Polyolefin-based resin foam particle and method for producing the same
By integrating a calcium compound and phosphorus stabilizer into polyolefin resin foam particles, the issues of moldability and flame retardancy are addressed, resulting in environmentally friendly and thermally stable molded articles.
Patent Information
- Application Number
- JP2024048305
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional polyolefin resin foam molded products face issues with moldability and flame retardancy due to the presence of sulfur-containing substances, which also pose environmental concerns and affect burning rates.
Incorporation of a calcium compound, phenolic antioxidant, and phosphorus processing stabilizer into polyolefin resin foam particles, with the calcium compound not containing sulfur or halogen elements, along with optional recycled polyolefin resin, to enhance moldability and flame retardancy while minimizing environmental impact.
The solution results in polyolefin resin foam particles that produce molded articles with excellent moldability and flame retardancy, reducing thermal decomposition and environmental burden, and contributing to sustainable development goals.
Smart Images

Figure 2024144291000001 
Figure 2024144291000002 
Figure 2024144291000003
Abstract
Description
[Technical field]
[0001] The present invention relates to expanded polyolefin resin beads and a method for producing the same. [Background technology]
[0002] Polyolefin resin foamed molded articles obtained using polyolefin resin expanded particles are used in various applications, including automobile interior components and / or core materials for automobile bumpers, as well as heat insulating materials, cushioning packaging materials, returnable boxes, etc. In order to improve the flame retardancy of polyolefin resin foamed molded articles, a technique is known in which a flame retardant and a metal salt hydrate are added to the polyolefin resin (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-35949 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the above-mentioned conventional technology, the substance added to the polyolefin resin (contained in the resin composition) contains elemental sulfur, and there was room for improvement from the viewpoint of balancing the environmental load with the moldability and burning rate of the resulting foamed molded body.
[0005] One embodiment of the present invention has been made in consideration of the above-mentioned problems, and its object is to provide expanded polyolefin resin beads that can provide expanded molded articles that are excellent in moldability and flame retardancy with a small environmental impact. [Means for solving the problem]
[0006] The present inventors conducted extensive research to solve the above problems and have now completed the present invention.
[0007] That is, one embodiment of the present invention includes the following configuration. [1] A polyolefin resin foam comprising (A), a calcium compound (C1), a phenol-based antioxidant (D) and a phosphorus-based processing stabilizer (E), wherein the calcium compound (C1) is a compound that does not contain elemental sulfur or halogen, and the content of the calcium compound (C1) is 0.10% by weight to 3.00% by weight in 100% by weight of the polyolefin resin foamed particles, and the calcium compound (C1) is dispersed inside a film that constitutes bubbles of the polyolefin resin foamed particles. [2] The expanded polyolefin resin particles according to [1], wherein the calcium compound (C1) comprises at least one selected from the group consisting of calcium oxide, calcium hydroxide, calcium carbonate and fatty acid calcium. [3] The expanded polyolefin resin particles according to [1] or [2], wherein the polyolefin resin (A) includes a recycled polyolefin resin. [4] The expanded polyolefin resin particles according to any one of [1] to [3], further comprising a hindered amine (B). [5] The expanded polyolefin resin particles according to any one of [1] to [4], further comprising carbon black and / or graphite. [6] The expanded polyolefin resin particles according to any one of [1] to [5], further comprising a metal deactivator. [7] A polyolefin resin foamed molded article obtained by molding the expanded polyolefin resin beads according to any one of [1] to [6]. [8] A method for producing expanded polyolefin resin particles, comprising: a dispersing step of dispersing polyolefin resin particles made of a polyolefin resin composition containing a polyolefin resin (A), a calcium compound (C2), a phenol-based antioxidant (D) and a phosphorus-based process stabilizer (E) in an aqueous dispersion medium in a container; and a releasing step of releasing the dispersion obtained in the dispersing step into a region having a lower pressure than the pressure in the container, wherein the calcium compound (C2) is a compound containing neither elemental sulfur nor elemental halogen, and the content of the calcium compound (C2) is 0.10% by weight to 3.00% by weight in 100% by weight of the expanded polyolefin resin particles. [9] The method for producing expanded polyolefin resin particles according to [8], wherein the calcium compound (C2) comprises at least one selected from the group consisting of calcium oxide, calcium hydroxide, calcium carbonate and calcium fatty acid.
[10] The method for producing expanded polyolefin resin particles according to [8] or [9], wherein the calcium compound (C2) comprises at least one selected from the group consisting of calcium oxide and fatty acid calcium.
[11] The method for producing expanded polyolefin resin particles according to any one of [8] to
[10] , wherein the polyolefin resin (A) contains a recycled polyolefin resin.
[12] A method for producing expanded polyolefin resin beads comprising a polyolefin resin (A), a calcium compound (C1), a phenolic antioxidant (D) and a phosphorus-based processing stabilizer (E), comprising: In the container, (i) a dispersing step of dispersing polyolefin-based resin particles made of a polyolefin-based resin composition containing a polyolefin-based resin (A), (ii) a calcium compound (C1) and / or a precursor of the calcium compound (C1), (iii) a phenol-based antioxidant (D), and (iv) a phosphorus-based processing stabilizer (E) in an aqueous dispersion medium, and a blowing agent; A discharging step of discharging the dispersion obtained in the dispersing step into a region with a lower pressure than the pressure inside the container, The calcium compound (C1) is a compound that does not contain sulfur element and halogen element, The precursor of the calcium compound (C1) is a compound that does not contain a sulfur element and a halogen element, The method for producing expanded polyolefin resin beads, wherein the content of the calcium compound (C1) in the expanded polyolefin resin beads is 0.10% by weight to 3.00% by weight based on 100% by weight of the expanded polyolefin resin beads.
[13] The precursor of the calcium compound (C1) is The method for producing expanded polyolefin resin particles according to
[12] , which contains at least one selected from the group consisting of calcium oxide, calcium hydroxide, calcium carbonate and calcium fatty acid.
[14] The precursor of the calcium compound (C1) is The method for producing expanded polyolefin resin particles according to
[12] or
[13] , which contains at least one selected from the group consisting of calcium oxide and fatty acid calcium salts.
[15] The method for producing expanded polyolefin resin particles according to any one of
[12] to
[14] , wherein the polyolefin resin (A) contains a recycled polyolefin resin. Effect of the Invention
[0008] According to one embodiment of the present invention, it is possible to provide expanded polyolefin resin beads that can provide an expanded molded article having excellent moldability and flame retardancy with a small environmental impact. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims. In addition, embodiments or examples obtained by combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment. All academic documents and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more (including A and greater than A) and B or less (including B and smaller than B)".
[0010] In this specification, a constitutional unit derived from an X monomer contained in a polymer or copolymer may be referred to as an "X unit".
[0011] Unless otherwise specified in this specification, the structural unit is X 1 Units and X 2 Units, ... and X n A copolymer containing units (n is an integer of 2 or more) is referred to as "X 1 / X 2 / ··· / X n Also called "copolymer". X 1 / X 2 / ··· / X n Unless otherwise specified, the polymerization mode of the copolymer is not particularly limited, and the copolymer may be a random copolymer, an alternating copolymer, a block copolymer, or a graft copolymer.
[0012] [1. Polyolefin resin foam particles] The expanded polyolefin resin particles according to one embodiment of the present invention comprise a polyolefin resin (A), a calcium compound (C1), a phenol-based antioxidant (D) and a phosphorus-based process stabilizer (E), the calcium compound (C1) being a compound that does not contain sulfur or halogen elements, the content of the calcium compound (C1) being 0.10% by weight to 3.00% by weight relative to 100% by weight of the expanded polyolefin resin particles, and the calcium compound (C1) being dispersed within a membrane that constitutes air bubbles of the expanded polyolefin resin particles.
[0013] The expanded polyolefin resin particles according to one embodiment of the present invention have the above-mentioned structure, and therefore have the advantage that they can provide an expanded molded article having excellent moldability and flame retardancy with a small environmental impact.
[0014] Furthermore, the above-mentioned configuration can reduce pollution of water, soil, etc. Such an effect also contributes to the achievement of, for example, Goal 14 of the Sustainable Development Goals (SDGs) advocated by the United Nations, "Conserve and sustainably use the oceans and marine resources for sustainable development."
[0015] In this specification, "polyolefin-based resin particles" may be referred to as "resin particles", "polyolefin-based expanded particles" may be referred to as "expanded particles", "polyolefin-based expanded particles according to one embodiment of the present invention" may be referred to as "the present expanded particles", and "polyolefin-based resin expanded molded body" may be referred to as "expanded molded body".
[0016] In this specification, moldability means the surface aesthetics of the foamed molded article.
[0017] In this specification, the flame retardancy is evaluated by the burning rate of the foam molded article. In this specification, when at least one of the maximum burning rate and the average burning rate of the foam molded article is excellent, the flame retardancy is evaluated as excellent. The evaluation method will be described in detail later.
[0018] <Polyolefin resin (A)> In this specification, the term "polyolefin resin" refers to a resin that contains 50 mol % or more of olefin units out of 100 mol % of all structural units constituting the resin.
[0019] The polyolefin resin (A) is not particularly limited, but examples thereof include polyethylene resins and polypropylene resins. These polyolefin resins may be used alone or in combination of two or more.
[0020] (Polyethylene resin) In this specification, the term "polyethylene resin" refers to a resin that contains more than 50 mol % of ethylene units, based on 100 mol % of all structural units constituting the resin.
[0021] Examples of polyethylene resins include, but are not limited to, high-density polyethylene, medium-density polyethylene, low-density polyethylene, linear low-density polyethylene, styrene-modified polyethylene resins, ethylene / vinyl acetate copolymers, ethylene / propylene copolymers, ethylene / 1-butene copolymers, ethylene / 1-butene / propylene copolymers, ethylene / hexene copolymers, and ethylene / 4-methyl-1-pentene copolymers.
[0022] The above-mentioned ethylene-based resins may be used alone or in combination of two or more.
[0023] (Polypropylene resin) In this specification, the term "polypropylene resin" refers to a resin that contains 50 mol % or more of propylene units in 100 mol % of all structural units constituting the resin.
[0024] The polypropylene-based resin may be (i) a homopolymer of propylene, (ii) a block copolymer, alternating copolymer, random copolymer, or graft copolymer of propylene and a monomer other than propylene, or (iii) a mixture of two or more of these. A block copolymer of propylene and a monomer other than propylene is sometimes called an impact copolymer. A homopolymer of propylene, a block copolymer, alternating copolymer, and random copolymer of propylene and a monomer other than propylene are all linear polymers. It is preferable that the polypropylene-based resin is a linear polymer.
