Zinc-based plated steel sheet for hot stamping and method of producing the same

A zinc-based galvanized steel sheet with controlled carbon concentration and specific elemental composition addresses LME cracking and corrosion issues, achieving high strength and resistance in hot stamping applications.

JP2024144147APending Publication Date: 2024-10-11KOBE STEEL LTD

Patent Information

Application Number
JP2024022727
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-02-19
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing zinc-based coated steel sheets for hot stamping suffer from Liquid Metal Embrittlement (LME) cracking and reduced corrosion resistance due to high alloying element concentrations, which compromise joint strength and weldability.

Method used

A galvanized steel sheet composition with controlled carbon concentration at the interface between the plating layer and the base steel, achieved by maintaining [Cf] ≦ 0.65 × [Cb], along with specific elemental balances and manufacturing conditions, including a reducing atmosphere annealing process followed by zinc plating.

Benefits of technology

The solution provides a high-strength steel sheet with excellent LME resistance and corrosion resistance, ensuring tensile strength of 1470 MPa or more and minimal LME cracking, while maintaining weldability and productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144147000001_ABST
    Figure 2024144147000001_ABST
Patent Text Reader

Abstract

To provide a zinc-based plated steel sheet for hot stamping with excellent LME resistance and high strength, and a method of producing the zinc-based plated steel sheet.SOLUTION: The zinc-based plated steel sheet for hot stamping has a base steel sheet comprising C: 0.15 to 0.50 mass%, Si: 0.02 to 2.5 mass%, Mn: 0.5 to 5 mass%, P: 0.03 mass% or less (including 0 mass%), S: 0.02 mass% or less (including 0 mass%), Al: 0.010 to 1 mass%, Ti: 0.005 to 0.080 mass%, and B: 0.0005 to 0.005 mass%, with the balance being Fe and unavoidable impurities, in which when elemental analysis is performed from the surface of a plating layer in the thickness direction of the plating layer by glow discharge optical emission spectrometry (GD-OES), a carbon concentration [Cf] (mass%) at a position where a concentration of Zn constituting the plating layer is 1.0 mass% and a bulk carbon concentration [Cb] (mass%) satisfy Equation (1): [Cf]≤0.65×[Cb].SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a zinc-based coated steel sheet for hot stamping and a method for producing the same. [Background technology]

[0002] There has been a demand for improved safety for vehicle occupants, and for this purpose, the strength of the materials used in vehicle bodies has been improved. On the other hand, against the background of the worsening of global warming and other issues, there has been an accelerating movement to improve the fuel efficiency of automobiles. It is known that reducing the weight of vehicle bodies is an effective way to improve fuel efficiency.

[0003] For example, hot stamping (hot forming) steel sheets can easily achieve both high strength and workability (shape fixability, etc.) for the purpose of realizing vehicle body weight reduction. Hot-dip galvanized hot stamping steel sheets are used in areas where corrosion resistance is particularly required.

[0004] The following steel sheets have been proposed as the above-mentioned hot stamping (hot forming) steel sheets. For example, Patent Document 1 discloses a steel sheet for hot forming in which the relationship between Ti and N is specified, as a steel sheet for hot forming that has excellent strength of the joint when spot welded and can realize good forming without causing breakage or cracking during hot forming. Patent Document 2 discloses a hot stamping steel sheet that has both excellent balance of strength and toughness and excellent hardness stability, in which the proportions of alloy elements are increased to achieve high strength, such as by adjusting the balance of the contents of C, Si, Mn, and Cr.

[0005] However, when the ratio of alloying elements in a zinc-based coated steel sheet is increased, cracks (LME cracks) due to molten metal embrittlement (LME liquid metal embrittlement or LMC liquid metal cracking) are likely to occur. In particular, when the zinc-based coated steel sheet is hot stamped and formed into a part, and then spot-welded for vehicle body assembly, if LME cracks occur, there is a problem that the joint strength of the welded part is insufficient. Regarding this problem, for example, Patent Document 3 discloses that in a formed body obtained by hot stamping a galvannealed steel sheet, in order to improve weldability and chemical conversion treatability and to suppress LME, it is necessary to set the heating time in a furnace (furnace time) to about 4 minutes or more, and that since hot stamping is inferior in press productivity to cold pressing, it is required to shorten the furnace time. In view of this, it is proposed to increase the Fe concentration of the galvannealed coating in a galvannealed steel sheet for hot stamping to more than 8.0 mass%, and to reduce the coating weight (Zn amount is 15.0 to 40.0 g / m) in order to avoid the time required for Fe-Zn solid solution formation. 2 ) to raise the melting point of the plating. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2007-169679 A [Patent Document 2] JP 2019-173158 A [Patent Document 3] Patent Publication No. 2022-131411 [Non-patent literature]

[0007] [Non-Patent Document 1] Kimitaka Hayashi et al., "Behavior of the corrosion tip in undercoat corrosion of Zn-Fe alloy plated steel sheets," Tetsu-to-Haganen, No. 9, 76th year (1990), pp. 1496-1503 Summary of the Invention [Problem to be solved by the invention]

[0008] Although the technology of Patent Document 3 can suppress LME, the coating weight of the coating is reduced, so the effective amount of zinc that contributes to ensuring the corrosion resistance of the coating is reduced, making it difficult to achieve the effect of improving corrosion resistance, which is the original role of the coating. As shown in Non-Patent Document 1, it is known that the corrosion resistance of the coating is significantly deteriorated, especially when the Fe concentration in the coating exceeds 65 mass %. Therefore, it has been desired to simultaneously achieve high strength, suppression of LME, and ensuring corrosion resistance. The present disclosure has been made in view of the above circumstances, and its purpose is to provide a zinc-based coated steel sheet for hot stamping that exhibits excellent LME resistance while ensuring the inherent corrosion resistance of the coating, and further exhibits high strength (especially tensile strength of 1.5G class or more) after hot stamping, and a manufacturing method thereof. [Means for solving the problem]

[0009] Aspect 1 of the present invention is The composition of the base steel sheet is C: 0.15~0.50% by mass, Si:0.02~2.5% by mass, Mn: 0.5~5% by mass, P: 0.03% by mass or less (including 0% by mass), S: 0.02% by mass or less (including 0% by mass), Al: 0.010~1% by mass, Ti: 0.005 to 0.080 mass%; and B: 0.0005 to 0.005% by mass; The balance is Fe and unavoidable impurities. The zinc-based plated steel sheet for hot stamping is such that, when elemental analysis is performed by glow discharge optical emission spectrometry (GD-OES) from the surface of the plated layer in the thickness direction of the plated layer, the carbon concentration [Cf] (mass%) at a position where the concentration of Zn constituting the plated layer is 1.0 mass% and the bulk carbon concentration [Cb] (mass%) satisfy the following formula (1): [Cf]≦0.65×[Cb] (1)

[0010] Aspect 2 of the present invention is A zinc-based plated steel sheet for hot stamping according to Aspect 1, wherein a chemical composition of the base steel sheet satisfies at least one of the following (a) and (b): (a) Furthermore, Cr: more than 0 mass%, 1.2 mass% or less, Mo: more than 0 mass% and 1 mass% or less, and Ca: Contains one or more elements selected from the group consisting of more than 0 mass % and 0.0040 mass % or less. (b) Furthermore, Nb: more than 0 mass%, 0.040 mass% or less, V: more than 0% by mass, 0.30% by mass or less, Cu: more than 0 mass%, 0.30 mass% or less, Ni: more than 0 mass%, 0.30 mass% or less, Mg: more than 0 mass% and 0.010 mass% or less, and REM: Contains one or more elements selected from the group consisting of more than 0 mass % and 0.010 mass % or less.

[0011] Aspect 3 of the present invention is The method for producing a zinc-based plated steel sheet for hot stamping includes an annealing step in which a hot-rolled steel sheet or a cold-rolled steel sheet satisfying the component composition according to embodiment 1 or 2 is allowed to stay in a reducing atmosphere having a dew point of −20° C. to +10° C. at 500 to 930° C. for 90 to 1000 seconds, and a subsequent zinc-based plating step.

