Treatment of calcium aluminate slag and utilization method

By treating calcium aluminate slag through crushing and hydration to form a hydrate coating, the rapid setting and strength limitations are overcome, allowing its effective use as a cement admixture.

JP2024144333APending Publication Date: 2024-10-11TAIHEIYO MATERIALS CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024051101
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-27
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Calcium aluminate slag, generated as a by-product, has not been effectively utilized due to its rapid setting and insufficient strength development when used as a cement admixture, limiting its application in construction materials.

Method used

The calcium aluminate slag is treated by crushing, hydrating, and coating its surface with hydrates to control hydration reactions, ensuring a sufficient pot life and strength development when used in cement admixtures.

Benefits of technology

The treated calcium aluminate slag provides a viable cement admixture with improved pot life and strength development, enabling effective utilization of this by-product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144333000001
    Figure 2024144333000001
  • Figure 2024144333000002
    Figure 2024144333000002
  • Figure 2024144333000003
    Figure 2024144333000003
Patent Text Reader

Abstract

To provide a method for treating calcium aluminate slag so that the calcium aluminate slag generated as a by-product can be used as a cement admixture.SOLUTION: In a calcium aluminate slag treatment method, the calcium aluminate slag generated as a byproduct during metal refining is pulverized into a calcium aluminate slag powder and then subjected to a hydration treatment, wherein the surface of the powder is coated with a hydrate. Further, in a method of using calcium aluminate slag, the calcium aluminate slag powder obtained by the treatment method is used as a cement admixture.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for treating and utilizing calcium aluminate slag generated as a by-product during metal refining. [Background technology]

[0002] It is known that calcium aluminate-based slag is generated as a by-product during metal refining. For example, it is known that calcium aluminate-based slag is generated when aluminum is used as a deoxidizer for steel in the steelmaking process of stainless steel, which is a by-product of steel slag produced during the steelmaking process of stainless steel. It is also disclosed that calcium aluminate is generated as the primary slag in a manufacturing method of metal chromium, which includes a process of charging chromium oxide, aluminum, and lime (Patent Document 1). Furthermore, Patent Document 2 proposes a method for inexpensively manufacturing useful metals such as V, Ni, and Mo and calcium aluminate from used catalysts such as waste desulfurization catalysts by a simple process. Such by-product calcium aluminate is widely used in the refining process of steel companies and the like as a roasting solvent to replace fluorite, or to adjust the composition of refining slag. In addition, it has been proposed to use it as a CaO-Al2O3 raw material during the production of alumina cement (Patent Document 3). Effective use of by-product calcium aluminate is an important technology that is currently required from the standpoint of energy saving and CO2 reduction. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication WO2013 / 187348 [Patent Document 2] JP 2004-35995 A [Patent Document 3] JP 2006-282486 A Summary of the Invention [Problem to be solved by the invention]

[0004] Since calcium aluminate slag has a chemical composition close to that of alumina cement, it may be possible to use it as a substitute for alumina cement in a rapid hardening material composed of alumina cement and gypsum, but it has hardly been used so far. Therefore, the present inventors prepared a cement admixture by replacing alumina cement with a powder obtained by crushing by-product calcium aluminate, and added it to cement to carry out an investigation. However, when calcium aluminate slag is used as a cement admixture, it was found that the setting of mortar concrete becomes fast, and sufficient construction time (working time) cannot be secured even if a large amount of setting regulator is added. In addition, the strength development is not necessarily sufficient. The object of the present invention is to provide a method for treating calcium aluminate slag so that calcium aluminate slag generated as a by-product can be used as a cement admixture. [Means for solving the problem]

[0005] In order to achieve the above object, the present inventors have conducted extensive research into methods for treating calcium aluminate slag, and have found a method for using calcium aluminate slag as a cement admixture, thereby completing the present invention, which is shown in [1] to [7]. [1] A method for treating calcium aluminate slag, which is produced as a by-product during metal refining, is pulverized to obtain calcium aluminate slag powder, and then the powder is hydrated to obtain a powder whose surface is coated with a hydrate. [2] The method for treating calcium aluminate slag according to [1], wherein the calcium aluminate slag has a molar ratio of CaO to Al2O3 (CaO / Al2O3 molar ratio) of 0.9 to 1.5. [3] The method for treating calcium aluminate slag according to [1], wherein the calcium aluminate slag contains crotite and mayenite as mineral phases, and has a molar ratio of CaO to Al2O3 (CaO / Al2O3 molar ratio) of 0.9 to 1.5. [4] The method for treating calcium aluminate slag according to [3], wherein the content of the mayenite is 1 to 20 mass%. [5] The method for treating calcium aluminate slag according to [1], characterized in that the calcium aluminate slag contains crotite and mayenite as mineral phases, has a molar ratio of CaO to Al2O3 (CaO / Al2O3 molar ratio) of 0.9 to 1.5, and has a vitrification rate of less than 20%. [6] The method for treating calcium aluminate slag according to any one of [1] to [5], wherein the calcium aluminate slag has an MgO content of 5 mass% or less. [7] A method for utilizing calcium aluminate slag, comprising using the calcium aluminate slag powder obtained by the treatment method according to any one of [1] to [6] as a cement admixture. Effect of the Invention

