Decorative sheet

The decorative sheet addresses the challenge of stain resistance and durability by using a polypropylene resin with nucleating agent vesicles and controlled surface roughness, achieving effective stain resistance and design quality.

JP2024144594AActive Publication Date: 2024-10-11TOPPAN HOLDINGS INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024119267
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-11
Estimated Expiration
2040-06-03

AI Technical Summary

Technical Problem

Existing decorative materials lack sufficient stain resistance and durability against household contaminants, particularly in high-traffic areas like kitchens and children's rooms, and existing methods to enhance stain resistance often compromise surface texture or require expensive equipment and complex curing processes.

Method used

A decorative sheet with a base layer containing a core layer of polypropylene resin and skin layers with encapsulated nucleating agent vesicles, combined with a surface protective layer having controlled surface roughness, to enhance scratch resistance and stain resistance while maintaining design quality.

Benefits of technology

The decorative sheet provides excellent stain resistance and design feel, with improved scratch resistance and durability, ensuring contaminants can be easily wiped off without compromising the aesthetic appeal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144594000001_ABST
    Figure 2024144594000001_ABST
Patent Text Reader

Abstract

To provide a decorative sheet excellent in stain resistance and designability.SOLUTION: A decorative sheet 10 includes at least a top coat layer 4 on a substrate layer 1. In the decorative sheet, arithmetic average roughness (Ra0.008) is 10 μm or less in accordance with JIS B0601:2001, measured vertically to a deposition direction when a cut-off value λc is 2.5 mm, a cut-off value λs is 8 μm and an evaluation length is 10 mm, with regard to a front side of the top coat layer 4, and an average length RSm and a ten point average roughness RzJIS of a roughness curve element satisfy a condition of the following equation (1): 5≤RSm / RzJIS≤40 ...(1).SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a decorative sheet. [Background technology]

[0002] Decorative sheets are used, for example, for interior and exterior materials of buildings such as houses, building materials such as fittings and fixtures, furniture and fixtures, home appliances, home appliances, etc. Some decorative sheets are used for semi-exterior applications such as exterior materials under the eaves and entrance door materials that are more or less exposed to wind and rain, and for applications such as children's rooms, kitchens, dining rooms, and washrooms that require wipeability, water repellency, and stain resistance against marker pens and everyday contaminants.

[0003] Decorative materials (including decorative boards, decorative papers, decorative sheets, etc.) used for the various applications mentioned above are required to be durable and weather resistant to withstand long-term use, in the order of decades, and may also be required to be stain-resistant so that even if contaminants adhere to the surface during use due to natural actions such as rainwater or dust, or due to the user's carelessness, they can be easily wiped off and the beauty of the material can be maintained.

[0004] In particular, kitchens and dining rooms where food-related contaminants such as salad oil, tempura oil, and other oils and fats, and colored condiments such as soy sauce and sauces are likely to be spilled or splashed, children's rooms where children are likely to bring in dirt from outside and stick to their hands, feet, and clothes, and where graffiti such as crayons and magic markers are likely to adhere, and toilets, washrooms, and laundry rooms where water and soapy solutions are likely to splash when flushing human waste, washing hands, and doing laundry, require a higher level of resistance to contamination by everyday pollutants than is required in ordinary living rooms or bedrooms, and general urethane coatings used in ordinary cosmetic materials are simply not capable of meeting this requirement.

[0005] One method for imparting a high level of stain resistance to the surface of a cosmetic material is to form an anti-stain layer on the surface by applying a silicone resin or a fluorine-based resin with low surface tension (see, for example, Patent Document 1). However, this can cause problems such as the surface becoming extremely slippery, which can deteriorate the feel and ease of handling, and the surface not being sufficiently hard, making it vulnerable to scratches and abrasion. Therefore, a method of adding silicone oil to a normal coating film made of urethane resin or the like to form an antifouling layer (see, for example, Patent Document 2) has been relatively widely used in the past. This method has an extremely excellent effect in that the coating film has sufficient surface physical properties such as scratch resistance, abrasion resistance, and weather resistance because the main component of the coating film is a normal paint for decorative materials such as urethane resin, and part of the silicone oil in the coating film seeps out onto the surface of the coating film to form an oil film, which prevents adhesion of contaminants and thereby exhibits antifouling properties.

[0006] However, this oil film is wiped off when the contaminant is wiped off, and as long as the silicone oil is sufficiently contained in the coating film, it exudes a new oil film and the stain resistance is restored, but if the silicone oil in the coating film is lost over a long period of time and after repeated wiping, the stain resistance is no longer exhibited, so there is a problem in terms of the durability of the stain resistance. In particular, in decorative materials supplied in a rolled state, such as decorative paper, decorative sheet, and wallpaper, the silicone oil that exudes from the surface of the coating film transfers to the back side of the decorative material, and when it is bonded to a base material or a substrate, it repels the adhesive, causing adhesion inhibition.

[0007] As a means of providing the surface coating of a decorative material with excellent stain resistance and long-term durability while ensuring sufficient surface properties, various methods have already been considered for chemically bonding the base resin of the coating with a silicone component for providing stain resistance. A representative example is a two-part crosslinking reactive resin with an acrylic resin as the base and a silicone compound as the hardener (see, for example, Patent Documents 3 and 4). Compared to the original acrylic resin, the introduction of the silicone component certainly improves stain resistance due to the decrease in surface tension. However, perhaps because the silicone component acts as a cross-linking agent and is tied to the two acrylic skeletons and cannot move freely, the stain resistance improvement effect is often not as great as when silicone oil is added.

[0008] There has also been a proposal for a method using a (meth)acrylate-based ionizing radiation curable resin containing a silicone (meth)acrylate compound (see, for example, Patent Document 5). However, since this utilizes a special curing system such as an electron beam or ultraviolet light, it requires expensive equipment, and there are problems such as applicability to special shapes where uniform irradiation is difficult and deterioration of the substrate due to irradiation, so that the range of application is often limited. In addition, ionizing radiation curable resins have a very high crosslink density, and the molecular motion of the silicone component is hindered by the extremely rigid three-dimensional crosslinked structure of the cured product, so it is often difficult to obtain a sufficient effect of improving contamination resistance. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 11-58614 [Patent Document 2] Japanese Patent Application Publication No. 10-58611 [Patent Document 3] Japanese Patent Application Publication No. 5-222819 [Patent Document 4] Japanese Patent Application Publication No. 5-246001 [Patent Document 5] Japanese Patent Application Publication No. 5-86306 Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention has been made to solve the above-mentioned problems in the prior art, and its object is to provide a stain-resistant decorative material (decorative sheet) that is not only excellent in stain resistance against various household pollutants, but also has excellent design properties such as feel and design feel. [Means for solving the problem]

[0011] The stain-resistant decorative material (decorative sheet) of the present invention is characterized in that the stain resistance and design are improved by the uneven shape given to the surface. Specifically, the stain-resistant decorative material (decorative sheet) according to one embodiment of the present invention has at least a surface protective layer on a substrate layer, and is characterized in that the surface side of the surface protective layer has an arithmetic mean roughness (Ra0.008) of 10 μm or less measured perpendicular to the film-forming direction with a cutoff value λc of 2.5 mm, a cutoff value λs of 8 μm, and an evaluation length of 10 mm according to JIS B0601:2001, and the average length RSm of the roughness curve element and the ten-point mean roughness RzJIS satisfy the condition of the following formula (1). 5 ≦ RSm / RzJIS ≦ 40 (1)

[0012] In addition, a nucleating agent that improves the crystallinity of polypropylene is encapsulated in a vesicle having a single-layer outer membrane to form a vesicle, which is then added to a polypropylene resin as a nucleating agent vesicle.Furthermore, after extensive consideration and experimentation of the manufacturing process, it has been discovered that a decorative sheet with improved scratch resistance can be provided by adjusting the Martens hardness to an optimal range. Specifically, a decorative sheet according to one embodiment of the present invention comprises a base layer having a core layer containing an inorganic pigment and polypropylene resin, and skin layers containing polypropylene resin formed on both sides of the core layer, and the skin layers may be formed by adding nucleating agent vesicles having a single-layer outer membrane and encapsulating a nano-sized nucleating agent to the polypropylene resin.

