Solid electrolyte, electrode for solid-state batteries and solid-state battery

A halide-based solid electrolyte with specific aluminum and gallium content improves the initial charge/discharge efficiency and reduces irreversible capacity in solid-state batteries, addressing performance limitations in existing technologies.

JP2024144208APending Publication Date: 2024-10-11TDK CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024037783
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-12
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing solid electrolytes in solid batteries face challenges in achieving high initial charge/discharge efficiency and small irreversible capacity, limiting their performance in portable electronic devices.

Method used

A halide-based solid electrolyte containing fluorine and chlorine with aluminum and gallium as metal elements, formulated as Li1+g M.O. g F h Cl 4-(g+h), where M is Al or Ga, is developed to enhance the efficiency of solid-state batteries.

Benefits of technology

The new electrolyte composition significantly improves initial charge/discharge efficiency and reduces irreversible capacity, enhancing the performance of solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144208000001_ABST
    Figure 2024144208000001_ABST
Patent Text Reader

Abstract

To provide a solid electrolyte that achieves improvement in initial charging / discharging efficiency, an electrode for solid-state batteries including the solid electrolyte, and a solid-state battery including the electrode for solid-state batteries.SOLUTION: The solid-state battery is represented by the formula (1): Li1+gMOgFhCl4-(g+h). In the formula (1), M denotes one or both of Al and Ga, and the following relationships hold: 0≤g<4, 0<h<4, 0<4-(g+h)<4.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a solid electrolyte, an electrode for a solid battery, and a solid battery.

Background Art

[0002] In recent years, the development of electronics technology has been remarkable, and the miniaturization, light weight, and thinness, as well as multifunctionalization, of portable electronic devices have been achieved. Along with this, for the battery that serves as the power source of the electronic device, miniaturization, light weight, and improvement in reliability are strongly desired, and solid batteries using solid electrolytes as electrolytes have attracted attention. As solid electrolytes, those with various compositions are known.

[0003] For example, Patent Document 1 discloses a halide-based solid electrolyte represented by the general formula A 2+a E 1-b+α G b X d (wherein A is any one of Li, K, and Na; E is one or more selected from the group consisting of Zr, Hf, Ti, and Sn; G is one or more selected from the group consisting of Mg, Ca, Sr, Cs, Ba, Y, Al, Sc, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Cu, Ag, Au, Pb, Bi, In, Sn, Sb, Nb, Ta, and W; X is one or more selected from the group consisting of F, Cl, Br, and I; a is -2b when G is a hexavalent element, -b when G is a pentavalent element, 0 when G is a tetravalent element or G is not included, b when G is a trivalent element, 2b when G is a divalent element, and 3b when G is a monovalent element. 0 ≦ b ≦ 0.5, -0.3 ≦ α ≦ 0.3, 5.0 < d < 6.0).

[0004] Patent Document 2 discloses a solid electrolyte represented by the general formula A 2+a E 1-b+α G b D c X d(In the formula, A is an element selected from the group consisting of Li, K, and Na. E is at least one tetravalent element selected from the group consisting of Zr, Hf, Ti, and Sn. G is at least one element selected from the group consisting of B, Si, Mg, Ca, Sr, Cs, Ba, Y, Al, Sc, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Cu, Au, Pb, Bi, In, Sn, Sb, Nb, Ta, and W. D is at least one element selected from the group consisting of O, Se, and Te. X is at least one selected from the group consisting of F, Cl, Br, and I. a is -2b when G is a hexavalent element, -b when G is a pentavalent element, 0 when G is a tetravalent element or when G is not included, b when G is a trivalent element, 2b when G is a divalent element, and 3b when G is a monovalent element. b is 0 to 0.5. α is -0.3 to 0.3. c is 0.01 to 3. d is 0.1 to 6.1).

[0005] In addition, Patent Document 3 discloses a compound of the general formula A a E b G c X d (In the formula, A is at least one element selected from the group consisting of Li, Cs, and Ca. E is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanides. G is OH, BO2, BO3, BO4, B3O6, B4O7, CO3, NO3, AlO2, SiO3, SiO4, Si2O7, Si3O9, Si4O 11 , SiO 18 , PO3, PO4, P2O7, P3O 10、SO3, SO4, SO5, S2O3, S2O4, S2O5, S2O6, S2O7, S2O8, BF4, PF6, BOB, (COO)2, N, AlCl4, CF3SO3, CH3COO, CF3COO, OOC-(CH2)2-COO, OOC-CH2-COO, OOC-CH(OH)-CH(OH)-COO, OOC-CH(OH)-CH2-COO, C6H5SO3, OOC-CH=CH-COO, OOC-CH=CH-COO, C(OH)(CH2COOH)2COO, AsO4, BiO4, CrO4, MnO4, PtF6, PtCl6, PtBr6, PtI6, SbO4, SeO4, TeO4, HCOO, CH3COO, and is at least one group selected from the group consisting of. X is at least one element selected from the group consisting of F, Cl, Br, and I. 0.5 ≦ a < 6, 0 < b < 2, 0.1 < c ≦ 6, 0 ≦ d ≦ 6.1. BOB is bisoxalate borate, OOC-(CH2)2-COO is succinate, OOC-CH2-COO is malonate, OOC-CH(OH)-CH(OH)-COO is tartrate, OOC-CH(OH)-CH2-COO is malate, C6H5SO3 is benzenesulfonate, OOC-CH=CH-COO is fumarate, OOC-CH=CH-COO is maleate, and C(OH)(CH2COOH)2COO is citrate. A solid electrolyte represented by ) is disclosed.

[0006] Patent Document 4 discloses a solid electrolyte represented by the general formula Li a Al b O c X d (wherein the values of a, b, c, and d are all greater than 0, and X is at least one selected from the group consisting of Cl and Br).

