Metal-clad laminate, printed wiring board and semiconductor package as well as producing method thereof
By controlling the thickness ratios and surface waviness of prepreg layers in the lamination process, the method addresses the challenges of thickness accuracy and warpage variations in metal-clad laminates and semiconductor packages, resulting in improved performance.
Patent Information
- Application Number
- JP2024118379
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-12-07
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-11
AI Technical Summary
Existing methods for manufacturing metal-clad laminates and semiconductor packages struggle to achieve the required thickness accuracy and uniformity of dimensional change, particularly when using fiber base materials with a thickness of 40 μm or more, and fail to reduce variations in warpage.
A method involving the lamination of prepreg and metal foil by heating and pressurizing, where the prepreg consists of a thermosetting resin composition and a fiber base material with specific thickness and resin layer ratios, and surface waviness is controlled to improve thickness accuracy and uniformity.
The method results in metal-clad laminates with enhanced thickness accuracy and reduced variations in dimensional change, leading to improved performance in printed wiring boards and semiconductor packages.
Smart Images

Figure 2024144549000001_ABST
Abstract
Description
[Technical field]
[0001] The present embodiment relates to a metal-clad laminate, a printed wiring board, and a semiconductor package, and methods for manufacturing these. [Background technology]
[0002] In recent years, electronic devices have become smaller, lighter, and more functional, and semiconductor devices mounted on the electronic devices are becoming more highly integrated. Accordingly, higher quality is being required for metal-clad laminates, semiconductor packages, and the like used in printed wiring boards.
[0003] For example, metal-clad laminates are required to have higher thickness accuracy than ever before in order to increase the productivity of the resulting printed wiring boards. In addition, metal-clad laminates may be subjected to various treatments such as heat treatment and chemical treatment, and it is required that the amount of dimensional change caused by these treatments does not vary between products. Furthermore, for semiconductor packages, there is a demand to reduce the variation in the amount of warpage between products more than ever before.
[0004] Patent Document 1 describes a method for producing a prepreg by immersing a substrate in a resin liquid and then drying it, characterized in that the prepreg is pressed with a roll during or after the drying process to crush convex resin protrusions that occur on the prepreg surface, thereby improving the smoothness of the surface. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 01-272416 Summary of the Invention [Problem to be solved by the invention]
[0006] The technology of Patent Document 1 aims to improve the smoothness by mechanically pressing the surface of the prepreg. However, as described above, there has been remarkable progress in the high integration of semiconductor devices, and it is difficult to achieve the recently required level of thickness precision of metal-clad laminates using the technology of Patent Document 1. Moreover, the technology of Patent Document 1 does not solve the problems of uniforming the amount of dimensional change of metal-clad laminates and reducing the variation in the amount of warpage of semiconductor packages. In particular, the inventors' research has revealed that when the thickness of the fiber base material used in the prepreg is 40 μm or more, it becomes even more difficult to improve the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate, and to reduce variation in the amount of warping of the semiconductor package.
[0007] In view of the current situation, the present embodiment has an objective of providing a method for manufacturing a metal-clad laminate that has excellent thickness accuracy and uniformity of dimensional change even when a fiber base material with a thickness of 40 μm or more is used, a method for manufacturing a printed wiring board and a semiconductor package that use the metal-clad laminate, and a metal-clad laminate that can reduce variation in the amount of warping of a semiconductor package even when a fiber base material with a thickness of 40 μm or more is used, and a printed wiring board and a semiconductor package that have the metal-clad laminate. [Means for solving the problem]
[0008] As a result of investigations conducted by the present inventors to solve the above problems, they have found that the problems can be solved by the present embodiment described below. That is, the present embodiment relates to the following [1] to
[11] . [1] A method for producing a metal-clad laminate in which a prepreg and a metal foil are laminated by heating and pressurizing, The prepreg is The present invention comprises a thermosetting resin composition and a fiber base material having a thickness of 40 μm or more, A first resin layer containing a thermosetting resin composition provided on one surface of the fiber substrate; A second resin layer containing a thermosetting resin composition is provided on the other surface of the fiber substrate, When the thickness of the first resin layer is d1 and the thickness of the second resin layer is d2, The ratio R of the thickness difference represented by the following formula (1) is −9.0% to +9.0%, R = (d1-d2) × 100 / (d1+d2) (1) The method for producing a metal-clad laminate, wherein the surface waviness (Wa) on both sides of the prepreg is 6 μm or less. [2] The method for producing a metal-clad laminate according to the above [1], wherein the prepreg has regions impregnated with the thermosetting resin composition and regions not impregnated with the fiber base material. [3] The method for producing a metal-clad laminate according to the above [1] or [2], wherein the thickness d1 of the first resin layer and the thickness d2 of the second resin layer are each 2 to 20 μm. [4] The method for producing a metal-clad laminate according to any one of the above [1] to [3], wherein the fiber base material has a thickness of 40 to 120 μm. [5] The method for producing a metal-clad laminate according to any one of the above [1] to [4], wherein the fiber base material is a glass cloth. [6] A method for producing a printed wiring board, comprising producing a metal-clad laminate by the method for producing a metal-clad laminate according to any one of the above [1] to [5], and forming a wiring pattern on the metal-clad laminate. [7] A method for producing a semiconductor package, comprising the steps of producing a printed wiring board by the method for producing a printed wiring board according to the above-mentioned [6], and mounting a semiconductor element on the printed wiring board. [8] A metal-clad laminate having a cured product of a thermosetting resin composition, one or more layers of a fiber substrate, and a metal foil, The thickness of the fiber base material is 40 μm or more, A metal-clad laminate having a value of 0.5% or less, as determined according to the following method: (method) A 500 mm x 500 mm area within the surface of the metal-clad laminate is divided into a grid at 50 mm intervals in both the vertical and horizontal directions, and 21 measurement unit areas 7, each with a square shape of 50 mm x 50 mm in plan view, are set at the positions shown in the plan view of the metal-clad laminate 30 in Figure 4. The thickness is measured at four thickness measurement points 8 shown in Figure 4, which are points located 10 mm inside the measurement unit area 7 from the vertical and horizontal sides of the measurement unit area 7, and the difference between the maximum and minimum thickness values at the four points is defined as the thickness difference V1 within the measurement unit area 7, and the average thickness value of the four points is defined as T1. V1 and T1 are calculated for each of the 21 measurement unit areas 7, and the average value V ave and the average value of T1 ave The value is calculated from the following formula. V ave ×100 / T ave [9] The metal-clad laminate has the metal foil on both sides, a first resin cured product layer containing a cured product of a thermosetting resin composition provided on a surface of the fiber substrate and in contact with the metal foil on one surface of the metal-clad laminate; a second resin cured product layer containing a cured product of a thermosetting resin composition, the second resin cured product layer being provided on the surface of the fiber base material and in contact with the metal foil on the other surface of the metal-clad laminate; When the thickness of the first cured resin layer is d'1 and the thickness of the second cured resin layer is d'2, The metal-clad laminate according to the above [8], wherein a ratio R' of the thickness difference represented by the following formula (1') is -9.0% to +9.0%. R'=(d'1-d'2)×100 / (d'1+d'2) (1')
[10] A printed wiring board having the metal-clad laminate described in [8] or [9] above.
[11] A semiconductor package comprising the printed wiring board according to
[10] above and a semiconductor element. Effect of the Invention
[0009] According to this embodiment, even when a fiber base material having a thickness of 40 μm or more is used, a method for manufacturing a metal-clad laminate having excellent thickness accuracy and uniformity of dimensional change, a method for manufacturing a printed wiring board and a semiconductor package using the metal-clad laminate, It is possible to provide a metal-clad laminate capable of reducing variations in the amount of warping of semiconductor packages even when a fiber base material with a thickness of 40 μm or more is used, and a printed wiring board and a semiconductor package having the metal-clad laminate. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a schematic cross-sectional view showing one embodiment of a prepreg used in the manufacturing method of the present embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing one embodiment of a prepreg having discontinuous unimpregnated regions in the surface direction. [Diagram 3] 1 is an image used when calculating the abundance ratio of impregnated regions in the prepreg produced in Example 1. [Figure 4] FIG. 2 is a schematic plan view for explaining a method for measuring the thickness of a metal-clad laminate. [Diagram 5] FIG. 2 is a schematic plan view for explaining a method for measuring the variation in the amount of dimensional change of a metal-clad laminate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In this specification, a numerical range indicated using "~" indicates a range that includes the numerical values before and after "~" as the minimum and maximum values, respectively. For example, the expression "numerical range "X to Y" (X and Y are real numbers) means a numerical range that is equal to or greater than X and equal to or less than Y. In this specification, the expression "equal to or greater than X" means X and a numerical value that exceeds X. In this specification, the expression "equal to or less than Y" means Y and a numerical value that is less than Y. Each lower limit and upper limit of a numerical range described herein may be arbitrarily combined with the lower limit or upper limit of any other numerical range. In the numerical ranges described in this specification, the lower or upper limit of the numerical range may be replaced with values shown in the examples.
[0012] Unless otherwise specified, each of the components and materials exemplified in this specification may be used alone or in combination of two or more. In this specification, the content of each component in a resin composition means, when a plurality of substances corresponding to each component are present in the resin composition, the total amount of the plurality of substances present in the resin composition, unless otherwise specified.
[0013] In this specification, the term "solid content" refers to components other than the solvent, and also includes components that are liquid at room temperature. Here, room temperature in this specification refers to 25°C.
[0014] The mechanism of action described in this specification is speculation and does not limit the mechanism by which the effects of the present embodiment are achieved.
[0015] The expression "containing" used in this specification not only means that "contains" is simply contained, but also includes the case where "contains" is in a reacted state if the thing described in "contains" is capable of reacting.
