Negative electrode composite material, preparation method thereof, negative electrode, and lithium ion secondary battery
A carbon-coated silicon oxide composite material with controlled lithium content addresses high residual lithium issues, improving slurry processability and battery performance in lithium ion secondary batteries.
Patent Information
- Application Number
- JP2024045558
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-03-21
AI Technical Summary
Conventional lithium ion secondary batteries face challenges in improving the initial coulombic efficiency and cycle characteristics due to high residual lithium content in silicon-based negative electrode materials, which complicates the processability of the slurry.
A negative electrode composite material is developed with a carbon coating layer on silicon oxide particles, incorporating specific amounts of lithium compounds like Li2CO3 and LiOH, and a controlled manufacturing process involving heat treatments and cleaning steps to reduce residual lithium.
The composite material significantly reduces residual lithium, enhancing the processability of the slurry and improving the initial coulombic efficiency and cycle characteristics of lithium ion secondary batteries.
Smart Images

Figure 2024144258000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of lithium ion secondary batteries, and in particular to an anode composite material, a method for producing the anode composite material, and an anode and a lithium ion secondary battery comprising the anode composite material. [Background technology]
[0002] In recent years, with the development of electronic technology, the demand for battery devices that support the energy supply of electronic devices is increasing. Currently, there is a demand for batteries that can store more power and output large power. Conventional lead-acid batteries and nickel-metal hydride batteries are no longer able to meet the requirements of new electronic devices such as mobile devices such as smartphones and stationary devices such as power storage systems. Therefore, lithium-ion secondary batteries have attracted widespread attention. In the development of lithium-ion secondary batteries, their capacity and characteristics have been effectively improved. Lithium-ion secondary batteries have the advantages of high energy density, high operating voltage, long cycle life, and little environmental pollution, and have become a new environmentally friendly high-energy chemical power source with great development potential in the current world.
[0003] A lithium ion secondary battery includes a positive electrode, a negative electrode containing a negative electrode material, and an electrolyte. Several types of negative electrode materials have been developed, among which silicon-based negative electrode materials are one type of negative electrode materials with relatively high potential. In the prior art, a prelithiation technique is adopted to improve the properties of silicon-based negative electrode materials, and the amount of residual lithium in the silicon-based negative electrode material is disclosed as being controlled. However, in the prior art, the upper and lower limits of the control of the amount of residual lithium in the silicon-based negative electrode material are both high, making it difficult to improve the processability of the slurry containing the negative electrode material, and making it difficult to effectively improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery. Therefore, there is a demand for the development of a new negative electrode composite material, a method for producing the negative electrode composite material, a negative electrode containing the negative electrode composite material, and a lithium ion secondary battery. Summary of the Invention [Problem to be solved by the invention]
[0004] The main objective of the present invention is to provide an anode composite material, a method for manufacturing the anode composite material, and an anode and a lithium ion secondary battery comprising the anode composite material, in order to solve the problems in the prior art that the residual lithium content of the anode material is too high, it is difficult to improve the processability of the slurry, and it is difficult to effectively improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery. [Means for solving the problem]
[0005] In order to achieve the above object, according to one aspect of the present invention, there is provided a negative electrode active material comprising: a negative electrode active material particle; and Li2CO3 and LiOH on a surface of the negative electrode active material particle, Granules containing silicon oxide and at least one lithium silicate selected from Li2SiO3 and Li2Si2O5; A carbon coating layer is coated on at least a portion of the surface of the granule, The present invention provides an anode composite material, characterized in that the Li2CO3 content is greater than 0 wt% and less than 0.01 wt%, and the LiOH content is greater than 0 wt% and less than 0.01 wt%, based on the weight of the anode active material particles.
[0006] Furthermore, in the negative electrode composite material, the silicon oxide is SiO x (0.5≦x≦1.6).
[0007] Furthermore, in the negative electrode composite material, the coating amount of the carbon coating layer is within a range of 1 wt % to 30 wt % based on the weight of the negative electrode active material particles.
[0008] Furthermore, in the negative electrode composite material, the carbon coating layer covers the entire surface of the granule.
[0009] According to another aspect of the present invention, there is provided a method for producing an anode composite material, comprising the steps of: performing a carbon coating process on the silicon oxide precursor using a carbon source to form a carbon-coated silicon oxide; combining the carbon-coated silicon oxide with a lithium source to form a first mixture, subjecting the first mixture to a first heat treatment to form a calcined product, and then subjecting the calcined product to a second heat treatment to form a prelithiated product; A method is provided in which the prelithiated product is washed and treated to form a negative electrode composite material.
[0010] Furthermore, in the method for producing the anode composite material, the washing process includes mixing the prelithiated product with water or acid, preferably to a solid content of 2 wt% to 10 wt%, to form a second mixture, ultrasonicating the second mixture to disperse it, then suction filtering, and finally drying the material after suction filtering.