[0007] Patent Document 5 discloses a solid electrolyte represented by the general formula Li 1-a Al a X 1+2a (wherein 0 < a < 1 (excluding a = 0.5) is satisfied, and X is at least one selected from the group consisting of Cl, Br, and I).

[0008] Non-Patent Document 1 states that 2LiCl-xAlF 3- A solid electrolyte represented by (1-x)GaF3 (0.5≦x≦0.9) is disclosed. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. 2021 / 024783 [Patent Document 2] International Publication No. 2021 / 024785 [Patent Document 3] International Publication No. 2021 / 261558 [Patent Document 4] International Publication No. 2021 / 199676 [Patent Document 5] International Publication No. 2022 / 137758 [Non-patent literature]

[0010] [Non-Patent Document 1] Advanced.Science, 2022, 9, 2204633 Summary of the Invention [Problem to be solved by the invention]

[0011] Solid electrolytes are important materials that greatly affect the characteristics of solid-state batteries, and various types of solid electrolytes are required in addition to the solid electrolytes disclosed in Patent Documents 1 to 5 and Non-Patent Document 1. In addition, it is considered that a high-capacity solid-state battery is desirable, and there is a demand for solid-state batteries with small irreversible capacity and high initial charge / discharge efficiency.

[0012] The present invention has been made in consideration of the above circumstances, and has an object to provide a solid electrolyte capable of increasing initial charge / discharge efficiency, a solid-state battery electrode containing the solid-state electrolyte, and a solid-state battery including the solid-state battery electrode. [Means for solving the problem]

[0013] In order to solve the above problems, the present inventors have conducted intensive studies. As a result, in a halide-based solid electrolyte containing fluorine and chlorine, by including one or both of aluminum and gallium as metal elements so as to have a predetermined composition ratio, it has been found that the initial charge-discharge efficiency can be increased when used in a solid battery.

[0014] That is, the present invention provides the following means in order to solve the above problems.

[0015] [1] The solid electrolyte according to one aspect of the present invention is represented by the composition formula (1), Li 1+g MO g F h Cl 4-(g+h) ···(1) In formula (1), M is one or both of Al and Ga, and satisfies 0≦g<4, 0<h<4, and 0<4-(g+h)<4.

[0016] [2] The electrode for a solid battery according to one aspect of the present invention contains the solid electrolyte of [1] above.

[0017] [3] The solid battery according to one aspect of the present invention includes the electrode for a solid battery of [2] above.

Effects of the Invention

[0018] According to the present invention, it is possible to provide a solid electrolyte capable of increasing the initial charge-discharge efficiency, an electrode for a solid battery containing the solid electrolyte, and a solid battery including the electrode for a solid battery.

Brief Description of the Drawings

[0019] [Figure 1] It is a cross-sectional view schematically showing a solid battery according to one aspect of the present invention. [Diagram 2] It is a graph of the initial charge-discharge curve of Example 1. [Diagram 3] It is a graph of the initial charge-discharge curves of Example 2 and Comparative Example 1. [Figure 4] 1 is a graph showing initial charge / discharge curves of Example 2 and Comparative Example 2. [Diagram 5] 1 is a graph showing initial charge / discharge curves of Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The present embodiment will be described in detail below with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto, and may be appropriately modified and implemented within the scope of the present invention.

[0021] "Solid electrolyte" A solid electrolyte is a solid substance that can move ions when an external electric field is applied.

[0022] The solid electrolyte according to this embodiment has the general formula Li 1+g MO g F h Cl 4-(g+h) The solid electrolyte is a halide-based solid electrolyte represented by the formula (1). The solid electrolyte may contain a substance originating from the raw material powder in addition to the compound represented by the formula (1).

[0023] The solid electrolyte may be in the form of a powder (particles) or in the form of a sintered body obtained by sintering the powder. The solid electrolyte may be a compact obtained by compressing and molding the powder, a compact obtained by molding a mixture of the powder and a binder, or a coating formed by applying a coating material containing the powder, a binder, and a solvent, and then removing the solvent by heating. The main structure of the solid electrolyte may be amorphous or crystalline.

[0024] In formula (1), Li is a lithium ion. g satisfies 1 ≦ 1 + g < 5, and may be 1 ≦ 1 + g < 3, may be 1 ≦ 1 + g ≦ 2, or may be 1 ≦ 1 + g ≦ 1.5.

[0025] In formula (1), M is one or both of Al and Ga. That is, M is Al a Ga b represented by 0 ≦ a ≦ 1, 0 ≦ b ≦ 1, and a + b = 1. It may be 0.5 ≦ a ≦ 1, 0 ≦ b ≦ 0.5, may be 0.7 ≦ a ≦ 1, 0 ≦ b ≦ 0.3, or may be 0.9 ≦ a ≦ 1, 0 ≦ b ≦ 0.1.

[0026] In formula (1), O is oxygen. g satisfies 0 ≦ g < 4. g may be 0 ≦ g < 2, may be 0 ≦ g ≦ 1, or may be 0 ≦ g ≦ 0.5.

[0027] In formula (1), F is fluorine. h satisfies 0 < h < 4. h may be 2.5 < h ≦ 3.9, may be 3.0 ≦ h ≦ 3.9, or may be 3.2 ≦ h ≦ 3.9. Also, h ≦ 3.5 may be satisfied.

[0028] Also, in the above formula (1), g and h satisfy 0 < 4 - (g + h) < 4. g and h may be 0 < 4 - (g + h) < 1.5, or may be 0 < 4 - (g + h) < 1.

[0029] Such a solid electrolyte is, for example, Li6AlF 0.1 Cl 3.9 Li 1.5 AlO 0.5 F 0.25 Cl 3.25 Li 1.5 AlO 0.5 F 0.5 Cl3, Li6GaF 0.1 Cl 3.9 Li 1.5 GaO 0.5 F 0.25 Cl 3.25 Li 1.5 GaO 0.5 F 0.5It is Cl3.

