Adhesive tape for semiconductor manufacturing process
The adhesive tape with a UV-absorbing first adhesive layer addresses poor peeling performance of thin chip components, ensuring high yield and accuracy in semiconductor manufacturing by maintaining adhesive strength post-irradiation.
Patent Information
- Application Number
- JP2024049426
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional adhesive tapes struggle with poor peeling performance when transferring thin chip components, leading to low yield and accuracy issues in semiconductor manufacturing processes.
The adhesive tape incorporates a base material layer with a first adhesive layer containing an ultraviolet absorber (UVA-1) and specific properties such as a maximum loss tangent (tanδ) of 0.1 or less in the 20°C to 40°C temperature range, wavelength of 365 nm, and irradiation intensity of 7.8 mW/cm², resulting in a 60% or less adhesive strength reduction after UV irradiation, enhancing peeling performance.
The tape achieves high accuracy and efficient transfer of thin chip components with reduced adhesive residue, improving manufacturing efficiency and quality by ensuring minimal adhesive strength loss post-irradiation.
Smart Images

Figure 2024144310000001 
Figure 2024144310000002 
Figure 2024144310000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive tape for use in semiconductor manufacturing processes. [Background technology]
[0002] In the manufacturing process of semiconductor devices, a large number of chip components arranged on an adhesive layer are often transferred onto a drive circuit board. For example, a micro LED display is a display device in which each chip that makes up a pixel is a tiny light emitting diode (LED, Light Emitting Diode) chip, and these micro LED chips emit light to display images. Micro LED displays have high contrast, a fast response speed, and can be made thin because they do not require the color filters used in liquid crystal displays, organic electroluminescence displays, etc., and are therefore attracting attention as next-generation display devices. In a micro LED display, many micro LED chips are densely packed in a flat surface.
[0003] In the manufacturing process of semiconductor devices such as micro LED displays, for example, a large number of chip components are attached onto an adhesive layer, the resulting transfer laminate is placed opposite a drive circuit board, and the chip components are peeled off from the transfer laminate to make electrical connection with the drive circuit board (transfer process).
[0004] As a method for peeling off chip components from a transfer laminate, for example, a method is known in which laser light is irradiated from the back surface of the support of the transfer laminate, focusing on the adhesive layer (for example, Patent Document 1). Such a method is also called laser ablation. Another method is known in which heat-expandable particles, heat-expandable microcapsules, etc. are blended into the adhesive layer, and the heat-expandable particles, heat-expandable microcapsules, etc. are thermally expanded by thermocompression bonding between the transfer laminate and the drive circuit board, thereby deforming the adhesive layer and reducing the adhesion area, thereby peeling off the chip components (for example, Patent Documents 2 and 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-138949 A [Patent Document 2] JP 2019-15899 A [Patent Document 3] JP 2003-7986 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, when the chip components are thin, there is a problem that it is difficult to transfer the chip components with a good yield using conventional tapes, due to poor peeling of the chip components attached to the adhesive layer.
[0007] An object of the present invention is to provide an adhesive tape for use in the semiconductor manufacturing process, which has excellent peeling performance for chip components and is capable of transferring chip components with high accuracy, even if the chip components are thin. [Means for solving the problem]
[0008] Disclosure 1 comprises a base layer and a first pressure-sensitive adhesive layer, the first pressure-sensitive adhesive layer contains an ultraviolet absorbing agent (UVA-1), the first pressure-sensitive adhesive layer has a maximum loss tangent (tan δ) of 0.1 or less in a temperature range of 20°C to 40°C, and is irradiated at a wavelength of 365 nm and an irradiation intensity of 7.8 mW / cm. 2 The cumulative amount of ultraviolet light is 190 mJ / cm 2 This adhesive tape is for use in the semiconductor manufacturing process, and has an adhesive strength reduction rate of 60% or less after irradiation so as to satisfy the above requirements. Disclosure 2 is a sheet-like adhesive having a base layer, an intermediate adhesive layer, and a first adhesive layer in this order, the first adhesive layer containing an ultraviolet absorbing agent (UVA-1), the first adhesive layer having a maximum loss tangent (tan δ) of 0.1 or less in a temperature range of 20°C to 40°C, and a wavelength of 365 nm and an irradiation intensity of 7.8 mW / cm 2The cumulative amount of ultraviolet light is 190 mJ / cm 2 This adhesive tape is for use in the semiconductor manufacturing process, and has an adhesive strength reduction rate of 60% or less after irradiation so as to satisfy the above requirements. The present disclosure 3 is the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process according to the present disclosure 1 or 2, wherein the base layer comprises a polyester film. Present Disclosure 4 is the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process according to Present Disclosure 1, 2 or 3, wherein the first pressure-sensitive adhesive layer contains a base polymer, and the base polymer contains a (meth)acrylic copolymer. Disclosure 5 is the pressure-sensitive adhesive tape for semiconductor manufacturing process according to Disclosure 4, wherein the (meth)acrylic copolymer has a structure derived from a hydroxyl group-containing monomer, and the content of the structure derived from the hydroxyl group-containing monomer in the (meth)acrylic copolymer is 2 mass% or more. The present disclosure 6 is the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process according to the present disclosure 1, 2, 3, 4, or 5, wherein the ultraviolet absorber (UVA-1) is liquid at room temperature. The present disclosure 7 is the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process according to the present disclosure 6, wherein the content of the ultraviolet absorbing agent (UVA-1) is 15 parts by mass or less per 100 parts by mass of the base polymer. The present disclosure 8 is the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process according to the present disclosure 1, 2, 3, 4, 5, 6, or 7, wherein the first pressure-sensitive adhesive layer has an ultraviolet ray absorptance of 80% or more at a wavelength of 355 nm. A ninth aspect of the present disclosure is the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process according to the first, second, third, fourth, fifth, sixth, seventh or eighth aspect of the present disclosure, wherein the first pressure-sensitive adhesive layer has a gel fraction of 60 mass % or more. Present Disclosure 10 is the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process of Present Disclosure 1, 2, 3, 4, 5, 6, 7, 8, or 9, wherein the first pressure-sensitive adhesive layer has a thickness of 40 μm or less. The present disclosure 11 is the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process according to the present disclosure 2, wherein the intermediate adhesive layer further contains an ultraviolet absorbing agent (UVA-2). The present disclosure 12 is the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process according to the present disclosure 11, wherein the ultraviolet absorber (UVA-2) is liquid at room temperature. Disclosure 13 is an adhesive tape for semiconductor manufacturing processes according to Disclosure 11 or 12, wherein the intermediate adhesive layer contains a base polymer, and the content of the ultraviolet absorber (UVA-2) is 15 parts by mass or less per 100 parts by mass of the base polymer. Disclosure 14 is the pressure-sensitive adhesive tape for use in semiconductor manufacturing processes according to Disclosure 2, 11, 12, or 13, wherein the intermediate adhesive layer has an ultraviolet ray absorptance of 80% or more at a wavelength of 355 nm. Disclosure 15 is the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process according to Disclosure 2, 11, 12, 13, or 14, further comprising a barrier layer between the intermediate adhesive layer and the first adhesive layer. Disclosure 16 is the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process of Disclosure 15, wherein the barrier layer comprises a polyester film. Present Disclosure 17 is the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process according to Present Disclosure 15 or 16, wherein the thickness of the barrier layer is 6 μm or less. The present disclosure 18 is an adhesive tape for use in the semiconductor manufacturing process according to the present disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, or 17, further having a second adhesive layer on the side of the base layer opposite to the side having the first adhesive layer. The present invention will be described in detail below.
[0009] The present inventors have investigated using an adhesive tape having an adhesive layer containing an ultraviolet absorber to set the maximum loss tangent (tan δ) of the adhesive layer in a specific temperature range to a specific value or less, and to adjust the adhesive strength reduction rate of the adhesive tape after irradiation with a specific ultraviolet ray to a specific range. As a result, they have found that an adhesive tape having excellent peeling performance for chip components by laser ablation can be obtained even when the chip components are thin, and have completed the present invention.
[0010] The adhesive tape for use in the semiconductor manufacturing process of the present invention has an irradiation intensity of 7.8 mW / cm and a wavelength of 365 nm. 2 The cumulative amount of ultraviolet light is 190 mJ / cm 2The upper limit of the adhesive strength loss rate after irradiation so as to become 60% (hereinafter, sometimes simply referred to as "adhesive strength loss rate after ultraviolet irradiation"). Since the adhesive strength loss rate after ultraviolet irradiation is 60% or less, the adhesive tape for use in the semiconductor manufacturing process of the present invention makes it possible to peel off chip components without the need for separate irradiation with ultraviolet rays before performing laser ablation, thereby improving the work efficiency of chip component manufacturing. The preferred upper limit of the adhesive strength loss rate after ultraviolet irradiation of the adhesive tape for use in the semiconductor manufacturing process of the present invention is 10%, and 0% is most preferred. The adhesive strength loss rate of the adhesive tape for use in the semiconductor manufacturing process of the present invention after irradiation with ultraviolet light is measured by the following method. That is, the adhesive tape is cut into a flat rectangular shape of 25 mm wide x 75 mm long, and the cut adhesive tape is attached to a glass plate using a 2 kg rubber roller, and left to stand for 20 minutes under conditions of 23 ° C. and 50% RH to prepare a test piece. The obtained test piece is subjected to a 180 ° peel test at 23 ° C., 50% RH, and a peel speed of 300 mm / min using a tensile tester (Shimadzu Corporation, "AGS-X" etc.) in accordance with JIS Z0237 to obtain the 180 ° peel force (mN / 25 mm) before ultraviolet irradiation. In addition, the adhesive tape cut in the same manner as above is irradiated with a UV irradiator using a black light (NEC Corporation, "FL20SBL") at a wavelength of 365 nm and an irradiation intensity of 7.8 mW / cm. 2 The cumulative amount of ultraviolet light is 190 mJ / cm 2 After irradiating the sample so that the 180° peel strength is measured in the same manner as above to obtain the 180° peel strength (mN / 25 mm) after UV irradiation. The adhesive strength loss rate after UV irradiation is then calculated using the following formula: Decrease in adhesive strength after UV irradiation (%) = 100 × {(180° peel strength before UV irradiation) - (180° peel strength after UV irradiation)} / (180° peel strength before UV irradiation)
[0011] The pressure-sensitive adhesive tape for use in the semiconductor manufacturing process of the present invention has a substrate layer. Since the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process of the present invention has a substrate layer, the pressure-sensitive adhesive tape has appropriate stiffness and is easy to handle.
[0012] From the viewpoint of peeling off the chip components by laser ablation, the preferable lower limit of the ultraviolet ray transmittance of the base layer at a wavelength of 355 nm is 1%, more preferably 50%, and still more preferably 80%. There is no particular preferable upper limit of the ultraviolet ray transmittance of the base layer at a wavelength of 355 nm, but the upper limit is substantially about 95%. The ultraviolet transmittance of the substrate layer at a wavelength of 355 nm can be measured, for example, using a spectrophotometer (Shimadzu Corporation, "UV-2600i" or the like) in accordance with JIS L1925.
