Steelmaking furnace operation method

The method of using a solid oxygen source and controlled bottom-blowing gas stirring in a steelmaking furnace addresses slag foaming issues in the MURC process, enabling low-cost production of low-phosphorus steel with improved dephosphorization efficiency and reduced iron loss.

JP2024144220APending Publication Date: 2024-10-11NIPPON STEEL CORPORATION
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024041451
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-15
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The MURC method for producing low-phosphorus steel faces challenges in controlling slag foaming during dephosphorization blowing, leading to insufficient phosphorus removal and increased costs due to the use of inert gases and sedatives, which affect productivity and economic efficiency.

Method used

A method for operating a steelmaking furnace with top-bottom blowing function, involving dephosphorization blowing, stirring with bottom-blowing gas, and intermediate slag discharge, where a solid oxygen source like iron ore is added to the hot metal, and bottom-blowing gas is used to stir the slag after top-blowing oxygen supply, controlling the slag height ratio and stirring time to prevent foaming and enhance dephosphorization.

Benefits of technology

This approach allows for the production of low-phosphorus steel at low cost by stabilizing the dephosphorization reaction, reducing slag foaming, and minimizing iron loss, thereby achieving a phosphorus concentration below 0.02% while maintaining economic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144220000001
    Figure 2024144220000001
  • Figure 2024144220000002
    Figure 2024144220000002
Patent Text Reader

Abstract

To provide a steelmaking furnace operation method for inexpensively producing low-phosphorus steel having a phosphorus concentration of less than 0.02 mass% in a steelmaking furnace, especially in a converter refining process.SOLUTION: A steelmaking furnace is operated using a steelmaking furnace having a top and bottom blowing function, and dephosphorization blowing, agitation treatment of molten iron by bottom blowing gas, intermediate slag discharge from a furnace throat, and decarburization blowing are carried out in this order. In the dephosphorization blowing, top and bottom blowing is performed on the molten iron held in the steelmaking furnace, a solid oxygen source of 2 kg / t-steel or more is added to the molten iron in terms of FeO equivalent mass (all iron oxides are calculated as FeO) from before the start to the end of a top-blown oxygen jet of the top and bottom blowing, the top-blown oxygen jet of the dephosphorization blowing is terminated when the ratio of the slag height to the height of the freeboard of the steelmaking furnace is 0.7 or more and 1.0 or less during the dephosphorization blowing, and the molten iron is agitated with bottom blowing gas for 1 minute or longer after the end of the top-blown oxygen jet.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for operating a steelmaking furnace, and more particularly to a method for operating a steelmaking furnace for inexpensively producing low phosphorus steel. [Background technology]

[0002] In recent years, requirements for steel materials have become more sophisticated, and there is an increasing demand for low-phosphorus steel with high strength, high toughness, etc. In addition, as environmental awareness grows, there is a demand for a reduction in the amount of slag generated in the steel refining process through efficient use of auxiliary materials, and a reduction in the amount of CO2 generated by increasing the amount of scrap used, etc. Therefore, even for low-phosphorus steel with a phosphorus concentration of less than 0.02 mass%, which uses a large amount of auxiliary materials in the steel refining process and makes it difficult to use a large amount of scrap, a new refining technology is required that has a low environmental impact similar to that of conventional general steel with a phosphorus concentration of about 0.02 mass%.

[0003] In an integrated steel refining process, the molten pig iron tapped from the blast furnace contains approximately 0.13 to 0.18% phosphorus. A widely used method for removing this phosphorus is to treat the molten pig iron under low temperature conditions that are favorable for the progress of the dephosphorization reaction shown in formula (1) and under molten pig iron conditions where the activity of phosphorus in the metal is high. Here, the elements in [ ] in formula (1) indicate the components in the molten pig iron, and the compounds in ( ) indicate the components in the slag. 2[P]+5(FeO)+3(CaO)=(3CaO P2O5)+5Fe ···(1)

[0004] Since the dephosphorization reaction proceeds more at low temperatures, dephosphorization blowing is performed at the molten pig iron stage, which is relatively low at about 1300 to 1400°C. Converters are often used for such molten pig iron dephosphorization, and top-bottom blown converters are particularly suitable. In a top-bottom blown converter, molten iron is refined by blowing oxygen from a top lance at the top of the converter while blowing bottom blown gas from the bottom of the converter. The oxygen blown into the molten pig iron from the top lance oxidizes the molten iron and forms (FeO) in the slag. This (FeO) and (CaO) in the slag formed by the addition of dephosphorization flux promote the reaction of formula (1) above, and dephosphorization blowing is performed. In other words, the oxygen blown into the molten pig iron from the top lance acts as an oxidizing agent necessary for dephosphorization. Furthermore, by performing bottom blowing with a large stirring force at the same time as top blowing, it is possible to improve the oxidation reaction rate of phosphorus.