[0030] "Solid battery" FIG. 1 is a cross-sectional view that typically illustrates a cross section of a solid-state battery according to this embodiment. The solid-state battery 100 illustrated in FIG. 1 includes a power generating element 40 and an exterior body 50. The exterior body 50 covers the periphery of the power generating element 40. The power generating element 40 is connected to the outside via a pair of terminals 60, 62 that are connected together. Although a laminated type battery is illustrated in FIG. 1, a wound type battery may also be used. The solid-state battery 100 is used, for example, in laminated batteries, square batteries, cylindrical batteries, coin batteries, button batteries, and the like.

[0031] <Power generation element> The power generating element 40 includes a solid electrolyte layer 10, a positive electrode 20, and a negative electrode 30. The power generating element 40 is charged or discharged by the exchange of ions between the positive electrode 20 and the negative electrode 30 via the solid electrolyte layer 10 and the exchange of electrons via an external circuit. In the power generating element 40, one or both of the positive electrode 20 and the negative electrode 30 contain the solid electrolyte represented by the above formula (1).

[0032] The solid electrolyte layer 10 is, for example, a halide-based solid electrolyte or a sulfide-based solid electrolyte. The solid electrolyte layer 10 includes, for example, the solid electrolyte represented by the above formula (1), and may include other halide-based solid electrolytes or sulfide-based solid electrolytes as follows.

[0033] As the halide-based solid electrolyte, in addition to the solid electrolyte represented by the above formula (1), for example, a E b G c X d ...(2) can be used.

[0034] A contains at least Li. A may contain at least one of Na or Ca in addition to Li. When A contains Na or Ca, the molar ratio of Li to Na or Ca (Li:Na or Ca) is preferably 1.00:0.03 to 1.00:0.20. a satisfies 0.5≦a<6. E is an essential component and is at least one element selected from the group consisting of Al, Sc, Y, Zr, Hf, and lanthanoids (La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu). b satisfies 0 < b < 2.

[0035] G is, for example, at least one group selected from the group consisting of OH, BO2, BO3, BO4, B3O6, B4O7, CO3, NO3, AlO2, SiO3, SiO4, Si2O7, Si3O9, Si4O 11 、Si6O 18 、PO3, PO4, P2O7, P3O 10 、SO3, SO4, SO5, S2O3, S2O4, S2O5, S2O6, S2O7, S2O8, BF4, PF6, BOB, (COO)2, N, AlCl4, CF3SO3, CH3COO, CF3COO, OOC-(CH2)2-COO, OOC-CH2-COO, OOC-CH(OH)-CH(OH)-COO, OOC-CH(OH)-CH2-COO, C6H5SO3, OOC-CH=CH-COO, OOC-CH=CH-COO, C(OH)(CH2COOH)2COO, AsO4, BiO4, CrO4, MnO4, PtF6, PtCl6, PtBr6, PtI6, SbO4, SeO4, TeO4, HCOO. c satisfies 0.1 < c ≤ 6. X is at least one selected from the group consisting of F, Cl, Br, and I. d satisfies 0 < d ≤ 6.1.

[0036] As the sulfide-based solid electrolyte, for example, a compound containing Li, S, and Si and / or P can be used. The sulfide-based solid electrolyte may further contain Ge, Cl, Br, and I. The sulfide-based solid electrolyte may be amorphous, crystalline, or argyrodite-type. Examples of the sulfide-based solid electrolyte include Li2S-P2S5-based solid electrolytes (Li7P3S 11 、Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2-based solid electrolytes (Li 13GeP3S 16 , Li 10 GeP2S 12 ), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x P.S. 6-x Cl x (x is 1.0 to 1.9).

[0037] (positive electrode) 1, the positive electrode 20 has a plate-shaped (foil-shaped) positive electrode current collector 22 and a positive electrode mixture layer 24. The positive electrode mixture layer 24 is in contact with at least one surface of the positive electrode current collector 22.

[0038] The positive electrode current collector 22 may be made of any electronically conductive material that is resistant to oxidation during charging and is not easily corroded. The positive electrode current collector 22 may be made of, for example, a metal such as aluminum, stainless steel, nickel, or titanium, or a conductive resin. The positive electrode current collector 22 may be in the form of a powder, a foil, a punched piece, or an expanded piece.

[0039] The positive electrode mixture layer 24 contains a positive electrode active material, and, if necessary, a solid electrolyte, a binder, and a conductive assistant.

[0040] The positive electrode active material is not particularly limited as long as it can reversibly absorb and release, and insert and remove (intercalate and deintercalate) lithium ions, and any positive electrode active material used in known solid-state batteries can be used. Examples of the positive electrode active material include lithium-containing metal oxides and lithium-containing metal phosphates.

[0041] Lithium-containing metal oxides include, for example, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese spinel (LiMn2O4), and lithium manganese oxides represented by the general formula: LiNi x Co y Mn zO2 (x+y+z=1), lithium vanadium compounds (LiVOPO4, Li3V2(PO4)3), olivine-type LiMPO4 (where M represents at least one selected from Co, Ni, Mn, and Fe), lithium titanate (Li4Ti5O 12 ) etc.

[0042] The positive electrode active material may not contain lithium. Examples of such positive electrode active materials include non-lithium-containing metal oxides (MnO2, V2O5, etc.), non-lithium-containing metal sulfides (MoS2, etc.), and non-lithium-containing fluorides (FeF3, VF3, etc.). When using a positive electrode active material that does not contain lithium, the negative electrode is doped with lithium ions in advance, or a negative electrode containing lithium ions is used.

