Hardmask composition, hardmask layer, and method of forming patterns
A hard mask composition with aromatic hydrocarbon rings and functional groups addresses the challenge of forming fine patterns by enhancing etching resistance and planarization in spin-coated hard mask layers, achieving performance comparable to traditional deposition methods with reduced costs.
Patent Information
- Application Number
- JP2024047873
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing lithographic techniques struggle to form fine patterns with good profiles due to the difficulty in achieving sufficient etching resistance and planarization in ultra-fine semiconductor technology, particularly when using spin coating methods for hard mask layers.
A hard mask composition containing a compound with an aromatic hydrocarbon ring and specific functional groups, such as hydroxy or alkoxy, is used to enhance etching resistance and solubility, allowing for improved hard mask layers formed via spin coating, which includes heat treatment to achieve excellent heat resistance and planarization.
The hard mask layer exhibits superior etching resistance, heat resistance, and planarization properties, comparable to those achieved with chemical or physical vapor deposition methods, while maintaining ease of processing and reducing costs.
Smart Images

Figure 2024144281000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a hardmask composition, a hardmask layer including a cured product of the hardmask composition, and a pattern forming method using the hardmask composition. [Background technology]
[0002] In recent years, the semiconductor industry has developed from patterns of several hundred nanometers to ultrafine technology with patterns of several to tens of nanometers. Effective lithographic techniques are essential to realize such ultrafine technology.
[0003] A typical lithographic technique includes the steps of forming a material layer on a semiconductor substrate, coating a photoresist layer thereon, exposing and developing the photoresist pattern to form a photoresist pattern, and then etching the material layer using the photoresist pattern as a mask.
[0004] In recent years, as the size of a pattern to be formed decreases, it is difficult to form a fine pattern having a good profile using only the above-mentioned typical lithographic techniques. Therefore, a supplementary layer called a hard mask layer can be formed between the material layer to be etched and the photoresist layer to form a fine pattern. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Korean Patent Publication No. 10-2022-0092160 Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a hard mask composition capable of forming a hard mask layer that can ensure excellent heat resistance, etching resistance and planarization characteristics.
[0007] Another object of the present invention is to provide a hard mask layer comprising a cured product of the above hard mask composition.
[0008] It is still another object of the present invention to provide a method for forming a pattern using the hard mask composition. [Means for solving the problem]
[0009] A hard mask composition according to one embodiment of the present invention includes a compound represented by the following Chemical Formula 1, and a solvent:
[0010] [ka]
[0011] In the above chemical formula 1, A 1 and A 2 each independently represents a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, or a group in which a substituted or unsubstituted aromatic hydrocarbon ring having 6 to 30 carbon atoms is linked by a single bond, a substituted or unsubstituted alkylene group having 1 to 5 carbon atoms, or a combination thereof; R 1 each independently represents a substituted or unsubstituted alkyl group having 1 to 30 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 30 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 30 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 30 carbon atoms, a substituted or unsubstituted cycloalkenyl group having 3 to 30 carbon atoms, a substituted or unsubstituted cycloalkynyl group having 3 to 30 carbon atoms, or a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, R 2are each independently a hydrogen atom, a deuterium atom, or a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, n is an integer from 1 to 6.
[0012] A in the above chemical formula 1 1 and A 2 may each independently be a substituted or unsubstituted group having at least one moiety selected from Group 1 below:
[0013] [ka]
[0014] A in the above chemical formula 1 1 and A 2 may each independently be a substituted or unsubstituted group having at least one moiety selected from Group 1-1 below:
[0015] [ka]
[0016] A in the above chemical formula 1 1 may be a substituted or unsubstituted group having at least one moiety selected from Group 1-2 below:
[0017] [ka]
[0018] A in the above chemical formula 1 2 may each independently be a substituted or unsubstituted group having at least one moiety selected from groups 1-3 below:
[0019] [ka]
[0020] R in the above Chemical Formula 1 1 are each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, or a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms.
[0021] R in the above Chemical Formula 1 2 may each independently be a hydrogen atom, a deuterium atom, a substituted or unsubstituted methyl group, a substituted or unsubstituted ethyl group, a substituted or unsubstituted propyl group, a substituted or unsubstituted butyl group, or a substituted or unsubstituted pentyl group.
[0022] R in the above Chemical Formula 1 1 are each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, or a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms; R 2 are each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted methyl group, or a substituted or unsubstituted ethyl group, and n can be one of the integers from 1 to 3.
[0023] In the above formula 1, n is 2 or 3, and in this case, all R 1 are identical to each other, and all R 2 are identical to each other and all A 2 may be identical to each other.
[0024] R in the above Chemical Formula 1 1 are each independently a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms; R 2 are each independently a hydrogen atom or a deuterium atom, and n can be 2.
[0025] The compound represented by Chemical Formula 1 above may be at least one of the compounds represented by Chemical Formulas 2 to 4 below:
[0026] [ka]
[0027] In the above Chemical Formula 2 to Chemical Formula 4, R 1 each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, or a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms, R 2 are each independently a hydrogen atom, a deuterium atom, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, X 1 and X 2 each independently represents a deuterium atom, a hydroxyl group, a halogen atom, a thiol group, a substituted or unsubstituted alkoxy group having 1 to 10 carbon atoms, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, Each n is independently an integer from 1 to 3; m1 and m2 each independently represent an integer of 0 to 5.
[0028] The compound represented by Chemical Formula 1 above may be at least one of the compounds represented by Chemical Formulas 5 to 10 below:
[0029] [ka]
[0030] [ka]
[0031] The molecular weight of the compound represented by Chemical Formula 1 may be 500 g / mol to 10,000 g / mol.