[0005] After dephosphorization blowing, the slag with high phosphorus concentration is separated from the hot metal, and new refining materials are added to the hot metal to remove the phosphorus remaining in the hot metal and to decarburize and raise the temperature. Decarburization blowing is performed by blowing oxygen at high speed from the top lance of the converter and blowing bottom gas from the bottom of the converter. The decarburization reaction in this decarburization blowing proceeds faster as the oxygen supply rate increases, so in order to improve production efficiency, it is preferable to increase the oxygen supply rate and increase the decarburization reaction rate. On the other hand, the dephosphorization reaction rate in dephosphorization blowing is controlled by the mass transfer rate of phosphorus on either the metal side or the slag side or both, so it is preferable to reduce the oxygen supply rate and suppress slag foaming, which will be described later, to make the blowing time as long as possible.

[0006] As a method for performing the above-mentioned dephosphorization blowing and decarburization blowing in one converter, the MURC (Multi-Refining Converter) method is known (for example, Non-Patent Document 1). This MURC method is characterized in that during dephosphorization blowing, slag is foamed to a height suitable for slag discharge from the converter throat, a part of the slag with a high phosphorus concentration is discharged from the throat to the outside of the converter by tilting the converter (intermediate slag discharge), and new refining materials are added to the converter with the molten pig iron with a low phosphorus concentration remaining, to perform further dephosphorization and decarburization (decarburization blowing). As a method for performing dephosphorization blowing and decarburization blowing using two converters, LD-ORP (for example, Non-Patent Document 2) and SRP (Non-Patent Document 3) are known. In these methods, the molten pig iron after dephosphorization blowing is discharged into a ladle from a hole provided in the belly of the converter, and the slag with a high phosphorus concentration is separated from the molten pig iron. The hot metal is then recharged into the converter after slag removal, and fresh refining materials are added to carry out further dephosphorization and decarburization.

[0007] The MURC process is characterized by the fact that it is possible to use a larger proportion of scrap as the main raw material, since it is not necessary to discharge hot metal from the converter and charge it into the next converter, and therefore the heat loss is small, compared to the LD-ORP and SRP processes. In addition, the decarburization slag with a low phosphorus concentration in the previous charge can be recycled in hot working as flux for dephosphorization blowing, which is excellent in productivity and economy. On the other hand, the MURC process has been considered to be difficult to reduce the phosphorus concentration in the metal compared to the LD-ORP and SRP processes, because a large amount of slag remains after dephosphorization blowing, and the P2O5 in the dephosphorization slag is carried over to the dephosphorization blowing. Therefore, low-phosphorus steel with a phosphorus concentration standard of less than 0.015 mass% is melted by the LD-ORP and SRP processes, and the MURC process is applied to other general steels. However, in light of the recent demand for reducing the environmental load, it is desired to stably produce such low-phosphorus steel by the MURC process, which is excellent in productivity and economy.

[0008] The top blowing lance of the converter has a nozzle with a certain number of holes at its tip, and oxygen is blown from the nozzle toward the surface of the molten iron in the converter. The upper and lower limits of the oxygen blowing rate are determined by the shape of the tuyere (nozzle diameter and number of holes).

[0009] In the MURC process, the oxygen flow rate needs to be controlled by a single top-blowing lance attached to the converter. In the decarburization blowing performed after the dephosphorization blowing, a high oxygen flow rate is required to burn and decarburize the large amount of carbon contained in the molten iron in a short time. In the top-blowing lance designed to realize such high-speed oxygen flow, the upper limit of the oxygen flow rate is set to a level that enables high-speed oxygen flow in the decarburization blowing, so the lower limit of the oxygen flow rate is necessarily high.

[0010] On the other hand, in dephosphorization blowing, even if the oxygen flow rate is reduced, it is necessary to feed oxygen at a rate higher than the lower limit of the above-mentioned fixed oxygen flow rate. If the oxygen flow rate is lower than the lower limit, oxygen gas may not be supplied to the molten pig iron sufficiently, resulting in poor dephosphorization, or there may be safety issues due to flashbacks. In this way, when attempting to perform MURC refining using a lance suitable for high-speed oxygen feeding in decarburization blowing, it is necessary to blow at an oxygen flow rate higher than the optimal oxygen flow rate for dephosphorization blowing. As a result, CO bubbles may be generated at the interface between the molten pig iron and the slag by reaction between C in the molten pig iron and FeO (iron oxide) in the slag, and CO bubbles may be generated inside the slag itself by reaction between FeO in the slag and C in the iron particles contained in the slag (foaming). When the FeO concentration in the slag is high, a large amount of CO bubbles are generated, so slag with a high FeO concentration has strong foaming properties (the property of rapidly expanding and easily overflowing).

[0011] If slag foaming is severe, slopping occurs, in which high-temperature slag overflows from the converter throat. If slopping occurs and damages the refining equipment around the converter or the transport vessel waiting below the converter, a great deal of time and effort is required to restore the equipment. Therefore, if slopping occurs during dephosphorization blowing, blowing must be stopped at that stage. As a result, it is not possible to secure sufficient time for dephosphorization blowing, and the phosphorus concentration in the steel cannot be reduced sufficiently.