[0043] The solid electrolyte contained in the positive electrode 20 is, for example, a solid electrolyte represented by the above formula (1). The solid electrolyte contained in the positive electrode 20 may be a halide-based solid electrolyte other than the solid electrolyte represented by the above formula (1), or a sulfide-based solid electrolyte. The solid electrolyte contained in the positive electrode 20 may be the same as or different from the solid electrolyte contained in the solid electrolyte layer 10 or the negative electrode 30.

[0044] The content of the solid electrolyte in the positive electrode mixture layer 24 is not particularly limited, but is preferably 1 mass % to 50 mass %, and more preferably 5 mass % to 30 mass %, based on the total mass of the positive electrode active material, the solid electrolyte, the conductive assistant, and the binder.

[0045] The binder bonds the positive electrode active material, the solid electrolyte, and the conductive assistant to one another in the positive electrode mixture layer 24, and also firmly bonds the positive electrode mixture layer 24 to the positive electrode current collector 22. The positive electrode mixture layer 24 preferably contains a binder. The binder preferably has oxidation resistance and good adhesiveness.

[0046] Examples of the binder used in the positive electrode mixture layer 24 include polyvinylidene fluoride (PVDF) or its copolymer, polytetrafluoroethylene (PTFE), polyamide (PA), polyimide (PI), polyamideimide (PAI), polybenzimidazole (PBI), polyethersulfone (PES), polyacrylic acid (PA) and its copolymer, metal ion crosslinked polyacrylic acid (PA) and its copolymer, polypropylene (PP) grafted with maleic anhydride, polyethylene (PE) grafted with maleic anhydride, and mixtures thereof. Among these, it is particularly preferable to use PVDF as the binder.

[0047] The content of the binder in the positive electrode mixture layer 24 is not particularly limited, but is preferably 1% by mass to 15% by mass, and more preferably 3% by mass to 5% by mass, based on the total mass of the positive electrode active material, solid electrolyte, conductive assistant, and binder. If the amount of binder is too small, it tends not to be possible to form a positive electrode 20 with sufficient adhesive strength. Conversely, if the amount of binder is too large, it tends to be difficult to obtain sufficient volume or mass energy density, since general binders are electrochemically inactive and do not contribute to discharge capacity.

[0048] The conductive assistant improves the electronic conductivity of the positive electrode mixture layer 24. Known conductive assistants can be used. Examples of the conductive assistant include carbon materials such as carbon black, graphite, carbon nanotubes, and graphene, metals such as aluminum, copper, nickel, stainless steel, iron, and amorphous metals, conductive oxides such as ITO, and mixtures thereof. The conductive assistant may be in the form of powder or fiber.

[0049] There is no particular limitation on the content of the conductive assistant in the positive electrode mixture layer 24. When the conductive assistant is added, the mass ratio of the conductive assistant is preferably 0.5 mass % to 20 mass %, and more preferably 1 mass % to 5 mass %, based on the total mass of the positive electrode active material, solid electrolyte, conductive assistant, and binder.

[0050] (Negative electrode) 1, the negative electrode 30 has a negative electrode current collector 32 and a negative electrode mixture layer 34. The negative electrode mixture layer 34 is in contact with the negative electrode current collector 32.

[0051] The negative electrode current collector 32 may have electronic conductivity. The negative electrode current collector 32 is made of, for example, a metal such as copper, aluminum, nickel, stainless steel, or iron, or a conductive resin. The negative electrode current collector 32 may be in the form of a powder, a foil, a punching, or an expandable material.

[0052] The negative electrode mixture layer 34 contains a negative electrode active material, and, if necessary, a solid electrolyte, a binder, and a conductive assistant.

[0053] The negative electrode active material is not particularly limited as long as it can reversibly absorb and release lithium ions and insert and extract lithium ions. The negative electrode active material may be any negative electrode active material used in known solid-state batteries.

[0054] Examples of the negative electrode active material include carbon materials such as natural graphite, artificial graphite, mesocarbon microbeads, mesocarbon fiber (MCF), cokes, glassy carbon, and organic compound sintered bodies, Si, SiO x Metals that can combine with lithium, such as Sn and aluminum, their alloys, composites of these metals and carbon materials, lithium titanate (Li4Ti5O 12 ), oxides such as SnO2, metallic lithium, etc. The negative electrode active material is preferably natural graphite.

[0055] The solid electrolyte contained in the negative electrode 30 is, for example, a solid electrolyte represented by the above formula (1). The solid electrolyte contained in the negative electrode 30 may be a halide-based solid electrolyte other than the solid electrolyte represented by the above formula (1), or a sulfide-based solid electrolyte. The solid electrolyte contained in the negative electrode 30 may be the same as or different from the solid electrolyte contained in the solid electrolyte layer 10 or the positive electrode 20.

[0056] The binder and conductive assistant contained in the negative electrode 30 are the same as the binder and conductive assistant contained in the positive electrode 20 .

[0057] In this embodiment, the positive electrode 20 and the negative electrode 30 are collectively referred to as electrodes for a solid battery. In this embodiment, it is preferable that both the positive electrode 20 and the negative electrode 30 contain the solid electrolyte represented by the above formula (1).

[0058] <Exterior body> The exterior body 50 houses the power generating element 40 therein. The exterior body 50 prevents moisture and the like from entering from the outside to the inside. For example, as shown in Fig. 1, the exterior body 50 has a metal foil 52 and a resin layer 54 laminated on each side of the metal foil 52. The exterior body 50 is a metal laminate film in which the metal foil 52 is coated with the resin layer 54 from both sides.

[0059] The metal foil 52 is, for example, an aluminum foil or a stainless steel foil. The resin layer 54 can be, for example, a resin film such as polypropylene. The materials constituting the resin layer 54 may be different between the inside and outside. For example, the outside material can be a polymer with a high melting point, such as polyethylene terephthalate (PET) or polyamide (PA), and the inside material can be polyethylene (PE) or polypropylene (PP).

