre-sintered powder (E) (containing a molding aid and a strength improver, if necessary) is supported on a carrier such as an inactive ceramic is preferred. Here, the widely known methods of loading include the rolling granulation method, the method using a centrifugal fluidized coating device, the wash coat method, etc., and are not particularly limited as long as the pre-calcined powder (E) can be uniformly loaded on the carrier, but when considering the production efficiency of the catalyst and the performance of the catalyst to be prepared, it is more preferable to use a device having a flat or uneven disk at the bottom of a fixed cylindrical container, which is rotated at high speed to vigorously stir the carrier charged in the container by the rotation and revolution of the carrier itself, and to add the pre-calcined powder (E) and, if necessary, a molding aid and / or a strength improver and a pore former to load the powder components on the carrier. It is preferable to use a binder when loading. Specific examples of binders that can be used include water, ethanol, methanol, propanol, polyhydric alcohols, polyvinyl alcohol as a polymer binder, and silica sol aqueous solution as an inorganic binder. Ethanol, methanol, propanol, and polyhydric alcohols are preferred, and diols such as ethylene glycol and triols such as glycerin are more preferred. By using an appropriate amount of glycerin aqueous solution, moldability is improved and a high-performance catalyst with high mechanical strength can be obtained. Specifically, a particularly high-performance catalyst can be obtained when an aqueous solution of glycerin with a concentration of 5% by mass or more is used. The amount of these binders used is usually 2 to 80 parts by mass per 100 parts by mass of the pre-calcined powder (E). An inert carrier of about 2 to 8 mm is usually used, and the pre-calcined powder (E) is supported on it. The support rate is determined in consideration of the catalyst use conditions, such as the space velocity of the reaction raw materials and the raw material concentration, and is usually 20% by mass to 80% by mass. Here, the support rate is expressed as the following formula (4) when a molding aid or strength improver is used in molding. In this way, a molded body (F) is obtained. In the production method of the present invention, it is preferable to add inactive inorganic fibers as a strength improver during the support molding, and it is particularly preferable to use glass fibers. The amount of these fibers used is usually 1 to 30 parts by mass per 100 parts by mass of the catalytically active component solids. As the material for the inert carrier, known materials such as alumina, silica, titania, zirconia, niobia, silica alumina, silicon carbide, carbides, and mixtures thereof can be used. Furthermore, there are no particular limitations on the particle size, water absorption rate, mechanical strength, crystallinity of each crystal phase, or mixing ratio, and appropriate ranges should be selected taking into consideration the final catalyst performance, moldability, production efficiency, etc.
[0041] [Formula (6)] Loading rate (mass%) = 100 × [mass of pre-calcined powder (E) used for molding / (mass of pre-calcined powder (E) used for molding + mass of inert carrier used for molding)] In addition, when it is clear that additives such as molding aids and strength improvers remain in the catalyst after main calcination, they are included in the total amount (denominator).
[0042] Step f) Main firing The molded body (F) tends to have improved catalytic activity and effective yield by calcining it at a temperature of 100 to 450°C for about 1 to 12 hours. The calcination temperature is preferably 270°C to 420°C, more preferably 350°C to 400°C. Air is the preferred gas to be circulated because it is simple, but other inert gases such as nitrogen, carbon dioxide, nitrogen oxide-containing gas for creating a reducing atmosphere, ammonia-containing gas, hydrogen gas, and mixtures thereof can also be used. In this way, the catalyst (G) is obtained.
[0043] In the method for producing an unsaturated carboxylic acid, the method for flowing the raw material gas may be a normal single flow method or a recycle method, and may be carried out under generally used conditions and is not particularly limited. For example, a mixed gas consisting of 1 to 10 volume %, preferably 4 to 9 volume %, of unsaturated aldehyde as a starting raw material substance, 3 to 20 volume %, preferably 4 to 18 volume %, of molecular oxygen, 0 to 60 volume %, preferably 4 to 50 volume %, of water vapor, and 20 to 80 volume %, preferably 30 to 60 volume % of an inert gas such as carbon dioxide or nitrogen is filled in a reaction tube and then, at 240 to 450° C., under a pressure of normal pressure to 10 atm, at a space velocity of 300 to 5000 h , is passed over the catalyst of the present invention filled in a reaction tube. -1 and the reaction is carried out. EXAMPLES
[0044] Although specific examples are given below, the present invention is not limited to these examples as long as they do not deviate from the spirit of the present invention.