[0016] Any combination of the descriptions in this specification is also included in this embodiment.
[0017] [Metal-clad laminate manufacturing method] The method for producing the metal-clad laminate of this embodiment is as follows: A method for producing a metal-clad laminate, comprising laminating a prepreg and a metal foil by heating and pressurizing the prepreg and a metal foil, The prepreg is The present invention comprises a thermosetting resin composition and a fiber base material having a thickness of 40 μm or more, A first resin layer containing a thermosetting resin composition provided on one surface of the fiber substrate; A second resin layer containing a thermosetting resin composition is provided on the other surface of the fiber substrate, When the thickness of the first resin layer is d1 and the thickness of the second resin layer is d2, The ratio R of the thickness difference represented by the following formula (1) is −9.0% to +9.0%, R = (d1-d2) × 100 / (d1+d2) (1) In the method for producing a metal-clad laminate, the surface waviness (Wa) on both sides of the prepreg is 6 μm or less. In the following description, a prepreg having the above configuration, i.e., a prepreg containing a thermosetting resin composition and a fiber base material having a thickness of 40 μm or more, having the first resin layer and the second resin layer, having the thickness difference ratio R of −9.0% to +9.0%, and having surface waviness (Wa) on both sides of 6 μm or less, may be referred to as a “prepreg (P)”.
[0018] The reason why the metal-clad laminate produced by the production method of this embodiment has excellent thickness precision and uniformity of dimensional change is not clear, but is presumed to be as follows. The prepreg (P) used in this embodiment has a thickness difference ratio R represented by the above formula (1) of -9.0% to +9.0%, and the surface waviness (Wa) on both sides is 6 μm or less. That is, the prepreg (P) used in this embodiment has a uniform amount of thermosetting resin composition attached to the front and back of the fiber base material, and its surface is smooth. This is presumably one of the reasons why the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate could be improved, because the thickness variation of the prepreg itself was reduced and the homogeneity of the flow behavior of the thermosetting resin composition on the front and back of the prepreg when pressed was improved.
[0019] Hereinafter, first, each member used in the method for producing a metal-clad laminate of this embodiment will be described, and then the lamination conditions for each member will be described.
[0020] <Prepreg (P)> The prepreg (P) used in this embodiment contains a thermosetting resin composition and a fiber base material having a thickness of 40 μm or more, and has a first resin layer containing the thermosetting resin composition provided on one surface of the fiber base material, and a second resin layer containing the thermosetting resin composition provided on the other surface of the fiber base material.
[0021] FIG. 1 is a schematic cross-sectional view showing an example of the prepreg (P) used in this embodiment. 1 includes a fiber base material 1, a first resin layer 2 having a thickness d1 provided on one surface of the fiber base material 1, and a second resin layer 3 having a thickness d2 provided on the other surface of the fiber base material 1. The fiber base material 1 preferably has a region impregnated with a thermosetting resin composition, and more preferably has a region impregnated with a thermosetting resin composition and a non-impregnated region. In the prepreg 10, the surface of the first resin layer 2 opposite the fiber base material 1 constitutes one surface of the prepreg 10, and the surface of the second resin layer 3 opposite the fiber base material 1 constitutes the other surface of the prepreg 10.
[0022] The thermosetting resin composition contained in the first resin layer and the thermosetting resin composition contained in the second resin layer may be the same or different, but it is preferable that they are the same. Furthermore, when the thermosetting resin composition contained in the first resin layer and the thermosetting resin composition contained in the second resin layer are the same, these thermosetting resin compositions and the thermosetting resin composition contained in the fiber base material may be the same or different, but it is preferable that they are the same. The first resin layer and the second resin layer preferably do not contain a fibrous base material.
[0023] (Thickness difference ratio R) In the prepreg (P) used in this embodiment, when the thickness of the first resin layer is d1 and the thickness of the second resin layer is d2, the thickness difference ratio R represented by the following formula (1) is −9.0% to +9.0%. R = (d1-d2) × 100 / (d1+d2) (1) From the viewpoint of further improving the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate, the thickness difference ratio R represented by the above formula (1) is preferably -8.0% to +8.0%, more preferably -7.0% to +7.0%, even more preferably -6.0% to +6.0%, and particularly preferably -5.0% to +5.0%. The thickness d1 of the first resin layer and the thickness d2 of the second resin layer used in calculating the thickness difference ratio R can be measured by the following method. More detailed conditions can be those described in the Examples. [Method of measuring thickness d1 of first resin layer and thickness d2 of second resin layer] A cross section of the prepreg that has been heat-treated as necessary is formed, and the cross section is observed by a metal microscope to obtain a cross section image. In the obtained cross section image, a fiber base material having a thickness of 40 μm or more, a first resin layer, and a second resin layer are identified, and the minimum thickness of the first resin layer and the minimum thickness of the second resin layer in the field of view are measured. The measurement of the minimum thickness is performed in any five fields of view that do not overlap, and the average value of all the minimum thicknesses of the five fields of view in the first resin layer is set to the thickness d1 of the first resin layer, and the average value of all the minimum thicknesses of the five fields of view in the second resin layer is set to the thickness d2 of the second resin layer.
[0024] (Thickness d1 of the first resin layer and thickness d2 of the second resin layer) The thickness d1 of the first resin layer and the thickness d2 of the second resin layer are not particularly limited, but from the viewpoint of further improving ease of production and the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate, each is preferably 2 to 20 μm, more preferably 5 to 15 μm, even more preferably 6 to 13 μm, and particularly preferably 7 to 10 μm. It is to be noted that only one of the thickness d1 of the first resin layer and the thickness d2 of the second resin layer may be within the above range. The method for measuring the thickness d1 of the first resin layer and the thickness d2 of the second resin layer is as described above.
[0025] (Surface waviness (Wa)) The surface waviness (Wa) on both sides of the prepreg (P) used in this embodiment is 6 μm or less. In this embodiment, the "surface" of the prepreg (P) refers to the surface that will be laminated when the prepreg (P) is laminated to produce a metal-clad laminate, or the opposite surface thereof. The surface waviness (Wa) on both sides of the prepreg (P) used in this embodiment is preferably 5.5 μm or less, more preferably 5 μm or less, and even more preferably 4 μm or less, from the viewpoint of further improving the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate. The surface waviness (Wa) on both sides of the prepreg (P) used in this embodiment is preferably smaller, but from the viewpoint of ease of manufacture, it may be 0.5 μm or more, or may be 0.8 μm or more. In the present embodiment, the surface waviness (Wa) refers to the arithmetic mean height (Wa) that can be obtained from a waviness curve in accordance with ISO 4287 (1997). The surface waviness (Wa) can be measured by the method described in the examples.
[0026] (Impregnated and non-impregnated areas) The prepreg (P) used in this embodiment preferably has, in a fiber base material, regions impregnated with the thermosetting resin composition and regions not impregnated with the thermosetting resin composition. When the thermosetting resin composition is completely impregnated into the fiber base material, the waviness of the fiber base material tends to easily appear on the surface of the prepreg (P). This tendency is particularly noticeable when the thickness of the fiber base material is 40 μm or more. On the other hand, by providing an unimpregnated region in the fiber base material, the waviness of the fiber base material is less likely to appear on the surface of the prepreg (P), and the surface waviness (Wa) of the prepreg (P) tends to be easily adjusted to 6 μm or less. Note that the fact that the fiber base material has an impregnated region and an unimpregnated region of the thermosetting resin composition only relates to the prepreg, that is, the prepreg in the B-stage state, and does not relate to the cured product of the prepreg.
[0027] The unimpregnated regions in the prepreg (P) used in this embodiment preferably exist intermittently, and more preferably exist intermittently in the plane direction. The presence of discontinuous unimpregnated regions facilitates the impregnation of the thermosetting resin composition into the unimpregnated regions during heating and pressure application when laminating the prepreg (P) and the metal foil, suppresses the generation of minute voids due to the unimpregnated regions, and tends to improve insulation reliability.
[0028] FIG. 2 shows a schematic cross-sectional view of a prepreg 20, which is an example of a prepreg (P) in which unimpregnated regions exist intermittently in the planar direction. The prepreg 20 shown in FIG. 2 has a thermosetting resin composition 5 on the front and back sides and inside of the fiber base material 1, and also includes an unimpregnated region 6 inside the fiber base material 1. The "plane direction" of the prepreg means the direction along the surface of the fiber base material, which is indicated by X in FIG.
[0029] The ratio of the impregnated regions in the prepreg (P) can be obtained as the area ratio of the impregnated regions by observing the surface of the prepreg (P) using an optical microscope to obtain a surface observation image at a magnification of, for example, 50 times, and identifying the impregnated regions and non-impregnated regions in the surface observation image. Specifically, in observation under the above conditions, a surface observation image taken at an appropriate brightness shows that the surfaces at the lower part of the observation surface where the unimpregnated areas of the thermosetting resin composition exist are void areas that tend to reflect light and therefore appear as relatively bright areas, whereas the other areas, i.e., the impregnated areas, appear as relatively dark areas. The surface observation image is binarized so that relatively bright areas representing unimpregnated areas are assigned one value and relatively dark areas representing impregnated areas are assigned the other value, and the area ratio of the impregnated areas to the total area can be calculated in the resulting binarized image.