[0032] The compound represented by Chemical Formula 1 may be included in the hard mask composition in an amount of 0.1% by mass to 30% by mass based on the total mass of the hard mask composition.
[0033] The solvent can be at least one of propylene glycol, propylene glycol diacetate, methoxypropanediol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidinone, acetylacetone, and ethyl 3-ethoxypropionate.
[0034] According to another aspect of the present invention, there is provided a hardmask layer comprising a cured product of the hardmask composition described above.
[0035] According to yet another aspect of the present invention, there is provided a pattern formation method including the steps of forming a material layer on a substrate, applying the above-described hard mask composition onto the material layer, heat-treating the hard mask composition to form a hard mask layer, forming a photoresist layer on the hard mask layer, exposing and developing the photoresist layer to form a photoresist pattern, selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer, and etching the exposed portion of the material layer.
[0036] The step of forming the hard mask layer may include a step of performing a heat treatment at 100°C to 1,000°C. Effect of the Invention
[0037] The hard mask layer formed from the hard mask composition according to the present invention can ensure excellent heat resistance, etching resistance and planarization properties. [Brief description of the drawings]
[0038] [Figure 1] FIG. 1 is a diagram for explaining a calculation formula (Calculation Formula 1) for evaluating the planarization property of a hard mask composition according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0039] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art will be able to easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.
[0040] Unless otherwise defined in this specification, "substituted" and "substituted" mean that a hydrogen atom in a compound has been replaced with a halogen atom (F, Br, Cl, or I), a hydroxy group, an alkoxy group, a nitro group, a cyano group, an amino group, an azide group, an amidino group, a hydrazino group, a hydrazono group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, a carboxyl group and salts thereof, a sulfonic acid group and salts thereof, a phosphoric acid group and salts thereof, a vinyl group, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, or a carboxyl group having 2 to 20 carbon atoms. It means that the aryl group is substituted with a substituent selected from the group consisting of an aromatic hydrocarbon group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, an arylaryl group having 9 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, a heteroalkyl group having 1 to 20 carbon atoms, a heteroarylalkyl group having 3 to 20 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, a cycloalkenyl group having 3 to 15 carbon atoms, a cycloalkynyl group having 6 to 15 carbon atoms, a heterocycloalkyl group having 3 to 30 carbon atoms, and combinations thereof.
[0041] In addition, two adjacent substituents among the above-mentioned substituted halogen atoms (F, Br, Cl, or I), hydroxy groups, nitro groups, cyano groups, amino groups, azide groups, amidino groups, hydrazino groups, hydrazono groups, carbonyl groups, carbamoyl groups, thiol groups, ester groups, carboxyl groups or salts thereof, sulfonic acid groups or salts thereof, phosphoric acid or salts thereof, alkyl groups having 1 to 30 carbon atoms, alkenyl groups having 2 to 30 carbon atoms, alkynyl groups having 2 to 30 carbon atoms, aromatic hydrocarbon groups having 6 to 30 carbon atoms, arylalkyl groups having 7 to 30 carbon atoms, alkoxy groups having 1 to 30 carbon atoms, heteroalkyl groups having 1 to 20 carbon atoms, heteroarylalkyl groups having 3 to 20 carbon atoms, cycloalkyl groups having 3 to 30 carbon atoms, cycloalkenyl groups having 3 to 15 carbon atoms, cycloalkynyl groups having 6 to 15 carbon atoms, or heterocyclic groups having 2 to 30 carbon atoms may be condensed to form a ring.
[0042] Unless otherwise defined in this specification, the terms "aromatic hydrocarbon ring," "aromatic hydrocarbon group," and "aryl group" refer to a group having one or more aromatic hydrocarbon moieties, and include not only non-fused aromatic hydrocarbon rings and fused aromatic hydrocarbon rings, but also forms in which aromatic hydrocarbon moieties are linked by single bonds, fused ring forms having a non-aromatic moiety to which an aromatic hydrocarbon moiety is directly or indirectly fused, and combinations thereof.
[0043] More specifically, the substituted or unsubstituted aromatic hydrocarbon group may be, but is not limited to, a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted phenanthryl group, a substituted or unsubstituted naphthacenyl group, a substituted or unsubstituted pyrenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted terphenyl group, a substituted or unsubstituted quaterphenyl group, a substituted or unsubstituted chrysenyl group, a substituted or unsubstituted triphenylenyl group, a substituted or unsubstituted perylenyl group, a substituted or unsubstituted indenyl group, a combination thereof, or a condensed form of a combination thereof.
[0044] As used herein, the term "polymer" includes both oligomers and polymers.
[0045] Unless otherwise specified in this specification, "molecular weight" refers to the sum of the atomic weights of the atoms contained in a molecule. In this specification, "molecular weight" is measured by dissolving a powder sample in tetrahydrofuran (THF) and then using 1200 series gel permeation chromatography (GPC) manufactured by Agilent Technologies (the column is LF-804 manufactured by Resonac Co., Ltd., and the standard sample is polystyrene manufactured by Resonac Co., Ltd.).
[0046] In the semiconductor industry, there is a constant demand to reduce the size of chips, and in order to meet this demand, the line width of the resist patterned by lithography technology needs to be several tens of nanometers in size. Therefore, the height that can withstand the line width of the resist pattern is limited, and the resist may not have sufficient resistance in the etching step. To compensate for this, an auxiliary layer called a hard mask layer is used between the material layer to be etched and the photoresist layer. This hard mask layer serves as an intermediate film that transfers the fine pattern of the photoresist to the material layer through selective etching. Therefore, the hard mask layer is required to have etching resistance so that it can withstand the etching process required for pattern transfer.