[0045] The present invention will be described in more detail below with reference to examples. In the examples, the conversion rate, effective yield, effective selectivity and loading rate were calculated according to the following formulas. Propylene conversion rate (%) = (number of moles of reacted propylene) / (number of moles of supplied propylene) x 100 Effective yield (%) = (total number of moles of acrolein and acrylic acid produced) / (number of moles of propylene fed) x 100 Effective selectivity (%) = (total number of moles of acrolein and acrylic acid produced) / (number of moles of propylene reacted) x 100 Loading rate (mass%)=(mass of pre-calcined powder used for molding) / {(mass of pre-calcined powder used for molding)+(mass of support used for molding)}×100
[0046] [Example 1] (Preparation of Catalyst 1) Catalyst 1 was prepared by the following method so that the composition ratio of the catalytically active components excluding oxygen was Mo:Bi:Fe:Co:Ni:Cs = 12:1.0:2.0:6.5:3.0:0.03 in atomic ratio. Distilled water was heated and stirred while ammonium molybdate (storage temperature 25 °C for 90 days in an environment, placed in a 0.2 mm thick plastic bag, sealed in a steel drum with a light shielding rate of 99.99%. Exp in condition 1 (保管温度[℃]-50) × number of days stored = 1.3 × 10 -9 (Prepared solution 1) was obtained by dissolving ammonium molybdate and potassium nitrate. Here, the amount of distilled water used was 3.5 times the mass of ammonium molybdate, and the water temperature when ammonium molybdate was added was 85°C. Separately, cobalt nitrate, nickel nitrate, and ferric nitrate were dissolved in distilled water to prepare an aqueous solution (Prepared solution 2), and bismuth nitrate was dissolved in distilled water that had been acidified with concentrated nitric acid to prepare an aqueous solution (Prepared solution 3). The aqueous solution (Prepared solution 1) was mixed with (Prepared solution 2) and (Prepared solution 3) in sequence while being vigorously stirred, the resulting suspension was dried using a spray dryer, and the resulting granules were fired at 440°C for 6 hours to obtain a pre-fired powder. After that, the powder obtained by mixing crystalline cellulose with the pre-fired powder was adjusted to the mass of the carrier and the mass of the pre-fired powder used for molding so that the loading rate defined by the above formula was 50 mass% on an inert carrier (a spherical material with a diameter of 4.5 mm mainly composed of alumina and silica). A 33% by mass aqueous solution of glycerin was used as a binder, and the catalyst was molded into a sphere having a diameter of 5.2 mm to obtain a supported catalyst. The supported catalyst was calcined at a calcination temperature of 530° C. for 4 hours in an air atmosphere to obtain catalyst 1.
[0047] [Example 2] (Preparation of Catalyst 2) In Example 1, the storage conditions for ammonium molybdate were a storage temperature of 35°C for 180 days, in which the bag was placed in a 0.2 mm thick vinyl bag and sealed in a steel drum with a light blocking rate of 99.99% (exp (保管温度[℃]-50) × number of days stored = 5.5 × 10 -5 A catalyst was prepared in exactly the same manner except for the above steps, and catalyst 2 was obtained.
[0048] [Comparative Example 1] (Preparation of Catalyst 3) In Example 1, the storage conditions for ammonium molybdate were a storage temperature of 60°C for 6 hours, placed in a 0.2 mm thick vinyl bag, and sealed in a steel drum with a light blocking rate of 99.99% (exp (保管温度[℃]-50) × number of days of storage = 5507 days) and other factors were similarly observed to prepare a catalyst, thereby obtaining catalyst 3.