[0006] According to the present invention, a good cement admixture can be obtained by using calcium aluminate slag, and thus the calcium aluminate slag generated as a by-product can be effectively utilized. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] <Calcium aluminate slag> The calcium aluminate slag in the present invention is calcium aluminate slag generated as a by-product during metal refining, such as calcium aluminate slag generated during the refining of nickel, molybdenum, vanadium, or alloys with iron, such as ferro-nickel and ferro-vanadium.

[0008] The main chemical components of the calcium aluminate slag are CaO and Al2O3. The contents are not particularly limited, but the CaO content is preferably 30-45 mass% and the Al2O3 content is preferably 45-65 mass%. The CaO / Al2O3 molar ratio is preferably 0.9-1.5. If the molar ratio is less than 0.9, there is a risk that the initial strength of the hardened cement body will not be fully developed. On the other hand, if the molar ratio exceeds 1.5, there is a risk that the pot life of the cement mixture will be affected.

[0009] In addition, examples of mineral phases contained in calcium aluminate slag include krotite (CaO·Al2O3), mayenite (12CaO·7Al2O3), gehlenite (2CaO·Al2O·SiO2), periclase (MgO), akermanite (2CaO·MgO·2SiO2), etc. Among these, those containing krotite as the main component (50 mass% or more) are preferred.

[0010] Furthermore, from the viewpoint of initial strength development, it is preferable to contain mayenite. Mayenite has high initial hydration activity and contributes to initial strength development. However, if it is contained in a large amount, it may accelerate the setting of mortar concrete and make it difficult to ensure the pot life. For this reason, the content is preferably 1 to 20 mass%, more preferably 2 to 10 mass%, and even more preferably 3 to 8 mass%. The content of mayenite can be measured by a calibration curve method, Rietveld method, or the like using an X-ray diffraction device.

[0011] The content of MgO in the chemical composition of calcium aluminate slag is preferably 5% by mass or less. If the content of MgO exceeds 5% by mass, the setting of mortar concrete may be delayed, and the short-term strength development may decrease. It is more preferable that the content is 4% by mass or less, and even more preferable that the content is 3% by mass or less. In addition, the content of TiO2 is preferably 1% by mass or less from the viewpoint of strength development.

[0012] In addition, calcium aluminate slag may contain small amounts of metals and metal oxides, such as iron, nickel, molybdenum, vanadium, chromium, cobalt, etc. The content of metals and metal oxides is preferably 5 mass% or less in terms of metal oxide.

[0013] The ignition loss of calcium aluminate slag usually increases (indicated by +). Here, ignition loss refers to the weight loss when heated in air at 950°C for one hour. The increase in ignition loss is believed to be due to the transition metals contained in the slag remaining in the metallic state or in the form of a compound with a low valence.

[0014] In addition, calcium aluminate slag is usually left to cool naturally, so the product is crystalline and contains almost no amorphous calcium aluminate. The vitrification rate of calcium aluminate slag is not particularly limited, but is usually less than 20%. The vitrification rate can be measured by the calibration curve method using an X-ray diffraction device or the Rietveld method.

[0015] <Method of treating calcium aluminate slag> Calcium aluminate slag, which is generated as a by-product, is usually obtained in the form of lumps of about several cm. Therefore, it is pulverized to obtain a powder. The pulverization method is not particularly limited, but for example, it can be roughly crushed with a crusher mill or the like, and then finely pulverized with a ball mill, a vibration mill, or the like. The degree of powderiness is 3000 to 8000 cm in terms of Blaine specific surface area. 2 / g. More preferably, it is adjusted to 4000 to 7000 cm. 2 / g.