[0047] Existing hard mask layers have been formed by chemical or physical deposition methods, which require large-scale equipment and have a high process cost, resulting in poor economic efficiency. Recently, a technology for forming a hard mask layer by a spin coating method has been developed. The spin coating method is easier to process than conventional methods, and the hard mask layer manufactured using the method may have better gap filling and planarization properties, but the hard mask layer formed using the spin coating method has a problem that the required etching resistance is somewhat reduced. Therefore, a hard mask composition that can be applied to the spin coating method is required, and the hard mask layer formed using the spin coating method is required to have the same etching resistance as the hard mask layer formed using the chemical or physical deposition method.
[0048] Therefore, in order to improve the etching resistance of the hard mask layer, research has been conducted to increase the carbon content contained in the hard mask composition. However, as the carbon content of the compound contained in the hard mask composition increases, the solubility in the solvent tends to decrease. Therefore, it is required to increase the carbon content of the compound contained in the hard mask composition, improve the etching resistance of the hard mask layer formed therefrom, and make the compound sufficiently soluble in the solvent.
[0049] The hard mask composition according to one embodiment of the present invention contains a compound having an aromatic hydrocarbon ring, so that the carbon content in the composition can be increased. Therefore, the hard mask layer obtained from the composition can ensure excellent etching resistance. In addition, the compound contains a specific functional group, so that the compound has a high carbon content and excellent solubility in a solvent.
[0050] Specifically, a hard mask composition according to an embodiment of the present invention includes a compound represented by the following Formula 1, and a solvent.
[0051] [ka]
[0052] In the above chemical formula 1, A 1 and A 2 each independently represents a substituted or unsubstituted aromatic hydrocarbon ring having 6 to 30 carbon atoms, or a group in which substituted or unsubstituted aromatic hydrocarbon rings having 6 to 30 carbon atoms are linked by a single bond, a substituted or unsubstituted alkylene group having 1 to 5 carbon atoms, or a combination thereof; R 1 each independently represents a substituted or unsubstituted saturated aliphatic hydrocarbon group having 1 to 30 carbon atoms, a substituted or unsubstituted unsaturated aliphatic hydrocarbon group having 2 to 30 carbon atoms, a substituted or unsubstituted saturated or unsaturated alicyclic hydrocarbon group having 3 to 30 carbon atoms, or a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, R 2 are each independently a hydrogen atom, a deuterium atom, or a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, n is an integer from 1 to 6.
[0053] As represented by Chemical Formula 1 above, the compound according to one embodiment of the present invention contains a quaternary carbon (a carbon substituted with four atoms other than hydrogen atoms), and an aromatic hydrocarbon, a saturated or unsaturated aliphatic hydrocarbon group, or a saturated or unsaturated alicyclic hydrocarbon group, etc., is directly bonded to the quaternary carbon, thereby increasing the carbon content in the compound, and thus increasing the carbon content in a hard mask composition containing the compound, thereby improving the etching resistance of a hard mask layer formed therefrom.
[0054] In addition, the compound according to one embodiment of the present invention includes a quaternary carbon, and a hydroxyl or alkoxy group is bonded to the quaternary carbon, thereby improving the solubility of the compound in a solvent, and a hard mask composition including the compound can be effectively applied to a spin-on coating process. Moreover, the hydroxyl or alkoxy group can help crosslink between compounds, and the composition including the compound can exhibit excellent crosslinking properties. In addition, the compound is crosslinked in a polymer form having a large molecular weight within a short time during heat treatment, so that the hard mask layer formed therefrom can have excellent heat resistance and excellent etching resistance.
[0055] Ar in the above formula 1 1 and Ar 2 may each independently be a substituted or unsubstituted group having at least one moiety selected from Group 1 below:
[0056] [ka]
[0057] For example, A in the above chemical formula 1 1 and A 2 are each independently a substituted or unsubstituted group having at least one moiety selected from Group 1-1 below:
[0058] [ka]
[0059] As an example, A in the above chemical formula 1 1 is a substituted or unsubstituted group having at least one moiety selected from group 1-2 below, such as, but not limited to, benzene, naphthalene, anthracene, phenanthrene, pyrene, or coronene, for example, benzene, pyrene, or coronene:
[0060] [ka]
[0061] As an example, A in the above chemical formula 1 2 are each independently a substituted or unsubstituted group having at least one moiety selected from Groups 1-3 below, such as, but not limited to, benzene, naphthalene, anthracene, phenanthrene, or pyrene, including, but not limited to, benzene or pyrene:
[0062] [ka]
[0063] R in the above Chemical Formula 1 1 are each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, or a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms, for example, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, or a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms, for example, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, but are not limited to these.
[0064] R in the above Chemical Formula 1 1 By having a substituent as listed above rather than a hydrogen atom, the carbon content of the compound according to the present invention can be increased.
[0065] R in the above Chemical Formula 1 2are each independently a hydrogen atom, a deuterium atom, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, for example, a hydrogen atom, a deuterium atom, a substituted or unsubstituted methyl group, a substituted or unsubstituted ethyl group, a substituted or unsubstituted propyl group, a substituted or unsubstituted butyl group, or a substituted or unsubstituted pentyl group, for example, a hydrogen atom, a deuterium atom, a substituted or unsubstituted methyl group, or a substituted or unsubstituted ethyl group, for example, a hydrogen atom or a deuterium atom, but is not limited to these.
[0066] In the above Chemical Formula 1, n is an integer of 1 to 6, for example, an integer of 1 to 3, for example, n is 2 or 3, for example, n is 2, but is not limited thereto. When n in the above Chemical Formula 1 is 2, the solubility of the compound represented by the above Chemical Formula 1 of the present invention in a solvent can be optimized, and the hard mask layer formed from the hard mask composition containing the above compound can have good etching resistance.