[0012] A fourth aspect of the present invention is In the method for producing a zinc-based plated steel sheet for hot stamping according to aspect 3, the zinc-based plating step is a hot-dip galvanizing step. Effect of the Invention

[0013] According to the present disclosure, it is possible to provide a high-strength zinc-based plated steel sheet for hot stamping having excellent LME resistance and a manufacturing method thereof. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a diagram showing the positions at which steel sheets for evaluation were taken in the examples. [Diagram 2] FIG. 1 shows carbon profiles of samples before hot stamping in the examples, with the carbon profile of a comparative example on the left and the carbon profile of an example of the present invention on the right. [Diagram 3] 1 is a SEM photograph showing an example of an EDX analysis area of ​​a sample before hot stamping in an example. [Figure 4] FIG. 1 is a diagram showing the results of EDX analysis of a sample before hot stamping in an example. [Diagram 5] FIG. 2 is a diagram showing a heat pattern of hot stamping in an embodiment. [Figure 6] FIG. 1 shows carbon profiles of samples after hot stamping in the examples, with the carbon profile of a comparative example shown on the left and the carbon profile of an example of the present invention shown on the right. [Figure 7] 1 is a SEM photograph showing an example of an EDX analysis area of ​​a sample after hot stamping in an example. [Figure 8] FIG. 1 is a diagram showing the results of EDX analysis of a sample after hot stamping in an example. [Figure 9] FIG. 4 is a diagram showing conditions of a welding test in the examples. [Figure 10] FIG. 2 is a diagram illustrating the positions at which samples for a welding test were taken in the examples. [Figure 11] FIG. 2 is a diagram illustrating the locations of crack observations on the cross section of a sample after a welding test in an example. [Figure 12] FIG. 1 is a diagram illustrating internal cracks and voids after a welding test in an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present inventors have conducted intensive research to obtain a zinc-based plated steel sheet for hot stamping, which exhibits high strength after hot stamping and is also excellent in LME resistance, on the premise of forming a zinc-plated layer for ensuring corrosion resistance. First, the present inventors conducted research and found that, unlike a general cold-rolled steel sheet, a phenomenon occurs in which carbon (C) is concentrated at the interface between the plated layer and the base steel (hereinafter referred to as the "plated base steel interface") when the steel sheet for hot stamping is heated during hot stamping (as shown in the carbon profile on the left in Fig. 6 described later, the carbon concentration [C] at the plated base steel interface after hot stamping: 0.303 mass % is higher than the carbon concentration of the bulk, 0.220 mass %). Carbon is known to be an element that deteriorates LME resistance, and the inventors first found that the main cause of the deterioration of LME resistance of steel sheets for hot stamping is this carbon concentration phenomenon.

[0016] The inventors have also found that, in order to suppress the phenomenon of carbon concentration at the plated steel base interface after hot stamping, it is important to suppress the carbon concentration at the plated steel base interface of a zinc-based plated steel sheet to be subjected to hot stamping, specifically, to satisfy the following formula (1). [Cf]≦0.65×[Cb] (1) In formula (1), [Cf] is the carbon concentration (mass%) at a position where the concentration of Zn constituting the plating layer is 1.0 mass% when elemental analysis is performed from the surface of the plating layer in the thickness direction of the plating layer by glow discharge optical emission spectrometry (GD-OES), and [Cb] is the bulk carbon concentration (mass%).

[0017] In the above formula (1), "the position where the concentration of Zn constituting the plating layer is 1.0 mass% when elemental analysis is performed from the surface of the plating layer in the thickness direction of the plating layer by glow discharge optical emission spectrometry (GD-OES)" refers to the interface with the plating base steel in this embodiment. In other words, the zinc plating layer refers to the region from the plating layer surface where the concentration of zinc (Zn) is 1 mass% or more. The elemental analysis performed from the surface of the plating layer in the thickness direction of the plating layer by glow discharge optical emission spectrometry (GD-OES) is performed by the method shown in the examples.

[0018] The bulk carbon concentration [Cb] (mass%) refers to the carbon (C) concentration determined by analyzing a hot stamping steel sheet having a size of total sheet thickness x 50 mm x 50 mm or more by a combustion-infrared absorption method. In determining the bulk carbon concentration, the analysis of the content of each bulk element may be performed by a conventional method, and is performed by the following method. Note that the steel sheet manufactured in the examples described below had a Si content of more than 0.7 mass%, so the Si content was determined by the gravimetric method as shown below, but when the Si content is 0.7 mass% or less, analysis by ICP is recommended. <Analysis method> Inductively coupled plasma atomic emission spectrometry (ICP): Si (when less than 0.7 mass%), Mn, P, Cu, sol-Al, Ni, Cr, Mo, V, Nb, Ti, B, Ca Frameless atomic absorption spectrometry: Sn Gravimetric method: Si (over 0.7% by mass) Combustion - Infrared absorption method: C, S Inert gas fusion - TCD method [N], inert gas fusion - infrared absorption method [O]: N, O

[0019] The present inventors have found that, as shown in the above formula (1), by reducing the carbon concentration at the interface between the plated steel and the base steel in the surface layer region of the zinc-based plated steel sheet before hot stamping to [bulk carbon concentration × 0.65] or less, i.e., by providing a surface decarburized layer, the carbon concentration at the interface between the plated steel and the base steel after hot stamping can be suppressed to 0.225 mass%, which is almost the same as the bulk carbon concentration, as shown in the carbon profile on the right side of FIG. 6, which will be described later. As a result, as shown in the examples, which will be described later, even when welding is performed using the plated steel sheet, LME cracking can be suppressed. From this, it is considered that by reducing the carbon in the surface layer region of the zinc-based plated steel sheet before hot stamping, the carbon concentration phenomenon after hot stamping can be suppressed, and as a result, an improvement effect in LME resistance is achieved. In the surface layer region of the zinc-based plated steel sheet before hot stamping, the carbon concentration at the interface between the plated steel and the base steel is preferably 0.60 or less of the bulk carbon concentration, more preferably 0.50 or less of the bulk carbon concentration. From the viewpoint of improving LME resistance, the smaller the ratio to the bulk carbon concentration, the more preferable. Taking into consideration the manufacturing conditions and the mechanical properties of the steel sheet after hot stamping, the lower limit of the ratio of the carbon concentration at the interface between the plated steel and the bulk carbon concentration may be about 0.01.

[0020] The reduction in the carbon concentration at the interface with the plated steel substrate in the zinc-based plated steel sheet before hot stamping can be achieved by manufacturing the steel sheet under the conditions described below.

[0021] [Component composition] Hereinafter, the composition of the base steel sheet (referring to the portion of the plated steel sheet excluding the plating layer) in the zinc-based plated steel sheet for hot stamping according to this embodiment will be described. In the zinc-based plated steel sheet for hot stamping according to this embodiment, by satisfying the composition of the following components, it is possible to ensure a strength of 1.5 GPa or more after hot stamping, and also to improve part productivity, plating property, and LME resistance.

[0022] [C:0.15~0.50% by mass] C is an element effective in improving the strength of steel sheets, and in order to achieve a strength of TS: 1470 MPa or more after hot stamping, the C content needs to be 0.15 mass% or more. The C content is preferably 0.18 mass% or more, more preferably 0.20 mass% or more. On the other hand, if the C content exceeds 0.50 mass%, high strength is easily achieved, but problems such as an excessive increase in strength of the original sheet such as a hot-rolled steel sheet and deterioration of weldability occur. In addition, C is also an element that adversely affects LME resistance. Therefore, the C content is 0.50 mass% or less, preferably 0.40 mass% or less, more preferably 0.38 mass% or less, and even more preferably 0.35 mass% or less.

[0023] [Si:0.02~2.5% by mass] Since Si has the effect of suppressing the self-tempering of martensite, it is an element effective in improving hardness stability and thus ensuring productivity during component manufacturing. In addition, the inclusion of a small amount of Si exerts the effect of suppressing non-plating during steel sheet manufacturing. In order to exert these effects, the Si content is set to 0.02 mass% or more. The Si content is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 0.7 mass% or more. On the other hand, if the Si content exceeds 2.5 mass%, the Ac3 point rises, which leads to an increase in the hot stamp heating temperature during component manufacturing. Furthermore, Si is an element that adversely affects LME resistance. Although the cause of this is not clear, it is considered that this is because Si dissolves in the plating and lowers the melting point of the plating from the research results of the present inventors. From these viewpoints, the Si content is set to 2.5 mass% or less. The Si content is preferably 2.4 mass% or less, more preferably 2.2 mass% or less.