[0025] The polypropylene-based resin is preferably a random copolymer of propylene and a monomer other than propylene, since this allows the resin particles and expanded particles to be processed at a low heating temperature in the foaming step and foam molding step described below.
[0026] In addition to the propylene unit, the polypropylene resin may have one or more units, or may have one or more types, of structural units derived from monomers other than the propylene monomer. The "monomer other than the propylene monomer" used in the production of the polypropylene resin may be referred to as a "comonomer". The "structural unit derived from a monomer other than the propylene monomer" contained in the polypropylene resin may be referred to as a "comonomer unit".
[0027] Comonomers include α-olefins having 2 or 4 to 12 carbon atoms, such as ethylene, 1-butene, isobutene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3,4-dimethyl-1-butene, 1-heptene, 3-methyl-1-hexene, 1-octene, and 1-decene.
[0028] Specific examples of polypropylene-based resins include polypropylene homopolymers, ethylene / propylene random copolymers, 1-butene / propylene random copolymers, 1-butene / ethylene / propylene random copolymers, ethylene / propylene block copolymers, 1-butene / propylene block copolymers, 1-butene / ethylene / propylene block copolymers, ethylene / propylene block alternating polymers, 1-butene / propylene block alternating polymers, 1-butene / ethylene / propylene block alternating polymers, propylene / chlorinated vinyl copolymers, propylene / maleic anhydride copolymers, and styrene-modified polypropylene-based resins.
[0029] As the polypropylene-based resin, one of the above-mentioned specific examples may be used alone, or two or more may be used in combination. Among the above-mentioned specific examples, the polypropylene-based resin preferably contains an ethylene / propylene random copolymer and / or a 1-butene / ethylene / propylene random copolymer, because the resin particles obtained have good expandability and the expanded particles obtained have good moldability. Furthermore, among the above-mentioned specific examples, the polypropylene-based resin preferably contains an ethylene / propylene random copolymer and / or a 1-butene / ethylene / propylene random copolymer, because the expanded molded product can be obtained with excellent moldability and flame retardancy.
[0030] When the polypropylene-based resin is a mixture of an ethylene / propylene random copolymer and a 1-butene / ethylene / propylene random copolymer, the preferred ratio of the ethylene / propylene random copolymer in the polypropylene-based resin is not particularly limited.
[0031] The polyolefin resin (A) preferably contains 70% by weight or more of polypropylene resin, more preferably 80% by weight or more, more preferably 90% by weight or more, even more preferably 95% by weight or more, and even more preferably 98% by weight or more, based on 100% by weight of the polyolefin resin (A). The polyolefin resin (A) particularly preferably contains 100% by weight of polypropylene resin, based on 100% by weight of the polyolefin resin (A). In other words, the polyolefin resin (A) is preferably composed only of polypropylene resin. When the amount of polypropylene resin contained in the polyolefin resin (A) is within the above-mentioned range, it has the advantage that a foamed molded product with excellent flame retardancy can be obtained.
[0032] The content of the polyolefin resin (A) in the present expanded beads is not particularly limited, but is preferably 93.00% by weight to 98.00% by weight, more preferably 94.00% by weight to 97.50% by weight, further preferably 95.50% by weight to 97.00% by weight, and particularly preferably 95.00% by weight to 96.50% by weight, based on 100% by weight of the present expanded beads. This configuration has the advantages of (i) small decrease in strength of the expanded molded article, and (ii) large cell diameter, resulting in excellent moldability and beautiful appearance of the expanded molded article.
[0033] The polyolefin resin (A) preferably contains a recycled polyolefin resin.
[0034] The present inventors have newly discovered that, compared to a case in which the polyolefin-based resin does not contain recycled polyolefin-based resin, (I) the polyolefin-based resin is more susceptible to thermal decomposition in the granulation process, resulting in an increase in the MFR of the resulting resin particles, and many inter-particle spaces are observed in the foamed molded article made of the expanded beads obtained from the resin particles, and (II) the flame retardancy of the resulting foamed molded article made of the expanded beads is deteriorated.
[0035] Here, it is presumed that the flame retardancy of the foamed molded article obtained when the polyolefin resin contains the recycled polyolefin resin is deteriorated because (i) the recycled polyolefin resin is repeatedly heated in the recycling process, which reduces its molecular weight and makes it prone to decomposition and volatilization, and (ii) the impurities contained in the recycled material containing the recycled polyolefin resin promote the decomposition of the recycled polyolefin resin and cancel the effect of the flame retardant. However, one embodiment of the present invention is not limited to such a presumption.
[0036] Therefore, in the course of intensive research, the present inventors have attempted to suppress the increase in MFR of the resulting resin particles by using an antioxidant when producing polyolefin-based resin particles containing recycled polyolefin-based resin, but have not seen sufficient improvement.In addition, in the course of intensive research, the present inventors have attempted to improve the flame retardancy of the resulting foamed molded product by increasing the amount of existing flame retardants and using two or more existing flame retardants in combination in the production of expanded particles made of polyolefin-based resin containing recycled polyolefin-based resin, but have not seen any improvement.
[0037] In addition, recycled materials (recycled materials containing recycled polyolefin resins) available on the market may contain carbon black. On the other hand, it has been generally known that polyolefin resin foam particles containing carbon black have poor flame retardancy.
[0038] As a result of intensive investigation, the present inventors have found that even when the polyolefin resin (A) contains recycled polyolefin resin, if the expanded polyolefin resin particles contain a calcium compound (C1), a phenol-based antioxidant (D) and a phosphorus-based process stabilizer (E), the calcium compound (C1) is a compound that does not contain elemental sulfur or halogen, the content of the calcium compound (C1) is 0.10% by weight to 3.00% by weight in 100% by weight of the expanded polyolefin resin particles, and the calcium compound (C1) is dispersed inside the membrane that constitutes the bubbles, then the polyolefin resin is prevented from thermally decomposing in the granulation step and the MFR is prevented from increasing, and the resulting expanded molded article has excellent moldability and flame retardancy.
[0039] Furthermore, the present inventors have newly discovered that even when the expanded beads contain carbon black, if the expanded polyolefin resin beads contain a calcium compound (C1), a phenol-based antioxidant (D) and a phosphorus-based process stabilizer (E), the calcium compound (C1) is a compound that does not contain elemental sulfur or halogen, the content of the calcium compound (C1) is 0.10% by weight to 3.00% by weight in 100% by weight of the expanded polyolefin resin beads, the calcium compound (C1) is dispersed inside the film that constitutes the bubbles, and the expanded beads contain a hindered amine (B), the resulting expanded molded article has excellent moldability and flame retardancy.
[0040] In addition, when the polyolefin resin (A) contains recycled polyolefin resin, the amount of plastic waste generated and the amount of plastic used in production can be reduced. Such an effect contributes to the achievement of, for example, Goal 12 of the Sustainable Development Goals (SDGs) advocated by the United Nations, "Ensure sustainable consumption and production patterns."
[0041] In this specification, the term "recycled polyolefin resin" refers to polyolefin resin that has been once or more in the form of a polyolefin resin product (e.g., foam particles; foam molded products; films; food trays; packaging containers such as bags and bottles; medical containers such as intravenous packs and syringes; costume cases; miscellaneous goods such as clear files; home appliances; automobile parts; etc.) and then used and / or discarded, and that has been re-formed into polyolefin resin (or polyolefin resin pellets) by any means (e.g., crushing, shredding, melting, and combinations thereof, etc.); and (ii) polyolefin resin that has been re-formed into polyolefin resin (or polyolefin resin pellets) by any means (e.g., crushing, shredding, melting, and combinations thereof, etc.) from waste generated in the production process of polyolefin resin products.
[0042] In this specification, the term "non-recycled polyolefin resin" refers to a polyolefin resin that has never been in the form of a polyolefin resin product.
[0043] When the polyolefin resin (A) contains a recycled polyolefin resin, the content of the recycled polyolefin resin in the present expanded beads is not particularly limited, but is preferably 10% by weight to 100% by weight, more preferably 20% by weight to 70% by weight, and even more preferably 25% by weight to 50% by weight, based on the weight percent of the polyolefin resin (A). This configuration has the advantage of being able to further reduce the burden on the environment.
[0044] (Other resins) In one embodiment of the present invention, the expanded beads may further contain a resin other than the polyolefin resin (A) (sometimes referred to as "other resins" in this specification) within a range that does not impair the effect of one embodiment of the present invention. Examples of other resins include styrene resins (polystyrene, styrene / maleic anhydride copolymers, styrene / ethylene copolymers, etc.).
[0045] When the present expanded beads contain other resins, the content of the other resins in the present expanded beads is not particularly limited, but is preferably 1 to 10 parts by weight, more preferably 2 to 5 parts by weight, relative to 100 parts by weight of the polyolefin resin (A). Since a polyolefin resin foam molded article having better flame retardancy can be provided, the content of the other resins in the expanded beads is preferably 5 parts by weight or less relative to 100 parts by weight of the polyolefin resin (A). In other words, the polyolefin resin particles further have a resin other than the polyolefin resin (A), and the content of the other resins is preferably 5 parts by weight or less relative to 100 parts by weight of the polyolefin resin (A). Since a polyolefin resin foam molded article having better flame retardancy can be provided, the content of the other resins in the expanded beads is more preferably 4 parts by weight or less, more preferably 3 parts by weight or less, more preferably 2 parts by weight or less, even more preferably 1 part by weight or less, and particularly preferably 0.1 parts by weight or less, relative to 100 parts by weight of the polyolefin resin (A). The content of other resins in the resin particles being 0.1 parts by weight or less per 100 parts by weight of the polyolefin resin (A) means that the expanded particles (resin particles) do not substantially contain other resins.
[0046] (Physical Properties) The melt flow rate (MFR) of the polyolefin resin (A) at 230±0.2° C. is not particularly limited, but is preferably 1 g / 10 min to 40 g / 10 min, more preferably 2 g / 10 min to 35 g / 10 min, even more preferably 3 g / 10 min to 30 g / 10 min, and particularly preferably 3 g / 10 min to 10 g / 10 min. The MFR may also be referred to as “melt index (MI)”. When the MFR of the polyolefin resin (A) is 1 g / 10 min or more, it has the advantage that it is easy to increase the expansion ratio of the expanded beads in the production of the present expanded beads. When the MFR of the polyolefin resin (A) is 30 g / 10 min or less, there is no risk of the cells of the obtained expanded beads becoming interconnected, and as a result, there is the advantage that (i) the compressive strength of the expanded molded article obtained from the present expanded beads tends to be good, or (ii) the surface beauty of the expanded molded article tends to be good. The method for measuring the MFR of the polyolefin resin will be described in detail in the Examples below.