[0067] When n in the above chemical formula 1 is an integer of 2 or more, R 1 may be the same or different, and R 2 may be the same or different, and A present in Chemical Formula 1 2 may be the same or different from each other. That is, when n is 2 or more, there are 2 or more R 1 may be the same or different, or some may be the same group and the rest may be different groups; 2 Each may be the same or different, or some may be the same group and the rest may be different groups. 2 These may be the same or different, or some may be the same groups and the rest may be different groups.
[0068] In one embodiment, the compound represented by Chemical Formula 1 above is at least one of the compounds represented by Chemical Formulas 2 to 4 below:
[0069] [ka]
[0070] R in the above Chemical Formula 2 to the above Chemical Formula 4 1 each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, or a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms, R 2 are each independently a hydrogen atom, a deuterium atom, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, X 1 and X 2 each independently represents a deuterium atom, a hydroxyl group, a halogen atom, a thiol group, a substituted or unsubstituted alkoxy group having 1 to 10 carbon atoms, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, Each n is independently an integer from 1 to 3; m1 and m2 each independently represent an integer of 0 to 5.
[0071] As an example, the compound represented by Chemical Formula 1 is at least one of the compounds represented by Chemical Formulas 5 to 10 below:
[0072] [ka]
[0073] [ka]
[0074] The compound represented by the above formula 1 may have a molecular weight of 500 g / mol to 10,000 g / mol. For example, it may have a molecular weight of 500 g / mol to 9,500 g / mol, for example, 500 g / mol to 9,000 g / mol, for example, 600 g / mol to 8,500 g / mol, for example, 600 g / mol to 8,000 g / mol, for example, 700 g / mol to 7,500 g / mol, for example, 700 g / mol to 7,000 g / mol, but is not limited thereto. By having a molecular weight in the above range, the carbon content and solubility in a solvent of the hard mask composition containing the above compound can be adjusted and optimized.
[0075] The compound represented by the above chemical formula 1 can be synthesized by appropriately referring to a conventionally known synthesis method. More specifically, a person skilled in the art can easily synthesize the compound by referring to the synthesis method described in the Examples.
[0076] The compound represented by the above formula 1 may be included in an amount of 0.1% by mass to 30% by mass based on the total mass of the hard mask composition. For example, it may be 0.2% by mass to 30% by mass, for example, 0.5% by mass to 30% by mass, for example, 1% by mass to 30% by mass, for example, 1% by mass to 25% by mass, for example, 1% by mass to 20% by mass, but is not limited thereto. By including the compound represented by the above formula 1 in the composition, the thickness, surface roughness, planarization characteristics, etc. of the hard mask can be easily adjusted.
[0077] The hard mask composition according to an embodiment of the present invention may include a solvent, and the solvent may include, but is not limited to, at least one selected from, for example, propylene glycol, propylene glycol diacetate, methoxypropanediol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidinone, acetylacetone, or ethyl 3-ethoxypropionate. The solvent is not particularly limited as long as it has sufficient solubility and / or dispersibility for the compound.
[0078] The hard mask composition may further include additives such as a surfactant, a crosslinking agent, a thermal acid generator, and a plasticizer.
[0079] Examples of the surfactant that can be used include, but are not limited to, fluoroalkyl compounds, alkylbenzenesulfonates, alkylpyridinium salts, polyethylene glycols, and quaternary ammonium salts.
[0080] Examples of the crosslinking agent include melamine-based agents, substituted urea-based agents, and polymers thereof. A crosslinking agent having at least two crosslink-forming substituents is preferable, and for example, compounds such as methoxymethylated glycoluril, butoxymethylated glycoluril, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguanamine, butoxymethylated benzoguanamine, methoxymethylated urea, butoxymethylated urea, methoxymethylated thiourea, and butoxymethylated thiourea can be used.
[0081] In addition, as the crosslinking agent, a crosslinking agent having high heat resistance can be used. As the crosslinking agent having high heat resistance, for example, a compound containing a crosslinking-forming substituent having an aromatic ring (e.g., a benzene ring, a naphthalene ring) in the molecule can be used.
[0082] Examples of the thermal acid generator that can be used include acidic compounds such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium p-toluenesulfonate, salicylic acid, sulfosalicylic acid, citric acid, benzoic acid, hydroxybenzoic acid, and naphthalenecarboxylic acid, and / or 2,4,4,6-tetrabromocyclohexadienone, benzoin tosylate, 2-nitrobenzyl tosylate, and other organic sulfonic acid alkyl esters, but are not limited to these.
[0083] According to another aspect of the present invention, there is provided a hardmask layer comprising a cured product of the hardmask composition described above.
[0084] A method for forming a pattern using the above-described hard mask composition will now be described.
[0085] A pattern formation method according to one embodiment of the present invention includes the steps of forming a material layer on a substrate, applying a hard mask composition containing the above-mentioned compound and a solvent onto the material layer, heat-treating the hard mask composition to form a hard mask layer, forming a photoresist layer on the hard mask layer, exposing and developing the photoresist layer to form a photoresist pattern, selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer, and etching the exposed portion of the material layer.
[0086] The substrate may be, for example, a silicon wafer, a glass substrate, or a polymer substrate. The material layer is the material to be ultimately patterned, and may be, for example, a metal layer such as aluminum or copper, a semiconductor layer such as silicon, or an insulating layer such as silicon oxide or silicon nitride. The material layer may be formed, for example, by chemical vapor deposition.