[0024] [Mn:0.5~5% by mass] Mn is an element necessary for ensuring hardenability and achieving a strength of TS: 1470 MPa or more after hot stamping. Therefore, the Mn content is set to 0.5 mass% or more. The Mn content is preferably 1.0 mass% or more, and more preferably 1.5 mass% or more. On the other hand, an excessive Mn content leads to an excessive increase in strength of the base sheet such as a hot-rolled steel sheet. Mn is also an element that deteriorates LME resistance. Therefore, the Mn content is set to 5 mass% or less. The Mn content is preferably 4.5 mass% or less, and more preferably 4.0 mass% or less.

[0025] [P: 0.03% by mass or less (including 0% by mass)] P is an element that is inevitably present as an impurity element. P has an adverse effect on toughness and delayed fracture resistance. Therefore, the less P, the better, and the P content is 0.03 mass% or less, and preferably 0.010 mass% or less. In this specification, "including 0 mass%" means that it is not intentionally added, that is, it includes the case where the content is below the unavoidable impurity level (it does not exclude the case where it is intentionally added).

[0026] [S: 0.02% by mass or less (including 0% by mass)] S is an element that is inevitably present as an impurity element. S has a detrimental effect on toughness and delayed fracture resistance. Therefore, the less S, the better. The S content is 0.02 mass% or less, preferably 0.010 mass% or less, and more preferably 0.005 mass% or less.

[0027] [Al:0.010~1% by mass] Al is an element that acts as a deoxidizer. To achieve this effect, the Al content is set to 0.010% by mass or more. The Al content is preferably 0.015% by mass or more. On the other hand, if the steel sheet contains excessive Al, the hardness after die cooling decreases. In addition, the low-temperature toughness deteriorates due to the excessive generation of Al2O3. For this reason, the Al content is set to 1% by mass or less. The Al content is preferably 0.8% by mass or less, and more preferably 0.1% by mass or less. The Al content here refers to the content of Al in a solid solution state (sol.Al).

[0028] [Ti:0.005~0.080% by mass] Ti has the effect of precipitating N, which has an adverse effect on the solid solution of B, with Ti to render it harmless, in order to realize the effect of B described later. In addition, Ti has the effect of increasing the amount of solid solution of B by being contained together with B, and improving resistance to LME cracking. In order to realize these effects, the Ti content is set to 0.005 mass% or more. The Ti content is preferably 0.010 mass% or more, more preferably 0.015 mass% or more, and further preferably 0.020 mass% or more. On the other hand, if the Ti content is excessive, precipitation of carbides, grain refinement, etc. occur, the strength of the original sheet such as a hot-rolled steel sheet increases more than necessary, and the workability is deteriorated, which adversely affects the economy. Therefore, the Ti content is 0.080 mass% or less. The Ti content is preferably 0.070 mass% or less, more preferably 0.060 mass% or less.

[0029] [B:0.0005~0.005% by mass] B is an element necessary for ensuring hardenability and achieving a strength of TS: 1470 MPa or more after hot stamping. It also has the effect of improving the resistance to LME cracking of the welded portion when welding. The reason why this effect is exhibited is unknown, but from the research results of the present inventors, it is considered that it is because it has the effect of strengthening the prior γ grain boundary which is the starting point of cracking. In order to exhibit these effects, the B content needs to be 0.0005 mass% or more. The B content is preferably 0.0010 mass% or more, and more preferably 0.0015 mass% or more. On the other hand, if the B content is excessive, the strength of the original sheet such as a hot-rolled steel sheet increases more than necessary, and the workability is deteriorated, which adversely affects the economy. Therefore, the B content is 0.005 mass% or less. The B content is preferably 0.004 mass% or less, and more preferably 0.003 mass% or less.

[0030] The zinc-based plated steel sheet according to the embodiment of the present invention includes the above-mentioned composition, and in one embodiment of the present invention, the balance is preferably iron and inevitable impurities. As inevitable impurities, the inclusion of elements brought in due to the conditions of raw materials, materials, manufacturing facilities, etc. is permitted. N is also an element that is inevitably present as an impurity element, and may be contained in a range of, for example, 0.0100 mass% or less (including 0 mass%). Note that, for example, like P and S, the lower the content is usually the better, and therefore they are inevitable impurities, but there are elements whose composition ranges are separately specified as above. For this reason, in this specification, the "unavoidable impurities" that constitute the balance are a concept that excludes elements whose composition ranges are separately specified.

[0031] The composition of the steel sheet in this embodiment does not need to contain the elements described below. Any other elements may be further contained as long as the desired properties can be maintained. By containing the elements described below as necessary, for example, it is possible to improve delayed fracture resistance and further improve LME resistance.

[0032] [(a) further, Cr: more than 0 mass%, 1.2 mass% or less, Mo: more than 0 mass% and 1 mass% or less, and Ca: one or more elements selected from the group consisting of more than 0 mass% and 0.0040 mass% or less. Cr is an element that can further improve resistance to LME cracking while ensuring hardenability. To achieve this effect, the Cr content is preferably more than 0 mass%, more preferably 0.05 mass% or more. On the other hand, if the Cr content is excessive, pickling properties required in the manufacturing process are deteriorated. Furthermore, it leads to an excessive increase in strength of the original sheet such as a hot-rolled steel sheet. Therefore, the Cr content is preferably 1.2 mass% or less, more preferably 1.0 mass% or less.

[0033] Mo has the effect of promoting the diffusion of B and suppressing the susceptibility to LME. From the viewpoint of exerting this effect, the Mo content is preferably more than 0 mass%, more preferably 0.05 mass% or more. On the other hand, if the Mo content is excessive, it leads to an excessive increase in strength of the base sheet such as a hot-rolled steel sheet, and has a negative effect on the economy due to poor workability, etc. Therefore, the Mo content is preferably 1 mass% or less.

[0034] Ca is an element that suppresses the formation of MnS, which adversely affects delayed fracture resistance, and improves delayed fracture resistance. From the viewpoint of exerting this effect, the Ca content is preferably more than 0 mass%, and more preferably 0.001 mass% or more. On the other hand, even if the Ca content is excessive, the effect is saturated and there is an adverse effect on economy, such as an increase in cost. Therefore, the Ca content is set to 0.0040 mass% or less.

[0035] [(b) further, Nb: more than 0 mass%, 0.040 mass% or less, V: more than 0% by mass, 0.30% by mass or less, Cu: more than 0 mass%, 0.30 mass% or less, Ni: more than 0 mass%, 0.30 mass% or less, Mg: more than 0 mass% and 0.010 mass% or less, and REM: one or more elements selected from the group consisting of more than 0% by mass and 0.010% by mass or less.

[0036] Nb forms fine carbides and refines the structure of steel through a pinning effect, thereby contributing to improving strength and toughness. In order to exert this effect, the Nb content is preferably more than 0 mass%, more preferably 0.0008 mass% or more. On the other hand, if the steel plate contains excessive Nb, coarse carbides are formed, which become the starting point of fracture and lead to deterioration of toughness. Therefore, the Nb content is preferably 0.040 mass% or less.

[0037] V forms fine carbides, refines the steel structure through a pinning effect, and contributes to improving strength and toughness. It also has a secondary effect by precipitating during tempering. In order to exert these effects, the V content is preferably more than 0 mass%, more preferably 0.008 mass% or more. On the other hand, if the steel plate contains too much V, coarse carbides are formed, which become the starting point of fracture and lead to a deterioration in toughness. Therefore, the V content is preferably 0.30 mass% or less.

[0038] Cu and Ni are elements effective in improving the delayed fracture resistance of components, and may be contained in amounts exceeding 0 mass% if necessary. On the other hand, excessive Cu and Ni in a steel sheet may cause defects on the surface of the steel sheet and ultimately on the surface of the component. For this reason, the individual contents of Cu and Ni are preferably 0.30 mass% or less, and the total content is more preferably 0.50 mass% or less.

[0039] Mg and REM have the function of refining inclusions in the steel sheet and preventing cracks caused by the inclusions during hot forming, so they may be contained as necessary. When contained, the content of each element is preferably more than 0 mass%, more preferably 0.0008 mass% or more. On the other hand, even if these elements are contained in excess, the effect is saturated and costs increase. Therefore, the content of each element is preferably 0.010 mass% or less, more preferably 0.008 mass% or less. The above-mentioned REM means to include lanthanoid elements (15 elements from La to Lu), Sc (scandium), and Y (yttrium).

