Negative electrode composite material, preparation method thereof, negative electrode, and lithium ion secondary battery
A composite negative electrode material with controlled lithium distribution and manufacturing process addresses high residual lithium issues, enhancing slurry processability and improving the efficiency and cycle characteristics of lithium ion secondary batteries.
Patent Information
- Application Number
- JP2024047009
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-03-22
AI Technical Summary
Conventional lithium ion secondary batteries face challenges in improving the initial coulombic efficiency and cycle characteristics due to high residual lithium content in the negative electrode material, which complicates the processability of the slurry.
A negative electrode composite material is developed, comprising silicon oxide particles coated with a carbon layer and specific ratios of lithium compounds (Li2CO3, LiOH, Li2SiO3, and Li2Si2O5), with controlled distribution and optimized content, along with a manufacturing process involving carbon coating, heat treatments, and washing steps to reduce residual lithium.
The solution significantly reduces residual lithium, enhances slurry processability, and improves the initial coulombic efficiency and cycle characteristics of lithium ion secondary batteries.
Smart Images

Figure 2024144278000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of lithium ion secondary batteries, and in particular to an anode composite material, a method for producing the anode composite material, and an anode and a lithium ion secondary battery comprising the anode composite material. [Background technology]
[0002] In recent years, with the development of electronic technology, the demand for battery devices that supply energy to electronic devices is increasing. Currently, there is a demand for batteries that can store more power and output large power. Conventional lead batteries and nickel-metal hydride batteries are no longer able to meet the requirements of new electronic devices such as mobile devices such as smartphones and stationary devices such as power storage systems. Therefore, lithium-ion secondary batteries have attracted attention. In the development of lithium-ion secondary batteries, their capacity and characteristics have been effectively improved. Lithium-ion secondary batteries have advantages such as high energy density, high operating voltage, long cycle life, and little environmental pollution, and have become a new environmentally friendly high-energy chemical power source with potential for development in the current world.
[0003] A lithium ion secondary battery includes a positive electrode, a negative electrode containing a negative electrode material, and an electrolyte. Several types of negative electrode materials have been developed, among which silicon-based negative electrode materials are one of the most promising negative electrode materials. In the prior art, a prelithiation technique is adopted to improve the properties of silicon-based negative electrode materials, and it is disclosed that the amount of residual lithium in the silicon-based negative electrode material is controlled. However, in the prior art, the upper and lower limits of the control of the amount of residual lithium in the silicon-based negative electrode material are high, making it difficult to improve the processability of the slurry containing the negative electrode material, and making it difficult to effectively improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery. Therefore, there is a demand for the development of a new negative electrode composite material, a method for producing this negative electrode composite material, a negative electrode containing this negative electrode composite material, and a lithium ion secondary battery. Summary of the Invention [Problem to be solved by the invention]
[0004] The main objective of the present invention is to provide an anode composite material, a method for manufacturing the anode composite material, and an anode and a lithium ion secondary battery comprising the anode composite material, in order to solve the problems in the prior art that the residual lithium content of the anode material is too high, it is difficult to improve the processability of the slurry, and it is difficult to effectively improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery. [Means for solving the problem]
[0005] In order to achieve the above object, according to one aspect of the present invention, Provided is a negative electrode composite material comprising: negative electrode active material particles; and Li2CO3 and LiOH on the surfaces of the negative electrode active material particles, the negative electrode active material particles comprising granules containing silicon oxide, Li2SiO3, and Li2Si2O5; and a carbon coating layer coating at least a portion of the surface of the granules, the Li2CO3 content being more than 0.01 wt% and less than 1 wt%, the LiOH content being more than 0.001 wt% and less than 0.1 wt%, and a weight ratio of Li2Si2O5 to Li2SiO3, Li2Si2O5 / Li2SiO3, in the range of 1.00 to 10.00, based on the weight of the negative electrode active material particles.
[0006] Furthermore, in the negative electrode composite material, the content of Li2SiO3 is more than 1.0 wt% and less than 48.0 wt% based on the weight of the negative electrode active material particles.
[0007] Furthermore, in the negative electrode composite material, Li2SiO3 is distributed within a granule so that the amount of Li2SiO3 decreases from a position close to the surface of the granule toward the center of the granule, and Li2Si2O5 is distributed closer to the center of the granule than Li2SiO3.
[0008] Furthermore, in the negative electrode composite material, the carbon coating layer covers the entire surface of the granule.
[0009] Furthermore, in the negative electrode composite material, the silicon oxide is SiOx (0.5≦x≦1.6).
[0010] Furthermore, in the negative electrode composite material, the silicon in the silicon oxide is present in the form of crystalline silicon having a size in the range of 5.0 nm to 12.0 nm.
[0011] Furthermore, in the negative electrode composite material, the intensity ratio I of the D peak to the G peak in the Raman spectrum of the negative electrode composite material D / I G is more than 0.8 and less than 2.0, preferably more than 1.5 and less than 1.8.
[0012] Furthermore, in the negative electrode composite material, the coating amount of the carbon coating layer is in the range of 1 wt % to 30 wt % based on the weight of the negative electrode active material particles.
[0013] According to another aspect of the present invention, there is provided a method for producing an anode composite material, comprising the steps of: performing a carbon coating process on the silicon oxide precursor using a carbon source to form a carbon-coated silicon oxide; combining the carbon-coated silicon oxide with a lithium source to form a first mixture, subjecting the first mixture to a first heat treatment to form a calcined product, and thereafter subjecting the calcined product to a second heat treatment to form a prelithiated product; and washing the prelithiated product to form a negative electrode composite material.
[0014] Furthermore, in the method for producing the anode composite material, the washing process includes mixing the prelithiated product with water, alcohol or acid, preferably with a solid content of 5 wt% to 20 wt%, to form a second mixture, ultrasonicating the second mixture, dispersing it, then suction filtering, and finally drying the material after suction filtering.
[0015] Furthermore, in the method for producing the negative electrode composite material, the acid is at least one selected from hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid, and boric acid.
[0016] Furthermore, in the method for producing the negative electrode composite material, the weight ratio of the lithium source to the carbon-coated silicon oxide ranges from 5:95 to 40:60.
[0017] Furthermore, in the method for producing the negative electrode composite material, the temperature of the first heat treatment is in the range of 400° C. to 750° C., and the time of the first heat treatment is in the range of 1 hour to 5 hours.
[0018] Furthermore, in the method for producing the negative electrode composite material, the temperature of the second heat treatment is in the range of 800° C. or more and less than 925° C., and the time of the second heat treatment is in the range of 1 hour to 6 hours.
[0019] Furthermore, in the method for producing the negative electrode composite material, the ultrasonic treatment time is in the range of 1 min to 30 min.
[0020] Furthermore, in the method for producing the negative electrode composite material, the dispersion time is in the range of 8h to 48h.