[0087] The hard mask composition may be prepared in the form of a solution and applied by spin coating, as described above. In this case, the thickness of the hard mask composition is not particularly limited, but may be, for example, 50 to 200,000 Å.
[0088] The step of heat treating the hard mask composition may be performed for 10 seconds to 1 hour at, for example, 100° C. to 1,000° C. For example, the step of heat treating the hard mask composition may include a plurality of heat treatment steps, for example, a first heat treatment step and a second heat treatment step.
[0089] In one embodiment, the step of heat treating the hard mask composition may include one heat treatment step performed at, for example, 100° C. to 1000° C. for 10 seconds to 1 hour. For example, the heat treatment step may be performed in an air or nitrogen atmosphere, or in an atmosphere having an oxygen concentration of 1% by mass or less.
[0090] In one embodiment, the step of heat treating the hard mask composition includes a first heat treatment step performed at a temperature of, for example, 100°C to 1,000°C, for example, 100°C to 800°C, for example, 100°C to 500°C, for example, 150°C to 400°C, for example, 30 seconds to 1 hour, for example, 30 seconds to 30 minutes, for example, 30 seconds to 10 minutes, for example, 30 seconds to 5 minutes.
[0091] Also, it may include a second heat treatment step successively performed at, for example, 100° C. to 1,000° C., for example, 300° C. to 1,000° C., for example, 500° C. to 1,000° C., for example, 500° C. to 600° C., for example, 30 seconds to 1 hour, for example, 30 seconds to 30 minutes, for example, 30 seconds to 10 minutes, for example, 30 seconds to 5 minutes. As an example, the first and second heat treatment steps may be performed in an air or nitrogen atmosphere, or in an atmosphere with an oxygen concentration of 1% by mass or less.
[0092] At least one of the steps of heat treating the hard mask composition is performed at a high temperature of 200° C. or more, thereby allowing the hard mask composition to exhibit high etching resistance that can withstand etching gases and chemical solutions to which the hard mask composition is exposed in subsequent processes, including an etching process.
[0093] In one embodiment, forming the hard mask layer may include an ultraviolet-visible (UV / Vis) curing step and / or a near infrared (near IR) curing step.
[0094] In one embodiment, the step of forming the hard mask layer may include at least one of the first heat treatment step, the second heat treatment step, the UV / Vis curing step, and the near IR curing step, or may include two or more steps consecutively.
[0095] In one embodiment, the method may further include forming a silicon-containing thin film layer on the hard mask layer, the silicon-containing thin film layer being formed of a material such as SiCN, SiOC, SiON, SiOCN, SiC, SiO, and / or SiN.
[0096] In one embodiment, before the step of forming the photoresist layer, a bottom anti-reflective coating (BARC) may be further formed on the silicon-containing thin film layer or the hard mask layer.
[0097] In one embodiment, the step of exposing the photoresist layer can be performed using, for example, ArF, KrF, or EUV, etc. After the exposure, a heat treatment process can be performed at 100°C to 700°C.
[0098] In one embodiment, the step of etching the exposed portions of the material layer can be performed by dry etching using an etching gas, which can be, for example, N2 / O2, CHF3, CF4, Cl2, BCl3, and mixtures thereof.
[0099] The etched material layer can be formed in a variety of patterns, which can be diverse, such as metal patterns, semiconductor patterns, insulating patterns, etc., and can be applied as various patterns within a semiconductor integrated circuit device, for example. EXAMPLES
[0100] The above-mentioned embodiments of the present invention will be described in more detail with reference to the following examples. However, the following examples are merely for illustrative purposes and are not intended to limit the scope of the present invention.
[0101] Compound synthesis Synthesis Example 1 Step 1: Friedel-Crafts acylation reaction A solution was prepared by adding 9.48g (0.05mol) of pyrene, 25.00g (0.09mol) of pyrene carboxylic acid chloride, and 237.92g of 1,2-dichloroethane to a flask. 25.00g (0.19mol) of aluminum chloride was gradually added to the above solution, and the solution was stirred at room temperature for 10 hours. After the reaction was completed, methanol was added to the solution, and the precipitate formed was filtered off to obtain bis(pyrenylcarbonyl)pyrene.
[0102] Step 2: Grignard reaction A solution was prepared by adding 30.00 g (0.05 mol) of the bis(pyrenylcarbonyl)pyrene obtained above and 235.73 g of tetrahydrofuran to a flask. 21.74 g (0.18 mol) of methylmagnesium bromide was gradually added to the above solution at room temperature, and the temperature was raised to 60° C. and the mixture was stirred for 4 hours. After the reaction was completed, the resulting reaction solution was neutralized to pH 7 with 1% hydrochloric acid. Then, the mixture was extracted with ethyl acetate to obtain compound A represented by the following chemical formula 5 (molecular weight = 690.84 g / mol).
[0103] [ka]
[0104] Synthesis Example 2 Compound B represented by the following chemical formula 6 was obtained (molecular weight=746.95 g / mol) in the same manner as in Synthesis Example 1 above, except that 26.83 g (0.18 mol) of propylmagnesium bromide was used instead of 21.74 g (0.18 mol) of methylmagnesium bromide in the second step.
[0105] [ka]
[0106] Synthesis Example 3 Step 1: Friedel-Crafts acylation reaction A solution was prepared by adding 10.73g (0.05mol) of 4-methoxypyrene, 24.76g (0.09mol) of pyrene carboxylic acid chloride, and 239.88g of 1,2-dichloroethane to a flask. 24.63g (0.18mol) of aluminum chloride was gradually added to the above solution, and the solution was stirred at room temperature for 4 hours. After the reaction was completed, methanol was added thereto, and the precipitate formed was filtered off to obtain bis(pyrenylcarbonyl)methoxypyrene.