[0030] Here, when photographing a surface observation image, it is preferable to adjust the exposure time during surface photographing within the range of 60 to 100 ms, so that the image can be photographed with appropriate brightness to adequately reflect the impregnated and unimpregnated areas. Regarding the surface observation image of the prepreg (P), the order of color intensity is "area where the fiber substrate does not exist in the resin layer", "area where the fiber substrate is sufficiently impregnated with the thermosetting resin composition", and "area where the fiber substrate is insufficiently impregnated with the thermosetting resin composition". In this embodiment, the "area where the fiber substrate does not exist in the resin layer" is also included in the impregnated area. If the surface observation image is too bright, not only the part where the resin is insufficiently impregnated in the fiber substrate but also the part where the resin is sufficiently impregnated in the fiber substrate is likely to be brightly displayed, and if the image is bright, the surface observation image after binarization tends to be bright overall. On the other hand, if the surface observation image is too dark, the surface observation image tends to be dark overall and the presence of the unimpregnated area tends to be difficult to reflect. Therefore, it is preferable to take the image at a moderate brightness. From the viewpoint of taking the image at a moderate brightness, the observation conditions described in the examples in detail are adopted as the observation conditions. An example of a surface observation image taken at a suitable brightness and processed by the above method is shown in Fig. 3. Fig. 3 is an image obtained by binarizing the surface observation image of the prepreg produced in Example 1. In Fig. 3, it can be observed that impregnated regions (black) and non-impregnated regions (white) alternate in the surface direction. The exposure time for taking the surface observation image is 85 ms.
[0031] The proportion of the impregnated regions measured by the above method is not particularly limited, but is preferably 30 to 99%, more preferably 50 to 98%, and further preferably 60 to 97%. When the ratio of the impregnated region is equal to or greater than the lower limit, the thickness precision and the uniformity of the dimensional change of the metal-clad laminate tend to be improved. When the ratio of the impregnated region is equal to or less than the upper limit, the powder falling of the prepreg (P) tends to be suppressed, and the handleability tends to be improved.
[0032] (Textile base material) The fiber base material contained in the prepreg (P) used in this embodiment is not particularly limited as long as it is a fiber base material having a thickness of 40 μm or more. The thickness of the fiber base material may be appropriately adjusted according to the desired thickness of the metal-clad laminate within the range of 40 μm or more, and is not particularly limited, but from the viewpoint of further improving the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate, and from the viewpoint of the productivity and handling of the prepreg (P), it is preferably 40 to 120 μm, more preferably 45 to 110 μm, even more preferably 50 to 105 μm, even more preferably 55 to 100 μm, even more preferably 60 μm or more and less than 100 μm, even more preferably 70 to 97 μm, and particularly preferably 80 to 95 μm. When the thickness of the fiber base material is the above upper limit value or less, the impregnation of the thermosetting resin composition into the fiber base material is improved, and the heat resistance and insulation reliability of the cured product of the prepreg (P) tend to be more improved. In the manufacturing method of this embodiment, when a plurality of prepregs are laminated, the thickness of the fiber base material contained in each prepreg may be the same as or different from each other. The thickness of the fiber substrate can be determined by measuring any five points of the fiber substrate with a micrometer and averaging the measurements.
[0033] Examples of the material for the fiber substrate include natural fibers such as paper and cotton linters, inorganic fibers such as glass fibers and asbestos, organic fibers such as aramid, polyimide, polyvinyl alcohol, polyester, tetrafluoroethylene, acrylic, and mixtures thereof. Among these, inorganic fibers are preferred from the viewpoint of flame retardancy, and glass fibers are more preferred. Examples of the glass fibers include glass fibers using E glass, C glass, D glass, S glass, and the like. The material of the fiber base material may be one type alone or a combination of two or more types.
[0034] Examples of the shape of the fiber substrate include woven fabric, nonwoven fabric, roving, chopped strand mat, surfacing mat, etc. Among these, woven fabric is preferred.
[0035] Among the above options, glass cloth is preferred as the fiber base material from the viewpoints of low thermal expansion, flame retardancy, versatility, and the like.
[0036] The fiber substrate may be a fiber substrate made of one layer or a fiber substrate made of multiple layers. However, in the case of a fiber substrate made of multiple layers, at least one layer includes a fiber substrate having a thickness of 40 μm or more. In addition, a fiber substrate made of one layer means a fiber substrate made of only entangled fibers, and when a fiber substrate without entanglement exists, it is classified as a fiber substrate made of multiple layers. The material and shape of two or more layers of fiber substrates may be the same or different.
[0037] The surface waviness (Wa) of the fiber substrate is not particularly limited, but may be greater than 6 μm and not greater than 40 μm, may be 6.5 to 35 μm, may be 7 to 30 μm, may be 10 to 25 μm, or may be 15 to 23 μm. According to the manufacturing method of this embodiment, even if the surface waviness (Wa) of the fiber base material is within the above range, by adjusting the surface waviness (Wa) of the prepreg (P) to a predetermined range, a metal-clad laminate having excellent thickness accuracy and uniformity of dimensional change can be obtained.
[0038] (Thermosetting resin composition) The thermosetting resin composition is contained in the first resin layer and the second resin layer in the prepreg (P) used in this embodiment, and can also be impregnated into at least a portion of the fiber base material. The thermosetting resin composition contained in the prepreg (P) used in this embodiment contains at least a thermosetting resin. In addition to the thermosetting resin, the thermosetting resin composition preferably contains, as necessary, at least one selected from the group consisting of a curing agent, a curing accelerator, an inorganic filler, an organic filler, a coupling agent, a leveling agent, an antioxidant, a flame retardant, a flame retardant assistant, a thixotropy imparting agent, a thickener, a flexible material, a surfactant, and a photopolymerization initiator. Hereinafter, each component that may be contained in the thermosetting resin composition will be described. Each of the components may be used alone or in combination of two or more.
[0039] [Thermosetting resin] Examples of thermosetting resins include epoxy resins, polyimide resins, maleimide resins, modified maleimide resins, phenol resins, polyphenylene ether resins, bismaleimide triazine resins, cyanate resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, unsaturated polyester resins, allyl resins, dicyclopentadiene resins, silicone resins, triazine resins, and melamine resins. Among these, from the viewpoints of moldability and electrical insulation, epoxy resins, polyimide resins, maleimide resins, modified maleimide resins, cyanate resins, polyphenylene ether resins, and bismaleimide triazine resins are preferred, and epoxy resins, maleimide resins, and modified maleimide resins are more preferred.
[0040] The epoxy resin is preferably an epoxy resin having two or more epoxy groups in one molecule. Here, the epoxy resin is classified into glycidyl ether type epoxy resin, glycidyl amine type epoxy resin, glycidyl ester type epoxy resin, etc. Among these, glycidyl ether type epoxy resin is preferable. Epoxy resins are classified into various epoxy resins according to the difference in the main skeleton. For example, the above-mentioned types of epoxy resins are further classified into bisphenol-type epoxy resins, alicyclic epoxy resins, aliphatic chain epoxy resins, novolac-type epoxy resins, stilbene-type epoxy resins, naphthalene-skeleton-containing epoxy resins, biphenyl-type epoxy resins, xylylene-type epoxy resins, dihydroanthracene-type epoxy resins, etc. Among these, phenol novolac-type epoxy resins and naphthalene-skeleton-containing epoxy resins are preferred.
[0041] The maleimide resin is preferably a maleimide resin having one or more N-substituted maleimide groups, and more preferably a maleimide resin having two or more N-substituted maleimide groups. The maleimide resin is preferably an aromatic maleimide resin having an N-substituted maleimide group directly bonded to an aromatic ring. Examples of the maleimide resin include aromatic bismaleimide resins having two N-substituted maleimide groups directly bonded to an aromatic ring, such as bis(4-maleimidophenyl)methane, bis(4-maleimidophenyl)ether, bis(4-maleimidophenyl)sulfone, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, m-phenylene bismaleimide, and 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane; aromatic polymaleimide resins having three or more N-substituted maleimide groups directly bonded to an aromatic ring, such as polyphenylmethane maleimide and biphenyl aralkyl maleimide; maleimide resins having an indane ring skeleton; and aliphatic maleimide resins such as 1,6-bismaleimido-(2,2,4-trimethyl)hexane and pyrophosphate binder type long-chain alkyl bismaleimide.
[0042] An example of a modified maleimide resin is an aminomaleimide resin having a structural unit derived from a maleimide resin and a structural unit derived from a diamine compound. As the diamine compound, a compound having two primary amino groups is preferable. The diamine compound is preferably an aromatic diamine compound having two primary amino groups directly bonded to an aromatic ring. Examples of the diamine compound include m-phenylenediamine, p-phenylenediamine, 1,4-bis(4-aminophenoxy)benzene, 4,4'-diaminodiphenylmethane, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminobenzophenone, and 4,4'-diaminodiphenyl ether. , 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, benzidine, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-diaminodiphenyl sulfide, 4,4'-diamino-3,3'-biphenyldiol, and other aromatic diamines having two primary amino groups directly bonded to the aromatic ring; silicone compounds having two primary amino groups.
[0043] The aminomaleimide resin can be synthesized by subjecting a maleimide resin and a diamine compound to a Michael addition reaction by a known method. In the aminomaleimide resin, the equivalent ratio (Ta2 / Ta1) between the total equivalent of the groups derived from the -NH2 groups of the diamine compound (Ta2) and the total equivalent of the groups derived from the N-substituted maleimide groups of the maleimide resin (Ta1) is not particularly limited, but is preferably 0.05 to 10, more preferably 1 to 8, and even more preferably 3 to 7, from the viewpoints of dielectric properties, heat resistance, flame retardancy, and glass transition temperature. The group derived from the -NH2 group of the diamine compound includes -NH2 itself. The group derived from the N-substituted maleimide group of the maleimide resin includes the N-substituted maleimide group itself.
[0044] The content of the thermosetting resin in the thermosetting resin composition is not particularly limited, but from the viewpoints of heat resistance, moldability, processability, and conductor adhesion, it is preferably 10 to 70 mass%, more preferably 15 to 50 mass%, and even more preferably 20 to 40 mass%, relative to the total solid content (100 mass%) of the thermosetting resin composition.
