Humidification element and scale suppression method

The use of a fiber-based humidifying element with controlled BET specific surface area and optional silica particles addresses the scale generation issue in evaporative humidifiers, enhancing performance and cost-effectiveness.

JP2024144528AInactive Publication Date: 2024-10-11UNITIKA LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024117850
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional evaporative humidifiers face issues with scale generation on the windward side of humidifying elements, leading to reduced performance and scattering of scale in the humidified space, which existing solutions with special water retention agents and cover members are costly.

Method used

A humidifying element with a plate-like member formed of fibers, having a BET specific surface area between 0.35 m²/g and 0.5 m²/g, and optionally containing silica particles, is used to suppress scale generation by dispersing it evenly across the surface.

Benefits of technology

The solution effectively reduces scale generation on the windward side of the humidifying element while maintaining humidifying performance and reducing costs by eliminating the need for specialized agents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144528000001_ABST
    Figure 2024144528000001_ABST
Patent Text Reader

Abstract

To provide a humidification element comprising scale suppressing means in a windward portion of the humidification element, which is completely different from scale suppression means in conventional evaporative humidifiers.SOLUTION: A humidification element is used in an evaporative humidifier, where the humidification element comprises a plate-shaped member formed of fibers, and a BET specific surface area of the plate-shaped member is 0.35 m2 / g or more and 0.5 m2 / g or less. This makes it possible to suppress the generation of scale on a windward portion of the humidification element.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a humidification element and a scale inhibition method, and more particularly to a humidification element and a scale inhibition method used in an evaporative humidification device. [Background technology]

[0002] Conventionally, evaporative humidifiers have been known as humidifiers. Evaporative humidifiers place multiple humidifying elements containing water at intervals, and ventilate between the humidifying elements to evaporate the water and humidify the humidified space. This method has the advantage of consuming less power because humidification is controlled only by blowing air.

[0003] In an evaporative humidifier, for example, a suction method and a drip method are known as means for supplying water to the humidifying element. The suction method utilizes the capillary phenomenon of the humidifying element, and the bottom end of the humidifying element is immersed in water supplied to a water tank or the like, so that the water is sucked up into the humidifying element and hydrates the humidifying element. Meanwhile, the drip method sprays water from the top of the humidifying element to hydrate the humidifying element.

[0004] Fig. 1 is a schematic diagram showing an example of ventilation between humidifying elements 1 in an evaporative humidifier. In Fig. 1, multiple humidifying elements 1 are arranged at approximately equal intervals from one another and approximately parallel to the direction of ventilation. Air blown from the windward side of the humidifying elements 1 is humidified by being ventilated between the multiple humidifying elements, passes through the downwind side of the humidifying elements, and is sent to the space to be humidified.

[0005] In evaporative humidifiers, water constantly flows through the humidifying element. When the humidifying element is used for a long period of time, compounds containing elements such as calcium and magnesium in the water turn into scale and gradually adhere to the humidifying element. When this scale grows, it can be blown away by the air blown, causing the scale to scatter into the space being humidified. Furthermore, the formation of scale in the humidifying element has a negative effect on the humidifying performance of the humidifying element.

[0006] In an evaporative humidifier, moisture evaporates quickly and scale tends to accumulate particularly in the windward portion of the humidifier element 1. Therefore, the amount of scale generated is particularly large in the windward portion of the humidifier element 1.

[0007] As an evaporation filter that suppresses the adhesion of scale, there is known an evaporation filter that is a laminated assembly of one-sided cardboard made of water-absorbent filter material containing an antibacterial agent and an antifungal agent, and that carries a water-retentive material on the open cross section on the windward side of the laminated assembly (see, for example, Patent Document 1). According to this filter, by carrying a water-retentive material on the windward side, it is said that the evaporation filter can be prevented from drying out and the adhesion of scale can be suppressed, thereby maintaining humidification performance for a long period of time.

[0008] Also, in a filter equipped with a filter member having water absorption and air permeability, a filter is known which is equipped with a cover member which has water absorption and can absorb water from the filter member and which detachably covers at least a part of the filter member (for example, see Patent Document 2). According to this filter, since the cover member detachably covers the filter member, it is said that by replacing the cover member on which scale has adhered with a new cover member, the water absorption and air permeability of the filter can be maintained, and the humidifying performance of the humidifier can be maintained. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2011-196638 A [Patent Document 2] JP 2013-170803 A Summary of the Invention [Problem to be solved by the invention]

[0010] The techniques disclosed in the above Patent Documents 1 and 2 have the problem of high costs due to the need for special water retention agents and cover materials. Therefore, the main object of the present invention is to provide a humidifying element equipped with scale suppression means in the upwind portion of the humidifying element, which is completely different from the scale suppression means in conventional evaporative humidifiers. [Means for solving the problem]

[0011] As a result of intensive research by the present inventors to solve the above problems, it has been found that a humidifying element for use in an evaporative humidifying device includes a plate-shaped member formed of fibers, and the BET specific surface area of ​​the plate-shaped member is 0.35 m 2 / g or more 0.5m 2 / g or less, it has been found that the formation of scale on the windward side of the humidifier element can be suppressed. The present invention has been completed based on these findings and through further investigations.

[0012] That is, the present invention provides the following aspects. Item 1. A humidification element for use in an evaporative humidification device, the humidification element including a plate-shaped member formed of fibers, the plate-shaped member having a BET specific surface area of ​​0.35 m 2 / g or more 0.5m 2 / g or less. Item 2. The humidifying element according to item 1, wherein the humidifying element comprises silica particles on at least a portion of a surface of the fiber. Item 3. The humidifying element according to item 1 or 2, wherein the average diameter of the fibers is 15 μm or more and 20 μm or less. Item 4. The plate-like member has an apparent density of 0.2 g / cm3 More than 0.6g / cm 3 Item 4. The humidifying element according to any one of items 1 to 3, which is as follows: Item 5. The humidifying element according to any one of Items 1 to 4, wherein the porosity of the plate-like member is 50% or more and 80% or less. Item 6. A method for inhibiting scale, comprising using the humidifying element according to any one of items 1 to 5. Effect of the Invention

[0013] According to the humidifying element of the present invention, there is provided a humidifying element for use in an evaporative humidifying device, the humidifying element including a plate-shaped member formed of fibers, the plate-shaped member having a BET specific surface area of ​​0.35 m 2 / g or more 0.5m 2 / g or less, it is possible to suppress the generation of scale in the windward portion of the humidifier element. [Brief description of the drawings]

[0014] [Figure 1] FIG. 13 is a schematic diagram showing an example of ventilation between humidification elements in an evaporative humidifier. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The humidifying element of the present invention is a humidifying element for use in an evaporative humidifying device, the humidifying element comprising a plate-shaped member formed of fibers, the plate-shaped member having a BET specific surface area of ​​0.35 m 2 / g or more 0.5m 2 / g or less. Details are given below.

