Sealant composition for self-sealing pneumatic tire
A sealant composition for tires, combining isobutylene and conjugated diene-based elastomers with fillers and peroxide, addresses flow issues and temperature variability, ensuring effective and balanced tire sealing.
Patent Information
- Application Number
- JP2024051551
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-11
AI Technical Summary
Existing sealant compositions for pneumatic tires often result in tire imbalance and cleaning difficulties due to excessive flow after puncture, and they are ineffective over a wide temperature range.
A sealant composition comprising 100 phr of an elastomer blend with at least 60 phr of an isobutylene-based elastomer and 5 phr of a conjugated diene-based elastomer, along with particulate fillers and organic peroxide, which minimizes flow by partial depolymerization during tire curing.
The composition effectively seals punctures while maintaining tire balance and pressure over extended periods, even in varying temperatures, with minimal excess sealant flow.
Smart Images

Figure 2024144344000001_ABST
Abstract
Description
[Technical field]
[0001] FIELD OF THEINVENTION Aspects of the present invention relate to sealant compositions adapted for use in sealing punctures in pneumatic tires, tires incorporating the compositions, and methods of manufacture. [Background technology]
[0002]
[0002] Puncture sealing tires are designed to slow or prevent the loss of air and resulting deflation after a tire has been punctured by a sharp object, such as a nail, screw, or another object capable of penetrating the tire.
[0003]
[0003] A sealant composition ("sealant") is typically contained or encapsulated between layers of a tire. For example, the sealant may be disposed in separate cells or sheets such that a puncturing object penetrating the tread portion of the tire passes through enough sealant to seal the tire against the escape of expanding air through the puncture.
[0004]
[0004] Pneumatic tires with puncture sealing capabilities first utilized an unvulcanized layer of rubber as a sealant (see, for example, U.S. Pat. Nos. 1,419,470A, 1,601,013A, and 1,977,281A). Later, sealant compositions were developed to provide longer life to tires after a puncture, allowing the tire to continue to be used until the tire can be driven to a more convenient location for repair or replacement. For example, U.S. Pat. No. 3,048,509A describes an unvulcanized synthetic rubber sealing composition containing 1,3-butadiene-styrene copolymer, softeners, and tackifiers in the form of sheets separated by covering sheets composed primarily of vulcanized rubber compounds.
[0005] Butyl rubber, i.e., copolymers of isobutylene and isoprene, have also been used in sealant compositions, see, for example, U.S. Patent No. 4,228,839A, U.S. Patent No. 4,171,237A, U.S. Patent No. 4,140,167A, and U.S. Patent No. 4,426,468A and U.S. Publication No. 2005 / 0034799A1.
[0006]
[0006] Sealant compositions incorporating dispersed particulate precured rubber materials have also been used as described in U.S. Pat. No. 6,837,287 B2. Inorganic particulate materials have also been used in sealant compositions. U.S. Pat. No. 9,427,918 B2 describes a sealant composition comprising raw rubber, polybutene, treated silica, and peroxide. The raw rubber in the sealant composition can be natural rubber, butyl rubber, or a blend of natural and butyl rubber. U.S. Pat. No. 9,802,446 B2 discloses a sealant comprising expandable graphene structures and microspheres.
[0007]
[0007] Other sealant compositions and tires containing them are disclosed in U.S. Patent No. 4,089,360A, U.S. Patent No. 4,140,167A, U.S. Patent No. 4,228,839A, U.S. Patent No. 4,426,468A, U.S. Patent No. 7,674,344 B2, U.S. Patent No. 8,221,849 B2, U.S. Patent No. 8,360,122 B2, U.S. Patent No. 9,677,025 B2, U.S. Patent No. 10,730,255 B2, and U.S. Publication Nos. 20080115872 A1, 20220097326 A1, 20220111609 A1, and 20220410516 A1.
[0008]
[0008] One weakness with many existing sealant compositions is that when a tire is punctured, the sealant composition continues to flow past the puncture hole. This can cause the tire to lose balance and present cleaning problems. In other cases, the sealant coating is not operable or effective over a wide temperature range from hot summer to cold winter environments. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] U.S. Patent No. 1,419,470A [Patent Document 2] U.S. Patent No. 1,601,013A [Patent Document 3] U.S. Patent No. 1,977,281A [Patent Document 4] U.S. Patent No. 3,048,509A [Patent Document 5] U.S. Patent No. 4,228,839A [Patent Document 6] U.S. Patent No. 4,171,237A [Patent Document 7] U.S. Patent No. 4,140,167A [Patent Document 8] U.S. Patent No. 4,426,468A [Patent Document 9] US Publication No. 2005 / 0034799A1 [Patent Document 10] U.S. Patent No. 6,837,287B2 [Patent Document 11] U.S. Patent No. 9,427,918B2 [Patent Document 12] U.S. Patent No. 9,802,446B2 [Patent Document 13] U.S. Patent No. 4,089,360A [Patent Document 14] U.S. Patent No. 7,674,344B2 [Patent Document 15] U.S. Patent No. 8,221,849B2 [Patent Document 16] U.S. Patent No. 8,360,122B2 [Patent Document 17] U.S. Patent No. 9,677,025B2 [Patent Document 18] U.S. Patent No. 10,730,255B2 [Patent Document 19] US Publication No. 20080115872A1 [Patent Document 20] US Publication No. 20220097326A1 [Patent Document 21] US Publication No. 20220111609A1 [Patent Document 22] US Publication No. 20220410516A1 [Patent Document 23] U.S. Patent No. 5,587,416A [Patent Document 24] U.S. Patent No. 5,800,608A [Patent Document 25] U.S. Patent No. 5,882,617A [Patent Document 26] U.S. Patent No. 6,107,226A [Patent Document 27] U.S. Patent No. 6,180,076B1 [Patent Document 28] U.S. Patent No. 6,221,149B1 [Patent Document 29] U.S. Patent No. 6,268,424B1 [Patent Document 30] U.S. Patent No. 6,335,396B1 [Patent Document 31] U.S. Patent No. 7,585,481B2 [Patent Document 32] U.S. Patent No. 9,334,169B2 [Patent Document 33] U.S. Patent No. 9,359,215B2 [Patent Document 34] US Publication No. 20020081247A1 [Patent Document 35] US Publication No. 20030118500A1 [Patent Document 36] US Publication No. 20040062701A1 [Patent Document 37] US Publication No. 20050032965A1 [Patent Document 38] EP0647591A1 issue [Patent Document 39] U.S. Patent No. 5,708,069A [Patent Document 40] U.S. Patent No. 7,550,610B1 [Patent Document 41] U.S. Patent No. 5,789,514A [Patent Document 42] U.S. Patent No. 7,071,258B1 [Patent Document 43] U.S. Patent No. 6,322,811B1 [Patent Document 44] U.S. Patent No. 4,082,703A [Non-patent literature]
[0010] [Non-Patent Document 1] Brunauer, Emmett and Teller, Journal of the American Chemical Society, vol. 60, p. 309 (1938) [Non-Patent Document 2] "Standard Methods for Analysis & Testing of Petroleum and Related Products" and "British Standard 2000 Parts", 2003, 62nd Edition, Institute of Petroleum, United Kingdom Summary of the Invention [Problem to be solved by the invention]
[0011]
[0009] A need remains for a sealant composition that is capable of self-sealing a puncture in a tire that would otherwise result in loss of air and eventual contraction of the tire, while also reducing excess flow of the sealant composition in the event of a puncture. [Means for solving the problem]
[0012] According to one aspect of the exemplary embodiment, the sealant composition includes 100 phr of an elastomer including at least 60 phr of an isobutylene-based elastomer component and at least 5 phr of a conjugated diene-based elastomer component. The sealant composition further includes at least 5 phr of a particulate filler and at least 0.5 phr of an organic peroxide.
[0013]
[0011] The sealant composition may include a colorant to provide a non-black color to the sealant. The colorant may be selected from yellow pigments, yellow dyes, and mixtures thereof. The isobutylene-based elastomer component of the sealant composition may be selected from the group consisting of butyl rubber, polyisobutylene, and mixtures thereof. The isobutylene-based elastomer component may be at least 80% by weight butyl rubber. The isobutylene-based elastomer component may have a weight average molecular weight of at least 5,000, or at least 30,000 and / or up to 800,000. The sealant composition may include at least 75 phr of isobutylene-based elastomer.
[0014] The conjugated diene-based elastomer component of the sealant composition may be selected from the group consisting of natural rubber, synthetic polyisoprene, polybutadiene, styrene-butadiene copolymers, and mixtures and copolymers thereof. The conjugated diene-based elastomer component may be at least 80% by weight natural rubber. The sealant composition may include at least 8 phr of the conjugated diene-based elastomer component.
[0015] The sealant composition may include up to 40 phr of particulate filler. The particulate filler may include at least one of silica, titanium dioxide, calcium carbonate, and carbon black. The sealant composition may include at least 5 phr of silica. The sealant composition may contain up to 1 phr total of black reinforcing fillers selected from carbon black, graphite, graphene, and mixtures thereof.
[0016]
[0015] The organic peroxide in the sealant composition may be selected from dicumyl peroxide; 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane; 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane; 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3; p-chlorobenzyl peroxide; 2,4-dichlorobenzyl peroxide; 2,2-bis-(tert-butylperoxy)-butane; tert-butylcumyl peroxide; di-tert-butyl peroxide; benzoyl peroxide; 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane; 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane; and mixtures thereof.
[0017] The sealant composition may further comprise at least 0.1 phr of a polyalkylene glycol.