[0011] Furthermore, in the method for producing the negative electrode composite material, the acid is at least one selected from hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid, and boric acid.
[0012] Furthermore, in the method for producing the negative electrode composite material, the weight ratio of the lithium source to the carbon-coated silicon oxide ranges from 5:95 to 15:85.
[0013] Furthermore, in the method for producing the negative electrode composite material, the temperature of the first heat treatment is in the range of 500° C. to 750° C., and the time of the first heat treatment is in the range of 2 hours to 5 hours.
[0014] Furthermore, in the method for producing the negative electrode composite material, the temperature of the second heat treatment is in the range of 925° C. to 1050° C., and the time of the second heat treatment is in the range of 3 hours to 6 hours.
[0015] Furthermore, in the method for producing the negative electrode composite material, the ultrasonic treatment time is in the range of 10 minutes to 30 minutes.
[0016] Furthermore, in the method for producing the negative electrode composite material, the dispersion time is in the range of 24 h to 72 h.
[0017] Further, in the method for producing the anode composite material, the carbon source includes at least one of an alkane, an alkene, and an alkyne.
[0018] According to a further aspect of the present invention, there is provided an anode for a lithium-ion secondary battery comprising the anode composite material described above.
[0019] According to a further aspect of the present invention, there is provided a lithium ion secondary battery comprising a positive electrode, a negative electrode, and a separator, the negative electrode comprising the negative electrode composite material described above. Effect of the Invention
[0020] The negative electrode composite material of the present invention, the method for producing the negative electrode composite material, and the negative electrode and lithium ion secondary battery including the negative electrode composite material can significantly reduce the amount of residual lithium, improve the processability of the slurry, and improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery. [Brief description of the drawings]
[0021] [Figure 1] 1 shows a photograph of the appearance of the negative electrode slurry in Comparative Example 4. [Diagram 2] 1 shows Li 1s XPS (X-ray photoelectron spectrum) maps of the negative electrode composite materials in Examples 1 and 2, Comparative Example 2, and Comparative Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] It should be noted that the various embodiments and features of the embodiments of the present application may be combined with each other without contradiction. The present invention will be described in detail below with reference to the following examples. The following examples are merely illustrative and do not limit the scope of protection of the present invention.
[0023] As described in the background art, in the prior art, the residual lithium content of the negative electrode material is too high, and it is difficult to improve the processability of the slurry containing the negative electrode material, and it is difficult to effectively improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery. In response to the problems in the prior art, a representative embodiment of the present invention provides a negative electrode composite material comprising: negative electrode active material particles; Li2CO3 and LiOH on the surface of the negative electrode active material particles; the negative electrode active material particles comprise granules containing silicon oxide and at least one lithium silicate selected from Li2SiO3 and Li2SiO5; and a carbon coating layer coated on at least a part of the surface of the granules; and the content of Li2CO3 is more than 0 wt% and less than 0.01 wt% and the content of LiOH is more than 0 wt% and less than 0.01 wt%, based on the weight of the negative electrode active material particles.
[0024] If the residual lithium value is high, it affects the processability of the slurry containing the negative electrode composite material, and the slurry is likely to become "jelly" in the process of producing the slurry using the negative electrode composite material. As a result of many experiments, the inventors have unexpectedly found that the present invention can significantly reduce the amount of residual lithium and obtain a negative electrode composite material with an extremely low amount of residual lithium. The negative electrode composite material of the present invention has an extremely low amount of residual lithium, and can effectively prevent the slurry from becoming "jelly" in the process of producing the slurry using the negative electrode composite material, significantly improve the processability of the slurry, and improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery.
[0025] The silicon oxide according to the present application may be a silicon oxide generally used in the field of negative electrode materials. In some embodiments of the present invention, the silicon oxide in the negative electrode composite material of the present invention is SiO x (0.5≦x≦1.6, preferably 0.8≦x≦1.2, and most preferably x=1.0).
[0026] In some embodiments of the present invention, the coating amount of the carbon coating layer is in the range of 1 wt% to 30 wt%, preferably in the range of 3 wt% to 20 wt%, more preferably in the range of 5 wt% to 10 wt%, based on the weight of the negative electrode active material particles in the negative electrode composite material of the present invention. By setting the coating amount of the carbon coating layer in the above range, a good balance is achieved between the capacity of the material and the coating uniformity.
[0027] In some embodiments of the present invention, in the negative electrode composite material of the present invention, the carbon coating layer may be coated on the entire surface of the granule, which can improve the electrical conductivity of the negative electrode composite material, increase the first coulombic efficiency, effectively reduce the amount of residual lithium, and improve the processability of the slurry.