[0060] <Terminal> The terminals 60 and 62 are connected to the positive electrode 20 and the negative electrode 30, respectively. The terminal 60 connected to the positive electrode 20 is a positive electrode terminal, and the terminal 62 connected to the negative electrode 30 is a negative electrode terminal. The terminals 60 and 62 are responsible for electrical connection to the outside. The terminals 60 and 62 are made of a conductive material such as aluminum, nickel, or copper. The connection method may be welding or screwing. The terminals 60 and 62 are preferably protected with insulating tape to prevent short circuits.

[0061] [Solid-state battery manufacturing method] Next, a method for manufacturing a solid-state battery according to this embodiment will be described. First, the solid electrolyte of the present invention represented by the above formula (1) is prepared. When forming a powdered solid electrolyte, for example, an Al-containing raw material powder or a Ga-containing raw material powder, which is a raw material powder, and a Li-containing raw material powder are mixed in a predetermined molar ratio and reacted. These powders are collectively called raw material powders. As the Al-containing raw material powder, one or more of AlCl3, AlF3, AlClF2, and AlCl2F can be used. As the GGa-containing raw material powder, one or both of GaCl3 and GaF3 can be used. As the Li-containing raw material powder, one or more of LiCl, LiF, and Li2O can be used.

[0062] Since the raw powder is easily hydrolyzed by moisture, the raw powder is handled in a dry atmosphere with low moisture content. The dry atmosphere can be obtained in an argon glove box or the like. The reaction can be appropriately selected from mechanochemical method, calcination method, solution method, etc. An example of the specific procedure for the mechanochemical method is described below. In a glove box with an argon gas atmosphere (dew point -70°C or less), the raw powder and a reaction vessel are prepared. The reaction vessel is made of a hard material such as zirconia. The reaction vessel contains zirconia balls (e.g., 5 mmφ) to promote the mechanochemical reaction. Before placing the reaction vessel in the glove box, dry it with an external dryer or a drying box attached to the glove box. The raw powder is also dried in the same way as necessary. The raw powder is weighed and put into the reaction vessel. The reaction vessel is covered with a zirconia lid and screwed, and the boundary between the reaction vessel and the lid is sealed with polyimide tape. The polyimide tape has the effect of blocking moisture. This reaction vessel is set in a planetary ball mill. The planetary ball mill is a device that rotates and revolves the reaction vessel to generate a mechanochemical reaction. The planetary ball mill may be installed in a dry atmosphere (dry room, glove box), but may also be installed in a normal atmosphere because the reaction vessel is highly sealed. The mechanochemical reaction may generate mechanical energy or heat due to the reaction. When utilizing such a mechanochemical reaction that generates heat, it is preferable to use a planetary ball mill equipped with a cooling device to prevent the temperature of the raw material powder from increasing due to heat. In addition, a planetary ball mill equipped with a heating device may be used to promote the mechanochemical reaction. The conditions of the mechanochemical reaction, i.e., the rotation speed, reaction time, and cooling / heating, may be appropriately selected. The rotation speed of the rotation and revolution is, for example, 100 to 1000 rpm, and may be 200 to 500 rpm, and the reaction time is 3 to 400 hours. The reaction time of the mechanochemical reaction may be 4 to 200 hours, or 5 to 100 hours. As described above, the solid electrolyte can be produced by a method of subjecting a mixed powder, which is mixed at a predetermined molar ratio, to a mechanochemical reaction.

[0063] The halide raw material contained in the raw material powder is likely to evaporate when the temperature is raised. For this reason, in the case of the firing method, halogen gas may be made to coexist in the atmosphere during firing to supplement the halogen. In addition, when the raw material powder contains a halide raw material, it may be manufactured by a hot pressing method using a mold with high sealing properties. In this case, since the mold has high sealing properties, evaporation of the halide raw material due to heat can be suppressed. By firing in this manner, a solid electrolyte in the form of a sintered body made of a compound having a predetermined composition is obtained.

[0064] When the solid electrolyte is obtained as a sintered body, the mixed raw material powder is molded into a predetermined shape and sintered in a vacuum or in an inert gas atmosphere.

[0065] Next, the positive electrode 20 is prepared. The positive electrode is manufactured by applying a paste containing a positive electrode active material onto a positive electrode current collector 22 and drying it to form a positive electrode mixture layer 24. A solid electrolyte may be added to the paste containing the positive electrode active material. For example, the solid electrolyte represented by the above formula (1) may be added.

[0066] Next, the negative electrode 30 is prepared. The negative electrode is manufactured by applying a paste containing a negative electrode active material onto a negative electrode current collector 32 and drying it to form a negative electrode mixture layer 34. The solid electrolyte represented by the above formula (1) may be added to the paste containing the negative electrode active material.

[0067] The power generating element 40 can be produced, for example, by powder molding. A guide with a hole is placed on the positive electrode 20, and the guide is filled with a solid electrolyte. The surface of the solid electrolyte is then smoothed, and the negative electrode 30 is placed on top of the solid electrolyte. This sandwiches the solid electrolyte between the positive electrode 20 and the negative electrode 30. Pressure is then applied to the positive electrode 20 and the negative electrode 30 to pressure mold the solid electrolyte. By pressure molding, a laminate is obtained in which the positive electrode 20, the solid electrolyte layer 10, and the negative electrode 30 are stacked in this order.

[0068] Next, external terminals are welded to the positive electrode current collector 22 of the positive electrode 20 and the negative electrode current collector 32 of the negative electrode 30, which form the laminate, by a known method, to electrically connect the positive electrode current collector 22 or the negative electrode current collector 32 to the external terminal. Thereafter, the laminate connected to the external terminal is housed in an exterior body 50, and the opening of the exterior body 50 is heat-sealed to seal it. Through the above steps, the solid-state battery 100 of this embodiment is obtained.