[0021] Further, in the method for producing the anode composite material, the carbon source includes at least one of an alkane, an alkene, and an alkyne.
[0022] Furthermore, in the method for producing the negative electrode composite material, the alcohol is at least one selected from ethanol, isopropanol, and butanol.
[0023] According to a further aspect of the present invention, there is provided a lithium ion secondary battery anode comprising the anode composite material described above.
[0024] According to a further aspect of the present invention, there is provided a lithium ion secondary battery comprising a positive electrode, a negative electrode, and a separator, the negative electrode comprising the above-described negative electrode composite material.
[0025] The negative electrode composite material of the present invention, the method for producing the negative electrode composite material, and the negative electrode and lithium ion secondary battery including the negative electrode composite material can significantly reduce the amount of residual lithium, improve the processability of the slurry, and improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery. [Brief description of the drawings]
[0026] [Figure 1] FIG. 2 shows a schematic structural diagram of an anode composite material according to one embodiment of the present invention. [Diagram 2] FIG. 1 shows a relationship diagram between the size of crystalline silicon in the negative electrode composite materials of Examples 1 to 10 and Comparative Examples 1 to 3, 5, 7, and 9 and the weight ratio of Li2Si2O5 to Li2SiO3, Li2Si2O5 / Li2SiO3, where the ordinate is the size of crystalline silicon in the negative electrode composite material and the abscissa is the weight ratio of Li2Si2O5 to Li2SiO3, Li2Si2O5 / Li2SiO3. [Diagram 3] FIG. 1 shows a relationship diagram between the discharge capacity retention rate (%) after 50 cycles and the intensity ratio ID / IG of the D peak to the G peak in the Raman spectrum of the negative electrode composite material for Examples 1 to 8 and Comparative Examples 1, 3, 4, 6, 8, and 9, where the ordinate is the discharge capacity retention rate (%) after 50 cycles and the abscissa is the intensity ratio ID / IG of the D peak to the G peak in the Raman spectrum of the negative electrode composite material. [Figure 4] 1 shows Li 1s XPS (X-ray photoelectron spectrum) spectra at each etching depth in Example 2. [Diagram 5] 1 shows Li 1s XPS (X-ray photoelectron spectrum) spectra at each etching depth in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] It should be noted that the various embodiments and features of the embodiments of the present application may be combined with each other without contradiction. The present invention will be described in detail below with reference to the following examples. The following examples are merely illustrative and do not limit the scope of protection of the present invention.
[0028] As described in the background art, in the prior art, the residual lithium content of the negative electrode material is too high, and it is difficult to improve the processability of the slurry containing the negative electrode material, and it is difficult to effectively improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery. In response to the problems in the prior art, a representative embodiment of the present invention provides a negative electrode composite material comprising: negative electrode active material particles; Li2CO3 and LiOH on the surface of the negative electrode active material particles; the negative electrode active material particles comprise granules containing silicon oxide, Li2SiO3 and Li2Si2O5; and a carbon coating layer coated on at least a part of the surface of the granules; the content of Li2CO3 is more than 0.01 wt% and less than 1 wt%, the content of LiOH is more than 0.001 wt% and less than 0.1 wt%, and the weight ratio of Li2Si2O5 to Li2SiO3, Li2Si2O5 / Li2SiO3, is in the range of 1.00 to 10.00, based on the weight of the negative electrode active material particles.
[0029] A high residual lithium value affects the processability of the slurry containing the negative electrode composite material, and the slurry is easily turned into "jelly" during the process of preparing the slurry using the negative electrode composite material. In the prior art, the influence of the distribution of lithium-containing compounds and the weight ratio Li2Si2O5 / Li2SiO3 of Li2Si2O5 to Li2SiO3 on the control of residual lithium has not been clarified. The inventors have unexpectedly found, after many experiments, that by designing the distribution of lithium-containing compounds in the negative electrode composite material and adjusting the weight ratio Li2Si2O5 / Li2SiO3 of Li2Si2O5 to Li2SiO3, not only can the size of crystalline silicon be adjusted, but also it is favorable for the control and optimization of residual lithium, and the amount of residual lithium can be greatly reduced, and the "jelly" of the slurry can be avoided during the process of preparing the slurry using the negative electrode composite material, the processability of the slurry can be improved, and the initial coulombic efficiency and cycle characteristics of the lithium-ion secondary battery can be improved. Therefore, the negative electrode composite material of the present invention can significantly reduce the amount of residual lithium, improve the processability of the slurry, and improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery.
[0030] In some embodiments of the present invention, the content of Li2SiO3 in the anode composite material of the present invention is more than 1.0wt% and less than 48.0wt% based on the weight of the anode active material particles. In the prior art, the control of the amount of water-soluble Li2SiO3 is not clear, and the effect of the amount of water-soluble Li2SiO3 on the electrochemical properties has not been thoroughly studied. The present inventors unexpectedly found that by making the content of Li2SiO3 in the above range, it is possible to ensure the acquisition of a sufficiently prelithiated anode composite material, and also improve the initial coulombic efficiency and cycle properties of the lithium-ion secondary battery.
[0031] In some embodiments of the present invention, in the anode composite material of the present invention, Li2SiO3 is distributed in the granule so that the amount of Li2SiO3 decreases from the surface of the granule toward the center of the granule, and Li2Si2O5 is distributed closer to the center of the granule than Li2SiO3. The distribution of water-soluble Li2SiO3 and water-insoluble Li2Si2O5 in the anode composite material is advantageous for controlling and optimizing the residual lithium, greatly reducing the amount of residual lithium, improving the processability of the slurry, and improving the initial coulombic efficiency and cycle characteristics of the lithium-ion secondary battery. Figure 1 shows a structural schematic diagram of an anode composite material according to one embodiment of the present invention.
[0032] In some embodiments of the present invention, in the negative electrode composite material of the present invention, the carbon coating layer may be coated on the entire surface of the granule, which can improve the electrical conductivity of the negative electrode composite material, increase the initial coulombic efficiency, more effectively reduce the amount of residual lithium, and improve the processability of the slurry.
[0033] The silicon oxide in the present application may be any silicon oxide commonly used in a negative electrode material in the field. In some embodiments of the present invention, the silicon oxide in the negative electrode composite material of the present invention is SiO x (0.5≦x≦1.6, preferably 0.8≦x≦1.2, and most preferably x=1.0).
[0034] In some embodiments of the present invention, in the negative electrode composite material of the present invention, silicon in the silicon oxide is present in the form of crystalline silicon having a size in the range of 5.0 nm to 12.0 nm, preferably in the range of 5.0 nm to 11.5 nm. By setting the size of the crystalline silicon in the above range, the volume expansion of the negative electrode composite material can be reduced, excellent cycle characteristics can be obtained, and the amount of residual lithium in the negative electrode composite material can be reduced while improving the cycle characteristics of the lithium ion secondary battery.