[0013] Here, the nucleating agent vesicle is a capsule-shaped vesicle having a single-layer outer membrane and encapsulating a nucleating agent therein, and can be prepared, for example, by supercritical reverse phase evaporation. A nucleating agent is a substance that acts as a starting point for crystallization in crystalline polypropylene resin. Effect of the Invention

[0014] According to one embodiment of the present invention, by controlling the surface irregularities imparted to a substrate, a decorative sheet having excellent stain resistance and design properties (feel and design) can be provided. [Brief description of the drawings]

[0015] [Figure 1] 1 is a cross-sectional view showing a configuration of a decorative sheet according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing the configuration of another decorative sheet according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Here, the drawings are schematic, and the relationship between thickness and planar dimensions, the thickness ratio of each layer, etc. are different from the actual ones. Furthermore, the embodiments shown below are examples of configurations for embodying the technical idea of ​​the present invention, and the technical idea of ​​the present invention does not specify the materials, shapes, structures, etc. of the components as described below. The technical idea of ​​the present invention can be modified in various ways within the technical scope defined by the claims.

[0017] The decorative material of this embodiment includes at least a substrate B and a decorative sheet 10. The substrate B and decorative sheet 10 of this embodiment will be described in detail below. 1 and 2, the symbol B represents a substrate. The substrate B is a substrate to which the decorative sheet 10 described below is attached. The substrate B is not particularly limited, and examples thereof include wood boards, inorganic boards, metal plates, and composite boards made of multiple materials. In addition, a primer layer, a concealing layer, and the like may be provided between the decorative sheet 10 and the substrate B as appropriate.

[0018] The decorative sheet 10 of this embodiment comprises, for example, in this order, a base layer 1, a design layer 2, a transparent resin layer 3, and a topcoat layer 4. Each layer constituting the decorative sheet 10 will be described below. <Base material layer 1> The base layer 1 is, for example, a three-layer colored polypropylene film having a core layer 1a at the center and skin layers 1b on both sides of the core layer 1a. The core layer 1a may be made mainly of polypropylene resin, and may be colored by mixing inorganic pigment into the polypropylene resin. The skin layer 1b may be formed containing polypropylene resin. The skin layer 1b may not contain inorganic pigment.

[0019] (Polypropylene resin) The polypropylene resin used for the core layer 1a is preferably a highly flexible random polypropylene resin having an ethylene content, or a mixture of a known amorphous polypropylene resin with a random polypropylene resin or a homopolypropylene resin with high crystallinity, taking into consideration the dispersibility of the inorganic pigment. The polypropylene resin used for the skin layer 1b is preferably a highly crystalline homopolypropylene because it is not necessary to consider the dispersibility of the inorganic pigment, but is not limited to the highly crystalline homopolypropylene. In applications where processability such as bending is more important, for example, a random polypropylene resin having an ethylene content within a certain range or a known amorphous polypropylene resin can be mixed with the highly crystalline homopolypropylene.

[0020] The skin layer 1b of the base layer 1 made of a colored polypropylene film has a Martens hardness of 80 N / mm 2 More than 120N / mm 2 The core layer 1a has a Martens hardness of 50 N / mm 2 More than 80N / mm 2 It is preferable that the content is within the following range:

[0021] The Martens hardness of the core layer 1a is 50N / mm 2If the Martens hardness of the core layer 1a is less than 80 N / mm 2 If it exceeds this value, the crystallinity is too high, so that defects such as whitening or cracking may occur during bending, or defects such as cracking may occur during an impact resistance test. The Martens hardness of the skin layer 1b is 80N / mm 2 If the Martens hardness of the skin layer 1b is less than 120 N / mm 2 If it exceeds this value, the crystallinity is too high, so that even when a nucleating agent vesicle is used, defects such as whitening or cracking may occur during bending, or defects such as cracking may occur during an impact resistance test.

[0022] The preferred range of the Martens hardness of the core layer 1a of the substrate layer 1 is 60 N / mm 2 More than 80N / mm 2 The preferred range of the Martens hardness of the skin layer 1b of the substrate layer 1 is 80 N / mm 2 More than 100N / mm 2 By setting the thickness within this range, scratch resistance, impact resistance, and bending workability can all be excellent. Here, Martens hardness is a kind of index showing the hardness (hardness) of a substance, and is defined as the quotient of the indentation force calculated from the load and the surface area of ​​the indentation calculated from the indentation depth, which is calculated by applying a load to an indenter and pressing it into the surface of a sample, and measuring the depth (indentation depth) of the indentation (impression) formed at that time. The measurement is performed according to the method specified in ISO14577.

[0023] The arithmetic mean height Ra and ten-point mean roughness Rz of the top coat layer (surface protection layer) 4 indicate information on the irregularities formed on the top coat layer 4 in the height direction. The average length RSm is the average value of the lengths Xs of the contour curve elements in the reference length, and indicates lateral information such as the pitch interval of the irregularities formed on the surface of the top coat layer 4. When Ra or Rz is small, the irregularities formed on the surface of the top coat layer 4 are small, resulting in a shape to which contaminants are less likely to adhere; when RSm is large, the pitch between the irregularities formed on the surface of the top coat layer 4 is wide, resulting in a shape to which contaminants, even if they do get in, can be easily wiped off.

[0024] In this embodiment, when the Ra of the top coat layer 4 is greater than 10 μm and RSm / RzJIS is less than 5, the unevenness formed on the surface of the top coat layer 4 is large and has a dense shape with a narrow pitch between the unevennesses. Therefore, if contaminants adhere firmly, they cannot be easily wiped off, and the surface cannot be said to have excellent contamination resistance. Furthermore, if RSm / RzJIS is greater than 40, the uneven shape will be gradual, and the design will often be impaired. Moreover, the Ra of the top coat layer 4 is preferably 1.0 μm or more. That is, the Ra of the top coat layer 4 in this embodiment is preferably within the range of 1.0 μm or more and 10 μm or less. If the Ra of the top coat layer 4 is less than 1.0 μm, the design will be poor, and the commercial value of the decorative sheet 10 may be impaired.

[0025] Here, Ra is measured using a surface roughness meter (Mitutoyo Corporation, model number SJ-310) in accordance with the measurement method in accordance with JIS B0601:2001, with a cutoff value λc of 2.5 mm, a cutoff value λs of 8 μm, and an evaluation length of 10 mm, measured in the direction of the pattern if there was one, and perpendicular to the film formation direction if there was no pattern. Measurements were performed at any five points, and the average value was taken as the measured value. The same applies to RSm and RzJIS.

[0026] Examples of methods for adjusting the surface roughness of the topcoat layer 4 include (1) adding an inorganic filler to the topcoat layer 4, and (2) forming an embossed shape using an embossing plate. In this embodiment, the surface roughness of the top coat layer 4 is adjusted by the method (2). In this embodiment, the thickness of the base layer 1 made of a colored polypropylene film may be within a range of 40 μm or more and 200 μm or less.