[0107] Step 2: Demethylation reaction 28.00 g (0.04 mol) of the bis(pyrenylcarbonyl)methoxypyrene obtained above, 24.68 g (0.12 mol) of 1-dodecanethiol, 9.12 g (0.16 mol) of potassium hydroxide, and 247.20 g of N,N-dimethylformamide were placed in a flask and stirred for 6 hours at 90° C. After stirring, the mixture was cooled and neutralized to pH 7 with 1% hydrochloric acid, and the formed precipitate was filtered off to obtain bis(pyrenylcarbonyl)hydroxypyrene.
[0108] Step 3: Grignard reaction A solution was prepared by adding 26.02 g (0.04 mol) of bis(pyrenylcarbonyl)hydroxypyrene obtained above and 240.00 g of tetrahydrofuran to a flask. 33.96 g (0.23 mol) of propylmagnesium bromide was gradually added to the above solution at room temperature, and the temperature was raised to 60° C. and the mixture was stirred for 12 hours. After the reaction was completed, the resulting reaction solution was neutralized to pH 7 with 1% hydrochloric acid. Then, the mixture was extracted with ethyl acetate to obtain compound C represented by the following chemical formula 7 (molecular weight=762.95 g / mol).
[0109] [ka]
[0110] Synthesis Example 4 Compound D represented by the following chemical formula 8 was obtained in the same manner as in Synthesis Example 1, except that in the second step, 26.83 g (0.18 mol) of isopropylmagnesium bromide was used instead of 21.74 g (0.18 mol) of methylmagnesium bromide. (Molecular weight: 746.95 g / mol)
[0111] [ka]
[0112] Synthesis Example 5 Step 1: Friedel-Crafts acylation reaction A solution was prepared by adding 20.60g (0.10mol) of terephthaloyl chloride, 47.00g (0.20mol) of 1-methoxypyrene, and 221.00g of 1,2-dichloroethane to a flask. 27.00g (0.20mol) of aluminum chloride was gradually added to the solution at room temperature, and the solution was heated to 60°C and stirred for 8 hours. After the reaction was completed, methanol was added to the solution, and the formed precipitate was filtered to obtain bis(methoxypyrenylcarbonyl)benzene.
[0113] Step 2: Demethylation reaction 53.50 g (0.09 mol) of the bis(methoxypyrenylcarbonyl)benzene obtained above, 91.10 g (0.45 mol) of 1-dodecanethiol, 30.30 g (0.54 mol) of potassium hydroxide, and 262.00 g of N,N-dimethylformamide were placed in a flask and stirred for 8 hours at 120° C. After stirring, the mixture was cooled and neutralized to pH 7 with 1% hydrochloric acid, and the formed precipitate was filtered off to obtain bis(hydroxypyrenylcarbonyl)benzene.
[0114] Step 3: Grignard reaction A solution was prepared by adding 18.44 g (0.03 mol) of the bis(hydroxypyrenylcarbonyl)benzene obtained above and 258.87 g of tetrahydrofuran to a flask. 38.89 g (0.26 mol) of propylmagnesium bromide was gradually added to the above solution at room temperature, and the temperature was raised to 60°C and stirred for 12 hours. After the reaction was completed, the mixture was neutralized to pH 7 with 1% hydrochloric acid and extracted with ethyl acetate to obtain compound E represented by the following chemical formula 9-1 (molecular weight = 654.81 g / mol).
[0115] [ka]
[0116] Synthesis Example 6 Step 1: Friedel-Crafts acylation reaction A solution was prepared by adding 50.00g (0.17mol) of coronene, 56.80g (0.34mol) of 4-methoxybenzochloride, and 353.00g of 1,2-dichloroethane to a flask. 44.4g (0.34mol) of aluminum chloride was gradually added to the solution at room temperature, and the solution was heated to 60°C and stirred for 8 hours. After the reaction was completed, methanol was added to the solution, and the formed precipitate was filtered to obtain bis(methoxybenzoyl)coronene.
[0117] Step 2: Demethylation reaction 50.00 g (0.88 mol) of the bis(methoxybenzoyl)coronene obtained above, 89.00 g (0.44 mol) of 1-dodecanethiol, 29.60 g (0.53 mol) of potassium hydroxide, and 253.00 g of N,N-dimethylformamide were placed in a flask and stirred for 8 hours at 120° C. After stirring, the mixture was cooled and neutralized to pH 7 with 1% hydrochloric acid, and the formed precipitate was filtered off to obtain bis(hydroxybenzoyl)coronene.
[0118] Step 3: Grignard reaction A solution was prepared by adding 17.86 g (0.03 mol) of bis(hydroxybenzoyl)coronene obtained above and 258.87 g of tetrahydrofuran to a flask. 38.97 g (0.26 mol) of propylmagnesium bromide was gradually added to the above solution at room temperature, and the temperature was raised to 60°C and stirred for 12 hours. After the reaction was completed, the solution was neutralized to pH 7 with 1% hydrogen chloride solution and extracted with ethyl acetate to obtain compound F represented by the following chemical formula 10-1 (molecular weight = 628.77 g / mol).
[0119] [ka]
[0120] Comparative synthesis example 1 Step 1: Friedel-Crafts acylation reaction A solution was prepared by adding 50.0g (0.166mol) of coronene, 56.8g (0.333mol) of 4-methoxybenzoyl chloride, and 353g of 1,2-dichloroethane to a flask. 44.4g (0.333mol) of aluminum chloride was gradually added to the solution at room temperature, and the temperature was raised to 60°C and the mixture was stirred for 8 hours. After the reaction was completed, methanol was added to the solution, and the precipitate formed was filtered to obtain disubstituted 4-methoxybenzoyl coronene.