[0047] The melting point of the polyolefin resin (A) is not particularly limited, but is preferably 135°C to 160°C, more preferably 137°C to 155°C, and even more preferably 139°C to 153°C. When the melting point of the polyolefin resin (A) is (i) 135°C or higher, the expanded molded article obtained from the expanded beads has an advantage of having excellent heat resistance, and (ii) when it is 160°C or lower, the expansion ratio of the expanded beads can be easily increased in the production of the expanded beads. The method for measuring the melting point of the polyolefin resin (A) will be described in detail in the Examples below.
[0048] <Hindered amine (B)> The expanded polyolefin resin beads according to one embodiment of the present invention preferably contain a hindered amine (B).
[0049] (Hindered amine) In this specification, the term "hindered amine" refers to a hindered amine having an OR group (wherein R is a saturated or unsaturated monovalent hydrocarbon group) directly substituted on the N atom (hereinafter, may be referred to as an N-substituted hindered amine). The hindered amine is not particularly limited as long as it is a hindered amine having an OR group directly substituted on the N atom, and known hindered amines may be used. As the hindered amine, one type of hindered amine may be used alone, or two or more types of hindered amines may be used in combination.
[0050] As the hindered amine, an N-substituted hindered amine containing a triazine component (hereinafter, sometimes referred to as a "triazine skeleton-containing hindered amine") is preferable because it can exert a flame retardant effect over a wide temperature range. The triazine skeleton-containing hindered amine is not particularly limited, but includes (i) a compound having a CAS number of 191680-81-6 ((i-1) a reaction product of a product obtained by reacting a reaction product of peroxidized N-butyl-2,2,6,6-tetramethyl-4-piperidinamine and 2,4,6-trichloro-1,3,5-triazine with cyclohexane, and N,N'-bis(3-aminopropyl)ethylenediamine, (i-2) 2,4-bis((1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)butyl (i-3) N,N',N'''-tris{2,4-bis[(1-hydrocarbyloxy-2,2,6,6-tetramethylpiperidin-4-yl)alkylamino]-s-triazin-6-yl}-3,3'-ethylenediiminodipropylamine, and / or (ii) bis(1-undecaneoxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate are preferred. Also, isomers of the above-mentioned triazine skeleton-containing hindered amines and crosslinked derivatives of the above-mentioned triazine skeleton-containing hindered amines can be used. More details about triazine skeleton-containing hindered amines are disclosed in European Patent No. 0889085, page 2, line 32 to page 4, line 6.
[0051] As the triazine skeleton-containing hindered amine, commercially available products can be suitably used. Commercially available products of the triazine skeleton-containing hindered amine include BASF's FLAMESTAB (registered trademark) NOR116 (a compound with CAS number 191680-81-6), CLARIANT's HOSTAVIN (registered trademark) NOW XP, and Adeka Corporation's Adeka STAB LA-81 (bis(1-undecaneoxy-2,2,6,6-tetramethylpiperidin-4-yl) carbonate).
[0052] In one embodiment of the present invention, the hindered amine may be a compound represented by the following structural formula (iv):
[0053] [ka]
[0054] In the above structural formula (iv), G 1 and G 2 is independently 1-8 an alkyl group, or pentamethylene; Z 1 and Z 2 are methyl groups or Z 1 and Z 2 together form a linking moiety, which may be additionally substituted with an ester, ether, amide, amino, carboxy or urethane group; and E is C 1-8 Alkoxy group, C 5-12 Cycloalkoxy group C 7-15 Aralkoxy group, -OC(O)-C 1-18 Alkyl group, or -OT-(OH) b group; where T is (i) C 1-18 (ii) an alkylene chain, 5-18 cycloalkylene chain, (iii) C 5-18 a cycloalkenylene chain, or (iv) a phenyl group or C 1-4 C substituted with alkyl-substituted phenyl groups 1-4 an alkylene chain; b is 1 to 3 and is not greater than the number of carbon atoms in T, and when b is 2 or 3, each hydroxyl group is linked to a different carbon atom in T.
[0055] The compound represented by the above structural formula (iv) is disclosed in more detail in EP 2225318, more specifically, in EP 2225318, from line 35 on page 5 to line 48 on page 25.
[0056] In one embodiment of the present invention, the hindered amine may be a compound represented by the following structural formula (v):
[0057] [ka]
[0058] In the above structural formula (v), R is hydrogen or a methyl group, and R 1 is C 1-18 Alkyl group, C 2-18 Alkenyl group, C 2-18 Alkynyl group, C 5-12 Cycloalkyl groups, C 5-8 Cycloalkenyl group, C 6-10 Aryl group or C 7-9 It is an aralkyl group.
[0059] The compound represented by the above structural formula (v) is disclosed in more detail in European Patent No. 0309402, from page 3, line 33 to page 8, line 58.
[0060] In one embodiment of the present invention, the hindered amine may be a compound represented by the following structural formula (vi):
[0061] [ka]
[0062] In the above structural formula (vi), E, k, Y, W, R1 to R7, and G1 to G4 are as defined in the specification of US Pat. No. 8,598,369.
[0063] The compound represented by the above structural formula (vi) is disclosed in more detail in Examples 1 to 12 and Tables 1 to 5 of US Pat. No. 8,598,369.
[0064] The content of the hindered amine (B) in the present expanded beads is not particularly limited, but is preferably 0.01% by weight to 3.00% by weight, more preferably 0.03% by weight to 1.00% by weight, more preferably 0.05% by weight to 0.75% by weight, even more preferably 0.07% by weight to 0.50% by weight, and particularly preferably 0.10% by weight to 0.25% by weight, based on 100% by weight of the expanded beads. This configuration has the advantage that an expanded molded product with excellent flame retardancy can be obtained.
[0065] <Calcium Compounds (C1)> The expanded polyolefin resin particles according to one embodiment of the present invention contain a calcium compound (C1) (the calcium compound (C1) is a compound that does not contain sulfur or halogen elements). This configuration has an advantage that it is possible to obtain an expanded molded product with excellent flame retardancy.
[0066] The calcium compound (C1) refers to a compound that contains calcium but does not contain sulfur or halogen elements.
[0067] The calcium compound (C1) may be a compound derived from the calcium compound (C2) described later. The calcium compound (C1) may be (I) the same compound as the calcium compound (C2) described later, or (II) a compound obtained by reacting the calcium compound (C2) described later with water or a blowing agent present in a pressure vessel in the production process of the present expanded beads.
[0068] Therefore, it is preferred that the calcium compound (C1) is either (i) the same compound as the calcium compound (C2), (ii) a hydrate of the calcium compound (C2), or (iii) a carbonate of the calcium compound (C2).
[0069] The calcium compound (C2) will be described in the section entitled "Calcium compound (C2)" in "2. Method for producing expanded polyolefin resin beads" below, and the description therein will be incorporated by reference, so a detailed description will be omitted here.
[0070] The calcium compound (C1) is, for example, a compound that does not contain sulfur element and halogen element, and is preferably one or more compounds selected from the group consisting of calcium salts (e.g., anhydrous inorganic salts containing calcium, hydrates of inorganic salts containing calcium, organic salts containing calcium, hydrates of organic salts containing calcium, etc.), calcium hydroxide, calcium oxide, calcium peroxide, and calcium carbide.
[0071] The "anhydride of an inorganic salt containing calcium" and "hydrate of an inorganic salt containing calcium" contained in the calcium compound (C1) are preferably at least one selected from the group consisting of, for example, calcium carbonate, calcium hydrogen carbonate, calcium phosphite, monocalcium aluminosilicate, dicalcium aluminosilicate, monocalcium aluminate, tricalcium aluminate, dicalcium silicate, tricalcium silicate, calcium hypophosphite, calcium hydroxide phosphate, magnesium calcium carbonate, calcium diphosphate, pentacalcium hexasilicate, hexacalcium hexasilicate, calcium hexafluorosilicate, calcium metasilicate, magnesium calcium metasilicate, calcium metaphosphate, tricalcium phosphate, tetracalcium phosphate, octacalcium phosphate, calcium monohydrogen phosphate, calcium dihydrogen phosphate, and hydrates thereof.
[0072] Furthermore, the "anhydride of an organic salt containing calcium" and the "hydrate of an organic salt containing calcium" contained in the calcium compound (C1) are preferably, for example, one or more types selected from the group consisting of fatty acid calcium and hydrates thereof.
[0073] The fatty acid calcium that can be contained in the calcium compound (C1) is preferably, for example, one or more types selected from the group consisting of calcium acetate, calcium citrate, calcium oxalate, and calcium stearate.
[0074] The expanded beads may contain only one type of the calcium compound described above, or may contain two or more types.
[0075] The calcium compound (C1) preferably contains one or more selected from the group consisting of calcium oxide, calcium hydroxide, calcium carbonate, and fatty acid calcium. In other words, the resin particles, which are the raw material of the expanded particles, preferably contain a calcium compound (C2) described below. This configuration has the advantages that in the granulation step for producing the resin particles, thermal decomposition of the polyolefin resin is suppressed, the MFR of the resin particles is less likely to increase, and an expanded molded product having excellent long-term thermal stability and flame retardancy can be obtained.
[0076] The content of the calcium compound (C1) in the expanded beads is 0.10% by weight to 3.00% by weight, more preferably 0.12% by weight to 3.00% by weight, still more preferably 0.14% by weight to 3.00% by weight, even more preferably 0.16% by weight to 3.00% by weight, and particularly preferably 0.18% by weight to 3.00% by weight, based on 100% by weight of the expanded beads. This configuration has the advantage that an expanded molded product having excellent flame retardancy can be obtained.
[0077] When the calcium compound (C1) contains one or more selected from the group consisting of calcium oxide, calcium hydroxide, and calcium carbonate, the total content of calcium oxide, calcium hydroxide, and calcium carbonate in 100% by weight of the expanded beads is preferably 0.03% by weight or more, more preferably 0.05% by weight or more, more preferably 0.10% by weight or more, more preferably 0.12% by weight or more, even more preferably 0.14% by weight or more, and particularly preferably 0.15% by weight or more. This configuration has the advantages that in the granulation step for producing the resin particles, the thermal decomposition of the polyolefin resin is suppressed, the MFR of the resin particles is less likely to increase, and an expanded molded product excellent in long-term thermal stability, flame retardancy, and surface beauty can be obtained.
[0078] When the calcium compound (C1) contains fatty acid calcium (containing neither sulfur nor halogen), the content of fatty acid calcium (containing neither sulfur nor halogen) is not particularly limited, but is preferably 0.01% by weight or more, more preferably 0.02% by weight or more, even more preferably 0.03% by weight or more, and particularly preferably 0.04% by weight or more, based on 100% by weight of the expanded beads. This configuration has the advantages that the thermal decomposition of the polyolefin resin is suppressed in the granulation step for producing the resin beads, the MFR of the resin beads is less likely to increase, and an expanded molded product having excellent long-term thermal stability, flame retardancy, and surface beauty can be obtained.