[0028] In another exemplary embodiment of the present invention, a method for producing an anode composite material is provided, the method including: performing a carbon-coating process on a silicon oxide precursor with a carbon source to form a carbon-coated silicon oxide; mixing the carbon-coated silicon oxide with a lithium source to form a first mixture, performing a first heat treatment on the first mixture to form a calcined product, and then performing a second heat treatment on the calcined product to form a pre-lithiated product; and washing the pre-lithiated product to form an anode composite material.
[0029] The method for producing the anode composite material according to the present invention can significantly reduce the amount of residual lithium, effectively prevent the slurry from becoming "jelly" during the process of producing a slurry using the anode composite material, improve the processability of the slurry, improve the initial coulombic efficiency and cycle characteristics of a lithium ion secondary battery, and suppress gas generation by the slurry. The anode composite material obtained by the above method according to the present invention has an extremely low amount of residual lithium, significantly improves the processability of the slurry, and can improve the initial coulombic efficiency and cycle characteristics of a lithium ion secondary battery.
[0030] The silicon oxide precursor in the present invention, for example, SiO x(0.5≦x≦1.6) can be prepared by a conventional method in the field. In some embodiments of the present invention, the silicon oxide precursor can be prepared by the following steps. Mix silicon powder and silica of a predetermined particle size in a molar ratio of about 1.1:1, then place in a vibrator and vibrate for about 12h to mix uniformly, take about 1kg of the above uniformly mixed material and press it into a mass, then put the mass into a vacuum sublimation furnace and heat it to a temperature of 1200℃-1500℃, adjust the vacuum degree to 0-30Pa, the heating time to 8h-10h, and the temperature at the collection end to 400℃-800℃ to prepare a mass silicon oxide precursor, put the mass silicon oxide precursor into a crusher to crush it to millimeter scale, then put the millimeter-scale silicon oxide precursor into a jet mill to crush it, classify the powders with different particle sizes by an air flow classifier, and finally blend the powders with different particle sizes according to size, and finally obtain a silicon oxide precursor with a desired particle size.
[0031] In some embodiments of the present invention, in the method for producing the above-mentioned negative electrode composite material, the silicon oxide precursor is carbon-coated by chemical vapor deposition using at least one of an alkane, an alkene, and an alkyne as a carbon source at a pressure of 50 Pa to 10,000 Pa and a temperature of 600° C. to 1,000° C. to form a carbon-coated silicon oxide. In some embodiments of the present invention, the carbon coating is performed in an apparatus such as a rotary kiln, a fixed bed, or a fluidized bed.
[0032] In some embodiments of the present invention, in the method for preparing the above-mentioned negative electrode composite material, the washing process includes mixing the prelithiated product with water or acid, preferably to a solid content of 2 wt% to 10 wt%, for example 2 wt% to 8 wt% or 5 wt% to 10 wt%, to form a second mixture, ultrasonicating the second mixture, then dispersing, then suction filtering, and finally drying the material after suction filtering. In the process of the washing process, water can be used to dissolve alkaline materials such as Li2CO3 and LiOH, and acid can be used to neutralize the alkali generated on the surface of the prelithiated product during washing. The ultrasonic treatment can wash the prelithiated product more cleanly, ensure a good washing effect, and improve the cycle characteristics of the lithium-ion secondary battery. By carrying out cleaning treatments such as water washing and acid washing, the amount of residual lithium can be significantly reduced, and the amount of residual lithium in the negative electrode composite material can be reduced to almost zero, thereby effectively avoiding the slurry from becoming "jelly" during the process of producing a slurry using the negative electrode composite material, significantly improving the processability of the slurry, and further improving the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery. By keeping the solid content within the above range, a sufficient amount of detergent can be ensured to clean a unit mass of the prelithiation product, and a good cleaning effect can be ensured.
[0033] In some embodiments of the present invention, the prelithiated product produced, e.g., prelithiated SiO x (0.5≦x≦1.6) The material is mixed with water to a solid content of 2wt% to 10wt% to form a second mixture, the second mixture is ultrasonically treated at room temperature for 10min to 30min, and then the second mixture is dispersed using a magnetic stirrer for 24h to 72h, and then suction filtered. After that, pure water is poured onto the material on the filter paper, and washed twice by suction filtration. Finally, the material after suction filtration is vacuum dried at 100℃ to 120℃ for 3 to 8 hours.
[0034] In some embodiments of the present invention, in the method for producing the above-mentioned negative electrode composite material, the acid is at least one selected from hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid, and boric acid to neutralize the alkali generated on the surface of the prelithiated product during washing.
[0035] In some embodiments of the present invention, the prelithiated product produced, e.g., prelithiated SiO x (0.5≦x≦1.6) The material is mixed with at least one of hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid, and boric acid, for example, citric acid with a concentration of 1 mol / L, so that the solid content is 2 wt% to 10 wt%, to form a second mixture, and the second mixture is ultrasonically treated at room temperature for 10 min to 30 min, and then the second mixture is dispersed using a magnetic stirrer for 24 h to 72 h, and then suction filtered, and then pure water is poured onto the material on the filter paper, and washed twice by suction filtration, and finally, the material after suction filtration is vacuum dried at 100°C to 120°C for 3 to 8 hours.