[0013] From the viewpoint of adjusting the ultraviolet ray transmittance at a wavelength of 355 nm within the above range, the base layer preferably includes a resin film. The resin film is not particularly limited, but from the viewpoint of excellent heat resistance, it is preferable to include a polyester film. Examples of the polyester film include a polyethylene terephthalate (PET) film, a polyethylene naphthalate (PEN) film, and a polybutylene terephthalate (PBT) film. Among them, a polyethylene terephthalate (PET) film is preferable from the viewpoint of a balance between price and excellent transparency. From the viewpoint of excellent ultraviolet transmittance, the resin film preferably includes a (meth)acrylic resin film. Examples of the (meth)acrylic resin film include a polymethyl methacrylate film. Further, examples of the resin film include polyacetal films, polyamide films, polycarbonate films, polyphenylene ether films, ultra-high molecular weight polyethylene films, syndiotactic polystyrene films, polyarylate films, polysulfone films, polyethersulfone films, polyphenylene sulfide films, polyetheretherketone films, polyimide films, polyetherimide films, fluororesin films, and liquid crystal polymer films. In this specification, "(meth)acrylic" means acrylic or methacrylic.
[0014] The thickness of the base layer is not particularly limited, but the preferred lower limit is 3 μm, and the preferred upper limit is 100 μm. By having the thickness of the base layer within the above range, the adhesive tape can have a suitable stiffness and be more easily handled. The more preferred lower limit of the thickness of the base layer is 12 μm, and the more preferred upper limit is 75 μm.
[0015] The preferred upper limit of the haze of the substrate layer is 10%. By setting the haze of the substrate layer to 10% or less, the substrate layer transmits laser light efficiently, and the peeling performance of the pressure-sensitive adhesive tape for semiconductor manufacturing process of the present invention for chip components is further improved. The more preferred upper limit of the haze of the substrate layer is 5%, and the even more preferred upper limit is 1%. Further, the lower limit of the haze of the substrate layer is preferably as small as possible, but the substantial lower limit is about 0.1%. The haze of the substrate layer can be measured, for example, by using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., "NDH4000" or the like).
[0016] The first adhesive layer is not particularly limited, but is preferably a pressure-sensitive adhesive layer. From the viewpoint of further improving the peeling performance for chip components, the first adhesive layer may be a curing adhesive layer such as a thermosetting or photocuring type.
[0017] The first pressure-sensitive adhesive layer preferably contains a base polymer. Examples of the base polymer contained in the first pressure-sensitive adhesive layer include an ABA block copolymer, a (meth)acrylic copolymer, a urethane copolymer, a silicone pressure-sensitive adhesive, etc. Among them, a (meth)acrylic copolymer is preferred because it can further improve the peeling performance of the pressure-sensitive adhesive tape for semiconductor manufacturing process of the present invention for chip components and can further suppress adhesive residue on the chip components.
[0018] The (meth)acrylic copolymer is a copolymer having a structure derived from a (meth)acrylic monomer. Examples of the (meth)acrylic monomer include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, isobornyl (meth)acrylate, etc. These (meth)acrylic monomers may be used alone or in combination of two or more. Among them, from the viewpoint of balancing the peeling performance for chip components and the effect of suppressing adhesive residue on the chip components, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and methyl (meth)acrylate are preferred. From the viewpoint of further suppressing adhesive residue on the chip components, butyl (meth)acrylate and methyl (meth)acrylate are more preferred. Furthermore, these acrylates are even more preferred. The above (meth)acrylic monomer may be a single monomer, or multiple monomers may be used. In this specification, the term "(meth)acrylate" means acrylate or methacrylate.
[0019] The (meth)acrylic copolymer preferably further contains a structure derived from a crosslinkable functional group-containing monomer. The (meth)acrylic copolymer contains a structure derived from the crosslinkable functional group-containing monomer, which increases the cohesive strength of the first pressure-sensitive adhesive layer, thereby improving the peeling performance of the pressure-sensitive adhesive tape for semiconductor manufacturing process of the present invention against chip components and further suppressing adhesive residue on the chip components. In addition, when the first pressure-sensitive adhesive layer contains a crosslinking agent described below, the crosslinkable functional group derived from the crosslinkable functional group-containing monomer reacts with the crosslinking agent to form a crosslinked structure in the (meth)acrylic copolymer, thereby improving the peeling performance of the pressure-sensitive adhesive tape for semiconductor manufacturing process of the present invention against chip components and further suppressing adhesive residue on the chip components.
[0020] The crosslinkable functional group-containing monomer is not particularly limited, and examples thereof include carboxyl group-containing monomers, hydroxyl group-containing monomers, epoxy group-containing monomers, double bond-containing monomers, triple bond-containing monomers, amino group-containing monomers, amide group-containing monomers, and nitrile group-containing monomers. These crosslinkable functional group-containing monomers may be used alone, or two or more may be used in combination. Among them, it is preferable to contain at least one selected from the group consisting of carboxyl group-containing monomers, hydroxyl group-containing monomers, epoxy group-containing monomers, double bond-containing monomers, triple bond-containing monomers, and amide group-containing monomers, because the peeling performance of the adhesive tape for semiconductor manufacturing process against chip components is further improved and adhesive residue on the chip components can be further suppressed. Among them, it is more preferable to contain at least one selected from the group consisting of carboxyl group-containing monomers and hydroxyl group-containing monomers, and it is particularly preferable to use a carboxyl group-containing monomer and a hydroxyl group-containing monomer in combination.
[0021] Examples of the carboxy group-containing monomer include (meth)acrylic acid-based monomers such as (meth)acrylic acid. Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as 4-hydroxybutyl (meth)acrylate and 2-hydroxyethyl (meth)acrylate. Examples of the epoxy group-containing monomer include glycidyl (meth)acrylate, etc. Examples of the double bond-containing monomer include allyl (meth)acrylate, hexanediol di(meth)acrylate, etc. The triple bond-containing monomer may, for example, be propargyl (meth)acrylate. The amide group-containing monomer includes (meth)acrylamide.
[0022] In the (meth)acrylic copolymer, the preferred lower limit of the content of the structure derived from the hydroxyl group-containing monomer is 2% by mass. When the content of the structure derived from the hydroxyl group-containing monomer is 2% by mass or more, the cohesive strength of the first pressure-sensitive adhesive layer is increased, the peeling performance of the pressure-sensitive adhesive tape for semiconductor manufacturing process with respect to chip components is improved, and adhesive residue on the chip components can be further suppressed. The more preferred lower limit of the content of the structure derived from the hydroxyl group-containing monomer is 3% by mass, and the even more preferred lower limit is 5% by mass. Moreover, the preferred upper limit of the content of the structure derived from the hydroxyl group-containing monomer is 10% by mass. By making the content of the structure derived from the hydroxyl group-containing monomer 10% by mass or less, the first pressure-sensitive adhesive layer does not become too hard, and the position of the chip component arranged on the first pressure-sensitive adhesive layer can be more firmly held, and the holding performance of the pressure-sensitive adhesive tape for semiconductor manufacturing process of the present invention for the chip component is further improved. The more preferred upper limit of the pressure-sensitive adhesive tape for semiconductor manufacturing process of the present invention is 8% by mass, and even more preferred upper limit is 5% by mass.
[0023] In the (meth)acrylic copolymer, the preferred lower limit of the total content of the structure derived from the crosslinkable functional group-containing monomer is 0.1% by mass, and the preferred upper limit is 30% by mass. When the total content of the structure derived from the crosslinkable functional group-containing monomer is within the above range, the cohesive force of the first pressure-sensitive adhesive layer is further increased, the peeling performance of the pressure-sensitive adhesive tape for semiconductor manufacturing process with respect to chip components is further improved, and adhesive residue on the chip components can be further suppressed. The more preferred lower limit of the total content of the structure derived from the crosslinkable functional group-containing monomer is 0.5% by mass, the more preferred upper limit is 25% by mass, the even more preferred lower limit is 1% by mass, and the even more preferred upper limit is 20% by mass. In addition, when only one type of structure derived from the crosslinkable functional group-containing monomer is present in the (meth)acrylic copolymer, the total content of the structures derived from the crosslinkable functional group-containing monomer indicates the content of the structures derived from the crosslinkable functional group-containing monomer that is present only in that one type.
[0024] The (meth)acrylic copolymer may further contain a structure derived from another monomer other than the structure derived from the (meth)acrylic monomer and the structure derived from the crosslinkable functional group-containing monomer.
[0025] Examples of the other monomers include 2-[2-hydroxy-5-[2-(methacryloyloxy)ethyl]phenyl]-2H-benzotriazole, which has ultraviolet absorbing properties.
[0026] The weight average molecular weight (Mw) of the (meth)acrylic copolymer has a preferred lower limit of 200,000 and a preferred upper limit of 2,000,000. When the weight average molecular weight of the (meth)acrylic copolymer is within the above range, the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip components is further improved, and adhesive residue on the chip components can be further suppressed. The weight average molecular weight of the (meth)acrylic copolymer has a more preferred lower limit of 1,000,000 and a more preferred upper limit of 1,800,000. In this specification, the weight average molecular weight (Mw) is a weight average molecular weight calculated using standard polystyrene as determined by gel permeation chromatography (GPC).
[0027] The molecular weight distribution (Mw / Mn) of the (meth)acrylic copolymer preferably has a lower limit of 2 and an upper limit of 8. When the molecular weight distribution of the (meth)acrylic copolymer is within the above range, the peeling performance of the adhesive tape for use in the semiconductor manufacturing process of the present invention for chip components is further improved, and adhesive residue on the chip components can be further suppressed. The molecular weight distribution of the (meth)acrylic copolymer is more preferably 3 and 5. Here, Mn means the number average molecular weight calculated as standard polystyrene by GPC measurement.
[0028] The weight average molecular weight (Mw) and the molecular weight distribution (Mw / Mn) of the (meth)acrylic copolymer are measured by the following method. That is, the (meth)acrylic copolymer is diluted 50 times with tetrahydrofuran (THF), and the obtained diluted solution is filtered through a filter (material: polytetrafluoroethylene, pore diameter: 0.2 μm) to prepare a measurement sample. Next, this measurement sample is supplied to a gel permeation chromatograph (for example, Waters' "2690 Separations Module" etc.), and GPC measurement is performed under conditions of a sample flow rate of 1 mL / min and a column temperature of 40°C. The polystyrene-equivalent molecular weight of the (meth)acrylic copolymer is measured to obtain the weight average molecular weight and number average molecular weight of the (meth)acrylic copolymer, and the molecular weight distribution is calculated. A GPC KF-806L (Showa Denko KK) is used as the column, and a differential refractometer is used as the detector.
[0029] The (meth)acrylic copolymer can be obtained, for example, by polymerizing a monomer mixture as a raw material through a radical reaction in the presence of a polymerization initiator. Examples of the radical reaction include living radical polymerization, free radical polymerization, etc. Living radical polymerization can provide a copolymer having a more uniform molecular weight and composition compared to free radical polymerization, and can suppress the generation of low molecular weight components, etc., thereby improving the cohesive force of the first pressure-sensitive adhesive layer, improving the peeling performance of the pressure-sensitive adhesive tape for semiconductor manufacturing process of the present invention for chip components, and suppressing adhesive residue on the chip components. The method for polymerizing the monomer mixture may be a conventionally known method, such as solution polymerization (boiling point polymerization or constant temperature polymerization), UV polymerization, emulsion polymerization, suspension polymerization, bulk polymerization, etc. Among these, solution polymerization and UV polymerization are preferred because they result in a higher adhesive strength of the resulting adhesive tape. When solution polymerization is used as a method for polymerizing the monomer mixture, examples of the reaction solvent include ethyl acetate, toluene, methyl ethyl ketone, dimethyl sulfoxide, ethanol, acetone, diethyl ether, etc. These reaction solvents may be used alone or in combination of two or more kinds.