[0049] [Comparative Example 2] In Example 1, the storage conditions for ammonium molybdate were a storage temperature of 60°C for 9 hours, placed in a 0.2 mm thick vinyl bag, and sealed in a steel drum with a light blocking rate of 99.99% (exp (保管温度[℃]-50) The catalyst was produced in exactly the same way except for the following: × number of days of storage = 8,260 days). However, when the mixed liquid was sent to the spray dryer for drying, clogging occurred in the piping due to residue that was thought to be insoluble ammonium molybdate, and it was no longer possible to produce catalyst after that.
[0050] [Reference Comparative Example 1] (Preparation of Catalyst 4) In Example 1, the storage conditions of ammonium molybdate were a storage temperature of 35°C and an average daily global solar radiation of 27 MJ / m 2 For 14 days under the condition 2 (the cumulative total solar radiation was 380 MJ / m 2 ), moisture permeability is 4.8g / (m 2 A catalyst was prepared in the same manner, except that the catalyst was placed in a transparent plastic bag for 10 min. / 24 h, to obtain catalyst 4.
[0051] [Reference Comparative Example 2] (Preparation of Catalyst 5) In Example 1, the storage conditions of ammonium molybdate were a storage temperature of 35° C. and an absolute humidity of 20 g / m 3 Storage absolute humidity [g / m 3 ])×Number of storage days [days]=12.5 days g / m 3 ) A catalyst was prepared in the same manner as above to obtain catalyst 5.
[0052] [Reference Comparative Example 3] In Example 1, the storage conditions of ammonium molybdate were a storage temperature of 35°C and an average daily global solar radiation of 29 MJ / m 2 for 30 days in a shaded environment (the cumulative total solar radiation in condition 2 was 857 MJ / m 2 ), moisture permeability is 4.8g / (m 2 A catalyst was produced in exactly the same way, except that the mixture was placed in a transparent plastic bag for 24 hours. However, when the mixture was sent to the spray dryer for drying, clogging occurred in the piping due to residue that was thought to be insoluble ammonium molybdate, and it was no longer possible to produce catalyst thereafter.
[0053] [Reference Comparative Example 4] In Example 1, the storage conditions of ammonium molybdate were a storage temperature of 35° C. and an absolute humidity of 19 g / m 3 (storage absolute humidity [g / m 3 ]×Number of storage days [days]=36.4 days·g / m 3 ) The catalyst was produced in exactly the same way, except for the above. However, clogging occurred around the atomizer in the spray dryer due to residue that was thought to be insoluble in the blended liquid, and it was no longer possible to produce any catalyst thereafter.
[0054] Using catalysts 1 to 5, the oxidation reaction of propylene was carried out by the following method, and the raw material conversion and effective yield were determined. 47.8 mL of catalyst was packed into a stainless steel reaction tube with an inner diameter of 22 mm, and a mixed gas with a gas volume ratio of propylene:oxygen:steam:nitrogen = 1.00:1.65:1.27:9.53 was pumped at a propylene space velocity of 110 h hr for the total catalyst in the reaction tube. -1 After aging reaction for 20 hours or more from the start of the reaction at a reaction bath temperature of 315°C, the raw material conversion and effective yield shown in Table 1 were obtained by analyzing the gas at the outlet of the reaction tube at a reaction bath temperature of 320°C.
[0055] [Table 1]
[0056] From Table 1, it can be seen that Catalyst 1 and Catalyst 2, in which the storage conditions of ammonium molybdate are within the range of the present invention, show a significantly higher effective yield. It is not known to those skilled in the art that such storage conditions of ammonium molybdate are related to the performance of the catalyst as a final product and a stable catalyst production method, but it can be said that this has been clarified by the present inventors.