[0040] The type of zinc-based coating in the zinc-based coated steel sheet for hot stamping according to the present embodiment is not limited. Examples include Fe-Zn coating, Al-Zn coating, etc. The Fe concentration in the coating layer of the zinc-based coated steel sheet for hot stamping according to the present embodiment is preferably 40 mass% or less, more preferably 30 mass% or less. Specific examples of the zinc-based coated steel sheet include hot-dip galvanized steel sheet (GI), alloyed hot-dip galvanized steel sheet (GA), and electrolytic galvanized steel sheet (EG).

[0041] The coating weight of the zinc-based coating (particularly hot-dip galvanizing and galvannealed hot-dip galvanizing) of the zinc-based coated steel sheet for hot stamping according to this embodiment is 45 g / m from the viewpoint of ensuring corrosion resistance. 2 More preferably, it is 60 g / m or more. 2 More preferably, it is 65 g / m 2 On the other hand, from the viewpoint of easily achieving the recommended Fe concentration in the plating layer, it is preferable that the coating weight of the zinc-based plating is small. Therefore, the coating weight of the zinc-based plating is 190 g / m 2 It is preferable that the thickness is 180 g / m or less, and more preferably 180 g / m 2 The following is the result.

[0042] The zinc-based plated steel sheet for hot stamping according to the present embodiment is used and hot stamped by the method described in the Examples below. The zinc-based plated steel sheet has an Fe concentration of 65 mass% or less, more preferably 60 mass% or less. From the viewpoint that the Fe concentration of the plated steel increases by hot stamping, the Fe concentration can be 20 mass% or more.

[0043] According to this embodiment, as described above, the predetermined component composition is satisfied and a predetermined surface decarburization layer is provided, thereby improving LME resistance without reducing the coating weight of the coating or increasing the Fe concentration in the hot-dip galvanized layer.

[0044] [Method of manufacturing zinc-based coated steel sheet for hot stamping] Next, a method for producing a zinc-based plated steel sheet for hot stamping according to this embodiment will be described.

[0045] The method for producing a zinc-based plated steel sheet for hot stamping according to this embodiment includes an annealing step in which a hot-rolled steel sheet or a cold-rolled steel sheet satisfying the above-mentioned component composition is allowed to stay at 500 to 930°C for 90 to 1000 seconds in a reducing atmosphere having a dew point of -20°C to +10°C, and a subsequent zinc-based plating step.

[0046] The annealing process and the subsequent zinc-based plating process, which are features of the manufacturing method according to this embodiment, will be described first. In the following, as an example, the annealing process and the subsequent zinc-based plating process (particularly the hot-dip galvanizing process) according to this embodiment are performed in a hot-dip galvanizing line of a reduction furnace type, but the present invention is not limited to this. The method according to this embodiment is not limited to the above-mentioned embodiment, and for example, the hot-dip galvanizing line can also be performed in a continuous annealing line of a non-oxidizing furnace type.

[0047] (Annealing process) The annealing process of a hot-dip galvanizing line is usually composed of a reducing furnace and a cooling zone. The present embodiment is characterized in that the annealing conditions in the reducing furnace, particularly the dew point of the reducing atmosphere, are appropriately controlled. The raw sheet is charged into the reducing furnace. The raw sheet charged into the reducing furnace may be subjected to a pretreatment process, such as degreasing, as described below, as necessary. The raw sheet charged into the reducing furnace may also be subjected to an oxidation treatment in an oxidation furnace after the pretreatment process, as necessary.

[0048] In the reduction furnace, the raw sheet is subjected to heat treatment in a reducing atmosphere. The dew point of the reducing atmosphere is set to -20°C to +10°C. By setting the dew point within this range, decarburization of the surface layer of the steel sheet occurs, and a desired surface layer region can be obtained. The dew point of the reducing atmosphere is preferably -15°C or higher, more preferably -10°C or higher. The dew point of the reducing atmosphere is preferably +5°C or lower, more preferably 0°C or lower.

[0049] The dew point can be controlled, for example, by introducing water vapor gas and mixing it with the atmospheric gas in the furnace, or by bubbling the atmospheric gas and mixing water vapor into it. The reducing atmosphere is not particularly limited as long as it satisfies the dew point and is reducing. The reducing atmosphere satisfies the dew point and is preferably, for example, a H2-N2 mixed gas having an H2 concentration of 1 to 30% by volume.

[0050] The annealing temperature is 500 to 930° C., and the residence time at the annealing temperature, i.e., the annealing time, is 90 to 1000 seconds. Annealing in the above temperature range is also called soaking treatment, and in this case, the annealing temperature is called the soaking temperature, and the annealing time is called the soaking time.

[0051] The annealing temperature is preferably 530°C or higher, more preferably 560°C or higher, and even more preferably 600°C or higher. The annealing temperature is preferably 900°C or lower, and more preferably 870°C or lower. The annealing time is preferably 100 seconds or higher, and more preferably 120 seconds or higher. The annealing time is preferably 900 seconds or lower, more preferably 700 seconds or lower, more preferably 500 seconds or lower, more preferably 400 seconds or lower, and even more preferably 350 seconds or lower. The annealing time can be controlled by the speed at which the original sheet passes through the reduction furnace (hereinafter also referred to as "line speed" or "LS" for short). "Staying at 500 to 930°C for 90 to 1000 seconds" means that the sheet stays within the annealing temperature range of 500 to 930°C for 90 to 1000 seconds, and the temperature may be constant or may vary within the above annealing temperature range.

[0052] According to the manufacturing method of this embodiment, a predetermined surface decarburized layer can be provided by particularly performing the above-mentioned annealing on a hot-rolled steel sheet or a cold-rolled steel sheet, which is an original sheet having the above-mentioned component composition.

[0053] A pretreatment process of the original sheet that can be performed before the annealing process will be described. The pretreatment is usually performed to remove oil (fat) and dirt attached to the surface of the original sheet, and is typically alkaline degreasing. The alkali contained in the degreasing solution used in the alkaline degreasing is not particularly limited as long as it can remove fats and oils as water-soluble soap, for example, caustic soda, silicate, or a mixture thereof. In addition, in order to improve the degreasing property, electrolytic cleaning, scrubber treatment, and addition of a surfactant or chelating agent to the degreasing solution can also be performed. In this embodiment, the method of pretreatment is not limited as long as the surface of the original sheet is appropriately degreased, and the above-mentioned treatments may be performed alone or in any combination.

[0054] The raw sheet that has left the reduction furnace can be cooled in a cooling zone. The cooling zone can be composed of a slow cooling zone, a quenching zone, and an adjustment zone. The adjustment zone is also called a holding zone. Cooling can be performed under commonly used conditions so as to prevent the occurrence of bare spots, and examples of such methods include cooling the steel sheet by blowing a gas in a reducing atmosphere onto the steel sheet.

[0055] In a hot-dip galvanizing line using a reduction furnace, the process can generally be divided into a pretreatment process, an annealing process, and a plating process. In the plating process, an alloying process is also performed as necessary.

[0056] From the viewpoint of energy saving, after the pretreatment step and before entering the reduction furnace, the pretreated raw sheet may be preheated in a preheating furnace having a reducing or oxidizing atmosphere using exhaust gas.

[0057] (Zinc-based plating process) After the annealing process (continuous annealing process), a galvanizing process is included. In the following, a hot-dip galvanizing process will be described as an example of a galvanizing process. A hot-dip galvanized steel sheet (GI) is produced by the hot-dip galvanizing process. Alternatively, the GI may be alloyed to produce an alloyed hot-dip galvanized steel sheet (GA).

[0058] The above hot-dip galvanizing step is not particularly limited, and a commonly used method can be adopted. For example, the temperature of the hot-dip galvanizing bath may be controlled to about 430 to 500°C. The coating weight of the hot-dip galvanizing layer (the same as the coating weight of the alloyed hot-dip galvanizing layer described below) is set to 45 g / m2 from the viewpoint of ensuring corrosion resistance. 2 More preferably, it is 60 g / m or more. 2 More preferably, it is 65 g / m 2 On the other hand, from the viewpoint of easily achieving the recommended Fe concentration in the coating layer, it is preferable that the coating weight of the hot-dip galvanized layer (particularly the alloyed hot-dip galvanized layer) is small. Therefore, the coating weight of the hot-dip galvanized layer is set to 190 g / m 2 It is preferable that the thickness is 180 g / m or less, and more preferably 180 g / m 2 The following is the result.