[0012] In order to prevent the foaming slag from overflowing, there is a method of destroying the layer in which the CO bubbles remain (hereinafter sometimes referred to as the "foam layer") to shrink the slag. For this purpose, a method is generally known in which a mass that gasifies inside the slag is added to the slag, and the foam layer is destroyed by utilizing the volume expansion energy generated when the mass is gasified by pyrolysis. Usually, such a mass that has a destructive effect is called a sedative (see Patent Documents 1 to 3).

[0013] However, it is difficult to stably and quickly settle the foamed slag with the above-mentioned method of destroying the foamed layer. One method for quickly settling the foamed slag is, for example, to add a large amount of a sedative, but this method increases the refining cost and is problematic in terms of economy. However, the method of destroying the foamed layer as in Patent Documents 1 to 3 not only increases the cost due to the addition of the sedative, but also increases the amount of slag due to the sedative, and further increases the heat loss due to the addition of the sedative.

[0014] Patent Document 4 discloses a method of delaying the timing of slag foaming and extending the dephosphorization time by starting to blow a mixed gas of oxygen gas and an inert gas onto the molten iron using the top blowing lance when the carbon concentration in the molten iron is 3.0 mass% or more. However, the use of the inert gas increases costs and inevitably leads to heat loss.

[0015] Patent Documents 5 to 7 disclose methods in which dephosphorization blowing and intermediate slag removal are repeated two or more times in the MURC process which performs dephosphorization blowing, intermediate slag removal, and decarburization blowing, or in the LD-ORP and SRP processes which perform dephosphorization blowing, tapping of molten iron, recharging the tapped molten iron into a steelmaking furnace after slag removal, and decarburization blowing.

[0016] Patent Document 8 discloses an invention in which, in a molten pig iron refining method in which a part of slag is discharged in an intermediate slag removal step between a plurality of divided refining steps, the slag height from the molten pig iron bath surface in the furnace is measured prior to the intermediate slag removal step, and when the ratio of the measured slag height to the height of the freeboard in the furnace (slag height ratio) is 0.3 or more and less than 0.6, the refining performed before the intermediate slag removal step is terminated, and then, while injecting bottom blown gas, the process is held for 1.0 minute or more and 5.0 minutes or less, and then, when the slag height ratio is 0.3 or more and less than 0.6, slag removal is started. A molten pig iron pretreatment method in which an intermediate slag removal step is performed between a desiliconization treatment step and a dephosphorization treatment step is described.

[0017] Patent Document 9 discloses a level measurement method and a level measurement device that use microwaves in a converter steelmaking process to measure the slag surface during blowing more accurately than ever before. [Prior art documents] [Patent documents]

[0018] [Patent Document 1] Japanese Patent Application Publication No. 54-032116 [Patent Document 2] Japanese Patent Application Publication No. 11-050124 [Patent Document 3] JP 2008-255446 A [Patent Document 4] International Publication No. WO2019 / 208557 [Patent Document 5] Patent No. 5671801 [Patent Document 6] Patent No. 6665884 [Patent Document 7] Patent Publication No. 2021-195558 [Patent Document 8] JP 2017-133060 A [Patent Document 9] JP 2019-112675 A [Non-patent literature]

[0019] [Non-Patent Document 1] Yuji Ogawa et al.: Iron and Steel Vol. 87 (2001) No. 1 [Non-Patent Document 2] K. Kato, et.al.: CAMP-ISIJ, 4(1991), 1153. [Non-Patent Document 3] T.Matsuo, et.al.: Sumitomo Met.,42 (1990), 96. Summary of the Invention [Problem to be solved by the invention]

[0020] In the MURC process, Patent Document 4 uses an inert gas for dephosphorization refining, but it is desirable to proceed with dephosphorization without using an inert gas. Recently, high productivity has been required even in the LD-ORP process and SRP process, which use top blowing lances in two converters, and high-speed oxygen supply for dephosphorization blowing has been implemented. In this case, slag foaming still progresses during dephosphorization blowing, and in order to prevent slopping, the dephosphorization blowing is terminated just before the occurrence of slopping, resulting in insufficient dephosphorization blowing and failure to sufficiently reduce the phosphorus concentration in steel.

[0021] An object of the present invention is to provide a method for operating a steelmaking furnace using a smelting vessel with top and bottom blowing functions, which produces low-phosphorus steel at low cost while stopping dephosphorization blowing so as to prevent the occurrence of slopping. [Means for solving the problem]