[0079] In one embodiment of the present invention, the calcium compound (C1) is dispersed inside the film constituting the bubbles (the film itself). In other words, the calcium compound (C1) is intended not to be present on the surface and / or periphery of the film constituting the bubbles. This configuration has the advantage that it is possible to obtain a foamed molded product with excellent flame retardancy and surface beauty. In addition, as in the granulation process described below, when a resin composition containing a polyolefin resin (A) and a calcium compound (C2) is melt-kneaded to obtain resin particles, and the resin particles are used to perform, for example, a dispersion process and a release process described below to obtain expanded beads, the calcium compound (C1) is dispersed inside the film constituting the bubbles of the expanded beads in the obtained expanded beads. In addition, by analyzing a cross section of the film constituting the bubbles of the expanded beads using a scanning electron microscope energy dispersive X-ray spectroscopy [SEM-EDX], it can be confirmed whether or not the calcium compound is dispersed inside the film constituting the bubbles of the expanded beads.
[0080] <Phenol-based antioxidants (D)> The expanded polyolefin resin particles contain a phenol-based antioxidant (D). This composition has the advantage that, in the granulation process for producing the resin particles, thermal decomposition of the polyolefin resin is suppressed, the MFR of the resin particles is less likely to increase, and an expanded molded product having excellent long-term thermal stability, surface beauty, and flame retardancy can be obtained.
[0081] The phenol-based antioxidant is not particularly limited, but is preferably at least one selected from the group consisting of tetrakis[methylene-3-(3',5'-di-t-butyl-4-hydroxyphenyl)propionate]methane, tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, n-octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, and 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane. Among these, tetrakis[3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]pentaerythritol is more preferable. According to this configuration, in the granulation process for producing the resin particles, the thermal decomposition of the polyolefin resin is suppressed, the MFR of the resin particles is less likely to increase, and it is possible to obtain a foamed molded product having excellent long-term thermal stability, surface beauty, and flame retardancy.
[0082] As the phenol-based antioxidant (D), commercially available products can also be suitably used. As commercially available products of the phenol-based antioxidant (D), it is preferable to use one or more selected from the group consisting of "Irganox 1010" manufactured by BASF (tetrakis [methylene-3-(3',5'-di-t-butyl-4-hydroxyphenyl) propionate] methane), "Irganox 1076" manufactured by BASF (octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl) propionate), and "Irganox 3114" manufactured by BASF and "ADEKA STAB AO-20" (1,3,5-tris (3,5-di-t-butyl-4-hydroxybenzyl) 1,3,5-triazine-2,4,6 (1H,3H,5H)-trione) manufactured by ADEKA. This configuration has the advantage that a foamed molded product with excellent flame retardancy can be obtained.
[0083] In the present expanded beads, the above-mentioned phenolic antioxidant (D) may be contained alone or in combination of two or more kinds.
[0084] The content of the phenol-based antioxidant (D) in the present expanded beads is not particularly limited, but is preferably 0.01% by weight to 1.00% by weight, more preferably 0.03% by weight to 0.50% by weight, more preferably 0.05% by weight to 0.30% by weight, and even more preferably 0.05% by weight to 0.20% by weight, based on 100% by weight of the expanded beads. This configuration has the advantage that the thermal decomposition of the polyolefin-based resin is suppressed in the granulation step for producing the resin particles, the MFR of the resin particles is less likely to increase, and an expanded molded product having excellent long-term thermal stability, surface beauty, and flame retardancy can be obtained.
[0085] <Phosphorus-based processing stabilizer (E)> The expanded polyolefin resin particles contain a phosphorus-based processing stabilizer (E). This configuration has the advantage that in the granulation process for producing the resin particles, thermal decomposition of the polyolefin resin is suppressed, the MFR of the resin particles is less likely to increase, and an expanded molded product having excellent long-term thermal stability, surface beauty, and flame retardancy can be obtained.
[0086] The phosphorus-based processing stabilizer is not particularly limited, but is preferably a trivalent phosphorus compound, for example, one or more selected from the group consisting of tris(2,4-di-t-butylphenyl)phosphite, bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite, and tris(mono, dinonylphenyl)phosphite. Among these, tris(2,4-di-t-butylphenyl)phosphite is more preferable. According to this configuration, in the granulation process for producing resin particles, the thermal decomposition of the polyolefin resin is suppressed, the MFR of the resin particles is less likely to increase, and it is advantageous in that a foamed molded product having excellent long-term thermal stability, surface beauty, and flame retardancy can be obtained.
[0087] Commercially available products can also be suitably used as the phosphorus-based processing stabilizer (E). The commercially available phosphorus-based processing stabilizer (E) is preferably one or more selected from the group consisting of "Irgafos 168" (tris(2,4-di-t-butylphenyl)phosphite) manufactured by BASF and "Adekastab PEP-24G" (bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite) manufactured by ADEKA. This configuration has the advantage that in the granulation process for producing resin particles, the thermal decomposition of the polyolefin resin is suppressed, the MFR of the resin particles is less likely to increase, and a foamed molded product having excellent long-term thermal stability, surface beauty, and flame retardancy can be obtained.
[0088] The expanded beads may contain only one type of phosphorus-based process stabilizer (E) or a combination of two or more types.
[0089] The content of the phosphorus-based processing stabilizer (E) in the present expanded beads is not particularly limited, but is preferably 0.01% by weight to 1.00% by weight, more preferably 0.03% by weight to 0.50% by weight, more preferably 0.05% by weight to 0.30% by weight, and even more preferably 0.07% by weight to 0.20% by weight, based on 100% by weight of the expanded beads. This configuration has the advantage that in the granulation step for producing the resin beads, thermal decomposition of the polyolefin resin is suppressed, the MFR of the resin beads is less likely to increase, and an expanded molded product having excellent long-term thermal stability, surface beauty, and flame retardancy can be obtained.
[0090] <Other additives> In one embodiment of the present invention, the expanded particles may contain other additives in addition to the polyolefin resin (A), the hindered amine (B), the calcium compound (C1), the phenolic antioxidant (D), and the phosphorus-based processing stabilizer (E), as long as the effect of one embodiment of the present invention is not impaired. Examples of additives include colorants, hydrophilic compounds, crystal nucleating agents, antistatic agents, flame retardants, antioxidants, light stabilizers, conductive agents, lubricants, carbon black, powdered activated carbon, metal deactivators, and the like. Such additives may be added to the resin particles obtained by adding them to the resin composition, or may be added directly to the dispersion when the resin particles are expanded.
[0091] The hydrophilic compound is a substance used for the purpose of increasing the amount of water impregnated in the resin particles. When the resin composition contains the hydrophilic compound, the resin particles can be given foamability. The foamability imparting effect of the hydrophilic compound to the resin particles is particularly remarkable when water is used as a foaming agent.
[0092] Examples of hydrophilic compounds that can be used in one embodiment of the present invention include glycerin, polyethylene glycol, C12 to C18 aliphatic alcohols (e.g., pentaerythritol, cetyl alcohol, stearyl alcohol), melamine, isocyanuric acid, melamine-isocyanuric acid condensates, borax, zinc borate, etc. One of these hydrophilic compounds may be used alone, or two or more may be mixed and used. In addition, when two or more hydrophilic compounds are mixed and used, the mixing ratio may be appropriately adjusted depending on the purpose.
[0093] The content of the hydrophilic compound in the expanded beads is preferably 0.01% by weight to 1.00% by weight, more preferably 0.05% by weight to 0.70% by weight, and even more preferably 0.10% by weight to 0.60% by weight, based on 100% by weight of the expanded beads. When the content of the hydrophilic compound is (i) 0.01% by weight or more, the foaming effect of the hydrophilic compound can be sufficiently obtained, and (ii) when it is 1.00% by weight or less, there is no risk of the obtained expanded beads excessively shrinking.
[0094] The crystal nucleating agent to be blended in the resin composition is a substance that can become an expansion nucleus when the resin particles are expanded. The expanded particles preferably contain a crystal nucleating agent.
[0095] Examples of the crystal nucleating agent that can be used in one embodiment of the present invention include talc, feldspar, zeolite, mica, silica, kaolin, barium sulfate, aluminum hydroxide, aluminum oxide, titanium oxide, bentonite, zinc borate, etc. It should be noted that one of these crystal nucleating agents may be used alone, or two or more may be used in combination. In addition, when two or more crystal nucleating agents are used in combination, the mixing ratio may be appropriately adjusted according to the purpose.
[0096] The content of the crystal nucleating agent in the expanded beads is preferably 0.01 to 2.00% by weight, more preferably 0.02 to 1.00% by weight, and even more preferably 0.03 to 0.50% by weight, relative to 100% by weight of the expanded beads, from the viewpoint of uniformity of the average cell diameter.
[0097] The present expanded beads preferably contain carbon black and / or graphite in order to color the resulting expanded molded article gray or black.
[0098] In the present expanded beads, the average particle size of the primary particles of the carbon black is preferably 10 nm to 200 nm, more preferably 15 nm to 150 nm, further preferably 20 nm to 100 nm, and particularly preferably 20 nm to 50 nm. According to this configuration, even when the amount of carbon black added is small, a foamed molded article with high blackness can be obtained, and the foamed molded article has the advantage of being excellent in flame retardancy.
[0099] The carbon black content in the expanded beads is not particularly limited, but is preferably 2.00% by weight to 5.00% by weight, more preferably 2.00% by weight to 4.00% by weight, and even more preferably 2.50% by weight to 3.50% by weight, based on 100% by weight of the expanded beads. When the carbon black content in 100% by weight of the expanded beads is 2.00% by weight or more, the blackness of the resulting expanded molded article tends to be good. When the carbon black content in 100% by weight of the expanded beads is 5.00% by weight or less, the flame retardancy of the resulting expanded molded article tends to be good.
[0100] The metal deactivator refers to a substance capable of capturing metal ions. Specifically, the metal deactivator refers to a substance capable of forming an ionic bond with a metal ion or forming a complex with a metal ion.
[0101] The present expanded beads preferably further contain a metal deactivator. When the present expanded beads contain a metal deactivator, it has the advantage of being able to reduce accelerated deterioration of the expanded beads or the expanded molded article due to oxidation caused by metal ions. The recycled polyolefin resin may contain metal ions. Therefore, when the present expanded beads contain a recycled polyolefin resin as the polyolefin resin (A), it is particularly preferable that the expanded beads further contain a metal deactivator.