[0036] In some embodiments of the present invention, in the method for producing the above-mentioned negative electrode composite material, the weight ratio of the lithium source to the carbon-coated silicon oxide is in the range of 5:95 to 15:85. By making the weight ratio of the lithium source to the carbon-coated silicon oxide in the above range, it is possible to ensure sufficient prelithiation of the silicon oxide, reduce the amount of residual lithium, and further improve the initial coulombic efficiency and cycle characteristics of the lithium-ion secondary battery. In some embodiments of the present invention, the lithium source may include any of lithium ingot, lithium metal powder, and lithium foil.
[0037] In some embodiments of the present invention, in the method for producing the above-mentioned negative electrode composite material, the temperature of the first heat treatment is in the range of 500°C to 750°C, and the time of the first heat treatment is in the range of 2h to 5h. By setting the temperature and time of the first heat treatment in the above ranges, it is favorable for the diffusion of lithium in the solid-phase reaction, and sufficient prelithiation of silicon oxide can be ensured, so that the amount of residual lithium can be reduced, and the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery can be further improved.
[0038] In some embodiments of the present invention, in the method for producing the above-mentioned negative electrode composite material, the temperature of the second heat treatment is in the range of 925°C to 1050°C, and the time of the second heat treatment is in the range of 3h to 6h. By setting the temperature of the second heat treatment in the above range, it is advantageous to decompose Li2CO3 and LiOH (the decomposition temperature is 924°C), and the decomposition product Li2O of Li2CO3 and LiOH begins to sublime at 1000°C or higher, which is advantageous to significantly reduce the amount of residual lithium. By setting the temperature and time of the second heat treatment in the above range, it is possible to ensure sufficient prelithiation of silicon oxide, significantly reduce the amount of residual lithium, and further improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery.
[0039] In some embodiments of the present invention, under the protection of inert atmosphere argon, the lithium source and the carbon-coated silicon oxide are ground and mixed in a weight ratio of 5:95 to 15:85 to form a first mixture, then the first mixture is put into a rotary kiln and calcined under argon atmosphere at 500°C to 750°C for 2h to 5h to fully react the carbon-coated silicon oxide with lithium metal, and then heat-treated at 925°C to 1050°C for 3h to 6h to obtain a pre-lithiated product.
[0040] In some embodiments of the present invention, in the method for preparing the above-mentioned negative electrode composite material, the ultrasonic treatment time is in the range of 10min to 30min. By making the ultrasonic treatment time in the above range, it is favorable to clean the residual lithium in the holes, and the prelithiation product can be cleaned more cleanly, and a good cleaning effect can be ensured, and the damage to the granules of the prelithiation product and the influence on the particle size distribution can be avoided.
[0041] In some embodiments of the present invention, in the method for producing the above-mentioned negative electrode composite material, the dispersion time may be controlled in the range of 24h to 72h, mainly considering the energy consumption, time cost and cleaning effect. If the dispersion time is too short, cleaning may not be performed cleanly, and if the dispersion time is too long, the energy consumption and time cost are high. By controlling the dispersion time in the above range, not only can a good cleaning effect be ensured, but also the energy consumption and time cost can be reduced.
[0042] In some embodiments of the present invention, in the method for producing the above-mentioned negative electrode composite material, in order to carbon-coat at least a part of the surface of the silicon oxide and obtain a good coating effect, the carbon source includes at least one of an alkane, an alkene, and an alkyne.
[0043] In a further exemplary embodiment of the present invention, a negative electrode for a lithium ion secondary battery is provided, which includes the above-mentioned negative electrode composite material. The negative electrode for a lithium ion secondary battery of the present invention includes the above-mentioned negative electrode composite material, which can greatly reduce the amount of residual lithium, significantly improve the processability of the slurry, and improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery.
[0044] The negative electrode sheet of the present invention can be prepared by a conventional method in the art. For example, the negative electrode composite material of the present invention, the conductive agent, and the binder are dispersed in water as a solvent to form a uniform negative electrode slurry, and the negative electrode slurry is applied onto a negative electrode collector and dried in an oven to obtain a negative electrode sheet. The conductive agent can be conductive carbon black, conductive graphite, vapor-grown carbon fiber, carbon nanotubes, or any combination thereof. The binder can be one or more of styrene butadiene rubber (SBR), polyacrylic acid (PAA), polyimide (PI), etc., and is preferably a polyacrylic acid (PAA) binder.