[0022] That is, the gist of the present invention is as follows. [1] A method for operating a steelmaking furnace having top and bottom blowing functions, comprising the steps of dephosphorization blowing, stirring of molten iron by bottom blowing gas, intermediate slag removal from the furnace throat, and decarburization blowing in this order, In the dephosphorization blowing, top-bottom blowing is performed on the molten pig iron held in the steelmaking furnace, and a solid oxygen source is added to the molten pig iron in an amount of 2 kg / t-steel or more in terms of FeO equivalent mass (calculated assuming that all iron oxide is FeO) from before the start of top-bottom blowing to the end of the top-bottom blowing, a slag height ratio is defined as a ratio of the slag height to the height of the freeboard from the surface of the molten iron in the steelmaking furnace to the throat of the steelmaking furnace during the dephosphorization blowing, and when the slag height ratio is 0.7 or more and 1.0 or less, top blowing of oxygen in the dephosphorization blowing is terminated, and after the termination of the top blowing of oxygen, the molten iron is stirred with bottom blown gas for one minute or more. [2] A method for operating a steelmaking furnace, comprising the steps of: performing top-and-bottom blowing of molten pig iron held in a smelting vessel having top-and-bottom blowing functions; adding a solid oxygen source to the molten pig iron in an amount of 2 kg / t-steel, calculated as FeO by mass (wherein all iron oxide is calculated as FeO), from before the start of top-blowing oxygen supply to the end of the top-and-bottom blowing; and stirring the molten pig iron with bottom-blowing gas for 1 minute or more after the end of top-blowing oxygen supply. [3] The method for operating a steelmaking furnace according to [1] or [2], characterized in that the time for stirring the molten iron with the bottom blown gas is 2 to 4 minutes. [4] The method for operating a steelmaking furnace according to any one of [1] to [3], characterized in that the solid oxygen source is added to 9 to 30 kg / t-steel molten iron in terms of FeO equivalent mass (all iron oxide is calculated as FeO). [5] The method for operating a steelmaking furnace according to any one of [1] to [4], characterized in that the slag after completion of the top-and-bottom oxygen blowing has a %T.Fe content of 23 to 33 mass%.

[0023] [6] A method for operating a steelmaking furnace according to any one of [2] to [5], characterized in that the top and bottom blowing is a dephosphorization blowing, and after the dephosphorization blowing, a stirring treatment of the molten iron with the bottom blown gas, intermediate slag removal from the furnace throat, and decarburization blowing are carried out in this order. [7] The method for operating a steelmaking furnace according to any one of [2] to [5], characterized in that the top and bottom blowing is a dephosphorization blowing, and after the dephosphorization blowing, the following steps are carried out in this order: stirring the molten iron with the bottom blown gas, tapping the molten iron, recharging the tapped molten iron into the steelmaking furnace after slag removal, and decarburization blowing. [8] A method for operating a steelmaking furnace according to any one of [1] to [6], characterized in that the dephosphorization blowing, the stirring treatment of the molten iron with bottom blown gas, and the intermediate slag removal are repeated two or more times. In this specification, the expression "lower limit value to upper limit value" means "not less than the lower limit value and not more than the upper limit value." Effect of the Invention

[0024] According to the present invention, low-phosphorus steel having a phosphorus concentration of less than 0.02 mass % can be produced at low cost. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] The present inventors focused on improving the dephosphorization ability of hot metal in the MURC process, which involves dephosphorization blowing, intermediate slag disposal, and decarburization blowing. First, the phosphorus concentration in steel after dephosphorization blowing and after intermediate slag disposal was investigated. As a result, it was discovered that under conditions in which a solid oxygen source was added to the hot metal before the start of dephosphorization blowing or during dephosphorization blowing at a mass equivalent to FeO (all iron oxide is calculated as FeO) of 2 kg / t-steel or more, the phosphorus concentration in steel decreased during intermediate slag disposal, and the dephosphorization reaction proceeded. This result indicates that under the same conditions, the slag after dephosphorization blowing has a high phosphorus absorption capacity, and that during dephosphorization blowing, this dephosphorization slag with its high phosphorus absorption capacity cannot be fully utilized to reduce the phosphorus concentration in steel. The present inventors further investigated the phosphorus concentration in steel after decarburization blowing under conditions in which the dephosphorization reaction proceeded during the intermediate slag disposal. As a result, it was confirmed that even if the dephosphorization reaction proceeded during intermediate slag draining, the phosphorus concentration in the steel was not reduced after decarburization blowing compared to when the dephosphorization reaction did not proceed during intermediate slag draining. Because the furnace was tilted during intermediate slag draining, the bottom blowing nozzle was positioned above the top surface of the molten iron, which meant that the bottom blown gas was not blown into the molten iron, and the molten iron was not stirred sufficiently, so the dephosphorization reaction proceeded only in an extremely narrow region near the metal bath. With intermediate slag draining, the dephosphorization slag with a high P2O5 concentration near the metal bath could not be drained, which is thought to be why the phosphorus concentration in the steel was not reduced after decarburization blowing.

[0026] Next, the inventors investigated the metallic iron concentration by collecting slag from the converter after dephosphorization blowing and after intermediate slag removal. As a result, it was confirmed that the metallic iron content in the total slag was about 30 mass% at the end of dephosphorization blowing, and that the metallic iron content in the slag after intermediate slag removal was about 25 mass% on average. Here, the metallic iron concentration was measured by the following method. First, the slag collected from the converter was crushed and magnetically separated to separate it into magnetic and non-magnetic materials. Then, the metallic iron concentration in these samples was quantified by bromine methanol separation-potassium dichromate titration method, and the metallic iron concentration in the collected slag was calculated using the mass of each sample.