[0017] In accordance with another aspect of an exemplary embodiment, an uncured pneumatic tire includes a circumferential tread, a supporting carcass bonded to the tread, a sealant layer including the sealant composition described above, and a containment layer, the sealant layer being disposed between the supporting carcass and the containment layer.
[0018]
[0018] The containment layer of the uncured pneumatic tire may include a halobutyl rubber.
[0019] A cured pneumatic tire may be formed by curing the uncured pneumatic tire described above at a temperature sufficient for the organic peroxide to at least partially depolymerize the isobutylene-based elastomer component.
[0019]
[0020] According to another aspect of the exemplary embodiment, a method of forming a sealant layer includes forming a sealant composition including 100 phr of an elastomer, a particulate filler, a colorant, and an organic peroxide, the elastomer including at least 60 phr of an isobutylene-based elastomer component and at least 5 phr of a conjugated diene-based elastomer component. The method further includes treating the sealant composition to a sufficient temperature and for a sufficient time to at least partially decompose the isobutylene-based elastomer component to form a sealant layer.
[0020]
[0021] The method may further include forming an uncured tire including a layer of the sealant composition prior to applying the sealant composition.
[0022] In accordance with another aspect of the exemplary embodiment, a method of manufacturing a pneumatic rubber tire having puncture sealing characteristics includes constructing an unvulcanized tire including a circumferential rubber tread, a supporting carcass, a containment layer, and a sealant layer disposed intermediate the supporting carcass and the containment layer. The sealant layer includes a sealant composition, the sealant composition including 100 phr of an elastomer. The elastomer includes at least 60 phr of an isobutylene-based elastomer component and at least 5 phr of a conjugated diene-based elastomer component. The sealant composition further includes a particulate filler and an organic peroxide. The method further includes curing the unvulcanized tire at a temperature sufficient to at least partially depolymerize the isobutylene-based elastomer component to produce a pneumatic rubber tire having puncture sealing characteristics. [Brief description of the drawings]
[0021] [Figure 1]
[0023] 1 is a cross-sectional view of a tire having a sealant layer disposed between an innerliner and a carcass of the tire according to one aspect of an exemplary embodiment; [Diagram 2]
[0024] FIG. 2 is a cross-sectional view of a tire having a sealant layer disposed between first and second innerliner layers according to another aspect of the exemplary embodiment. [Diagram 3]
[0025] 2 is a cross-sectional view of a tire having a sealant layer disposed between a containment layer and a carcass of the tire according to another aspect of the exemplary embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022]
[0026] Described herein is a sealant composition (or "sealant") adapted for use in pneumatic tire enclosures. The sealant serves to seal punctures in tires by flowing to fill voids while minimizing flow of excess sealant from the enclosure and maintaining sealing performance over time.
[0023]
[0027] In the present specification, the term "phr" refers to parts by weight of a respective material per 100 parts by weight of rubber or elastomer. The term "phf" refers to parts by weight per 100 parts by weight of filler. By convention, the unreacted rubber utilized in the sealant composition (i.e., excluding any precured rubber particles used as a filler) totals 100 phr.
[0024]
[0028] The terms "rubber" and "elastomer" may be used interchangeably unless otherwise noted.
[0029] As used herein, Mooney viscosity is measured at 125° C. according to ASTM D1646-19a, "Standard Test Methods for Rubber-Viscosity, Stress Relaxation, and Pre-Vulcanization Characteristics (Mooney Viscometer)."
[0025]
[0030] The glass transition temperature (Tg) of an elastomer or elastomeric composition referred to herein represents the glass transition temperature(s) of the respective elastomer or elastomeric composition in its unreacted state or, in the case of elastomeric compositions, possibly in its reacted state. The Tg values referred to herein are those determined as the peak midpoint by differential scanning calorimetry (DSC) at a temperature rate of increase of 10° C. per minute, in accordance with ASTM D3418-21, "Standard Test Method for Transition Temperatures and Enthalpies of Fusion and Crystallization of Polymers by Differential Scanning Calorimetry."
[0026]
[0031] Described below are sealant compositions, methods of preparation, and exemplary tires incorporating the sealant compositions. Sealant Composition
[0032] An exemplary sealant composition is formed by curing a mixture including an isobutylene-based elastomer having a low level of unsaturation, a conjugated diene-based elastomer having a high level of unsaturation, and a peroxide, such as an organic peroxide that generates free radicals. The butylene-based elastomer of the sealant composition can be partially depolymerized in situ in the tire by an organic peroxide that generates free radicals. The sealant can incorporate one or more particulate filler materials, such as silica and clay. One or more colorants can be present in the sealant composition to contrast with the black color of the tire as an aid in identifying tire punctures. Processing oils and / or polyalkylene oxide polymers, such as polyethylene glycol, can also be present in the sealant composition. As will be appreciated, the sealant composition is not limited to these components.
[0027]
[0033] The sealant composition is used to provide an inlaid sealant layer (or two or more layers) for a pneumatic tire. Each sealant layer is obtained by (partial) depolymerization of the butylene units of the butylene-based elastomer in the sealant composition. The sealant layer(s) can be located inside the tread of the tire, depending on the location of the inlaid sealant layer. The sealant layer can be inlaid in the tire to form a tire assembly in a suitable mold or on the core. The butylene units of the butylene-based elastomer of the sealant composition can be depolymerized during the subsequent curing of the tire at high temperature, resulting in the formation of a tire inlaid with a sealant layer.
[0028]
[0034] Although not fully understood, it is hypothesized that the conjugated diene-based elastomer component forms a matrix within the reacted sealant that binds the lower molecular weight butyl chains obtained by depolymerization of the isobutylene-based elastomer component. This creates a reacted sealant layer within the tire that, in the event of a puncture, can flow only to a limited extent (noticeably enough), while allowing pressure within the tire to be maintained at drivable levels for extended periods of time, such as days or weeks.
[0029] 1. Elastomer
[0035] An exemplary sealant composition includes two elastomer components, an isobutylene-based elastomer component and a conjugated diene-based elastomer component, which together may comprise at least 80 phr, or at least 90 phr, or at least 95 phr, or 100 phr of the sealant composition.
[0030] A. Isobutylene-based elastomer component
[0036] The isobutylene-based elastomer component may be at least 60 phr, at least 70 phr, at least 75 phr, or at least 80 phr, and / or up to 95 phr, up to 92 phr, or up to 90 phr in the sealant composition. The isobutylene-based elastomer component comprises one or more elastomers derived from isobutylene. For example, the isobutylene-based elastomer component may be selected from butyl rubber, polyisobutylene, and mixtures thereof. In one embodiment, the isobutylene-based elastomer is at least 80 wt%, or at least 90 wt%, or at least 95 wt%, or 100 wt% butyl rubber.
[0031]
[0037] Butyl rubber is a copolymer of isobutylene and a conjugated diene, particularly isoprene. In one embodiment, the isobutylene derived units make up the majority of the units in the copolymer, while the isoprene derived units make up a minority of the units. For example, the ratio of isobutylene derived units to isoprene derived units may be at least 90:10, or at least 95:5, or at least 98:2, or at least 98.5:1.5, or at least 99:1, or up to 99.5:0.5. The use of butyl rubber with a low unsaturation content (e.g., a ratio of isobutylene derived units to isoprene derived units up to 2) promotes more efficient depolymerization by organic peroxides. The presence of double bonds in butyl rubber tends to terminate the depolymerization process when it reaches the unsaturation of the double bonds in the butyl rubber, allowing partial, incomplete depolymerization to occur. When butyl rubber is at least partially depolymerized by organic peroxides present in the sealant composition, the by-product of such depolymerization is isobutylene.
[0032]
[0038] The butyl rubber may have a weight average molecular weight Mw of at least 30,000, or at least 40,000, such as up to 800,000, or up to 600,000, or up to 400,000. The butyl rubber has a relatively high Mooney viscosity at 125° C., for example in the range of 25 to 60, or at least 40, or up to 60.
[0033]
[0039] Exemplary butyl rubbers include those sold by ExxonMobil Company under the trademark Exxon068™, which is a copolymer of isobutylene and isoprene having less than 1% units derived from isoprene and having a Mooney viscosity of about 51 at 125° C.
[0034]
[0040] Polyisobutylene (PIB) is a homopolymer of isobutylene, i.e., a homopolymer of isobutylene formed without an unsaturated monomer such as isoprene. Polyisobutylene suitable for use in the isobutylene-based elastomer component may have a weight average molecular weight Mw of at least 5,000, or at least 10,000, or at least 30,000, or at least 40,000, or at least 50,000, such as up to 800,000, or up to 600,000, or up to 400,000, or up to 150,000. Additionally, the polyisobutylene may have a polydispersity (Mw / Mn) in the range of 1.6 to 4.0, and a glass transition temperature in the range of -55°C to -70°C, such as in the range of -62°C to -66°C, or in the range of -63°C to -65°C. The polyisobutylene elastomer may be optionally stabilized with small amounts of antioxidants, for example, from 100 ppm to 1,000 ppm of antioxidant, or from 300 ppm to about 700 ppm of antioxidant. A variety of antioxidants are available, for example, butylated hydroxytoluene (BHT).
[0035]
[0041] Examples of polyisobutylenes suitable for use are available from BASF as Oppanol® B10, Oppanol® B12, and Oppanol® B15. Oppanol® B10 has a weight average molecular weight Mw of 53,000, a viscosity average molecular weight Mv of 40,000, and a glass transition temperature (Tg) of -64°C. Oppanol® B12 has a weight average molecular weight of 70,000, a viscosity average molecular weight of 55,000, and a glass transition temperature (Tg) of -64°C. And Oppanol® B15 has a weight average molecular weight of 108,000, a viscosity average molecular weight of 85,000, and a glass transition temperature (Tg) of -64°C.