[0035] In some embodiments of the present invention, in the negative electrode composite material of the present invention, the intensity ratio I of the D peak to the G peak in the Raman spectrum of the negative electrode composite material is D / I G is more than 0.8 and less than 2.0, preferably more than 1.5 and less than 1.8. D / I G By setting the above range, the electrical conductivity of the carbon coating layer can be improved, and the lithium ion secondary battery can have excellent cycle characteristics. -1 ) and G band (~1580cm -1 ) peak intensity I D and I G are obtained by Raman spectroscopy. The Raman instrument used is, for example, a Renishaw Qontor model, and the wavenumber range used is, for example, 100 to 1800 cm -1 and the laser wavelength used is, for example, 532 nm.
[0036] In some embodiments of the present invention, the coating amount of the carbon coating layer is in the range of 1 wt% to 30 wt%, preferably in the range of 3 wt% to 20 wt%, and more preferably in the range of 5 wt% to 10 wt%, based on the weight of the negative electrode active material particles in the negative electrode composite material of the present invention. By setting the coating amount of the carbon coating layer in the above range, a good balance between the capacity of the material and the coating uniformity can be achieved.
[0037] In another exemplary embodiment of the present invention, a method for producing an anode composite material is provided, the method including: performing a carbon-coating process on a silicon oxide precursor with a carbon source to form a carbon-coated silicon oxide; mixing the carbon-coated silicon oxide with a lithium source to form a first mixture, performing a first heat treatment on the first mixture to form a calcined product, and then performing a second heat treatment on the calcined product to form a prelithiated product; and washing the prelithiated product to form the anode composite material.
[0038] The method for producing the anode composite material of the present invention is advantageous in controlling and optimizing the residual lithium, greatly reducing the amount of residual lithium, avoiding the "jelly" of the slurry during the process of producing the slurry using the anode composite material, improving the processability of the slurry, improving the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery, and inhibiting gas generation by the slurry. The anode composite material obtained by the above method of the present invention has an extremely low amount of residual lithium, improves the processability of the slurry, and improves the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery.
[0039] The silicon oxide precursor in the present invention, for example, SiO x(0.5≦x≦1.6) can be prepared by a conventional method in the field. In some embodiments of the present invention, the silicon oxide precursor can be prepared by the following steps. Mix silicon powder and silica of a predetermined particle size in a molar ratio of about 1.1:1, then place in a vibrator to vibrate for about 12h to mix uniformly, and press about 1kg of the above uniformly mixed material into a block, then place the block in a vacuum sublimation furnace to heat to a temperature of 1200°C to 1500°C, adjust the vacuum degree to 0-30Pa, the heating time to 8h-10h, and the temperature at the collection end to 400°C to 800°C to prepare a lump silicon oxide precursor, put the lump silicon oxide precursor into a crusher to crush it to millimeter scale, then put the millimeter-scale silicon oxide precursor into a jet mill to crush it, classify the powders with different particle sizes by an air flow classifier, and finally blend the powders with different particle sizes according to size, and finally obtain a silicon oxide precursor with a desired particle size.
[0040] In some embodiments of the present invention, in the method for producing the above-mentioned negative electrode composite material, the silicon oxide precursor is carbon-coated by chemical vapor deposition at a pressure of 50 Pa to 10,000 Pa and a temperature of 600° C. to 1,000° C. using at least one of an alkane, an alkene, and an alkyne as a carbon source, to form a carbon-coated silicon oxide. In some embodiments of the present invention, the carbon coating is performed in an apparatus such as a rotary kiln, a fixed bed, or a fluidized bed.
[0041] In some embodiments of the present invention, in the method for producing the anode composite material, the washing process includes mixing the prelithiated product with water, alcohol or acid, preferably to a solid content of 5 wt% to 20 wt%, for example 5 wt% to 10 wt%, 10 wt% to 15 wt%, or 15 wt% to 20 wt%, to form a second mixture, ultrasonicating the second mixture, then dispersing, then suction filtering, and finally drying the material after suction filtering. In the washing process, when water is used, alkaline materials such as Li2CO3, LiOH, and Li2SiO3 are dissolved, when alcohol is used, LiOH is slightly dissolved, and when acid is used, the alkali generated on the surface of the prelithiated product during washing can be neutralized. By ultrasonication, the prelithiated product can be washed more reliably, a good washing effect can be ensured, and the cycle characteristics of the lithium-ion secondary battery can be improved. The washing process can greatly reduce the amount of residual lithium, avoid the "jelly" of the slurry during the process of preparing the slurry using the negative electrode composite material, improve the processability of the slurry, and further improve the initial coulombic efficiency and cycle characteristics of the lithium-ion secondary battery. Because Li2Si2O5 is insoluble in water and Li2SiO3 is soluble in water, the washing process can also adjust the weight ratio of Li2Si2O5 to Li2SiO3, Li2Si2O5 / Li2SiO3.
[0042] In some embodiments of the present invention, the prelithiated product produced, e.g., prelithiated SiO x (0.5≦x≦1.6) The material is mixed with water to a solid content of 5wt%-20wt% to form a second mixture, the second mixture is ultrasonically treated at room temperature for 1min-30min, and then the second mixture is dispersed using a magnetic stirrer for 8h-48h, and then suction filtered. After that, pure water is poured onto the material on the filter paper, and washed twice by suction filtration. Finally, the material after suction filtration is vacuum dried at 100℃-120℃ for 3-8 hours.
[0043] In some embodiments of the present invention, in the method for producing the anode composite material, the acid is at least one selected from hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid, and boric acid, in order to better neutralize the alkali generated on the surface of the prelithiated product during washing.
[0044] In some embodiments of the present invention, the prelithiated product produced, e.g., prelithiated SiO x (0.5≦x≦1.6) The material is mixed with at least one of hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid, and boric acid, for example, citric acid with a concentration of 1 mol / L, so that the solid content is 5 wt% to 20 wt%, to form a second mixture, and the second mixture is ultrasonically treated at room temperature for 1 min to 30 min, and then the second mixture is dispersed using a magnetic stirrer for 8 h to 48 h, and then suction filtered, and then pure water is poured onto the material on the filter paper, and it is washed twice by suction filtration, and finally, the material after suction filtration is vacuum dried at 100°C to 120°C for 3 to 8 hours.
[0045] In some embodiments of the present invention, in the method for producing the negative electrode composite material, the weight ratio of the lithium source to the carbon-coated silicon oxide is in the range of 5:95 to 40:60. By setting the weight ratio of the lithium source to the carbon-coated silicon oxide in the above range, it is possible to ensure sufficient prelithiation of the silicon oxide, reduce the amount of residual lithium, and further improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery. In some embodiments of the present invention, the lithium source may include any of lithium ingot, lithium metal powder, and lithium foil.