[0027] The metallic iron contained in the slag is considered to be due to the scattering of molten iron by CO gas generated during dephosphorization blowing and the iron nuggets generated by the reduction reaction between FeO in the slag and C in the metal. Since the concentration of metallic iron in the slag decreases from dephosphorization blowing to intermediate slag removal, it is presumed that the generation of iron nuggets and the settling of iron nuggets from the slag to the metal occur simultaneously during dephosphorization blowing, and the proportion of metallic iron decreases during intermediate slag removal due to the settling of iron nuggets. The iron nuggets remaining in the slag during intermediate slag removal are discharged from the converter together with the slag during intermediate slag removal, causing yield loss. Therefore, if the concentration of metallic iron in the slag before intermediate slag removal could be further reduced, it would lead to a reduction in iron loss and a reduction in production costs.

[0028] Based on the above results, the inventors have intensively studied a method for stably and economically suppressing slag foaming, and have come up with the idea of ​​adding at least 2 kg / t-steel of a solid oxygen source such as iron ore, calculated as FeO by mass (all iron oxide is calculated as FeO), and stirring the slag metal with bottom blown gas from the converter between the end of dephosphorization blowing and the start of intermediate slag disposal, thereby allowing the dephosphorization reaction to proceed under conditions that fully utilize the high dephosphorization ability of the slag after dephosphorization blowing, and at the same time reducing the proportion of metallic iron in the slag, and then performing intermediate slag disposal.

[0029] Here, the effect of adding a solid oxygen source such as iron ore during dephosphorization blowing was examined by examining the composition of the slag sampled after dephosphorization blowing. As a result, the FeO concentration in the slag was higher when a solid oxygen source was added than when no solid oxygen source was added. This result is considered to be due to the fact that the Fe2O3 solid oxygen source decomposes into FeO and oxygen according to formula (2), and the decomposed oxygen becomes an oxygen source for the molten iron, and the decomposed FeO increases the FeO concentration in the slag, improving the phosphorus absorption ability of the slag. Fe2O3 → 2FeO+1 / 2O2 (2)

[0030] Based on the above idea, the inventors carried out dephosphorization blowing, intermediate slag removal and decarburization blowing of molten pig iron using a 300-ton converter (a smelting vessel having top and bottom blowing functions). In the dephosphorization blowing carried out as top and bottom blowing, oxygen was blown into the molten pig iron from a top blowing oxygen supply lance at a flow rate of 73 to 110 Nm 3 / (hr·ton-steel) onto the molten iron, and gas containing N2, O2, and CO2 is blown from the bottom blowing nozzle at a rate of 5 to 13 Nm 3 The oxygen was then blown into the molten pig iron so that the oxygen ratio was 1.0 to 2.0. A certain amount of iron ore or sintered powder was added to the molten pig iron as a solid oxygen source before and after the top blowing of oxygen. Quicklime and recycled slag were used as dephosphorization fluxes, and the basicity of the slag after dephosphorization (C / S) was adjusted to be about 1.0 to 2.0.

[0031] As shown in Table 1 below, the iron ore used had a particle size of 5 to 50 mm and contained approximately 66% by mass of iron present as iron oxides such as FeO and Fe2O3, with the remainder being trace components of CaO, SiO2, Al2O3, P2O5, and MgO. The sintered powder had a composition of approximately 59% by mass of iron present as iron oxides such as FeO and Fe2O3, with the remainder being trace components of CaO, SiO2, Al2O3, P2O5, MgO, and MnO, and had a particle size of 1 to 10 mm.

[0032] [Table 1]

[0033] During the dephosphorization blowing, when signs of slopping from the converter throat appeared, the top blowing was stopped, and the dephosphorization blowing was terminated at this point.

[0034] In addition, the distance from the molten iron bath surface in the converter to the top surface of the formed slag at the end of dephosphorization blowing was measured using a microwave level meter, and the ratio of the measured slag height to the distance from the molten iron bath surface to the throat of the converter (freeboard) was defined as the slag height ratio, and was investigated as the slag height ratio at the end of dephosphorization blowing.

[0035] After the dephosphorization blowing was completed, metal and slag samples were taken to confirm their compositions and temperatures, and the metal temperature was measured at the same time as the top blowing was stopped. Then, with the converter throat facing vertically upward, top blowing was not performed, and bottom blown gas was continuously blown at the same flow rate as during the dephosphorization blowing, and the molten iron and slag were stirred by this bottom blown gas for a specified period of time. After that, metal and slag samples were taken, the metal temperature was measured, and intermediate slag removal was performed.

[0036] In this intermediate slag removal, when the slag height ratio at the end of dephosphorization blowing was 0.7 or more and 1.0 or less, slag flowed out of the converter, but when it was less than 0.6, slag did not flow out of the converter and could not be removed. When the slag height ratio at the end of dephosphorization blowing was 0.8 or more and 1.0 or less, the amount of slag flowed out was large, and slag could be removed without problems. In Patent Document 4, when the slag height ratio was less than 0.6, refining performed before the intermediate slag removal process was terminated, and then bottom blown gas was injected. Patent Document 4 exemplifies a case where the blowing before the intermediate slag removal is a desiliconization treatment. The present invention is directed to slag foaming before the intermediate slag removal after dephosphorization blowing, and it can be assumed that this difference causes a difference in the suitable range of the slag height ratio.