[0057] [Example 3] (Preparation of Catalyst 6) Catalyst 9 was prepared by the method described below so that the composition ratio of the catalytically active components excluding oxygen was Mo:Bi:Fe:Co:Ni:Cs = 12:1.7:1.8:7.2:0.8:0.2 in atomic ratio. Ammonium heptamolybdate (stored in a 0.2 mm thick plastic bag in a drum with a light shielding rate of 99.99% for 75 days at a storage temperature of 25°C. Exp. (保管温度[℃]-50) × number of days stored = 1.0 × 10 -9 The ammonium molybdate was added to the mother liquor 1. The distilled water used was 3.6 times the mass of ammonium molybdate, and the water temperature at the time of adding the ammonium molybdate was 82°C. Next, cesium nitrate was dissolved in pure water and added to the mother liquor 1. Next, ferric nitrate, cobalt nitrate, and nickel nitrate were dissolved in pure water heated to 60°C and added to the mother liquor 1. Next, nitric acid was dissolved in an aqueous nitric acid solution prepared by adding nitric acid (60 mass%) to pure water heated to 60°C, and added to the mother liquor 1. This mother liquor 1 was dried by a spray drying method, and the obtained dried powder was pre-calcined at 440°C for 5 hours. Crystalline cellulose was added to the pre-calcined powder (having the above-mentioned composition ratio) thus obtained, and after thorough mixing, the pre-calcined powder was subjected to a rolling granulation method using a 33% by mass glycerin solution as a binder, and the pre-calcined powder was shaped into spheres so that the loading rate on the inactive carrier was 40% by mass. The spheres thus obtained, each having a particle size of 4.4 mm, were calcined at 520°C for 5 hours to obtain catalyst 6 of the present invention.
[0058] Catalyst 6 was evaluated for reaction by the following method. 34 ml of catalyst was packed into a stainless steel reaction tube, and a mixed gas with a gas volume ratio of isobutylene:oxygen:nitrogen:steam=1:2.2:12.5:1.0 was used under an outlet pressure of 50 kPaG and a GHSV of 1500 hr. -1 After aging reaction for 20 hours or more at a reaction bath temperature of 350℃ under the above conditions, the condensate and gas components were separated at the outlet of the reaction tube using a condenser, and each component in the gas and condensate was quantitatively analyzed using a gas chromatograph equipped with a flame ionization detector and a thermal conductivity detector. Each data obtained by the gas chromatograph was factor-corrected to calculate the raw material conversion rate and effective yield. The reaction results of catalyst 6 after aging at 350°C were an isobutylene conversion of 99.1% and an effective yield of 82.3% at a reaction bath temperature of 345°C.
[0059] [Example 4] (Preparation of Catalyst 7) Catalyst 7 was prepared by the method described below so that the composition ratio of the catalytically active components excluding oxygen was Mo12V3.0W1.3Cu1.2Sb0.5 in atomic ratio. Ammonium paratungstate was completely dissolved in distilled water heated to 95°C. Here, 4.8 times the mass of ammonium molybdate was used as the distilled water, and the water temperature when ammonium molybdate was added was 98°C. While stirring this solution, ammonium metavanadate and ammonium molybdate (stored in a 0.2 mm thick plastic bag and sealed in a drum with a light shielding rate of 99.99% for 90 days in an environment with a storage temperature of 25°C. The exp (保管温度[℃]-50) × number of days stored = 1.3 × 10 -9(days), antimony acetate was gradually added and thoroughly stirred. Next, a solution in which copper sulfate was added to pure water heated to 80°C and completely dissolved was added to the above solution and mixed by stirring. This mixed solution (A) was dried by spray drying, and the obtained dried powder (B) was pre-calcined at 350°C for 4 hours to obtain pre-calcined powder (C). The obtained pre-calcined powder (C) was pulverized with a vibration mill to obtain pre-calcined powder (E). Crystalline cellulose and a strength aid were added to the pre-calcined powder (E) and thoroughly mixed, and then the mixture was granulated by rolling granulation using a 20% by mass glycerin solution as a binder to form a spherical support on an inactive spherical support made of a mixture of silica and alumina so that the support rate was 33% by mass. Next, the main calcination was performed at 375°C for 4 hours to obtain a spherical catalyst 7 of the present invention.