[0102] The metal deactivator is not particularly limited as long as it can capture metal ions, and examples thereof include 2-hydroxy-N-1H-1,2,4-triazol-3-ylbenzamide, N'1,N'12-bis(2-hydroxybenzoyl)dodecane dihydrazide, N,N'-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, 1,3,5-triazine-2,4,6-triamine, 2',3-bis[[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionyl]]propionohydrazide, EDTA, and EDTA-2Na. Commercially available products may be used as the metal deactivator. Commercially available products that can be used as metal deactivators include IRGANOX (registered trademark) MD1024 manufactured by BASF, and ADK STAB (registered trademark) CDA-1, ADK STAB (registered trademark) CDA-1M, ADK STAB (registered trademark) CDA-6S, ADK STAB (registered trademark) CDA-10, and ADK STAB (registered trademark) ZS series manufactured by ADEKA.
[0103] <Physical Properties> (MFR of polyolefin resin particles) The MFR of the polyolefin resin particles according to one embodiment of the present invention is not particularly limited, but is more preferably 3 g / 10 min to 35 g / 10 min, further preferably 5 g / 10 min to 25 g / 10 min, and particularly preferably 7 g / 10 min to 15 g / 10 min. When the MFR of the polyolefin resin particles is 3 g / 10 min or more, there is an advantage that it is easy to increase the expansion ratio of the expanded beads in the production of the expanded beads. When the MFR of the polyolefin resin particles is 35 g / 10 min or less, there is no risk of the cells of the resulting expanded beads becoming interconnected, and as a result, (i) the compressive strength of the expanded molded article obtained from the expanded beads tends to be good, or (ii) the surface beauty of the expanded molded article tends to be good. The method for measuring the MFR of the polyolefin resin particles will be described in detail in the examples below.
[0104] (Oxygen index of polyolefin resin particles) The oxygen index of the polyolefin-based resin particles according to one embodiment of the present invention is not particularly limited, but is preferably 18.7% or more, more preferably 19.0% or more, even more preferably 19.1% or more, and particularly preferably 19.2% or more. The higher the oxygen index of the resin particles, the higher the flame retardancy of the foamed molded product tends to be. The method for measuring the oxygen index of the polyolefin-based resin particles will be described in detail in the examples below.
[0105] (DSC ratio of polyolefin resin foam particles) The DSC ratio of the present expanded beads is not particularly limited, but is preferably 10.0% to 50.0%, more preferably 15.0% to 40.0%, further preferably 18.0% to 30.0%, and particularly preferably 20.0% to 25.0%. When the DSC ratio of the expanded beads is 10.0% or more, the expanded beads have an advantage that they can provide an expanded molded article having sufficient strength. On the other hand, when the DSC ratio of the expanded beads is 40.0% or less, the expanded beads have an advantage that they can be molded at a relatively low temperature (molding temperature) to provide an expanded molded article. The method for measuring the DSC ratio of the expanded beads will be described in detail in the examples below.
[0106] (Bulk density of polyolefin resin foam particles) The bulk density of the present expanded beads is not particularly limited, but is preferably 15.0 g / L to 55.0 g / L, more preferably 20.0 g / L to 40.0 g / L, and even more preferably 20.0 g / L to 30.0 g / L. In addition, within the range of 20.0 g / L to 30.0 g / L, the larger the bulk density, the slower the burning rate of the foam tends to be. When the bulk density is less than 15.0 g / L, the resulting foamed molded body of the polyolefin resin tends to shrink or deform easily, and the mechanical performance tends to decrease. In this specification, the foamed molded body tends to shrink or deform easily, which means that the dimensional shrinkage rate or deformation shrinkage rate of the molded body tends to be large. When the bulk density exceeds 55.0 g / L, the mechanical strength of the resulting in-mold expanded molded body tends to be high, but the advantage of reducing the weight of the in-mold expanded molded body is not obtained, and the flexibility and cushioning properties of the resulting in-mold expanded molded body tend to be insufficient. In this specification, the mechanical strength of the in-mold foam tends to be high, which means that the dimensional shrinkage of the in-mold foam tends to be suppressed. The method for measuring the bulk density of the expanded beads will be described in detail in the Examples below.
[0107] 2. Method for producing expanded polyolefin resin particles A method for producing expanded polyolefin resin beads according to one embodiment of the present invention includes a dispersing step of dispersing polyolefin resin particles made of a polyolefin resin composition containing a polyolefin resin (A), a calcium compound (C2), a phenol-based antioxidant (D) and a phosphorus-based process stabilizer (E) and a blowing agent in an aqueous dispersion medium in a container, and a releasing step of releasing the dispersion obtained in the dispersing step into a region of a lower pressure than the pressure in the container, wherein the calcium compound (C2) is a compound that does not contain elemental sulfur or elemental halogen, and the content of the calcium compound (C2) is 0.10% by weight to 3.00% by weight in 100% by weight of the expanded polyolefin resin beads.
[0108] Another embodiment of the present invention relates to a method for producing expanded polyolefin resin beads comprising a polyolefin resin (A), a calcium compound (C1), a phenol-based antioxidant (D) and a phosphorus-based process stabilizer (E), and the method comprises the steps of: (i) producing a polyolefin resin (A), a calcium compound (C1) and / or a precursor of the calcium compound (C1), (iii) a phenol-based antioxidant (D) and (iv) a phosphorus-based process stabilizer (E) from a polyolefin resin composition in a vessel; The method includes a dispersing step of dispersing polyolefin resin particles and a blowing agent in an aqueous dispersion medium, and a releasing step of releasing the dispersion obtained in the dispersing step into a region having a lower pressure than the pressure inside the container, wherein the calcium compound (C1) is a compound not containing elemental sulfur or elemental halogen, and the precursor of the calcium compound (C1) is a compound not containing elemental sulfur or elemental halogen, and the content of the calcium compound (C1) in the expanded polyolefin resin particles is 0.10% by weight to 3.00% by weight based on 100% by weight of the expanded polyolefin resin particles.
[0109] In this specification, the "polyolefin resin composition" may be referred to as the "resin composition", and the "method for producing expanded polyolefin resin beads according to one embodiment of the present invention" may be referred to as the "present production method".
[0110] Because the present manufacturing method has the above-mentioned configuration, it has the advantage that, in the granulation process for producing resin particles, thermal decomposition of the polyolefin-based resin is suppressed, and the MFR of the resin particles is less likely to increase, and polyolefin-based resin foam particles can be provided that can provide foamed molded articles that have excellent long-term thermal stability, surface beauty, and flame retardancy, with a small environmental impact.
[0111] In the present production method, the polyolefin resin (A) may contain a recycled polyolefin resin. According to the present production method, even when the polyolefin resin (A) contains a recycled polyolefin resin, the thermal decomposition of the polyolefin resin is suppressed in the granulation step for producing the resin particles, the MFR of the resin particles is unlikely to increase, and the obtained foamed molded article has the advantages of being excellent in long-term thermal stability, surface beauty, and flame retardancy.
[0112] <Calcium compounds (C2)> In the present production method, the polyolefin resin composition contains a calcium compound (C2), and the calcium compound (C2) is dispersed within the resin composition.
[0113] The calcium compound (C2) is intended to mean a compound that contains calcium but does not contain sulfur and halogen elements. In this specification, the "calcium compound (C2)" may also be referred to as the "precursor of the calcium compound (C1)", and the terms "calcium compound (C2)" and "precursor of the calcium compound (C1)" are interchangeable. In other words, in this specification, the explanation of the "calcium compound (C2)" can be replaced with the explanation of the "precursor of the calcium compound (C1)".
[0114] The calcium compound (C2) is preferably a compound that does not contain sulfur element and halogen element, and is, for example, one or more compounds selected from the group consisting of calcium salts (e.g., anhydrous inorganic salts containing calcium, hydrates of inorganic salts containing calcium, organic salts containing calcium, hydrates of organic salts containing calcium, etc.), calcium hydroxide, calcium oxide, calcium peroxide, and calcium carbide.
[0115] The "anhydride of an inorganic salt containing calcium" and "hydrate of an inorganic salt containing calcium" contained in the calcium compound (C2) are preferably at least one selected from the group consisting of, for example, calcium carbonate, calcium hydrogen carbonate, calcium phosphite, monocalcium aluminosilicate, dicalcium aluminosilicate, monocalcium aluminate, tricalcium aluminate, dicalcium silicate, tricalcium silicate, calcium hypophosphite, calcium hydroxide phosphate, magnesium calcium carbonate, calcium diphosphate, pentacalcium hexasilicate, hexacalcium hexasilicate, calcium hexafluorosilicate, calcium metasilicate, magnesium calcium metasilicate, calcium metaphosphate, tricalcium phosphate, tetracalcium phosphate, octacalcium phosphate, calcium monohydrogen phosphate, calcium dihydrogen phosphate, and hydrates thereof.
[0116] Furthermore, the "anhydride of an organic salt containing calcium" and the "hydrate of an organic salt containing calcium" contained in the calcium compound (C2) are preferably, for example, one or more types selected from the group consisting of fatty acid calcium and hydrates thereof.
[0117] In the heating step of the present manufacturing method, the resin particles are dispersed in an aqueous dispersant. Therefore, the calcium compound (C2) contained in the resin particles may change to a hydrate of the calcium compound (C2) during the manufacturing process. As a result, the expanded particles obtained by the manufacturing method (the present expanded particles) may contain a hydrate of the calcium compound (C2) used as the calcium compound (C1). Furthermore, when carbon dioxide is used as a blowing agent in the heating step of the present manufacturing method, the calcium compound (C2) contained in the resin particles may change to a carbonate of the calcium compound (C2) during the manufacturing process. As a result, the expanded particles obtained by the manufacturing method (the present expanded particles) may contain a carbonate of the calcium compound (C2) used as the calcium compound (C1).
[0118] The above calcium compounds (C2) may be used alone or in combination of two or more.
[0119] The calcium compound (C2) preferably contains at least one selected from the group consisting of calcium oxide, calcium hydroxide, calcium carbonate, and fatty acid calcium. This configuration has the advantage that a foamed molded article having excellent flame retardancy can be obtained.
[0120] The calcium compound (C2) is preferably calcium oxide and / or fatty acid calcium. That is, the calcium compound (C2) preferably contains one or more compounds selected from the group consisting of calcium oxide and fatty acid calcium. This configuration has the advantage that a foamed molded article having excellent flame retardancy can be obtained.
[0121] The amount of each component used in the resin composition is preferably in the same range as the amount of each component described in [1. Expanded polyolefin resin particles]. The amount of calcium compound (C2) used is preferably in the same range as the amount of calcium compound (C1).
[0122] Each aspect (for example, each step) of the present production method will be described below, but for matters other than those described in detail below, the description in the section [1. Expanded polyolefin resin particles] will be used as appropriate.
[0123] (granulation process) The present production method preferably includes a granulation step of preparing resin particles prior to the expansion step.