[0059] The alloying treatment is not particularly limited, and a method that is usually used can be adopted. In the alloying treatment, when the Fe concentration in the plating layer is increased, the alloying temperature is controlled to, for example, about 400 to 700°C. The alloying temperature is furthermore 430°C or higher, furthermore 440°C or higher, and furthermore 450°C or higher. On the other hand, if the alloying temperature is too high, the Fe concentration in the plating layer becomes too high, so the alloying temperature is preferably 680°C or lower, more preferably 650°C or lower.

[0060] The steps after the plating step are not particularly limited, and a commonly used method can be adopted. Usually, skin pass treatment, tension leveler treatment, oil coating, etc. are performed, but these may be performed under commonly used conditions as necessary, and may not be performed if unnecessary. The zinc-plated steel sheet (GI or GA) obtained in this way is suitably used as a steel sheet for hot stamping.

[0061] Instead of the above-mentioned hot-dip galvanizing, electroplating may be performed. For example, the base sheet may be subjected to the above-mentioned annealing and then electroplated to obtain an electrogalvanized steel sheet having the plated base steel interface specified in this embodiment.

[0062] (Other processes) The manufacturing method according to the present embodiment may include the annealing step and the subsequent zinc-based plating step, and other steps are not limited and may include steps that are normally performed. Therefore, the manufacturing method of the hot-rolled steel sheet or cold-rolled steel sheet to be subjected to the annealing step does not matter, and for example, the hot-rolled steel sheet or cold-rolled steel sheet can be manufactured as follows. First, a slab is manufactured. In the slab manufacturing step, a slab is obtained by melting steel according to a normal method, pouring the molten steel into a mold and continuously casting it. In this step, the composition of the steel is adjusted during melting so as to satisfy the above-mentioned composition range. After casting and before hot rolling, a heating step may be provided so as not to cause cracks during hot rolling (this step is different from the slab heating step in the hot rolling step described below). The heating conditions are not particularly limited, and normally used conditions can be appropriately adopted, but it is preferable to perform the heating at a temperature of about 1100°C to 1300°C.

[0063] In the hot rolling process, the slab is first placed in a heating furnace and heated to a predetermined temperature (approximately 1100° C. to 1300° C., for example, 1200° C.), and then held at that heating temperature for a predetermined time (for example, 30 minutes).

[0064] Next, the heated slab is placed upstream of a hot rolling line, and the slab is rolled into a steel plate having a predetermined thickness by passing between rolls of the rolling stands of a roughing mill and a finishing mill in sequence and proceeding downstream. After hot rolling, the steel plate is cooled to a predetermined temperature in a cooling device and then wound up by a coiler.

[0065] The hot-rolled steel sheet may be a hot-rolled pickled steel sheet that is subsequently pickled in a pickling process. In the pickling process, at least the hot-rolled scale may be removed by pickling. The hot-rolled pickled steel sheet may be cold-rolled as necessary. In the cold rolling process, the hot-rolled steel sheet is further rolled to reduce the sheet thickness. Specifically, the hot-rolled steel sheet after pickling is passed between rolls of a rolling stand to further reduce the thickness. The cold-rolled steel sheet is particularly suitable for use in automobile parts for the purpose of reducing the weight of automobiles. The base steel sheet constituting the zinc-based plated steel sheet is preferably a cold-rolled steel sheet from the viewpoints of dimensional accuracy and flatness. The hot-rolled steel sheet (including the hot-rolled pickled steel sheet) or the cold-rolled steel sheet (hereinafter, these are collectively referred to as "original sheet") may be subjected to the annealing process and the zinc-based plating process, for example, a continuous plating process using a reduction furnace. EXAMPLES

[0066] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples, and can be practiced with appropriate modifications within the scope of the above and below-mentioned aims, and all such modifications are included in the technical scope of the present invention.

[0067] A steel material having the composition shown in Table 1 was melted in a converter, and then a slab was produced by continuous casting. The obtained slab was heated at a temperature of 1100°C to 1300°C, and then hot-rolled under the conditions of FDT: 890°C to 950°C and coiling temperature of 500°C to 700°C, and then descaling treatment was performed in a pickling process, and then cold rolling was performed to obtain a cold-rolled steel sheet. The cold rolling rate during cold rolling was 20% or more. The obtained cold-rolled steel sheet had a sheet thickness of 1.2 mm. In this example, a plated steel sheet was produced using the cold-rolled steel sheet as a base sheet. In Table 1, the underlined values ​​indicate that they are outside the range specified in this embodiment. The same applies to the following tables. Steel type 2 in Table 1 is a comparative steel type because the carbon (C) is too low.

[0068] [Table 1]

[0069] The obtained cold-rolled steel sheet was subjected to reduction annealing in a hot-dip galvanizing annealing line under the conditions (soaking temperature (annealing temperature), soaking time (annealing time), dew point) shown in Table 2. In Experiments Nos. 1 to 7, after immersion in the galvanizing bath, alloying was performed under the conditions (alloying temperature, alloying time) shown in Table 2 to obtain a galvannealed hot-dip galvanized steel sheet (GA steel sheet) having a width of about 1000 mm and having both sides of the steel sheet subjected to alloying hot-dip galvanizing. The GA steel sheet is also a steel sheet for hot stamping. The GA steel sheet is sometimes called the "steel sheet before hot stamping". In Experiments Nos. 8 to 10, a small sample of 150 mm x 80 mm was used for plating (decarburization) annealing. It was separately confirmed that the decarburization state and strength of this small sample were equivalent to those of the above-mentioned steel sheet. In Experiments Nos. 8 to 10, the coating weight was not measured. A separate evaluation of a material annealed under the same conditions showed a coating weight of 180 g / m 2 Therefore, it is assumed that the same coating weight (weight per unit area) is applied in Experiments 8 to 10. In Table 2, the coating weight is set to 180 g / m 2 It shows that:

[0070] [Table 2]

[0071] In Experiments No. 1 to 7, evaluation steel sheets with dimensions of 150 mmW x 70 mmL or 220 mmW x 150 mmL were taken from the central portion (range W / 4 to 3W / 4 in the width direction) a and the end portion (region furthest from the end) b of the above GA steel sheets in Fig. 1. The positions from which the evaluation steel sheets were taken in each example are shown in Table 5. In Experiments No. 8 to 10, the small samples (size: 150 mmW x 80 mmL) obtained above were used without cutting.

[0072] Using each evaluation steel sheet, the decarburization state of the surface layer of the steel sheet and the Fe concentration in the plating layer before hot stamping were measured as follows.

[0073] [Measurement of the decarburization state of the surface layer (before hot stamping) (measurement of carbon profile by GD-OES)] As described below, the carbon profile was measured by GD-OES (glow discharge optical emission spectrometry) to investigate the decarburization behavior.

[0074] (Sample preparation) Materials with dimensions of 50 mm x 40 mm x 1.2 mm (total thickness) or 30 mm x 30 mm x 1.2 mm (total thickness) or 30 mm x 40 mm x 1.2 mm (total thickness) were collected. After that, samples were prepared by degreasing in the usual manner. Then, using the samples, the mass% concentration of each element was measured by GD-OES under the following conditions.

[0075] (Measurement conditions) Equipment used: Horiba, Ltd. Marcus type radio frequency glow discharge optical emission surface analyzer (rf-GD-OES) GD-Profiler2 Sputtering method: Normal sputtering Measurement range: φ4mm Gas type: Ar Analyzed elements: B, C, O, Al, Si, Ti, Cr, Mn, Fe, Zn, P, S, N (In this example, the evaluation was performed on these elements, but if elements other than the above are contained in, for example, the plating layer or steel sheet, the other elements will also be analyzed.)

[0076] (Measurement method) GD-OES measurements were performed on the plated surface of the sample up to a depth of 150 μm in the plate thickness direction.

[0077] (Analysis method) Since the sputtering rate of this device is almost constant, the sputter crater depth of the sample was measured after the analysis was completed, and the value (sputter depth) was plotted on the horizontal axis.