[0046] In some embodiments of the present invention, in the method for producing the negative electrode composite material, the temperature of the first heat treatment is in the range of 400°C to 750°C, and the time of the first heat treatment is in the range of 1h to 5h. By setting the temperature and time of the first heat treatment in the above ranges, it is possible to ensure sufficient prelithiation of the silicon oxide, reduce the amount of residual lithium, and further improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery.
[0047] In some embodiments of the present invention, in the method for preparing the negative electrode composite material, the temperature of the second heat treatment is in the range of 800°C or more and less than 925°C, and the time of the second heat treatment is in the range of 1h to 6h. By setting the temperature and time of the second heat treatment in the above range, it is possible to ensure sufficient prelithiation of silicon oxide, to avoid the size of crystalline silicon being too large, to greatly reduce the amount of residual lithium, and to further improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery.
[0048] In some embodiments of the present invention, under the protection of inert atmosphere argon, the lithium source and the carbon-coated silicon oxide are ground and mixed in a weight ratio of 5:95-40:60 to form a first mixture, then the first mixture is put into a rotary kiln and calcined for 1h-5h at 400℃-750℃ under argon atmosphere to fully react the carbon-coated silicon oxide with lithium metal, and then heat-treated at 800℃-924℃ for 1h-6h, thereby adjusting the prelithiation depth and the amount of lithium-containing silicate to obtain a prelithiation product.
[0049] In some embodiments of the present invention, in the method for preparing the negative electrode composite material, the ultrasonic treatment time is in the range of 1 min to 30 min. By setting the ultrasonic treatment time in the above range, the prelithiation product can be sufficiently washed, and the damage to the granules of the prelithiation product can be avoided while ensuring a good washing effect.
[0050] In some embodiments of the present invention, in the method for producing the negative electrode composite material, the dispersion time may be in the range of 8h to 48h, mainly considering energy consumption, time cost and cleaning effect. If the dispersion time is too short, cleaning may be insufficient, and if the dispersion time is too long, energy consumption is high and time is required. By setting the dispersion time in the above range, not only can a good cleaning effect be ensured, but also energy consumption and time cost can be reduced.
[0051] In some embodiments of the present invention, in the method for producing the negative electrode composite material, in order to better carbon-coat at least a part of the surface of the silicon oxide and obtain a good coating effect, the carbon source comprises at least one of an alkane, an alkene, and an alkyne.
[0052] In some embodiments of the present invention, in the method for manufacturing the negative electrode composite material, the alcohol may be at least one selected from ethanol, isopropanol, and butanol, thereby obtaining a better cleaning effect. The alcohol is preferably ethanol, which slightly dissolves LiOH. When ethanol is used for cleaning, ethanol is easy to volatilize, which is advantageous for drying in the subsequent step. Water is generally contained in ethanol, and the water contained in ethanol can dissolve alkaline substances such as Li2CO3, LiOH, and Li2SiO3. As the ethanol, ethanol with a concentration of 75% is usually used.
[0053] In some embodiments of the present invention, the prelithiated product produced, e.g., prelithiated SiO x(0.5≦x≦1.6) The material is mixed with at least one of ethanol, isopropanol, butanol, etc. to a solid content of 5 wt% to 20 wt% to form a second mixture, and the second mixture is ultrasonically treated at room temperature for 1 min to 30 min, and then the second mixture is dispersed using a magnetic stirrer for 8 h to 48 h, and then suction filtered. After that, pure water is poured onto the material on the filter paper, and washed twice by suction filtration. Finally, the material after suction filtration is vacuum dried at 100°C to 120°C for 3 to 8 hours.
[0054] In a further exemplary embodiment of the present invention, a lithium ion secondary battery negative electrode is provided, which comprises the above-mentioned negative electrode composite material. The lithium ion secondary battery negative electrode of the present invention comprises the above-mentioned negative electrode composite material, which can significantly reduce the amount of residual lithium, improve the processability of the slurry, and improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery.
[0055] The negative electrode plate of the present invention can be prepared by a conventional method in the art. For example, the negative electrode composite material of the present invention, the conductive agent, and the binder are dispersed in water as a solvent to form a uniform negative electrode slurry, and the negative electrode slurry is applied onto the negative electrode collector fluid and baked to obtain a negative electrode plate. The conductive agent can be conductive carbon black, conductive graphite, vapor-grown carbon fiber, carbon nanotubes, or any combination thereof. The binder can be one or more of styrene butadiene rubber (SBR), polyacrylic acid (PAA), polyimide (PI), etc., and is preferably a polyacrylic acid (PAA) binder.
[0056] In a further exemplary embodiment of the present invention, a lithium ion secondary battery is provided, comprising a positive electrode, a negative electrode, and a separator, the negative electrode comprising the above-mentioned negative electrode composite material. Since the lithium ion secondary battery of the present invention comprises the above-mentioned negative electrode composite material, the amount of residual lithium can be significantly reduced, the processability of the slurry can be improved, and the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery can be improved.
[0057] The positive electrode of the present invention includes a positive electrode current collector and a positive electrode active material layer containing a positive electrode active material. The positive electrode active material layer is formed on two surfaces of the positive electrode current collector. As the positive electrode current collector, for example, a metal foil such as an aluminum foil, a nickel foil, or a stainless steel foil can be used.
[0058] The positive electrode active material layer may contain one or more positive electrode materials capable of occluding and releasing lithium ions as the positive electrode active material, and optionally, other materials such as a positive electrode binder and / or a positive electrode conductive agent may be included.
[0059] Preferably, the positive electrode material is a lithium-containing compound. Examples of such lithium-containing compounds include lithium-transition metal composite oxides and lithium-transition metal phosphate compounds. The lithium-transition metal composite oxide is an oxide containing Li and one or more transition metal elements as constituent elements, and the lithium-transition metal phosphate compound is a phosphate compound containing Li and one or more transition metal elements as constituent elements. One or more of Co, Ni, Mn, Fe, etc. are suitable as the transition metal element.
[0060] Examples of the lithium-transition metal composite oxide may include, for example, LiCoO2 and LiNiO2. Examples of the lithium-transition metal phosphate compound may include, for example, LiFePO4 and LiFe 1-u Mn u PO4 (0 < u < 1), etc. may be included.
[0061] The negative electrode of the present invention includes a negative electrode current collector and a negative electrode active material layer containing a negative electrode composite material. The negative electrode active material layer is formed on two surfaces of the negative electrode current collector. As the negative electrode current collector, for example, a metal foil such as a copper (Cu) foil, a carbon-coated copper foil, a nickel foil, or a stainless steel foil can be used.