[0037] As a result, it was found that the dephosphorization reaction proceeded during the bottom blowing and stirring process when FeO supply sources such as iron ore and sintered powder were added to the molten iron during dephosphorization blowing at an FeO equivalent mass (all iron oxide was calculated as FeO) of 2 kg / t-steel or more.

[0038] Furthermore, regardless of whether metal and slag sampling and temperature measurements were performed or not, the height of the foamed slag did not change significantly during bottom blowing and stirring, and the amount of slag discharged during intermediate slag removal was equal to or greater than that without bottom blowing and stirring, which was good. This result is thought to be due to the bottom blowing gas causing the carbon in the molten iron and the FeO in the slag to react, continuing the reaction of formula (3) below, and maintaining the foamed height. In fact, the FeO concentration in the slag tended to decrease the longer the bottom blowing gas stirring was performed. The FeO concentration was analyzed by bromine methanol separation-EDTA titration method. (FeO)+[C]→Fe+CO(g) ···(3)

[0039] In addition, a specified amount of refining agent was added to the hot metal after intermediate slag removal and decarburization blowing was performed. As a result, when the hot metal and slag were stirred with bottom blown gas for 1 minute or more after dephosphorization blowing and before intermediate slag removal, the steel after decarburization blowing had a [%P] of <0.020%, confirming the effect of reducing phosphorus. This is considered to be a synergistic effect of the effect of promoting the dephosphorization reaction by stirring the hot metal with bottom blown gas after the end of top oxygen blowing in dephosphorization blowing, and the effect of removing the slag with concentrated P2O5 by intermediate slag removal.

[0040] Next, the inventors sampled the slag after bottom-blowing stirring and investigated the proportion of metallic iron contained in the sampled slag. As a result, it was confirmed that the proportion of metallic iron in the slag, which was 30% by mass when the conventional bottom-blowing stirring was not performed, was reduced to about 5 to 25% by mass when the bottom-blowing stirring was performed. In addition, the proportion of metallic iron in the slag was lower as the bottom-blowing stirring time was longer. During dephosphorization blowing with top-bottom blowing, oxygen blown at high speed from the top-blowing lance reacts violently with the molten pig iron at a hot spot (the fire point where the top-blowing oxygen collides with the molten pig iron), and the molten pig iron is physically blown away by the generated CO gas and oxygen jet, turns into fine iron particles, and is continuously supplied into the slag, and at the same time, the iron particles settle in the slag and return to the molten pig iron side. It is considered that, as a result of these factors, approximately 30% by mass of iron remained in the slag at the end of the conventional dephosphorization blowing. In the present invention, during bottom blowing stirring after the end of dephosphorization blowing, there is no oxygen supply from the top blowing lance, no supply of iron nuggets to the slag, and bottom blowing stirring causes the iron nuggets remaining in the slag to combine and only settle, which is thought to be the reason why the proportion of metallic iron in the slag decreased.The inventors evaluated the amount of molten steel after tapping through decarburization blowing using a weighing machine and confirmed that the amount of molten steel increased in the present invention, in which bottom blowing stirring is performed after dephosphorization blowing, compared to conventional MURC operation, in which bottom blowing stirring is not performed after dephosphorization blowing.

[0041] As described above, the effect of the present invention can be achieved if the bottom blowing stirring time after dephosphorization blowing is 1 minute or more. The inventors have also confirmed that the [%P] after decarburization blowing is further reduced when the bottom blowing stirring time is 2 to 4 minutes. When the compositions of metal and slag samples after dephosphorization blowing and after bottom blowing stirring were investigated, it was confirmed that the T.Fe (Fe content present as iron oxide) in the slag and the carbon concentration in the molten pig iron decreased during bottom blowing stirring. This is believed to be due to the progress of the reaction of formula (3).

[0042] As mentioned above, T.Fe in the slag affects the progress of the dephosphorization reaction, so when the bottom blowing stirring time was longer than 4.1 minutes, the excessive reduction of FeO probably had a negative effect on the progress of the dephosphorization reaction. Also, when the bottom blowing stirring time was shorter than 2 minutes, the stirring time was too short and it is thought that the dephosphorization reaction was not promoted sufficiently in relation to the phosphorus absorption capacity of the slag.

[0043] The bottom blowing stirring time is preferably 2 to 3 minutes, and in this case, the [%P] after decarburization blowing is the lowest. This is for the same reason as above, and it is considered that under these conditions, the dephosphorization reaction proceeds sufficiently with respect to the phosphorus absorption capacity of the slag while suppressing the excessive reduction of FeO.

[0044] Furthermore, the inventors have confirmed that the dephosphorization reaction rate during bottom blowing stirring after dephosphorization is high when a solid oxygen source such as iron ore or sintered powder is added in an amount of 9 kg / t-steel to 30 kg / t-steel in terms of FeO mass (all iron oxide is calculated as FeO) before or during dephosphorization blowing.