[0027] If the thickness of the base layer 1 is less than 40 μm, even if the Martens hardness of the skin layer 1b is within the optimal range, the film strength will be insufficient, making it difficult to prevent defects during printing and deterioration of scratch resistance, and also difficult to maintain surface smoothness during wrapping. On the other hand, if the thickness of the base layer 1 exceeds 200 μm, there is a high possibility of defects such as whitening and cracking occurring during bending, and during wrapping, the ability to conform to the edge of the wood board and the laminated parts will be significantly reduced, and the adhesive strength will be insufficient, which may cause defects such as peeling over time. A more preferable range for the thickness of the base layer 1 is from 60 μm to 150 μm. Within this range, defects during printing, surface smoothness during wrapping, scratch resistance, and bending can be achieved with a sufficient margin.

[0028] Regarding the thickness of the skin layer 1b and the core layer 1a of the base layer 1, it is preferable that the thickness of the core layer 1a is in the range of 3 times or more and 50 times or less than the thickness of the skin layer 1b. If the thickness of the core layer 1a is less than 3 times, it is difficult to satisfy the minimum required hiding power as a decorative sheet. If the thickness of the core layer 1a is more than 50 times, the thickness of the skin layer 1b becomes too small relatively, so that the film strength is insufficient, and even if the Martens hardness is in the optimal range, it is difficult to suppress defects during printing processing and deterioration of scratch resistance. A more preferable range of the thickness of the core layer 1a is 10 to 40 times the thickness of the skin layer 1b. By setting the thickness in this range, it is possible to achieve a sufficient balance between the hiding power, defects during printing processing, surface smoothness during wrapping processing, scratch resistance, and bending processability.

[0029] In this embodiment, as described above, it is preferable to use a polypropylene resin having high crystallinity as the polypropylene resin used for the skin layer 1b. In particular, it is preferable to use a highly crystalline homopolypropylene resin, which is a propylene homopolymer having an isotactic pentad fraction (mmmm fraction) of 95% or more, in an amount of 30% by mass to 100% by mass based on the mass of the total polypropylene resin. The crystallization temperature of polypropylene resin is generally within the range of 100°C to 130°C, and when a nucleating agent is added, it is within the range of 110°C to 140°C. In the skin layer 1b of the colored polypropylene film in the decorative sheet 10 of this embodiment, the cooling time from the crystallization temperature within this range to the hardening completion temperature is controlled by a known cooling process, thereby making it possible to maintain a Martens hardness of 80 N / mm 2 More than 120N / mm 2 It is adjusted to within the following range. If the content of the highly crystalline homopolypropylene resin is less than 30% by mass, the crystallinity is insufficient, and the Martens hardness may be lower than the preferred range even if the cooling process is controlled.

[0030] Here, the isotactic pentad fraction (mmmm fraction) is calculated from a numerical value (electromagnetic wave absorption rate) obtained by resonating a resin material at a predetermined resonance frequency by 13C-NMR measurement (nuclear magnetic resonance measurement) using carbon C (nuclear species) with a mass of 13, and specifies the atomic arrangement, electronic structure, and molecular microstructure in the resin material. The pentad fraction of a crystalline polypropylene resin is the ratio of five propylene units lined up as determined by 13C-NMR, and is used as a measure of crystallinity or stereoregularity. The pentad fraction is one of the important factors that mainly determine the scratch resistance of the surface, and basically, the higher the pentad fraction, the higher the crystallinity.

[0031] (Inorganic pigments) The inorganic pigment may be a known inorganic pigment, such as titanium oxide, which is used to provide hiding power. Examples of inorganic pigments for coloring include iron-zinc, chromium-antimony, and iron-aluminum composite oxides, and iron oxide, which may be freely mixed according to the desired color. In addition, lustrous materials such as aluminum flakes and pearl pigments may also be added as inorganic pigments. Organic pigments such as carbon black may also be used in combination. Furthermore, additives such as fatty acid metal salts may be added to improve dispersibility and extrudability.

[0032] (Nucleating Agent Vesicle) The skin layer 1b of the base layer 1 may also contain a nano-sized nucleating agent. The nano-sized nucleating agent may be added to the polypropylene resin in the form of a nucleating agent vesicle encapsulated in a vesicle having a single-layer outer membrane. When the nucleating agent is contained in the skin layer 1b of the base layer 1, the crystallinity of the polypropylene resin can be improved, and the scratch resistance (scratch resistance) of the base layer 1 can be improved. In this embodiment, the nucleating agent in the resin constituting the skin layer 1b of the base layer 1 may be encapsulated in a vesicle with a part of the nucleating agent exposed. It is preferable that the average particle size of the nano-sized nucleating agent is 1 / 2 or less of the wavelength range of visible light. Specifically, since the wavelength range of visible light is 400 nm or more and 750 nm or less, it is preferable that the average particle size is 375 nm or less.

[0033] Nano-sized nucleating agents have extremely small particle diameters, so the number of nucleating agents present per unit volume and the surface area increase inversely proportional to the cube of the particle diameter. As a result, the distance between each nucleating agent particle becomes closer, so that when crystal growth occurs from the surface of one nucleating agent particle added to the polypropylene resin, the end from which the crystal is growing immediately comes into contact with the end of the crystal growing from the surface of another nucleating agent particle adjacent to the one nucleating agent particle, and the ends of the crystals inhibit the growth of each crystal, stopping the growth of each crystal. Therefore, the average particle size of the spherulites in the crystalline part of the crystalline polypropylene resin can be reduced, for example, the spherulite size can be reduced to 1 μm or less. As a result, a colored polypropylene film with high crystallinity and high hardness can be obtained, and the stress concentration between the spherulites that occurs during bending processing can be efficiently dispersed, so that a colored polypropylene film that suppresses cracking and whitening during bending processing can be realized.

[0034] Here, when the nucleating agent is simply added, the particle size of the nucleating agent in the polypropylene resin increases due to secondary aggregation, and the number of crystal nuclei relative to the amount of nucleating agent added may be significantly smaller than when the nucleating agent is added as a vesicle. As a result, the average particle size of the spherulites in the crystalline portion of the polypropylene resin becomes large, and cracking and whitening during bending may not be suppressed. Therefore, it may not be possible to improve the elastic modulus and processability by increasing the crystallinity at the same time.

[0035] The skin layer 1b of the base layer 1 made of a colored polypropylene film constituting the decorative sheet 10 of this embodiment may be added in an amount of 0.05 parts by mass or more and 0.5 parts by mass or less in terms of the amount of nucleating agent added relative to 100 parts by mass of polypropylene resin as the main component, and it is preferable that the nucleating agent vesicle is added in an amount of 0.1 parts by mass or more and 0.3 parts by mass or less. If the amount of the nucleating agent vesicle added is less than 0.05 parts by mass, the crystallinity may not be sufficiently improved and the required elastic modulus (hardness) may not be reached. In addition, if the amount of the nucleating agent vesicle added is more than 0.5 parts by mass, the crystal nuclei are excessive, so that spherulite growth is inhibited, and as a result, the crystallinity may not be sufficiently improved and the required elastic modulus (hardness) may not be reached.

[0036] In addition, methods for nano-sizing nucleating agents include, for example, a solid phase method in which the nucleating agent is mainly subjected to mechanical crushing to obtain nano-sized particles, a nano-sized method in which the nucleating agent is dissolved in a solution, and a method in which the nucleating agent is dissolved in a solution to obtain nano-sized particles. Methods such as a liquid phase method for synthesizing or crystallizing nano-sized particles from a nucleating agent or a gas or vapor containing a nucleating agent can be appropriately used. Examples of solid phase methods include a ball mill, a bead mill, a rod mill, a colloid mill, a conical mill, a disk mill, a hammer mill, and a jet mill. Examples of liquid phase methods include a crystallization method, a coprecipitation method, a sol-gel method, a liquid phase reduction method, and a hydrothermal synthesis method. Examples of gas phase methods include an electric furnace method, a chemical flame method, a laser method, and a thermal plasma method.