[0062] The separator of the present invention separates the positive and negative electrodes of a battery, and allows lithium ions to pass through while preventing current short circuit caused by contact between the positive and negative electrodes. The separator is, for example, a porous film made of synthetic resin or ceramic, and may also be a laminated film made by laminating two or more types of porous films. Examples of synthetic resins include, for example, polytetrafluoroethylene, polypropylene, and polyethylene.
[0063] In an embodiment of the present invention, when charging a lithium ion secondary battery, for example, lithium ions are released from the positive electrode and embedded in the negative electrode via the electrolyte soaked in the separator. When discharging a lithium ion secondary battery, for example, lithium ions are released from the negative electrode and embedded in the positive electrode via the electrolyte soaked in the separator.
[0064] The present application will now be described in more detail with reference to specific examples, which do not limit the scope of the protection claimed by the present application.
[0065] Example 1 Manufacture of anode composite material At a pressure of 50 Pa and a temperature of 920 °C, methane was used as the carbon source to produce the silicon oxide precursor SiO x (x=1) Silicon oxide precursor SiO is deposited by chemical vapor deposition on the surface of 20 g of material. x (x=1) The material is carbon-coated, and the carbon-coated SiO x (x=1) 21 g of material was formed.
[0066] Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 20:80 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 500 °C under an argon atmosphere for 3 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 850 °C for 3 h to obtain prelithiated SiO x Got the material.
[0067] Produced prelithiated SiO x The material and 1 mol / L hydrochloric acid were placed in a beaker to give a solid content of 5 wt%, and mixed to form a second mixture. The second mixture was ultrasonically treated at room temperature for 30 minutes, and then dispersed using a magnetic stirrer for 48 hours. It was then suction filtered, and then pure water was poured onto the material on the filter paper, and it was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material.
[0068] Manufacture of negative electrode pieces 4 g of the negative electrode composite material produced by the above process was weighed out, and the negative electrode composite material, conductive carbon black Super-P as a conductive agent, and polyacrylic acid PAA as a binder were mixed in a mass ratio of 82:8:10 with an appropriate amount of deionized water by sufficient stirring, and the solid content was adjusted to 42 wt % to form a uniform negative electrode slurry. Thereafter, the negative electrode slurry was applied onto the surface of copper foil as a negative electrode collector, and dried to obtain a negative electrode plate.
[0069] Battery Assembly The produced negative electrode plate, separator, lithium sheet, gasket, and battery case were stacked in this order, 100 μl of electrolyte was poured into the battery, and the battery was sealed with a sealing machine to assemble the desired half cell.
[0070] Example 2 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 15:85 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 450 °C under an argon atmosphere for 3 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 900°C for 4 hours to produce prelithiated SiO x Obtaining materials, Produced prelithiated SiO xThe material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 5 wt%, and the second mixture was ultrasonically treated at room temperature for 10 minutes. The second mixture was then dispersed for 48 hours using a magnetic stirrer. It was then suction filtered. Then, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0071] Example 3 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 10:90 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600 °C under an argon atmosphere for 2 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 920°C for 5 hours to produce prelithiated SiO x Obtaining materials, Produced prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 15 wt%, and the second mixture was ultrasonically treated at room temperature for 5 minutes. The second mixture was then dispersed using a magnetic stirrer for 16 hours, and then suction filtered. After that, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0072] Example 4 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 5:95 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 400 °C under an argon atmosphere for 1 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 924°C for 6 hours to produce prelithiated SiO xObtaining materials, Produced prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 20 wt%, and the second mixture was ultrasonically treated at room temperature for 1 min. The second mixture was then dispersed using a magnetic stirrer for 8 h. The mixture was then filtered by suction. After that, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0073] Example 5 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 25:75 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600 °C under an argon atmosphere for 4 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 850°C for 2 hours to produce prelithiated SiO x Other than obtaining the materials, Produced prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 5 wt%, and the second mixture was ultrasonically treated at room temperature for 20 minutes. The second mixture was then dispersed using a magnetic stirrer for 36 hours. The mixture was then filtered by suction. After that, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0074] Example 6 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 30:70 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600 °C under an argon atmosphere for 5 h to produce a carbon-coated SiO xThe material was allowed to react sufficiently with lithium metal, and then heat-treated at 820°C for 2 hours to obtain prelithiated SiO x Obtaining materials, Produced prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 10 wt%, and the second mixture was ultrasonically treated at room temperature for 30 minutes. The second mixture was then dispersed using a magnetic stirrer for 40 hours. The mixture was then filtered by suction. After that, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0075] Example 7 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 40:60 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 750 °C under an argon atmosphere for 5 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 800 °C for 1 h to obtain prelithiated SiO x Obtaining materials, Produced prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 5 wt%, and the second mixture was ultrasonically treated at room temperature for 30 minutes. The second mixture was then dispersed for 48 hours using a magnetic stirrer. It was then suction filtered. Then, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0076] Example 8 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x(x=1) material and (x=2) material were ground and mixed in a weight ratio of 20:80 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 550 °C under an argon atmosphere for 4 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 900°C for 5 hours to produce prelithiated SiO x Obtaining materials, Produced prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 10 wt%, and the second mixture was ultrasonically treated at room temperature for 10 minutes. The second mixture was then dispersed for 24 hours using a magnetic stirrer. It was then suction filtered. Then, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0077] Example 9 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 30:70 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600 °C under an argon atmosphere for 5 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 820°C for 2 hours to obtain prelithiated SiO x Obtaining materials, Produced prelithiated SiO x The material and 75% ethanol were put into a beaker so that the solid content was 5 wt%, and mixed to form a second mixture. The second mixture was ultrasonically treated at room temperature for 30 minutes, and then dispersed with a magnetic stirrer for 40 hours. Then, the second mixture was suction filtered. Then, pure water was poured onto the material on the filter paper, and washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0078] Example 10 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 30:70 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600 °C under an argon atmosphere for 5 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 820°C for 2 hours to obtain prelithiated SiO x Obtaining materials, Produced prelithiated SiO x The material and pure water were put into a beaker so that the solid content was 5 wt%, and mixed to form a second mixture. The second mixture was ultrasonically treated at room temperature for 30 minutes, and then the second mixture was dispersed using a magnetic stirrer for 48 hours. Then, it was suction filtered. Then, pure water was poured onto the material on the filter paper, and it was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0079] Comparative Example 1 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 50:50 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 750 °C under an argon atmosphere for 5 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 800 °C for 1 h to obtain prelithiated SiO x Obtaining materials, Produced prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 5 wt%, and the second mixture was ultrasonically treated at room temperature for 30 minutes. The second mixture was then dispersed for 48 hours using a magnetic stirrer. It was then suction filtered. Then, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0080] Comparative Example 2 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 40:60 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 750 °C under an argon atmosphere for 5 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 800 °C for 1 h to obtain prelithiated SiO x Obtaining materials, Prelithiated SiO x The material was prelithiated with SiO x A half cell was fabricated in the same manner as in Example 1, except that the material was used as the negative electrode composite material.