[0030] Examples of the polymerization initiator include organic peroxides and azo compounds. Examples of the organic peroxides include 1,1-bis(t-hexylperoxy)-3,3,5-trimethylcyclohexane, t-hexylperoxypivalate, t-butylperoxypivalate, 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy)hexane, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyisobutyrate, t-butylperoxy-3,5,5-trimethylhexanoate, and t-butylperoxylaurate. Examples of the azo compound include azobisisobutyronitrile and azobiscyclohexanecarbonitrile. These polymerization initiators may be used alone or in combination of two or more kinds. In addition, when the radical reaction method is the living radical polymerization, the polymerization initiator may be, for example, an organic tellurium polymerization initiator. The organic tellurium polymerization initiator is not particularly limited as long as it is one that is generally used in living radical polymerization, and may be, for example, an organic tellurium compound, an organic telluride compound, etc. In addition to the organic tellurium polymerization initiator, an azo compound may also be used as the polymerization initiator in the living radical polymerization in order to accelerate the polymerization rate.
[0031] The first pressure-sensitive adhesive layer contains an ultraviolet absorbing agent (UVA-1). Since the first adhesive layer contains an ultraviolet absorber (UVA-1), heat or vibration is efficiently generated by irradiation with laser light, and deformation due to ablation occurs easily, so that the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip components is improved. In addition, since the adhesive layer appropriately absorbs laser light, the chip attached thereto can be prevented from absorbing light, so that the manufacturing quality of the chip manufactured using the adhesive tape for semiconductor manufacturing process of the present invention is improved.
[0032] The ultraviolet absorber (UVA-1) may be an ultraviolet absorber that is solid at room temperature, but is preferably an ultraviolet absorber that is liquid at room temperature. When the first adhesive layer contains the ultraviolet absorber that is liquid at room temperature, the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip components is further improved. In addition, if the ultraviolet absorber is liquid at room temperature, the ultraviolet absorber is less likely to precipitate, and the holding performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip components is further improved. In this specification, "room temperature" refers to a temperature range of 20°C or higher and 25°C or lower.
[0033] Examples of the ultraviolet absorber (UVA-1) include benzotriazole-based ultraviolet absorbers and hydroxylphenyltriazine-based ultraviolet absorbers. Examples of the ultraviolet absorber include ethylhexyl methoxycinnamate, octyl methoxycinnamate, ethylhexyl paramethoxycinnamate, diethylaminohydroxybenzoylhexyl benzoate, bisethylhexyloxyphenol methoxyphenyltriazine, and t-butylmethoxydibenzoylmethane. Among these, benzotriazole-based ultraviolet absorbers and hydroxylphenyltriazine-based ultraviolet absorbers are preferred from the viewpoint of excellent compatibility with other components in the first adhesive layer. These ultraviolet absorbers may be used alone or in combination of two or more.
[0034] The preferred upper limit of the content of the ultraviolet absorber (UVA-1) is 15 parts by mass relative to 100 parts by mass of the (meth)acrylic copolymer. If the content of the ultraviolet absorber (UVA-1) is 15 parts by mass or less, the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip parts is further improved. The more preferred upper limit of the content of the ultraviolet absorber (UVA-1) is 12 parts by mass, and the even more preferred upper limit is 10 parts by mass. The preferred lower limit of the content of the ultraviolet absorber (UVA-1) is 1 part by mass. When the content of the ultraviolet absorber (UVA-1) is 1 part by mass or more, the first adhesive layer generates heat or vibration more efficiently by irradiation with laser light, and deformation due to ablation occurs more easily, so that the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip components is further improved. In addition, the adhesive layer appropriately absorbs laser light, so that the chip components attached thereto can be more effectively prevented from absorbing light, and the manufacturing quality of the chip components manufactured using the adhesive tape for semiconductor manufacturing process of the present invention is further improved. The more preferred lower limit of the content of the ultraviolet absorber (UVA-1) is 2 parts by mass, and the even more preferred lower limit is 4 parts by mass.
[0035] The first pressure-sensitive adhesive layer preferably further contains a crosslinking agent. The crosslinking agent is not particularly limited and is selected depending on the type of crosslinkable functional group contained in the (meth)acrylic copolymer, and examples thereof include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, metal chelate-based crosslinking agents, etc. Among these, isocyanate-based crosslinking agents are preferred because they make it easy to adjust the gel fraction, etc. of the first pressure-sensitive adhesive layer to the range described below.
[0036] Examples of the isocyanate crosslinking agent include toluene diisocyanate (TDI) crosslinking agents, hexamethylene diisocyanate (HDI) crosslinking agents, and the like. Examples of the epoxy crosslinking agent include N,N'-(cyclohexane-1,3-diylbismethylene)bis(diglycidylamine), N,N,N',N'-tetraglycidyl-1,3-benzenedi(methanamine), and the like.
[0037] The content of the crosslinking agent is not particularly limited, and the degree of crosslinking (gel fraction) of the first pressure-sensitive adhesive layer can be adjusted by adjusting the amount of crosslinkable functional groups in the base polymer contained in the first pressure-sensitive adhesive layer and the content of the crosslinking agent. The content of the crosslinking agent relative to 100 parts by mass of the base polymer contained in the first adhesive layer is preferably 0.01 parts by mass and preferably 15 parts by mass. By the content of the crosslinking agent being within the above range, the base polymer contained in the first adhesive layer can be appropriately crosslinked to increase the cohesive force of the first adhesive layer, and the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip components can be further improved and adhesive residue on the chip components can be further suppressed. The content of the crosslinking agent is more preferably 0.1 parts by mass and more preferably 12 parts by mass, more preferably 0.15 parts by mass and more preferably 8 parts by mass.
[0038] The first pressure-sensitive adhesive layer may further contain a tackifier (tackifier). The tackifier may be a tackifier that is solid at room temperature, or a tackifier that is liquid at room temperature.
[0039] The tackifier is not particularly limited, and examples thereof include rosin ester resin, terpene phenol resin, terpene resin, and coumarone resin.
[0040] The content of the tackifier is not particularly limited, but from the viewpoint of the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention against chip parts, it is preferable that the tackifier is not contained in the first adhesive layer. When the tackifier is contained, the preferred upper limit of the content is 40 parts by mass relative to 100 parts by mass of the base polymer contained in the first adhesive layer. By making the content of the tackifier 40 parts by mass or less, the performance of reattaching the chip to the adhesive tape for semiconductor manufacturing process of the present invention is further improved. The more preferred upper limit of the content of the tackifier is 30 parts by mass.
[0041] The first pressure-sensitive adhesive layer may further contain an inorganic filler such as fumed silica. By incorporating the inorganic filler, the cohesive strength of the first adhesive layer can be increased, the peeling performance of the adhesive tape for semiconductor manufacturing processes of the present invention for chip components can be improved, and adhesive residue on the chip components can be further reduced.
[0042] The first pressure-sensitive adhesive layer may further contain known additives such as plasticizers, resins, surfactants, waxes, particulate fillers, etc. These additives may be used alone or in combination of two or more kinds.
[0043] The upper limit of the maximum value of the loss tangent (tan δ) of the first adhesive layer in the temperature range of 20° C. to 40° C. is 0.1. When the maximum value of the loss tangent of the first adhesive layer in the temperature range of 20° C. to 40° C. is 0.1 or less, the first adhesive layer loses less energy during ablation, and the adhesive tape for semiconductor manufacturing process of the present invention has improved peeling performance for chip components. The upper limit of the maximum value of the loss tangent of the first adhesive layer in the temperature range of 20° C. to 40° C. is preferably 0.08, more preferably 0.05. There is no particular preferred lower limit for the maximum value of the loss tangent (tan δ) of the first pressure-sensitive adhesive layer in the temperature range of 20° C. or higher and 40° C. or lower, but the substantial lower limit is about 0.01. The loss tangent (tan δ) of the first pressure-sensitive adhesive layer in a temperature range of 20° C. to 40° C. can be measured by dynamic viscoelasticity measurement. Specifically, for example, the first pressure-sensitive adhesive layer can be measured using a dynamic viscoelasticity measuring device (for example, Rheometrics Dynamic Analyze RDA-700 manufactured by Rheometrics) under conditions of a measurement temperature of −40 to 150° C., a temperature rise rate of 5° C. / min, and a frequency of 1 Hz. When the thickness of the first pressure-sensitive adhesive layer is less than 500 μm, the first pressure-sensitive adhesive layer is laminated to prepare a sample of only the first pressure-sensitive adhesive layer having a thickness of about 500 μm, and the measurement is performed. In addition, the sample of only the first pressure-sensitive adhesive layer can be prepared by removing the base layer of the semiconductor manufacturing process adhesive tape, separating only the first pressure-sensitive adhesive layer, and then stacking the separated first pressure-sensitive adhesive layer. The method of removing the base layer is not particularly limited as long as it avoids treatment with a solvent, treatment involving a chemical reaction, treatment at high temperature, etc., in order to avoid denaturation of the pressure-sensitive adhesive layer. As a specific method, a method of bonding the first pressure-sensitive adhesive layers together, selecting an appropriate temperature and peeling speed, peeling the base layer and the first pressure-sensitive adhesive layer by peeling them off, and removing the base layer, or a method of physically grinding the base layer can be selected. In addition, a sample of only the first pressure-sensitive adhesive layer may be prepared using a sheet consisting of only the first pressure-sensitive adhesive layer prepared separately.
[0044] Methods for adjusting the loss tangent (tan δ) of the first adhesive layer in the temperature range of 20°C or higher and 40°C or lower within the above range include, for example, a method of changing the composition of the base polymer contained in the first adhesive layer, a method of adjusting the weight average molecular weight (Mw) or molecular weight distribution (Mw / Mn) of the base polymer contained in the first adhesive layer, a method of adjusting the type or content of the crosslinking agent, etc.
[0045] The preferred lower limit of the ultraviolet ray absorptance of the first adhesive layer at a wavelength of 355 nm is 80%. When the first adhesive layer has an ultraviolet ray absorptance of 80% or more at a wavelength of 355 nm, the first adhesive layer generates heat or vibration more efficiently by irradiation with laser light, and deformation due to ablation occurs more easily, so that the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip components is further improved. In addition, the first adhesive layer moderately absorbs laser light, so that the chip attached thereto can be more effectively prevented from absorbing light, and thus the manufacturing quality of the chip manufactured using the adhesive tape for semiconductor manufacturing process of the present invention is improved. The more preferred lower limit of the ultraviolet ray absorptance of the first adhesive layer at a wavelength of 355 nm is 90%, and the even more preferred lower limit is 95%. There is no particular upper limit to the absorptance of the first pressure-sensitive adhesive layer for ultraviolet light having a wavelength of 355 nm. As a method for measuring the ultraviolet absorptance of the first adhesive layer at a wavelength of 355 nm, for example, the adhesive layer may be measured using a spectrophotometer (Shimadzu Corporation, "UV-2600i", etc.) in accordance with JIS L1925.
[0046] Methods for adjusting the ultraviolet absorptivity of the first adhesive layer at a wavelength of 355 nm within the above range include, for example, changing the composition of the base polymer contained in the first adhesive layer, adjusting the type and content of the ultraviolet absorber (UVA-1), and adjusting the thickness of the first adhesive layer.