[0016] <Textile> The humidifying element of the present invention includes a plate-shaped member formed of fibers. As described below, for example, the humidifying element can be formed into the plate-shaped member by compression molding a nonwoven fabric made of fibers.

[0017] As the fibers, for example, organic fibers, inorganic fibers, or composite fibers combining these can be used. As the organic fibers, for example, polyester fibers such as polyethylene terephthalate, polyamide fibers, polyolefin fibers, cellulose fibers, etc. can be mentioned, and preferably polyester fibers. As the inorganic fibers, for example, glass fibers can be mentioned. Among these, it is preferable to use organic fibers having a melting point or softening point of 200°C or more. The fibers may be used alone or in combination of two or more types. In the present invention, the melting point or softening point means the endothermic peak temperature in differential scanning calorimetry (DSC).

[0018] In addition, the plate-shaped member preferably contains, as the fiber, a heat-fusible fiber that acts as a binder. Examples of the heat-fusible fiber include heat-fusible fibers formed of two or more polymer components having different melting points or softening points. A suitable example of the heat-fusible fiber is a composite fiber having a core-sheath structure in which a high-melting point polymer that is a non-heat-fusible component is a core component and a low-melting point polymer that is a heat-fusible component is a sheath component. Examples of the composite fiber having a core-sheath structure include composite fibers having a core made of polypropylene and a sheath made of modified polyethylene, composite fibers having a core made of polyethylene terephthalate and a sheath made of polyolefin, and composite fibers having a core made of polyethylene terephthalate and a sheath made of low-melting point polyester. These heat-fusible fibers may be used alone or in combination of two or more types. Here, the term "low melting point" refers to a property in which the melting point (Tm) measured by a differential scanning calorimeter (DSC) is about 160° C. or lower, preferably about 140° C. or lower, and the term "high melting point" refers to a property in which the melting point (Tm) measured by DSC is about 200° C. or higher, preferably about 220° C. or higher. The melting point or softening point of the heat-fusible component in the heat-fusible fiber is, for example, 80 to 130° C., preferably 100 to 120° C., and more preferably 110 to 120° C.

[0019] In particular, from the viewpoint of facilitating control of the porosity of the humidifying element and the apparent density of the plate-shaped member, which will be described later, it is preferable that the plate-shaped member contains, as fibers, fibers having a melting point or softening point of 200° C. or higher and heat-fusible fibers. In this case, the mass ratio of the fibers having a melting point or softening point of 200° C. or higher and the heat-fusible fibers in the plate-shaped member (mass of fibers having a melting point or softening point of 200° C. or higher / mass of heat-fusible fibers) is preferably 50 / 50 to 90 / 10, and more preferably 60 / 40 to 80 / 20.

[0020] The cross-sectional shape of the fibers forming the plate-like member is not particularly limited. For example, it may be circular. In addition, in order to easily increase the BET specific surface area of ​​the plate-like member, the cross-sectional shape of the fibers may be an irregular cross-sectional shape. Examples of the irregular cross-sectional shape include flat cross-sections, polygonal cross-sections such as approximately triangular, rectangular, and pentagonal cross-sections, wedge-shaped cross-sections, arrow-shaped cross-sections, and cross-sections in the shape of alphabetical characters such as approximately C-shaped, H-shaped, I-shaped, and W-shaped.

[0021] The average diameter of the fibers forming the plate-like member is preferably 10 to 25 μm, and more preferably 15 to 20 μm, from the viewpoint of increasing the BET specific surface area of ​​the plate-like member and improving the water diffusibility of the humidifying element. In the present invention, the average diameter of the fibers is calculated by randomly selecting 100 fibers and measuring the diameter (largest part) of each of the 100 fibers at any point in the longitudinal direction using a scanning electron microscope, and then calculating the average value.

[0022] The average fineness of the fibers forming the plate-like member is preferably 1 to 4 d (denier), and more preferably 2.5 to 4 d, from the viewpoint of increasing the BET specific surface area of ​​the plate-like member and improving the water diffusibility of the humidifying element. In the present invention, the average fineness can be calculated from the average diameter and the density of the fibers.

[0023] The average fiber length of the fibers forming the plate-like member is preferably 1 to 100 mm, more preferably 5 to 80 mm, from the viewpoint of increasing the BET specific surface area of ​​the plate-like member. In the present invention, the average fiber length of the fibers is determined by observing 100 arbitrarily selected fibers at a magnifying glass and an image analyzer at a magnification of 1000 times, measuring the fiber length of each fiber, and averaging the fiber lengths of these 100 fibers.

[0024] <Plate-shaped components> The humidifying element of the present invention includes a plate-shaped member formed of fibers. The plate-shaped member has many pores formed by gaps between the fibers, and typically has many continuous pores that penetrate from one side to the other side, and non-penetrating pores that do not connect from one side to the other side. Examples of continuous pores include those that bend and penetrate from one side to the other side by filling in the gaps between the constituent materials, and those that penetrate linearly from one side to the other side.

[0025] The plate-like member is preferably a fiber assembly obtained by compression molding a nonwoven fabric made of the above-mentioned fibers.

[0026] Examples of the nonwoven fabric include needle-punched nonwoven fabric, spunlace nonwoven fabric, wet-laid nonwoven fabric, etc. Among these, needle-punched nonwoven fabric is preferred from the viewpoint of making the nonwoven fabric bulky and increasing the internal surface area of ​​the plate-like member.

[0027] The humidifying element of the present invention has a plate-shaped member with a BET specific surface area of ​​0.35 m 2 / g or more 0.5m 2 / g or less. This makes it possible to suppress the generation of scale on the windward side of the humidifying element. From the viewpoint of achieving both the suppression of the generation of scale on the windward side of the humidifying element and the water diffusibility of the humidifying element, 2 / g or more 0.45m 2 / g or less. In the present invention, the BET specific surface area is a value calculated based on the nitrogen adsorption isotherm at 77.4K. Specifically, the nitrogen adsorption isotherm is created as follows. The sample to be measured is cooled to 77.4K (the boiling point of nitrogen), nitrogen gas is introduced, and the adsorption amount V [cc / g] of the nitrogen gas is measured by the volumetric method. At this time, the pressure P [hPa] of the introduced nitrogen gas is gradually increased, and the value divided by the saturated vapor pressure P0 [hPa] of the nitrogen gas is set as the relative pressure P / P0, and the adsorption amount for each relative pressure is plotted to create a nitrogen adsorption isotherm. The adsorption amount of nitrogen gas can be measured using a commercially available automatic gas adsorption amount measuring device (for example, the product name "AUTOSORB-1-MP" (manufactured by QUANTCHROME), etc.). In the present invention, the specific surface area is calculated according to the BET method based on the nitrogen adsorption isotherm. This analysis can be performed using known means such as an analysis program attached to the above device. When the humidifying element contains a plate-like member and a substance other than fibers, such as silica particles contained in at least a part of the surface of the plate-like member, the substance other than fibers is removed before the measurement. One method for removing the substance is to immerse the element in an alkaline aqueous solution with a pH of about 9 to 11 for 5 hours, rinse the element with water, and dry the element at 50°C for 12 hours.