[0060] An oxidation reaction was carried out using the obtained catalyst 7. 67.6 ml of catalyst 7 was packed into a reaction tube with an inner diameter of 28.4 mm, and a gas having the composition shown below, which was obtained by adding oxygen and nitrogen to the gas obtained by gas-phase catalytic oxidation of propylene using a molybdenum-bismuth catalyst, was introduced into the tube, and the reaction was carried out at an SV (space velocity; flow rate of raw gas per unit time / apparent volume of packed catalyst) of 1020 / hr and a reaction bath temperature of 260°C. Acrolein 5.9vol% Unreacted propylene + other organic compounds 1.7 vol% Oxygen 4.7vol% 17.2vol% Nitrogen-containing inert gas 70.5vol% The reaction results for catalyst 7 were an acrolein conversion of 99.4% and an acrylic acid selectivity of 96.7%.
[0061] As described in Examples 3 and 4, it was found that superior catalytic performance can be achieved by using molybdenum stored under the conditions of the present invention in the production of methacrolein from isobutylene and in the production of acrylic acid from acrolein. From the above, it has been found that in the production catalyst for catalysts for producing unsaturated aldehydes and / or unsaturated carboxylic acids, catalysts using molybdenum that satisfy the storage conditions of the present application can exhibit superior and stable performance under realistic storage conditions as an industrial catalyst.
[0062] [Example 5] (Preparation of Catalyst 8) In Example 1, the storage conditions for ammonium molybdate were a storage temperature of 60°C for 5 hours, placed in a 0.2 mm thick vinyl bag, and sealed in a steel drum with a light blocking rate of 99.99% (exp (保管温度[℃]-50) × number of days of storage = 4589 days) to prepare a catalyst in exactly the same manner, and catalyst 8 was obtained.
[0063] [Example 6] (Preparation of Catalyst 9) In Example 1, the storage conditions of ammonium molybdate were a storage temperature of 35°C and an average daily global solar radiation of 6.3 MJ / m 2 For 25 days under the environment (the cumulative total solar radiation in condition 2 was 158 MJ / m 2 ), moisture permeability is 4.8g / (m 2 A catalyst was prepared in the same manner, except that the catalyst was placed in a transparent plastic bag for 10 min. / 24 h, to obtain catalyst 9.
[0064] [Example 7] (Preparation of Catalyst 10) In Example 1, the storage conditions of ammonium molybdate were a storage temperature of 22°C and an absolute humidity of 13 g / m 3 Storage absolute humidity [g / m 3 ])×Number of storage days [days]=4.4 days g / m 3 ) A catalyst was prepared in exactly the same manner as above to obtain catalyst 10.
[0065] [Example 8] (Preparation of Catalyst 11) In Example 1, the storage conditions for ammonium molybdate were as follows: storage temperature: 4°C; storage for 28 days in a 0.2 mm thick plastic bag; storage in a refrigerator with a light shielding rate of 99.99% (exp (保管温度[℃]-50) × number of days stored = 2.9 × 10 -19 A catalyst was prepared in the same manner except for the above steps (a) and (b), to obtain catalyst 11.
[0066] [Example 9] (Preparation of Catalyst 12) In Example 1, the storage conditions of ammonium molybdate were a storage temperature of 22° C. and an absolute humidity of 5.4 g / m 3 Storage absolute humidity [g / m 3 ])×Number of storage days [days]=0.5 days g / m 3 ) A catalyst was prepared in the same manner as above to obtain catalyst 12.
[0067] [Example 10] (Preparation of Catalyst 13) In Example 1, the storage conditions of ammonium molybdate were a storage temperature of 22°C and an absolute humidity of 13 g / m 3 The specimen was placed in a dark-shielded environment for 20.5 hours without being placed in a plastic bag (condition 3 (storage absolute humidity [g / m 3 ])×Number of storage days [days]=11.2 days g / m 3 ) A catalyst was prepared in exactly the same manner as above to obtain catalyst 13.