[0016] Next, the powder of the pulverized calcium aluminate slag is subjected to a hydration treatment. As a result, a coating layer of calcium aluminate hydrate is formed on the surface of the powder particles, which suppresses the hydration reaction when the powder particles come into contact with water, and even when the powder is used in mortar or concrete, sufficient pot life can be ensured. Alternatively, good fluidity can be ensured. As a method of hydration treatment, for example, a powder mixer is used to spray and add a predetermined amount of water little by little with a sprayer, and mixing the water is preferable because the hydrate phase can be relatively uniformly coated. As the powder mixer, a Lödige mixer, a Henschel mixer, a Nauter mixer, a VH powder mixer, etc. can be used. The mixing time is appropriately adjusted depending on the amount of mixture and the device, but is preferably 2 to 30 minutes. The amount of water to be sprayed is preferably 0.2 to 3.5 mass% based on the weight of the calcium aluminate slag. Instead of the water to be sprayed, other liquids (water-containing organic solvents, carbonated water, etc.) can be used as long as they react with calcium aluminate to form hydrates.

[0017] Hydrates formed on the surface of calcium aluminate slag powder particles include, for example, CaO·Al2O3·10H2O, 2CaO·Al2O3·8H2O, 3CaO·Al2O3·6H2O, 3CaO·Al2O3·8H2O, 4CaO·Al2O3·13H2O, 4CaO·Al2O3·19H2O, CaO·H2O, Al2O3·H2O, Al2O3·3H2O, 3CaO·Al2O3·CaSO4·12H2O, 3CaO·Al2O3·3CaSO4·32H2O, 3CaO·Al2O3·CaCO3·12H2O, 3CaO·Al2O3·3CaCO3·30H2O, etc. Hydrates containing transition metals and other impurity elements contained in calcium aluminate slag are also included.

[0018] <Cement admixture> The calcium aluminate slag treated by the manufacturing method of the present invention can be suitably used as a cement admixture, that is, when this cement admixture is added to cement, it can ensure sufficient pot life and good fluidity, and can also provide good strength development.

[0019] The cement admixture preferably contains gypsum in addition to the calcium aluminate slag. Examples of gypsum include anhydrous gypsum, dihydrate gypsum, and hemihydrate gypsum. Anhydrous gypsum is preferable from the viewpoint of strength development. In addition, both natural gypsum and chemical gypsum generated as a by-product can be used. The Blaine specific surface area of ​​gypsum is 3000 to 12000 cm. 2 / g is preferred, and 4000 to 10000 cm 2 The content of the gypsum is preferably from 20 to 400 parts by mass, more preferably from 30 to 300 parts by mass, and further preferably from 40 to 200 parts by mass, relative to 100 parts by mass of the calcium aluminate slag.

[0020] The cement admixture may further contain one or more metal salts selected from the group consisting of sulfates, nitrates, nitrites, carbonates and hydroxides of alkali metals or alkaline earth metals, or aluminum sulfates. The content of these metal salts is preferably 1 to 20 parts by mass, more preferably 2 to 10 parts by mass, per 100 parts by mass of calcium aluminate slag.

[0021] The cement admixture may further contain one or more retarders selected from organic acids or their salts. Examples of organic acids include citric acid, gluconic acid, malic acid, tartaric acid, etc., and examples of their salts include sodium citrate, potassium citrate, sodium gluconate, Rochelle salt, etc. From the viewpoint of the retarding effect on calcium aluminate-based materials (calcium aluminate slag) and compatibility with strength development, oxycarboxylic acids such as citric acid and tartaric acid, or alkali metal salts thereof, are particularly preferred. The amount of retarder to be added is preferably 0.5 to 5 mass % in the cement admixture, more preferably 1 to 3 mass %.

[0022] It is possible to use industrially produced alumina cement or amorphous calcium aluminate to replace part of the calcium aluminate slag. However, from the viewpoint of effective utilization of the calcium aluminate slag, it is desirable to keep the amount as small as possible.

[0023] The above cement admixture is used by adding it to various cements such as Portland cement. The amount of the cement admixture added is appropriately adjusted depending on the application, but is preferably 5 to 50 parts by mass, more preferably 10 to 40 parts by mass, per 100 parts by mass of the total of the cement and the cement admixture.

[0024] In addition, a setting retarder can be used in the mortar or concrete using the above cement admixture to adjust the pot life. Examples of setting retarders include organic acids or their salts such as citric acid, gluconic acid, malic acid, and tartaric acid, boric acid, borates such as sodium borate, phosphates, and sugars. The amount of setting retarder added is appropriately adjusted within the range of 0.1 to 5.0 parts by mass per 100 parts by mass of the total of cement and cement admixture. Furthermore, in order to adjust the fluidity, cement dispersants such as water reducing agents, AE water reducing agents, high performance water reducing agents, high performance AE water reducing agents, and fluidizing agents used in general mortar and concrete can be used. EXAMPLES

[0025] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples.