[0028] In the humidifying element of the present invention, the mechanism by which the BET specific surface area of ​​the plate-shaped member is set within the above range to suppress the generation of scale on the windward side of the humidifying element is not necessarily clear, but it can be considered as follows, for example. That is, scale is formed when hardness components contained in the supply water are concentrated on the surface of the fibers constituting the humidifying element during drying, and precipitate and accumulate. Although the amount of scale generated varies depending on the portion of the humidifying element that dries easily, the amount of scale generated in the entire humidifying element is considered to depend on the amount of water retained in the humidifying element and the frequency of repeated drying and wetting. In this case, by increasing the surface area of ​​the fibers constituting the plate-shaped member, the amount of scale generated in the entire humidifying element does not change, but the amount of scale generated per unit area of ​​the fibers is reduced, that is, the scale is dispersed. It is considered that this effect reduces the amount of scale even in the windward portion, where scale is significantly generated.

[0029] Methods for adjusting the BET specific surface area of ​​the plate-like member include controlling the average diameter, average fineness, and cross-sectional shape of the fibers forming the plate-like member, and controlling the apparent density of the plate-like member, which will be described later.

[0030] The plate-shaped member has an apparent density of 0.2 g / cm 3 More than 0.6g / cm 3 It is preferable that the concentration is 0.3 g / cm or less. 3 More than 0.5g / cm 3 More preferably, it is 0.33 g / cm or less. 3 More than 0.5g / cm 3 It is more preferable that the apparent density is equal to or less than 50°C. This makes it easier to control the BET specific surface area and the porosity described below. In the present invention, the apparent density is calculated by drying the plate-shaped member at 50°C for 3 hours in a hot air dryer, cooling it to room temperature in a desiccator, weighing the mass, and multiplying the mass [g] by the volume [cm3] of the plate-shaped member. 3The apparent density of the plate-like member can be adjusted by controlling the average diameter, fineness, or cross-sectional shape of the fibers forming the plate-like member, or by controlling the basis weight of the nonwoven fabric and the thickness of the plate-like member when the nonwoven fabric is compressed.

[0031] The porosity of the plate-like member is preferably 50% or more and 80% or less, more preferably 60% or more and 75% or less, and even more preferably 60% or more and 70% or less. By setting it in such a range, the humidifying performance of the humidifying element is excellent, while the occurrence of scale in the windward portion of the humidifying element is more easily suppressed. In the present invention, the porosity of the plate-like member is the volume ratio of the pores to the total volume of the plate-like member expressed as a percentage, and is a value obtained by measuring as follows. That is, first, the dry weight W [g] and volume V [cm3] of the plate-like member are calculated. 3 ], and then measure the true specific gravity ρ [g / cm 3 ] can be measured and calculated according to the following formula.

[0032]

number

[0033] The true specific gravity of the plate-shaped member is ρ [g / cm 3 The density d [g / cm 2 ] can be measured as follows. That is, it can be measured by the pycnometer method, which is used to measure the density of fibers. First, a plate-shaped member to be used as a sample is dried at 50°C for 24 hours and its weight a [g] is measured. Next, the weight of the pycnometer is measured, and the sample is placed in it. ... 3 ] of replacement liquid (boiled distilled water or kerosene). If air bubbles have formed, degas them in a vacuum desiccator, then pour replacement liquid again up to the marked line. Measure the weight b [g] of the pycnometer in this state. Prepare an empty pycnometer separately, and pour only the replacement liquid up to the marked line. Measure the weight c [g] of the pycnometer in this state. From these measurement results, the true specific gravity can be calculated using the following formula. ρ=(a×d) / (c-b+a)

[0034] The thickness of the plate-like member (in the direction perpendicular to the wind direction in FIG. 1) is, for example, 0.5 to 10 mm. The height of the plate-like member (in the vertical direction of the paper in FIG. 1) is, for example, 30 to 300 mm. The length of the plate-like member (in the wind direction in FIG. 1) is, for example, 30 to 300 mm. The basis weight [g / m 2 ] is 100 to 3000 g / m 2 and 200 to 2000 g / m 2 is preferably 330 to 550 g / m 2 are more preferred.

[0035] <Humidification element> The humidifying element of the present invention includes a plate-shaped member made of fibers, and at least a portion of the surface of the plate-shaped member may contain materials other than fibers as long as the effects of the present invention are achieved.

[0036] The material contained in the humidifying element other than the fibers may be a material that improves the humidifying performance, such as silica particles. The primary particle diameter of the silica particles is about 1 to 300 nm, preferably about 1 to 100 nm. The primary particle diameter of the silica particles is a value obtained by converting the specific surface area measured by the nitrogen adsorption BET method of JIS Z 8830 2013 into the diameter of a spherical particle.

[0037] The content (mass %) of the silica particles relative to the mass of the humidifying element is 0.1 to 5.0 mass %, and preferably 0.2 to 2.0 mass %.

[0038] In addition, the humidifying element of the present invention may contain an antimicrobial agent as a substance other than the fibers. Known antibacterial agents and antifungal agents may be used as the antimicrobial agent. Specific examples of antibacterial agents include Irgasan (registered trademark, also known as Triclosan, IUPAC name: 5-chloro-2-[2,4-dichlorophenoxyl]phenol), chlorhexidine hydrochloride, zinc pyrithione (IUPAC name: bis(2-pyridylthio)zinc-1,1'-dioxide), and 2-bromo-2-nitropropane-1,3-diol. Specific examples of antifungal agents include 3-iodo-2-propynyl butylcarbamate, thiabendazole, fluorofolpet (IUPAC name: 2-(dichloro-fluoromethyl)sulfanylisoindole-1,3-dione), chloroxylenol, carbendazine, captan, chlorothalonil, and methylsulfonyltetrachlorpyridine. The antimicrobial agent may be used alone or in combination of two or more kinds. Also, an antibacterial agent may be used in combination with an antifungal agent.

[0039] The content (mass %) of the antimicrobial agent relative to the mass of the humidifying element is, for example, 0.01 to 1.0 mass %, and preferably 0.02 to 0.5 mass %.

[0040] In the humidifying element of the present invention, the content (mass %) of the material other than fibers contained in at least a portion of the surface of the plate-like member is 0.11 to 6.0 mass %, preferably 0.24 to 2.5 mass %.

[0041] <humidifier> The humidifying element of the present invention is applied to an evaporative humidifying device. Examples of the evaporative humidifying device include the above-mentioned suction type and drip type humidifying devices.