[0068] Using catalysts 8 to 13, a propylene oxidation reaction was carried out in exactly the same manner as for catalysts 1 to 5, and the raw material conversion rate and effective yield were determined. The results of determining the raw material conversion rate, effective yield, and effective selectivity for Examples 5 to 10, along with the storage conditions for Examples 1 and 2, Comparative Examples 1 and 2, and Reference Comparative Examples 1 to 4, are shown in Table 2.
[0069] [Table 2]
[0070] From Table 2, it can be seen that in addition to the knowledge of Condition 1 in Table 1, Catalyst 9, Catalyst 10, Catalyst 12, and Catalyst 13 produced under Conditions 2 and 3 also exhibit superiorly high effective selectivity. It is not known to those skilled in the art that such storage conditions of ammonium molybdate are related to the performance of the catalyst as a final product and a stable catalyst production method, but it can be said that this has been clarified by the present inventors. [Industrial Applicability]
[0071] The storage conditions of the ammonium molybdate of the present invention enable stable production of catalysts for producing unsaturated aldehydes and unsaturated carboxylic acids, which contain molybdenum as an essential active component, and also enable the achievement of high-yield catalytic performance.
Claims
1. The composition of the catalytically active component is represented by the following general formula (1A) or (1B): Mo a1 Bi b1 Ni c1 Co d1 Fe e1 X f1 Y g1 Z h1 O i1 ・・・(1A) (In the formula, Mo, Bi, Ni, Co and Fe represent molybdenum, bismuth, nickel, cobalt and iron, respectively; X represents at least one element selected from tungsten, antimony, tin, zinc, chromium, manganese, magnesium, silicon, aluminum, cerium and titanium; Y represents at least one element selected from sodium, potassium, cesium, rubidium and thallium; Z represents an element belonging to Groups 1 to 16 of the periodic table; and , and at least one element selected from elements other than Y, and a1, b1, c1, d1, e1, f1, g1, h1, and i1 respectively represent the numbers of atoms of molybdenum, bismuth, nickel, cobalt, iron, X, Y, Z, and oxygen, and when a1=12, 0<b1≦7, 0≦c1≦10, 0<d1≦10, 0<c1+d1≦20, 0<e1≦5, 0≦f1≦2, 0≦g1≦3, 0≦h1≦5, and i1=a value determined by the oxidation state of each element). Mo 12 V a W b Cu c Sb d X e Y f Z g O h ・・・(1B) (In the formula, Mo, V, W, Cu, Sb, and O represent molybdenum, vanadium, tungsten, copper, antimony, and oxygen, respectively; X represents at least one element selected from the group consisting of alkali metals and thallium; Y represents at least one element selected from the group consisting of magnesium, calcium, strontium, barium, and zinc; Z represents bismuth, tellurium, silver, selenium, silicon, aluminum, boron, niobium, cerium, tin, chromium, manganese, iron, cobalt, nickel, samarium, germanium, zinc, and tin.) Each of the elements represents at least one element selected from the group consisting of zinc, titanium, chromium, tantalum, lead, indium, sulfur, palladium, gallium, lanthanum, and arsenic. In addition, a, b, c, d, e, f, g, and h represent the atomic ratio of each element, and with respect to 12 molybdenum atoms, a represents 0<a≦10.0, b represents 0≦b≦10.0, c represents 0<c≦6.0, d represents 0≦d≦10.0, e represents 0≦e≦0.50, f represents 0≦f≦1.0, and g represents 0≦g<6.
0. In addition, h represents the number of oxygen atoms required to satisfy the valence of each of the components. A method for producing a catalyst for producing an unsaturated aldehyde and / or an unsaturated carboxylic acid, wherein the storage conditions for ammonium heptamolybdate used as a molybdenum raw material include the following condition 1: Condition 1: The product is stored in a light-shielding, moisture-impermeable container, and the following formula (2) is satisfied throughout the entire storage period. exp (保管温度[℃]-50) × Number of storage days [days] ≦ 5200 ... (2) However, a light-shielding container is a container with a visible light and / or ultraviolet light shielding rate (measured according to a method conforming to JIS L 1055) of 95% or more, and a moisture-impermeable container is a container with a moisture permeability (moisture permeability) of 5 g / (m 2 - The container is one that is below the storage temperature of 24 hours. The storage temperature is the average temperature of the stored molasses itself during the storage period.