[0045] [Hardening agent] Examples of the curing agent include a phenol-based curing agent, a cyanate ester-based curing agent, an acid anhydride-based curing agent, an amine-based curing agent, an active ester group-containing compound, etc. Among these, when an epoxy resin is used as the thermosetting resin, a phenol-based curing agent is preferable as the curing agent. Preferred examples of the phenol-based curing agent include cresol novolac type phenol resins, biphenyl aralkyl type phenol resins, phenol novolac type phenol resins, naphthylene ether type phenol resins, and triazine skeleton-containing phenol resins.
[0046] When the thermosetting resin composition contains a curing agent, the content thereof is not particularly limited, but from the viewpoint of obtaining good curability, it is preferably 20 to 200 parts by mass, more preferably 25 to 150 parts by mass, and even more preferably 30 to 100 parts by mass relative to 100 parts by mass of the thermosetting resin. When the thermosetting resin composition contains a curing agent, the equivalent ratio of the functional group of the thermosetting resin to the functional group of the curing agent [functional group of the thermosetting resin / functional group of the curing agent] is not particularly limited, but is preferably 0.8 to 1.2 when the functional group of the curing agent is a phenolic hydroxyl group, 0.2 to 0.4 when it is an amino group, and 0.3 to 0.6 when it is an active ester group.
[0047] [Curing Accelerator] Examples of the curing accelerator include imidazole-based curing accelerators such as imidazole compounds and derivatives of imidazole compounds, phosphorus-based compounds, tertiary amine compounds, quaternary ammonium compounds, etc. Among these, imidazole-based curing accelerators are preferred from the viewpoint of obtaining a sufficient curing acceleration effect. Examples of the imidazole compound include 2-methylimidazole, 2-ethylimidazole, 2-undecylimidazole, 2-phenylimidazole, 1,2-dimethylimidazole, and 2,4-diamino-6-[2'-methylimidazolyl-(1')]ethyl-s-triazine. Examples of derivatives of imidazole compounds include salts of imidazole compounds, such as 1-cyanoethyl-2-phenylimidazolium trimellitate, and trimellitic acid; salts of imidazole compounds and isocyanuric acid; and salts of imidazole compounds and hydrobromic acid.
[0048] When the thermosetting resin composition contains a curing accelerator, the content thereof is not particularly limited, but from the viewpoints of the curing acceleration effect and storage stability, the content is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.4 to 2 parts by mass relative to 100 parts by mass of the thermosetting resin.
[0049] [Inorganic filler] Examples of inorganic fillers include silica, alumina, titanium oxide, mica, beryllia, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay, talc, aluminum borate, silicon carbide, etc. Among these, silica and alumina are preferred from the viewpoint of reducing the thermal expansion coefficient, the relative dielectric constant and the dielectric loss tangent, and silica and aluminum hydroxide are preferred from the viewpoint of heat resistance. The inorganic filler may be surface-treated using a surface treatment agent such as a silane coupling agent.
[0050] When the thermosetting resin composition contains an inorganic filler, the content thereof on a mass basis is not particularly limited, but is preferably 10 to 80 mass%, more preferably 20 to 75 mass%, further preferably 40 to 70 mass%, and particularly preferably 45 to 65 mass%, relative to the total solid content (100 mass%) of the thermosetting resin composition. When the content of the inorganic filler is equal to or more than the lower limit, the low thermal expansion and heat resistance tend to be improved. When the content of the inorganic filler is equal to or less than the upper limit, the moldability and conductor adhesion tend to be improved.
[0051] (Thickness of prepreg (P)) The thickness of the prepreg (P) used in this embodiment is not particularly limited and may be appropriately adjusted depending on the thickness of the fiber base material used and the desired thickness of the metal-clad laminate, etc., but from the viewpoints of the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate, as well as the productivity and handleability of the prepreg (P), the thickness is preferably 50 to 160 μm, more preferably 70 to 140 μm, even more preferably 80 to 125 μm, and particularly preferably 90 to 100 μm. In this embodiment, the thickness of the prepreg means the thickness of one prepreg. In this embodiment, the thickness of the prepreg can be determined by measuring any five points of the prepreg using a digimatic indicator and averaging these measurements.
[0052] (Production method of prepreg (P)) The manufacturing method of the prepreg (P) used in this embodiment may be, for example, a method of laminating a film-like thermosetting resin composition (hereinafter also referred to as a "resin film") on both sides of a fiber substrate having a thickness of 40 μm or more (hereinafter also referred to as a "lamination method"), or a method of immersing a fiber substrate having a thickness of 40 μm or more in a thermosetting resin composition (hereinafter also referred to as a "resin varnish") diluted with an organic solvent and then drying (hereinafter also referred to as a "dipping method"). Among these, the prepreg (P) used in this embodiment is preferably manufactured by a method of laminating a film-like thermosetting resin composition on both sides of a fiber substrate having a thickness of 40 μm or more, from the viewpoint of easily adjusting the ratio R of the thickness difference to -9.0% to +9.0% and easily adjusting the surface waviness (Wa) to 6 μm or less.
[0053] [Lamination method] The resin film used in the lamination method can be produced, for example, by a method in which a resin varnish is applied to the surface of a support and then dried. The resin varnish can be prepared, for example, by adding a thermosetting resin and, if necessary, other components to an organic solvent, and then mixing and stirring the mixture using a known mixer.
[0054] Examples of organic solvents used in the resin varnish include alcohol-based solvents such as methanol, ethanol, methyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether; ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, butanone, cyclohexanone, and 4-methyl-2-pentanone; ester-based solvents such as ethyl acetate, butyl acetate, propylene glycol monomethyl ether acetate, and γ-butyrolactone; ether-based solvents such as tetrahydrofuran; aromatic solvents such as toluene, xylene, and mesitylene; nitrogen-containing solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; and sulfur-containing solvents such as dimethyl sulfoxide. The solid content concentration of the resin varnish is not particularly limited, but is preferably 20 to 85 mass %, more preferably 40 to 80 mass %, and further preferably 50 to 70 mass %.
[0055] Examples of methods for applying the resin varnish include methods using known coating devices such as a comma coater, a bar coater, a kiss coater, a roll coater, a gravure coater, and a die coater. The drying temperature and drying time after application of the resin varnish may be determined according to the type and amount of organic solvent used. For example, in the case of a resin varnish containing 30 to 70 mass % of an organic solvent, a resin film can be suitably formed by drying at 50 to 160°C for 1 to 8 minutes.
[0056] Examples of the support include organic films such as polyethylene terephthalate (PET), biaxially oriented polypropylene (OPP), polyethylene, polyvinyl fluoride, and polyimide; metal foils of metals such as copper and aluminum, or alloys thereof, etc. The support may be a release film whose surface has been treated with a release agent for release.
[0057] The thickness of the resin film may be appropriately determined depending on the thickness of the fiber base material, the desired thickness of the prepreg (P), etc., and is not particularly limited, but is preferably 10 to 100 μm, more preferably 15 to 70 μm, and even more preferably 18 to 50 μm. The thickness of the resin film is determined by measuring the total thickness of any five points of the resin film with the support, peeling off the resin film at the measurement points with adhesive tape, measuring the thickness of the support alone, and subtracting the thickness of the support alone from the total thickness to obtain the average value. A digimatic indicator can be used to measure the thickness.
[0058] Next, a method for laminating a resin film on both sides of a fiber base material will be described. First, two resin films with supports are prepared and placed on both sides of a fiber substrate so that the resin films are in contact with the fiber substrate. Then, the resin films with supports are laminated onto the fiber substrate to impregnate the fiber substrate with the resin films. When the prepreg (P) is produced by a lamination method, for example, the thickness difference between the resin film laminated on one side of the fiber base material and the resin film laminated on the other side of the fiber base material is reduced, thereby adjusting the thickness difference ratio R to -9.0% to +9.0%. The absolute value of the thickness difference between the resin film laminated on one side of the fiber base material and the resin film laminated on the other side of the fiber base material is not particularly limited, but is preferably 2.5 μm or less, more preferably 1.5 μm or less, and even more preferably 0.5 μm or less.
[0059] The lamination method is not particularly limited, and for example, roll lamination or press lamination using a hot plate may be used. The heating temperature during lamination is not particularly limited, but from the viewpoint of easily adjusting the thickness difference ratio R and surface waviness (Wa) of the prepreg (P) within the above ranges, it is preferably 50 to 180°C, more preferably 100 to 170°C, and even more preferably 120 to 165°C. The pressure applied during lamination is not particularly limited, but from the viewpoint of easily adjusting the thickness difference ratio R of the prepreg (P) and the surface waviness (Wa) within the above ranges, it is preferably 0.05 to 1.5 MPa, more preferably 0.1 to 1.3 MPa, and even more preferably 0.3 to 1.2 MPa. The lamination may be performed under reduced pressure. In this case, the degree of vacuum is not particularly limited, but from the viewpoint of easily adjusting the thickness difference ratio R of the prepreg (P) and the surface waviness (Wa) within the above ranges, the degree of vacuum is preferably 200 kPa or less, more preferably 150 kPa or less, and even more preferably 120 kPa or less.