[0047] The preferred lower limit of the gel fraction of the first pressure-sensitive adhesive layer is 60% by mass, and the preferred upper limit is 95% by mass. If the gel fraction of the first pressure-sensitive adhesive layer is 60% by mass or more, the peeling performance of the pressure-sensitive adhesive tape for use in semiconductor manufacturing processes with respect to chip components is further improved. If the gel fraction of the first pressure-sensitive adhesive layer is 95% by mass or less, the holding performance of the pressure-sensitive adhesive tape for use in semiconductor manufacturing processes with respect to chip components is further improved. The more preferred lower limit of the gel fraction of the first pressure-sensitive adhesive layer is 80% by mass, and the more preferred upper limit is 90% by mass. The gel fraction of the first pressure-sensitive adhesive layer can be measured by the following method. Only the first adhesive layer W0 (g) is taken out from the adhesive tape for semiconductor manufacturing process, immersed in 50 mL of ethyl acetate, and shaken in a shaker at 23°C and 200 rpm for 24 hours. After shaking, the ethyl acetate and the first adhesive layer that has absorbed and swollen with the ethyl acetate are separated using a metal mesh (opening #200 mesh, W1 (g)). The separated first adhesive layer is dried for 1 hour at 110°C. The mass W2 (g) of the first adhesive layer including the dried metal mesh is measured, and the gel fraction of the first adhesive layer is calculated using the following formula. Gel fraction (mass%) = 100 × (W2-W1) / W0 (W0: initial mass of the first adhesive layer, W1: initial mass of the metal mesh, W2: mass of the first adhesive layer including the metal mesh after drying) However, if the first adhesive layer is not completely dissolved in ethyl acetate, a solvent such as toluene, hexane, water, etc. is used instead of ethyl acetate. Specifically, if the first adhesive layer contains, for example, a styrene-based elastomer, toluene or hexane is used, and if it contains polyvinyl alcohol, hot water at 90°C is used.
[0048] Methods for adjusting the gel fraction of the first pressure-sensitive adhesive layer to within the above range include, for example, methods for adjusting the composition or weight average molecular weight (Mw) of the base polymer contained in the first pressure-sensitive adhesive layer, or the type or amount of the crosslinking agent, as described above.
[0049] The preferred upper limit of the thickness of the first pressure-sensitive adhesive layer is 40 μm. If the thickness of the first pressure-sensitive adhesive layer is 40 μm or less, adhesive residue on chip components can be further suppressed. Since the adhesive tape for semiconductor manufacturing processes has improved holding and peeling performance for chip components and adhesive residue on chip components can be further suppressed, the more preferred upper limit of the thickness of the first pressure-sensitive adhesive layer is 30 μm, and the even more preferred upper limit is 20 μm. The preferred lower limit of the thickness of the first pressure-sensitive adhesive layer is 5 μm. If the thickness of the first pressure-sensitive adhesive layer is 5 μm or more, the adhesive tape for semiconductor manufacturing process has improved retention and peeling performance for chip components. The more preferred lower limit of the thickness of the first pressure-sensitive adhesive layer is 10 μm, and the even more preferred lower limit is 20 μm.
[0050] The adhesive tape for the semiconductor manufacturing process of the present invention only needs to have the base layer and the first adhesive layer as described above, but may further have other layers as long as the effects of the present invention are not impaired.
[0051] The adhesive tape has a base layer, an intermediate adhesive layer, and a first adhesive layer in this order, the first adhesive layer contains an ultraviolet absorbing agent (UVA-1), the first adhesive layer has a maximum loss tangent (tan δ) of 0.1 or less in a temperature range of 20°C to 40°C, and is irradiated at a wavelength of 365 nm and an irradiation intensity of 7.8 mW / cm. 2 The cumulative amount of ultraviolet light is 190 mJ / cm 2 The present invention also provides an adhesive tape for use in semiconductor manufacturing processes, the adhesive strength of which decreases by 60% or less after irradiation so as to satisfy the above requirement.
[0052] By having the intermediate adhesive layer in the adhesive tape for semiconductor manufacturing process of the present invention, when the chip components are transferred from the dicing tape or the like to the adhesive tape for semiconductor manufacturing process of the present invention in order to transfer the chip components, the intermediate adhesive layer acts as a cushion layer, improving the ease of attachment to the chip components and increasing production efficiency. In addition, when the intermediate adhesive layer contains an ultraviolet absorber, the vibration of ablation caused by the irradiation of laser light can be efficiently transmitted to the first adhesive layer, improving the peeling performance of the adhesive tape for conductor manufacturing process of the present invention for chip components and allowing the chip components to be peeled off without leaving any adhesive residue. In addition, since the ablation site is different from the adhesive, it is possible to suppress the adhesion of adhesive residue to the chip components due to scattering of the ablation site that occurs during ablation.
[0053] When the adhesive tape for a conductor manufacturing process of the present invention has a base layer, an intermediate adhesive layer, and a first adhesive layer, the base layer and the first adhesive layer can be the same as the base layer and the first adhesive layer described above.
[0054] The intermediate adhesive layer preferably contains a base polymer. Examples of the base polymer contained in the intermediate adhesive layer include ABA block copolymers, (meth)acrylic copolymers, urethane copolymers, silicone adhesives, etc. Among them, when the intermediate adhesive layer contains an ultraviolet absorber, the intermediate adhesive layer can be appropriately deformed by ablation by irradiating laser light, and the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip components is further improved, so ABA block copolymers and (meth)acrylic copolymers are preferred. When the adhesive layer contains an ultraviolet absorber, ABA block copolymers are more preferred from the viewpoint that ablation occurring at the irradiated area when the intermediate adhesive layer is irradiated with laser light is not too large. In addition, (meth)acrylic copolymers are more preferred from the viewpoint of ensuring adhesion between the intermediate adhesive layer and the base layer and the barrier layer described later, and suppressing defects such as the edge lifting.
[0055] As the (meth)acrylic copolymer in the intermediate adhesive layer, for example, the same (meth)acrylic copolymer as in the first adhesive layer described above can be used.
[0056] The ABA block copolymer is a copolymer including a block A having a rigid structure (hereinafter also referred to as a "hard segment") and a block B having a flexible structure (hereinafter also referred to as a "soft segment"). The ABA block copolymer may have a non-uniform phase separation structure in which the two blocks are poorly compatible with each other, and in which spherical islands formed by aggregation of block A are scattered in a sea of block B, or in which cylindrical structures formed by aggregation of block A are scattered in a sea of block B. Such a phase separation structure in which spherical islands are scattered is also called a spherical phase separation structure, and a phase separation structure in which cylindrical structures are scattered is also called a cylindrical phase separation structure. The islands of the phase separation structure become pseudo-crosslinking points, and rubber elasticity can be imparted to the ABA block copolymer, so that the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip components is further improved.
[0057] In the ABA block copolymer, the block A is not particularly limited as long as it has a rigid structure, but it is preferable that the block A contains a structure derived from an aromatic vinyl monomer. The block A may further have, in addition to the structure derived from the aromatic vinyl monomer, for example, a structure derived from a compound having a cyclic structure, a compound having a short side chain substituent, or the like, within the scope of the invention.
[0058] Examples of the aromatic vinyl monomer include styrene, alpha-methylstyrene, para-methylstyrene, and chlorostyrene. These aromatic vinyl monomers may be used alone or in combination of two or more. Among them, styrene is preferred because it further improves the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention against chip components. In this specification, the structure derived from an aromatic vinyl monomer refers to a structure as shown in the following formula (1) or (2).
[0059] [ka]
[0060] In formulas (1) and (2), R 1 represents a substituent having an aromatic ring. 1 Examples of the phenyl group include a phenyl group, a methylphenyl group, and a chlorophenyl group.
[0061] In the ABA block copolymer, the preferred lower limit of the content ratio of the structure derived from the aromatic vinyl monomer is 1% by mass, and the preferred upper limit is 30% by mass. By having the content of the structure derived from the aromatic vinyl monomer within the above range, the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip components and the performance of reattaching the chip components to the adhesive tape for semiconductor manufacturing process are improved. The more preferred lower limit of the content of the structure derived from the aromatic vinyl monomer is 5% by mass, the more preferred upper limit is 28% by mass, the even more preferred lower limit is 8% by mass, the even more preferred upper limit is 25% by mass, the particularly preferred lower limit is 10% by mass, and the particularly preferred upper limit is 20% by mass.
[0062] In the ABA block copolymer, block B is not particularly limited as long as it has a flexible structure, but since the gel fraction and the like of the intermediate adhesive layer are easily adjusted to the range described below, it is preferable that block B contains a structure derived from a conjugated diene monomer or a structure derived from a (meth)acrylic monomer. From the viewpoint of improving the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip components and the performance of replacing chip components with the adhesive tape for semiconductor manufacturing process, it is more preferable that block B contains a structure derived from a (meth)acrylic monomer. The block B may have a structure derived from a monomer other than the conjugated diene monomer and the (meth)acrylic monomer, as long as the effects of the present invention are not impaired.
[0063] Examples of the conjugated diene monomer include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-octadiene, 1,3-hexadiene, 1,3-cyclohexadiene, 4,5-diethyl-1,3-octadiene, 3-butyl-1,3-octadiene, myrcene, and chloroprene. These conjugated diene monomers may be used alone or in combination of two or more. Among them, 1,3-butadiene and isoprene are preferred because they have high polymerization reactivity and are easily available industrially.
[0064] The double bond (unsaturated bond) of the structure derived from the conjugated diene monomer may be converted to a saturated bond by hydrogenation. For example, when the double bond (unsaturated bond) of the structure derived from 1,3-butadiene as the structure derived from the conjugated diene monomer is hydrogenated, it is converted to an ethylene-butylene structure. The ratio of the hydrogenation (hydrogenation rate) is not particularly limited, and the structure may be partially hydrogenated or mostly hydrogenated. The hydrogenation ratio (hydrogenation rate) was measured using deuterated chloroform as the solvent at 20 Hz. 1 It can be calculated by measuring the H-NMR spectrum.
[0065] In the ABA block copolymer, the content ratio of the structure derived from the conjugated diene monomer may be 0% by mass, and the substantial upper limit is 99% by mass, so long as the effects of the present invention are exhibited. From the viewpoint of improving the peeling performance of the pressure-sensitive adhesive tape for semiconductor manufacturing processes of the present invention for chip components and the performance of replacing chip components with the pressure-sensitive adhesive tape for semiconductor manufacturing processes, the content ratio of the structure derived from the conjugated diene monomer is preferably 30% by mass, more preferably 95% by mass, more preferably 40% by mass, even more preferably 90% by mass, and still more preferably 70% by mass.
[0066] Examples of the (meth)acrylic monomer include the same (meth)acrylic monomers as those used in the pressure-sensitive adhesive layer described above. These monomers may be used alone or in combination.
[0067] It is preferable that the block B further contains a structure derived from a crosslinkable functional group-containing monomer. The block B contains a structure derived from the crosslinkable functional group-containing monomer, which increases the cohesive strength of the intermediate adhesive layer, thereby improving the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention against chip components. In addition, when the intermediate adhesive layer contains a crosslinking agent described below, the crosslinkable functional group derived from the crosslinkable functional group-containing monomer reacts with the crosslinking agent to form a crosslinked structure, thereby improving the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention against chip components.
[0068] Examples of the crosslinkable functional group-containing monomer include the same crosslinkable functional group-containing monomers as those used in the pressure-sensitive adhesive layer described above. These monomers may be used alone or in combination.
[0069] In addition to the block B, the block A also preferably contains a structure derived from the crosslinkable functional group-containing monomer.