[0026] Example 1 Calcium aluminate slag (CAS) generated during metal refining was used as slag produced after refining ferrovanadium. The chemical composition of calcium aluminate slag is shown in Table 1. This calcium aluminate slag contained 0.66 mass% vanadium in oxide equivalent. The CaO / Al2O3 molar ratio was 1.1, and the ignition loss was +0.25 mass% (increase). The mineral composition contained 80 mass% krotite, 5 mass% mayenite, 10 mass% gehlenite, and 2 mass% periclase. The vitrification rate was 2%. The mineral content and vitrification rate were calculated by the Rietveld method using an X-ray diffractometer. This calcium aluminate slag was coarsely crushed and then pulverized in a ball mill to obtain a slag with a Blaine specific surface area of ​​50-20 cm. 2 / g powder.

[0027] [Table 1]

[0028] For 100 parts by mass of calcium aluminate slag powder that had been subjected to hydration treatment, anhydrous gypsum (commercial product; Blaine specific surface area 7100 cm) was added. 2 The cement admixture (AD1) was obtained by mixing 100 parts by mass of sodium sulfate (reagent, manufactured by Kanto Chemical Co., Ltd.), 6 parts by mass of sodium sulfate (reagent, manufactured by Kanto Chemical Co., Ltd.), and 6 parts by mass of lithium carbonate (reagent, manufactured by Kanto Chemical Co., Ltd.) for 10 minutes in a powder mixer. Mortar specimens were prepared using this cement admixture. The cement (C) was ordinary Portland cement (manufactured by Taiheiyo Cement Co., Ltd., density: 3.16 g / cm 3 ), JIS standard sand was used as the aggregate (S), and tap water was used as the water (W). The content of the cement admixture was 30 parts by mass per 100 parts by mass of the cement and cement admixture combined. In addition, citric acid (commercially available first-class reagent) was added as a setting retarder at 0.6% by mass relative to the total amount of the cement and cement admixture. The mortar mix is ​​shown in Table 2. The preparation and curing of mortar specimens were carried out in a 20°C environment.

[0029] [Table 2]

[0030] (Test Method) (1) Pot life In accordance with JIS A 1147 "Test method for setting time of concrete," the initial setting time was measured and used as the pot life. (2) Compressive strength The compressive strength of each age was measured in accordance with the Japan Society of Civil Engineers standard JSCE-G541 "Test method for compressive strength of filling mortar."

[0031] (Test Results) When using a cement admixture made from calcium aluminate slag that had not been hydrated, the pot life could not be secured for more than 20 minutes, but when using a cement admixture made from calcium aluminate slag powder that had been hydrated, the pot life could be secured for 80 minutes. In addition, the strength of the cement admixture was 32 N / mm at 4 hours of age. 2 , 44N / mm at 24 hours 2 The compressive strength was also good at an early stage of strength development.

[0032] Example 2 A cement admixture for promoting carbonation was prepared and evaluated using the calcium aluminate slag powder prepared in the same manner as in Example 1. The details are described below.

[0033] 70 parts by mass of calcium aluminate slag powder and anhydrous gypsum (commercially available, Blaine specific surface area 7100 cm 2 The cement (C) was mixed with 30 parts by mass of ordinary Portland cement (manufactured by Taiheiyo Cement Corporation, density: 3.16 g / cm3) to prepare a cement admixture (AD2). Mortar specimens were prepared using this cement admixture. 3 ), JIS standard sand was used as the aggregate (S), and tap water was used as the water (W). The content of the cement admixture was 20 parts by mass per 100 parts by mass of the total of the cement and cement admixture. The mortar mix is ​​shown in Table 3. The mortar was mixed for 3 minutes using a mortar mixer and then subjected to various tests.

[0034] [Table 3]

[0035] (Test Method) (1) Mortar flow The test was conducted in accordance with "JIS R 5201 Physical Testing of Mortar." (2) Compressive strength test In accordance with "JIS R 5201 Physical Tests of Mortar," compressive strength was tested at ages of 1 and 14 days. The curing temperature was 20°C until immediately before the test. (3) Carbonation depth The test was conducted in accordance with "JIS A 1152 Measurement method for carbonation depth of concrete." The pieces were sealed and cured for up to three days, after which they were demolded and tested in a neutralization tank at a temperature of 20°C, humidity of 60%, and CO2 concentration of 5%, for a material age of 28 days.