[0036]
[0042] In one embodiment, the sealant composition is free or substantially free (less than 1 phr) of polybutene, especially low molecular weight polybutene (Mw less than 8,000). Polybutene is a polymer formed from a mixture of 1-butene, 2-butene, and isobutylene.
[0037] B. Conjugated diene-based elastomer components
[0043] The conjugated diene-based elastomer component may be at least 5 phr, at least 6 phr, or at least 8 phr, and / or up to 40 phr, up to 25 phr, up to 20 phr, or up to 15 phr in the sealant composition. The conjugated diene-based elastomer component consists of one or more elastomers derived exclusively or predominantly (at least 60 wt%, or at least 80 wt%, or at least 90 wt%, or at least 95 wt%) from conjugated dienes. The conjugated diene-based elastomer component may be selected from natural rubber, synthetic polyisoprene, polybutadiene, styrene-butadiene copolymers, and mixtures and copolymers thereof. In one embodiment, the conjugated diene-based elastomer component is at least 80 wt% natural rubber.
[0038]
[0044] Natural rubber is derived primarily from isoprene (2-methyl-1,3-butadiene) and is therefore primarily (e.g., at least 99% by weight) polyisoprene. As used herein, the term "natural rubber" means that rubber of natural origin can be collected from sources such as the Hevea rubber tree, as well as from non-Hevea sources (e.g., guayule shrub and dandelion, e.g., TKS). In other words, the term "natural rubber" should be interpreted to exclude synthetic polyisoprene. Natural rubber produced from field grade coagulum (cup lumps) obtained from Hevea brasiliensis trees is a common form of natural rubber. For example, technically specified rubber or block rubber (TSR) is natural rubber available from Indonesia, where it may also be called standard Indonesian rubber (SIR), Malaysian (SMR), and Thai (STR). This natural rubber can be obtained in several grades, including TSR10 and TSR20, with the TSR10 grade having a higher purity.
[0039]
[0045] In one embodiment, the conjugated diene based elastomer component is at least 80% by weight natural rubber, or at least 90% by weight, or up to 100% by weight natural rubber.
[0040]
[0046] Synthetic polyisoprenes are also suitable, particularly cis-1,4-polyisoprene having a cis content of at least 94% by weight. The cis-1,4-content of the synthetic polyisoprene may be at least 96% by weight. The Tg of the synthetic polyisoprene may be in the range of -60°C to -70°C.
[0041]
[0047] The weight ratio of the conjugated diene-based elastomeric component (particularly natural rubber) to the isobutylene-based elastomeric component (particularly butyl rubber) in the sealant composition may be at least 5:95, or at least 10:90, or at least 15:85, or at least 17:83, or at least 20:80, or at least 25:75, or up to 40:60, or up to 30:70.
[0042] 2. Filler
[0048] Particulate fillers may be included in the sealant composition, but fillers which are hereinafter referred to as being absent from the sealant composition may be present in trace amounts, for example, when they are customarily found as impurities in other particulate fillers.
[0043]
[0049] The particulate filler(s) may be present in the sealant composition in an amount of at least 5 phr, or at least 10 phr, or at least 15 phr, or at least 20 phr, or up to 75 phr, or up to 60 phr, or up to 50 phr, or up to 40 phr, or up to 30 phr, or up to 25 phr, or up to 20 phr.
[0044]
[0050] Exemplary particulate fillers useful herein include silica, calcium carbonate (CaCO), titanium dioxide, hydrated aluminum silicate clays, 2:1 layered silicate clays and organophilic clays formed therefrom, calcium silicate, carbon black, graphite, graphene, carbon nanotubes, wollastonite, talc, diatomaceous earth, starch, lignin, alumina, polymeric fillers, and mixtures thereof.
[0045]
[0051] In one embodiment, the filler comprises silica particles, such as amorphous (e.g., precipitated) silica and / or crystalline silica. The term "silica" is used herein to refer to silicon dioxide, SiO2 (which may contain minor impurities, generally less than 1% by weight, generated from the process in which silica is formed). The term "precipitated silica" is used to refer to synthetic amorphous silica, which is usually obtained by the process of precipitating silicate using an acidifying agent.
[0046]
[0052] Precipitated silica can be prepared, for example, by digesting amorphous silica found in rice husks or other biological waste with sodium hydroxide to form sodium silicate, and precipitating silica from the sodium silicate by reaction with an acidifying agent, such as sulfuric acid or carbon dioxide. The resulting silica precipitate is washed and filtered. Methods for the preparation of precipitated silica are described in U.S. Pat. Nos. 5,587,416A, 5,800,608A, 5,882,617A, 6,107,226A, 6,180,076B1, 6,221,149B1, 6,268,424B1, 6,335,396B1, U.S. Pat. No. 6,421,262, and U.S. Pat. No. 6,513,636. It is disclosed in Patent No. 7,585,481B2, U.S. Patent No. 9,334,169B2, U.S. Patent No. 9,359,215B2, U.S. Publication No. 20020081247A1, U.S. Publication No. 20030118500A1, U.S. Publication No. 20040062701A1, U.S. Publication No. 20050032965A1, and EP0647591A1. Precipitated silica can also be formed from silica gel, as described, for example, in U.S. Patent No. 5,708,069A, U.S. Patent No. 7,550,610B1, and U.S. Patent No. 5,789,514A. Silica gel can be derived, for example, by hydrophobizing silica hydrogel, for example, with organomercaptosilanes and alkylsilanes, and drying the product.
[0047]
[0053] Precipitated silica is 100-350m 2The BET (nitrogen) surface area of the precipitated silica may be determined according to ASTM D1993-18, "Standard Test Method for Precipitated Silica-Surface Area by Multipoint BET Nitrogen Adsorption", which relates to the conventional theory described by Brunauer, Emmett and Teller, Journal of the American Chemical Society, Vol. 60, p. 309 (1938).
[0048]
[0054] Exemplary precipitated silicas include Hi-Sil™ 532, and Hi-Sil™ 532EP, manufactured by PPG Industries; Hubersil™ 4155, manufactured by JMHuber Company; Zeosil™, with the designations 115GR, 125GR, 165GR, 175GR, 185GR, 195GR, 1085GR, 1165MP, 1115MP, HRS1200MP, Premium MP, Premium 200MP, Premium SW, and 195HR, manufactured by Solvay; Ultrasil™, with the designations VN2, VN3, VN3GR, 5000GR, 7000GR, 9000GR, manufactured by Evonik; Zeopol™, with the designations 8755LS and 8745, manufactured by Evonik; Newsil™, with the designations 115GR and 2000MP, manufactured by Wuxi and Tokusil™ 315, manufactured by Maruo Calcium Co., Ltd.
[0049]
[0055] The silica may also be surface treated, for example with a coupling agent and / or a polyalkylene oxide, such as polyethylene glycol, prior to incorporation of the pretreated silica into the sealant composition to enhance dispersion and / or adhesion to elastomers. The coupling agent and / or polyalkylene oxide may also help to reduce the tendency of water associated with hydration or hydroxyl groups on the silica to prematurely decompose the organic peroxide intended to depolymerize the butyl rubber in the sealant composition. In another embodiment, the silica may be treated in situ in the sealant composition with the coupling agent and / or polyalkylene oxide prior to addition to the organic peroxide.
[0050]
[0056] Polyalkylene glycols that can be used for the pretreatment or in situ in the sealant composition are described in more detail below.
[0057] Suitable coupling agents generally include a first portion, which is reactive with the hydroxyl groups (e.g., silanol groups) present on the surface of the precipitated silica, and a second portion capable of reacting with the diene-based elastomer. The two portions are linked by a linking group, such as a hydrocarbyl or sulfide-based bridge, so that the precipitated silica is chemically bonded to the elastomer. Examples of silica coupling agents include those containing groups such as alkyl, alkoxy, mercapto, blocked mercapto, sulfide-containing groups (e.g., monosulfide-based alkoxy-containing groups, disulfide-based alkoxy-containing groups, tetrasulfide-based alkoxy-containing groups), amino, vinyl, epoxy, and combinations thereof. The silica coupling agent can be present in an amount sufficient to obtain a weight ratio of the total amount of coupling agent to the silica filler of at least 0.1:100 or up to 1:5, such as at least 1:100, or at least 1:50, or up to 1:20, or up to 1:10.
[0051]
[0058] In one embodiment, silica is present in the sealant composition at 1 phr or more, for example at least 2 phr, or at least 5 phr, or at least 6 phr, or at least 7 phr, or up to 20 phr, or up to 18 phr, or up to 15 phr, or up to 14 phr, or up to 12 phr, or up to 10 phr. Silica may be at least 10 phf, or at least 20 phf, or at least 30 phf, or up to 100 phf, or up to 99 phf, or up to 95 phf of particulate filler.
[0052]
[0059] In one embodiment, the ratio of silica to natural rubber is at least 0.4:1 and may be up to 1:1. In one embodiment, the ratio of silica to butyl rubber is at least 0.7:10 and may be up to 1.1:10.
[0053]
[0060] The silicate clays that can be used in the sealant composition include layered silicate clays and organophilic clays derived therefrom. Exemplary layered silicate clays include montmorillonite, bentonite, hectorite, saponite, nontronite, beidellite, fluorohectorite, stevensite, volkonskoite, sauconite-laponite, and physical blends thereof. Useful organophilic clays are silicate clays that have been chemically modified to make them compatible with organic materials. The silicate clays used as starting materials may include one or more of montmorillonite, hectorite, saponite, attapulgite, and sepiolite. These clays contain exchangeable cationic species, such as sodium, potassium, or calcium ions, on their surfaces and between the clay galleries or layers. During the preparation of the organophilic clays, at least a portion of these exchangeable cationic species are replaced with organic cations, such as quaternary amines, organophosphorus ions, and the like.