2. The composition of the catalytically active component is represented by the following general formula (1A) or (1B): Mo a1 Bi b1 Ni c1 Co d1 Fe e1 X f1 Y g1 Z h1 O i1 ・・・(1A) (In the formula, Mo, Bi, Ni, Co and Fe represent molybdenum, bismuth, nickel, cobalt and iron, respectively; X represents at least one element selected from tungsten, antimony, tin, zinc, chromium, manganese, magnesium, silicon, aluminum, cerium and titanium; Y represents at least one element selected from sodium, potassium, cesium, rubidium and thallium; Z represents an element belonging to Groups 1 to 16 of the periodic table; and , and at least one element selected from elements other than Y, and a1, b1, c1, d1, e1, f1, g1, h1, and i1 respectively represent the numbers of atoms of molybdenum, bismuth, nickel, cobalt, iron, X, Y, Z, and oxygen, and when a1=12, 0<b1≦7, 0≦c1≦10, 0<d1≦10, 0<c1+d1≦20, 0<e1≦5, 0≦f1≦2, 0≦g1≦3, 0≦h1≦5, and i1=a value determined by the oxidation state of each element). Mo 12 V a W b Cu c Sb d X e Y f Z g O h ・・・(1B) (In the formula, Mo, V, W, Cu, Sb, and O represent molybdenum, vanadium, tungsten, copper, antimony, and oxygen, respectively; X represents at least one element selected from the group consisting of alkali metals and thallium; Y represents at least one element selected from the group consisting of magnesium, calcium, strontium, barium, and zinc; Z represents bismuth, tellurium, silver, selenium, silicon, aluminum, boron, niobium, cerium, tin, chromium, manganese, iron, cobalt, nickel, samarium, germanium, zinc, and tin.) Each of the elements represents at least one element selected from the group consisting of zinc, titanium, chromium, tantalum, lead, indium, sulfur, palladium, gallium, lanthanum, and arsenic. In addition, a, b, c, d, e, f, g, and h represent the atomic ratio of each element, and with respect to 12 molybdenum atoms, a represents 0<a≦10.0, b represents 0≦b≦10.0, c represents 0<c≦6.0, d represents 0≦d≦10.0, e represents 0≦e≦0.50, f represents 0≦f≦1.0, and g represents 0≦g<6.
0. In addition, h represents the number of oxygen atoms required to satisfy the valence of each of the components. A method for producing a catalyst for producing an unsaturated aldehyde and / or an unsaturated carboxylic acid, wherein the storage conditions for ammonium heptamolybdate used as a molybdenum raw material include the following condition 2: Condition 2: The storage temperature during the storage period is 45°C or less, the container is non-permeable to moisture, and the following formula (3) is satisfied throughout the entire storage period. Accumulative total solar radiation during storage period [MJ / m 2 ]≦345 ... (3)
3. The composition of the catalytically active component is represented by the following general formula (1A) or (1B): Mo a1 Bi b1 Ni c1 Co d1 Fe e1 X f1 Y g1 Z h1 O i1 ・・・(1A) (In the formula, Mo, Bi, Ni, Co and Fe represent molybdenum, bismuth, nickel, cobalt and iron, respectively; X represents at least one element selected from tungsten, antimony, tin, zinc, chromium, manganese, magnesium, silicon, aluminum, cerium and titanium; Y represents at least one element selected from sodium, potassium, cesium, rubidium and thallium; Z represents an element belonging to Groups 1 to 16 of the periodic table; and , and at least one element selected from elements other than Y, and a1, b1, c1, d1, e1, f1, g1, h1, and i1 respectively represent the numbers of atoms of molybdenum, bismuth, nickel, cobalt, iron, X, Y, Z, and oxygen, and when a1=12, 0<b1≦7, 0≦c1≦10, 0<d1≦10, 0<c1+d1≦20, 0<e1≦5, 0≦f1≦2, 0≦g1≦3, 0≦h1≦5, and i1=a value determined by the oxidation state of each element). Mo 12 V a W b Cu c Sb d X e Y f Z g O h ・・・(1B) (In the formula, Mo, V, W, Cu, Sb, and O represent molybdenum, vanadium, tungsten, copper, antimony, and oxygen, respectively; X represents at least one