[0124] The granulation step in this manufacturing method is not particularly limited as long as resin particles can be obtained, and a known method can be adopted. An example of the granulation step is a method of performing the following (S1) to (S3) in order: (S1) melt-kneading a resin composition containing a predetermined amount of polyolefin resin (A), a calcium compound (C2), a phenol-based antioxidant (D), and a phosphorus-based processing stabilizer (E), and optionally a hindered amine (B) and other additives, using an extruder to prepare a melt-kneaded product; (S2) extruding the melt-kneaded product from a die equipped in the extruder; (S3) chopping the extruded melt-kneaded product into a desired shape (e.g., cylindrical, spherical, etc.) to obtain polyolefin resin particles.
[0125] In the above (S1), a resin composition containing predetermined amounts of the polyolefin resin (A), the calcium compound (C2), the phenolic antioxidant (D), and the phosphorus-based process stabilizer (E), and optionally the hindered amine (B) and other additives, may be prepared in advance, and then the resin composition may be fed to an extruder for melt-kneading to prepare a melt-kneaded product.
[0126] In the above (S3), before the molten kneaded material is chopped, the extruded molten kneaded material may be cooled and solidified using a cooling medium such as water.
[0127] (Dispersion process) Examples of the vessel include a pressure vessel and an autoclave type pressure vessel. The vessel may be equipped with a stirrer therein.
[0128] Examples of the aqueous dispersion medium include (a) a dispersion medium obtained by adding methanol, ethanol, ethylene glycol, glycerin, or the like to water, (b) water such as tap water and industrial water, and (c) a solution (aqueous solution) containing a salt such as sodium chloride or sodium sulfate, etc. In terms of enabling stable production of expanded particles, it is preferable to use pure water such as RO water (water purified by a reverse osmosis membrane method), distilled water, deionized water (water purified by an ion exchange resin), or ultrapure water as the aqueous dispersion medium.
[0129] Examples of the blowing agent include (a) (a-1) inorganic blowing agents such as nitrogen, carbon dioxide, air (a mixture of oxygen, nitrogen, and carbon dioxide), and (a-2) water; and (b) organic blowing agents such as (b-1) saturated hydrocarbons having 3 to 5 carbon atoms, such as propane, normal butane, isobutane, normal pentane, isopentane, and neopentane, (b-2) ethers, such as dimethyl ether, diethyl ether, and methyl ethyl ether, and (b-3) halogenated hydrocarbons, such as monochloromethane, chloroethane, and hydrofluoroolefins.
[0130] In the present method for producing expanded beads, it is preferable to use a dispersant (e.g., a poorly water-soluble inorganic compound such as kaolin or talc) and a dispersion aid (e.g., an anionic surfactant such as sodium dodecylbenzenesulfonate). This configuration can reduce adhesion between resin particles (sometimes called blocking) and can increase the stability of the dispersion in the container. As a result, it has the advantage of being able to stably produce expanded beads.
[0131] Regarding the above-mentioned aqueous dispersion medium and blowing agent, one type may be used alone, or two or more types may be used in combination.
[0132] The amounts of the aqueous dispersion medium, the foaming agent, the dispersant and the dispersion aid used are not particularly limited, and can be appropriately set taking into consideration (i) the stability of the dispersion (dispersibility of the resin particles), (ii) the density of the resulting expanded beads, (iii) the fusion properties of the expanded molded article obtained by molding the resulting expanded beads, (iv) productivity, and (v) economic efficiency.
[0133] The method for dispersing the polyolefin resin particles and the blowing agent in the aqueous dispersion medium in the container, i.e., the specific method for the dispersion step, is not particularly limited. For example, a method of supplying the aqueous dispersion medium, the polyolefin resin particles, and the blowing agent into the container, and stirring the mixture in the container with a stirrer provided in the container, etc., can be mentioned.
[0134] (Heating-pressure increase process and holding process) The present production method preferably further includes, in this order, after the dispersion step and before the release step, (1) a temperature-pressure increase step in which the temperature in the container is increased to a constant temperature and the pressure in the container is increased to a constant pressure, and (2) a holding step in which the temperature and pressure in the container are held at a constant temperature and constant pressure. In this specification, the (a) constant temperature in the temperature-pressure increase step and the holding step may be referred to as the foaming temperature, and the (b) constant pressure in the (a) constant pressure step may be referred to as the foaming pressure.
[0135] The expansion temperature is not particularly limited, but is preferably 130° C. to 165° C., more preferably 135° C. to 160° C., more preferably 140° C. to 158° C., and even more preferably 150° C. to 158° C. The DSC ratio of the expanded particles can be adjusted by the expansion temperature, and according to this configuration, the DSC ratio is 10% to 50%.
[0136] The expansion pressure is not particularly limited, but is preferably 0.5 MPa (gauge pressure) to 10.0 MPa (gauge pressure), more preferably 1.0 MPa (gauge pressure) to 5.0 MPa (gauge pressure), more preferably 2.0 MPa (gauge pressure) to 3.0 MPa (gauge pressure), and even more preferably 2.2 MPa (gauge pressure) to 2.5 MPa (gauge pressure). If the expansion pressure is 0.5 MPa (gauge pressure) or more, expanded particles with a suitable density can be obtained.
[0137] In the holding step, the time (holding time) for which the dispersion in the container is held at near the foaming temperature and foaming pressure is not particularly limited, but is preferably, for example, 10 minutes to 60 minutes, more preferably 12 minutes to 50 minutes, and even more preferably 15 minutes to 40 minutes.
[0138] (Release process) In the releasing step, the dispersion obtained after the heating step is released under low pressure. The releasing step allows the resin particles to expand, resulting in expanded particles. The releasing step can also be said to be a step of opening one end of the container and releasing the dispersion (dispersion) in the container into a region (space) with a pressure lower than the expansion pressure (i.e., the pressure inside the container).
[0139] In the releasing step, the "region under a pressure lower than the foaming pressure" means "a region under a pressure lower than the foaming pressure" or "a space under a pressure lower than the foaming pressure", and can also be called "an atmosphere under a pressure lower than the foaming pressure". The region under a pressure lower than the foaming pressure may be, for example, a region under atmospheric pressure.
[0140] In the releasing step, the temperature of the releasing region (atmosphere) is not particularly limited, but is preferably 20° C. to 110° C., more preferably 50° C. to 105° C., more preferably 80° C. to 100° C., and even more preferably 90° C. to 100° C. This configuration has the advantage that expanded beads having a relatively low bulk density can be obtained even at a low expansion pressure, and there is no risk of the expanded beads sticking to each other in the releasing region.
[0141] (Foaming process) The process from the dispersion step to the release step is sometimes called the expansion step. The process of producing expanded beads from resin beads in this way is called the "first-stage expansion step," and the obtained expanded beads are called "first-stage expanded beads."
[0142] (2nd stage foaming process) In order to obtain expanded beads with a high expansion ratio, the first-stage expanded beads obtained in the first-stage expansion step may be expanded again. The step of increasing the expansion ratio of the first-stage expanded beads is called the "second-stage expansion step", and the polyolefin resin expanded beads obtained in the second-stage expansion step are called "second-stage expanded beads". The specific method of the second-stage expansion step is not particularly limited, and a known method can be used.
[0143] [3. Polyolefin resin foam molding] The polyolefin resin foam molded article according to one embodiment of the present invention is a foam molded article obtained by foam molding the polyolefin foam beads described in the section [1. Polyolefin foam beads]. In this specification, the "polyolefin resin foam molded article according to one embodiment of the present invention" may be referred to as the "present foam molded article".
[0144] The foamed molded article of the present invention has the above-mentioned structure and thus has the advantages of being excellent in long-term thermal stability, surface beauty, and flame retardancy.
[0145] <Physical Properties> (Burning rate of polyolefin resin foam moldings) The maximum burning rate of the foamed molded article is preferably less than 100 mm / min, more preferably less than 95 mm / min, more preferably less than 90 mm / min, more preferably 89 mm / min or less, more preferably 87 mm / min or less, even more preferably 80 mm / min or less, and particularly preferably 75 mm / min or less.
[0146] In addition, the average burning rate of the foamed molded article is preferably less than 95 mm / min, more preferably less than 90 mm / min, more preferably 88 mm / min or less, more preferably 87 mm / min or less, more preferably 85 mm / min or less, more preferably 80 mm / min or less, even more preferably 75 mm / min or less, and particularly preferably 70 mm / min or less.
[0147] In this specification, the foam molded article is "excellent in flame retardancy" means that the foam molded article has either a maximum burning rate of less than 100 mm / min or an average burning rate of less than 95 mm / min. In this specification, the foam molded article is also included in the foam molded article having "excellent in flame retardancy" when it has non-flammability.
[0148] The method for measuring the maximum burning rate and the average burning rate of the foamed molded article will be described in detail in the Examples below.
[0149] (Density of polyolefin resin foam molding) The density of the foamed molded article is not particularly limited, but is preferably 20.0 g / L to 60.0 g / L, preferably 26.5 g / L to 50.0 g / L, preferably 25.0 g / L to 45.0 g / L, preferably 30.0 g / L to 45.0 g / L, and preferably 35.0 g / L to 40.0 g / L. If the density of the foamed molded article is 26.5 g / L or more, there is an advantage that the foamed molded article has no sink marks on the surface of the foamed molded article, is smooth, and has better surface beauty, and if it is 50.0 g / L or less, a sufficiently lightweight foamed molded article can be obtained. In addition, according to the above-mentioned configuration, there is an advantage that a foamed molded article having excellent moldability and flame retardancy can be obtained. The method for measuring the density of the foamed molded article will be described in detail in the examples described later.
[0150] <Method of manufacturing foamed molded product> The manufacturing method of the present foamed molded product is not particularly limited as long as the present foamed beads can be molded (preferably in-mold foam molding), and a known method can be applied. As the manufacturing method of the present foamed molded product, for example, the manufacturing method described in the section <Method of manufacturing foamed molded product> of International Publication WO2022 / 149538 can be suitably adopted. EXAMPLES
[0151] Hereinafter, one embodiment of the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0152] 〔material〕 Materials used in the Examples and Comparative Examples are described below. The materials used in the Examples and Comparative Examples were not particularly purified before use.
[0153] <Polyolefin resin (A)> Polypropylene resin 1: Ethylene / propylene random copolymer [recycled polyolefin resin, propylene unit content: 91 mol%, MFR = 7.1 g / 10 min, melting point 153°C] Polypropylene resin 2:1-butene / ethylene / propylene random copolymer [non-recycled polyolefin resin, propylene unit content: 96 mol%, MFR=10g / 10min, melting point 148℃] Polypropylene resin 3: Ethylene / propylene random copolymer [recycled polyolefin resin, propylene unit content: 91 mol%, MFR = 12 g / 10 min, melting point 152°C].