[0081] Comparative Example 3 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 5:95 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 400 °C under an argon atmosphere for 1 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 1000°C for 6 hours to produce prelithiated SiO x Obtaining materials, Produced prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 20 wt%, and the second mixture was ultrasonically treated at room temperature for 1 min. The second mixture was then dispersed using a magnetic stirrer for 8 h. The mixture was then filtered by suction. After that, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0082] Comparative Example 4 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x(x=1) material and (x=2) material were ground and mixed in a weight ratio of 5:95 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 350°C under an argon atmosphere for 1 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 924°C for 6 hours to produce prelithiated SiO x Obtaining materials, Produced prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 20 wt%, and the second mixture was ultrasonically treated at room temperature for 1 min. The second mixture was then dispersed using a magnetic stirrer for 8 h. The mixture was then filtered by suction. After that, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0083] Comparative Example 5 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 30:70 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 600 °C under an argon atmosphere for 5 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 820°C for 2 hours to obtain prelithiated SiO x Obtaining materials, Produced prelithiated SiO x The material and pure water were placed in a beaker so that the solid content was 5 wt%, and mixed to form a second mixture. The second mixture was dispersed at room temperature using a magnetic stirrer for 48 hours, and then suction filtered. After that, pure water was poured onto the material on the filter paper, and washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours to obtain a negative electrode composite material. A half cell was manufactured in the same manner as in Example 1.
[0084] Comparative Example 6 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiOx (x=1) material and the SiO2 material were ground and mixed in a weight ratio of 2:98 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 400 °C under an argon atmosphere for 1 h to produce a carbon-coated SiO2 material. x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 924°C for 6 hours to produce prelithiated SiO x Obtaining materials, Produced prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 20 wt%, and the second mixture was ultrasonically treated at room temperature for 1 min. The second mixture was then dispersed using a magnetic stirrer for 8 h. The mixture was then filtered by suction. After that, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0085] Comparative Example 7 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 40:60 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 750 °C under an argon atmosphere for 5 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 800 °C for 1 h to obtain prelithiated SiO x Obtaining materials, Produced prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 5 wt%, and the second mixture was ultrasonically treated at room temperature for 40 minutes, and then dispersed using a magnetic stirrer for 48 hours. The second mixture was then suction filtered, and then pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0086] Comparative Example 8 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 5:95 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 400 °C under an argon atmosphere for 0.5 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 924°C for 6 hours to produce prelithiated SiO x Obtaining materials, Produced prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 20 wt%, and the second mixture was ultrasonically treated at room temperature for 1 min. The second mixture was then dispersed using a magnetic stirrer for 8 h. The mixture was then filtered by suction. After that, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0087] Comparative Example 9 Under the protection of an inert argon atmosphere, lithium ingots and carbon-coated SiO x (x=1) material and (x=2) material were ground and mixed in a weight ratio of 5:95 to form a first mixture, and then the first mixture was placed in a rotary kiln and calcined at 400 °C under an argon atmosphere for 1 h to produce a carbon-coated SiO x The material was allowed to react sufficiently with lithium metal, and then heat-treated at 924°C for 7 hours to produce prelithiated SiO x Other than obtaining the materials, Produced prelithiated SiO x The material and 1 mol / L hydrochloric acid were mixed in a beaker to obtain a solid content of 20 wt%, and the second mixture was ultrasonically treated at room temperature for 1 min. The second mixture was then dispersed using a magnetic stirrer for 8 h. The mixture was then filtered by suction. After that, pure water was poured onto the material on the filter paper, and the material was washed twice by suction filtration. Finally, the material after suction filtration was vacuum dried at 120°C for 8 hours. A half cell was manufactured in the same manner as in Example 1, except that a negative electrode composite material was obtained.
[0088] Material property testing Tests were performed on the negative electrode composite materials in Examples 1 to 10 and Comparative Examples 1 to 9. D / I G The results of Li2CO3 content, LiOH content, Li2SiO3 content, weight ratio of Li2Si2O5 to Li2SiO3 Li2Si2O5 / Li2SiO3, and size of crystalline silicon were obtained.
[0089] The mass percentages of Li2Si2O5 and Li2SiO3 were calculated from the XRD (Druker Advanced D8) test results, and the weight ratios of Li2Si2O5 and Li2SiO3, Li2Si2O5 / Li2SiO3, were obtained.
[0090] The Li2SiO3 content was calculated from the XRD patterns.
[0091] The size of the crystalline silicon was calculated from the XRD (Druker Advanced D8) test results (calculated from the half-width of the crystalline silicon peak in the XRD spectrum using the Scherrer formula).
[0092] XRD test conditions: 10~80°, 1° / min.
[0093] Neutralization titration method: The negative electrode composite material and pure water were placed in a beaker in a mass ratio of 1:9, mixed, and dispersed in a magnetic stirrer at room temperature for 1 hour, then allowed to stand for 1 hour, and the dispersion was filtered. The resulting 10 mL filtrate was automatically titrated with 0.2 M hydrochloric acid using an automatic acid-alkali titrator, and the first end point (a mL) and second end point (b mL) were determined.
[0094] (Number 1) Li2CO3 content = [pure water volume (g) / filtrate volume (g)] × 2 × (b / 1000) × (equivalent concentration of hydrochloric acid titration × coefficient) × (1 / 2) × (molar mass of Li2CO3) × [100 (%) / sample volume (g)]
[0095] (Number 2) LiOH content = [volume of pure water (g) / volume of filtrate (g)] × [(ab) / 1000] × (equivalent concentration of hydrochloric acid titration amount × coefficient) × (1 / 2) × (molar mass of LiOH) × [100 (%) / volume of sample (g)].
[0096] Battery performance testing Charge and discharge tests were performed on the half-cells in Examples 1 to 10 and Comparative Examples 1 to 9 at a voltage of 0V to 1.5V in an environment of 25°C. First, the half-cells in the above Examples and Comparative Examples were tested by cycling once (the charge and discharge voltage range was 0V to 1.5V) at a charge and discharge current of 0.1C in an environment of 25°C to measure the initial discharge capacity and initial coulombic efficiency of the battery, and then the battery was tested by cycling 50 times (the charge and discharge cutoff voltage was 0V to 1.5V) using a current of 1C to determine the capacity retention rate of the battery after 50 cycles. Initial coulombic efficiency (%) = initial discharge capacity / initial charge capacity x 100%. The experimental results are shown in Table 1 and Figures 2 to 5 below.