[0054]
[0061] The silicate clay may be absent from the sealant composition or may be present in the sealant composition at from 0.5 to 20 phr, such as at least 1 phr, or at least 2 phr, or at least 5 phr, or up to 10 phr.
[0055]
[0062] Calcium carbonate may also be used in combination with a filler, such as silica. The benefit of using calcium carbonate is that it provides a modified degree of reinforcement compared to silica, which can aid in processing the sealant composition and in combination with silica to provide the appropriate stiffness and associated dimensional integrity to the partially depolymerized sealant composition.
[0056]
[0063] In one embodiment, calcium carbonate can be used as a support for the organic peroxide.
[0064] Calcium carbonate may be absent from the sealant composition or may be present in the sealant composition at 0.5 phr or more, for example at least 5 phr, or at least 10 phr, or at least 15 phr, or at least 18 phr, or up to 30 phr, or up to 25 phr, for example serving as a carrier for the organic peroxide. The ratio of calcium carbonate to organic peroxide may be at least 20:80, or at least 30:70, or up to 70:20, or up to 60:40, or up to 50:50.
[0057]
[0065] Carbon black, when used in the sealant composition, has an average molecular weight of at least 100, or at least 102, or at least 104, or up to 120, or up to 118, or up to 116 m. 2Exemplary carbon blacks include the ASTM designations N110, N121, N134, N220, N231, N234, N242, N293, N299, N315, N326, N330, N332, N339, N343, N347, N351, N358, N375, N539, N550, N582, N630, N642, N650, N683, N754, N762, N765, N774, N787, N907, N908, N990, and N991, as specified by ASTM D1765-21, "Standard Classification System for Carbon Blacks Used in Rubber Products";
[0066] In one embodiment, the sealant composition is free or substantially free (1 phr or less) of carbon black, hi another embodiment, carbon black is present in the sealant composition at 2 to 20 phr, or up to 10 phr, or up to 5 phr.
[0058]
[0067] Graphene, when used in sealant compositions, is generally a one-atom-thick crystalline form of carbon in which the carbon atoms are held together by SIGMA bonds arranged in a two-dimensional honeycomb lattice. More specifically, graphene is a crystalline allotrope of carbon with two-dimensional properties. The carbon atoms in graphene are densely packed in a regular atomic-scale hexagonal (tortoiseshell) pattern. Each atom has four bonds, one σ-bond with each of its three neighbors, and one π-bond oriented out of the plane. The distance between adjacent carbon atoms in graphene is approximately 0.142 nanometers. Graphene used as a granular filler may have zigzag, armchair, K-region, gulf, bay, cove, and / or fjord-type edge configurations. At least 50%, at least 60%, at least 70%, or at least 80% of the carbon-carbon bonds in the graphene structure edges may be one of the zigzag, armchair, and bay configurations. For example, at least 40%, 50%, or 60% of the carbon-carbon bonds at the edge of the graphene structure may be in a zigzag configuration, less than 40%, or less than 30% may be in a cove configuration, and less than 20% may be in a fjord configuration.
[0059]
[0068] Exemplary graphene that can be used as a particulate filler is exfoliated into nanoscale graphene plate (NGP) material, which is essentially an individual single sheet of graphene or multiple sheets of graphite planes. Each graphite plane is generally a two-dimensional hexagonal structure of carbon atoms. Each plane has a length and width parallel to the graphite plane and a thickness perpendicular to the graphite plane, with at least one of the length, width, and thickness being 100 nanometers (nm) or less. Typically, each of the length, width, and thickness is less than 100 nm. This NGP material can be produced, for example, by the process described in U.S. Pat. No. 7,071,258 B1.
[0060]
[0069] In one embodiment, the sealant composition is free or substantially free (1 phr or less) of graphene, hi another embodiment, graphene is present in the sealant composition at 2 to 20 phr, or up to 10 phr, or up to 5 phr.
[0061]
[0070] In one particular embodiment, black particulate fillers derived from forms or carbon such as carbon black, graphite, graphene, and / or carbon nanotubes are present in the sealant composition at no more than 5 phr, or no more than 1 phr.
[0062]
[0071] Titanium dioxide, when used as a filler, can also function as a colorant. Titanium dioxide useful herein may have an average particle diameter of at least 0.1 micrometers (μm), for example, at least 0.2 μm, or up to 5 μm, or up to 4 μm. Light scattering by titanium dioxide is greatest in particles with diameters of 0.2 to 0.3 μm. Thus, to function as a colorant, at least 50% by weight of the particles may be within this range.
[0063]
[0072] In one embodiment, the sealant composition is free or substantially free (0.1 phr or less) of titanium dioxide. In another embodiment, titanium dioxide is at least 0.1 phr in the sealant composition, such as at least 1 phr, or up to 10 phr, or up to 5 phr, or up to 3 phr.
[0064]
[0073] Exemplary polymeric fillers in particulate form useful herein include polypropylene, precured rubber, and mixtures thereof. Generally, the particles of such fillers may have an average size of less than 10 micrometers (μm).
[0065]
[0074] Polypropylene suitable for use as a filler may be of low molecular weight. Such low molecular weight polypropylene has a weight average molecular weight (M) of at least 4,000, or at least 6,000, or at least 8,000, or at least 10,000, or up to 40,000, or up to 25,000, or up to 20,000, or up to 15,000. w Polypropylene may be utilized as a replacement or partial replacement for carbon black and / or mineral fillers, and lower levels (e.g., less than 30-40% by weight) may be utilized than with other fillers.
[0066]
[0075] In one embodiment, the polymeric filler is absent from the sealant composition, hi another embodiment, the polymeric filler is present in the sealant composition in a total amount of at least 1 phr, or up to 15 phr.
[0067] 3. processing oil
[0076] The sealant composition may optionally include one or more processing oils. Suitable processing oils include aromatic oils, paraffinic oils, naphthenic oils, triglyceride oils, and low polycyclic aromatic (PCA) oils, such as light extractive solvates (MES), oils treated with aromatic extracts from distillate oils (TDAE), aromatic special extracts from residual oils (SRAE), and heavy naphthenic oils, and mixtures thereof. Suitable low PCA oils may include oils with polycyclic aromatic content of less than 3% by weight, as determined by the IP346 method. A description of the IP346 method may be found in "Standard Methods for Analysis & Testing of Petroleum and Related Products" and "British Standard 2000 Parts", 2003, 62nd edition, published by the Institute of Petroleum, United Kingdom. Suitable naphthenic, paraffinic processing oils with a maximum aromatic content of less than 15% by weight are exemplary oils. Such processing oils may have a naphthenic content of 35-45 wt.%, a paraffinic content of 45-55 wt.%, and an aromatic content of less than 15 wt.% (eg, 10-14 wt.%).
[0068]
[0077] Exemplary naphthenic processing oils include Hyprene™ 100 manufactured by Ergon Refining, Inc., and Tufflo 100™ manufactured by Barton Solvent Company.
[0069]
[0078] Triglyceride oils that can be used include vegetable oils, including castor oil, soybean oil, canola oil (rapeseed oil), corn oil, cottonseed oil, olive oil, palm oil, safflower oil, sunflower oil, coconut oil, and peanut oil. Castor oil is a triglyceride oil that contains approximately 87% by weight ricinoleic acid, 7% by weight oleic acid, 3% by weight linoleic acid, 2% by weight palmitic acid, and 1% by weight stearic acid.
[0070]
[0079] Processing oils, in relatively small concentrations, aid in mixing of the components for the sealant composition and / or facilitate processing of the sealant composition.
[0080] The processing oil may be absent from the sealant composition or may be utilized in the sealant composition at 0.1 phr or higher, or at least 1 phr, or at least 2 phr, or at least 4 phr, or at least 5 phr, or up to 40 phr, or up to 20 phr, or up to 10 phr, or up to 8 phr.
[0071] 4. Polyalkylene Oxide
[0081] Suitable polyalkylene oxides for use in the sealant composition include polyethylene glycol, polypropylene glycol, and mixtures thereof. In one embodiment, the polyalkylene oxide is polyethylene glycol. The polyalkylene oxide may have a weight average molecular weight Mw of at least 500, for example, at least 2,000, or at least 4,000, or up to 15,000, or up to 12,000, or up to 10,000, or up to 8,500. The polyalkylene oxide may be absent from the sealant composition. When a polyalkylene oxide, such as polyethylene glycol, is utilized, it may be included in an amount of at least 0.1 phr, for example, at least 0.2 phr, or at least 0.3 phr, or up to 5 phr, or up to 3 phr, or up to 2 phr, or up to 1 phr, or up to 0.6 phr.
[0072]
[0082] Examples of commercially available polyethylene glycols include Carbowax™ PEG 3350 and Carbowax™ PEG 8000, manufactured by Dow Chemical Company, where the numbers indicate the approximate weight average molecular weight. Other polyalkylene oxide polymers, such as those described in U.S. Patent No. 6,322,811 B1 and U.S. Patent No. 4,082,703 A, can also be used.