[0154] <Additives> (Hindered amine (B)) Hindered amine [BASF, FLAMESTAB (registered trademark) NOR116 (compound with CAS number 191680-81-6)] (Calcium compounds (C2)) Calcium oxide [manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.] Calcium stearate [manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.] (Phenol-based antioxidant (D)) Phenolic antioxidant [BASF, IRGANOX® 1010 (tetrakis[3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionic acid]pentaerythritol)] (Phosphorus-based processing stabilizer (E)) Phosphorus-based processing stabilizer [BASF, Irgafos 168 (tris(2,4-di-t-butylphenyl)phosphite)] (Calcium oxide mixture) Calcium oxide mixture (BASF, PS032G (a mixture containing at least calcium oxide, calcium stearate, a phenolic antioxidant, and a phosphorus-based processing stabilizer. In the mixture, the only compounds containing calcium are calcium oxide and calcium stearate, and the total content of calcium oxide and calcium stearate is 45% by weight in the product (100% by weight)) (Other flame retardants) Phosphate ester flame retardant [PX-200 (tetrakis(2,6-dimethylphenyl)-m-phenylene bisphosphate), manufactured by Daihachi Chemical Industry Co., Ltd.] (Other additives) Talc [Talc Powder PK-S, manufactured by Hayashi Kasei Co., Ltd.] Glycerin [Refined glycerin D, manufactured by Lion Corporation] Carbon black (average primary particle size 30 nm) Calcium sulfate dihydrate [Wako Pure Chemical Industries, Ltd.] Metal deactivator [BASF, IRGANOX(R) MD1024].
[0155] [Measurement method] The measurement and evaluation methods for various items carried out in the examples and comparative examples will be described below.
[0156] (MFR of polyolefin resin (A) and polyolefin resin particles) The MFR of the polyolefin resin (A) and the polyolefin resin particles was measured using an MFR measuring device described in JIS K7210-1: 2014. The measurement conditions were an orifice diameter of 2.0959±0.005 mmφ, an orifice length of 8.000±0.025 mm, a load of 2160 g, and a temperature of 230±0.2°C.
[0157] <Melting point of polyolefin resin (A)> The melting point of the polyolefin resin (A) was measured using a differential scanning calorimeter [DSC7020, manufactured by Hitachi High-Tech Science Corporation]. The specific operation procedures were as follows (1) to (4): (1) the temperature of 5 mg to 6 mg of polyolefin resin (A) was raised from 40.0°C to 220.0°C at a heating rate of 10.0°C / min to melt the polyolefin resin (A); (2) the temperature of the molten polyolefin resin (A) was then lowered from 220.0°C to 40.0°C at a heating rate of 10.0°C / min to crystallize the polyolefin resin (A); (3) the temperature of the crystallized polyolefin resin (A) was then further raised from 40.0°C to 220.0°C at a heating rate of 10.0°C / min; (4) the temperature of the peak (melting peak) of the DSC curve of the polyolefin resin (A) obtained during the second heating (i.e., during (3)) was taken as the melting point of the polyolefin resin (A). In addition, when there are multiple peaks (melting peaks) in the DSC curve of the polyolefin resin (A) obtained during the second heating by the above-mentioned method, the temperature of the peak (melting peak) with the maximum heat of fusion was determined as the melting point of the polyolefin resin (A).
[0158] (Average particle size of primary particles of carbon black) A cross-section of the membrane constituting the bubbles of the obtained polyolefin resin foamed beads was photographed at 40,000 times magnification using a transmission electron microscope. In the obtained transmission electron microscope photograph, the particle diameters (Ferret diameters) of 50 randomly selected carbon black primary particles were measured in the X and Y directions, respectively, and the average value was calculated to be the average particle diameter of the carbon black primary particles.
[0159] (Oxygen index of polyolefin resin particles) The oxygen index of the polyolefin resin particles was measured by the following methods (1) to (3): (1) the polyolefin resin particles were heat-pressed at 200°C for 1 minute using a spacer of 150 mm length x 150 mm width x 1 mm thickness to obtain a resin plate made of polyolefin resin particles; (2) a sample of 100 mm length x 6.5 mm width was cut out from the resin plate made of polyolefin resin particles; (3) the oxygen index of the cut out sample was measured in accordance with JIS K7201 (test method for flammability based on oxygen index).
[0160] (Measurement of DSC ratio of polyolefin resin foam particles) The DSC ratio of the polyolefin resin foamed particles was measured using a differential scanning calorimeter [DSC7020, Hitachi High-Tech Science Corporation]. Specifically, the DSC ratio was calculated by [Qh / (Ql+Qh)×100], where the melting peak area on the low-temperature side of the DSC curve during the first heating step obtained when heating 5 mg to 6 mg of polyolefin resin foamed particles from 40°C to 220°C at a heating rate of 10°C / min was Ql, and the melting peak area on the high-temperature side was Qh. Strictly speaking, the area surrounded by the melting peak on the low-temperature side and the tangent line to the melting start baseline from the maximum point between the melting peak on the low-temperature side and the melting peak on the high-temperature side was Ql. In addition, the melting peak heat quantity on the high-temperature side, which is the heat quantity surrounded by the melting peak on the high-temperature side and the tangent line to the melting end baseline from the maximum point between the melting peak on the low-temperature side and the melting peak on the high-temperature side, was Qh.
[0161] (Bulk density of polyolefin resin foam particles) The weight w (g) of the polyolefin resin foam particles was weighed, and the volume v (L) was measured using a measuring cylinder at 23°C under atmospheric pressure (standard atmospheric pressure 0.1 MPa), to calculate the bulk density in w / v (g / L).
[0162] (Density of foamed molded body) The density of the foamed molded product was measured by the following methods (1) to (3); (1) the length (mm), width (mm), and thickness (mm) of the foamed molded product were measured, and the volume V (L) of the foamed molded product was calculated; (2) the weight W (g) of the foamed molded product was measured; (3) the density of the foamed molded product was calculated based on the following formula: Density of foamed molding (g / L) = W / V.
[0163] (Evaluation of surface aesthetics of polyolefin resin foam molded products) The side surface of the obtained foamed molded article was visually observed, and the surface aesthetics was judged according to the following criteria, where a larger number means a more excellent surface aesthetics. 2 (Good): There are almost no gaps between the particles (between the polyolefin resin foam particles), the surface irregularities are not noticeable, and it is beautiful with no wrinkles, shrinkage, or color unevenness. 1 (Fair): Some intergranular or surface irregularities, shrinkage, wrinkles or color unevenness are observed. 0 (Unacceptable): Clearly noticeable gaps, surface irregularities, shrinkage, wrinkles or color unevenness across the entire observation surface.
[0164] (Burning rate of polyolefin resin foam moldings) From the obtained polyolefin resin foam molded body, a flame retardant test sample of 350 mm in length × 100 mm in width × 12 mm in thickness was cut out, and an A mark was made at a position 38 mm from one end of the sample in the longitudinal direction, and a B mark was made at a position 292 mm from the other end. Ten test samples were prepared, and tests were carried out on all of them. Using an FMVSS flammability tester [manufactured by Suga Test Instruments Co., Ltd.], a flame from a burner adjusted to a height of 38 mm was applied to the one end of the sample in the longitudinal direction for 15 seconds so that the end of the sample was the center of the flame, and the burning rate of the test pieces that did not have "non-flammability" was calculated based on the criteria shown in (i) to (iii) below, and the maximum burning rate and the average burning rate were calculated from the results.
[0165] (i) The flame was extinguished before it reached the A mark: It was deemed to have "non-combustible properties." (ii) The flame burned beyond the A-marked line and was extinguished before reaching the B-marked line: The burning speed {(L1) / T1} (mm / min) was calculated from the time T1 (min) from when the flame passed the A-marked line until it was extinguished and the burning distance L1 (mm) from the A-marked line. (iii) The flame burned beyond the A-marked line and continued to burn until it reached the B-marked line: The burning speed 254 / T2 (mm / min) was calculated from the time T2 (min) from when the flame passed the A-marked line until it reached the B-marked line and the distance from the A-marked line to the B-marked line, 254 mm. Based on these results, the highest burning speed among the 10 sample samples was determined as the "maximum burning speed." The average burning speed of the 10 sample samples was determined as the "average burning speed."
[0166] The methods for producing polyolefin resin particles, expanded polyolefin resin particles, and in-mold polyolefin resin foamed articles in the examples and comparative examples will be described below.
[0167] (Examples 1 to 8 and Comparative Examples 1 to 6) [Preparation of polyolefin resin particles] The polyolefin resin and the materials shown in Table 1 or Table 2 were hand-blended to obtain the weight ratios shown in Table 1 or Table 2, and melt-kneaded using a twin-screw extruder at a resin temperature of 220° C. The resulting melt-kneaded product was then extruded from the extruder in the form of strands, and the resulting strands were cooled with water and cut to obtain polyolefin resin particles with an average weight of 1.2 mg.
[0168] [Preparation of polyolefin resin foam particles] In a 10L pressure-resistant autoclave, 100 parts by weight (2.4 kg) of the polyolefin resin particles obtained by the above method, 200 parts by weight of water, 0.3 parts by weight of kaolin [BASF, ASP170] as a poorly water-soluble inorganic compound, and 0.38 parts by weight of sodium dodecylbenzenesulfonate aqueous solution [Kao Corporation, Neopelex G-15] as a surfactant were charged. Then, while stirring the charged raw materials, 4 parts by weight of carbon dioxide was added to the autoclave as a foaming agent to prepare a dispersion (dispersion process). Next, the contents of the autoclave were heated to the foaming temperature shown in Table 1 or Table 2, and held for 10 minutes, and then carbon dioxide was additionally injected to increase the pressure inside the autoclave to the foaming pressure shown in Table 1 or Table 2 (heating-pressure increase process). After maintaining the foaming temperature and foaming pressure for 20 minutes (maintenance step), the valve at the bottom of the autoclave was opened, and the foam was released through an orifice with a diameter of 3.6 mm into an atmosphere at 97°C under atmospheric pressure to obtain polyolefin resin foamed particles (release step). During the release, carbon dioxide was injected to maintain the pressure in the container so that the pressure would not decrease.
[0169] [Preparation of second-stage expanded particles] In all cases except for Example 2, the polyolefin resin expanded particles obtained were dried at 80°C, impregnated with pressurized air in a pressure vessel to adjust the internal pressure to 0.3 MPa (absolute pressure), and then contacted with water vapor at 0.07 MPa (gauge pressure) to perform second-stage expansion. The bulk density of the obtained second-stage expanded particles was approximately 21 g / L.