[0037] The method of nano-sizing the nucleating agent is preferably the supercritical reverse phase evaporation method. The supercritical reverse phase evaporation method is a method of producing a capsule (nano-sized vesicle) encapsulating a target substance using carbon dioxide in a supercritical state or under temperature or pressure conditions above the critical point. Carbon dioxide in a supercritical state means carbon dioxide in a supercritical state above the critical temperature (30.98°C) and critical pressure (7.3773±0.0030MPa), and carbon dioxide under temperature or pressure conditions above the critical point means carbon dioxide under conditions where only the temperature or only the pressure exceeds the critical condition.

[0038] In addition, a specific nano-processing method using the supercritical reverse phase evaporation method involves first injecting an aqueous phase into a mixed fluid of supercritical carbon dioxide, phospholipids as an outer membrane forming substance, and a nucleating agent as an encapsulating substance, and stirring the mixture to generate an emulsion of supercritical carbon dioxide and aqueous phase. Next, the pressure is reduced, causing the carbon dioxide to expand and evaporate, resulting in phase inversion, and generating nanocapsules (nanovesicles) in which the phospholipids cover the surface of the nucleating agent particles with a single layer membrane. Unlike conventional encapsulation methods in which the outer membrane on the surface of the nucleating agent particles becomes multiple membranes, this supercritical reverse phase evaporation method makes it easy to generate capsules with a single layer membrane, making it possible to prepare capsules with smaller diameters. The nucleating agent vesicle can be prepared by, for example, the Bangham method, the extrusion method, the hydration method, the surfactant dialysis method, the reverse phase evaporation method, the freeze-thaw method, the supercritical reverse phase evaporation method, etc. Among these, the supercritical reverse phase evaporation method is particularly preferred.

[0039] The outer membrane constituting the nucleating agent vesicle is, for example, composed of a monolayer membrane, and the outer membrane is composed of a substance containing a biological lipid such as a phospholipid. In this embodiment, a nucleating vesicle whose outer membrane is composed of a material containing a biological lipid such as a phospholipid is referred to as a nucleating liposome. Examples of phospholipids constituting the outer membrane include glycerophospholipids such as phosphatidylcholine, phosphatidylethanolamine, phosphatidylserine, phosphatidic acid, phosphatidylglycerol, phosphatidylinositol, cardiopin, yolk egg lecithin, hydrogenated yolk egg lecithin, soybean lecithin, and hydrogenated soybean lecithin; and sphingophospholipids such as sphingomyelin, ceramide phosphorylethanolamine, and ceramide phosphorylglycerol.

[0040] Other substances that become the outer membrane of the vesicle include dispersants such as nonionic surfactants and mixtures of these with cholesterols or triacylglycerol. Among these, the nonionic surfactants may be one or more of polyglycerol ether, dialkylglycerin, polyoxyethylene hydrogenated castor oil, polyoxyethylene alkyl ether, polyoxyethylene sorbitan fatty acid ester, sorbitan fatty acid ester, polyoxyethylene polyoxypropylene copolymer, polybutadiene-polyoxyethylene copolymer, polybutadiene-poly 2-vinylpyridine, polystyrene-polyacrylic acid copolymer, polyethylene oxide-polyethylethylene copolymer, polyoxyethylene-polycaprolactam copolymer, etc. The cholesterols may be, for example, cholesterol, α-cholestanol, β-cholestanol, cholestane, desmosterol (5,24-cholestadiene-3β-ol), sodium cholate, cholecalciferol, etc.

[0041] The outer membrane of the liposome may be formed from a mixture of a phospholipid and a dispersant. In the decorative sheet 10 of this embodiment, it is preferable that the nucleating agent vesicle is a radical scavenger liposome having an outer membrane made of a phospholipid, and by forming the outer membrane from a phospholipid, it is possible to improve the compatibility between the resin material, which is the main component of the base layer 1, and the vesicle.

[0042] The nucleating agent is not particularly limited as long as it is a substance that is the starting point of crystallization when the resin crystallizes. Examples of the nucleating agent include metal phosphate salts, metal benzoates, metal pimelate salts, metal rosin salts, benzylidene sorbitol, quinacridone, cyanine blue, and talc. In particular, in order to maximize the effect of the nano-processing, it is preferable to use metal phosphate salts, metal benzoates, metal pimelate salts, and metal rosin salts that are non-melting and can be expected to have good transparency, but if the material itself can be made transparent by the nano-processing, colored quinacridone, cyanine blue, talc, etc. can also be used. In addition, a non-melting nucleating agent may be appropriately mixed with melting benzylidene sorbitol.

[0043] As described above, one of the features (invention specific matters) of the decorative sheet 10 of this embodiment is that "the skin layer 1b of the base layer 1 contains a nucleating agent encapsulated in a vesicle." By adding the nucleating agent encapsulated in a vesicle to the resin composition, the effect of dramatically improving the dispersibility of the nucleating agent in the resin material, i.e., in the skin layer 1b of the base layer 1, is achieved, but it is assumed that there are cases in which it is difficult to directly specify this feature in the structure or properties of the object in the completed decorative sheet 10, depending on the circumstances, and it is said to be impractical. The reason is as follows. The nucleating agent added in the form of a vesicle is in a dispersed state with high dispersibility, and the nucleating agent is highly dispersed in the skin layer 1b of the base layer 1 even in the state of the produced decorative sheet 10. However, in the process of producing the decorative sheet 10 after the nucleating agent is added in the form of a vesicle to the resin composition constituting the skin layer 1b of the base layer 1 to produce the base layer 1, various treatments such as compression and hardening of the laminate are usually performed, but such treatments may cause the outer membrane of the vesicle containing the nucleating agent to be crushed or chemically reacted, and the nucleating agent is likely not enclosed (enveloped) by the outer membrane, and the state in which the outer membrane is crushed or chemically reacted varies depending on the treatment process of the decorative sheet 10. In a situation where the nucleating agent is not enclosed by the outer membrane, it is difficult to specify the physical properties themselves in a numerical range, and it is also expected that it may be difficult to determine whether the constituent material of the crushed outer membrane is the outer membrane of the vesicle or a material added separately from the nucleating agent. Thus, the present invention differs from the prior art in that the nucleating agent is highly dispersed in the base layer 1, but it is anticipated that there may be cases where it is impractical to determine within a numerical range a structure or characteristics of the decorative sheet 10 that are analyzed based on measurements, whether this is because the nucleating agent is added in the form of vesicles encapsulating the nucleating agent. The nucleating agent vesicle having the above structure may also be contained in the transparent resin layer 3 .

[0044] <Pattern layer 2> A pattern layer 2 can be provided on the surface of the colored polypropylene film (base layer 1) to impart a pattern to the decorative sheet 10. Examples of the pattern that can be used include wood grain, stone grain, sand grain, tiled, brickwork, fabric, leather, and geometric shapes. Furthermore, a base solid ink layer (not shown) may be provided between the base material layer 1 and the picture layer 2 depending on the level of the desired design. The base solid ink layer is provided so as to cover the entire surface of the base material layer 1. The base solid ink layer may be multi-layered, having two or more layers, as required for hiding properties, etc. Furthermore, the picture layer 2 may be formed by laminating as many plates as necessary to express the desired design. In this way, the picture layer 2 and the base solid ink layer are provided so as to cover the entire surface of the base material layer 1 depending on the level of the desired design. There are various combinations depending on the design to be expressed, that is, the design to be expressed, but there are no particular limitations.