[0078] The details of the calibration curve method for converting the measured emission intensity of each element into a concentration are shown below. Sputter weight of element i per unit time W i (g / sec) and luminescence intensity I i The relationship is expressed by the following formula (I) using the slope a and intercept b of the calibration curve. W i =aI i +b...Formula (I) The sputter weight W of the above element i per unit time i is the concentration C i (wt.%), density ρ(g / cm 3 ), and the sputtering rate Δd (cm / sec) of the reference sample are known. 2 ) and is calculated according to the following formula (II). W i =C i ×ρ×Δd×S...Formula (II)

[0079] W i Using two or more reference samples with known emission intensities I i was measured, the slope a and intercept b of the above formula (I) were determined, and a calibration curve was prepared in which the horizontal axis is the emission intensity and the vertical axis is the sputter weight. The reference samples used are shown in Table 3 below. Using the prepared calibration curve, the sputter weight was calculated from the emission intensity of each target element, and the concentration was converted from the weight ratio. The calibration curve used to convert the O concentration was corrected using SiO2 so that the concentration ratio of Si to O was 1:2.

[0080] [Table 3]

[0081] From the above analysis results, a zinc and carbon profile was obtained, which is the result of analyzing zinc and carbon. From the zinc and carbon profile, the carbon concentration [Cf] at the position where the concentration of Zn constituting the plating layer was 1.0 mass% was obtained. The bulk carbon concentration [Cb] was obtained by the analysis described above. The value of [Cf] / [Cb] was then calculated. The results are shown in Table 5.

[0082] As an example of the carbon profile, the carbon profile of Experiment No. 4, which is a conventional steel as a comparative example, is shown on the left side of Figure 2, and the carbon profile of Experiment No. 1, which is an example of the present invention, is shown on the right side of Figure 2. From the comparison of these carbon profiles, it can be seen that in the example of the present invention, the carbon concentration at the interface between the plating layer and the base steel plate is sufficiently suppressed.

[0083] Note that in Experiment No. 6, the C concentration at the subway plating interface was not evaluated. However, since it has the same component composition as Experiment No. 7 and the reduction annealing conditions are also approximated, it is considered that the C concentration at the subway plating interface is approximated to that of Experiment No. 7. Therefore, since the C concentration at the subway plating interface of No. 6 is estimated to be about 0.070, which is equivalent to that of Experiment No. 7, the value is entered in Table 5.

[0084] [Measurement of Fe Concentration in the Plating Layer (Before Hot Stamping)] Samples with a size of 20 mmW × 10 mmL × plate thickness were cut and collected from the above GA steel plate (the steel plate before hot stamping). Degreasing was performed as necessary.

[0085] [Preparation of Observation Samples] Embedded in resin so that the L-direction cross-section, that is, the surface formed by the plate thickness and 10 mmL as sides, becomes the observation surface, polished, and then gold vapor deposition was performed.

[0086] [SEM Observation] SEM observation and EDX analysis were performed under the following conditions. In this example, the observation magnification was set to 1500 times. However, since the observation magnification depends on the deposition amount of the plating, for example, when the plating thickness increases, it is advisable to select an appropriate magnification for the measurement of the Fe concentration, such as reducing the measurement magnification. [SEM Observation Conditions] · Equipment: Field Emission Scanning Electron Microscope (FE-SEM) Supra-35 manufactured by Carl Zeiss · Observation Image: Backscattered Electron Image · Observation Location: Near the surface layer including the plating layer · Observation Magnification: 1500 times · Number of Observation Fields: 1 field / 1 sample representing the sample

[0087] <EDX Analysis> · Equipment: Energy Dispersive X-ray (EDX) Detector X-max80 manufactured by Oxford Instruments · Analysis method: Area analysis (qualitative semi-quantitative analysis) · Analysis location: The entire plating layer. An example of the analysis area is shown in Figure 3. · Number of analysis fields of view: 1 field of view per sample representative of the sample · Analyzed elements: When considering the elements detected by EDX excluding C as the population, the percentage by mass of Fe evaluated was defined as the Fe concentration (%). As an example, the analysis results of Experiment No. 4 are shown in Figure 4. Also, as an example, the calculation results of the Fe concentration (12.0 mass%) for Experiment No. 4 are shown in Table 4. Table 5 shows the Fe concentrations in the plating layers of each example calculated in the same manner as the following Table 4.

[0088]

Table 4

[0089]

Table 5

[0090] [Evaluation of Steel Sheet after Hot Stamping] To evaluate the steel sheet after hot stamping, the above evaluation steel sheet was hot stamped as follows. First, degreasing was performed by a conventional method to suppress carburization during hot stamping heating. Subsequently, hot stamping was carried out according to the following conditions and the heat pattern in Figure 5 to obtain a sample after hot stamping.

[0091] (Hot Stamping Conditions) · Size of the sample used: 150 mm W × 70 mm L or 150 mm W × 220 mm L or 150 mm W × 80 mm L (small sample) · Mold used: Flat mold <Heating Conditions> · Set temperature of the atmospheric electric furnace: 910 °C Heating time: After the sheet temperature reached 870℃, it was held at that temperature for 45 seconds (during that time, the sheet temperature was controlled to be between 870℃ and 900℃). <Cooling conditions> After that, it was left to cool naturally, and when the plate temperature reached 550℃ or 700℃, both flat surfaces were pressed with a die for flat plates to cool them down. Press load: 0.5MPa Press speed: 20spm Push-in depth: 5mm Bottom dead center holding time: The bottom dead center was held until the temperature dropped below 50°C (10 seconds in this case).

[0092] The hot stamped samples were used to evaluate the tensile strength TS, LME resistance, and other properties as described in detail below.

[0093] [Shot blasting] The resistance value of the steel sheet was measured for the samples after hot stamping in accordance with a method partially described in ISO-18594:2007(E). Shot blasting was performed under the following resistance measurement conditions so that the surface resistance would be 2.0 mΩ or less. The respective shot blasting conditions are shown in Table 6. Note that in Experiments No. 8 to 10, the resistance value after shot blasting was not measured, but since the average resistance value of materials prepared under approximately the same conditions (Experiments No. 1 to 5) was 0.9 mΩ, it was assumed to be approximately the same, and is shown as 0.9 (mΩ) in Table 6 below.

[0094] (Shot blasting conditions) Shot material: GH-3 (grid 0.3 mm) Shot pressure: Approx. 0.4MPa - Manage the shot blasting time per 150mm x 120mm area (details of shot blasting time are shown in Table 6) -Shot blasting on both sides Shot blasting was performed until the resistance of the steel plate reached 2.0 mΩ or less.

[0095] (Resistance measurement conditions) Three pieces of material measuring 30mm x 30mm x thickness were cut and collected. ·Electrode material: Cu-Cr ·Electrode diameter Φ8mm Tip R: 40mm DC current: 2A Pressure: 350±17.5×10N However, each sample was measured once, and a total of three measurements were made for each experimental sample. The average value of N3 was taken as the value. The plated side of one steel sheet was clamped between electrodes and the measurement was performed. The resistance value was calculated by subtracting the setup resistance from the total resistance.

[0096] [Table 6]

[0097] [Measurement of the decarburization state of the surface layer after hot stamping (measurement of carbon profile by GD-OES)] As described below, the carbon profile was measured by GD-OES (Glow discharge optical emission spectrometry) to investigate the decarburization behavior after hot stamping.

[0098] (Sample preparation) Materials measuring 30 mm x 90 mm x thickness or 30 mm x 70 mm x thickness were collected. After that, samples were prepared by degreasing in the usual manner. Then, using the samples, the mass% concentration of each element was measured by GD-OES under the following conditions.

[0099] (Measurement conditions) Equipment used: Horiba, Ltd. Marcus type radio frequency glow discharge optical emission surface analyzer (rf-GD-OES) GD-Profiler2 Sputtering method: Normal sputtering Measurement range: φ4mm Gas type: Ar Analyzed elements: B, C, O, Al, Si, Ti, Cr, Mn, Fe, Zn (In this embodiment, the evaluation was performed on these elements, but if elements other than those mentioned above are contained in, for example, the plating layer or the steel sheet, the elements other than those mentioned above will also be analyzed.)

[0100] (Measurement method) GD-OES measurements were performed on the plated surface of the sample up to a depth of 100 μm in the plate thickness direction.

[0101] (Analysis method) The analysis was performed in the same manner as in the measurement of the decarburization state of the surface layer (before hot stamping) described above (measurement of the carbon profile by GD-OES).