[0121] Step 2: Demethylation reaction The disubstituted 4-methoxybenzoylcoronene (50.0 g, 0.880 mol) obtained above, 1-dodecanethiol (89.0 g, 0.440 mol), potassium hydroxide (29.6 g, 0.528 mol), and N,N-dimethylformamide (53 g) were placed in a flask and stirred for 8 hours at 120° C. After stirring, the mixture was cooled, neutralized to pH 7 with 10% hydrochloric acid, and extracted with ethyl acetate to obtain disubstituted 4-hydroxybenzoylcoronene.
[0122] Step 3: Reduction reaction A solution was prepared by adding 25.0 g (0.0463 mol) of the disubstituted 4-hydroxybenzoylcoronene obtained above and 170 g of tetrahydrofuran to a flask. 17.5 g (0.463 mol) of sodium borohydride aqueous solution was gradually added to the above solution and stirred at room temperature for 24 hours. After the reaction was completed, the solution was neutralized to pH 7 with 10% hydrochloric acid and extracted with ethyl acetate to obtain compound G represented by the following chemical formula 11 (molecular weight = 544.61 g / mol).
[0123] [ka]
[0124] Preparation of the hard mask composition Examples 1 to 6 and Comparative Example 1 Each of Compounds A to G obtained in Synthesis Examples 1 to 6 and Comparative Synthesis Example 1 was uniformly dissolved in a solvent in which propylene glycol monomethyl ether acetate (PGMEA) and cyclohexanone were mixed in a volume ratio of 3:7 to prepare a hard mask composition having a compound content of 10.0 mass %.
[0125] Evaluation 1: Heat resistance evaluation The hard mask compositions according to Examples 1 to 6 and Comparative Example 1 were each coated on a silicon wafer by spin coating, and then heat-treated on a hot plate at 160°C for 1 minute to form a hard mask layer. The thickness of the hard mask layer was measured using a thin film thickness measuring device manufactured by K-MAC. Next, the hard mask layer was re-heat-treated at 400°C for 2 minutes, and the thickness of the hard mask layer was measured. If the change rate of the thickness of the hard mask layer before and after the re-heat-treatment at 400°C for 2 minutes was less than 5%, it was evaluated as "A (very good)", if it was 5% or more but less than 10%, it was evaluated as "B (good)", and if it was 10% or more, it was evaluated as "C (poor)". The results are shown in Table 1 below.
[0126] [Table 1]
[0127] Referring to Table 1, it was confirmed that the hard mask layers formed from the compositions according to Examples 1 to 6 had a thickness change rate of less than 5% before and after the re-heat treatment, and the hard mask layer formed from the composition according to Comparative Example 1 had a thickness change rate of 10% or more before and after the re-heat treatment. In other words, it was confirmed that the heat resistance of the hard mask layers formed from the compositions according to the Examples was superior to that of the hard mask layers formed from the compositions according to the Comparative Examples.
[0128] Evaluation 2: Gap-fill properties The hard mask compositions according to Examples 1 to 6 and Comparative Example 1 were each coated on a patterned silicon wafer by spin coating, and then heat-treated at 400°C for 60 seconds to form a hard mask layer. A field emission scanning electron microscope (FE-SEM) was used to observe the cross-sectional image of the pattern of the hard mask layer to check whether voids were generated. The results are shown in Table 2 below.
[0129] [Table 2]
[0130] Referring to Table 2 above, it was found that no voids were generated in the hard mask layers formed from the hard mask compositions according to Examples 1 to 6, whereas voids were generated in the hard mask layer formed from the hard mask composition according to Comparative Example 1. This shows that the gap-fill characteristics of the hard mask layers formed from the hard mask compositions according to the Examples are superior to those of the hard mask layers formed from the hard mask compositions according to Comparative Examples.
[0131] Evaluation 3: Flattening properties The hard mask compositions according to Examples 1 to 6 and Comparative Example 1 were coated on a patterned silicon wafer by spin coating, and then heat-treated at 400° C. for 60 seconds. Then, a cross-sectional image of the pattern was observed using a field emission scanning electron microscope (FE-SEM). The thickness of the hard mask layer appearing in the cross-sectional image of the pattern was measured, and the planarization characteristic was quantified using the calculation formula of FIG. 1. The planarization characteristic was evaluated as the ratio of the planarization characteristic of the hard mask layer formed from the composition according to Examples 1 to 6 to the planarization characteristic of the hard mask layer formed from the composition according to Comparative Example 1. When the ratio was less than 5%, it was evaluated as “A (very good)”, when it was 5% or more but less than 10%, it was evaluated as “B (good)”, and when it was 10% or more, it was evaluated as “C (poor)”. The results are shown in Table 3 below.
[0132] [Table 3]
[0133] Rating 4: Etching resistance The hard mask compositions according to Examples 1 to 6 and Comparative Example 1 were coated on a silicon wafer by spin coating, and then heat-treated on a hot plate at 160°C for 1 minute to form a hard mask layer. The hard mask layer was dry-etched for 30 seconds using a mixed gas of CF4 / Ar, and the thickness of the hard mask before and after etching was measured using a thin film thickness measuring device manufactured by K-MAC, to calculate the etching rate. The etching resistance was evaluated as the ratio of the etching rate of the hard mask layer formed from the composition according to Examples 1 to 6 to the etching rate of the hard mask layer formed from the composition according to Comparative Example 1. Specifically, when the ratio was less than 0.95, it was evaluated as "A (very good)", when it was 0.95 or more and less than 1.00, it was evaluated as "B (good)", and when it was 1.00 or more, it was evaluated as "C (poor)". The results are shown in Table 4 below.