[0045] In a further exemplary embodiment of the present invention, a lithium ion secondary battery is provided, comprising a positive electrode, a negative electrode, and a separator, the negative electrode comprising the above-mentioned negative electrode composite material. Since the lithium ion secondary battery of the present invention comprises the above-mentioned negative electrode composite material, the amount of residual lithium can be significantly reduced, the processability of the slurry can be significantly improved, and the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery can be improved.
[0046] The positive electrode of the present invention includes a positive electrode collector and a positive electrode active material layer containing a positive electrode active material. The positive electrode collector has a positive electrode active material layer formed on two surfaces thereof. The positive electrode collector may be, for example, a metal foil such as an aluminum foil, a nickel foil, or a stainless steel foil.
[0047] The positive electrode active material layer may contain, as a positive electrode active material, one or more types of positive electrode materials capable of absorbing and releasing lithium ions, and may contain other materials, such as a positive electrode binder and / or a positive electrode conductive agent, as necessary.
[0048] Preferably, the positive electrode material is a lithium-containing compound. Examples of such lithium-containing compounds include lithium-transition metal composite oxides and lithium-transition metal phosphate compounds. The lithium-transition metal composite oxide is an oxide containing Li and one or more transition metal elements as constituent elements, and the lithium-transition metal phosphate compound is a phosphate compound containing Li and one or more transition metal elements as constituent elements. The transition metal element is preferably one or more of Co, Ni, Mn, Fe, etc.
[0049] Examples of the lithium-transition metal composite oxide may include, for example, LiCoO2 and LiNiO2. Examples of the lithium-transition metal phosphate compound may include, for example, LiFePO4 and LiFe 1-u Mn u PO4 (0 < u < 1), etc.
[0050] The negative electrode of the present invention includes a negative electrode current collector and a negative electrode active material layer containing a negative electrode composite material. The negative electrode active material layer is formed on two surfaces of the negative electrode current collector. As the negative electrode current collector, for example, metal foils such as copper (Cu) foil, carbon-coated copper foil, nickel foil, and stainless steel foil can be used.
[0051] The separator of the present invention is for separating the positive electrode and the negative electrode of the battery, and can pass lithium ions and prevent current short circuit due to contact between the positive electrode and the negative electrode. The separator is, for example, a porous membrane formed of a synthetic resin or a ceramic, and may also be a laminated membrane in which two or more types of porous membranes are laminated. Examples of the synthetic resin include, for example, polytetrafluoroethylene, polypropylene, and polyethylene.
[0052] In an embodiment of the present invention, when charging the lithium ion secondary battery, for example, lithium ions are released from the positive electrode and inserted into the negative electrode through the electrolytic solution immersed in the separator. When discharging the lithium ion secondary battery, for example, lithium ions are released from the negative electrode and inserted into the positive electrode through the electrolytic solution immersed in the separator.
[0053] The present application will now be described in more detail with reference to specific examples, which do not limit the scope of the protection claimed by the present application.
[0054] Example 1 Manufacture of anode composite material At a pressure of 50 Pa and a temperature of 920 °C, 20 g of silicon oxide precursor SiO was x (x=1) Silicon oxide precursor SiO x (x=1) The material was carbon-coated, and 21 g of carbon-coated SiO x (x=1) material was formed.
[0055] Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and the SiO2 material were ground and mixed in a weight ratio of 10:90 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 550°C for 3h under an argon atmosphere to produce a carbon-coated SiO2 material. x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 925°C for 3 hours to obtain prelithiated SiO x Got the material.
[0056] Fabricated prelithiated SiO x The material and 1 mol / L hydrochloric acid were placed in a beaker to give a solid content of 8 wt%, and mixed to form a second mixture. The second mixture was first ultrasonically treated at room temperature for 20 minutes, then dispersed for 48 hours using a magnetic stirrer, and then suction filtered. After that, pure water was poured onto the material on the filter paper, and washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.
[0057] Manufacture of negative electrode sheets 4 g of the negative electrode composite material produced by the above process was weighed out, and the negative electrode composite material, conductive carbon black Super-P as a conductive agent, and polyacrylic acid PAA as a binder were mixed in a mass ratio of 82:8:10 with an appropriate amount of deionized water by sufficient stirring, and the solid content was adjusted to 42 wt % to form a uniform negative electrode slurry. Thereafter, the negative electrode slurry was applied onto the surface of copper foil, which was the negative electrode collector, and dried to obtain a negative electrode sheet.
[0058] Battery Assembly The produced negative electrode sheet, separator, lithium sheet, gasket, and battery case were laminated in this order, 100 μl of electrolyte was poured, and the opening was sealed with a sealing machine to assemble the desired half cell.