[0045] The constituent materials of the base solid ink layer and the pattern layer 2 are not particularly limited. For example, printing inks or coating agents obtained by dissolving or dispersing a matrix and a colorant such as a dye or pigment in a solvent can be used. As the matrix, for example, various synthetic resins such as oil-based nitrocellulose resin, two-liquid type urethane resin, acrylic resin, styrene resin, polyester resin, urethane resin, polyvinyl resin, alkyd resin, epoxy resin, melamine resin, fluorine resin, silicone resin, and rubber resin, or mixtures or copolymers thereof can be used. In addition, as the colorant, for example, inorganic pigments such as carbon black, titanium white, zinc oxide, red oxide, yellow lead, Prussian blue, and cadmium red, organic pigments such as azo pigments, lake pigments, anthraquinone pigments, phthalocyanine pigments, isoindolinone pigments, and dioxazine pigments, or mixtures thereof can be used. As the solvent, for example, toluene, xylene, ethyl acetate, butyl acetate, methyl alcohol, ethyl alcohol, isopropyl alcohol, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, water, or a mixture thereof can be used.

[0046] In addition, functional additives such as extender pigments, plasticizers, dispersants, surfactants, tackifiers, adhesion aids, drying agents, hardeners, hardening accelerators, and hardening retarders may be added to the base solid ink layer and the picture layer 2 in order to impart various functions. Here, the base solid ink layer and the design layer 2 can be formed by various printing methods such as gravure printing, offset printing, screen printing, electrostatic printing, inkjet printing, etc. In addition, since the base solid ink layer covers the entire surface of the base layer 1, it can also be formed by various coating methods such as roll coating, knife coating, microgravure coating, die coating, etc. These printing and coating methods may be selected separately depending on the layer to be formed, but it is more efficient to select the same method and process them all at once.

[0047] <Transparent resin layer 3> The resin material used as the main component of the transparent resin layer 3 is preferably made of an olefin-based resin, and in addition to polypropylene, polyethylene, polybutene, etc., α-olefins (e.g., propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-pent ... Examples of the copolymer include a homopolymer or copolymer of two or more of α-olefins (such as ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, ethylene-methyl methacrylate copolymer, ethylene-ethyl methacrylate copolymer, ethylene-butyl methacrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, ethylene-butyl acrylate copolymer, etc.) and a copolymer of ethylene or α-olefin with other monomers, such as ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, ethylene-butyl acrylate copolymer, etc. In addition, when the surface strength of the decorative sheet 10 is to be improved, it is preferable to use a highly crystalline polypropylene resin as in the skin layer 1b of the base layer 1. In this embodiment, the term "main component" refers to 90% by mass or more of the target material unless otherwise specified.

[0048] When the transparent resin layer 3 is provided, the thickness of the transparent resin layer 3 is in the range of 50 μm to 100 μm. If the thickness of the transparent resin layer 3 is less than 50 μm, the effect of improving the scratch resistance of the surface of the transparent resin layer 3 is low, and there is a possibility that the purpose of providing the transparent resin layer 3 is reduced. If the thickness of the transparent resin layer 3 exceeds 100 μm, problems such as whitening and cracking during bending may occur. However, when the topcoat layer 4 is provided on the transparent resin layer 3, the thickness of the transparent resin layer 3 may be less than 50 μm. In addition, the resin composition constituting the transparent resin layer 3 may contain various functional additives, such as a heat stabilizer, a light stabilizer, an antiblocking agent, a catalyst trap, a colorant, a light scattering agent, and a gloss adjuster, as necessary. These various functional additives can be appropriately selected from well-known additives.

[0049] <Topcoat layer 4> If further improvement in scratch resistance or adjustment of gloss is required, a top coat layer (surface protection layer) 4 can be provided on the surface of the transparent resin layer 3. In this embodiment, the surface shape (uneven shape) of the top coat layer 4 is designed so that the cutoff value λc on the surface side of the top coat layer 4 is 2.5 mm, the cutoff value λs is 8 μm, the evaluation length is 10 mm, the arithmetic mean roughness (Ra0.008) measured perpendicular to the deposition direction of the top coat layer 4 in accordance with JIS B0601:2001 is 10 μm or less, and the average length RSm of the roughness curve elements and the ten-point mean roughness RzJIS satisfy the condition of the following formula (1). 5 ≦ RSm / RzJIS ≦ 40 (1) When the surface shape of the top coat layer 4 satisfies the above conditions, it is possible to improve the stain resistance and design properties.

[0050] The resin material as the main component of the topcoat layer 4 can be appropriately selected from polyurethane, acrylic silicone, fluorine, epoxy, vinyl, polyester, melamine, aminoalkyd, urea, and other resin materials. The form of the resin material is not particularly limited, and may be water-based, emulsion, solvent-based, or the like. The curing method may also be appropriately selected from one-liquid type, two-liquid type, ultraviolet curing method, and the like.

[0051] As the resin material used as the main component of the topcoat layer 4, a urethane-based material using isocyanate is preferable from the viewpoints of workability, cost, cohesive strength of the resin itself, etc. As the isocyanate, for example, a curing agent such as an adduct, a biuret, or an isocyanurate, which is a derivative of tolylene diisocyanate (TDI), xylylene diisocyanate (XDI), hexamethylene diisocyanate (HMDI), diphenylmethane diisocyanate (MDI), lysine diisocyanate (LDI), isophorone diisocyanate (IPDI), bis(isocyanatemethyl)cyclohexane (HXDI), trimethylhexamethylene diisocyanate (TMDI), etc., can be appropriately selected and used, but in consideration of weather resistance, a curing agent based on hexamethylene diisocyanate (HMDI) or isophorone diisocyanate (IPDI) having a linear molecular structure is preferable. In addition, when improving the surface hardness, it is preferable to use a resin that is cured by active energy rays such as ultraviolet rays and electron beams. These resins can be used in combination with each other, and for example, by using a hybrid type of a thermosetting type and a photosetting type, it is possible to improve the surface hardness, suppress the cure shrinkage, and improve the adhesion.

[0052] A gloss adjuster can be added to the top coat layer 4 to adjust the gloss. Any known gloss adjuster available on the market may be used. For example, fine particles made of inorganic materials such as silica, glass, alumina, calcium carbonate, barium sulfate, etc. may be used. Alternatively, fine particles made of organic materials such as acrylic may be used. However, when high transparency is required, it is preferable to use fine particles of highly transparent silica, glass, acrylic, etc. In particular, Among fine particles such as silica and glass, gloss regulators that are not solid spherical particles but are formed by secondary aggregation of fine primary particles and have a low bulk density have a high matting effect relative to the amount added. Therefore, by using such gloss regulators, the amount of gloss regulator added can be reduced.

[0053] In order to impart various functions to the topcoat layer 4, functional additives such as antibacterial agents and antifungal agents may be added. Also, if necessary, ultraviolet absorbers and light stabilizers may be added. As the ultraviolet absorbers, for example, benzotriazole-based, benzoate-based, benzophenone-based, triazine-based, and cyanoacrylate-based agents can be used. As the light stabilizers, hindered amine-based agents can be used. The thickness of the topcoat layer 4 is preferably within the range of 3 μm to 15 μm. If the thickness of the topcoat layer 4 is less than 3 μm, the effect of improving scratch resistance is low, and there is a possibility that providing the topcoat layer 4 is not meaningful. If the thickness of the topcoat layer 4 exceeds 15 μm, cracks or breaks may occur during bending, which may cause design problems or problems of deteriorated weather resistance.