[0070] In the ABA block copolymer, the content of the structure derived from the crosslinkable functional group-containing monomer (the total content in the block A and the block B) is preferably 0.1% by mass at the lower limit and 30% by mass at the upper limit. When the content of the structure derived from the crosslinkable functional group-containing monomer is within the above range, the cohesive force of the intermediate adhesive layer is further increased, and the peeling performance of the adhesive tape for semiconductor manufacturing process for chip components is further improved. The more preferred lower limit of the content of the structure derived from the crosslinkable functional group-containing monomer is 0.5% by mass, the even more preferred lower limit is 1% by mass, the more preferred upper limit is 20% by mass, and the even more preferred upper limit is 10% by mass.
[0071] In the ABA block copolymer, the glass transition temperature of the block B is not particularly limited, but is preferably not less than −70° C. and not more than 0° C. When the glass transition temperature of the block B is within the above range, the peeling performance of the adhesive tape for chip components is further improved even when chip components having protrusions or small-sized chip components are transferred, and adhesive residue on the chip components can be further suppressed. The glass transition temperature of the block B is more preferably -50°C, even more preferably -30°C, and more preferably -5°C, even more preferably -10°C. The glass transition temperature of the block B can be measured using a dynamic viscoelasticity measuring device (e.g., Rheometrics Dynamic Analyze RDA-700 manufactured by Rheometrics) under conditions of a measurement temperature of −40 to 150° C., a heating rate of 5° C. / min, and a frequency of 1 Hz.
[0072] The method for adjusting the glass transition temperature of the block B to be within the above range is not particularly limited. In order to adjust the glass transition temperature of the block B to be within the above range, it is preferable that the (meth)acrylic monomer contains a (meth)acrylic acid ester monomer having a glass transition temperature of −10° C. or lower when formed into a homopolymer.
[0073] The (meth)acrylic monomer contains a (meth)acrylic acid ester monomer having a glass transition temperature of -10°C or less when made into the homopolymer, so that the storage modulus of the intermediate adhesive layer can be adjusted to a more preferred range. Examples of the (meth)acrylic acid ester monomer having a glass transition temperature of -10°C or less when made into the homopolymer include butyl acrylate, ethyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, lauryl acrylate, and methoxyethyl acrylate. In particular, butyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, and methoxyethyl acrylate are preferred.
[0074] In the ABA block copolymer, the content of the structure derived from the (meth)acrylic acid ester monomer having a glass transition temperature of -10°C or less when made into the homopolymer is not particularly limited and may be 0 mass%, but the preferred lower limit is 40 mass%. If the content of the structure derived from the (meth)acrylic acid ester monomer having a glass transition temperature of -10°C or less when made into the homopolymer is 40 mass% or more, the peeling performance of the adhesive tape for chip components is further improved. A more preferred lower limit of the content of the structure derived from the (meth)acrylic acid ester monomer having a glass transition temperature of -10°C or less when made into the homopolymer is 50 mass%. The upper limit of the content of the structure derived from the (meth)acrylic acid ester monomer having a glass transition temperature of −10° C. or lower when made into the above-mentioned homopolymer is not particularly limited, but from the viewpoint of temporarily fixing the chip components, a preferred upper limit is 95 mass %, and a more preferred upper limit is 90 mass %.
[0075] In the ABA block copolymer, the content of the block A (hard segment) is not particularly limited, but is preferably 1% by mass or more and 40% by mass or less. When the content of the block A is within the above range, the breaking strength of the intermediate adhesive layer is increased, and adhesive residue on the chip components can be further suppressed. A more preferred lower limit of the content of the block A is 2% by mass, an even more preferred lower limit is 5% by mass, and a particularly preferred lower limit is 10% by mass. A more preferred upper limit of the content of the block A is 35% by mass, an even more preferred upper limit is 30% by mass, an even more preferred upper limit is 25% by mass, an even more preferred upper limit is 22% by mass, and a particularly preferred upper limit is 20% by mass.
[0076] The weight average molecular weight (Mw) of the ABA block copolymer is not particularly limited, but is preferably 50,000 or more and 800,000 or less. When the weight average molecular weight is within the above range, the peeling performance of the adhesive tape for semiconductor manufacturing process for chip components is further improved, and adhesive residue on the chip components can be further suppressed. A more preferred lower limit of the weight average molecular weight is 75,000, an even more preferred lower limit is 100,000, and an even more preferred lower limit is 200,000. A more preferred upper limit of the weight average molecular weight is 600,000. The weight average molecular weight can be determined, for example, by gel permeation chromatography (GPC) in terms of standard polystyrene. More specifically, the weight average molecular weight can be measured using a Waters 2690 Separations Module as a measuring instrument, a Showa Denko GPC KF-806L column, ethyl acetate as a solvent, at a sample flow rate of 1 mL / min and a column temperature of 40°C.
[0077] To obtain the ABA block copolymer, raw material monomers for the block A and the block B are respectively subjected to a radical reaction in the presence of a polymerization initiator to obtain the block A and the block B, and then the two are reacted or copolymerized. Alternatively, after obtaining the block A, raw material monomers for the block B may be added and copolymerized. As the method for carrying out the radical reaction, that is, the polymerization method, a conventionally known method can be used, and examples thereof include solution polymerization (boiling point polymerization or constant temperature polymerization), emulsion polymerization, suspension polymerization, bulk polymerization, and the like.
[0078] The intermediate adhesive layer preferably further contains an ultraviolet absorbing agent (UVA-2). By containing an ultraviolet absorber (UVA-2) in the intermediate adhesive layer, the stimulation of the laser light is more efficiently converted into heat or vibration in the intermediate adhesive layer, making deformation due to ablation more likely to occur, and further improving the peeling performance of the adhesive tape for semiconductor manufacturing processes of the present invention for chip components.
[0079] The ultraviolet absorber (UVA-2) may be a solid ultraviolet absorber at room temperature, but is preferably a liquid ultraviolet absorber at room temperature. By containing the ultraviolet absorber in the intermediate adhesive layer, the ultraviolet absorber (UVA-2) is less likely to precipitate, and the storage stability of the adhesive tape for semiconductor manufacturing process of the present invention is further improved.
[0080] Examples of the ultraviolet absorbing agent (UVA-2) include the same as the ultraviolet absorbing agent (UVA-1) described above. These ultraviolet absorbing agents may be used alone or in combination of two or more.
[0081] The preferred upper limit of the content of the ultraviolet absorber (UVA-2) is 15 parts by mass relative to 100 parts by mass of the base polymer contained in the intermediate adhesive layer. If the content of the ultraviolet absorber (UVA-2) is 15 parts by mass or less, the adhesion between the intermediate adhesive layer and other layers and the retention performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip components are further improved. The more preferred upper limit of the content of the ultraviolet absorber (UVA-2) is 12 parts by mass, and the even more preferred upper limit is 10 parts by mass. The preferred lower limit of the content of the ultraviolet absorber (UVA-2) is 1 part by mass. By having the content of the ultraviolet absorber (UVA-2) be 1 part by mass or more, the stimulation of the laser light is converted into heat or vibration more efficiently in the intermediate adhesive layer, so that deformation due to ablation occurs more easily, and the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip components is further improved. The more preferred lower limit of the content of the ultraviolet absorber (UVA-2) is 2 parts by mass, and the even more preferred lower limit is 4 parts by mass.
[0082] The preferred lower limit of the ultraviolet ray absorptance of the intermediate adhesive layer at a wavelength of 355 nm is 80%. When the intermediate adhesive layer has an ultraviolet ray absorptance of 80% or more at a wavelength of 355 nm, heat or vibration is generated more efficiently by irradiation with laser light, and deformation due to ablation occurs more easily, improving the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip components. The more preferred lower limit of the ultraviolet ray absorptance of the intermediate adhesive layer at a wavelength of 355 nm is 90%, and the even more preferred lower limit is 95%. In addition, there is no particular upper limit to the ultraviolet ray absorptance of the intermediate adhesive layer at a wavelength of 355 nm. The ultraviolet ray absorptance at a wavelength of 355 nm of the intermediate adhesive layer can be measured, for example, by the same method as that for measuring the ultraviolet ray absorptance at a wavelength of 355 nm of the first adhesive layer.
[0083] The gel fraction of the intermediate adhesive layer is not particularly limited, but a preferred lower limit is 70% by mass, and a preferred upper limit is 95% by mass. If the gel fraction of the intermediate adhesive layer is 70% by mass or more, the peeling performance of the adhesive tape for semiconductor manufacturing process for chip components is further improved. If the gel fraction of the intermediate adhesive layer is 95% by mass or less, the holding performance of the adhesive tape for semiconductor manufacturing process for chip components is further improved. A more preferred lower limit of the gel fraction is 80% by mass, and a more preferred upper limit is 90% by mass. The gel fraction of the intermediate adhesive layer can be measured, for example, by the same method as that for measuring the gel fraction of the first adhesive layer described above.
[0084] The thickness of the intermediate adhesive layer is not particularly limited, but the preferred lower limit is 3 μm and the preferred upper limit is 50 μm. If the thickness of the intermediate adhesive layer is within the above range, when the chip component is transferred from the dicing tape or the like to the adhesive tape for semiconductor manufacturing process of the present invention in order to transfer the chip component, the intermediate adhesive layer becomes a cushion layer, improving the repositionability of the chip component and increasing production efficiency. In addition, when the intermediate adhesive layer contains an ultraviolet absorber, if the thickness of the intermediate adhesive layer is within the above range, the intermediate adhesive layer can be appropriately deformed by ablation by irradiating laser light, and the peeling performance of the adhesive tape for semiconductor manufacturing process for chip components is further improved. The more preferred lower limit of the thickness of the intermediate adhesive layer is 5 μm, the more preferred upper limit is 30 μm, the even more preferred lower limit is 8 μm, and the even more preferred upper limit is 20 μm.
[0085] When the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process of the present invention has an intermediate pressure-sensitive adhesive layer, it preferably further has a barrier layer between the intermediate pressure-sensitive adhesive layer and the first pressure-sensitive adhesive layer. Since the adhesive tape for semiconductor manufacturing processes of the present invention has a barrier layer, the barrier layer further suppresses scattering of the intermediate adhesive layer when the intermediate adhesive layer is ablated by irradiation with laser light, thereby further improving the peeling performance of the adhesive tape for semiconductor manufacturing processes of the present invention for chip components.
[0086] The barrier layer preferably comprises a resin film having a polar functional group. Since the barrier layer has a resin film having a polar functional group, the anchoring property between the barrier layer and the first adhesive layer or the intermediate adhesive layer is increased, thereby further improving the peeling performance of the adhesive tape for semiconductor manufacturing process of the present invention for chip components and further reducing adhesive residue on the chip components.
[0087] The resin film having a polar functional group is not particularly limited, but from the viewpoint of excellent heat resistance, it is preferable to include a polyester film. Examples of the polyester film include a polyethylene terephthalate (PET) film, a polyethylene naphthalate (PEN) film, a polybutylene terephthalate (PBT) film, etc. Among them, a polyethylene terephthalate (PET) film is preferable from the viewpoint of a balance between price and excellent permeability. From the viewpoint of excellent ultraviolet transmittance, the resin film having a polar functional group is preferably a (meth)acrylic resin film. Examples of the (meth)acrylic resin film include polymethyl methacrylate films. Further, examples of the resin film having the polar functional group include a polyacetal film, a polyamide film, a polycarbonate film, a polyphenylene ether film, an ultra-high molecular weight polyethylene film, a syndiotactic polystyrene film, a polyarylate film, a polysulfone film, a polyethersulfone film, a polyphenylene sulfide film, a polyetheretherketone film, a polyimide film, a polyetherimide film, a fluororesin film, and a liquid crystal polymer film.