[0042] Fig. 1 is a schematic diagram showing an example of ventilation between humidifying elements 1 in an evaporative humidifier. As shown in Fig. 1, the humidifier preferably has a plurality of humidifying elements 1 arranged at substantially equal intervals so as to be substantially parallel to the direction of ventilation, and air blown from the upwind side of the humidifying elements 1 is humidified by being ventilated between the plurality of humidifying elements, passes through the downwind side of the humidifying elements, and is sent to a space to be humidified.

[0043] <Manufacturing method of humidifier element> A manufacturing method for a humidifying element of the present invention can include, for example, a step of preparing fibers that form a plate-shaped member, a step of preparing a nonwoven fabric using the fibers, and a step of compression molding the nonwoven fabric to form a plate-shaped member.

[0044] In the step of preparing the nonwoven fabric, the nonwoven fabric can be produced by a needle punch method, a spunlace method, a wet papermaking method, etc. In this case, the basis weight of the nonwoven fabric is 100 to 3,000 g / m 2 It is preferable that the thickness is 200 to 2,000 g / m 2 It is more preferable to set the above.

[0045] In the above-mentioned step of compression molding into a plate-like member, the heating temperature during compression molding may be appropriately set according to the melting point of the fibers. In particular, when the fibers forming the plate-like member include fibers having a melting point or softening point of 200° C. or more and heat-fusible fibers, the heating temperature is preferably in the range of not less than the melting point or softening point of the heat-fusible component of the heat-fusible fibers and not more than the melting point or softening point of the fibers having a melting point or softening point of 200° C. or more, specifically, for example, 160 to 190° C. The pressure during compression molding may be, for example, 10,000 to 30,000 kg / m. 2 Following the heat compression, the heat-fusible fiber is cooled and compressed at a temperature below the melting point or softening point of the heat-fusible component, specifically below 70° C., more preferably from 50° C. to 70° C., thereby fixing the shape such as thickness, ensuring the strength of the plate-like member, and stabilizing the BET specific surface area of ​​the plate-like member.

[0046] In addition, the manufacturing method of the humidifying element of the present invention may include a step of attaching a substance other than fibers to at least a part of the surface of the plate-shaped member, if necessary. For example, when silica particles and an antimicrobial agent are contained as the substance other than fibers, an immersion step can be performed in which the plate-shaped member is immersed in a dispersion in which the silica particles and the antimicrobial agent are dispersed in a polar organic solvent. The polar organic solvent used in the immersion step is not particularly limited as long as it can disperse the silica particles and the antimicrobial agent, but from the viewpoint of excellent dispersibility of the silica particles and the antimicrobial agent and highly uniformly attaching the silica particles to the entire plate-shaped member in a state in which the antimicrobial agent is supported on the silica particles, lower alcohols having about 1 to 6 carbon atoms, acetone, diethyl ether, etc. are preferred, and among these, methanol and isopropyl alcohol (IPA) are particularly preferred. By using these polar solvents, it is possible to uniformly support the silica particles even inside the plate-shaped member, and it is also possible to incorporate the antimicrobial agent inside the aggregates formed by the silica particles, so that a humidifying element can be obtained that can maintain high antimicrobial properties for a long period of time and has excellent water absorption. The polar organic solvent may be used alone, or in combination with two or more kinds, or may be used by mixing with water. In the immersion step, the concentration of the silica particles contained in the polar organic solvent may be, for example, about 1 to 30 mass %. The concentration of the antimicrobial agent may be, for example, about 0.1 to 10 mass %.

[0047] Next, a drying step is performed to dry the plate-like member immersed in the immersion step. The drying step can be performed by lifting the plate-like member from the dispersion and drying the polar organic solvent. There are no particular limitations on the method for drying the polar organic solvent, but for example, a centrifuge, a roll press, or the like is used to squeeze the immersed porous substrate so that the squeeze rate of the dispersion is about 10 to 150 mass%, and then the substrate is dried in a dryer at a temperature of about 40 to 60° C. for about 3 to 15 hours. EXAMPLES

[0048] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the examples.

[0049] <Example 1> (1) A step of preparing fibers that form a plate-shaped member We prepared polyethylene terephthalate staple fibers (melting point 255°C) with a fineness of 3d (denier) and a fiber length of 51 mm, and core-sheath type composite staple fibers with a fineness of 4d and a fiber length of 51 mm, with a core made of polyethylene terephthalate (melting point 255°C) and a sheath made of a polyethylene terephthalate / isophthalate copolymer with a melting point of 110°C.

[0050] (2) A process for preparing a nonwoven fabric using the fibers The polyethylene terephthalate staple fiber was mixed with the core-sheath composite staple fiber in a ratio of 70 parts by mass and 30 parts by mass, totaling 100 parts by mass, and carded to form a web. The web was needle-punched, heat-treated at an atmospheric temperature of 180°C, and cooled to obtain a needle-punched nonwoven fabric. The nonwoven fabric had a basis weight of 350 g / m 2 , and the thickness was 3.0 mm.

[0051] (3) A process of compressing and molding the nonwoven fabric into a plate-shaped component The nonwoven fabric was heated in a press at 170°C and 2.0 kg / cm 2 Heat and press for 8 minutes at 60°C and 2.0 kg / cm 2 The plate was cooled and pressed at 40° C. for 8 minutes to obtain a partially fused plate member having a thickness of 1.0 mm. The BET specific surface area of ​​the plate member was 0.38 m 2 The average diameter of the fibers forming the plate-like member was 18 μm, the average fineness was 3.3 d, the average fiber length was 51 mm, and the apparent density was 0.35 g / cm 3 , porosity 68%, basis weight 350g / m 2 The length of the plate-like member (in the wind direction in FIG. 1) was 100 mm, and its height (in the vertical direction on the paper in FIG. 1) was 150 mm.

[0052] (4) A step of attaching silica particles and an antimicrobial agent to at least a part of the surface of a plate-like member Next, the obtained plate-like member was impregnated with a dispersion liquid having the following formulation 1, and squeezed to a squeezing rate of 50% by mass using a centrifuge, and then dried for 12 hours in a dryer with an atmospheric temperature of 50°C to obtain a humidifying element. The content of colloidal silica in the humidifying element was 0.6% by mass. The total content of Irgasan and 3-iodo-2-propynyl butylcarbamate in the humidifying element was 0.12% by mass.

[0053] (Formulation 1) Colloidal silica (primary particle diameter 10 nm): 4.0 mass% Irgasan: 0.5% by mass 3-iodo-2-propynyl butylcarbamate: 0.5% by mass Isopropyl alcohol (IPA): Remainder

[0054] <Example 2> (1) A step of preparing fibers that form a plate-shaped member We prepared polyethylene terephthalate staple fibers (melting point 255°C) with a fineness of 3d (denier) and a fiber length of 51 mm, and core-sheath type composite staple fibers with a fineness of 2d and a fiber length of 51 mm, with a core made of polyethylene terephthalate (melting point 255°C) and a sheath made of polyethylene terephthalate / isophthalate copolymer with a melting point of 110°C.