[0097] As can be seen from Fig. 2, the crystalline silicon size in the negative electrode composite material and the weight ratio of Li2Si2O5 to Li2SiO3 Li2Si2O5 / Li2SiO3 show a linear relationship. As can be seen from Fig. 3, the intensity ratio I D / I G When the ratio is more than 0.8 and less than 2.0, preferably more than 1.5 and less than 1.8, excellent cycle characteristics were obtained. In Fig. 4 and Fig. 5, the direction from bottom to top is from the surface to the inside. As can be seen from Fig. 4 and Fig. 5, water-soluble Li2CO3 and LiOH are mostly present on the surface of the granules (in Example 2, the signals in the XPS spectrum of the surface are very weak because there is very little Li2CO3 and LiOH), and Li2SiO3 is distributed in the granules so that it decreases from the position close to the surface to the center of the granule. Other lithium silicates (Li2SiO5) that are insoluble in water are distributed closer to the center of the granules than Li2SiO3.
[0098] [Table 1]
[0099] As can be seen from the above test results, the above embodiments of the present invention achieve the following technical effects:
[0100] As a result of comparing the results of Examples 1 to 10 and Comparative Examples 1 to 9, it was clear that the batteries in Examples 1 to 10, in which the Li2CO3 content, the LiOH content, and the weight ratio Li2Si2O5 to Li2SiO3 / Li2Si2O5 based on the weight of the negative electrode active material particles are all not within the range of the present invention, had higher initial coulombic efficiency and higher discharge capacity retention rate after 50 cycles, as compared with Comparative Examples 1 to 9, in which the Li2CO3 content is more than 0.01 wt% and less than 1 wt%, the LiOH content is more than 0.001 wt% and less than 0.1 wt%, and the weight ratio Li2Si2O5 to Li2SiO3 / Li2Si2O5 is in the range of 1.00 to 10.00 based on the weight of the negative electrode active material particles.
[0101] As a result of comparing the results of Examples 1 to 10 with Comparative Example 9, in which the weight ratio Li2Si2O5 / Li2SiO3 of Li2Si2O5 to Li2SiO3 and the Li2SiO3 content based on the weight of the negative electrode active material particles are both outside the range of the present invention, it was revealed that the batteries in Examples 1 to 10, in which the weight ratio Li2Si2O5 / Li2SiO3 of Li2Si2O5 to Li2SiO3 is in the range of 1.00 to 10.00 and the Li2SiO3 content is more than 1.0 wt% and less than 48.0 wt%, have higher initial coulombic efficiency and higher discharge capacity retention rate after 50 cycles, compared to Comparative Example 9, in which the weight ratio Li2Si2O5 / Li2SiO3 of Li2Si2O5 to Li2SiO3 and the Li2SiO3 content based on the weight of the negative electrode active material particles are both within the range of the present invention.
[0102] From the results of Examples 6, 9, and 10, it was revealed that the negative electrode composite material of the present invention can be obtained by the production method of the present invention including the acid washing, alcohol washing, or water washing treatment, and thereby the amount of residual lithium can be significantly reduced, the processability of the slurry can be improved, and the initial coulombic efficiency of the battery and the discharge capacity retention rate after 50 cycles can be improved.
[0103] Comparing the results of Example 7 and Comparative Example 1, it was found that when the weight ratio of the lithium source to the carbon-coated silicon oxide is in the range of 5:95 to 40:60, a negative electrode composite material with an appropriate Li2CO3 content, LiOH content, Li2SiO3 content, and weight ratio of Li2Si2O5 to Li2SiO3, Li2Si2O5 / Li2SiO3, can be obtained, thereby significantly reducing the amount of residual lithium, improving the processability of the slurry, and improving the initial coulombic efficiency of the battery and the discharge capacity retention rate after 50 cycles.
[0104] As a result of comparing the results of Example 7 and Comparative Example 2, it was found that the prelithiated SiO x It was found that by washing the material, anode composite materials with appropriate Li2CO3 content, LiOH content, Li2SiO3 content, and weight ratio of Li2Si2O5 to Li2SiO3, Li2Si2O5 / Li2SiO3, could be obtained, which significantly reduced the amount of residual lithium, improved the processability of the slurry, and increased the initial coulombic efficiency of the battery and the discharge capacity retention rate after 50 cycles.
[0105] Comparing the results of Example 4 and Comparative Example 3, it is found that when the temperature of the second heat treatment is in the range of 800°C or more and less than 925°C, a negative electrode composite material with appropriate LiOH content, Li2SiO3 content, and weight ratio of Li2Si2O5 to Li2SiO3, Li2Si2O5 / Li2SiO3, can be obtained, which can control the size of crystalline silicon and prevent the size of crystalline silicon from being too large, greatly reduce the amount of residual lithium, improve the processability of the slurry, and improve the initial coulombic efficiency of the battery and the discharge capacity retention rate after 50 cycles.
[0106] As a result of comparing the results of Example 4 and Comparative Example 4, it was found that when the temperature of the first heat treatment is in the range of 400°C to 750°C, a negative electrode composite material with an appropriate Li2CO3 content, LiOH content, Li2SiO3 content, and weight ratio of Li2Si2O5 to Li2SiO3, Li2Si2O5 / Li2SiO3, can be obtained, thereby ensuring a good prelithiation effect and improving the initial coulombic efficiency of the battery and the discharge capacity retention rate after 50 cycles. If the temperature of the first heat treatment is too low, prelithiation cannot be performed, and further, the initial coulombic efficiency of the battery may decrease.
[0107] Comparing the results of Example 10 and Comparative Example 5, it was found that when the cleaning treatment included ultrasonic treatment of the second mixture, a negative electrode composite material with an appropriate LiOH content, Li2SiO3 content, and weight ratio of Li2Si2O5 to Li2SiO3, Li2Si2O5 / Li2SiO3, could be obtained, thereby improving the initial coulombic efficiency and the discharge capacity retention rate after 50 cycles of the battery.
[0108] As a result of comparing the results of Example 4 and Comparative Example 6, it was found that when the weight ratio of the lithium source to the carbon-coated silicon oxide is in the range of 5:95 to 40:60, a negative electrode composite material with an appropriate Li2CO3 content, LiOH content, Li2SiO3 content, and weight ratio Li2Si2O5 to Li2SiO3 / Li2SiO3 can be obtained, thereby ensuring a good prelithiation effect and improving the initial coulombic efficiency of the battery and the discharge capacity retention rate after 50 cycles. If the weight ratio of the lithium source to the carbon-coated silicon oxide is too low, prelithiation cannot be performed, lithium silicate cannot be obtained, and the initial coulombic efficiency of the battery may decrease.
[0109] Comparing the results of Example 7 and Comparative Example 7, it was found that when the ultrasonic treatment time is in the range of 1 min to 30 min, a negative electrode composite material with an appropriate weight ratio of Li2Si2O5 to Li2SiO3, Li2Si2O5 / Li2SiO3, can be obtained, thereby preventing the collapse of granules and improving the initial coulombic efficiency of the battery and the discharge capacity retention rate after 50 cycles.