[0059] Example 2 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and the SiO2 material were ground and mixed in a weight ratio of 15:85 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600 °C for 4 h under an argon atmosphere to produce a carbon-coated SiO2 material. x The material was fully reacted with lithium metal and then heat-treated at 1000°C for 4 hours to obtain prelithiated SiO x Obtaining the materials, Fabricated prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 5 wt%, and the second mixture was first ultrasonically treated at room temperature for 15 minutes, and then dispersed using a magnetic stirrer for 36 hours. The second mixture was then suction filtered. After that, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtering. Finally, the material after suction filtering was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0060] Example 3 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x(x=1) material and the SiO2 material were ground and mixed in a weight ratio of 5:95 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 500 °C for 2 h under an argon atmosphere to produce a carbon-coated SiO2 material. x The material was fully reacted with lithium metal and then heat-treated at 1050 °C for 6 h to obtain prelithiated SiO x Obtaining the materials, Fabricated prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 2 wt%, and the second mixture was first ultrasonically treated at room temperature for 30 minutes, and then dispersed using a magnetic stirrer for 72 hours. The second mixture was then suction filtered. After that, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtering. Finally, the material after suction filtering was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0061] Example 4 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and the SiO2 material were ground and mixed in a weight ratio of 15:85 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 750 °C for 5 h under an argon atmosphere to produce a carbon-coated SiO2 material. x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 1025°C for 4 hours to obtain prelithiated SiO x Obtaining the materials, Fabricated prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 10 wt%, and the second mixture was first ultrasonically treated at room temperature for 10 minutes, and then dispersed using a magnetic stirrer for 24 hours. The second mixture was then suction filtered. After that, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0062] Example 5 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and the SiO2 material were ground and mixed in a weight ratio of 5:95 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 650°C for 2h under an argon atmosphere to produce a carbon-coated SiO2 material. x The material was fully reacted with lithium metal and then heat-treated at 1050 °C for 6 h to obtain prelithiated SiO x Obtaining the materials, Fabricated prelithiated SiO x The material and pure water were put into a beaker so that the solid content was 2 wt%, and mixed to form a second mixture. The second mixture was first ultrasonically treated at room temperature for 30 minutes, and then dispersed using a magnetic stirrer for 72 hours. Then, the second mixture was suction filtered. Then, pure water was poured onto the material on the filter paper, and washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0063] Comparative Example 1 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and the SiO2 material were ground and mixed in a weight ratio of 15:85 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 750 °C for 5 h under an argon atmosphere to produce a carbon-coated SiO2 material. x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 775°C for 4 hours to obtain prelithiated SiO x Obtaining the materials, Fabricated prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 10 wt%, and the second mixture was first ultrasonically treated at room temperature for 10 minutes, and then dispersed using a magnetic stirrer for 24 hours. The second mixture was then suction filtered. After that, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0064] Comparative Example 2 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and the SiO2 material were ground and mixed in a weight ratio of 2:98 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 400°C for 2h under an argon atmosphere to produce a carbon-coated SiO2 material. x The material was fully reacted with lithium metal and then heat-treated at 950°C for 7 hours to obtain prelithiated SiO x Obtaining the materials, Fabricated prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 20 wt%, and the second mixture was first ultrasonically treated at room temperature for 10 minutes, and then dispersed with a magnetic stirrer for 8 hours. The second mixture was then suction filtered. After that, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0065] Comparative Example 3 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and the SiO2 material were ground and mixed in a weight ratio of 15:85 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600 °C for 4 h under an argon atmosphere to produce a carbon-coated SiO2 material. x The material was fully reacted with lithium metal and then heat-treated at 1000°C for 4 hours to obtain prelithiated SiO x Obtaining the materials, Fabricated prelithiated SiO xThe material and 1 mol / L hydrochloric acid were placed in a beaker to give a solid content of 5 wt%, mixed to form a second mixture, and the second mixture was dispersed at room temperature using a magnetic stirrer for 36 hours. Then, the mixture was suction filtered. After that, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material. A half cell was manufactured in the same manner as in Example 1.
[0066] Comparative Example 4 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and the SiO2 material were ground and mixed in a weight ratio of 10:90 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 550°C for 3h under an argon atmosphere to produce a carbon-coated SiO2 material. x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 925°C for 3 hours to obtain prelithiated SiO x Obtaining the materials, Prelithiated SiO x The material was prelithiated with SiO x A half cell was produced in the same manner as in Example 1, except that the material was used as it was for the negative electrode composite material.
[0067] Comparative Example 5 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and the SiO2 material were ground and mixed in a weight ratio of 30:70 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600 °C for 5 h under an argon atmosphere to produce a carbon-coated SiO2 material. x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 820°C for 2 hours to obtain prelithiated SiO x Obtaining the materials, Fabricated prelithiated SiO xThe material and pure water were placed in a beaker so that the solid content was 5 wt%, and mixed to form a second mixture. The second mixture was dispersed at room temperature using a magnetic stirrer for 48 hours, and then suction filtered. After that, pure water was poured onto the material on the filter paper, and washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material. A half cell was manufactured in the same manner as in Example 1.