[0054] The tensile modulus of the decorative sheet 10 of this embodiment, particularly the tensile modulus of the base layer 1 alone, may be in the range of 700 MPa or more and 2000 MPa or less. If the tensile modulus is less than 700 MPa, defects during printing may not be suppressed, or surface smoothness during wrapping may not be maintained. If the tensile modulus exceeds 2000 MPa, the crystallinity is too high, so even if a nucleating agent vesicle is used, defects such as whitening and cracking may occur during bending. The preferred range of the tensile modulus is in the range of 1000 MPa or more and 1800 MPa or less. By keeping it within this range, defects during printing, scratch resistance, surface smoothness during wrapping, and bending can all be achieved in an excellent state.

[0055] "Manufacturing method" A manufacturing example of the decorative sheet 10 will now be described. A nucleating agent vesicle is prepared by encapsulating a nucleating agent in a vesicle, and the prepared nucleating agent vesicle is added to a polypropylene resin to prepare a resin material for a skin layer. Also, an inorganic pigment is added to the polypropylene resin to prepare a resin material for a core layer. The nucleating agent vesicle is prepared, for example, by encapsulating the nucleating agent in a vesicle having a monolayer membrane by supercritical reverse phase evaporation to form a vesicle. The polypropylene resin used for the skin layer 1b is preferably a highly crystalline homopolypropylene resin having an isotactic pentad fraction (mmmm fraction) of 95% or more, which accounts for 30% by mass to 100% by mass.

[0056] The above-mentioned resin materials for the base layer are individually heated and melted, and formed into a sheet having a thickness of 40 μm or more and 200 μm or less by extrusion molding or the like to form the base layer 1. The skin layer 1b and the core layer 1a can be molded separately and then bonded together, for example, using dry lamination to produce the base layer 1. However, it is simpler and more productive to merge the molten resins in a T-die or a feed block before the T-die during extrusion molding and produce the base layer 1 by co-extrusion molding and shaping. At this time, by adjusting the cooling time from the crystallization temperature to the hardening completion temperature by a known adjustment method, the Martens hardness of the skin layer 1b of the base layer 1 can be adjusted to 80 N / mm 2 More than 120N / mm 2 The Martens hardness of the core layer 1a of the substrate layer 1 is controlled within the following range. 2 More than 80N / mm 2 Control within the following ranges.

[0057] Furthermore, if necessary, a design layer 2 is formed on the upper surface of the base layer 1 by printing, and at least one of a transparent resin layer 3 and a top coat layer 4 is formed thereon by printing. In this case, it is preferable that the thickness of the transparent resin layer 3 is within the range of 50 μm or more and 100 μm or less, the thickness of the topcoat layer 4 is within the range of 3 μm or more and 15 μm or less, and the total thickness of the decorative sheet 10 is within the range of 100 μm or more and 250 μm or less. The top coat layer 4 is formed by embossing the surface side of the top coat layer 4 so that the cutoff value λc is 2.5 mm, the cutoff value λs is 8 μm, the evaluation length is 10 mm, and the arithmetic mean roughness (Ra0.008) measured perpendicular to the film-forming direction in accordance with JIS B0601:2001 is 10 μm or less, and the average length RSm of the roughness curve elements and the ten-point mean roughness RzJIS satisfy the condition of the following formula (1). 5 ≦ RSm / RzJIS ≦ 40 (1)

[0058] <Other effects> (1) The decorative sheet 10 of this embodiment has a topcoat layer 4 on a base layer 1. For the surface side of the topcoat layer 4, the arithmetic mean roughness (Ra0.008) according to JIS B0601:2001 measured perpendicular to the film-forming direction of the topcoat layer 4 with a cutoff value λc of 2.5 mm, a cutoff value λs of 8 μm, and an evaluation length of 10 mm is 10 μm or less, and the average length RSm of the roughness curve elements and the ten-point mean roughness RzJIS satisfy the condition of the following formula (1). 5 ≦ RSm / RzJIS ≦ 40 (1) With this configuration, contaminants can be easily wiped off even if they get into the spaces between the projections and recesses formed on the surface of the decorative sheet 10. In addition, because an appropriate projection and recess shape is maintained, the design is not impaired.

[0059] (2) The decorative sheet 10 of this embodiment has a base layer 1 made of a colored polypropylene film having a core layer 1a containing an inorganic pigment and polypropylene resin, and skin layers 1b formed of polypropylene resin on both sides of the core layer 1a. The skin layer 1b of the base layer 1 contains a nano-sized nucleating agent, and the nucleating agent is added in the form of nucleating agent vesicles that are encapsulated in an outer membrane and turned into vesicles. The skin layer 1b has a Martens hardness of 80 N / mm 2 More than 120N / mm 2 The core layer 1a has a Martens hardness of 50 N / mm 2 More than 80N / mm 2The thickness of the base layer 1 is within the range of 40 μm or more and 200 μm or less. According to this configuration, a nucleating agent that improves the crystallinity of polypropylene resin is vesiculated and added as a nucleating agent vesicle, and by further optimizing the Martens hardness and film thickness, a decorative sheet 10 with excellent scratch resistance can be provided.

[0060] (3) In the decorative sheet 10 of this embodiment, the thickness of the core layer 1a is preferably in the range of 3 to 50 times the thickness of one of the skin layers 1b of the base layer 1. According to this configuration, scratch resistance, impact resistance, high concealment properties, and bending workability can all be achieved with a sufficient margin. (4) In the decorative sheet 10 of this embodiment, it is preferable that the amount of nucleating agent vesicle added to the skin layer 1b of the base material layer 1 is within the range of 0.05 parts by mass or more and 0.5 parts by mass or less, calculated as the nucleating agent in the nucleating agent vesicle, per 100 parts by mass of polypropylene resin. According to this configuration, the degree of crystallinity of the polypropylene resin constituting the skin layer 1b of the base layer 1 is sufficiently improved, and the necessary elastic modulus (hardness) can be reliably ensured.

[0061] (5) In the decorative sheet 10 of this embodiment, the nucleating agent vesicle is preferably a nucleating agent liposome having an outer membrane made of phospholipid. This configuration can ensure good compatibility between the resin material, which is the main component of the base layer 1, and the vesicles. (6) In the decorative sheet 10 of this embodiment, the nucleating agent vesicle is preferably one obtained by encapsulating a nucleating agent in a vesicle having a monolayer membrane by supercritical reverse phase evaporation. stomach. According to this configuration, the degree of crystallinity of the polypropylene resin constituting the skin layer 1b of the base material layer 1 is reliably improved, and the necessary elastic modulus (hardness) can be reliably ensured.

[0062] (7) In the decorative sheet 10 of this embodiment, it is preferable that a pattern layer 2 is laminated on one surface of the base layer 1 . According to this configuration, the design of the decorative sheet 10 can be improved. (8) In the decorative sheet 10 of this embodiment, at least one of a transparent resin layer 3 and a top coat layer 4 is laminated on one side of the base layer 1, and it is preferable that the total thickness of the decorative sheet 10 is in the range of 100 μm or more and 250 μm or less. With this configuration, the ability to conform to the edge faces and layered portions of the wood substrate during wrapping processing becomes significantly poor, resulting in insufficient adhesive strength, which can prevent problems such as peeling over time.