[0069] The solid-state battery 100 according to this embodiment contains the solid electrolyte represented by the above formula (1) in one or both of the positive electrode 20 and the negative electrode 30, and therefore has a small irreversible capacity and exhibits high initial charge / discharge efficiency.

[0070] The above describes the embodiments of the present invention in detail with reference to the drawings. However, each configuration and combination thereof in each embodiment is merely an example, and addition, omission, substitution, and other modifications of the configuration are possible without departing from the spirit of the present invention. EXAMPLES

[0071] EXAMPLES Examples of the present invention will be described below, but the present invention is not limited to the following examples.

[0072] [Example 1] (Preparation of solid electrolyte for electrode mixture layer) In a glove box with a dew point of approximately -70 to -85°C, the raw material powders were weighed out so that LiCl, LiF, and AlCl3 were in a molar ratio of 0.9:0.1:1. First, LiCl, LiF, and AlCl3 were charged into a zirconia reaction vessel for a planetary ball mill, which had already contained zirconia balls. Next, a zirconia lid was placed on the reaction vessel, the lid was screwed onto the vessel body, and the gap between the lid and the vessel was sealed with polyimide tape. The polyimide tape has the effect of blocking moisture. Next, the zirconia reaction vessel was set in the planetary ball mill. The rotation speed was set to 500 rpm, the revolution speed was set to 500 rpm, and the rotation direction and the revolution direction were reversed to each other, and a mechanochemical reaction was carried out for 24 hours to produce a solid electrolyte (LiAlF 0.1 Cl 3.9Mechanochemical Milling is abbreviated as MM, and the time for the mechanochemical reaction is called the MM time.

[0073] The planetary ball mill is installed in a normal atmosphere (air). The zirconia sealed container for the planetary ball mill is screwed and sealed with polyimide tape, and when the zirconia sealed container is set in the planetary ball mill, the zirconia sealed container is firmly pressed and fixed in place. Therefore, even in a normal atmosphere, it is believed that there is almost no moisture from the air entering the zirconia sealed container.

[0074] (Preparation of negative electrode mixture layer) The negative electrode mixture was also prepared in a glove box with a dew point of approximately -70 to -85°C. Lithium titanate (Li4Ti5O 12 In addition, vapor grown carbon fiber (VGCF (registered trademark)) was used as a conductive additive. The negative electrode active material, solid electrolyte, and conductive additive were mixed in a mass ratio of 55:40:5 (=Li4Ti5O 12 :Li6AlF 0.1 Cl 3.9 The mixture was mixed for 30 minutes using an agate pestle and mortar to obtain a negative electrode mixture.

[0075] (Preparation of half-cell) The half-cell was also fabricated in a glove box with a dew point of approximately -70 to -85°C. The negative electrode mixture and solid electrolyte of the half-cell were formed into pellets. The pellets were formed using a die and a punch. The die was made of PEEK (polyether ether ketone) and had an outer diameter of 30 mm and an inner diameter of 10 mm. The punches were made of die steel (SKD11 material), with upper and lower punches having an outer diameter of 9.99 mm. Screw holes were provided on the sides of the upper and lower punches, and screws were inserted into these screw holes to form connection terminals.

[0076] A lower punch was inserted into the die, and 80 mg of Li6PS5Cl was placed on top of the lower punch as a solid electrolyte. The die was then vibrated to smooth the surface of the solid electrolyte, after which an upper punch was inserted on top of the solid electrolyte and pressed with a press at a gauge pressure of about 4 KN.

[0077] Next, the upper punch was removed, and 10 mg of the negative electrode mixture was placed on the solid electrolyte. Next, the die was vibrated to level the surface of the negative electrode mixture, and then the upper punch was inserted on the negative electrode mixture and pressed with a gauge pressure of 30 KN using a press. Next, the die was turned upside down, the lower punch was removed, and a Li foil with a diameter of 10 mm was placed on the solid electrolyte, and the lower punch was inserted. In this way, a negative electrode half cell was produced in which a negative electrode mixture layer, a solid electrolyte layer, and a Li foil were laminated in this order. Here, Li is the most base metal (having the lowest potential) among metals. Therefore, in the above negative electrode half cell, the potential is negative electrode mixture layer>Li. An electrode with a high potential is usually called a positive electrode, and an electrode with a low potential is usually called a negative electrode. Therefore, in the above half cell, the negative electrode mixture layer is the positive electrode, and Li is the negative electrode. In this embodiment, to avoid confusion, in the following paragraphs, the negative electrode mixture layer is called the working electrode, and Li is called the counter electrode.

[0078] Next, two stainless steel plates with a diameter of 50 mm and a thickness of 5 mm and two Bakelite plates with a diameter of 50 mm and a thickness of 2 mm were prepared. Then, four holes for passing screws were made in each of the two stainless steel plates and the two Bakelite plates. The screw holes were made at positions where the two stainless steel plates and the two Bakelite plates overlap in a plan view when the negative electrode half-cell, the two stainless steel plates, and the two Bakelite plates are stacked, but where they do not overlap with the negative electrode half-cell in a plan view.

[0079] Then, a stainless steel plate, a Bakelite plate, a negative electrode half cell, a Bakelite plate, and a stainless steel plate were stacked in this order, and screws were inserted into the screw holes and tightened with a torque of 1 N m. In addition, screws were inserted into the screw holes on the sides of the upper and lower punches to serve as the working and counter electrode terminals, respectively. By carrying out the above steps, the negative electrode half cell of Example 1 was produced, in which the upper and lower punches were insulated by the Bakelite plate.

[0080] Furthermore, to prevent hydrolysis of the negative electrode mixture, solid electrolyte, and lithium in a normal atmosphere (air), the negative electrode half-cell was inserted into an exterior body. The exterior body was composed of an exterior bag made of a film consisting of polyamide (PA) / aluminum (Al) / polypropylene (PP), and by inserting the negative electrode half-cell into this exterior bag and sealing it, it is possible to prevent the influence of moisture even in a normal atmosphere (air).