[0170] [Preparation of polyolefin resin in-mold foamed bodies] The obtained two-stage foamed particles were placed in a pressure-resistant container, impregnated with pressurized air, and the polyolefin resin foamed particles, which had been adjusted in advance to have an internal pressure of 0.20 MPa (absolute pressure), were filled into a mold measuring 370 mm in length, 320 mm in width, and 50 mm in thickness. The inside of the mold chamber was then heated with steam at 0.32 MPa (gauge pressure) to fuse the foamed particles together. After the inside of the mold and the surface of the molded body were cooled with water, the molded body was removed to obtain a polyolefin resin in-mold foamed molded body. The obtained in-mold foamed molded body was left to stand at 23°C for 2 hours, and then cured at 75°C for 16 hours.
[0171] (Example 9 and Comparative Example 8) The polyolefin resin and the materials shown in Table 1 or Table 2 were hand-blended to the weight ratios shown in Table 1 or Table 2, and melt-kneaded using a twin-screw extruder at a resin temperature of 220°C. The resulting melt-kneaded product was then extruded from the extruder in the form of strands, and the resulting strands were cooled with water and cut to obtain polyolefin resin particles with an average weight of 1.2 mg. The resulting polyolefin resin particles were fed into a twin-screw extruder, and polyolefin resin particles with an average weight of 1.2 mg were obtained by the same procedure. This process was repeated four times to obtain polyolefin resin particles that had been melt-kneaded four times.
[0172] The evaluation results of the obtained polyolefin resin particles, expanded polyolefin resin particles, and in-mold polyolefin resin foamed articles are shown in Tables 1 and 2.
[0173] [Table 1]
[0174] [Table 2]
[0175] In Examples 1 to 4 and 6, calcium oxide was used as the calcium compound (C2). The amount of calcium oxide used was 0.15% by weight based on 100% by weight of the expanded beads. Therefore, the expanded beads obtained in Examples 1 to 4 and 6 contain at least one calcium compound (C1) selected from the group consisting of calcium oxide, calcium oxide hydrate and calcium carbonate, and the total content of calcium oxide, calcium oxide hydrate and calcium carbonate in the expanded beads is at least in the range of 0.10% by weight to 3.00% by weight based on 100% by weight of the expanded beads, and can be said to be approximately 0.15% by weight to 0.27% by weight.
[0176] In Examples 1 to 3, calcium stearate was used as the calcium compound (C2). The amount of calcium stearate used was 0.04% by weight based on 100% by weight of the expanded beads. Therefore, the expanded beads obtained in Examples 1 to 3 contained 0.04% by weight of calcium stearate as the calcium compound (C1) based on 100% by weight of the expanded beads.
[0177] In Example 5, a calcium oxide mixture was used as the calcium compound (C2). As described above, the calcium oxide mixture is a mixture containing at least calcium oxide, calcium stearate, a phenol-based antioxidant, and a phosphorus-based processing stabilizer. In addition, in the mixture, the only compounds containing calcium are calcium oxide and calcium stearate, and the total content of calcium oxide and calcium stearate is 45% by weight in 100% by weight of the product. Therefore, the expanded beads obtained in Example 5 contain, as the calcium compound (C1), at least one selected from the group consisting of calcium oxide, calcium oxide hydrate, and calcium carbonate, and calcium stearate. The total content of calcium oxide, calcium oxide hydrate, calcium carbonate, and calcium stearate in the expanded beads is at least in the range of 0.10% by weight to 3.00% by weight in 100% by weight of the expanded beads, and can be said to be approximately 0.225% by weight to 0.400% by weight.
[0178] Examples 1 to 6 show the evaluation results of polyolefin resin particles, expanded polyolefin resin particles, and polyolefin resin in-mold foamed molded articles according to one embodiment of the present invention. In Examples 1 to 5, the in-mold foamed molded articles obtained were excellent in flame retardancy, even though the expanded particles contained carbon black. In Example 6, in which the expanded particles did not contain carbon black, the in-mold foamed molded article obtained had "non-flammability". Thus, the in-mold foamed molded articles made of expanded polyolefin resin particles obtained by the manufacturing method of the present invention were excellent in flame retardancy. As shown in Comparative Examples 1 to 4, when the expanded particles did not contain a calcium compound (C2), the resulting foamed molded articles did not have excellent flame retardancy, and even when the amount of hindered amine (B) was increased as in Comparative Example 2, there was still room for improvement in flame retardancy.
[0179] Moreover, the polyolefin resin particles of Examples 3 to 6, which contain the calcium compound (C2), had a lower MFR than the polyolefin resin particles of Comparative Examples 1 to 3, which do not contain the calcium compound (C2). That is, the polyolefin resin particles contained the calcium compound (C2), so that the increase in MFR was suppressed. The polyolefin resin particles obtained in Comparative Example 4 contained the phenol-based antioxidant (D) and the phosphorus-based processing stabilizer (E), so that the MFR value was lower than that of Comparative Examples 1 to 3, but the MFR was not equivalent to that of Examples 3 to 6. Moreover, Comparative Examples 5 to 6 show the results when the calcium compound (C2) was contained, but the content of the calcium compound (C2) was low, or the content of the calcium compound (C2) was high. In the cases of Comparative Examples 5 to 6, the MFR value of the polyolefin resin particles was also lower than that of Comparative Examples 1 to 3, but the MFR of the polyolefin resin particles was not equivalent to that of Examples 3 to 6. Furthermore, in Reference Example 2, in which a calcium oxide mixture containing calcium oxide, calcium stearate, a phenol-based antioxidant, and a phosphorus-based process stabilizer was added, the increase in MFR was suppressed compared to Reference Example 1. Therefore, it was shown that in order to suppress the increase in MFR, the calcium compound (C2), the phenol-based antioxidant (D), and the phosphorus-based process stabilizer (E) in contents of 0.10 wt % to 3.00 wt % relative to 100 wt % of the polyolefin resin particles are necessary. [Industrial Applicability]
[0180] In one embodiment of the present invention, the thermal decomposition of the polyolefin resin in the granulation step is not easily accelerated, thereby suppressing the increase in MFR of the resin particles, and the polyolefin expanded particles obtained from the resin particles are foamed to provide a polyolefin resin foam molded product having excellent moldability and flame retardancy. In one embodiment of the present invention, even when the polyolefin resin contains recycled polyolefin resin and / or carbon black, a polyolefin resin foam molded product having excellent moldability and flame retardancy can be provided. The polyolefin resin foam molded product having excellent flame retardancy can be used for various applications such as cushioning packaging materials, logistics materials, heat insulation materials, civil engineering and construction materials, and automobile parts, and can be particularly used suitably in various fields that require the fulfillment of strict flame retardancy standards, such as transportation, buildings, structures, furniture, electrical equipment, and electronic equipment.
Claims
1. The present invention comprises a polyolefin resin (A), a calcium compound (C1), a phenolic antioxidant (D) and a phosphorus-based processing stabilizer (E), The calcium compound (C1) is a compound that does not contain a sulfur element or a halogen element, The content of the calcium compound (C1) is 0.10% by weight to 3.00% by weight based on 100% by weight of the expanded polyolefin resin beads, The calcium compound (C1) is a polyolefin resin foam particle dispersed inside the membrane constituting the air bubbles.
2. The calcium compound (C1) is 2. The expanded polyolefin resin particles according to claim 1, comprising at least one selected from the group consisting of calcium oxide, calcium hydroxide, calcium carbonate and calcium fatty acid.
3. The expanded polyolefin resin particles according to claim 1 , wherein the polyolefin resin (A) comprises a recycled polyolefin resin.
4. The expanded polyolefin resin particles according to claim 1 , further comprising a hindered amine (B).
5. The expanded polyolefin resin particles according to claim 4, further comprising carbon black and / or graphite.
6. The expanded polyolefin resin particles according to claim 1 , further comprising a metal deactivator.
7. A polyolefin resin foamed molded article obtained by molding the expanded polyolefin resin beads according to any one of claims 1 to 6.
8. In the container, a dispersing step of dispersing polyolefin-based resin particles made of a polyolefin-based resin composition containing a polyolefin-based resin (A), a calcium compound (C2), a phenol-based antioxidant (D), and a phosphorus-based process stabilizer (E) in an aqueous dispersion medium, and a foaming agent; A discharging step of discharging the dispersion obtained in the dispersing step into a region with a lower pressure than the pressure inside the container, The calcium compound (C2) is a compound that does not contain a sulfur element or a halogen element, The content of the calcium compound (C2) is 0.10% by weight to 3.00% by weight based on 100% by weight of the expanded polyolefin resin beads.
9. The calcium compound (C2) is The method for producing expanded polyolefin resin beads according to claim 8, which contains at least one selected from the group consisting of calcium oxide, calcium hydroxide, calcium carbonate and calcium fatty acid.
10. The calcium compound (C2) is The method for producing expanded polyolefin resin beads according to claim 8, which contains at least one selected from the group consisting of calcium oxide and fatty acid calcium salts.
11. The method for producing expanded polyolefin resin beads according to any one of claims 8 to 10, wherein the polyolefin resin (A) contains a recycled polyolefin resin.
12. A method for producing expanded polyolefin resin beads, comprising: a polyolefin resin (A), a calcium compound (C1), a phenol-based antioxidant (D), and a phosphorus-based process stabilizer (E), the method comprising the steps of: In the container, A dispersing step of dispersing polyolefin-based resin particles made of a polyolefin-based resin composition containing (i) a polyolefin-based resin (A), (ii) a calcium compound (C1) and / or a precursor of the calcium compound (C1), (iii) a phenol-based antioxidant (D), and (iv) a phosphorus-based process stabilizer (E) in an aqueous dispersion medium, and a blowing agent; A discharging step of discharging the dispersion obtained in the dispersing step into a region with a lower pressure than the pressure inside the container, The calcium compound (C1) is a compound that does not contain a sulfur element or a halogen element, The precursor of the calcium compound (C1) is a compound that does not contain a sulfur element and a halogen element, In the expanded polyolefin resin beads, the content of the calcium compound (C1) is 0.10% by weight to 3.00% by weight based on 100% by weight of the expanded polyolefin resin beads.
13. The precursor of the calcium compound (C1) is The method for producing expanded polyolefin resin beads according to claim 12, comprising at least one selected from the group consisting of calcium oxide, calcium hydroxide, calcium carbonate and fatty acid calcium.
14. The precursor of the calcium compound (C1) is The method for producing expanded polyolefin resin beads according to claim 12, which contains at least one selected from the group consisting of calcium oxide and fatty acid calcium salts.
15. The method for producing expanded polyolefin resin beads according to any one of claims 12 to 14, wherein the polyolefin resin (A) contains a recycled polyolefin resin.
Citation Information
Patent Citations
Polyolefin resin foamed particle and in-mold foam molding thereof
JP2013035949A
Cited By
Polyolefin-based resin foam particles, method for producing same, and polyolefin-based resin foam molded body
WO2026182162A1