[0088] The thickness of the barrier layer is not particularly limited, but the preferred lower limit is 0.1 μm, and the preferred upper limit is 8 μm. If the thickness of the barrier layer is within the above range, the peeling performance of the adhesive tape for semiconductor manufacturing process for chip parts is further improved. The more preferred lower limit of the thickness of the barrier layer is 3 μm, and the more preferred upper limit is 6 μm.
[0089] The barrier layer may contain additives such as plasticizers, emulsifiers, softeners, fillers, pigments, dyes, other resins, and the like, as required.
[0090] The adhesive tape for semiconductor manufacturing process of the present invention may have a second adhesive layer on the surface of the base layer opposite to the surface having the first adhesive layer. The second adhesive layer allows the adhesive tape for semiconductor manufacturing process of the present invention to be easily attached to a support such as a glass substrate, and after peeling off the chip components, the adhesive tape can be removed from the support such as a glass substrate, allowing the glass substrate to be reused.
[0091] The second pressure-sensitive adhesive layer may be the same pressure-sensitive adhesive layer as the first pressure-sensitive adhesive layer, or may be a different pressure-sensitive adhesive layer.
[0092] When the second pressure-sensitive adhesive layer is a pressure-sensitive adhesive layer different from the first pressure-sensitive adhesive layer, the second pressure-sensitive adhesive layer is not particularly limited, but is preferably a pressure-sensitive adhesive layer. Examples of the base polymer contained in the second pressure-sensitive adhesive layer include ABA block copolymers, acrylic copolymers, urethane copolymers, silicone pressure-sensitive adhesives, etc. Among these, ABA block copolymers and acrylic copolymers are preferred from the viewpoints of enabling the pressure-sensitive adhesive tape for semiconductor manufacturing processes of the present invention to be firmly attached to a support such as a glass substrate and to be removably peeled off without leaving any adhesive residue. The phase-separated structure of the second pressure-sensitive adhesive layer is not particularly limited, but from the viewpoint of easily achieving both strong adhesiveness and removability, the phase-separated structure is preferably a spherical phase-separated structure. In the above ABA block copolymer, block B is not particularly limited as long as it has a flexible structure. However, block B preferably contains a structure derived from a (meth)acrylic monomer, and more preferably contains butyl acrylate or 2-ethylhexyl acrylate.
[0093] The acrylic copolymer as the base polymer contained in the second pressure-sensitive adhesive layer is a copolymer having a structure derived from a (meth)acrylic monomer. As the (meth)acrylic monomer, butyl acrylate and 2-ethylhexyl acrylate are more preferable from the viewpoint of easily achieving both strong adhesion and removability.
[0094] From the viewpoint of removability without leaving any adhesive residue, the acrylic copolymer preferably further contains a structure derived from a monomer containing a crosslinkable functional group.
[0095] In the acrylic copolymer, the content of the structure derived from the monomer having the crosslinkable functional group is not particularly limited, but is preferably 0.1% by mass or more and 30% by mass or less. By the content of the structure derived from the monomer having the crosslinkable functional group being within the above range, it is possible to achieve both strong adhesion and removability. The more preferred lower limit of the content of the structure derived from the monomer having the crosslinkable functional group is 0.5% by mass, the even more preferred lower limit is 1% by mass, the more preferred upper limit is 25% by mass, and the even more preferred upper limit is 20% by mass.
[0096] The weight average molecular weight (Mw) of the acrylic copolymer is not particularly limited, but is preferably 200,000 or more and 2,000,000 or less. By having the weight average molecular weight in the above range, both strong adhesion and removability can be achieved. The more preferred lower limit of the weight average molecular weight is 400,000, and the more preferred upper limit is 1,500,000.
[0097] The second pressure-sensitive adhesive layer preferably further contains a crosslinking agent. The crosslinking agent is not particularly limited and is selected according to the type of crosslinkable functional group in the base polymer contained in the second pressure-sensitive adhesive layer, and examples thereof include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, metal chelate-based crosslinking agents, etc. More specifically, for example, when the crosslinkable functional group in the base polymer contained in the second pressure-sensitive adhesive layer is a carboxy group, examples of the crosslinking agent include epoxy-based crosslinking agents, isocyanate-based crosslinking agents, metal chelate-based crosslinking agents, etc. Among these, from the viewpoint of achieving both strong adhesion and removability, epoxy-based crosslinking agents and isocyanate-based crosslinking agents are preferred.
[0098] The content of the crosslinking agent is not particularly limited, and the crosslinking degree (gel fraction) of the second pressure-sensitive adhesive layer can be adjusted by adjusting the amount of crosslinkable functional groups in the base polymer contained in the second pressure-sensitive adhesive layer and the content of the crosslinking agent. The content of the crosslinking agent is preferably 0.01 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the base polymer contained in the second pressure-sensitive adhesive layer. By having the content of the crosslinking agent in the above range, both strong adhesion and removability can be achieved. The more preferred lower limit of the content of the crosslinking agent is 0.1 parts by mass, the more preferred upper limit is 8 parts by mass, the even more preferred lower limit is 0.15 parts by mass, and the even more preferred upper limit is 5 parts by mass.
[0099] The second pressure-sensitive adhesive layer may further contain a tackifier (tackifier). The tackifier is not particularly limited, but preferably has a moderate ultraviolet transmittance. The ultraviolet transmittance of the tackifier is not particularly limited, but the preferred lower limit of the ultraviolet transmittance at a wavelength of 365 nm is 1%, more preferably 50%, and even more preferably 80%. The upper limit of the ultraviolet transmittance at a wavelength of 365 nm is not particularly limited, but is substantially about 95%. From the viewpoint of high ultraviolet transmittance, a hydrogenated tackifier is preferred.
[0100] The tackifier is not particularly limited, and examples thereof include rosin ester resin, terpene phenol resin, terpene resin, coumarone resin, etc. Among them, hydrogenated rosin ester, hydrogenated terpene phenol, and hydrogenated terpene resin are preferred.
[0101] The content of the tackifier is not particularly limited, but from the viewpoint of removability, it is most preferable that the second pressure-sensitive adhesive layer does not contain a tackifier. When the tackifier is contained, the preferred upper limit is 10 parts by mass per 100 parts by mass of the base polymer contained in the second pressure-sensitive adhesive layer. When the content of the tackifier that is solid at room temperature is within the above range, adhesive residue is less likely to be left when peeled off. The more preferred upper limit of the tackifier content is 5 parts by mass, and the even more preferred upper limit is 3 parts by mass.
[0102] The second pressure-sensitive adhesive layer may further contain an inorganic filler such as fumed silica. By incorporating an inorganic filler in the second pressure-sensitive adhesive layer, the cohesive strength of the second pressure-sensitive adhesive layer is improved, making it easier to achieve both strong adhesion and removability.
[0103] The second pressure-sensitive adhesive layer may further contain known additives such as plasticizers, resins, surfactants, waxes, particulate fillers, etc. These additives may be used alone or in combination of two or more kinds.
[0104] The adhesive strength of the second adhesive layer is not particularly limited, but a preferred lower limit is 0.8 N / 25 mm. If the adhesive strength of the second adhesive layer is 0.8 N / 25 mm or more, peeling of the tape from a support such as a glass substrate can be prevented when peeling off chip components. A more preferred lower limit of the adhesive strength of the second adhesive layer is 2 N / 25 mm, an even more preferred lower limit is 3 N / 25 mm, and an even more preferred lower limit is 4 N / 25 mm. Furthermore, the upper limit of the adhesive strength of the second adhesive layer is not particularly limited, but from the viewpoint of removability, the upper limit is preferably 20 N / 25 mm, more preferably 18 N / 25 mm, and even more preferably 16 N / 25 mm. The adhesive strength of the second adhesive layer can be measured, for example, in accordance with JIS Z0237:2009, by cutting an adhesive tape to a width of 25 mm, attaching it to a glass plate at room temperature of 23°C and relative humidity of 50% at a speed of 300 mm / min using a 2 kg pressure rubber roller, leaving it to stand for 30 minutes, and then peeling the adhesive tape at a speed of 300 mm / min using an autograph (Shimadzu Corporation, "AGS-500NX") or the like to measure the 180° peel strength.
[0105] The gel fraction of the second pressure-sensitive adhesive layer is not particularly limited, but the preferred lower limit is 30% by mass and the preferred upper limit is 90% by mass. If the gel fraction of the second pressure-sensitive adhesive layer is 30% by mass or more, adhesive residue is less likely to occur when peeled off. If the gel fraction of the second pressure-sensitive adhesive layer is 90% by mass or less, the adhesive strength is easily adjusted to a high level. The more preferred lower limit of the gel fraction of the second pressure-sensitive adhesive layer is 40% by mass and the more preferred upper limit is 80% by mass. The gel fraction of the second pressure-sensitive adhesive layer can be measured by the same method as that for the gel fraction of the first pressure-sensitive adhesive layer.
[0106] The method for adjusting the adhesive strength, gel fraction, etc. of the second adhesive layer to be within the above range is not particularly limited, and examples include a method of adjusting the composition or weight average molecular weight (Mw) of the base polymer contained in the second adhesive layer, or the type or amount of the crosslinking agent, as described above.
[0107] The second adhesive layer preferably has a suitable ultraviolet transmittance. The ultraviolet transmittance is not particularly limited, but the lower limit of the ultraviolet transmittance at a wavelength of 365 nm is preferably 1%, more preferably 50%, and even more preferably 80%. The upper limit of the ultraviolet transmittance at a wavelength of 365 nm is not particularly limited, but is substantially about 95%. The UV transmittance of the second pressure-sensitive adhesive layer at a wavelength of 365 nm can be measured by measuring the UV transmittance at a wavelength of 365 nm using a method similar to that for measuring the UV transmittance at a wavelength of 355 nm of the base layer described above.
[0108] The thickness of the second adhesive layer is not particularly limited, but the preferred lower limit is 3 μm and the preferred upper limit is 30 μm. If the thickness of the second adhesive layer is 3 μm or more, it is possible to prevent the tape from peeling off from the support such as a glass substrate when peeling off the chip component. If the thickness of the second adhesive layer is 30 μm or less, it is possible to facilitate re-peeling. The more preferred lower limit of the thickness of the second adhesive layer is 5 μm, the more preferred upper limit is 20 μm, the even more preferred lower limit is 8 μm, and the even more preferred upper limit is 12 μm.
[0109] The method for producing the adhesive tape for use in the semiconductor manufacturing process of the present invention is not particularly limited. For example, the above-mentioned (meth)acrylic copolymer, an ultraviolet absorber, and other additives as necessary are added and stirred to obtain an adhesive solution, and then the adhesive solution is applied to a substrate layer and dried to obtain an adhesive tape for use in the semiconductor manufacturing process having a substrate and a first adhesive layer.
[0110] When the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process of the present invention has an intermediate pressure-sensitive adhesive layer and a barrier layer, it can be produced, for example, by the following method. That is, the adhesive solution obtained by the above-mentioned method is applied onto a base layer and dried to form an intermediate adhesive layer, and then a film to be used as a barrier layer is laminated onto the intermediate adhesive layer to obtain a laminate film. Furthermore, the adhesive solution obtained separately from the laminate film can be applied onto a release-treated surface of a release-treated PET film or the like and dried to form a first adhesive layer, which can then be laminated onto the barrier layer side of the laminate film, for example, to produce the laminate film.