[0081] Here, the means for forming the exterior bag will be described. First, a laminate film was prepared in which PA, Al, and PP were laminated in this order. The thicknesses of PA, Al, and PP in this laminate film were 25 μm, 40 μm, and 40 μm, respectively.

[0082] In addition, a nickel terminal was prepared as an external terminal and an internal terminal. The nickel terminal was 4 mm wide, 50 mm long, and 80 μm thick, and a 10 mm wide, 80 μm thick acid-modified PP film was pre-heat-sealed around the entire circumference of the nickel terminal at the center in the longitudinal direction. The acid-modified PP was obtained by grafting maleic anhydride or the like onto PP. This acid-modified PP was provided because the PP of the laminate film does not have adhesive properties to metals such as nickel. Specifically, in a process described later, in order to improve the adhesion between the PP of the laminate film and the nickel terminal, an acid-modified PP that has adhesive properties to both is interposed between the PP of the laminate film and the nickel terminal.

[0083] This laminate film was cut to a width of 200 mm and a length of 400 mm, and the laminate film was folded at the center in the length direction so that the PA was on the outside and the PP was on the inside. On one side of the folded laminate film, two of the nickel terminals were placed between the folded laminate film at a distance of 50 mm, and were used as the working electrode terminal and the counter electrode terminal, respectively. In addition, one of the two sides of the folded laminate film, excluding the folded side and the side having the terminal, was heat-sealed to leave one side open. Of these working electrode and counter electrode terminals, there are parts that extend outward from the exterior bag (exterior body) and parts that extend into the interior of the exterior body. Here, of the working electrode terminal and counter electrode terminal, the parts that extend outward from the exterior body are referred to as external terminal parts, and the parts that extend into the interior of the exterior body are referred to as internal terminal parts.

[0084] The negative half-cell was inserted into the outer bag. The internal terminal of the working electrode of the outer bag was connected to the working electrode terminal of the negative half-cell, and the internal terminal of the counter electrode of the outer bag was connected to the counter electrode terminal of the negative half-cell with lead wires. One open side was then heat-sealed to complete a negative half-cell that could be handled in a normal atmosphere.

[0085] (Measurement of ionic conductivity of solid electrolyte for electrode mixture layer) Next, the ionic conductivity of the solid electrolyte for the electrode mixture layer was measured. First, in a glove box with argon gas circulating at a dew point of about -70 to -85°C, the obtained solid electrolyte powder was filled into a die and pressed with a gauge pressure of about 30 KN to prepare a measurement cell for the ionic conductivity.

[0086] The die is made of PEEK (polyether ether ketone) and has an outer diameter of 30 mm and an inner diameter of 10 mm. The punches are made of die steel (SKD11 material), and are the upper punch and the lower punch with an outer diameter of 9.99 mm.

[0087] After that, a stainless steel disk and a Bakelite disk, both 50 mm in diameter and 5 mm thick with four screw holes, were prepared and the pressure molding die was set up as follows. The plates were loaded in the following order: stainless steel disk / Bakelite disk / pressure molded die / Bakelite disk / stainless steel disk, and the four screws were tightened with a torque of approximately 3 N m. Screws were also inserted into the screw holes on the sides of the upper and lower punches to serve as connection terminals.

[0088] As in the case of the negative electrode half-cell, the ion conductivity measurement cell was inserted into an exterior body and measured in a normal atmosphere (air).

[0089] The external connection terminal was connected to a potentiostat (VersaSTAT3 manufactured by Princeton Applied Research) equipped with a frequency response analyzer, and the ionic conductivity was measured using the impedance measurement method. Measurements were performed at a measurement frequency range of 1 MHz to 0.1 Hz, an amplitude of 10 mV, and a temperature of 25°C.

[0090] [Example 2] The solid electrolyte used to prepare the negative electrode mixture layer is Li 1.5 AlO 0.5 F 0.25 Cl 3.25 A negative electrode half-cell was prepared in the same manner as in Example 1, except that the Li 1.5 AlO 0.5 F 0.25 Cl 3.25 In the example, the raw material powders were weighed out so that the molar ratio of LiCl, LiF, Li2O, and AlCl3 was 0.25:0.25:0.5:1, respectively. Except for this, the same procedure as in Example 1 was carried out to produce the sample.

[0091] [Example 3] The solid electrolyte used to prepare the negative electrode mixture layer is Li 1.5 AlO 0.5 F 0.5 A solid-state battery was fabricated in the same manner as in Example 1, except that Li was used instead of Cl. 1.5 AlO 0.5 F 0.5Cl3 was prepared by weighing out raw material powders of LiF, Li2O, and AlCl3 in a molar ratio of 0.5:0.5:1, respectively. Except for this, the same procedure was followed as in Example 1.

[0092] [Example 4] The solid electrolyte used to prepare the negative electrode mixture layer is Li 1.5 AlO 0.5 F 0.25 Cl 3.25 A solid-state battery was fabricated in the same manner as in Example 1, except that the MM time was changed to 6 hours. 1.5 AlO 0.5 F 0.25 Cl 3.25 In the example, the raw material powders were weighed out so that the molar ratio of LiCl, Li2O, LiF, and AlCl3 was 0.25:0.5:0.25:1, respectively. Except for this, the same procedure as in Example 1 was carried out to prepare the sample. [Example 5] A solid-state battery was produced in the same manner as in Example 4, except that the MM time was changed to 12 hours.