[0063] [Example] Specific examples of the decorative sheet 10 of this embodiment will be described below. The raw material for the core layer 1a of the colored polypropylene film was 60 parts by mass of random polypropylene resin containing 4% ethylene and having a melt flow rate (MFR) of 12g / 10min (230°C), to which 40 parts by mass of titanium oxide pigment was added as an inorganic pigment. The raw material for the skin layer 1b was 50 parts by mass of highly crystalline homopolypropylene resin with a pentad fraction of 97.8%, a melt flow rate (MFR) of 15g / 10min (230°C), and a molecular weight distribution MWD (Mw / Mn) of 2.3, to which 50 parts by mass of random polypropylene resin containing 4% ethylene and having a melt flow rate (MFR) of 12g / 10min (230°C) was added. The mixture was co-extruded and shaped using a melt extruder to produce a film with a core layer thickness of 100 μm and a skin layer thickness of 5 μm. Next, both sides of the base layer 1 were subjected to a corona treatment, and a pattern was printed on one of them using a two-component curing urethane ink (V180; manufactured by Toyo Ink Mfg. Co., Ltd.) to form a pattern layer 2. Furthermore, a two-component curing urethane top coat (W184; manufactured by DIC Graphics, application amount 10 g / m) was applied to the surface of the pattern layer 2. 2 ) was applied to form a topcoat layer 4, and a decorative sheet 10 was obtained.

[0064] The case where a nucleating agent is added to the skin layer will be described below. (Method of producing nucleating agent vesicles) First, the method for producing the nucleating agent liposome used in this example will be described. Nucleating agent liposomes were prepared by the above-mentioned supercritical reverse phase evaporation method, by placing 100 parts by mass of methanol, 70 parts by mass of a phosphate metal salt nucleating agent (Adeka STAB NA-21; manufactured by ADEKA) as a nucleating agent, and 5 parts by mass of phosphatidylcholine as a phospholipid constituting the outer membrane of the vesicle in a high-pressure stainless steel container kept at 60°C and sealing it, and injecting carbon dioxide into the container so that the pressure became 20 MPa to create a supercritical state. After that, the container was vigorously stirred and 100 parts by mass of ion-exchanged water was injected. After stirring and mixing for another 15 minutes while keeping the temperature and pressure in the supercritical state, carbon dioxide was discharged from the container and the pressure was returned to atmospheric pressure, thereby obtaining a nucleating agent vesicle in which a nucleating agent is encapsulated in a vesicle having a monolayer outer membrane made of phospholipid.

[0065] The raw material for the core layer 1a of the colored polypropylene film was a mixture of 60 parts by mass of random polypropylene resin with a melt flow rate (MFR) of 12g / 10min (230°C) containing 4% ethylene component and 40 parts by mass of titanium oxide pigment as an inorganic pigment, and the raw material for the skin layer 1b was a mixture of 50 parts by mass of highly crystalline homopolypropylene resin with a pentad fraction of 97.8%, a melt flow rate (MFR) of 15g / 10min (230°C) and a molecular weight distribution MWD (Mw / Mn) of 2.3 containing 4% ethylene component and 50 parts by mass of highly crystalline homopolypropylene resin with a pentad fraction of 97.8%, a melt flow rate (MFR) of 15g / 10min (230°C) and a molecular weight distribution MWD (Mw / Mn) of 2.3 containing 4% ethylene component. 50 parts by mass of random polypropylene resin with a low rate (MFR) of 12 g / 10 min (230 ° C.) and 0.1 parts by mass of the above-mentioned nucleating agent vesicle were added as a nucleating agent, and a film was formed with a core layer thickness of 100 μm and a skin layer thickness of 5 μm by co-extrusion molding and shaping using a melt extruder. The subsequent steps were the same.

[0066] Example 1 After forming the topcoat layer 4, a decorative sheet having an arithmetic mean roughness Ra of 3.7 and a mean length of roughness curve elements RSm / ten-point mean roughness RzJIS of 7.7 was produced as the decorative sheet 10 of Example 1. Example 2 After forming the topcoat layer 4, a decorative sheet having an arithmetic mean roughness Ra of 6.1 and a mean length of roughness curve elements RSm / ten-point mean roughness RzJIS of 11.0 was produced as the decorative sheet 10 of Example 2. Example 3 After forming the topcoat layer 4, a decorative sheet having an arithmetic mean roughness Ra of 2.4 and a mean length of roughness curve elements RSm / ten-point mean roughness RzJIS of 14.1 was produced as the decorative sheet 10 of Example 3. Example 4 After forming the topcoat layer 4, a decorative sheet having an arithmetic mean roughness Ra of 3.8 and a mean length of roughness curve elements RSm / ten-point mean roughness RzJIS of 15.0 was produced, which was designated as the decorative sheet 10 of Example 4.

[0067] Example 5 After forming the topcoat layer 4, a decorative sheet having an arithmetic mean roughness Ra of 5.5 and a mean length of roughness curve elements RSm / ten-point mean roughness RzJIS of 18.6 was produced, which was designated as the decorative sheet 10 of Example 5. Example 6 After forming the topcoat layer 4, a decorative sheet having an arithmetic mean roughness Ra of 2.9 and a mean length of roughness curve elements RSm / ten-point mean roughness RzJIS of 21.8 was produced, which was designated as the decorative sheet 10 of Example 6. Example 7 After forming the topcoat layer 4, a decorative sheet having an arithmetic mean roughness Ra of 4.9 and a mean length of roughness curve elements RSm / ten-point mean roughness RzJIS of 22.1 was produced, which was designated as the decorative sheet 10 of Example 7.

[0068] Example 8 After forming the topcoat layer 4, a decorative sheet having an arithmetic mean roughness Ra of 3.9 and a mean length of roughness curve elements RSm / ten-point mean roughness RzJIS of 25.8 was produced as the decorative sheet 10 of Example 8. Example 9 After forming the topcoat layer 4, a decorative sheet having an arithmetic mean roughness Ra of 3.9 and a mean length of roughness curve elements RSm / ten-point mean roughness RzJIS of 28.9 was produced, which was designated as the decorative sheet 10 of Example 9. Example 10 After forming the topcoat layer 4, a decorative sheet having an arithmetic mean roughness Ra of 3.9 and a mean length of roughness curve elements RSm / ten-point mean roughness RzJIS of 31.1 was produced as the decorative sheet 10 of Example 10.

[0069] Example 11 The skin layer 1b was formed using the polypropylene resin to which the above-mentioned nucleating agent was added. After forming the topcoat layer 4, a decorative sheet having an arithmetic mean roughness Ra of 3.5 and a mean length of roughness curve elements RSm / ten-point mean roughness RzJIS of 7.6 was produced, which was designated as the decorative sheet 10 of Example 11. Example 12 The skin layer 1b was formed using the polypropylene resin with the nucleating agent added thereto. After forming the topcoat layer 4, a decorative sheet was produced with an arithmetic mean roughness Ra of 3.8 and a mean length of roughness curve elements RSm / ten-point mean roughness RzJIS of 33.9, which was designated as the decorative sheet 10 of Example 12.

[0070] Comparative Example 1 The skin layer 1b was formed using the polypropylene resin with the nucleating agent added thereto. After forming the topcoat layer 4, a decorative sheet was produced with an arithmetic mean roughness Ra of 7.8 and a mean length of roughness curve elements RSm / ten-point mean roughness RzJIS of 2.0, which was designated as the decorative sheet 10 of Comparative Example 1. Comparative Example 2 The skin layer 1b was formed using the polypropylene resin with the nucleating agent added thereto. After forming the topcoat layer 4, a decorative sheet was produced with an arithmetic mean roughness Ra of 1.9 and a mean length of roughness curve elements RSm / ten-point mean roughness RzJIS of 47.9, which was designated as the decorative sheet 10 of Comparative Example 2. Comparative Example 3 After forming the topcoat layer 4, a decorative sheet having an arithmetic mean roughness Ra of 7.8 and a mean length of roughness curve elements RSm / ten-point mean roughness RzJIS of 2.0 was produced, which was designated as the decorative sheet 10 of Comparative Example 3.