[0102] Using the hot stamped samples, the carbon profile was measured by GD-OES under the conditions described above to investigate the decarburization behavior. As an example, the carbon profile of Experiment No. 4, which is a conventional steel as a comparative example, is shown on the left in Figure 6, and the carbon profile of Experiment No. 1, which is an example of the present invention, is shown on the right in Figure 6. Comparing these carbon profiles, as shown in Figure 6 by the vertical double arrows indicating the difference in carbon concentration at the interface between the coating layer and the base steel sheet, it can be seen that in the example of the present invention, the carbon concentration at the interface between the coating layer and the base steel sheet is sufficiently suppressed even after hot stamping. In Table 8, the "-" for the C concentration at the base steel coating interface indicates that it was not measured.

[0103] [Measurement of Fe concentration in plating layer after hot stamping] The Fe concentration in the plating layer after hot stamping was measured in the same manner as the Fe concentration in the plating layer before hot stamping. An example of an analysis area of ​​EDX analysis in measuring the Fe concentration in the plating layer after hot stamping is shown in FIG. 7. As an example of EDX analysis, the analysis result of Experiment No. 4 is shown in FIG. 8. As an example, the calculation result of the Fe concentration (53.4 mass%) in Experiment No. 4 is shown in Table 7. The Fe concentration in the plating layer of each example, calculated in the same manner as in Table 7 below, is shown in Table 8.

[0104] [Table 7]

[0105] [Tensile test] Using the hot stamped samples, a tensile test was carried out under the following conditions to measure the tensile strength (TS, unit: MPa). (Preparation of test specimen) For materials with dimensions of 150mmW x 70mmL x thickness, 150mmW x 220mmL x thickness, or 150mmW x 80mmL (small sample), a test piece sample of 150mmW x 30mmL was taken from the center of the plate. JIS No. 5 test pieces were then made from the 150mmW x 30mmL test piece sample. (Tensile test method) The tensile strength (TS, unit: MPa) of the above JIS No. 5 test piece was measured at a strain rate of 10 mm / min using an AG-IS 250 kN autograph tensile tester manufactured by Shimadzu Corporation in accordance with the method specified in JIS Z 2241.

[0106] [Welding test] The hot stamped sample was cut to prepare multiple samples for welding tests measuring 30 mm × 30 mm × plate thickness, and a welding test was performed under the following conditions and as shown in Figure 9. In Figure 9, the X in "XkA" for the 2nd pulse (second current) indicates 15 current conditions that were changed in 0.5 kA increments between 5.0 kA and 12.0 kA as shown below.

[0107] <Welding conditions> ·Preliminary RBI point: In order to allow the tip to become familiar with the welding before the actual welding, 20 welds were made at 6.5kA on two pieces of mild steel. The other conditions for the pre-weld and the actual welding are as follows: Current application time: 10 cycles Pressure: 1.7kN Hold time: 1 cycle Main welding: Equipment name: Servo pressure spot welding equipment Manufacturer: Nastoa Welding Technology Co., Ltd. Electrode: Upper and lower dome radius type Cu-Cr Electrode diameter: outer diameter Φ16mm, tip diameter: Φ6mm Hitting angle: 0° Cooling water flow rate: Approximately 2 liters / min up and down Pressure: 500kgf Initial pressure time: 60 cycles / 60 Hz Upslope: 1 cycle / 60Hz First energization: energization time 36cycle / 60Hz Current value: 4.5kA Second energization: 18cycle / 60Hz Current values: 5.0kA, 5.5kA, 6.0kA, 6.5kA, 7.0kA, 7.5kA, 8.0kA, 8.5kA, 9.0kA, 9.5kA, 10.0kA, 10.5kA, 11.0kA, 11.5kA, 12.0kA Hold time: 10 cycles / 60 Hz <Board group> Two-piece set: upper and lower plates are the same type of steel plate Test pieces were prepared for the second current application under a total of 15 current conditions, n1 each.

[0108] [Evaluation of LME break] A test piece for evaluating LME cracking was prepared from the sample (welded test piece) after the above welding test as follows. Fig. 10 is a schematic diagram of the top surface of sample 1 after the welding test, in which the upper and lower plates were welded together. The shaded area in Fig. 10 (including part of nugget 3) was taken from sample 1 after the welding test as test piece 2 for evaluating LME cracking. When taking the sample, first, taking into consideration the polishing allowance, the cut was made at cut surface 4 so that the center of nugget 3 (diameter surface of the nugget) could be photographed, and then polishing was performed so that the center of the nugget (diameter surface of the nugget) became observation surface 5.

[0109] Next, the observation surface 5 was subjected to a conventional corrosion treatment so that the HAZ and nugget diameter could be identified. Then, for all samples, cross-sections were photographed at a magnification that covered the HAZ (photographs were taken in the direction of the white arrow in Figure 10). An example of a photograph is shown in Figure 11. This photograph was taken at a magnification of 25x. Since there were 15 current conditions for one experiment, 15 samples for LME crack evaluation were photographed for one experiment.

[0110] Cracks were observed at eight locations, (1) to (8), shown in Figure 11, for each current condition. In other words, a total of 120 cracks were confirmed for 15 current conditions x 8 locations. The total number of locations where cracks with lengths of 300 μm or more were confirmed out of the total of 120 locations was calculated. Note that (1) to (6) in Figure 11 are likely to be observed as cracks extending from the surface in the thickness direction (surface cracks), while (7) and (8) in Figure 11 are likely to be observed as cracks extending generally toward the center of the nugget (internal cracks). Note that void Q shown in Figure 12 is not a crack. Internal crack R extending from void Q shown in Figure 12 is counted.

[0111] These results are shown in Table 8. In the properties shown in Table 8, when the tensile strength TS after hot stamping is 1470 MPa or more and the crack evaluation result after the welding test (the total number of places where LME cracks were confirmed) is 3 or less, it is determined to be an inventive example having high strength and excellent LME resistance. The tensile strength TS can be further 1500 MPa or more, further 1550 MPa or more, and further 1600 MPa or more. On the other hand, a comparative example was determined to be one in which at least one of the strength and the crack evaluation result after the welding test did not satisfy the above evaluation criteria. In this embodiment, the case where the Fe concentration in the plating layer is 65 mass% or less was evaluated to be excellent in corrosion resistance. The measurement results of the Fe concentration in the plating layer are also shown in Table 8.

[0112] [Table 8]

[0113] From the above results, the following can be seen. Experiments Nos. 1 to 3, 8, and 9 satisfy the component composition and manufacturing conditions (reduction annealing conditions) specified in this embodiment, and as a result, the tensile strength (TS) after hot stamping satisfies 1470 MPa or more. Furthermore, the carbon concentration in the surface layer of the steel sheet before hot stamping satisfies formula (1), and excellent LME resistance is shown with three or less LME cracks confirmed after welding. In this embodiment, the LME resistance was evaluated by a welding test after hot stamping, but the LME resistance is also a property required during hot stamping at high temperatures. In other words, the LME resistance is also required for the hot-dip galvanized steel sheet before hot stamping. Since the hot-dip galvanized steel sheets for hot stamping in the above Experiments Nos. 1 to 3, 8, and 9 were hot-stamped well, it can be said that the hot-dip galvanized steel sheets for hot stamping in these examples also have excellent LME resistance.

[0114] On the other hand, Experiments Nos. 4 to 7 and 10 did not satisfy at least one of the component composition and the manufacturing conditions (reduction annealing conditions) specified in this embodiment, and the desired characteristics were not obtained.

[0115] Experiments Nos. 4 and 5 satisfied the component composition defined in this embodiment, and the tensile strength after hot stamping was 1470 MPa or more. However, in these examples, the manufacturing conditions (reduction annealing conditions) were not satisfied, and the dew point during reduction annealing was -20°C or less. As a result, the carbon concentration in the surface layer of the steel sheet before hot stamping did not satisfy formula (1), and therefore the total number of cracks confirmed in the LME resistance evaluation was 4 or more, resulting in poor LME resistance.