[0110] Comparing the results of Example 4 and Comparative Example 8, it was found that when the first heat treatment time is 1 to 5 hours, a negative electrode composite material with appropriate Li2CO3 content, LiOH content, Li2SiO3 content, and weight ratio of Li2Si2O5 to Li2SiO3, Li2Si2O5 / Li2SiO3, can be obtained, thereby ensuring a good prelithiation effect and improving the initial coulombic efficiency of the battery and the discharge capacity retention rate after 50 cycles.
[0111] Comparing the results of Example 4 and Comparative Example 9, it was found that when the second heat treatment time is in the range of 1 h to 6 h, a negative electrode composite material with an appropriate Li2SiO3 content and weight ratio of Li2Si2O5 to Li2SiO3, Li2Si2O5 / Li2SiO3, can be obtained, thereby controlling the size of crystalline silicon and preventing the size of crystalline silicon from being too large, and improving the initial coulombic efficiency of the battery and the discharge capacity retention rate after 50 cycles.
[0112] It is apparent from the above battery performance test results that the anode composite material of the present invention, the method for producing the anode composite material, and the anode and lithium ion secondary battery including the anode composite material can significantly reduce the amount of residual lithium, improve the processability of the slurry, and improve the initial coulombic efficiency and cycle characteristics of the lithium ion secondary battery.
[0113] The above is merely a preferred embodiment of the present invention, and is not intended to limit the present invention. Those skilled in the art may make various modifications and changes to the present invention. Any modifications, equivalent replacements, improvements, etc. made without departing from the spirit and principles of the present invention shall be included in the patent scope of the present invention.
Claims
1. A negative electrode active material particle and Li on the surface of the negative electrode active material particle. 2 CO 3 and LiOH, and the negative electrode active material particles include Silicon oxide, Li 2 SiO 3 and Li 2 S 2 O 5 Granules comprising: A carbon coating layer is coated on at least a portion of the surface of the granule, Li based on the weight of the negative electrode active material particles 2 CO 3 The content of LiOH is more than 0.001 wt% and less than 0.1 wt%, and the content of LiOH is more than 0.001 wt% and less than 0.1 wt%, and Li 2 S 2 O 5 and Li 2 SiO 3 Weight ratio of Li 2 S 2 O 5 / Li 2 SiO 3 is in the range of 1.00 to 10.
00.
2. Li based on the weight of the negative electrode active material particles 2 SiO 3 The negative electrode composite material according to claim 1, characterized in that the content of is more than 1.0 wt% and less than 48.0 wt%.
3. Li 2 SiO 3 is distributed within the granule so as to decrease from a position close to the surface of the granule toward the center of the granule, and Li 2 S 2 O 5 Li 2 SiO 3 2. The negative electrode composite material according to claim 1, characterized in that the granules are distributed closer to the center than the granules.
4. 2. The negative electrode composite material according to claim 1, wherein the carbon coating layer is applied to the entire surface of the granule.
5. The silicon oxide is SiO x 2. The negative electrode composite material according to claim 1, wherein x is 0.5≦x≦1.
6.
6. 2. The negative electrode composite material of claim 1, wherein the silicon in the silicon oxide is present in the form of crystalline silicon having a size ranging from 5.0 nm to 12.0 nm.
7. The intensity ratio I of the D peak to the G peak in the Raman spectrum of the negative electrode composite material D / I G 2. The negative electrode composite material according to claim 1, wherein the anode composite material has a capacitance of 1.5 or more and a capacitance of 2.0 or less, and more preferably 1.5 or more and a capacitance of 2.0 or less.
8. 2. The negative electrode composite material according to claim 1, wherein the amount of the carbon coating layer is in the range of 1 wt % to 30 wt % based on the weight of the negative electrode active material particles.
9. 1. A method for producing an anode composite material, comprising: performing a carbon coating process on the silicon oxide precursor using a carbon source to form a carbon-coated silicon oxide; combining the carbon-coated silicon oxide with a lithium source to form a first mixture, subjecting the first mixture to a first heat treatment to form a calcined product, and thereafter subjecting the calcined product to a second heat treatment to form a prelithiated product; and washing the prelithiated product to form the negative electrode composite material.
10. 10. The method for manufacturing anode composite material as claimed in claim 9, wherein the washing treatment includes mixing the prelithiated product with water, alcohol or acid to a solid content of 5 wt% to 20 wt% to form a second mixture, ultrasonicating the second mixture, dispersing it, then suction filtering, and finally drying the material after suction filtering.
11. 11. The method for producing a negative electrode composite material according to claim 10, wherein the acid is at least one selected from hydrochloric acid, citric acid, oxalic acid, phosphoric acid, sulfurous acid, acetic acid, chloric acid, hypochlorous acid, and boric acid.
12. 10. The method for producing an anode composite material according to claim 9, wherein the weight ratio of said lithium source to said carbon-coated silicon oxide ranges from 5:95 to 40:
60.
13. 10. The method for manufacturing a negative electrode composite material as claimed in claim 9, wherein the temperature of the first heat treatment is in the range of 400°C to 750°C, and the time of the first heat treatment is in the range of 1h to 5h.
14. 10. The method for manufacturing a negative electrode composite material according to claim 9, wherein the temperature of the second heat treatment is in the range of 800° C. or more and less than 925° C., and the time of the second heat treatment is in the range of 1 h to 6 h.
15. The method for manufacturing a negative electrode composite material according to claim 10, wherein the ultrasonic treatment time is in the range of 1 min to 30 min.
16. The method for preparing an anode composite material as claimed in claim 10, wherein the dispersion time ranges from 8h to 48h.
17. 10. The method for producing an anode composite material of claim 9, wherein the carbon source comprises at least one of an alkane, an alkene, and an alkyne.
18. 11. The method for producing an anode composite material according to claim 10, wherein the alcohol is at least one selected from ethanol, isopropanol, and butanol.
19. A lithium ion secondary battery negative electrode comprising the negative electrode composite material according to any one of claims 1 to 8.
20. A lithium ion secondary battery including a positive electrode, a negative electrode, and a separator, A lithium ion secondary battery, wherein the negative electrode comprises the negative electrode composite material according to any one of claims 1 to 8.
Citation Information
Patent Citations
Negative electrode active substance, mixed negative electrode active substance material, and method for manufacturing negative electrode active substance
JP2017188319A
Method of producing negative electrode material
JP2018032603A
Negative electrode active material for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, and manufacturing method of negative electrode material for nonaqueous electrolyte secondary battery
JP2020113495A
Negative electrode material for lithium ion secondary battery, its manufacturing method and use
JP2021521622A
Silicon-oxygen composite negative electrode material, its preparation method and lithium-ion battery
JP2022515463A
Cited By
Negative electrode composite material, preparation method thereof, negative electrode, and lithium ion secondary battery
JP2024144258A
Anode composite material, anode for lithium ion secondary battery, and lithium ion secondary battery