[0068] Material property testing Tests were carried out on the negative electrode composite materials in Examples 1 to 5 and Comparative Examples 1 to 5 to obtain the results of the Li2CO3 content and the LiOH content.
[0069] Neutralization titration method: A negative electrode composite material and pure water were weighed in a beaker in a mass ratio of 1:9, mixed, and dispersed in a magnetic stirrer at room temperature for 1 hour, then allowed to stand for 1 hour, and the dispersion was filtered. 10 mL of the resulting filtrate was automatically titrated with 0.2 M hydrochloric acid using an automatic acid-alkali titrator, and the first end point (a mL) and the second end point (b mL) were determined.
[0070] Li2CO3 content = [pure water volume (g) / filtrate volume (g)] × 2 × (b / 1000) × (equivalent concentration of hydrochloric acid titration × coefficient) × (1 / 2) × (molar mass of Li2CO3) × [100 (%) / sample volume (g)] LiOH content = [volume of pure water (g) / volume of filtrate (g)] × [(ab) / 1000] × (equivalent concentration of hydrochloric acid titration amount × coefficient) × (1 / 2) × (molar mass of LiOH) × [100 (%) / volume of sample (g)].
[0071] Battery characteristic test Charge and discharge tests were performed on the half-cells in Examples 1 to 5 and Comparative Examples 1 to 5 at a voltage of 0V to 1.5V in an environment of 25°C. First, the half-cells in the above Examples and Comparative Examples were cycled once at a charge and discharge current of 0.1C (the charge and discharge voltage range was 0V to 1.5V) in an environment of 25°C to measure the initial discharge capacity and initial coulombic efficiency of the battery, and then the battery was cycled and discharged 50 times at a current of 1C (the charge and discharge cutoff voltage was 0V to 1.5V) to obtain the capacity retention rate of the battery after 50 cycles. Initial coulombic efficiency (%) = initial discharge capacity / initial charge capacity x 100%. The experimental results are shown in Table 1 and Figures 1 and 2 below.
[0072] [Table 1]
[0073] As can be seen from the above test results, the above embodiments of the present invention achieve the following technical effects:
[0074] As a result of comparing the results of Examples 1 to 5 and Comparative Examples 1 to 5, in which the Li2CO3 content and LiOH content relative to the weight of the negative electrode active material particles are not within the range of the present invention, it was revealed that the batteries in Examples 1 to 5, in which the Li2CO3 content relative to the weight of the negative electrode active material particles is more than 0 wt% and less than 0.01 wt%, and the LiOH content is more than 0 wt% and less than 0.01 wt%, have higher initial coulombic efficiency and higher discharge capacity retention rate after 50 cycles, compared to Comparative Examples 1 to 5, in which the Li2CO3 content and LiOH content relative to the weight of the negative electrode active material particles are not within the range of the present invention.
[0075] FIG. 2 shows Li 1s XPS (X-ray photoelectron spectrum) maps of the negative electrode composite materials in Examples 1-2, Comparative Example 2, and Comparative Example 4. The XPS maps show a comparison of the amount of lithium carbonate Li2CO3, which is one of the components of residual lithium, in the negative electrode composite materials in Examples 1-2, Comparative Example 2, and Comparative Example 4. From FIG. 2, it is clear that there is no Li2CO3 peak in the XPS map of the negative electrode composite materials in Examples 1-2. This indicates that the amount of Li2CO3 in the negative electrode composite materials in Examples 1-2 does not reach the amount required for the XPS test.
[0076] As a result of comparing the results of Example 1 and Comparative Example 4, it was found that the prelithiated SiO x It was found that by washing the material, a negative electrode composite material with extremely low Li2CO3 content and extremely low LiOH content was obtained, which significantly reduced the amount of residual lithium, significantly improved the processability of the slurry, and improved the initial discharge capacity, initial coulombic efficiency, and discharge capacity retention rate after 50 cycles of the battery. Figure 1 shows a photograph of the appearance of the negative electrode slurry in Comparative Example 4. From Figure 1, it can be seen that the negative electrode slurry in Comparative Example 4 became gelled due to the high amount of residual lithium in the negative electrode composite material.
[0077] Comparing the results of Example 2 and Comparative Example 3, it is clear that when the cleaning treatment includes ultrasonicating the second mixture, a negative electrode composite material having extremely low Li2CO3 content and extremely low LiOH content can be obtained, which can reduce the amount of residual lithium, significantly improve the processability of the slurry, and improve the first discharge capacity, first coulombic efficiency, and discharge capacity retention rate after 50 cycles of the battery.