[0055] (2) A process for preparing a nonwoven fabric using the fibers The polyethylene terephthalate staple fiber was mixed with the core-sheath composite staple fiber in a ratio of 80 parts by mass and 20 parts by mass, totaling 100 parts by mass, and carded to form a web. The web was then needle-punched, heat-treated at an atmospheric temperature of 180°C, and cooled to obtain a needle-punched nonwoven fabric. The nonwoven fabric had a basis weight of 450 g / m 2 , and the thickness was 3.0 mm.

[0056] (3) A process of compressing and molding the nonwoven fabric into a plate-shaped component The nonwoven fabric was heated in a press at 170°C and 2.0 kg / cm 2Heat and press for 8 minutes at 60°C and 2.0 kg / cm 2 The plate was cooled and pressed at 40° C. for 8 minutes to obtain a partially fused plate member having a thickness of 1.0 mm. The BET specific surface area of ​​the plate member was 0.43 m 2 The average diameter of the fibers forming the plate-like member was 17 μm, the average fineness was 2.8 d, the average fiber length was 51 mm, and the apparent density was 0.45 g / cm 3 , porosity 63%, basis weight 450g / m 2 The length of the plate-like member (in the wind direction in FIG. 1) was 100 mm, and its height (in the vertical direction on the paper in FIG. 1) was 150 mm.

[0057] (4) A step of attaching silica particles and an antimicrobial agent to at least a part of the surface of a plate-like member Next, the obtained plate-like member was impregnated with the dispersion liquid of Formulation 1, and squeezed to a squeezing rate of 50% by mass using a centrifuge, and then dried for 12 hours in a dryer with an atmospheric temperature of 50°C to obtain a humidifying element. The content of colloidal silica in the humidifying element was 1.0% by mass. The total content of Irgasan and 3-iodo-2-propynyl butylcarbamate in the humidifying element was 0.2% by mass.

[0058] <Example 3> (1) A step of preparing fibers for forming a plate-shaped member We prepared polyethylene terephthalate staple fibers (melting point 255°C) with a fineness of 3d (denier) and a fiber length of 51 mm, and core-sheath type composite staple fibers with a fineness of 4d and a fiber length of 51 mm, with a core made of polyethylene terephthalate (melting point 255°C) and a sheath made of a polyethylene terephthalate / isophthalate copolymer with a melting point of 110°C.

[0059] (2) A process for preparing a nonwoven fabric using the fibers The polyethylene terephthalate staple fiber was mixed with the core-sheath composite staple fiber in a ratio of 80 parts by mass and 20 parts by mass, totaling 100 parts by mass, and carded to form a web. The web was then needle-punched, heat-treated at an atmospheric temperature of 180°C, and cooled to obtain a needle-punched nonwoven fabric. The nonwoven fabric had a basis weight of 450 g / m 2, and the thickness was 3.0 mm.

[0060] (3) A process of compressing and molding the nonwoven fabric into a plate-shaped component The nonwoven fabric was heated in a press at 170°C and 2.0 kg / cm 2 Heat and press for 8 minutes at 60°C and 2.0 kg / cm 2 The plate was cooled and pressed at 40° C. for 8 minutes to obtain a partially fused plate member having a thickness of 1.0 mm. The BET specific surface area of ​​the plate member was 0.40 m 2 The average diameter of the fibers forming the plate-like member was 18 μm, the average fineness was 3.2d, the average fiber length was 51 mm, and the apparent density was 0.45 g / cm 3 , porosity 65%, basis weight 450g / m 2 The length of the plate-like member (in the wind direction in FIG. 1) was 100 mm, and its height (in the vertical direction on the paper in FIG. 1) was 150 mm.

[0061] (4) A step of attaching silica particles and an antimicrobial agent to at least a part of the surface of a plate-like member Next, the obtained plate-like member was impregnated with the dispersion liquid of Formulation 1, and squeezed to a squeezing rate of 50% by mass using a centrifuge, and then dried for 12 hours in a dryer with an atmospheric temperature of 50°C to obtain a humidifying element. The content of colloidal silica in the humidifying element was 1.0% by mass. The total content of Irgasan and 3-iodo-2-propynyl butylcarbamate in the humidifying element was 0.20% by mass.

[0062] <Example 4> (1) A step of preparing fibers for forming a plate-shaped member We prepared polyethylene terephthalate staple fibers (melting point 255°C) with a fineness of 3d (denier) and a fiber length of 51 mm, and core-sheath type composite staple fibers with a fineness of 4d and a fiber length of 51 mm, with a core made of polyethylene terephthalate (melting point 255°C) and a sheath made of a polyethylene terephthalate / isophthalate copolymer with a melting point of 110°C.

[0063] (2) A process for preparing a nonwoven fabric using the fibers The polyethylene terephthalate staple fiber was mixed with the core-sheath composite staple fiber in a ratio of 60 parts by mass and 40 parts by mass, totaling 100 parts by mass, and carded to form a web. The web was then needle-punched, heat-treated at an atmospheric temperature of 180°C, and cooled to obtain a needle-punched nonwoven fabric. The nonwoven fabric had a basis weight of 300 g / m 2 , and the thickness was 3.0 mm.

[0064] (3) A process of compressing and molding the nonwoven fabric into a plate-shaped component The nonwoven fabric was heated in a press at 170°C and 2.0 kg / cm 2 Heat and press for 8 minutes at 60°C and 2.0 kg / cm 2 The plate was cooled and pressed at 40° C. for 8 minutes to obtain a partially fused plate member having a thickness of 1.0 mm. The BET specific surface area of ​​the plate member was 0.39 m 2 The average diameter of the fibers forming the plate-like member was 18 μm, the average fineness was 3.4d, the average fiber length was 51 mm, and the apparent density was 0.30 g / cm 3 , porosity 72%, basis weight 300g / m 2 The length of the plate-like member (in the wind direction in FIG. 1) was 100 mm, and its height (in the vertical direction on the paper in FIG. 1) was 150 mm.

[0065] (4) A step of attaching silica particles and an antimicrobial agent to at least a part of the surface of a plate-like member Next, the obtained plate-like member was impregnated with the dispersion liquid of Formulation 1, and squeezed to a squeezing rate of 50% by mass using a centrifuge, and then dried for 12 hours in a dryer with an atmospheric temperature of 50°C to obtain a humidifying element. The content of colloidal silica in the humidifying element was 0.6% by mass. The total content of Irgasan and 3-iodo-2-propynyl butylcarbamate in the humidifying element was 0.12% by mass.