[0071] <Surface roughness> The arithmetic mean roughness (Ra 0.008) of the surface side of the topcoat layer 4 provided on the decorative sheet 10 in each Example and Comparative Example was measured using a surface roughness meter (manufactured by Mitutoyo Corporation, model number: SJ-310) according to a measurement method in accordance with JIS B0601:2001 under measurement conditions of a cutoff value of 0.008 mm and an evaluation length of 10 mm. Measurements were performed at any five points along a direction perpendicular to the film formation direction, and the average value was taken as the measured value. The measurement results are shown in Table 1.

[0072] <Stain resistance> Blue ink (marker pen) was applied to the decorative sheet 10 of each Example and Comparative Example, and after leaving it for 4 hours, it was wiped off with a neutral detergent or alcohol. In the same manner, crayon, neutral detergent, chemical (ethanol), and food (soy sauce) were applied, left for 6 hours, and then wiped off. The state of the stain after wiping was visually observed and evaluated according to the following evaluation criteria. The evaluation results are shown in Table 1. A rating of ++ or higher is deemed to pose no problems in practical use. +++: No stains left behind ++: Slight staining +: There is some dirt remaining -: A lot of dirt remains

[0073] <Design and tactile feel> Twenty subjects visually observed the surface of the decorative sheet 10 of each Example and Comparative Example, then touched the surface with their hands and evaluated it according to the following evaluation criteria. The evaluation results are shown in Table 1. In addition, if the evaluation is △ or higher, it is evaluated that there is no problem in practical use. 〇: More than 10 people feel that the texture is smooth and the design is good △: 5 to 10 people feel that the texture is natural and the design is good ×: Less than 5 people feel that the texture and design are good

[0074] <Scratch resistance> The scratch resistance was evaluated by conducting a pencil hardness test. In the pencil hardness test, an HB pencil was used, and the angle of the pencil was fixed at 45±1° with respect to the decorative sheet 10 of each Example and Comparative Example, and the pencil was slid with a load of 750 kg applied to it to observe the surface condition of the decorative sheet 10 (based on the old JIS standard JISK5400). The test was conducted five times, and pencil scratches and marks were evaluated according to the following evaluation criteria. The evaluation results are shown in Table 1. If the rating is O or higher, it is evaluated as having no problems in practical use. If the rating is △ or higher, it is evaluated as having no problems in practical use, although its use is limited to furniture and high vertical surfaces that people cannot touch. A rating of O or higher is desirable. ◎: No scratches or marks are visible ○: A slight pencil mark is visible △: Pencil marks are visible ×: Pencil scratches and tears in the colored polypropylene film are visible

[0075] [Table 1]

[0076] As can be seen from Table 1, the decorative sheets 10 of Examples 1 to 12 have optimal surface roughness, so there are no problems with stain resistance and design, and good results are obtained in the pencil hardness test. In particular, Examples 11 and 12 use a base layer containing a nucleating agent, so they obtained very good results in the pencil hardness test.

[0077] On the other hand, in the decorative sheets 10 of Comparative Examples 1 and 2, the Martens hardness was suitable and therefore the scratch resistance was good, but the surface roughness was outside the range, and in Comparative Example 1, the RSm / RzJIS was 2, and the unevenness formed on the surface was large and densely packed, so that the strongly adsorbed contaminants could not be easily wiped off, and dirt remained. In addition, in Comparative Example 2, the RSm / RzJIS was 47.9, and since there were few irregularities formed on the surface and the structure was gentle, it was easy to wipe off contaminants, but it was found that the design and good tactile feel were impaired. Finally, in Comparative Example 3, not only the surface roughness but also the Martens hardness was outside the preferred range, so that not only were the stain resistance and design properties impaired, but the scratch resistance was also reduced.

[0078] From the above, it was clear that the decorative sheets 10 of Examples 1 to 12 were decorative sheets 10 that did not cause any defects in the surface of the base layer 1 and had stain resistance and design properties. The decorative sheet of the present invention is not limited to the above-mentioned embodiments and examples, and various modifications are possible without departing from the characteristics of the invention. [Industrial Applicability]

[0079] The decorative sheet according to the present invention can be used for the surface decoration of interior and exterior materials of buildings such as houses, building materials such as fittings and fixtures, furniture and fixtures, housing equipment, home appliances, etc. In particular, the decorative sheet according to the present invention is suitable for semi-exterior applications such as exterior materials for under-eaves and entrance door materials that are more or less affected by wind and rain, and for applications such as children's rooms, kitchens, dining rooms, washrooms, etc. that require wipeability, water repellency, and stain resistance against marker pens and everyday contaminants. [Explanation of symbols]

[0080] 10 Decorative Sheet 1 Base material layer 2. Picture layer 3 Transparent resin layer 4 Topcoat layer B Substrate

Claims

1. A decorative sheet having at least a surface protective layer on a substrate layer, The cutoff value λc was 2.5 mm, the cutoff value λs was 8 μm, and the evaluation length was 10 mm for the surface side of the surface protective layer. (1) The arithmetic mean roughness (Ra0.008) is 10 μm or less, (2) A decorative sheet characterized in that the average length RSm of the roughness curve elements and the ten-point average roughness Rz JIS satisfy the condition of the following formula (1). 5 ≦ RSm / RzJIS ≦ 40...(1)

2. the base layer has a core layer containing an inorganic pigment and a polypropylene resin, and a skin layer formed on both sides of the core layer and containing a polypropylene resin; A nucleating agent vesicle having a single-layer outer membrane and a nano-sized nucleating agent encapsulated therein is added to the polypropylene resin to form the skin layer; The Martens hardness of the skin layer is 80 N / mm 2 120N / mm or more 2 Within the following range: The Martens hardness of the core layer is 50 N / mm 2 80N / mm or more 2 Within the following range:

2. The decorative sheet according to claim 1, wherein the thickness of the base layer is within a range of 40 μm or more and 200 μm or less.

3. 3. The decorative sheet according to claim 2, wherein the thickness of said core layer is within a range of 3 times to 50 times the thickness of one of said skin layers.

4. A decorative sheet according to claim 2 or claim 3, characterized in that the amount of the nucleating agent vesicle added is within the range of 0.05 parts by mass or more and 0.5 parts by mass or less, calculated as the nucleating agent in the nucleating agent vesicle, per 100 parts by mass of the polypropylene resin.

5. 5. The decorative sheet according to claim 2, wherein the nucleating agent vesicle is a nucleating agent liposome having an outer membrane made of a phospholipid.

6. The decorative sheet according to any one of claims 2 to 5, characterized in that the nucleating agent vesicle is formed by encapsulating the nucleating agent in a vesicle having a monolayer membrane by supercritical reverse phase evaporation.

7. 7. The decorative sheet according to claim 1, further comprising a pattern layer laminated on one surface of said base layer.

Citation Information

Patent Citations

  • Sheet and decorative laminated sheet

    JP2015187378A

  • Decorative sheet

    JP2016097510A

  • Decorative sheet and manufacturing method thereof

    JP2020076015A

  • Decorative sheet and method for producing the same

    JP2021066099A

  • Decorative sheet

    JP7528543B2