[0045] Furthermore, the inventors investigated the (%T.Fe) in the non-magnetic slag (iron in the form of iron oxide such as FeO, Fe2O3, etc.) by magnetically separating the slag collected from the converter after the end of the top-blowing oxygen supply in the dephosphorization blowing in which a solid oxygen source was added under the above conditions, and obtained a result of 21 to 35 mass%. Furthermore, when a solid oxygen source such as iron ore or sintered powder was added at 19 kg / t-steel to 25 kg / t-steel in terms of FeO (calculated assuming that all iron oxide is FeO), an even higher dephosphorization rate was obtained, and the (%T.Fe) in the slag was 23 to 33 mass%. As explained above, the (%T.Fe) in the slag in the present invention means the (%T.Fe) in the non-magnetic slag obtained by magnetically separating the slag collected from the converter.

[0046] It is known that T.Fe in slag has a large effect on the phosphorus distribution ratio between slag and metal, and a high T.Fe concentration is effective in promoting the dephosphorization reaction. On the other hand, Non-Patent Document 1 reports that an excessive increase in T.Fe in slag leads to a deterioration in dephosphorization. This is thought to be because, based on formula (1), the increased T.Fe reduces the concentration of CaO in the slag, which is necessary for fixing phosphorus. Non-Patent Document 1 reports that in a hot metal dephosphorization experiment using an 8-ton melting furnace, the highest phosphorus distribution was achieved when the basicity was approximately 1.0 and the T.Fe was about 30 mass%, and when the basicity was 1.5 and the T.Fe was about 25 mass%. Similarly, results close to these results were obtained in the present invention, and it is thought that a high dephosphorization rate was obtained by optimizing the amount of solid oxygen source added, which is the source of T.Fe.

[0047] In addition, when a solid oxygen source such as iron ore or sintered powder, which is a source of T.Fe, is added in a large amount during dephosphorization blowing, slag foaming may be promoted during dephosphorization blowing. According to the findings of the present inventors, particularly when the top blowing oxygen rate is 114 Nm 3 When iron ore, sintered powder, etc. were added at a rate of 30 kg / t-steel or more in terms of FeO (all iron oxide is calculated as FeO) or more, and when some of these were added in the latter half of the blow, slag foaming was promoted during the dephosphorization blow, and the dephosphorization blowing time tended to be shortened. However, it was confirmed that the dephosphorization reaction could proceed without any problems during the subsequent bottom blowing stirring, and a blow end [%P] of <0.015% after the decarburization blow could be achieved.

[0048] The present invention has been described above in terms of the dephosphorization blowing and intermediate slag removal processes, taking as an example the MURC process, which performs dephosphorization blowing, intermediate slag removal from the throat, and decarburization blowing. The present invention is not limited to the MURC process, and similar effects can be achieved by using the present invention in LD-ORP or SRP for the process from dephosphorization blowing to the subsequent process of removing the molten metal from the hole in the belly of the converter. EXAMPLES

[0049] Using a 300-ton top-bottom blowing converter, dephosphorization blowing, intermediate slag removal from the throat, and decarburization blowing were carried out. In the dephosphorization blowing, oxygen was blown into the molten pig iron from a top-blowing oxygen lance at a flow rate of 73 to 110 Nm. 3 / (hr·ton-steel) onto the molten iron, and gas containing N2, O2, and CO2 is blown from the bottom blowing nozzle at a rate of 5 to 13 Nm 3 The hot metal was blown with oxygen at a ratio of 1.2 to 1.8 / (hr·ton-steel). During the first half of the dephosphorization blowing (less than 50% of the blowing time) from before the start of top oxygen blowing, a certain amount of iron ore or sintered powder was added to the hot metal, and quicklime and recycled slag were used after adjusting the basicity of the slag after dephosphorization blowing (C / S) to about 1.2 to 1.8.

[0050] During dephosphorization blowing, when signs of slopping from the converter throat appeared, top blowing was stopped and the dephosphorization blowing was terminated at this point. In addition, the distance from the molten iron bath surface in the converter to the top surface of the foamed slag at the end of the dephosphorization blowing was measured using a microwave level meter, and the ratio of the measured slag height to the distance from the molten iron surface in the converter to the throat (freeboard height) was defined as the slag height ratio, which is shown in Table 1 as the slag height ratio at the end of the dephosphorization blowing. During the dephosphorization blowing, the dephosphorization blowing was terminated before the slag foaming became sufficiently large, and intermediate slag removal was performed after bottom blowing stirring. It was confirmed that a sufficient amount of slag could not be removed in the intermediate slag removal if the slag height ratio at the end of the dephosphorization blowing was 0.6 or less.

[0051] After the top blowing of the dephosphorization blowing was completed, bottom blowing gas was stirred at the same flow rate as during the dephosphorization blowing for the bottom blowing gas stirring time shown in Table 2, and then intermediate slag removal was performed. Quicklime was used in the decarburization blowing, and the slag basicity after the decarburization blowing (C / S) was adjusted to be approximately 3.0 to 3.5, and the blow-out rate [%P] after the decarburization blowing was evaluated.