[0066] <Example 5> (1) A step of preparing fibers for forming a plate-shaped member We prepared polyethylene terephthalate staple fibers (melting point 255°C) with a fineness of 3d (denier) and a fiber length of 51 mm, and core-sheath type composite staple fibers with a fineness of 4d and a fiber length of 51 mm, with a core made of polyethylene terephthalate (melting point 255°C) and a sheath made of a polyethylene terephthalate / isophthalate copolymer with a melting point of 110°C.

[0067] (2) A process for preparing a nonwoven fabric using the fibers The polyethylene terephthalate staple fiber and the core-sheath composite staple fiber were mixed in a ratio of 80 parts by mass and 20 parts by mass, totaling 100 parts by mass, and carded to form a web. The web was needle-punched, heat-treated at an atmospheric temperature of 180°C, and cooled to obtain a needle-punched nonwoven fabric. The nonwoven fabric had a basis weight of 350 g / m 2 , and the thickness was 3.0 mm.

[0068] (3) A process of compressing and molding the nonwoven fabric into a plate-shaped component The nonwoven fabric was heated in a press at 170°C and 2.0 kg / cm 2 Heat and press for 8 minutes at 60°C and 2.0 kg / cm 2 The plate was cooled and pressed at 40° C. for 8 minutes to obtain a partially fused plate member having a thickness of 1.0 mm. The BET specific surface area of ​​the plate member was 0.40 m 2 The average diameter of the fibers forming the plate-like member was 18 μm, the average fineness was 3.2d, the average fiber length was 51 mm, and the apparent density was 0.35 g / cm 3 , porosity 69%, basis weight 350g / m 2 The length of the plate-like member (in the wind direction in FIG. 1) was 100 mm, and its height (in the vertical direction on the paper in FIG. 1) was 150 mm.

[0069] (4) Step of attaching silica particles and an antimicrobial agent to at least a part of the surface of the plate-like member Next, the obtained plate-like member was impregnated with the dispersion liquid of Formulation 1, and squeezed to a squeezing rate of 50% by mass using a centrifuge, and then dried for 12 hours in a dryer with an atmospheric temperature of 50°C to obtain a humidifying element. The content of colloidal silica in the humidifying element was 2.0% by mass. The total content of Irgasan and 3-iodo-2-propynyl butylcarbamate in the humidifying element was 0.20% by mass.

[0070] <Example 6> (1) A step of preparing fibers for forming a plate-shaped member We prepared polyethylene terephthalate staple fibers (melting point 255°C) with a fineness of 2d (denier) and fiber length BR>T1mm, and core-sheath type composite staple fibers with a fineness of 2d and fiber length of 51mm, with a core of polyethylene terephthalate (melting point 255°C) and a sheath of polyethylene terephthalate / isophthalate copolymer with a melting point of 110°C.

[0071] (2) A process for preparing a nonwoven fabric using the fibers The polyethylene terephthalate staple fiber and the core-sheath composite staple fiber were mixed in a ratio of 80 parts by mass and 20 parts by mass, totaling 100 parts by mass, and carded to form a web. The web was needle-punched, heat-treated at an atmospheric temperature of 180°C, and cooled to obtain a needle-punched nonwoven fabric. The nonwoven fabric had a basis weight of 350 g / m 2 , and the thickness was 3.0 mm.

[0072] (3) A process of compressing and molding the nonwoven fabric into a plate-shaped component The nonwoven fabric was heated in a press at 170°C and 2.0 kg / cm 2 Heat and press for 8 minutes at 60°C and 2.0 kg / cm 2 The plate was cooled and pressed at 40° C. for 8 minutes to obtain a partially fused plate member having a thickness of 1.0 mm. The BET specific surface area of ​​the plate member was 0.50 m 2 The average diameter of the fibers forming the plate-like member was 14 μm, the average fineness was 2d, the average fiber length was 51 mm, and the apparent density was 0.35 g / cm 3, porosity 68%, basis weight 350g / m 2 The length of the plate-like member (in the wind direction in FIG. 1) was 100 mm, and its height (in the vertical direction on the paper in FIG. 1) was 150 mm.

[0073] (4) Step of attaching silica particles and an antimicrobial agent to at least a part of the surface of the plate-like member Next, the obtained plate-like member was impregnated with the dispersion liquid of Formulation 1, and squeezed to a squeezing rate of 50% by mass using a centrifuge, and then dried for 12 hours in a dryer with an atmospheric temperature of 50°C to obtain a humidifying element. The content of colloidal silica in the humidifying element was 2.4% by mass. The total content of Irgasan and 3-iodo-2-propynyl butylcarbamate in the humidifying element was 0.24% by mass.

[0074] <Comparative Example 1> (1) A step of preparing fibers for forming a plate-shaped member We prepared polyethylene terephthalate staple fibers (melting point 255°C) with a fineness of 10d (denier) and a fiber length of 64 mm, and core-sheath type composite staple fibers with a fineness of 4d and a fiber length of 51 mm, with a core made of polyethylene terephthalate (melting point 255°C) and a sheath made of a polyethylene terephthalate / isophthalate copolymer with a melting point of 110°C.

[0075] (2) A process for preparing a nonwoven fabric using the fibers The polyethylene terephthalate staple fiber was mixed with the core-sheath composite staple fiber in a ratio of 80 parts by mass and 20 parts by mass, totaling 100 parts by mass, and carded to form a web. The web was then needle-punched, heat-treated at an atmospheric temperature of 180°C, and cooled to obtain a needle-punched nonwoven fabric. The nonwoven fabric had a basis weight of 450 g / m 2 , and the thickness was 3.0 mm.

[0076] (3) A process of compressing and molding the nonwoven fabric into a plate-shaped component The nonwoven fabric was heated at 170°C and 2 kg / cm in a heat press molding machine. 2 Heat and press for 8 minutes at 60°C and 2.0 kg / cm 2The plate was cooled and pressed at 40° C. for 8 minutes to obtain a partially fused plate member having a thickness of 1.0 mm. The BET specific surface area of ​​the plate member was 0.25 m 2 The average diameter of the fibers forming the plate-like member was 28 μm, the average fineness was 8.8 d, the average fiber length was 58 mm, and the apparent density was 0.45 g / cm 3 , porosity 61%, basis weight 450g / m 2 The length of the plate-like member (in the wind direction in FIG. 1) was 100 mm, and its height (in the vertical direction on the paper in FIG. 1) was 150 mm.

[0077] (4) A step of attaching silica particles and an antimicrobial agent to at least a part of the surface of the plate-like member Next, the obtained plate-like member was impregnated with the dispersion liquid of the above-mentioned formulation 1, and squeezed to a squeezing rate of 50 mass% using a centrifuge, and then dried for 12 hours in a dryer with an atmospheric temperature of 60°C to obtain a humidifying element. The content of colloidal silica in the humidifying element was 0.6 mass%. The total content of Irgasan and 3-iodo-2-propynyl butylcarbamate in the humidifying element was 0.12 mass%.