[0111] When the adhesive tape for semiconductor manufacturing process of the present invention has a second adhesive layer, it can be manufactured by forming the second adhesive layer in the same manner as for the first adhesive layer, and bonding the second adhesive layer to the side opposite to the side having the first adhesive layer of the substrate of the adhesive tape for semiconductor manufacturing process prepared by the method described above.
[0112] The visible light transmittance of the pressure-sensitive adhesive tape for semiconductor manufacturing process of the present invention is not particularly limited, but from the viewpoint of peeling off chip components by laser ablation, it is preferable that the visible light transmittance has a moderate level. The lower limit of the visible light transmittance is preferably 50%, and the more preferred lower limit is 80%. The upper limit of the visible light transmittance is not particularly limited, but is practically about 95%. The haze of the adhesive tape for semiconductor manufacturing process of the present invention is not particularly limited, but from the viewpoint of peeling off chip components by laser ablation, it is preferable that the haze is small. The upper limit of the haze is preferably 10%, more preferably 5%, and even more preferably 3%. The lower limit of the haze is not particularly limited, and the smaller the haze, the more preferable, and the substantial lower limit is about 0.1%. The visible light transmittance and haze of the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process can be measured, for example, using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., "NDH4000", etc.).
[0113] The application of the adhesive tape for semiconductor manufacturing process of the present invention is not particularly limited, but it is preferably used in manufacturing a semiconductor device having a step of irradiating laser light. The adhesive tape for semiconductor manufacturing process of the present invention has excellent peeling performance for chip parts and can suppress adhesive residue on the chip parts, so it is further preferably used in manufacturing a semiconductor device having a step of peeling and transferring the chip parts arranged on the adhesive layer by laser ablation. The above chip components are not particularly limited, and examples thereof include Mini LED chips, micro LED chips, and optical chips of image sensors, with the micro LED chips being particularly preferred.
[0114] The method for transferring chip components using the adhesive tape for semiconductor manufacturing process of the present invention is not particularly limited, and examples thereof include a method for transferring chip components, which includes a step of placing chip components on the adhesive layer of the adhesive tape for semiconductor manufacturing process of the present invention, and a step of irradiating laser light to peel off the chip components. The method for manufacturing a semiconductor device using the adhesive tape for semiconductor manufacturing process of the present invention is also not particularly limited, and examples thereof include a method for manufacturing a semiconductor device, which includes the above-mentioned method for transferring chip components. According to these methods, chip components can be transferred with good yield and adhesive residue on the chip components can be suppressed. Effect of the Invention
[0115] According to the present invention, it is possible to provide an adhesive tape for use in the semiconductor manufacturing process, which has excellent peeling performance for chip components even when the chip components are thin, and is capable of transferring the chip components with high accuracy. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0116] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0117] (Preparation of Acrylic Copolymers (1) to (6) and (8) to (10)) 52 parts by mass of ethyl acetate and the monomer mixture shown in Table 1 were placed in a reactor equipped with a thermometer, a stirrer, and a cooling tube, and the inside of the reactor was replaced with nitrogen. The reactor was then placed in a water bath set at 60°C and heated to start reflux. 30 minutes after the start of reflux, 0.05 parts by mass of azobisisobutyronitrile was added as a polymerization initiator and the polymerization reaction was carried out for 5 hours. Ethyl acetate was added to the reactor to dilute the contents while cooling, thereby obtaining a solution containing acrylic copolymers (1) to (6) and (8) to (10). The weight average molecular weight of the obtained acrylic copolymers (1) to (6) and (8) to (10) was measured by the GPC method using a Waters "2690 Separations Module" as the measuring device, a Showa Denko "GPC KF-806L" as the column, ethyl acetate as the solvent, a sample flow rate of 1 mL / min, and a column temperature of 40°C.
[0118] (Preparation of ABA block copolymer (11)) 0.902 g of 1,6-hexanedithiol, 1.83 g of carbon disulfide, and 11 mL of dimethylformamide were added to a two-neck flask and stirred at 25 ° C. 2.49 g of triethylamine was added dropwise over 15 minutes and stirred at 25 ° C for 3 hours. Next, 2.75 g of methyl-α-bromophenylacetic acid was added dropwise over 15 minutes and stirred at 25 ° C for 4 hours. After that, 100 mL of extraction solvent (n-hexane: ethyl acetate = 50: 50) and 50 mL of water were added to the reaction liquid for liquid separation and extraction. The organic layers obtained in the first and second liquid separation extractions were mixed and washed with 50 mL of 1 M hydrochloric acid, 50 mL of water, and 50 mL of saturated saline in that order. Sodium sulfate was added to the organic layer after washing and dried, and then the sodium sulfate was filtered, and the filtrate was concentrated with an evaporator to remove the organic solvent. The obtained concentrate was purified by silica gel column chromatography to obtain a RAFT agent.
[0119] 87 parts by mass of styrene (St), 12 parts by mass of acrylic acid (AAc), 1 part by mass of 2-hydroxyethyl acrylate (HEA), 1.9 parts by mass of a RAFT agent, and 2,2'-azobis(2-methylbutyronitrile) (ABN-E) were placed in a two-neck flask, and the flask was heated to 85°C while replacing the atmosphere with nitrogen gas. The mixture was then stirred at 85°C for 6 hours to carry out a polymerization reaction (first stage reaction). After the reaction was completed, 4,000 parts by mass of n-hexane was added to the flask and stirred to precipitate the reaction product. The unreacted monomer and RAFT agent were then filtered off, and the reaction product was dried under reduced pressure at 70°C to obtain a copolymer (Block A).
[0120] A mixture containing 49 parts by mass of butyl acrylate (BA), 49 parts by mass of lauryl acrylate (LA), 2 parts by mass of acrylic acid (AAc), 0.058 parts by mass of ABN-E, and 50 parts by mass of ethyl acetate and the copolymer (block A) obtained above were placed in a two-neck flask, and the temperature was raised to 85° C. while replacing the atmosphere in the flask with nitrogen gas. Thereafter, the mixture was stirred at 85° C. for 6 hours to carry out a polymerization reaction (second-stage reaction), and a reaction liquid containing a block copolymer formed from blocks A and B was obtained. A portion of the reaction liquid was collected, and 4,000 parts by mass of n-hexane was added thereto and stirred to precipitate the reaction product. The unreacted monomer and the solvent were then filtered off, and the reaction product was dried under reduced pressure at 70° C. to obtain an ABA block copolymer (11). The weight average molecular weight of the resulting ABA block copolymer (11) was measured by GPC using a Waters 2690 Separations Module as a measuring instrument, a Showa Denko GPC KF-806L column, ethyl acetate as a solvent, a sample flow rate of 1 mL / min, and a column temperature of 40°C.
[0121] The alphabetic symbols in Tables 1 and 2 are as follows: BA: Butyl acrylate MA: Methyl acrylate 2-EHA: 2-Ethylhexyl acrylate 4-HBA: 4-hydroxybutyl acrylate AAc: acrylic acid U250-A: Urethane adhesive (manufactured by Lion Specialty Chemicals) St: styrene HEA: 2-hydroxyethyl acrylate LA: Lauryl acrylate The urethane compound (7) in Table 1 is U250-A used as is.
[0122] [Table 1]
[0123] [Table 2]
[0124] (Preparation of Adhesive Solutions of Adhesives A to T) The obtained base polymer was dissolved in ethyl acetate so that the solid content was 20% by mass, and each component shown in Tables 3 to 4 was added to 100 parts by mass of the base polymer, followed by thorough stirring to prepare adhesive solutions of Adhesives A to T.
[0125] [Table 3]
[0126] [Table 4]
[0127] (Adhesive tape manufacturing) (Examples 1 to 11, Comparative Examples 1 to 4) An adhesive solution of the adhesive shown in Tables 5-6 and 8 was applied to a corona-treated polyethylene terephthalate (PET) film having a thickness of 50 μm and a haze of 3.8% as a base layer using an applicator so that the dried film had a thickness shown in Tables 5-6 and 8, and dried at 110° C. for 3 minutes to form a first adhesive layer, thereby obtaining a laminated film (a). Furthermore, a release-treated 75 μm release PET film was overlaid on the laminated film (a) so that the release-treated surface faced the adhesive layer, and then cured at 40° C. for 48 hours to obtain an adhesive tape having a base layer and an adhesive layer.
[0128] (Examples 12 to 16) An adhesive solution of the adhesive shown in Table 6 was applied to a corona-treated polyethylene terephthalate (PET) film with a thickness of 50 μm and a haze of 3.8% as a base layer using an applicator so that the dried film had a thickness shown in Table 6, and then dried at 110° C. for 3 minutes to form an intermediate adhesive layer, which was used as laminate film (b). Next, a corona-treated PET film with a thickness shown in Table 6 was used as a barrier layer and superimposed on the intermediate adhesive layer side of laminate film (b) to produce laminate film (c). On the other hand, an adhesive solution of the adhesive shown in Table 6 was applied to the release-treated surface of a release-treated 75 μm PET film using an applicator so that the dried film had a thickness shown in Table 6, and then dried at 110° C. for 3 minutes to form a first adhesive layer, thereby obtaining laminated film (a). The first adhesive layer of laminated film (a) was attached to the barrier layer side of laminated film (c), and then heat-cured at 40° C. for 48 hours to obtain an adhesive tape having, in this order, the base layer, intermediate adhesive layer, barrier layer, and first adhesive layer.
[0129] (Examples 17 to 18) An adhesive solution of the adhesive shown in Table 7 was applied using an applicator to the release-treated surface of a polyethylene terephthalate film, one side of which had been release-treated, so that the dry film thickness was 10 μm, and the film was dried at 110° C. for 3 minutes to produce a laminated film (d) having a second adhesive layer on the release-treated surface of the polyethylene terephthalate film. An adhesive tape was prepared in the same manner as in Example 1, and the second adhesive layer of the prepared laminate film (d) was laminated onto the surface of the obtained adhesive tape opposite to the surface having the first adhesive layer of the substrate, thereby obtaining a double-sided adhesive tape having a substrate layer, a first adhesive layer on one side of the substrate layer, and a second adhesive layer on the surface of the substrate layer opposite the first adhesive layer.
[0130] (Measurement of maximum loss tangent (tan δ) of the first adhesive layer in the temperature range of 20°C to 40°C) The obtained first adhesive layer was stacked to prepare a 500 μm sample (width 6 mm × length 10 mm). The obtained sample was subjected to dynamic viscoelasticity measurement using a dynamic viscoelasticity measuring device (Rheometrics Dynamic Analyze RDA-700 manufactured by Rheometrics) under conditions of a nitrogen atmosphere, a measurement temperature of -40 to 150°C, a heating rate of 5°C / min, shear mode, and a frequency of 1 Hz, to obtain the maximum loss tangent (tan δ) of the adhesive layer in the temperature range of 20°C to 40°C. The results are shown in Tables 5 to 8.