[0052] The results are shown in Table 2. In Table 2, values ​​outside the range of the present invention are underlined. In the table, Δ[%P] is the value obtained by subtracting the [%P] obtained by analyzing a metal sample collected using a sublance after the top blowing of the dephosphorization blowing with an optical emission spectrometer from the [%P] obtained by similarly collecting and analyzing the metal sample before the intermediate slag discharge. Also, Δ(%T.Fe) is the value obtained by subtracting the (%T.Fe) measured in the same manner before the intermediate slag discharge from the (%T.Fe) in the non-magnetic material recovered by magnetically separating the slag collected using a sublance after the top blowing of the dephosphorization blowing with an X-ray fluorescence device. Also, Δ(%M.Fe) is the value obtained by subtracting the (%M.Fe) measured in the same manner before the intermediate slag discharge from the (%M.Fe) measured by the bromine methanol separation-potassium dichromate titration method for the slag collected using a sublance after the top blowing of the dephosphorization blowing.

[0053] Inventive examples No. 1 and No. 2 had a lower (g) blow-end [%P] than comparative examples No. 10 and No. 11. This is because in the table for inventive examples No. 1 and No. 2, (a) the FeO-equivalent mass of the solid oxygen source was 2 kg / ton-steel or more, (b) the bottom blown gas stirring time from the end of dephosphorization blowing was 1 minute or more, and (c) as shown in Δ[%P], dephosphorization proceeded during the period (b). Inventive examples No. 3 and No. 4 had a lower (g) blow-end [%P] of 0.016% or less than inventive examples No. 1 and No. 2. (b) The bottom blown gas stirring time from the end of dephosphorization blowing was 2 to 4 minutes, and (c) as shown in Δ[%P], dephosphorization proceeded further during the period (b). In addition, in invention examples Nos. 5 and 6, the (g) blow-end [%P] was lowered to 0.013% or less compared to Nos. 3 and 4. This is thought to be because (a) the FeO-equivalent mass of the solid oxygen source was 9-30 kg / t-steel, and (c) as shown in Δ[%P], dephosphorization progressed further during the period (b).

[0054] In addition, in Examples 7 to 9, the (g) end-point [%P] was 0.010% or less, lower than that in Examples 5 and 6. (d) The (%T.Fe) after dephosphorization blowing was 23 to 33 mass%, and as shown in (c) Δ[%P], it is considered that dephosphorization progressed further during the period (b).

[0055] Furthermore, in the case of the invention examples Nos. 1 to 9, in addition to the (g) lower end point [%P] compared to the comparative example, (e) Δ(%T.Fe) and (f) Δ(%M.Fe) were high, indicating that the iron loss was also improved.

[0056] [Table 2]

Claims

1. A method for operating a steelmaking furnace having top and bottom blowing functions, comprising the steps of dephosphorization blowing, stirring of molten pig iron by bottom blown gas, intermediate slag removal from the furnace throat, and decarburization blowing in this order, comprising: In the dephosphorization blowing, top-bottom blowing is performed on the molten pig iron held in the steelmaking furnace, and a solid oxygen source is added to the molten pig iron in an amount of 2 kg / t-steel or more in terms of FeO equivalent mass (calculated assuming that all iron oxide is FeO) from before the start of top-bottom blowing to the end of the top-bottom blowing, a ratio of the slag height to the height of the freeboard from the surface of the molten iron in the steelmaking furnace to the throat of the steelmaking furnace during the dephosphorization blowing is defined as a slag height ratio, and when the slag height ratio is 0.7 or more and 1.0 or less, top blowing of oxygen in the dephosphorization blowing is terminated, and after the termination of the top blowing of oxygen, the molten iron is stirred by bottom blown gas for one minute or more.

2. 2. The method for operating a steelmaking furnace according to claim 1, wherein the time for stirring the molten iron with the bottom blown gas is 2 to 4 minutes.

3. 3. The method for operating a steelmaking furnace according to claim 1 or 2, wherein the solid oxygen source is added to 9 to 30 kg / t-steel molten iron in terms of FeO equivalent mass (iron oxide is calculated as all FeO).

4. The method for operating a steelmaking furnace according to claim 1 or 2, characterized in that the slag (%T.Fe) after completion of the top-bottom blowing of the top-bottom blowing is 23 to 33 mass%.

5. The method for operating a steelmaking furnace according to claim 3, characterized in that the slag (%T.Fe) after completion of the top-bottom blowing of the top-blowing oxygen supply is 23 to 33 mass%.

Citation Information

Patent Citations

  • Killing material for foaming of converter slag

    JP1979032116A

  • Measuring device for record playing time

    JP1981071801A

  • Repressing material of foaming slag in containing vessel for molten metal and molten slag

    JP1999050124A

  • Method for killing slag

    JP2008255446A

  • Method for refining molten iron

    JP2017133060A