[0078] <Comparative Example 2> (1) A step of preparing fibers for forming a plate-shaped member We prepared polyethylene terephthalate staple fibers (melting point 255°C) with a fineness of 10d (denier) and a fiber length of 64 mm, and core-sheath type composite staple fibers with a fineness of 4d and a fiber length of 51 mm, with a core made of polyethylene terephthalate (melting point 255°C) and a sheath made of a polyethylene terephthalate / isophthalate copolymer with a melting point of 110°C.

[0079] (2) A process for preparing a nonwoven fabric using the fibers The polyethylene terephthalate staple fiber was mixed with the core-sheath composite staple fiber in a ratio of 70 parts by mass and 30 parts by mass, totaling 100 parts by mass, and carded to form a web. The web was then needle-punched, heat-treated at an atmospheric temperature of 180°C, and cooled to obtain a needle-punched nonwoven fabric. The nonwoven fabric had a basis weight of 350 g / m 2 , and the thickness was 3.0 mm.

[0080] (3) A process of compressing and molding the nonwoven fabric into a plate-shaped component The nonwoven fabric was heated at 170°C and 2 kg / cm in a heat press molding machine. 2 Heat and press for 8 minutes at 60°C and 2.0 kg / cm 2 The plate was cooled and pressed at 40° C. for 8 minutes to obtain a partially fused plate member having a thickness of 1.0 mm. The BET specific surface area of ​​the plate member was 0.26 m 2 The average diameter of the fibers forming the plate-like member was 26 μm, the average fineness was 8.2d, the average fiber length was 57 mm, and the apparent density was 0.35 g / cm 3 , porosity 67%, basis weight 350g / m 2 The length of the plate-like member (in the wind direction in FIG. 1) was 100 mm, and its height (in the vertical direction on the paper in FIG. 1) was 150 mm.

[0081] (4) A step of attaching silica particles and an antimicrobial agent to at least a part of the surface of the plate-like member Next, the obtained plate-like member was impregnated with the dispersion liquid of the above-mentioned formulation 1, and squeezed to a squeezing rate of 50 mass% using a centrifuge, and then dried for 12 hours in a dryer with an atmospheric temperature of 60°C to obtain a humidifying element. The content of colloidal silica in the humidifying element was 0.6 mass%. The total content of Irgasan and 3-iodo-2-propynyl butylcarbamate in the humidifying element was 0.12 mass%.

[0082] <Comparative Example 3> (1) A step of preparing fibers that form a plate-shaped member We prepared polyethylene terephthalate staple fibers (melting point 255°C) with a fineness of 10d (denier) and a fiber length of 64 mm, and core-sheath type composite staple fibers with a fineness of 4d and a fiber length of 51 mm, with a core made of polyethylene terephthalate (melting point 255°C) and a sheath made of a polyethylene terephthalate / isophthalate copolymer with a melting point of 110°C.

[0083] (2) A process for preparing a nonwoven fabric using the fibers The polyethylene terephthalate staple fiber was mixed in a ratio of 80 parts by mass and the core-sheath type composite staple fiber in a ratio of 20 parts by mass, totaling 100 parts by mass, and carded to form a web. The web was needle-punched, heat-treated at an atmospheric temperature of 180°C, and cooled to obtain a needle-punched nonwoven fabric. The nonwoven fabric had a basis weight of 300 g / m 2 , and the thickness was 3.0 mm.

[0084] (3) A process of compressing and molding the nonwoven fabric into a plate-shaped component The nonwoven fabric was heated at 170°C and 2 kg / cm in a heat press molding machine. 2 Heat and press for 8 minutes at 60°C and 2.0 kg / cm 2 The plate was cooled and pressed at 40° C. for 8 minutes to obtain a partially fused plate member having a thickness of 1.0 mm. The BET specific surface area of ​​the plate member was 0.25 m 2 The average diameter of the fibers forming the plate-like member was 28 μm, the average fineness was 8.8 d, the average fiber length was 58 mm, and the apparent density was 0.30 g / cm 3 , porosity 68%, basis weight 300g / m 2 The length of the plate-like member (in the wind direction in FIG. 1) was 100 mm, and its height (in the vertical direction on the paper in FIG. 1) was 150 mm.

[0085] (4) A step of attaching silica particles and an antimicrobial agent to at least a part of the surface of the plate-like member Next, the obtained plate-like member was impregnated with the dispersion liquid of the above-mentioned formulation 1, and squeezed to a squeezing rate of 50 mass% using a centrifuge, and then dried for 12 hours in a dryer with an atmospheric temperature of 60°C to obtain a humidifying element. The content of colloidal silica in the humidifying element was 0.6 mass%. The total content of Irgasan and 3-iodo-2-propynyl butylcarbamate in the humidifying element was 0.12 mass%.

[0086] <Comparative Example 4> (1) A step of preparing fibers that form a plate-shaped member We prepared polyethylene terephthalate staple fibers (melting point 255°C) with a fineness of 10d (denier) and fiber length of 64 mm, and core-sheath type composite staple fibers with a fineness of 2d and fiber length of 51 mm, with a core made of polyethylene terephthalate (melting point 255°C) and a sheath made of polyethylene terephthalate / isophthalate copolymer with a melting point of 110°C.

[0087] (2) A process for preparing a nonwoven fabric using the fibers The polyethylene terephthalate staple fiber was mixed with the core-sheath composite staple fiber in a ratio of 80 parts by mass and 20 parts by mass, totaling 100 parts by mass, and carded to form a web. The web was then needle-punched, heat-treated at an atmospheric temperature of 180°C, and cooled to obtain a needle-punched nonwoven fabric. The nonwoven fabric had a basis weight of 450 g / m 2 , and the thickness was 3.0 mm.

[0088] (3) A process of compressing and molding the nonwoven fabric into a plate-shaped component The nonwoven fabric was heated at 170°C and 2 kg / cm in a heat press molding machine. 2 Heat and press for 8 minutes at 60°C and 2.0 kg / cm 2 The plate was cooled and pressed at 40° C. for 8 minutes to obtain a partially fused plate member having a thickness of 1.0 mm. The BET specific surface area of ​​the plate member was 0.28 m 2 The average diameter of the fibers forming the plate-like member was 22 μm, the average fineness was 8.4d, the average fiber length was 56 mm, and the apparent density was 0.45 g / cm 3 , porosity 58%, basis weight 450g / m 2 The length of the plate-like member (in the wind direction in FIG. 1) was 100 mm, and its height (in the vertical direction on the paper in FIG. 1) was 150 mm.