[0131] (Measurement of Gel Fraction of First Pressure-Sensitive Adhesive Layer and Second Pressure-Sensitive Adhesive Layer) Only the adhesive layer W0 (g) was taken out from the laminated film (a), laminated film (b), or laminated film (d), and each was immersed in 50 mL of ethyl acetate and shaken in a shaker at 23°C and 200 rpm for 24 hours. After shaking, the ethyl acetate and the adhesive layer swollen by absorbing the ethyl acetate were separated using a metal mesh (opening #200 mesh, W1 (g)). The separated adhesive layer was dried for 1 hour under the condition of 110°C. The mass W2 (g) of the adhesive layer including the dried metal mesh was measured, and the gel fraction of the first adhesive layer and the second adhesive layer was calculated using the following formula. The results are shown in Tables 5 to 8. Gel fraction (mass%) = 100 × (W2-W1) / W0 (W0: initial adhesive layer mass, W1: initial metal mesh mass, W2: adhesive layer mass including metal mesh after drying)
[0132] (Measurement of UV absorbance at 355 nm for the first adhesive layer and the intermediate adhesive layer) The obtained first adhesive layer and intermediate adhesive layer were measured for their ultraviolet absorptance at a wavelength of 355 nm using a spectrophotometer (Shimadzu Corporation, UV-2600i) in accordance with JIS L 1925, and the ultraviolet absorptance at a wavelength of 355 nm of the first adhesive layer and the intermediate adhesive layer were measured, respectively. The results are shown in Tables 5 to 8.
[0133] (Adhesive strength loss rate of adhesive tape after UV irradiation) The obtained adhesive tape was cut into a flat rectangular shape with a width of 25 mm and a length of 75 mm, and the cut adhesive tape was attached to a glass plate using a 2 kg rubber roller and left to stand for 20 minutes under conditions of 23 ° C. and 50% RH to prepare a test piece. The obtained test piece was subjected to a 180 ° peel test at 23 ° C., 50% RH, and a tensile speed of 300 mm / min using a tensile tester (Shimadzu Corporation, "AGS-X" etc.) in accordance with JIS Z0237, to measure the 180 ° peel force (mN / 25 mm) before ultraviolet irradiation. In addition, the adhesive tape cut in the same manner was subjected to a UV irradiator using a black light (NEC Corporation, "FL20SBL") with a wavelength of 365 nm and an irradiation intensity of 7.8 mW / cm. 2The cumulative amount of ultraviolet light is 190 mJ / cm 2 After irradiating the sample so that the 180° peel strength was measured in the same manner as above, and the 180° peel strength (mN / 25 mm) after ultraviolet irradiation was measured. The adhesive strength reduction rate after ultraviolet irradiation was calculated using the following formula. The results are shown in Tables 5 to 8. Decrease in adhesive strength after UV irradiation (%) = 100 × {(180° peel strength before UV irradiation) - (180° peel strength after UV irradiation)} / (180° peel strength before UV irradiation)
[0134] <Evaluation> The pressure-sensitive adhesive tapes obtained in the Examples and Comparative Examples were evaluated by the following methods. The results are shown in Tables 5 to 8.
[0135] (Preparation of Adhesive Tape A for Evaluation) 52 parts by mass of ethyl acetate was placed in a reactor equipped with a thermometer, a stirrer, and a cooling tube, and the reactor was heated to start refluxing after replacing with nitrogen. 30 minutes after the ethyl acetate boiled, 0.08 parts by mass of azobisisobutyronitrile was added as a polymerization initiator. 47.5 parts by mass of butyl acrylate, 47.5 parts by mass of lauryl acrylate, 4.7 parts by weight of 4-hydroxybutyl acrylate, and 0.3 parts by mass of acrylic acid were added dropwise evenly and gradually over 1 hour and 30 minutes to react. 30 minutes after the end of the dropwise addition, 0.1 parts by mass of azobisisobutyronitrile was added, and the polymerization reaction was continued for another 5 hours. Ethyl acetate was added to the reactor to dilute it while cooling, and a solution of a (meth)acrylic polymer was obtained. To the obtained (meth)acrylic polymer solution, isocyanate crosslinking agent Coronate L-45 (manufactured by Tosoh Corporation) was added so that the solid content was 1.7 parts by mass per 100 parts by mass of the (meth)acrylic polymer, and the mixture was further thoroughly stirred to obtain an adhesive solution. The obtained adhesive solution was applied to a 100 μm thick corona-treated polyethylene terephthalate (PET) film as a substrate using an applicator so that the dried film thickness was 75 μm, and the film was dried at 110° C. for 3 minutes to form an adhesive layer, thereby obtaining an evaluation adhesive tape A.
[0136] (peeling performance) The adhesive tape obtained in the above "(Production of adhesive tape)" was attached to the Si chip side of the wafer on which one Si chip (500 μm × 500 μm square, 50 μm thick) was arranged. Thereafter, the wafer was peeled off to place the Si chip on the adhesive tape to obtain a measurement sample. Furthermore, the evaluation adhesive tape A was placed at 500 μm intervals from the Si chip so that the adhesive layer of the evaluation adhesive tape A faced the measurement sample. For the obtained measurement sample, a semiconductor solid-state laser was used to irradiate the Si chip with a 355 nm laser light with an output of 4 W and 4 KHz from the base layer side of the adhesive tape, and the Si chip was peeled off from the adhesive tape and transferred to the adhesive layer of the evaluation adhesive tape A. The positions of a specific side of the Si chip before transfer and the Si chip after transfer were observed with a digital microscope (manufactured by Keyence Corporation, "VHX-6000"), and the angle between the side before transfer and the side after transfer was measured. Evaluation was performed according to the following criteria. The peeling performance for chip components was evaluated as follows: when the angle was 5° or less, it was marked "◎", when the angle was greater than 5° and less than 10°, it was marked "○", when the angle was greater than 5° and less than 20°, it was marked "△", and when the angle was greater than 20°, it was marked "X". In the case of the double-sided adhesive tapes of Examples 17 to 18, in which the adhesive tape had a second adhesive layer, the second adhesive layer was bonded to a glass substrate having a thickness of 2 mm, and then the first adhesive layer of the adhesive tape to which the glass substrate was bonded was bonded to a wafer on which Si chips were arranged to prepare a measurement sample, and evaluation was performed.
[0137] (residue) In the above-mentioned "(Peeling performance)", the peeled surface of the Si chip peeled from the adhesive tape was observed with a digital microscope (Keyence Corporation, "VHX-6000") to confirm the presence or absence of residue. The residue was evaluated as "◎" when there was absolutely no residue, "◯" when the residue was less than 20% of the surface area of the chip component, and "×" when the residue was 20% or more of the surface area of the chip component.
[0138] (Peeling from glass substrate) After evaluating the peeling performance of the adhesive tapes of Examples 17 to 18 against chip components, the interface between the adhesive tape and the glass substrate was observed under a microscope (Keyence Corporation, "VHX-6000", 100x magnification) to confirm the state of peeling of the second adhesive layer from the glass substrate. After peeling the adhesive tape from the glass substrate, the case where no adhesive residue was left on the glass substrate was marked as "good", and the case where adhesive residue was found on the glass substrate was marked as "bad". The peeling from the glass substrate was evaluated as "good". Even if the evaluation is "x", the pressure-sensitive adhesive tape for use in the semiconductor manufacturing process of the present invention can be used without problems depending on the application.
[0139] [Table 5]
[0140] [Table 6]
[0141] [Table 7]
[0142] [Table 8] [Industrial Applicability]
[0143] According to the present invention, it is possible to provide an adhesive tape for use in semiconductor manufacturing processes, which has excellent peeling performance for chip components even when the chip components are thin, and is capable of transferring the chip components with high accuracy.
Claims
1. A substrate layer and a first pressure-sensitive adhesive layer are included. The first pressure-sensitive adhesive layer contains an ultraviolet absorber (UVA-1), the first pressure-sensitive adhesive layer has a maximum loss tangent (tan δ) of 0.1 or less in a temperature range of 20° C. or more and 40° C. or less; Wavelength 365nm, irradiation intensity 7.8mW / cm 2 The cumulative amount of ultraviolet light is 190 mJ / cm 2 The adhesive strength loss rate after irradiation is 60% or less.
1. An adhesive tape for use in semiconductor manufacturing processes.
2. The adhesive sheet has a base layer, an intermediate adhesive layer, and a first adhesive layer in this order, The first pressure-sensitive adhesive layer contains an ultraviolet absorber (UVA-1), the first pressure-sensitive adhesive layer has a maximum loss tangent (tan δ) of 0.1 or less in a temperature range of 20° C. or more and 40° C. or less; Wavelength 365nm, irradiation intensity 7.8mW / cm 2 The cumulative amount of ultraviolet light is 190 mJ / cm 2 The adhesive strength loss rate after irradiation is 60% or less.
1. An adhesive tape for use in semiconductor manufacturing processes.
3. 3. The adhesive tape for use in the semiconductor manufacturing process according to claim 1, wherein the base layer comprises a polyester film.
4. 3. The adhesive tape for use in semiconductor manufacturing processes according to claim 1, wherein the first adhesive layer contains a base polymer, and the base polymer contains a (meth)acrylic copolymer.
5. 5. The pressure-sensitive adhesive tape for semiconductor manufacturing processes according to claim 4, wherein the (meth)acrylic copolymer has a structure derived from a hydroxyl group-containing monomer, and the content of the structure derived from the hydroxyl group-containing monomer in the (meth)acrylic copolymer is 2 mass% or more.
6. 3. The adhesive tape for use in the semiconductor manufacturing process according to claim 1, wherein the ultraviolet absorber (UVA-1) is in a liquid state at room temperature.
7. 7. The pressure-sensitive adhesive tape for use in semiconductor manufacturing processes according to claim 6, wherein the content of the ultraviolet absorber (UVA-1) is 15 parts by mass or less per 100 parts by mass of the base polymer.
8. 3. The adhesive tape for use in semiconductor manufacturing processes according to claim 1, wherein the first adhesive layer has an ultraviolet ray absorptance of 80% or more at a wavelength of 355 nm.
9. 3. The pressure-sensitive adhesive tape for use in semiconductor manufacturing processes according to claim 1, wherein the first pressure-sensitive adhesive layer has a gel fraction of 60 mass % or more.
10. 3. The adhesive tape for use in the semiconductor manufacturing process according to claim 1, wherein the first adhesive layer has a thickness of 40 [mu]m or less.
11. 3. The adhesive tape for use in the semiconductor manufacturing process according to claim 2, wherein the intermediate adhesive layer further contains an ultraviolet absorbing agent (UVA-2).
12. 12. The adhesive tape for use in the semiconductor manufacturing process according to claim 11, wherein the ultraviolet absorber (UVA-2) is in a liquid state at room temperature.
13. The adhesive tape for semiconductor manufacturing processes according to claim 11, wherein the intermediate adhesive layer contains a base polymer, and the content of the ultraviolet absorber (UVA-2) is 15 parts by mass or less per 100 parts by mass of the base polymer.
14. 12. The adhesive tape for use in semiconductor manufacturing processes according to claim 2, wherein the intermediate adhesive layer has an ultraviolet ray absorptance of 80% or more at a wavelength of 355 nm.
15. 12. The adhesive tape for use in the semiconductor manufacturing process according to claim 2, further comprising a barrier layer between the intermediate adhesive layer and the first adhesive layer.
16. 16. The adhesive tape for use in semiconductor manufacturing processes according to claim 15, wherein the barrier layer comprises a polyester film.
17. 16. The adhesive tape for use in semiconductor manufacturing processes according to claim 15, wherein the barrier layer has a thickness of 6 μm or less.
18. 3. The adhesive tape for use in semiconductor manufacturing processes according to claim 1, further comprising a second adhesive layer on the surface of said base layer opposite to the surface having said first adhesive layer.
Citation Information
Patent Citations
Transfer method for element and arrangement method for element by using the same as well as method of manufacturing image display device
JP2003007986A
Display device manufacturing method, chip component transferring method, and transferring member
JP2019015899A
Method for manufacturing LED display
JP2019138949A