[0116] In Experiments No. 6 and No. 7, the C content in the composition was below the range specified in this embodiment, so the strength after hot stamping was TS1470MPa or less. Note that Experiments No. 6 and No. 7 did not satisfy the manufacturing conditions (reduction annealing conditions), and the carbon concentration in the surface layer of the steel sheet before hot stamping did not satisfy formula (1), but the total number of locations where LME cracking was confirmed in the LME resistance evaluation was three or less. The reason for this is that the bulk components, especially carbon, were quite low.

[0117] Experiment No. 10 satisfied the chemical composition specified in this embodiment, and the tensile strength after hot stamping was 1470 MPa or more. However, the manufacturing conditions (reduction annealing conditions) were not satisfied, and the dew point during reduction annealing was -20°C or less. As a result, the carbon concentration in the surface layer of the steel sheet before hot stamping did not satisfy formula (1), and therefore the total number of cracks confirmed in the LME resistance evaluation was 4 or more, resulting in poor LME resistance.

[0118] Table 8 includes some estimated values ​​for Experiments Nos. 6 to 10, which will be explained below. First, the C concentration at the base steel-plating interface after hot stamping in Experiment No. 6 was not measured. However, Experiment No. 6 has the same chemical composition as Experiment No. 7 and the reduction annealing conditions are similar. In addition, the hot stamp heating conditions are also nearly the same, so it is assumed that the C concentration at the base steel-plating interface will be equivalent to that in Experiment No. 7. Therefore, the C concentration at the base steel-plating interface after hot stamping in Experiment No. 6 is listed assuming that it will be nearly the same as that in Experiment No. 7.

[0119] In addition, in experiment No. 6, the tensile strength after hot stamping was not measured. However, experiment No. 6 had the same chemical composition as experiment No. 7, and the reduction annealing conditions were also similar. Furthermore, the hot stamp heating conditions and shot blasting conditions were also almost the same. On the other hand, since the forming start temperature during hot stamping in experiment No. 6 was higher than in experiment No. 7, it is assumed that the cooling rate after hot stamping was faster than in experiment No. 7. Therefore, it is assumed that the martensite structure formed also becomes harder. In addition, it is assumed that the strength will increase by about 80 MPa, and the strength (about 1300 MPa) estimated based on the value of experiment No. 7 is listed.

[0120] Furthermore, in experiment No. 6, the Fe concentration in the coating layer after hot stamping was not measured. However, experiment No. 6 has the same chemical composition as experiment No. 7, and the reduction annealing conditions were also similar, so it is assumed that the decarburized layer formed is the same. Furthermore, the hot stamp heating conditions and shot blasting conditions were also the same. However, the coating weight in experiment No. 6 was less than that in experiment No. 7, and it is assumed that the Fe concentration in the coating layer after hot stamping is approximately 1% higher than that in experiment No. 7. Therefore, it is assumed that the Fe concentration in the coating layer after hot stamping in experiment No. 6 will be approximately 60% of the value in experiment No. 7, and this assumed value is shown.

[0121] In Test No. 7, no LME cracking evaluation was performed. However, Test No. 7 had the same chemical composition as Test No. 6, and the reduction annealing conditions were also similar, so it is assumed that the decarburized layer that was formed was the same. Furthermore, the hot stamp heating conditions and shot blasting conditions were also the same. It is also assumed that there is no significant difference in the Fe concentration in the plating layer after hot stamping. Therefore, LME cracking in Test No. 7 is assumed to be 0, just like in Test No. 6, and this assumed value is listed.

[0122] In Experiment No. 8, the Fe concentration in the coating layer after hot stamping was not measured. However, if the hot stamping conditions are the same, the Fe concentration in the coating layer after hot stamping is largely determined by the coating weight (weight) before hot stamping and the Fe concentration in the coating layer. Here, in Experiment No. 1 (coating weight (weight) 120 g / m 2 , the Fe concentration in the plating layer was 8.8% by mass. The Fe concentration in the plating layer before hot stamping in Experiment No. 8 was equivalent to that in Experiment No. 1, whereas the plating coating weight (weight per unit area) in Experiment No. 8 was greater than that in Experiment No. 1. Therefore, the Fe concentration in the plating layer after hot stamping in Experiment No. 8 is assumed to be lower than the value (44% by mass) measured in Experiment No. 1. Therefore, Table 8 shows an Fe concentration of 44% by mass or less in the plating layer after hot stamping that is assumed for Experiment No. 8.

[0123] In Experiments No. 9 and 10, the Fe concentration in the coating layer after hot stamping was not measured. However, as mentioned above, if the hot stamping conditions are the same, the Fe concentration in the coating layer after hot stamping is largely determined by the coating weight (weight per unit area) before hot stamping and the Fe concentration in the coating layer. Here, Experiment No. 4 was used as a reference. The Fe concentration in the coating layer before hot stamping in Experiments No. 9 and 10 was equivalent to that in Experiment No. 4, while the coating weight (weight per unit area) in Experiments No. 9 and 10 was greater than that in Experiment No. 4. Therefore, the Fe concentration in the coating layer after hot stamping in Experiments No. 9 and 10 is assumed to be lower than the value (53 mass%) measured in Experiment No. 4. Therefore, Table 8 shows 53 mass% or less as the Fe concentration in the coating layer after hot stamping assumed for Experiments No. 9 and 10.

[0124] In addition, in all of Experiments Nos. 1 to 3, 8 and 9, the coating weight was 45 g / m 2 As described above, since the Fe concentration in the plating layer after hot stamping is 65 mass % or less, it is believed that excellent corrosion resistance is exhibited. [Explanation of symbols]

[0125] 1. Sample after welding test (welded test piece) 2. Test piece for evaluating LME cracking 3. Nugget 4 Cut surface 5 Observation surface a Center of steel plate b End of steel plate Q Void R Internal crack

Claims

1. The composition of the base steel sheet is C: 0.15 to 0.50% by mass, Si: 0.02 to 2.5% by mass, Mn: 0.5 to 5% by mass, P: 0.03% by mass or less (including 0% by mass), S: 0.02% by mass or less (including 0% by mass), Al: 0.010 to 1% by mass, Ti: 0.005 to 0.080 mass%; and B: 0.0005 to 0.005 mass%, The balance is Fe and unavoidable impurities. A zinc-based plated steel sheet for hot stamping, in which, when elemental analysis is performed by glow discharge optical emission spectrometry (GD-OES) from the surface of the plating layer in the thickness direction of the plating layer, a carbon concentration [Cf] (mass %) at a position where the concentration of Zn constituting the plating layer is 1.0 mass % and a bulk carbon concentration [Cb] (mass %) satisfy the following formula (1): [Cf]≦0.65×[Cb]...(1)

2. The zinc-based plated steel sheet for hot stamping according to claim 1, wherein a chemical composition of the base steel sheet satisfies at least one of the following (a) and (b): (a) further comprising: Cr: more than 0 mass%, 1.2 mass% or less, Mo: more than 0 mass% and 1 mass% or less, and Ca: Contains one or more elements selected from the group consisting of more than 0 mass % and 0.0040 mass % or less. (b) further comprising: Nb: more than 0 mass%, 0.040 mass% or less, V: more than 0 mass%, 0.30 mass% or less, Cu: more than 0 mass%, 0.30 mass% or less, Ni: more than 0 mass%, 0.30 mass% or less, Mg: more than 0% by mass and 0.010% by mass or less; and REM: Contains one or more elements selected from the group consisting of more than 0 mass % and 0.010 mass % or less.

3. 3. A method for producing a zinc-based plated steel sheet for hot stamping, comprising: an annealing step including allowing a hot-rolled steel sheet or a cold-rolled steel sheet satisfying the component composition according to claim 1 or 2 to remain in a reducing atmosphere having a dew point of −20° C. to +10° C. at 500 to 930° C. for 90 to 1000 seconds; and a subsequent zinc-based plating step.

4. The method for producing a zinc-based plated steel sheet for hot stamping according to claim 3, wherein the zinc-based plating step is a hot-dip galvanizing step.

Citation Information

Patent Citations

  • JP1496-1503A

  • Steel sheet for hot forming having excellent joining strength in spot weld zone and hot formability, and hot formed article

    JP2007169679A

  • Steel sheet for hot stamp

    JP2019173158A

  • Hot stamping alloyed hot-dip galvanized steel sheet, hot stamping molding and method for manufacturing them

    JP2022131411A

Cited By

  • Production method of LME-resistant galvanized steel sheet

    CN122326878A

  • Automotive component and method for manufacturing same

    WO2026221102A1