[0060] In the lamination method, an example of a method for providing discontinuous non-impregnated regions in the fiber substrate is a method of adjusting the heating and pressure conditions when laminating the supported resin film and the fiber substrate. Here, when the lamination conditions are the same for the thin fiber substrate and the thick fiber substrate, the thick fiber substrate tends to be more difficult to impregnate the resin film into the fiber substrate. Therefore, even if the lamination conditions of this embodiment are the same as those of the conventional thin fiber substrate, the fiber substrate can be provided with intermittent regions that are not impregnated with the thermosetting resin composition. Specific methods for adjusting the heating and pressurizing conditions include, for example, the following methods. First, a prepreg is prepared under a predetermined heating and pressurizing condition, and then the ratio of the impregnated region of the thermosetting resin composition in the fiber base material is calculated based on the above-mentioned calculation method. As a result, if the impregnated region is 100%, that is, if there is no unimpregnated region, the heating temperature or the pressurizing pressure is lowered, or both the heating temperature and the pressurizing pressure are lowered, the prepreg is reprepared, and the ratio of the impregnated region is calculated again. By repeating this process as necessary, the conditions for producing a prepreg having an unimpregnated region can be easily grasped. If it is desired to adjust the proportion of unimpregnated regions to a lower value, the heating temperature or the pressurizing pressure may be increased, or both the heating temperature and the pressurizing pressure may be increased, and the prepreg may be re-prepared. By the above-mentioned operations, conditions under which the waviness of the fiber substrate is unlikely to appear on the surface of the prepreg may be extracted, and the surface waviness (Wa) of the prepreg may be adjusted to 6 μm or less.
[0061] After the resin film has been impregnated into the fiber base material, it may be cooled if necessary, and then the support may be peeled off from the prepreg (P) with the support obtained, thereby obtaining the prepreg (P).
[0062] [Immersion method] The resin varnish used in the immersion method may be the same as the resin varnish used in producing the resin film in the above-mentioned lamination method. The drying temperature and drying time after immersing the fiber substrate in the resin varnish are not particularly limited, and may be appropriately determined taking into consideration the type of organic solvent, etc.
[0063] <Metal foil> Examples of the metal species of the metal foil used in the manufacturing method of this embodiment include copper, gold, silver, nickel, platinum, molybdenum, ruthenium, aluminum, tungsten, iron, titanium, chromium, and alloys containing one or more of these metal elements. Examples of the alloy include copper-based alloys, aluminum-based alloys, and iron-based alloys. Examples of the copper-based alloys include copper-nickel alloys. Examples of the iron-based alloys include iron-nickel alloys. Among these, from the viewpoints of electrical conductivity and availability, copper, nickel, aluminum, and iron-nickel alloys are preferred, copper and aluminum are more preferred, and copper is even more preferred. When copper foil is used as the metal foil, the resulting metal-clad laminate may be called a copper-clad laminate. The thickness of the metal foil is not particularly limited, but is preferably 1 to 200 μm, more preferably 2 to 100 μm, and further preferably 3 to 50 μm. The number of metal foils used in the manufacturing method of this embodiment is not particularly limited, and may be one, but is preferably two. In the metal-clad laminate obtained by the manufacturing method of this embodiment, the metal foil is preferably disposed on at least one surface of the metal-clad laminate, and more preferably disposed on both surfaces of the metal-clad laminate.
[0064] <Method of laminating prepreg and metal foil> Metal-clad laminates can be produced by placing metal foil on one or both sides of a prepreg, and then applying heat and pressure. When heating and pressing, only one prepreg may be used, or two or more prepregs may be stacked, but at least one prepreg (P) is used. When two or more prepregs are used, it is preferable that all the prepregs are prepregs (P). When two or more prepregs are used, the total number of prepregs may be, for example, 2 to 20, 5 to 18, or 8 to 16. As a method for producing a metal-clad laminate having metal foil on both sides, the production method described later in the section "Metal-clad laminate" is also preferred. In addition to the prepreg and metal foil, a substrate on which an inner layer circuit has been processed may also be molded under heat and pressure.
[0065] For the application of heat and pressure, for example, a multi-stage press, a multi-stage vacuum press, a continuous molding machine, an autoclave molding machine, or the like can be used. The heating temperature during heating and pressurization is not particularly limited, but is preferably 100 to 300°C, more preferably 150 to 260°C, and further preferably 170 to 230°C. The heating and pressurizing time during heating and pressurization is not particularly limited, but is preferably 10 to 300 minutes, more preferably 30 to 200 minutes, and even more preferably 60 to 150 minutes. The pressure during heating and pressurization is not particularly limited, but is preferably 1.0 to 6 MPa, more preferably 1.5 to 3 MPa, and further preferably 1.8 to 2.5 MPa.
[0066] Heating and pressurization may be a method of increasing the temperature while applying pressure. In this case, it is preferable that the maximum temperature is within the above-mentioned suitable heating temperature range, and the holding time at the maximum temperature is within the above-mentioned suitable heating and pressurization time range. When the temperature is increased while applying pressure, the rate of temperature increase is not particularly limited, but is preferably 1 to 10° C. / min, and more preferably 2 to 5° C. / min. When the temperature is increased while pressure is being applied, the timing of application of pressure is not particularly limited, but pressure may be applied at room temperature and then the temperature may be increased.
[0067] The thickness of the metal-clad laminate produced by the production method of this embodiment is not particularly limited, and may be 400 to 2,500 μm, 450 to 2,000 μm, 500 to 1,800 μm, or 550 to 1,600 μm. The thickness of the metal-clad laminate is T ave It can be measured by the measurement method described above.
[0068] As described above, the manufacturing method of this embodiment can manufacture a metal-clad laminate with excellent thickness accuracy. Therefore, in the manufacturing method of this embodiment, it is possible to omit the smoothing treatment applied to the cured prepreg in order to improve the thickness accuracy of the metal-clad laminate. Examples of the smoothing treatment include a method of pressing the cured prepreg with a roll, a method of polishing the surface of the cured prepreg, and the like.
[0069] When the metal-clad laminate produced by the manufacturing method of this embodiment and the metal-clad laminate of this embodiment described later contain a plurality of fiber substrates, from the viewpoint of productivity, the thickness of the fiber substrate located on the outermost side on at least one side of the metal-clad laminate may be in the range of 0.6 to 1.3 times, 0.7 to 1.3 times, 0.8 to 1.2 times, or 0.9 to 1.1 times the thickness of the fiber substrate adjacent to the fiber substrate. It is preferable that the thickness of the fiber substrate located on the outermost side on both sides of the metal-clad laminate is in the above range with respect to the thickness of the adjacent fiber substrate.
[0070] [Manufacturing method for printed wiring boards] The method for producing a printed wiring board according to the present embodiment is a method for producing a printed wiring board by producing a metal-clad laminate by the method for producing a metal-clad laminate according to the present embodiment, and forming a wiring pattern on the metal-clad laminate. The wiring pattern can be formed by a known method. In addition, etching of the metal foil, drilling, metal plating, etc. may be appropriately performed by a known method, if necessary.
[0071] [Semiconductor package manufacturing method] The method for manufacturing a semiconductor package of this embodiment is a method for manufacturing a semiconductor package in which a printed wiring board is manufactured by the method for manufacturing a printed wiring board of this embodiment, and a semiconductor element is mounted on the printed wiring board. The method for mounting the semiconductor element is not particularly limited, and a conventionally known method can be applied. Specifically, for example, after aligning the electrodes of the printed wiring board with the bumps of the semiconductor chip, they are temporarily fixed, and the semiconductor chip is bonded to the printed wiring board by applying a reflow method, a TCB (Thermal Compression Bonding) method, or the like. Thereafter, the gap between the printed wiring board and the semiconductor chip may be sealed with a liquid encapsulant. A part or the entire surface of the semiconductor chip may be sealed with a semiconductor encapsulant. The liquid encapsulant and semiconductor encapsulant may be any conventionally known material.
[0072] [Metal-clad laminate] The metal-clad laminate of this embodiment is A metal-clad laminate having a cured product of a thermosetting resin composition, one or more layers of a fiber substrate, and a metal foil, The thickness of the fiber base material is 40 μm or more, The value obtained according to the following method is 0.5% or less. (method) The surface of the metal-clad laminate is divided into a grid at intervals of 50 mm in both the vertical and horizontal directions, and 21 measurement unit areas 7, each of which has a square shape of 50 mm long x 50 mm wide in plan view, are set at the positions shown in the plan view of the metal-clad laminate 30 in Figure 4. The thickness is measured at four thickness measurement points 8 shown in Figure 4, which are points located 10 mm inside the measurement unit area 7 from the vertical and horizontal sides of the measurement unit area 7, and the difference between the maximum and minimum thickness values at the four points is defined as the thickness difference V1 within the measurement unit area 7, and the average thickness value of the four points is defined as T1. V1 and T1 are calculated for each of the 21 measurement unit areas 7, and the average value V ave and the average value of T1 ave The value is calculated from the following formula. V ave ×100 / T ave More specifically, it can be measured by the method described in the Examples.
[0073] The reason why the semiconductor package using the metal-clad laminate of this embodiment has small variations in the amount of warping of the semiconductor package is not clear, but is presumed to be as follows. The metal-clad laminate of this embodiment has a value determined by the above method of 0.5% or less, and has excellent thickness accuracy, which is presumably due in part to the fact that the amount of thermal expansion of the substrates included in semiconductor packages manufactured using the metal-clad laminate is uniform between products.
[0074] The metal-clad laminate of this embodiment has metal foil on both sides, a first resin cured product layer containing a cured product of a thermosetting resin composition provided on a surface of the fiber substrate and in contact with the metal foil on one surface of the metal-clad laminate; a second resin cured product layer containing a cured product of a thermosetting resin composition, the second resin cured product layer being provided on the surface of the fiber base material and in contact with the metal foil on the other surface of the metal-clad laminate; When the thickness of the first cured resin layer is d'1 and the thickness of the second cured resin layer is d'2, The thickness difference ratio R' represented by the following formula (1') is preferably from -9.0% to +9.0%. R'=(d'1-d'2)×100 / (d'1+d'2) (1')
[0075] The thickness difference ratio R' represented by the above general formula (1') is preferably -8.0% to +8.0%, more preferably -7.0% to +7.0%, even more preferably -6.0% to +6.0%, and particularly preferably -5.0% to +5.0%, from the viewpoint of further improving the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate. More detailed measurement conditions for the thickness difference ratio R' can be those described in the Examples.