[0093] [Comparative Example 1] A solid-state battery was produced in the same manner as in Example 1, except that the solid electrolyte used to produce the negative electrode mixture layer was changed to Li2ZrCl6. Li2ZrCl6 was produced by the following method. In a glove box with a dew point of about -70 to -85°C, raw material powders of LiCl and ZrCl4 were weighed out so that the molar ratio was 2:1. Next, LiCl and ZrCl4 were put into a zirconia reaction vessel for a planetary ball mill in which zirconia balls had been placed in advance. Li2ZrCl6 was produced by carrying out the same procedures as in Example 1 except for this.

[0094] [Comparative Example 2] The solid electrolyte used to prepare the negative electrode mixture layer is Li 1.5 AlO 0.5 Cl 3.5 A solid-state battery was produced in the same manner as in Example 1, except that the Li 1.5 AlO 0.5 Cl3.5 In the example, the raw material powders were weighed out so that the molar ratio of LiCl, Li2O, and AlCl3 was 0.5:0.5:1, respectively. Except for this, the same procedure as in Example 1 was carried out to prepare the sample.

[0095] First, in Examples 2 to 5 and Comparative Examples 1 and 2, the ionic conductivity of the solid electrolyte prepared for the negative electrode mixture layer was measured in the same manner as in Example 1.

[0096] (Initial charge / discharge capacity measurement) Next, the initial charge capacity and initial discharge capacity were measured for the solid-state batteries of Examples 1 to 5 and Comparative Examples 1 and 2, and the initial charge / discharge efficiency, which is the ratio of the initial discharge capacity to the initial charge capacity, was calculated.

[0097] First, two stainless steel plates with a diameter of 50 mm and a thickness of 5 mm and two Bakelite plates with a diameter of 50 mm and a thickness of 2 mm were prepared. Next, four holes for passing screws were made in each of the two stainless steel plates and the two Bakelite plates. The screw holes were made in positions where the two stainless steel plates and the two Bakelite plates overlap in a plan view when the half cell, the two stainless steel plates, and the two Bakelite plates are stacked, but do not overlap in a plan view with the electrochemical cell.

[0098] Then, a stainless steel plate, a Bakelite plate, a half cell, a Bakelite plate, and a stainless steel plate were stacked in that order, and screws were inserted into the screw holes and tightened with a torque of 1 N m. In this way, a negative electrode half cell was obtained in which the upper and lower punches of the electrochemical cell were insulated by the Bakelite plate. This half cell was placed in a thermostatic chamber at 25°C.

[0099] The electrochemical characteristics of the working electrode were evaluated using the negative half-cell thus fabricated. The measurements were performed by placing the half-cell in a thermostatic chamber at 25°C. The C rate was used to indicate the charge and discharge. The half-cell was charged to 1.0 V (E / V vs. Li / Li) at a current of 0.05 C. +Charge it until + and measure the initial charge capacity. After a 10-minute rest state, discharge it at a current of 0.05C until 2.5V (E / V vs. Li / Li and measure the initial discharge capacity. The initial charge-discharge efficiency was obtained by the following formula.

[0100] Table 1 summarizes the configurations of the half-cells of Examples 1 to 5, Comparative Example 1, and Comparative Example 2, the ionic conductivity [S / cm] of the solid electrolyte used in the negative electrode binder layer, the initial charge capacity [mAh / g], the initial discharge capacity [mAh / g], the initial charge-discharge efficiency [%], the time for which the mechanochemical reaction was carried out when preparing the solid electrolyte for the electrode binder layer, and the composition of the obtained solid electrolyte, including g, h, and {4-(g+h)} in formula (1).

[0101] [Table 1]

[0102] Figures 2 to 5 show graphs of the initial charge-discharge curves of Examples 1 to 5, Comparative Example 1, and Comparative Example 2. Figure 2 is a graph of the initial charge-discharge curve of Example 1. Figure 3 is a graph of the initial charge-discharge curves of Example 2 and Comparative Example 1. Figure 4 is a graph of the initial charge-discharge curves of Example 2 and Comparative Example 2. Figure 5 is a graph of the initial charge-discharge curve of Example 3.

[0103] As shown in Figures 2 to 5 and Table 1, in Examples 1 to 5, the irreversible capacity was smaller and the initial charge-discharge efficiency was higher than in Comparative Example 1 and Comparative Example 2. Therefore, it was confirmed that by using the solid electrolyte represented by the composition formula Li 1+g MO g F h Cl 4-(g+h) (where M is one or both of Al and Ga, and 0≦g<4, 0<h<4, 0<4-(g+h)<4), a high initial charge-discharge efficiency is shown. Also, it was confirmed that excellent characteristics can be obtained in any of Examples 2, 4, and 5 in which only the mechanochemical reaction time was adjusted. [Explanation of symbols]

[0104] 10...solid electrolyte layer, 20...positive electrode, 22...positive electrode current collector, 24...positive electrode mixture layer, 30...negative electrode, 32...negative electrode current collector, 34...negative electrode mixture layer, 40...power generating element, 50...exterior body, 52...metal foil, 54...resin layer, 60, 62...terminal, 100...solid-state battery

Claims

1. Represented by the composition formula (1), Li 1+g MO g F h Cl 4-(g+h) ・・・(1) In formula (1), M is one or both of Al and Ga; A solid electrolyte satisfying 0≦g<4, 0<h<4, and 0<4-(g+h)<4.

2. An electrode for a solid-state battery comprising the solid electrolyte according to claim 1.

3. A solid-state battery comprising the electrode for a solid-state battery according to claim 2.

Citation Information

Patent Citations

  • Solid electrolyte, solid electrolyte layer, and solid electrolyte battery

    WO2021024783A1

  • Solid electrolyte, solid electrolyte layer, and solid electrolyte cell

    WO2021024785A1

  • Solid electrolyte material and battery using same

    WO2021199676A1

  • Solid electrolyte and solid electrolyte battery

    WO2021261558A1

  • Solid electrolyte material and battery

    WO2022137758A1