[0134] [Table 4]
[0135] Referring to Table 4, it was found that the etching rate of the hard mask layer formed from the composition according to Examples 1 to 6 was less than 0.95 relative to the etching rate of the hard mask layer formed from the composition according to Comparative Example 1. Therefore, it was found that the etching resistance of the hard mask layer formed from the composition according to Examples 1 to 6 was superior to that of the hard mask layer formed from the composition according to Comparative Example 1.
Claims
1. A hard mask composition comprising a compound represented by the following Chemical Formula 1 and a solvent: 【Chemistry 1】 In the above Chemical Formula 1, A 1 and A 2 each independently represents a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, or a group in which a substituted or unsubstituted aromatic hydrocarbon ring having 6 to 30 carbon atoms is linked by a single bond, a substituted or unsubstituted alkylene group having 1 to 5 carbon atoms, or a combination thereof; R 1 each independently represents a substituted or unsubstituted alkyl group having 1 to 30 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 30 carbon atoms, a substituted or unsubstituted alkynyl group having 2 to 30 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 30 carbon atoms, a substituted or unsubstituted cycloalkenyl group having 3 to 30 carbon atoms, a substituted or unsubstituted cycloalkynyl group having 3 to 30 carbon atoms, or a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, R 2 are each independently a hydrogen atom, a deuterium atom, or a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, n is an integer from 1 to 6.
2. In the above Chemical Formula 1, A 1 and A 2 is each independently a substituted or unsubstituted group having at least one moiety selected from Group 1: 【Chemistry 2】
3. In the above Chemical Formula 1, A 1 and A 2 is each independently a substituted or unsubstituted group having at least one moiety selected from Group 1-1 below: 【Chemistry 3】
4. In the above Chemical Formula 1, A 1 is a substituted or unsubstituted group having at least one moiety selected from Group 1-2 below: 【Chemistry 4】
5. In the above Chemical Formula 1, A 2 is each independently a substituted or unsubstituted group having at least one moiety selected from the following Groups 1-3: 【Chemistry 5】
6. R in Formula 1 1 are each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, or a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms.
7. R in Formula 1 2 10. The hard mask composition of claim 1, wherein each independently is a hydrogen atom, a deuterium atom, a substituted or unsubstituted methyl group, a substituted or unsubstituted ethyl group, a substituted or unsubstituted propyl group, a substituted or unsubstituted butyl group, or a substituted or unsubstituted pentyl group.
8. R in Formula 1 1 are each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, or a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms; R 2 is each independently a hydrogen atom, a deuterium atom, a substituted or unsubstituted methyl group, or a substituted or unsubstituted ethyl group; and n is an integer from 1 to 3.
9. In the formula 1, n is 2 or 3, and in this case, all R 1 are identical to each other, and all R 2 are identical to each other, and all A 2 8. The hardmask composition of claim 7, wherein:
10. R in Formula 1 1 are each independently a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms; R 2 is each independently a hydrogen atom or a deuterium atom, and n is 2.
11. The hard mask composition according to claim 1, wherein the compound represented by Chemical Formula 1 is at least one of compounds represented by the following Chemical Formulas 2 to 4: 【Chemistry 6】 In Chemical Formula 2 to Chemical Formula 4, R 1 each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 20 carbon atoms, or a substituted or unsubstituted aromatic hydrocarbon group having 6 to 20 carbon atoms, R 2 are each independently a hydrogen atom, a deuterium atom, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms; X 1 and X 2 each independently represents a deuterium atom, a hydroxyl group, a halogen atom, a thiol group, a substituted or unsubstituted alkoxy group having 1 to 10 carbon atoms, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms; n is independently an integer from 1 to 3; m1 and m2 each independently represent an integer of 0 to 5.
12. The hard mask composition according to claim 1, wherein the compound represented by Chemical Formula 1 is at least one of compounds represented by the following Chemical Formulas 5 to 10: 【Chemistry 7】 【Chemistry 8】
13. 2. The hard mask composition of claim 1, wherein the compound represented by Formula 1 has a molecular weight of 500 g / mol to 10,000 g / mol.
14. The hard mask composition of claim 1, wherein the compound represented by Formula 1 is present in an amount of 0.1% by weight to 30% by weight based on the total weight of the hard mask composition.
15. 2. The hard mask composition of claim 1, wherein the solvent is at least one of propylene glycol, propylene glycol diacetate, methoxypropanediol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidinone, acetylacetone, and ethyl 3-ethoxypropionate.
16. A hardmask layer comprising a cured product of the hardmask composition according to any one of claims 1 to 15.
17. forming a layer of material on a substrate; applying a hard mask composition according to any one of claims 1 to 15 onto the material layer; heat-treating the hard mask composition to form a hard mask layer; forming a photoresist layer over the hard mask layer; exposing and developing the photoresist layer to form a photoresist pattern; selectively removing the hard mask layer utilizing the photoresist pattern to expose portions of the material layer; and c) etching the exposed portions of the layer of material.
18. The method of claim 17, wherein the step of forming the hard mask layer comprises a step of performing a heat treatment at 100° C. to 1,000° C.
Citation Information
Patent Citations
Composition for hard mask formation and method for manufacturing electronic component, and compound and resin
JP2021081686A
Composition for forming resist underlayer film, resist underlayer film, formation method for resist underlayer film, production method for patterned substrate, and compound
WO2018074534A1
Hardmask composition, hardmask layer and method of forming patterns
KR1020220092160A