[0036] (Test Results) The test results are shown in Table 4. The compressive strength ratio in the table (at 14 days) indicates the strength ratio relative to the compressive strength of mortar without added cement admixture. It can be seen that when a cement admixture made from hydrated calcium aluminate slag is used, both the fluidity and strength development are better than those without added water. It can also be seen that the carbonation rate is faster than those without added cement admixture.

[0037] [Table 4]

[0038] Example 3 The test was carried out using four types of calcium aluminate slag with different chemical compositions. The chemical compositions of the calcium aluminate slags used are shown in Table 5. All calcium aluminate slags contained krotite as the main component and 1 to 8 mass% mayenite. The vitrification rate was 3% or less.

[0039] [Table 5]

[0040] These calcium aluminate slags were coarsely crushed and then pulverized in a ball mill to obtain a powder with a Blaine specific surface area of ​​5000±100cm. 2 The calcium aluminate slag powder was adjusted to have a concentration of 1 / g. 50 kg of the prepared calcium aluminate slag powder was charged into a Lödige mixer, and 250 g of water was added by spraying with a sprayer while rotating the mixer. The mixture was mixed for 10 minutes to obtain a calcium aluminate slag powder that had been treated with water.

[0041] Powder of hydrated calcium aluminate slag, anhydrous gypsum (commercial product, Blaine specific surface area 7000 cm 2 / g), anhydrous sodium sulfate (reagent grade 1, commercially available product), and citric acid (reagent grade 1, commercially available product) were mixed to prepare a cement admixture. The composition of each cement admixture is shown in Table 6.

[0042] [Table 6]

[0043] 450g of cement composition consisting of cement admixtures shown in Table 6 and blast furnace cement type B (manufactured by Taiheiyo Cement Corporation) was mixed with 1350g of fine aggregate (JIS standard sand) and 225g of water (tap water) to prepare mortar. The mixture was mixed for 3 minutes using a mortar mixer. This mortar was placed in a formwork to prepare a specimen for evaluation testing. The test method for the evaluation testing is shown below.

[0044] (Test Method) (1) Pot life The central temperature of a φ5 × 10 cm test specimen was measured, and the pot life was determined as the time from when the mixture was mixed until the temperature rose by 1°C. (2) Compressive strength test The compressive strength of each age was tested according to the Soil Science Society standard JSCE-G541 "Test method for compressive strength of filling mortar." The curing temperature was 20℃ until just before the test.

[0045] (Test Results) The test results are shown in Table 7. The cement composition of the present invention can be set to have a pot life of 30 minutes or more, and exhibited good early strength development in 24 hours. In addition, the compressive strength at 14 days was also good.

[0046] [Table 7]

Claims

1. A method for treating calcium aluminate slag, comprising crushing calcium aluminate slag generated as a by-product during metal refining to obtain calcium aluminate slag powder, and then adding water to obtain a powder whose surface is coated with a hydrate.

2. The calcium aluminate slag is composed of CaO and Al 2 O 3 The molar ratio of CaO / Al 2 O 3 2. The method for treating calcium aluminate slag according to claim 1, characterized in that the molar ratio of calcium aluminate slag to calcium aluminate slag is 0.9 to 1.

5.

3. The calcium aluminate slag contains krotite and mayenite as mineral phases, and contains CaO and Al 2 O 3 The molar ratio of CaO / Al 2 O 3 2. The method for treating calcium aluminate slag according to claim 1, characterized in that the molar ratio of calcium aluminate slag to calcium aluminate slag is 0.9 to 1.

5.

4. The method for treating calcium aluminate slag according to claim 3, wherein the content of the mayenite is 1 to 20 mass%.

5. The calcium aluminate slag contains krotite and mayenite as mineral phases, and contains CaO and Al 2 O 3 The molar ratio of CaO / Al 2 O 3 2. The method for treating calcium aluminate slag according to claim 1, characterized in that the vitrification rate of the slag is less than 20% and the molar ratio of the slag is 0.9 to 1.

5.

6. 2. The method for treating calcium aluminate slag according to claim 1, characterized in that the calcium aluminate slag has an MgO content of 5 mass% or less.

7. A method for utilizing calcium aluminate slag, comprising using the calcium aluminate slag powder obtained by the method according to any one of claims 1 to 6 as a cement admixture.

Citation Information

Patent Citations

  • Method for manufacturing ferroalloy from spent catalyst

    JP2004035995A

  • Alumina cement, alumina cement composition, and monolithic refractory

    JP2006282486A

  • Metal chrome fabrication method

    WO2013187348A1