[0073] 5. Coloring agent
[0083] The sealant composition may include one or more colorants in the form of pigments and / or dyes. Both organic and inorganic colorants may be utilized. The inclusion of one or more non-black colorants in the sealant composition may make the fact that the tire is punctured obvious and the location of the puncture may be more easily identified. A wide variety of colors may be used for this purpose, with light or bright colors that stand out from the characteristic black color of the tire tread being suitable. For example, white, red, orange, yellow, green, or blue colorants may be included. A red iron pigment may be used to impart a brilliant red color, or a yellow pigment may be used to impart a brilliant yellow color. The colorants may be utilized at 0.1 phr to 5 phr, for example at least 0.2 phr or up to 4 phr.
[0074]
[0084] Some representative examples of pigments that may be utilized include Pigment Yellow 1 (CAS No. 2512-29-0), Pigment Yellow 110 (CAS No. 5590-18-1), Pigment Yellow 12 (CAS No. 15541-56-7), Pigment Yellow 126 (CAS No. 90268-23-8), Pigment Yellow 127 (CAS No. 68610-86-6), Pigment Yellow 13 (CAS No. 5102-83-0), Pigment Yellow 138 (CAS No. 30125-47-4), Pigment Yellow 14 (CAS No. 5468-75-7), Pigment Yellow 150 (CAS No. 68511-62-6), Pigment Yellow 151 (CAS No. 31837-42-0), Pigment Yellow 154 (CAS number 68134-22-5), Pigment Yellow 168 (CAS number 71832-85-4), Pigment Yellow 17 (CAS number 4531-49-1), Pigment Yellow 174 (CAS number 78952-72-4), Pigment Yellow 180 (CAS number 77804-81-0), Pigment Yellow 183 (CAS number 65212-77-3), Pigment Yellow 191 (CAS number 129423-54-7), Pigment Yellow 3 (CAS number 6486-23-3), Pigment Yellow 34 (CAS number 1344-37-2), Pigment Yellow 42 (CAS number 51274-00-1), Pigment Yellow 65 (CAS number 6528-34-3), Pigment Yellow 74 (CAS number 6358-31-2), Pigment Yellow 75 (CAS number 52320-66-8), Pigment Yellow 81 (CAS number 22094-93-5), Pigment Yellow 83 (CAS number 5567-15-7), CI Pigment Yellow 42 (iron oxide), CI Pigment Yellow 34 (lead chromate), CI Pigment Yellow 184 (bismuth nadate), CICI Pigment Yellow 53 (nickel-antimony), CI Pigment Orange 20 (cadmium sulfide), CI Pigment Red 101 (iron oxide), CI Pigment Red 104, CI Pigment Red 29 (ultramarine blue pigment), CI Pigment Blue 29 (ultramarine blue pigment), CI Pigment Blue 28, CI Pigment Blue 36, CI Pigment Violet 15 (ultramarine blue pigment), CI Pigment Violet 16 (manganese violet), Pigment Green 17 (chromium oxide green), CI Pigment Green 19 (cobalt-based mixed metal oxides), CI Pigment Green 26 (cobalt-based mixed metal oxides), and CI Pigment Green 50 (cobalt-based mixed metal oxides). Some additional inorganic pigments that can be used are Ultramarine Blue, Persian Blue, Cobalt Blue (CAS number 1345-16-0), Cerulean Blue, Egyptian Blue, and Chinese Blue (BaCuSiO. 10), Azurite Blue (Cu3(CO3)2(OH)2), Prussian Blue (CAS number 14038-43-8), YInMn Blue (Oregon Blue), Realgar Red (α-As4S4), Cadmium Red (Cd2SSe), Cerium Sulfide Red, Venetian Red (Fe2O3), Red Ochre (Anhydrous Fe2O3), Burnt Sienna Red, Red Lead (Pb3O4), Vermilion Red, Cinnabar Red, Ultramarine Blue Violet, Han Purple (BaCuSi2O6), Cobalt Violet (CO3(PO4)2), Manganese Violet (NH4MnP2O7), Oak Pale violet, primrose yellow (BiVO4), cadmium yellow (CdS), chrome yellow (PbCrO4), aureolin yellow (K3Co(NO2)6), yellow ochre (Fe2O3·H2O), Naples yellow, titanium yellow (NiO·Sb2O3·20TiO2), zinc yellow (ZnCrO4), and chrome orange (PbCrO4·PbO). Mixtures of colorants may also be utilized.
[0075]
[0085] In one particular embodiment, the sealant composition includes a white mineral pigment, such as titanium dioxide, and / or a yellow or other non-white pigment or dye, however, for purposes of calculating phr and phf, the titanium dioxide is considered a filler rather than a colorant.
[0076] 6. organic peroxide
[0086] Organic peroxides (organic peroxides) are commonly present in sealant compositions and act as depolymerization agents for the isobutylene-based elastomer component.
[0077]
[0087] The organic peroxide utilized may be one of those commonly used for crosslinking rubbery polymers. Peroxide compounds that decompose only at higher temperatures, e.g., above 75°C or above 80°C, may be used. Suitable organic peroxides include dialkyl peroxides, e.g., dialkylbenzene peroxides, and alkyl peresters, with the same or different radical groups. The organic peroxide may contain two peroxide groups. Frequently, the peroxide group is attached to a tertiary butyl group. The basic moiety from which the two peroxide groups are pendant may be an aliphatic, cycloaliphatic, or aromatic radical group.
[0078]
[0088] Examples of suitable organic peroxides include bis(α,α-dimethylbenzyl)peroxide (more commonly known as dicumyl peroxide); tert-butyl peroxybenzoate; 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane; 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane; 2,5-dimethyl-2,5-di(tert-butylperoxy)-hexyne-3; p-chlorobenzyl peroxide; 2,4-dichlorobenzyl peroxide; 2,2-bis-(tert-butylperoxy)-butane; tert-butylcumyl peroxide; di-tert-butyl peroxide; benzoyl peroxide; 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane; 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane; and mixtures thereof.
[0079]
[0089] In one embodiment, the first organic peroxide acts as a depolymerization initiator, and the second organic peroxide acts as a depolymerization propagator. The first organic peroxide activates at a lower temperature than the second organic peroxide, but tends to decompose more rapidly. For example, the organic peroxide may include a trace amount of n-butyl 4,4-di(tert-butylperoxy)valerate as a depolymerization initiator and a large amount of dicumyl peroxide as a depolymerization propagator.
[0080]
[0090] Suitable peroxides include those with an active oxygen content (AOC) of at least 2. The active oxygen content is determined by dividing the weight of the active oxygen atoms in the compound by its total molecular weight in the compound (this is done on a one active oxygen atom basis for each peroxide moiety (-OO-)). For example, tert-butylcumyl peroxide has one active oxygen atom (molecular weight 16) and a total molecular weight of 208. Thus, the active oxygen content of tert-butylcumyl peroxide is 16 / 208 (7.7%). Peroxides with active oxygen contents greater than 7%, 8%, 9%, or even 10% are particularly suitable because they produce less gas during the tire curing process than peroxides with lower active oxygen contents.
[0081]
[0091] The organic peroxide can be added to the sealant composition in pure form (100% active peroxide) or it can be carried on an inert, free-flowing mineral carrier or dispersed in an oil, such as silicone oil. Calcium carbonate is an inert mineral carrier frequently utilized for this purpose. Another carrier is a combination of calcium carbonate and calcium silicate.
[0082]
[0092] One exemplary peroxide is in the form of a complex of dicumyl peroxide on precipitated calcium carbonate (40.5% active) available as Di-Cup® 40C from Arkema Inc. Another exemplary peroxide is in the form of a complex of n-butyl 4,4-di-(tert-butylperoxy)valerate with a combination of calcium carbonate and calcium silicate as mineral carriers, available from Nouryon as Trigonox 17-40B pd™, with a weight ratio of organic peroxide to carrier of 40 / 60.
[0083]
[0093] It is desirable that the isobutylene-based elastomeric component (e.g., butyl rubber) of the sealant composition is depolymerized by the free radicals generated by the organic peroxide such that the resulting sealant layer has a storage modulus (G') in the range of at least 50 kPa, or at least 60 kPa, or at least 80 kPa, or at least 90 kPa, or up to 200 kPa, or up to 180 kPa, or up to 170 kPa, as measured by a Rubber Process Analyzer (RPA) (measured at 40°C, 1 Hertz, and 5% strain) after exposure to 170°C for 5 minutes. To promote the sealant efficiency of the installed tire sealant and its ability to effectively seal against various puncture objects, such as nails, the appropriate storage modulus (G') may depend in part on the type of tire, including the size of the tire, and the intended conditions of use of the tire.
[0084]
[0094] The natural rubber in the sealant composition tends to react with the organic peroxide, thus reducing the amount available to depolymerize the isobutylene-based elastomer component (e.g., butyl rubber). Thus, the amount of organic peroxide added to the composition is selected to be sufficient to cause partial depolymerization of the isobutylene-based elastomer component in situ in the tire. The organic peroxide can be added to the sealant composition in an amount of at least 0.1 phr (expressed as active peroxide), for example, at least 0.5 phr, or at least 1 phr, or at least 2 phr, or at least 4 phr, or up to 20 phr, or up to 10 phr, or up to 8 phr.
[0085]
[0095] The exemplary sealant composition does not include a sulfur-based vulcanizing (curing) agent.
[0096] In one embodiment, the organic peroxide is activated with an activator, such as a 2,2,6,6-tetraalkylpiperidine hindered amine. Examples of such hindered amines are, for example, poly[[6-[1,1,3,3-tetramethylbutyl)amino]-s-triazine-2,4-diyl][2,2,6,6-tetramethyl-4-piperidyl)imino]hexamethylene[(2,2,6,6-tetramethyl-4-piperidyl)imino]] compounds, such as those described in, for example, U.S. Pat. No. 7,674,344 B2.