[0089] (4) A step of attaching silica particles and an antimicrobial agent to at least a part of the surface of the plate-like member Next, the obtained plate-like member was impregnated with the dispersion liquid of the above-mentioned formulation 1, and squeezed to a squeezing rate of 50 mass% using a centrifuge, and then dried for 12 hours in a dryer with an atmospheric temperature of 60°C to obtain a humidifying element. The content of colloidal silica in the humidifying element was 0.7 mass%. The total content of Irgasan and 3-iodo-2-propynyl butylcarbamate in the humidifying element was 0.14 mass%.

[0090] <Comparative Example 5> (1) A step of preparing fibers for forming a plate-shaped member We prepared polyethylene terephthalate staple fibers (melting point 255°C) with a fineness of 6d (denier) and fiber length of 64 mm, and core-sheath type composite staple fibers with a fineness of 4d and fiber length of 51 mm, with a core of polyethylene terephthalate (melting point 255°C) and a sheath of polyethylene terephthalate / isophthalate copolymer with a melting point of 110°C.

[0091] (2) A process for preparing a nonwoven fabric using the fibers The polyethylene terephthalate staple fiber and the core-sheath composite staple fiber were mixed in a ratio of 80 parts by mass and 20 parts by mass, totaling 100 parts by mass, and carded to form a web. The web was needle-punched, heat-treated at an atmospheric temperature of 180°C, and cooled to obtain a needle-punched nonwoven fabric. The nonwoven fabric had a basis weight of 350 g / m 2 , and the thickness was 3.0 mm.

[0092] (3) A process of compressing and molding the nonwoven fabric into a plate-shaped component The nonwoven fabric was heated at 170°C and 2 kg / cm in a heat press molding machine. 2 Heat and press for 8 minutes at 60°C and 2.0 kg / cm 2 The plate was cooled and pressed at 40° C. for 8 minutes to obtain a partially fused plate member having a thickness of 1.0 mm. The BET specific surface area of ​​the plate member was 0.33 m 2 The average diameter of the fibers forming the plate-like member was 20 μm, the average fineness was 5.6 d, the average fiber length was 58 mm, and the apparent density was 0.35 g / cm 3, porosity 67%, basis weight 350g / m 2 The length of the plate-like member (in the wind direction in FIG. 1) was 100 mm, and its height (in the vertical direction on the paper in FIG. 1) was 150 mm.

[0093] (4) A step of attaching silica particles and an antimicrobial agent to at least a part of the surface of the plate-like member Next, the obtained plate-like member was impregnated with the dispersion liquid of the above-mentioned formulation 1, and squeezed to a squeezing rate of 50 mass% using a centrifuge, and then dried for 12 hours in a dryer with an atmospheric temperature of 60°C to obtain a humidifying element. The content of colloidal silica in the humidifying element was 0.8 mass%. The total content of Irgasan and 3-iodo-2-propynyl butylcarbamate in the humidifying element was 0.16 mass%.

[0094] <Evaluation method> (1) Amount of scale generated on the windward side of the humidifier element The weight of scale generated was measured for the plate-like members produced in the examples and comparative examples by the following wet-dry cycle test. First, an air conditioner was used to blow air adjusted to a temperature of 40°C, a relative humidity of 10% to 30%, and an air speed of 1.5 m / s to 2.2 m / s in the length direction of the plate-like member (wind direction in FIG. 1). Next, a mixed aqueous solution containing 1.68 g / L of sodium bicarbonate and 1.47 g / L of calcium chloride dihydrate was prepared and supplied to the upper end and center of the length direction of the plate-like member at a rate of 3 mL per minute from a tube with an inner diameter of 4 mm using a water pump. 10 minutes after the start of supply, the supply of the mixed aqueous solution was stopped, and the state of only blowing air was maintained for 110 minutes. This operation for a total of 120 minutes was defined as one cycle, and this was repeated 25 times. After this wet-dry cycle test, the scale that had formed on the windward side was scraped off 10 times with tweezers from the end face and up to 5 mm in the longitudinal direction from the end face, and the weight was measured. The total weight of the measurements for the 20 humidifying elements was taken as the amount of scale formed on the windward side of the humidifying elements.

[0095] (2) Overall amount of scale generated in the humidifier element The weight of the plate-shaped member was measured before and after the repeated wet-dry test in (1), and the difference was recorded as the amount of scale generated in the humidifying element. The total amount of scale generated in the humidifying element for the 20 plate-shaped members was recorded as the total amount of scale generated in the humidifying element.

[0096] (3) Water diffusibility Water was supplied to the upper end and longitudinal center of the plate-like member from a tube with an inner diameter of 4 mm using a water pump at a rate of 5 mL per minute, and the state of the water diffusing toward the lower end of the plate-like member was observed. If the water diffused concentrically from the supply point, it was evaluated as ○, and if there was a part where the water did not diffuse concentrically from the supply point, it was evaluated as ×.

[0097] The results of each example are shown in Table 1.

[0098] [Table 1]

[0099] The humidifying elements of Examples 1 to 6 are humidifying elements used in an evaporative humidifier, and the humidifying elements include a plate-shaped member formed of fibers, and the BET specific surface area of ​​the plate-shaped member is 0.35 m 2 / g or more 0.5m 2 / g or less, it was possible to suppress the generation of scale in the upwind portion of the humidifier element.

[0100] In particular, the humidifying elements of Examples 1 to 5 have a BET specific surface area of ​​the plate-shaped member of 0.35 m 2 / g or more 0.45m 2 / g or less, it was possible to suppress the generation of scale on the windward side of the humidifier element while improving the water diffusivity of the humidifier element.

[0101] Furthermore, the humidifier elements of Examples 1 to 3, 5 and 6 had a porosity of 60 to 70%, which made it even easier to suppress scale generation in the upwind portion of the humidifier element.

[0102] On the other hand, in Comparative Examples 1 to 5, the BET specific surface area of ​​the plate-like member was 0.35 m 2 / g, it was not possible to suppress the generation of scale in the windward portion of the humidifier element.

Claims

1. A humidification element for use in an evaporative humidification device, comprising: The humidifying element includes a plate-like member formed of fibers, The BET specific surface area of ​​the plate-like member is 0.35 m 2 / g or more 0.5m 2 / g or less.

2. The humidifier element of claim 1 , wherein the humidifier element comprises silica particles on at least a portion of a surface of the fibers.

3. 3. The humidifying element according to claim 1, wherein the average diameter of the fibers is 15 μm or more and 20 μm or less.

4. The apparent density of the plate-like member is 0.2 g / cm 3 0.6g / cm or more 3 The humidifying element according to any one of claims 1 to 3, wherein:

5. The humidifying element according to any one of claims 1 to 4, wherein the porosity of the plate-like member is 50% or more and 80% or less.

6. A method for inhibiting scale, comprising using the humidifying element according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Vaporization filter

    JP2011196638A

  • Filter and humidifier

    JP2013170803A