[0076] The cured product of the thermosetting resin composition contained in the first resin cured product layer and the cured product of the thermosetting resin composition contained in the second resin cured product layer may be the same or different, but it is preferable that they are the same. Furthermore, when the cured product of the thermosetting resin composition contained in the first resin cured product layer and the cured product of the thermosetting resin composition contained in the second resin cured product layer are the same, the cured products of these thermosetting resin compositions and the cured product of the thermosetting resin composition contained in the fiber base material may be the same or different, but it is preferable that they are the same. The first and second cured resin layers preferably do not contain a fibrous base material.
[0077] The metal-clad laminate of this embodiment is preferably manufactured by the manufacturing method described in the above [Method for manufacturing metal-clad laminate]. That is, the metal-clad laminate of this embodiment is preferably manufactured using the prepreg (P). Therefore, the preferred aspects of the cured product of the thermosetting resin composition and the fiber substrate contained in the metal-clad laminate of this embodiment are the same as the preferred aspects of the cured product of the thermosetting resin composition contained in the prepreg (P) and the fiber substrate contained in the prepreg (P). The preferred aspects of the lamination configuration, manufacturing conditions, etc. of each member when manufacturing a metal-clad laminate using the prepreg (P) are also as described in the above [Method for manufacturing metal-clad laminate].
[0078] When manufacturing a metal-clad laminate having metal foils on both sides, it is preferable that when the metal foil and the prepreg are heated and pressed, the prepreg in contact with the metal foil on one side and the prepreg in contact with the metal foil on the other side are both prepregs (P) from the viewpoint of thickness accuracy of the metal-clad laminate. As a result, the first resin cured product layer and the second resin cured product layer of the metal-clad laminate become layers made of the cured products of the first resin layer or the second resin layer of the prepreg (P). An embodiment in which the prepreg in contact with the metal foil on one side and the prepreg in contact with the metal foil on the other side are both prepregs (P) may be, for example, an embodiment in which metal foils are laminated on both sides of one prepreg (P). In addition, when a plurality of prepregs including two or more prepregs (P) are used, the prepregs may be stacked so that one of the prepregs (P) is exposed on one side and another prepreg (P) is exposed on the other side, and one metal foil is laminated on the prepreg (P) exposed on the one side, and the other metal foil is laminated on the prepreg (P) exposed on the other side.
[0079] The thickness of the metal-clad laminate of the present embodiment may be 400 to 2,500 μm, 450 to 2,000 μm, 500 to 1,800 μm, or 550 to 1,600 μm. The method for measuring the thickness of the metal-clad laminate is as described above.
[0080] [Printed wiring board] The printed wiring board of the present embodiment is a printed wiring board having the metal-clad laminate of the present embodiment. The printed wiring board of the present embodiment can be manufactured by using the metal-clad laminate of the present embodiment as the metal-clad laminate in the method described above in [Method for manufacturing a printed wiring board].
[0081] [Semiconductor package] The semiconductor package of the present embodiment is a semiconductor package having the printed wiring board of the present embodiment and a semiconductor element. The semiconductor package of the present embodiment can be manufactured by using the printed wiring board of the present embodiment as the printed wiring board in the method described above in [Method of manufacturing a semiconductor package]. EXAMPLES
[0082] The present embodiment will now be described in more detail with reference to the following examples, but these examples are not intended to limit the present embodiment.
[0083] [Method of measuring thickness d1 of first resin layer, thickness d2 of second resin layer, and thickness difference ratio R of prepreg] (1) Preparation of test specimens The prepregs produced in the examples and comparative examples were heat-treated in an air atmosphere at 170° C. for 1 hour, and then at 200° C. for 1 hour. The prepregs after the heat treatment were cast with epoxy resin and polished with a polishing machine (manufactured by Refine Tech Co., Ltd., product name "Refine Polisher") to obtain test pieces by cutting out the cross sections. (2) Measurement of thickness d1 of the first resin layer and thickness d2 of the second resin layer The cross section of the test piece obtained in (1) above was observed at an arbitrary magnification of 20 to 200 times using a metal microscope to obtain a cross section image. In the obtained cross section image, the fiber base material, the first resin layer, and the second resin layer, each having a thickness of 40 μm or more, were identified, and the minimum thickness of the first resin layer and the minimum thickness of the second resin layer in the corresponding visual field were measured. The measurement of the minimum thickness was performed in any five visual fields in which the regions did not overlap, and the average value of all the minimum thicknesses in the five visual fields in the first resin layer was defined as the thickness d1 of the first resin layer, and the average value of all the minimum thicknesses in the five visual fields in the second resin layer was defined as the thickness d2 of the second resin layer. From the thickness d1 of the first resin layer and the thickness d2 of the second resin layer obtained above, a thickness difference ratio R was calculated based on the following formula (1). R = (d1-d2) × 100 / (d1+d2) (1)
[0084] [Method of measuring thickness d'1 of first cured resin layer, thickness d'2 of second cured resin layer, and thickness difference ratio R' of metal-clad laminate] (1) Preparation of test specimens The metal-clad laminates produced in the examples and comparative examples were polished using a polishing machine (manufactured by Refine Tech Co., Ltd., product name "Refine Polisher"), and the cross sections were cut out to prepare test specimens. (2) Measurement of thickness d'1 of the first cured resin layer and thickness d'2 of the second cured resin layer The cross section of the test piece obtained in (1) above was observed using a metallurgical microscope at an arbitrary magnification of 20 to 200 times to obtain a cross section image. In the obtained cross-sectional image, the first resin cured material layer provided on the surface of the fiber substrate and in contact with the metal foil (copper foil) on one surface of the metal-clad laminate, and the second resin cured material layer provided on the surface of the fiber substrate and in contact with the metal foil (copper foil) on the other surface of the metal-clad laminate were identified, and the minimum thickness of the first resin cured material layer and the minimum thickness of the second resin cured material layer were measured. The minimum thickness was measured in any five visual fields that did not overlap, and the average value of all the minimum thicknesses of the five visual fields in the first resin cured material layer was defined as the thickness d'1 of the first resin cured material layer, and the average value of all the minimum thicknesses of the five visual fields in the second resin cured material layer was defined as the thickness d'2 of the second resin cured material layer. From the thickness d'1 of the first cured resin layer and the thickness d'2 of the second cured resin layer obtained above, a thickness difference ratio R' was calculated according to the following formula (1'). R'=(d'1-d'2)×100 / (d'1+d'2) (1')
[0085] [Method of measuring surface waviness (Wa)] The prepregs produced in the examples and comparative examples were used as measurement objects, and shape measurements were automatically performed using an observation application with a shape analysis laser microscope (manufactured by Keyence Corporation, product name "VK-X100") to obtain waviness curves in accordance with ISO 4287 (1997). Surface roughness analysis was performed on the obtained waviness curves using an analysis application to calculate the surface waviness (Wa). Here, the waviness curve is a curve obtained by applying a phase compensation high-pass filter λc (λc=80 μm) to the profile curve to remove wavelengths less than 80 μm from the profile curve. The analysis range was 1,000 μm x 1,000 μm. The surface waviness (Wa) was measured on both sides of the prepreg, and the larger value is shown in Table 1.
[0086] [Method for measuring the proportion of impregnated areas] The ratio of the impregnated regions was measured by the following method. (1) Obtaining surface observation images The surface of the prepreg was observed under the following conditions using an optical microscope (manufactured by Olympus Corporation, product name "MX61L-F") to obtain a surface observation image. <Observation conditions> ·Magnification: 50x Observation mode: dark field Sensitivity: ISO400 Exposure time for surface photography: 60-100ms - Brightness of the observation environment: Two 35W fluorescent lamps were installed 2m above the observation stage. The exposure time was adjusted between 60 and 100 ms to obtain an appropriate brightness that could adequately reflect the impregnated and non-impregnated regions. (2) Image processing The surface observation image obtained above was binarized using image editing software so that the impregnated areas were black and the non-impregnated areas were white, and saved in BMP (Microsoft Windows Bitmap Image) format. Next, the pixel value data for each pixel of the binarized surface observation image saved in BMP format was saved in CSV (comma-separated values) format using image conversion software. The image editing software used was "Microsoft Paint" (Microsoft Corporation), and the image conversion software used was the free software "bmp2csv." (3) Calculation of the ratio of impregnated regions The pixel value data saved in CSV format was pasted into Microsoft Excel (Microsoft Corporation), and the number of black areas (pixel value = 0) corresponding to the impregnated areas and the number of white areas (pixel value = 1) corresponding to the non-impregnated areas were counted. From these numbers, the ratio of the black areas to the total of the black and white areas was calculated, and this was taken as the abundance ratio of the impregnated areas. In addition, the prepregs obtained in Comparative Examples 3 to 5 were marked as "measurable" because the regions corresponding to the unimpregnated regions could not be identified.
[0087] [Measuring the thickness of metal-clad laminates] FIG. 4 shows a plan view for explaining a method for measuring the thickness of a metal-clad laminate. As shown in Figure 4, a 500 mm x 500 mm area on the surface of the metal-clad laminate 30 was divided into a grid at 50 mm intervals in both the vertical and horizontal directions, and 21 measurement unit areas 7 (shaded areas in Figure 4) each having a square shape of 50 mm x 50 mm in plan view were set. Next, as shown in the enlarged view of Figure 4, the thickness was measured at four points (point 8 in Figure 4) located 10 mm inside the measurement unit area 7 from the vertical and horizontal sides of the measurement unit area 7, and the difference between the maximum and minimum thickness values at the four points was defined as the thickness difference V1 within the measurement unit area 7, and the average thickness value of the four points was defined as T1. Using the same method, V1 and T1 were obtained for each of the 21 measurement unit areas 7. The average value V1 obtained was ave and the average value of T1 ave was calculated and the value was obtained from the following formula. V ave ×100 / T ave The value (unit: %) calculated from the above formula was used as an index of thickness precision.