[0086]
[0097] Exemplary sealant compositions, expressed as phr, are shown in Table 1.
[0087] [Table 1]
[0088]
[0098] As will be appreciated, combinations of the above ranges may be utilized. Formation of the sealant composition
[0099] The various components of the sealant layer can be mixed together using any convenient rubber mixing equipment, such as an internal rubber mixer. Typically, the elastomers, such as butyl rubber and natural rubber, are blended in at least one successive preparatory, or non-productive, mixing step in the absence of organic peroxide, followed by a final, or productive, mixing step in which the organic peroxide (and possibly one or more of the additional ingredients) are added.
[0089]
[0100] In one embodiment, in a first, non-productive stage(s), ingredients other than the organic peroxide are stirred in a mixer set at a suitable temperature, for example, at least 100°C, or at least 110°C, or up to 180°C. The temperature of the mixture increases as it is stirred. Once the desired temperature is reached, the mixture is dripped from the mixer and allowed to cool before being returned to the mixer. In a second, productive stage, the mixture is returned to the mixer with the organic peroxide. The mixer is set at a temperature below the decomposition temperature of the organic peroxide, for example, 70°C or less, for example, about 60°C. The mixture is dripped from the mixer at a maximum temperature of about 85°C to minimize premature decomposition of the peroxide.
[0090] Tire Construction
[0101] A sealant layer formed from the above-described sealant composition can be fitted into an unvulcanized tubeless pneumatic rubber tire prior to vulcanization. During tire construction, the sealant composition can be encapsulated in the form of a layer(s) within one or more enclosures within the tire. The enclosure(s) can be defined, at least in part, by one or more containment layers formed of hard rubber, which allows for relatively easy handling of the sealant composition and construction into a tire.
[0091]
[0102] In one embodiment, the tire includes a supporting carcass generally formed into a doughnut shape, an outer circumferential tread, and an inner containment layer, e.g., an innerliner (or "innerliner"). As used herein, the term "tread" refers to both the portion of the tire that contacts the road under normal inflation and load, and any subtreads. The innerliner is an air barrier layer that acts to prevent air or another gas, e.g., nitrogen, (used to inflate the tire), from escaping through the tire structure by diffusion. The innerliner may be formed of halobutyl rubber or some other suitable material that is highly resistant to gas permeation. A sealant layer is disposed intermediate the supporting carcass and the innerliner or other containment layer. In another embodiment, two or more innerliner layers act as containment layers for the sealant.
[0092]
[0103] In one embodiment, the sealant layer may be disposed between, and optionally in direct contact with, the supporting carcass and innerliner of the tire, as illustrated in FIG. 1. In another embodiment, the sealant layer formulation may be disposed between, and optionally in direct contact with, two innerliner layers, as illustrated in FIG. 2. In this case, the sealant layer is sandwiched between the first and second layers of the innerliner and spaced apart from the tire carcass and tread by the first and second layers of the innerliner, respectively. As an alternative to one or more of the innerliner layer(s), one or more other containment layers may be utilized. In another embodiment, the tire does not include any innerliner layer, and the sealant composition is embedded (extruded) between the supporting carcass and a different type of containment layer of the tire, as illustrated in FIG. 3. As will be appreciated, multiple sealant layers may be provided, with each pair of adjacent sealant layers spaced apart from the intermediate containment layer. The carcass and / or tread may include one or more reinforcing layers formed of fabric, polyethylene sheeting, and / or metal.
[0093]
[0104] In the embodiment of FIG. 1, a self-sealing pneumatic rubber tire 2 of the tubeless type is shown. The tire has sidewalls 3, a supporting carcass 4, inelastic beads 5, an innerliner (air barrier layer) 6, a sealant layer 7, and an outer circumferential tread (tread portion) 8 (which extends from the sidewalls). Each sidewall 3 extends radially inward from an axially outer edge 8 of the tread portion to connect each of the inelastic beads 5. The supporting carcass 4 acts as a support structure for the tread portion 8 and the sidewalls 3. The sealant layer 7 is disposed inwardly from the supporting carcass 4 and outwardly from the innerliner 6. The outer circumferential tread 8 is adapted to contact the ground when the tire is in use.
[0094]
[0105] In the embodiment of Fig. 2, a self-sealing pneumatic rubber tire 10 is shown. The pneumatic tire is of the tubeless type and includes a tread portion 11, a crown region 12, a sidewall 13, a supporting carcass 14, a non-stretching bead 15, an innerliner consisting of inner and outer layers 16A, 16B, and a sealant layer 17. In this embodiment, the sealant layer 17 is sandwiched between two layers of the innerliner 16A and 16B. Thus, the sealant layer 17 is disposed radially inward from one layer of the innerliner 16A and outward from another layer of the innerliner 16B. Both layers of the innerliner 16 and the sealant layer 17 are disposed radially inward from the supporting carcass 14.
[0095]
[0106] In the embodiment of FIG. 3, a self-sealing pneumatic rubber tire 22 of the tubeless type without an inner liner is illustrated. The self-sealing pneumatic rubber tire 22 includes a sidewall 23, a supporting carcass 24, an inelastic bead 25, a containment layer 26, a sealant layer 27, and an outer circumferential tread (tread portion) 28. Each sidewall 23 extends radially inward from an axially outer edge 28 of the tread portion connected with each inelastic bead 25. The supporting carcass 24 acts as a support structure for the tread portion 28 and the sidewall 23. The sealant layer 27 is disposed inward from the supporting carcass 24 and outward from the containment layer 26. In particular, the sealant layer 25 is sandwiched between the supporting carcass 24 and the containment layer 26. The outer circumferential tread 28 is adapted to contact the ground when the tire is in use. In this embodiment, the containment layer 26 is disposed inward from the sealant layer 27 and is the innermost layer of the tire 22.
[0096]
[0107] The sealant layer 7,17,27 may extend from at least one sidewall of the tire to the other, in other words the sealant layer may have a length that encompasses the tread region 8,11,28 of the tire.
[0097]
[0108] The thickness of the sealant layer can vary widely in unvulcanized puncture sealant tires. In one embodiment, the thickness of the sealant layer is 0.2 mm to 8.5 mm, for example, at least 3 mm, or at least 4 mm, or up to 6 mm, or up to 5 mm. In passenger tires, a thickness of about 4.5 mm can be used.
[0098]
[0109] The tread, sidewalls, and carcass may each be formed from a sulfur vulcanizable rubber composition, which may be the same or different. Exemplary elastomers for forming the rubber compositions used in these sections include natural rubber, synthetic polyisoprene, natural polyisoprene, styrene-butadiene copolymers, solution polymerized styrene-butadiene (SSBR), emulsion polymerized styrene-butadiene rubber (ESBR), butadiene rubber (BR), halobutyl rubber, bromobutyl rubber, chlorobutyl rubber, nitrile rubber, liquid rubber, polynorbornene copolymer, isoprene-isobutylene copolymer, ethylene-propylene-diene rubber, chloroprene rubber, acrylate rubber, fluororubber, silicone rubber, polysulfide rubber, epichlorohydrin rubber, styrene-isoprene-butadiene terpolymer, hydrated acrylonitrile butadiene rubber, isoprene-butadiene copolymer, butyl rubber, hydrogenated styrene-butadiene rubber, butadiene acrylonitrile rubber, terpolymers formed from ethylene monomer, propylene monomer, and / or ethylene propylene diene monomer (EPDM), isoprene-based block copolymers, butadiene-based block copolymers, and / or ethylene propylene diene monomer (EPDM). copolymers, styrenic block copolymers, styrene-butadiene-styrene block copolymers (SBS), styrene-ethylene / butylene-styrene block copolymers (SEBS), styrene-[ethylene-(ethylene / propylene)]-styrene block copolymers (SEEPS), styrene-isoprene-styrene block copolymers (SIS), random styrene copolymers, hydrogenated styrenic block copolymers, styrene-butadiene copolymers, polyisobutylene, ethylene vinyl acetate (EVA) polymers, polyolefins, amorphous polyolefins, semi-crystalline polyolefins, alpha-polyolefins, reactor-ready polyolefins, acrylates, metallocene-catalyzed polyolefin polymers and elastomers, reactor-made thermoplastic polyolefin elastomers, olefin block copolymers, copolyester block copolymers, polyurethane block copolymers, polyamide block copolymers, thermoplastic polyolefins, thermoplastic vulcanizates, ethylene vinyl acetate copolymers,Ethylene n-butyl acrylate copolymer, ethylene methyl acrylate copolymer, neoprene, acrylic acid, urethane, poly(acrylate), ethylene acrylic acid copolymer, polyether ether ketone, polyamide, atactic polypropylene, polyethylene including atactic polypropylene, ethylene-propylene polymers, propylene-hexene polymers, ethylene-butene polymers, ethylene octene polymers, propylene-butene polymers, propylene-octene polymers, metallocene catalyzed polypropylene polymers, metallocene catalyzed polyethylene polymers, ethylene-propylene-butylene terpolymers, copolymers produced from propylene, ethylene, C4-C, 10 The polymer may include one or more of alpha-olefin monomers, polypropylene polymers, maleated polyolefins, polyester copolymers, copolyester polymers, ethylene acrylic acid copolymers, and / or polyvinyl acetate, and / or the polymer optionally includes modifications and / or functionalizations selected from one or more of hydroxyl-, ethoxy-, epoxy-, siloxane-, amine-, amine siloxane-, carboxy-, phthalocyanine-, and silane-sulfide-groups at the polymer chain ends and / or pendant positions within the polymer.