[0078] Comparing the results of Example 4 and Comparative Example 1, it was found that when the temperature of the second heat treatment is in the range of 925°C to 1050°C, a negative electrode composite material having an extremely low Li2CO3 content and an extremely low LiOH content can be obtained, thereby reducing the amount of residual lithium, significantly improving the processability of the slurry, and improving the initial discharge capacity, initial coulombic efficiency, and discharge capacity retention rate after 50 cycles of the battery.
[0079] As can be seen from the above battery characteristic test results, the anode composite material, the method for manufacturing the anode composite material, and the anode and lithium ion secondary battery comprising the anode composite material according to the present invention can significantly reduce the amount of residual lithium, significantly improve the processability of the slurry, and improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery.
[0080] The above is merely a preferred embodiment of the present invention, and is not intended to limit the present invention. Those skilled in the art can make various modifications and changes to the present invention. Any modifications, equivalent replacements, improvements, etc. made without departing from the spirit and principle of the present invention should be included in the patent scope of the present invention.
Claims
1. A negative electrode active material particle and Li on the surface of the negative electrode active material particle. 2 CO 3 and LiOH, and the negative electrode active material particles include Silicon oxide and Li 2 SiO 3 and Li 2 S 2 O 5 Granules containing at least one lithium silicate selected from the group consisting of: A carbon coating layer is coated on at least a portion of the surface of the granule, Li based on the weight of the negative electrode active material particles 2 CO 3 % and less than 0.01 wt %, and the content of LiOH is more than 0 wt % and less than 0.01 wt %.
2. The silicon oxide is SiO x 2. The negative electrode composite material according to claim 1, wherein x is 0.5≦x≦1.
6.
3. 3. The negative electrode composite material according to claim 1, wherein the amount of the carbon coating layer is within a range of 1 wt % to 30 wt % based on the weight of the negative electrode active material particles.
4. 3. The negative electrode composite material according to claim 1, wherein the carbon coating layer covers the entire surface of the granule.
5. 1. A method for producing an anode composite material, comprising: performing a carbon coating process on the silicon oxide precursor using a carbon source to form a carbon-coated silicon oxide; combining the carbon coated silicon oxide with a lithium source to form a first mixture, subjecting the first mixture to a first heat treatment to form a calcined product, and thereafter subjecting the calcined product to a second heat treatment to form a prelithiated product; and washing said prelithiated product to form said negative electrode composite material.
6. 6. The method for producing an anode composite material as claimed in claim 5, wherein the washing treatment comprises mixing the prelithiated product with water or acid to a solid content of 2 wt % to 10 wt % to form a second mixture, ultrasonicating the second mixture to disperse it, then suction filtering, and finally drying the material after suction filtering.
7. 7. The method for producing a negative electrode composite material according to claim 6, wherein the acid is at least one selected from hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid, and boric acid.
8. 6. The method for producing an anode composite material according to claim 5, wherein the weight ratio of said lithium source to said carbon-coated silicon oxide ranges from 5:95 to 15:
85.
9. 6. The method for manufacturing an anode composite material as claimed in claim 5, wherein the temperature of the first heat treatment is in the range of 500°C to 750°C, and the time of the first heat treatment is in the range of 2h to 5h.
10. 6. The method for manufacturing an anode composite material as claimed in claim 5, wherein the temperature of the second heat treatment is in the range of 925°C to 1050°C, and the time of the second heat treatment is in the range of 3h to 6h.
11. 7. The method for manufacturing a negative electrode composite material as claimed in claim 6, wherein the ultrasonic treatment time is in the range of 10 min to 30 min.
12. The method for manufacturing an anode composite material as claimed in claim 6, wherein the time of said dispersion is in the range of 24h to 72h.
13. 6. The method for producing an anode composite material of claim 5, wherein the carbon source comprises at least one of an alkane, an alkene, and an alkyne.
14. A negative electrode for a lithium ion secondary battery, comprising the negative electrode composite material according to claim 1 or 2.
15. A lithium ion secondary battery comprising a positive electrode, a negative electrode, and a separator, A lithium ion secondary battery, wherein the negative electrode comprises the negative electrode composite material according to claim 1 or 2.
Citation Information
Patent Citations
Powder for negative electrode of lithium ion secondary battery, and method of manufacturing the same
JP2015153520A
Negative electrode active substance, mixed negative electrode active substance material, and method for manufacturing negative electrode active substance
JP2017188319A
Method of producing negative electrode material
JP2018032603A
Negative electrode material for lithium ion secondary battery, its manufacturing method and use
JP2021521622A
Modified silicon material and manufacturing method, negative electrode material, negative electrode plate, secondary battery, battery module, battery pack, and power consumption device
JP2023547582A
Cited By
Negative electrode composite material, preparation method thereof, negative electrode, and lithium ion secondary battery
JP2024144278A
Anode composite material, lithium ion secondary battery anode, and lithium ion secondary battery
JP7743891B2