[0088] [Measurement of variation in dimensional change of metal-clad laminate] Four evaluation substrates measuring 340 mm × 250 mm were cut out from the metal-clad laminate prepared in each example, as shown in Figure 5. A total of four reference holes were made in each of the four evaluation substrates, 1 cm vertically and 1 cm horizontally from each of the four corners, and the distance between adjacent holes was measured using a CNC image measuring machine (manufactured by Mitutoyo Corporation, product name: QV-H606T1L-D), and this value was taken as the "reference dimension." The evaluation substrate thus obtained was immersed in a copper etching solution (type of chemical solution: ammonium persulfate, temperature: 40° C., treatment time: 5 minutes) to remove the copper foil from the evaluation substrate. Next, the evaluation board from which the copper foil had been removed by etching was heated in air at 180° C. for 1 hour, then allowed to cool to 25° C., and heated again in air at 180° C. for 1 hour. Thereafter, the distance between adjacent holes was measured using the same method as above, and this value was taken as the "dimension after heating." From the dimensions obtained above, the dimensional change rate after heating was calculated for the four evaluation substrates based on the following formula. Dimensional change rate (%) = (dimension after heating - reference dimension) x 100 / reference dimension The dimensional change rates of the four evaluation substrates (two data points in the vertical direction and two data points in the horizontal direction per substrate) were measured, and the standard deviation was calculated to represent the variation in the amount of dimensional change of the metal-clad laminate (unit: %).
[0089] [Method for evaluating the heat resistance of metal-clad laminates] The metal-clad laminate obtained in each example was cut into 25 mm squares to prepare evaluation boards, which were then floated in a solder bath at 288°C for 90 minutes to check for the occurrence of blistering. The evaluation results were rated as "A" for boards that showed no blistering after 90 minutes of floating, and "B" for boards that showed blistering.
[0090] [Method for measuring variation in warpage of semiconductor packages] Using the metal-clad laminate obtained in each example as a core layer, a substrate (rectangular with an outer dimension of 60 mm x 60 mm in plan view) having the following layer structure was produced using a build-up material (manufactured by Ajinomoto Co., Inc., product name "GX92", thickness 30 μm) (hereinafter also referred to as "BU"), copper foil (manufactured by Mitsui Mining & Smelting Co., Ltd., product name "3EC-M3-VLP", thickness 12 μm), and solder resist (manufactured by Resonac Inc., product name "SR-7300") (hereinafter also referred to as "SR"). (Layer structure of the substrate) SR / Copper foil (Remaining copper rate 65%) / BU / BU / Copper foil (Remaining copper rate 100%) / BU / BU / Copper foil (Remaining copper rate 100%) / BU / BU / Core layer / BU / BU / Copper foil (Remaining copper rate 100%) / BU / BU / Copper foil (Remaining copper rate 100%) / BU / BU / Copper foil (Remaining copper rate 65%) / SR
[0091] In the above substrate, the SR thickness was 20 μm, the solder resist opening radius was 100 μm, the pad diameter was 150 μm, and the pad pitch was 200 μm.
[0092] Each layer was laminated in the following order (1) to (5). (1) Two sheets of build-up material were laminated on each side of the metal-clad laminate obtained in each example, and copper foil was placed on the exposed surfaces of the build-up materials on both sides, and then the laminate was heat-cured under conditions of 180°C, 0.5 MPa, and 90 minutes. (2) Two sheets of build-up material were further laminated on each side of the obtained laminate, and copper foil was placed on the exposed surfaces of the build-up materials on both sides, followed by heating and curing under the same conditions as above. (3) The same operation as in (2) above was carried out, and two build-up materials and copper foil were further laminated on both sides. (4) The copper foil on both sides of the laminate obtained in (3) above was etched to obtain a predetermined pattern. (5) On both sides of the laminated plate that had been subjected to the above step (4), a solder resist layer having predetermined openings was formed using the above solder resist.
[0093] Next, a silicon semiconductor chip was mounted in the center of one surface of the substrate obtained above. The semiconductor chip was mounted by bonding the bumps on the circuit surface of the semiconductor chip to the pads of the substrate using the TCB (Thermal Compression Bonding) method. The configuration of the semiconductor chip is as follows: (Configuration of semiconductor chip) Chip size: 25mm x 25mm rectangular in plan view, thickness 0.725mm Bump pitch: 200μm Bump metal: Sn-Ag solder alloy on Cu pillar Bump height: Cu pillar; 45μm, Sn-Ag solder alloy; 15μm Bump size: φ90μm
[0094] Thereafter, the gap between the semiconductor chip and the substrate was sealed with a liquid sealing material (manufactured by Resonac Corporation, product name "CEL-C-3730 series") to obtain a semiconductor package. Four semiconductor packages were fabricated from each of the metal-clad laminates obtained in the above-mentioned manner, and the maximum warpage of each of the four semiconductor packages obtained was measured at 25°C and 260°C using a warpage measuring device (manufactured by Akrometrix, product name "Thermoray"). The heating rate was 20°C per minute. Next, the standard deviation (unit: μm) of the maximum warpage at 25° C. was calculated from the maximum warpage at 25° C. for each of the four semiconductor packages, and this was used as the value of variation in the warpage of the semiconductor packages at 25° C. In addition, the standard deviation (unit: μm) of the maximum warpage at 260° C. was calculated from the maximum warpage at 260° C. for each of the four semiconductor packages, and this was used as the value of variation in the warpage of the semiconductor packages at 260° C. Note that the standard deviations listed in Table 1 are values rounded off to the first decimal place.
[0095] [Synthesis of modified maleimide resin] Synthesis Example 1 595.8 g of bis(4-maleimidophenyl)methane, 54.2 g of 4,4'-diaminodiphenylmethane, and 350.0 g of propylene glycol monomethyl ether were added to a 2 L reaction vessel equipped with a thermometer, a stirrer, and a moisture meter equipped with a reflux condenser, and the mixture was reacted for 5 hours under reflux to obtain a solution of a modified maleimide resin.
[0096] [Manufacturing of resin varnish] Manufacturing Example 1 (Resin varnish A) 60 parts by mass of phenol novolac type epoxy resin "EPICLON (registered trademark) N-770" (manufactured by DIC Corporation, epoxy equivalent: 188 g / eq), 40 parts by mass of biphenyl aralkyl type phenol resin (manufactured by Meiwa Kasei Co., Ltd., product name "MEH-7700"), 17.5 parts by mass of aluminum hydroxide, 86 parts by mass of fused silica, 0.5 parts by mass of 2-methylimidazole, and methyl isobutyl ketone and cyclohexanone as dilution solvents were added and mixed to prepare resin varnish A with a solids concentration of 65% by mass.
[0097] Manufacturing Example 2 (Resin varnish B) 107 parts by mass of the modified maleimide resin solution obtained in Synthesis Example 1, 30 parts by mass of tetrafunctional naphthalene-type epoxy resin "EXA-4710" (manufactured by DIC Corporation), 17.5 parts by mass of aluminum hydroxide, 130 parts by mass of fused silica, 0.5 parts by mass of 2,4-diamino-6-[2'-undecylimidazolyl-(1)']-ethyl-S-triazine, and methyl isobutyl ketone and cyclohexanone as dilution solvents were added and mixed to prepare resin varnish B with a solids concentration of 65% by mass.
[0098] Example 1 (1) Preparation of resin film The resin varnish shown in Table 1 was applied onto a PET film using a comma coater so that the thickness of the resin film after drying would be 30 μm. Then, the film was dried by heating at 130° C. for 2 minutes to produce a resin film with a PET film.
[0099] (2) Prepreg Preparation Next, the resin film with the PET film was placed so that the resin film surface of the resin film was in contact with the glass cloth on both sides of the fiber substrate shown in Table 1, and laminated using a vacuum laminator. The conditions for vacuum lamination were: hot plate temperature 130°C, pressure bonding pressure 0.5 MPa, heating and pressurizing time 30 seconds, vacuum degree 100 kPa or less, and vacuum time 30 seconds.
[0100] (3) Preparation of metal-clad laminate The obtained prepregs were stacked in the number shown in Table 1, and copper foil (manufactured by Furukawa Electric Co., Ltd., product name "GTS-12", thickness 12 μm) was placed on the top and bottom of them. Then, pressing was performed under the following conditions to produce a metal-clad laminate having a square shape of 1,000 mm in length and 1,000 mm in width in plan view. -Press conditions- Heating conditions: the temperature was increased from 25° C. to 185° C. at a rate of 3° C. / min, and the sample was kept at 185° C. for 90 minutes, and then cooled for 30 minutes. Pressure conditions: 4 MPa from the start of heating to the end of cooling.
[0101] Example 2 A resin film, a prepreg, and a metal-clad laminate were produced by the same procedure as in Example 1, except that the number of prepregs stacked in "(3) Production of metal-clad laminate" in Example 1 was changed to 8.
[0102] Example 3 A resin film, a prepreg, and a metal-clad laminate were produced by the same operations as in Example 1, except that the conditions for vacuum lamination in “(2) Preparation of prepreg” in Example 1 were changed to a hot plate temperature of 150° C., a bonding pressure of 0.7 MPa, a heating and pressurizing time of 60 seconds, a vacuum degree of 100 kPa or less, and a vacuum time of 60 seconds.