[0099]
[0110] As an example, a tire tread rubber composition may include 100 phr of an elastomer component, such as a mixture of styrene-butadiene rubber and polybutadiene, optionally with natural rubber, polyisoprene, or a combination thereof.
[0100]
[0111] In one embodiment, the rubber composition used to form the tread, sidewall, carcass and / or containment layer(s) is free of butyl rubber or contains 5 phr or less of butyl rubber.
[0101]
[0112] In addition to the elastomer, the rubber compositions for forming the tread, sidewall, and carcass may include one or more reinforcing fillers; one or more processing aids, such as liquid plasticizers (e.g., oils), resins, waxes, antioxidants, antidegradants, and / or antiozonants; and a cure package (including a sulfur-based vulcanizing agent). The cure package may further include one or more cure accelerators and / or activators, which act as catalysts for the vulcanizing agents.
[0102]
[0113] The reinforcing fillers may include one or more of silica, carbon black, alumina, aluminum hydroxide, clay (reinforcing grades), magnesium hydroxide, boron nitride, aluminum nitride, and titanium dioxide in a total amount of at least 1 phr, or up to 200 phr. Suitable silicas and carbon blacks may be as described above for the sealant composition. Silica may be present in the rubber composition from 1 to 200 phr, such as at least 3 phr, or at least 10 phr. Carbon black may be present from 5 phr to 200 phr, such as at least 10 phr, or up to 80 phr, or up to 50 phr.
[0103]
[0114] Examples of sulfur-based vulcanizing agents include elemental sulfur (free sulfur), insoluble polymeric sulfur, soluble sulfur, sulfur donating vulcanizing agents such as amine disulfides, polymeric polysulfides, or sulfur olefin adducts, and mixtures thereof. Sulfur vulcanizing agents can be used in amounts of 0.1 to 10 phr, such as at least 0.5 phr, or at least 1 phr, or up to 8 phr, or up to 5 phr. In another embodiment, sulfur vulcanizing agents are not present in the rubber composition.
[0104]
[0115] Examples of cure activators include zinc oxide, and fatty acids, such as stearic acid, and combinations thereof. Examples of cure accelerators include amines, disulfides, guanidines, thioureas, thiazoles, thiurams, sulfenamides, dithiocarbamates, xanthates, and combinations thereof.
[0105]
[0116] An exemplary composition for forming the tread includes a mixture of elastomer, fillers consisting of silica and carbon black, stearic acid, processing oil, zinc oxide, antioxidants, paraffin wax, and optionally a silane coupling agent.
[0106]
[0117] The tire innerliner, when used, may be a halobutyl rubber-based layer formed from a sulfur curable-containing halobutyl rubber composition of halobutyl rubber, such as chlorobutyl rubber or bromobutyl rubber. The innerliner layer may also contain one or more sulfur curable diene-based elastomers, such as cis-1,4-polyisoprene natural rubber, cis-1,4-polybutadiene rubber, and styrene / butadiene rubber, and mixtures thereof, particularly a combination of one or more of the halobutyl rubbers with one or more of the diene-based elastomers.
[0107] Incorporation of the sealant composition into tires
[0118] The sealant composition, for example in the form of a strip of material, is incorporated into an uncured tire. The tire components can be assembled in a mold or on a core and then cured.
[0108]
[0119] In one embodiment, the tire is formed in a mold. In another embodiment, the tire is formed on a donut-shaped core or tire blank. When formed on a core, the tire can be built up layer by layer, starting with the innermost layer, which can be an innerliner layer or other containment layer. The innerliner / other containment layer can be applied by an extruder using a strip or sheet form of rubber, or by other suitable methods. An optional bead, for example, one or more wire column beads, can be applied to the bead area on the innerliner / containment layer. Then, a layer of unreacted sealant is applied, optionally followed by a second innerliner layer. Finally, the carcass, sidewall, and tread are built. As will be appreciated, two layers of innerliner incorporating the sealant composition can also be applied to the core as one piece. When formed in a mold, the tire can be built from the outside, i.e., in reverse order. The formation of the green tire is not limited to any particular method, so long as the sealant layer is encapsulated therein.
[0109]
[0120] In one embodiment, the sealant layer is disposed between a carbon black reinforced rubber innerliner layer and the tire carcass of the tire, or between two carbon black reinforced tire rubber innerliner layers. The tire may also have a rubber tread and rubber sidewalls containing carbon black for rubber reinforcement.
[0110]
[0121] After the green tire is constructed to include a layer of unreacted sealant formulation, it is vulcanized, which may include heating the tire to a temperature of at least 80° C. to partially depolymerize the butyl rubber. Higher temperatures are then used to cure the rubber composition to the tread, carcass, and sidewalls.
[0111]
[0122] Vulcanization of the green tire can be carried out over a wide temperature range, for example, at temperatures ranging from 100°C to 200°C, for example, at least 130°C, or at least 140°C, or up to 170°C, or up to 165°C. In one embodiment, the tire can reach a maximum cure temperature of 160°C to 165°C. The cure cycle used to vulcanize the green tire may have a duration of 4 minutes to 240 minutes, for example, 10 minutes to 25 minutes, or 10 minutes to 17 minutes, or 11 minutes to 13 minutes. Any suitable vulcanization process can be used, for example, heating in a press or mold and / or heating with superheated steam or hot air.
[0112]
[0123] At least partial depolymerization of the isobutylene-based elastomer component of the sealant composition layer embedded in the tire (e.g., between the tire innerliner and the tire carcass) occurs during the vulcanization of the tire itself at high temperature via organic peroxide. In fact, by vulcanization of the tire assembly under high temperature conditions, a large portion of the isobutylene-based elastomer component in the sealant composition is depolymerized in the presence of activated organic peroxide. Thus, the unreacted sealant layer is transformed into a puncture sealant layer during the curing of the tire. The sealant layer can be bonded to adjacent layers of the tire in this process.
[0113]
[0124] In one embodiment, the sealant composition is incorporated into the uncured tire in the form of a strip(s) of material. The strip(s) can be prepared using conventional equipment, such as a calender, extruder, or combinations thereof, and the strips of sealant composition can be assembled into the tire. The thickness of the sealant composition layer can be at least 1 mm, or up to 12 mm. For passenger tires, the sealant composition layer can have a thickness of 2-5 mm, whereas for truck tires, a thickness of 5-9 mm can be used. The width of the sealant layer can be sufficient to span at least the width of the tread of the tire, for example, at least 5 cm, or at least 10 cm.
[0114]
[0125] Without intending to limit the scope of the invention, the following examples illustrate the preparation and evaluation of sealant compositions. EXAMPLES
[0115]
[0126] To demonstrate that the viscosity and hysteresis of the sealant composition upon reaction can be modified to reduce excess runoff compared to compositions without natural rubber, sealant compositions are prepared using different ratios of butyl rubber to natural rubber, different amounts of peroxide, and different amounts of silica. In the examples below, it is shown that the hysteresis can also be reduced by lowering the amount of filler and / or the amount of peroxide. However, since natural rubber tends to crosslink with peroxide, a sufficient amount of peroxide is utilized to ensure the degradation of the butyl rubber.
[0116]
[0127] The unreacted sealant composition shown in Table 2 is prepared in two stages. In the non-productive stage, the ingredients except the peroxide are mixed in a mixer set at 120°C and about 100 rpm. The temperature is increased to about 160°C and the mixture is added dropwise after about 4 minutes. In the productive stage, the mixture is returned to the mixer set at about 60°C and about 60 rpm. The mixture is added dropwise at a maximum temperature of 85°C (to minimize decomposition of the peroxide).
[0117]
[0128] Example 1 is a comparative sealant composition. Two batches of Example 1 are prepared to evaluate reproducibility. Examples 2-4 are exemplary compositions containing a mixture of butyl rubber and natural rubber. Examples 5 and 6 are comparative compositions without natural rubber.
[0118]
[0129] All ingredients are expressed as parts by weight per 100 parts of rubber (phr).
[0119] [Table 2]
[0120] Sample evaluation
[0130] After the production stage, the samples are ground to a thickness of less than 0.5 cm. After they have cooled, a die cutter is used to cut the samples to the appropriate dimensions for the RPA test.
[0121]
[0131] The samples are characterized using a Rubber Process Analyzer (RPA), RPA2000. After the samples are mounted, they are exposed to a temperature of 170° C. for 5 minutes. Dynamic mechanical analysis is performed to obtain values for storage modulus G' at 1%, 3% and 5% strain (MPa) at a temperature of 40° C. Tangent delta values (ratio of G'' to G') are also obtained.
[0122]
[0132] The RPA results are shown in Table 3.
[0123] [Table 3]
[0124]
[0133] Example 5, prepared with lower levels of filler and organic peroxide than Example 1, has comparable G' values but lower hysteresis as shown by the lower tangent delta results. Example 6, which used the same levels of filler as for Example 5 but an even lower level of organic peroxide, has a slightly increased G' while showing a further reduction in tangent delta. Examples 2, 3 and 4, which contain natural rubber, also showed lower hysteresis than Example 1.
[0125] Sealing ability
[0134] To evaluate the ability of the example compositions to seal punctures, a simulated tire assembly is prepared in which a 3 mm thick compressed sealant layer is placed between a 5 mm layer of "tread" and two piles of material, each 1 mm thick, which have a sealant layer on one side and a 1 mm innerliner layer on the other side. The assembly is sealed along its edges and cured at 170°C for 11-12 minutes. After cooling, the sample is clamped in a test fixture and an air pressure of 138 kPa is applied to the innerliner side of the assembly.