element selected from the group consisting of alkali metals and thallium; Y represents at least one element selected from the group consisting of magnesium, calcium, strontium, barium, and zinc; Z represents bismuth, tellurium, silver, selenium, silicon, aluminum, boron, niobium, cerium, tin, chromium, manganese, iron, cobalt, nickel, samarium, germanium, zinc, and tin.) Each of the elements represents at least one element selected from the group consisting of zinc, titanium, chromium, tantalum, lead, indium, sulfur, palladium, gallium, lanthanum, and arsenic. In addition, a, b, c, d, e, f, g, and h represent the atomic ratio of each element, and with respect to 12 molybdenum atoms, a represents 0<a≦10.0, b represents 0≦b≦10.0, c represents 0<c≦6.0, d represents 0≦d≦10.0, e represents 0≦e≦0.50, f represents 0≦f≦1.0, and g represents 0≦g<6.
0. In addition, h represents the number of oxygen atoms required to satisfy the valence of each of the components. A method for producing a catalyst for producing an unsaturated aldehyde and / or an unsaturated carboxylic acid, wherein the storage conditions for ammonium heptamolybdate used as a molybdenum raw material include the following condition 3: Condition 3: The product is stored in a light-shielding container and satisfies the following formula (4) throughout the entire storage period. Storage absolute humidity [g / m 3 ] × number of storage days [days] ≦ 12.0 ... (4)
4. 4. A method for producing a catalyst for producing an unsaturated aldehyde and / or an unsaturated carboxylic acid according to claim 1, wherein ammonium heptamolybdate used as a molybdenum raw material is stored under storage conditions including two or more of the conditions 1 to 3, and the method for producing a catalyst for producing an unsaturated aldehyde and / or an unsaturated carboxylic acid according to any one of claims 1 to 3 satisfies the following formula (5): exp (保管温度[℃]-50) × number of days of storage [days] / 5200 + cumulative total solar radiation during the storage period [MJ / m 2 ] / 345 + storage absolute humidity [g / m 3 ] × number of storage days [days] / 12.0 ≦ 1.0 ・・・(5)
5. A method for producing a catalyst for producing an unsaturated aldehyde and / or an unsaturated carboxylic acid, comprising the steps of: preparing a mixture of ammonium heptamolybdate stored under the storage conditions according to any one of claims 1 to 3 and water; adding other raw materials; and obtaining an aqueous solution or aqueous slurry.
6. A method for producing a catalyst for producing an unsaturated aldehyde and / or an unsaturated carboxylic acid, comprising subjecting the aqueous solution or aqueous slurry according to claim 5 to the following steps (a) to (c): (a) drying the aqueous solution or aqueous slurry to obtain a dry body; (b) forming the dried slurry obtained in step (a) into a formed product; (c) A step of firing the molded product obtained in step (b) in an atmosphere having a controlled oxygen concentration.
Citation Information
Patent Citations
Catalyst for producing unsaturated aldehyde and / or unsaturated carboxylic acid and method for producing the same, and method for producing unsaturated aldehyde and / or unsaturated carboxylic acid
JP2015147188A
Oxide catalyst
JP2017024009A
Method for producing composite metal oxide catalyst for producing unsaturated aldehyde and unsaturated carboxylic acid, and method for producing unsaturated aldehyde and unsaturated carboxylic acid using the same
JP7024194B2
Catalyst for acrolein and / or acrylic acid production and process for producing acrolein and / or acrylic acid using the catalyst
WO2010038677A1
Catalyst for manufacturing unsaturated aldehyde and / or unsaturated carboxylic acid and manufacturing method of same, and manufacturing method of unsaturated aldehyde and / or unsaturated carboxylic acid
WO2016136882A1