[0103] Example 4 (1) Preparation of resin film Resin films were prepared in the same manner as in Example 1, except that the thickness of the resin film after drying was changed to 30.5 μm and 29.5 μm. (2) Prepreg Preparation A prepreg was produced by carrying out the same operations as in Example 1, except that a 30.5 μm thick resin film was abutted against one side of the fiber substrate and a 29.5 μm thick resin film was abutted against the other side of the fiber substrate, and the vacuum lamination conditions were changed to a hot plate temperature of 150° C., a bonding pressure of 0.7 MPa, a heating and pressurizing time of 60 seconds, a vacuum degree of 100 kPa or less, and a vacuum time of 60 seconds. (3) Preparation of metal-clad laminate A metal-clad laminate was produced in the same manner as in Example 1, except that the prepreg obtained above was used.
[0104] Example 5 (1) Preparation of resin film Resin films were prepared in the same manner as in Example 1, except that the thickness of the resin film after drying was changed to 20.5 μm and 19.5 μm. (2) Prepreg Preparation A prepreg was produced by the same procedure as in Example 1, except that the type of fiber substrate was changed to that shown in Table 1, a 20.5 μm thick resin film was abutted on one side of the fiber substrate and a 19.5 μm thick resin film was abutted on the other side of the fiber substrate, and the vacuum lamination conditions were changed to a hot plate temperature of 150° C., a bonding pressure of 0.7 MPa, a heating and pressurizing time of 60 seconds, a vacuum degree of 100 kPa or less, and a vacuum time of 60 seconds. (3) Preparation of metal-clad laminate A metal-clad laminate was produced in the same manner as in Example 1, except that the prepreg obtained above was used.
[0105] Example 6 (1) Preparation of resin film Resin films were prepared in the same manner as in Example 1, except that the thickness of the resin film after drying was changed to 31 μm and 29 μm. (2) Prepreg Preparation A prepreg was produced by carrying out the same operations as in Example 1, except that a 31 μm-thick resin film was abutted against one side of the fiber substrate and a 29 μm-thick resin film was abutted against the other side of the fiber substrate, and the vacuum lamination conditions were changed to a hot plate temperature of 160° C., a bonding pressure of 1.0 MPa, a heating and pressurizing time of 60 seconds, a vacuum degree of 100 kPa or less, and a vacuum time of 60 seconds. (3) Preparation of metal-clad laminate A metal-clad laminate was produced in the same manner as in Example 1, except that the prepreg obtained above was used.
[0106] Example 7 In "(1) Preparation of resin film" of Example 6, the same operations as in Example 6 were carried out except that the type of resin varnish was changed to that shown in Table 1, to prepare a resin film, a prepreg, and a metal-clad laminate.
[0107] Comparative Example 1 (1) Preparation of resin film Resin films were prepared in the same manner as in Example 1, except that the thickness of the resin film after drying was changed to 32 μm and 28 μm. (2) Prepreg Preparation A prepreg was produced by performing the same operations as in Example 1, except that a 32 μm-thick resin film was abutted against one side of the fiber substrate and a 28 μm-thick resin film was abutted against the other side of the fiber substrate, and the vacuum lamination conditions were changed to a hot plate temperature of 100° C., a bonding pressure of 0.2 MPa, a heating and pressurizing time of 30 seconds, a vacuum degree of 100 kPa or less, and a vacuum time of 30 seconds. (3) Preparation of metal-clad laminate A metal-clad laminate was produced in the same manner as in Example 1, except that the prepreg obtained above was used.
[0108] Comparative Example 2 (1) Preparation of resin film Resin films were prepared in the same manner as in Example 1, except that the thickness of the resin film after drying was changed to 32 μm and 29 μm. (2) Prepreg Preparation A prepreg was produced by the same procedure as in Example 1, except that a 32 μm thick resin film was abutted against one side of the fiber substrate and a 29 μm thick resin film was abutted against the other side of the fiber substrate. (3) Preparation of metal-clad laminate A metal-clad laminate was produced in the same manner as in Example 1, except that the prepreg obtained above was used.
[0109] Comparative Example 3 A fiber substrate shown in Table 1 was immersed in a resin varnish shown in Table 1 and dried at 140° C. for 3.5 minutes to obtain a prepreg. Thereafter, the same operation as in Example 1 was carried out to produce a metal-clad laminate.
[0110] Comparative Example 4 A fiber substrate shown in Table 1 was immersed in a resin varnish shown in Table 1 and dried at 140° C. for 3.5 minutes to obtain a prepreg. Thereafter, the same operation as in Example 1 was carried out to produce a metal-clad laminate.
[0111] Comparative Example 5 A fiber substrate shown in Table 1 was immersed in a resin varnish shown in Table 1 and dried at 140° C. for 3.5 minutes to obtain a prepreg. Thereafter, the same operation as in Example 1 was carried out to produce a metal-clad laminate.
[0112] [Table 1]
[0113] The details of the fiber base materials shown in Table 1 are as follows. "2116": Glass cloth "IPC#2116" (manufactured by Nitto Boseki Co., Ltd., basis weight: 104g / m 2 , thickness: 91μm, surface waviness (Wa): 21.9μm) "1078": Glass cloth "IPC#1078" (manufactured by Nitto Boseki Co., Ltd., basis weight: 47g / m 2 , thickness: 44μm, surface waviness (Wa): 7.3μm)
[0114] As can be seen from Table 1, the metal-clad laminates produced in Examples 1 to 7 of this embodiment were excellent in thickness accuracy and uniformity of dimensional change. Furthermore, the semiconductor packages produced using the metal-clad laminates produced in Examples 1 to 7 of this embodiment had small variations in warpage. [Explanation of symbols]
[0115] 10, 20, 30 metal clad laminate 1. Fiber base material 2. First Resin Layer 3. Second resin layer 5 Thermosetting resin composition 6 Unimpregnated area 7. Measurement Unit Area 8 thickness measurement points X plane direction
Claims
1. A method for producing a metal-clad laminate, comprising laminating a prepreg and a metal foil by heating and pressing the prepreg and a metal foil, The prepreg is The present invention comprises a thermosetting resin composition and a fiber base material having a thickness of 40 μm or more, A first resin layer containing a thermosetting resin composition provided on one surface of the fiber substrate; A second resin layer containing a thermosetting resin composition is provided on the other surface of the fiber substrate, The thickness of the first resin layer is d 1 The thickness of the second resin layer is d 2 , then, The ratio R of the thickness difference represented by the following formula (1) is −9.0% to +9.0%, R = (d 1 -d 2 ) × 100 / (d 1 +d 2 ) (1) The method for producing a metal-clad laminate, wherein the surface waviness (Wa) of both surfaces of the prepreg is 6 μm or less.
2. The method for producing a metal-clad laminate according to claim 1 , wherein the prepreg has an area impregnated with the thermosetting resin composition and an area not impregnated with the thermosetting resin composition in the fiber base material.
3. The thickness d of the first resin layer 1 and the thickness d of the second resin layer 2 The method for producing a metal-clad laminate according to claim 1 or 2, wherein each of the thicknesses is 2 to 20 μm.
4. The method for producing a metal-clad laminate according to claim 1 or 2, wherein the thickness of the fiber base material is 40 to 120 μm.
5. The method for producing a metal-clad laminate according to claim 1 or 2, wherein the fiber base material is a glass cloth.
6. A method for producing a printed wiring board, comprising the steps of producing a metal-clad laminate by the method for producing a metal-clad laminate according to claim 1 or 2, and forming a wiring pattern on the metal-clad laminate.
7. A method for producing a semiconductor package, comprising the steps of producing a printed wiring board by the method for producing a printed wiring board according to claim 6, and mounting a semiconductor element on the printed wiring board.
8. A metal-clad laminate having a cured product of a thermosetting resin composition, one or more layers of a fiber substrate, and a metal foil, The thickness of the fiber base material is 40 μm or more, A metal-clad laminate having a value of 0.5% or less, as determined by the following method. (method) A 500 mm x 500 mm area within the surface of the metal-clad laminate is divided into a grid at 50 mm intervals in both the vertical and horizontal directions, and 21 measurement unit areas 7, each of which has a square shape in plan view of 50 mm x 50 mm, are set at the positions shown in the plan view of the metal-clad laminate 30 in Figure 4. The thickness was measured at four thickness measurement points 8 shown in FIG. 4, which are points spaced 10 mm from the vertical and horizontal sides of the measurement unit area 7 on the inside of the measurement unit area 7, and the difference between the maximum and minimum thickness values at the four points was defined as the thickness difference V within the measurement unit area 7. 1 The average thickness of the four points is T 1 Let us assume that. For each of the 21 measurement unit areas 7, V 1 and T 1 Looking for V 1 The average value of V ave and T 1 The average value of T ave The value is calculated from the following formula. V ave x 100 / T ave
9. The metal-clad laminate has the metal foil on both sides, a first resin cured product layer containing a cured product of a thermosetting resin composition, the first resin cured product layer being provided on a surface of the fiber substrate and in contact with the metal foil on one surface of the metal-clad laminate; a second resin cured product layer containing a cured product of a thermosetting resin composition, the second resin cured product layer being provided on the surface of the fiber base material and in contact with the metal foil on the other surface of the metal-clad laminate; The thickness of the first cured resin layer is d' 1 The thickness of the second cured resin layer is d' 2 , then, The metal-clad laminate according to claim 8, wherein the thickness difference ratio R' represented by the following formula (1') is -9.0% to +9.0%. R'=(d' 1 -d' 2 ) × 100 / (d' 1 +d' 2 ) (1')
10. A printed wiring board comprising the metal-clad laminate according to claim 8 or 9.
11. A semiconductor package comprising the printed wiring board according to claim 10 and a semiconductor element.
Citation Information
Patent Citations
Manufacture of prepreg
JP1989272416A