[0126]
[0135] Each specimen is punctured with two small nails (2.5 mm diameter), two medium sized nails (3.4 mm diameter), and two large nails (5 mm diameter), taking care to ensure that the nails move completely through the test specimen, but leave the nails protruding far enough from the specimen so that they can be withdrawn during testing.
[0127]
[0136] The sample is pressurized to 241 kPa and maintained at that pressure for several minutes. The nail is then removed. The sealability measurement is calculated, taking into account:
[0137] 1. Puncture Sealing: A weighted measure of the number of punctures sealed (heavier weights correspond to larger nails).
[0128]
[0138] 2. Sealing efficiency: Was the puncture sealed promptly or not?
[0139] Thus, the sealing measurement generally gives higher values to samples exhibiting better sealing characteristics. Table 4 shows the results obtained.
[0129] [Table 4]
[0130]
[0140] Example 4 is not a direct comparison because the evaluation was done using a tire sealability test in which cured tires were clamped, inflated, and punctured with 9 nails, 36 nails of each size. All samples performed relatively well, with Example 5 showing the poorest sealability measurement.
[0131]
[0141] Once the sealability test is complete, the samples are reinflated and the nail is reinserted to create any small leaks in the temporarily repaired samples and monitored for 2 days. All samples are then reinflated and monitored for another 7 days. The samples are then visually examined. All natural rubber containing samples retained the air pressure perfectly and virtually no sealant escaped from the puncture. Significant leakage of sealant and loss of pressure was observed for samples without natural rubber.
[0132]
[0142] It is concluded that the natural rubber network plays a significant role in containing the sealant within the enclosure and in maintaining pressure for the duration of the experiment.
[0143] Unexpectedly, it was observed that compositions with comparable RPA properties and similar sealability measurements had significant differences in long-term behavior: the natural rubber-containing compositions maintained a sealant in the samples throughout the one week experimental period, and they maintained full air pressure thereafter.
[0133]
[0144] These results demonstrate that the natural rubber-containing composition is capable of sealing nail punctures in tires by flowing to fill the void, but does not exhibit continued flow out of the enclosure and into the tire cavity or into the tread.
[0134]
[0145] Each of the documents referenced above is incorporated herein by reference. Except in the examples or where otherwise expressly indicated, all numerical amounts herein specifying amounts of materials, reaction conditions, molecular weights, number of carbon atoms, and the like, shall be understood to be modified by the word "about." Unless otherwise indicated, each chemical or composition referenced herein should be construed as being a commercial grade material that may contain isomers, by-products, derivatives, and other materials as would normally be expected to be present in a commercial grade. However, unless otherwise indicated, the amount of each chemical component is presented exclusive of any solvents or diluent oils that may normally be present in the commercial material. It is to be understood that the upper and lower limits of amounts, ranges, and ratios set forth herein may be independently combined. Similarly, the ranges and amounts for each element of the invention may be used together with the ranges or amounts for any of the other elements.
[0135]
[0146] It will be appreciated that the above-disclosed and other features and functions, or alternatives thereof, can be combined to create many other different systems or applications. Various presently unforeseen or unanticipated alternatives, modifications, or improvements thereon may be made by those skilled in the art, which are also intended to be encompassed by the following claims. [Embodiment of the invention] 1. At least 60 phr of an isobutylene-based elastomer component; and At least 5 phr of conjugated diene-based elastomer component 100 phr elastomer, At least 5 phr of granular filler, and At least 0.5 phr of organic peroxides A sealant composition comprising: 2. The sealant composition of 1, further comprising a colorant that provides a non-black color to the sealant. 3. The sealant composition according to 2, wherein the colorant is selected from a yellow pigment, a yellow dye, and mixtures thereof. 4. The sealant composition of 1, wherein the isobutylene-based elastomer component is selected from the group consisting of butyl rubber, polyisobutylene, and mixtures thereof. 5. The sealant composition according to 3, wherein the isobutylene-based elastomer component is at least 80% by weight butyl rubber. 6. The sealant composition of 1, wherein the isobutylene-based elastomer component comprises a butyl rubber having a weight average molecular weight of at least 5,000 and / or no more than 800,000. 7. The sealant composition according to 1, comprising at least 75 phr of an isobutylene-based elastomer. 8. The sealant composition of 1, wherein the conjugated diene-based elastomer component is selected from the group consisting of natural rubber, synthetic polyisoprene, polybutadiene, styrene-butadiene copolymers, and mixtures and copolymers thereof. 9. The sealant composition according to claim 8, wherein the conjugated diene-based elastomer component is at least 80% by weight natural rubber. 10. The sealant composition according to 1, comprising at least 8 phr of a conjugated diene-based elastomer component. 11. The sealant composition according to 1, comprising up to 40 phr of particulate filler. 12. The sealant composition of 1, wherein the particulate filler comprises at least one of silica, titanium dioxide, calcium carbonate, and carbon black. 13. The sealant composition according to claim 12, comprising at least 5 phr of silica. 14. The sealant composition of 1, wherein the organic peroxide is selected from dicumyl peroxide; 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane; 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane; 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3; p-chlorobenzyl peroxide; 2,4-dichlorobenzyl peroxide; 2,2-bis-(tert-butylperoxy)-butane; tert-butylcumyl peroxide; di-tert-butyl peroxide; benzoyl peroxide; 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane; 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane; and mixtures thereof. 15. The sealant composition of 1, further comprising at least 0.1 phr of a polyalkylene glycol. 16. Circumferential tread, a supporting carcass attached to the tread; A sealant layer comprising the sealant composition of claim 1; and An uncured pneumatic tire including a containment layer, the sealant layer being disposed between a supporting carcass and the containment layer. 17. The uncured pneumatic tire of claim 16, wherein the containment layer comprises a halobutyl rubber. 18. A cured pneumatic tire formed by curing the uncured pneumatic tire of 17 at a temperature sufficient for an organic peroxide to at least partially depolymerize the isobutylene-based elastomer component. 19. A method for forming a sealant layer, comprising: forming a sealant composition comprising 100 phr of an elastomer, a particulate filler, a colorant, and an organic peroxide, the elastomer comprising at least 60 phr of an isobutylene-based elastomer component and at least 5 phr of a conjugated diene-based elastomer component; treating the sealant composition to a sufficient temperature and for a sufficient time to at least partially decompose the isobutylene-based elastomer component. A method for forming a sealant layer comprising: 20. The method of claim 19, further comprising forming an uncured tire including a layer of the sealant composition prior to applying the sealant composition. 21. A method of manufacturing a pneumatic rubber tire having a puncture sealing feature, comprising: constructing an unvulcanized tire including a circumferential rubber tread, a supporting carcass, a containment layer, and a sealant layer disposed on the intermediate supporting carcass and containment layer, the sealant layer including a sealant composition, the sealant composition including 100 phr of an elastomer, a particulate filler, and an organic peroxide, the elastomer including at least 60 phr of an isobutylene-based elastomer component and at least 5 phr of a conjugated diene-based elastomer component; curing the unvulcanized tire at a temperature sufficient to at least partially depolymerize the isobutylene-based elastomer component to produce a pneumatic rubber tire having puncture sealing characteristics. A method comprising: [Explanation of symbols]
[0136] 2 Tubeless self-sealing pneumatic rubber tires 3 side wall 4 Supporting carcass 5. Non-elastic beads 6 Inner liner (air barrier layer) 7 Sealant Layer 8 Outer circumferential tread (tread portion) 10 Self-sealing pneumatic rubber tires 11 Tread area 12 Crown Region 13 Side wall 14 Supporting carcass 15 Non-elastic bead 16A Inner liner that constitutes the outer layer 16B Inner liner that constitutes the inner layer 17 Sealant layer 22 Self-sealing pneumatic rubber tires 23 Side wall 24 Supporting carcass 25 Non-elastic bead 26 Confinement Layer 27 Sealant Layer 28 Outer circumferential tread (tread portion)
Claims
1. 100 phr of an elastomer characterized by at least 60 phr of an isobutylene-based elastomer component and at least 5 phr of a conjugated diene-based elastomer component; at least 5 phr of a particulate filler, and At least 0.5 phr of organic peroxide The sealant composition according to claim 1,
2. The sealant composition of claim 1 further characterized by a colorant that provides a non-black color to the sealant.
3. 10. The sealant composition of claim 1, wherein the isobutylene-based elastomer component is selected from the group consisting of butyl rubber, polyisobutylene, and mixtures thereof.
4. 4. The sealant composition of claim 3, wherein said isobutylene-based elastomer component is at least 80% by weight butyl rubber.
5. 10. The sealant composition of claim 1, wherein the isobutylene-based elastomer component comprises a butyl rubber having a weight average molecular weight of at least 5,000 and / or up to 800,000.
6. 10. The sealant composition of claim 1 comprising at least 75 phr of said isobutylene-based elastomer.
7. 10. The sealant composition of claim 1 comprising at least 8 phr of said conjugated diene-based elastomer component.
8. Circumferential tread, a supporting carcass attached to the tread; A sealant layer characterized by the sealant composition of claim 1, and Confinement Layer wherein the sealant layer is disposed between the supporting carcass and the containment layer.
9. 9. The uncured pneumatic tire of claim 8, wherein the containment layer comprises a halobutyl rubber.
10. 10. A cured pneumatic tire formed by curing the uncured pneumatic tire of claim 8 at a temperature sufficient for said organic peroxide to at least partially depolymerize said isobutylene-based elastomer component.
Citation Information
Patent Citations
Precipitated silicas
EP0647591A1
GB2003、62
US10,730,255B2
Pneumatic tire
US1419470A
Self-sealing inner tube
US1601013A