Method for producing pulp fiber raw material and pulp fiber raw material as cellulose raw material
The ozonation and alkaline treatment of pulp fibers from used sanitary products reduce hemicellulose and lignin content, transforming them into a high-quality cellulose raw material for various cellulose-derived products.
Patent Information
- Application Number
- JP2024119474
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-12-31
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2039-12-20
AI Technical Summary
Existing methods for recycling pulp fibers from used sanitary products do not effectively utilize the fibers as cellulose raw materials due to the presence of hemicellulose and lignin, which interfere with the properties of cellulose-derived products.
A method involving ozonation and alkaline treatment of pulp fibers to reduce hemicellulose and lignin content to less than 8.0% and 0.10% by mass, respectively, producing a pulp fiber raw material suitable for cellulose applications.
The method effectively transforms pulp fibers into a suitable cellulose raw material by minimizing hemicellulose and lignin content, enhancing the quality of cellulose-derived products such as cellulose nanofibers, viscose rayon, cellulose derivatives, bioethanol, biobutanol, molding materials, and paper products.
Smart Images

Figure 2024144608000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a pulp fiber raw material as a cellulosic raw material from pulp fibers to be treated, and to a pulp fiber raw material as a cellulosic raw material derived from used hygiene products containing pulp fibers. [Background technology]
[0002] 2. Description of the Related Art Technologies for recycling sanitary products such as used disposable diapers are being considered. For example, Patent Document 1 discloses a method for producing recycled pulp that can be reused mainly as sanitary products. Specifically, Patent Document 1 discloses a method for producing recycled pulp that can be reused as sanitary products by recovering pulp fibers from used sanitary products containing pulp fibers and superabsorbent polymers, the method comprising the steps of: decomposing the used sanitary products into pulp fibers and other materials by applying a physical force to the used sanitary products in an aqueous solution containing polyvalent metal ions or an acidic aqueous solution having a pH of 2.5 or less; separating the pulp fibers from the mixture of pulp fibers and other materials produced in the decomposition step; and treating the separated pulp fibers with an ozone-containing aqueous solution having a pH of 2.5 or less.
[0003] In Patent Document 1, the reason for treating pulp fibers with an ozone-containing aqueous solution is that a certain amount of superabsorbent polymer remains in the separated pulp fibers, and the superabsorbent polymer is removed from the pulp fibers by oxidative decomposition and solubilization. Patent Document 1 discloses a method for treating pulp fibers with an ozone-containing aqueous solution, in which an ozone-containing aqueous solution is placed in a treatment tank and the separated pulp fibers are placed in the ozone-containing aqueous solution. In the above method, it is preferable to moderately stir the ozone-containing aqueous solution during treatment to create a water flow, and ozone gas may be blown into the aqueous solution placed in a container to generate a water flow in the ozone-containing aqueous solution by the rising bubbles of ozone gas. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-881 A Summary of the Invention [Problem to be solved by the invention]
[0005] Patent Document 1 describes the reuse of "recycled pulp fiber" as "pulp fiber" itself, but does not describe the use of recycled pulp fiber as a pulp fiber raw material.
[0006] In sanitary products, pulp fibers are often used in absorbents and the like, and the pulp fibers are often derived from coniferous trees. It is known that pulp fibers derived from coniferous trees contain about 50 to about 60% by mass of cellulose as well as about 10 to about 25% by mass of hemicellulose. Hemicellulose is found in large amounts in the cell walls of plants. When pulp fibers are used as a cellulose raw material, for example, the hemicellulose present in the pulp fibers remains in the cellulose recovered from the pulp fibers and thus in the cellulose-derived product, and the remaining hemicellulose may inhibit the function of the cellulose-derived product.
[0007] In the field of sanitary products, pulp fibers are used in absorbents, etc., and hemicellulose contained in pulp fibers is generally not removed from the pulp fibers for the following reasons: (i) it is unlikely to impair the function of the sanitary products (e.g., absorbency), (ii) it imparts elasticity to the pulp fibers, and (iii) it contributes to the yield of the pulp fibers produced. It is also preferred that cellulose-derived products can be produced not only from pulp fibres originating from hygiene products, but also from other pulp fibres to be treated, for example virgin pulp fibres. Accordingly, an object of the present disclosure is to provide a method for producing a pulp fiber raw material suitable as a cellulose raw material. [Means for solving the problem]
[0008] The present inventors have discovered a method for producing a pulp fiber raw material as a cellulose raw material from pulp fibers to be treated, the method comprising an ozone treatment step of forming ozone-treated pulp fibers from the pulp fibers to be treated by supplying an ozone-containing gas to a treatment tank containing a treatment liquid containing a pulp fiber-containing material including the pulp fibers to be treated, and an alkali treatment step of treating the ozone-treated pulp fibers with an alkaline aqueous solution to form the pulp fiber raw material having a hemicellulose content of less than 8.0 mass%. Effect of the Invention
[0009] The method of producing a pulp fiber raw material of the present disclosure is capable of producing a pulp fiber raw material suitable as a cellulose raw material. [Brief description of the drawings]
[0010] [Figure 1] 1 is a flow chart illustrating an embodiment of a method of the present disclosure. [Diagram 2] FIG. 2 is a schematic diagram showing an example of the configuration of an apparatus for the ozone treatment step of FIG. 1. [Diagram 3] FIG. 2 is a schematic diagram showing another example of the configuration of the device for the ozone treatment step in FIG. 1. [Figure 4] FIG. 2 is a schematic diagram showing still another example of the configuration of the device for the ozone treatment step in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Specifically, the present disclosure relates to the following aspects: [Aspect 1] A method for producing a pulp fiber raw material as a cellulose raw material from a pulp fiber to be treated, comprising the steps of: an ozone treatment step of forming ozone-treated pulp fibers from the pulp fibers to be treated by supplying an ozone-containing gas to a treatment tank containing a treatment liquid containing a pulp fiber-containing material containing the pulp fibers to be treated; an alkali treatment step of treating the ozone-treated pulp fibers with an aqueous alkali solution to form the pulp fiber raw material having a hemicellulose content of less than 8.0% by weight; The above method, comprising:
[0012] In the above-mentioned production method, a pulp fiber raw material having a predetermined hemicellulose content, that is, a pulp fiber raw material suitable as a cellulose raw material, can be produced from the pulp fibers to be treated.
[0013] [Aspect 2] 2. The method of claim 1, wherein the pulp fiber material has a lignin content of less than or equal to 0.10% by weight.
[0014] Pulp fibers are known to contain lignin in addition to cellulose. For example, coniferous trees, which are often used in sanitary products, are known to contain 20 to 30% by mass of lignin. Furthermore, when pulp fibers are used, for example, as a cellulose raw material, the lignin present in the pulp fibers may remain in the cellulose recovered from the pulp fibers, and ultimately in cellulose-derived products, and the remaining lignin may inhibit the function of the cellulose-derived products. In the above-described production method, a pulp fiber raw material having a predetermined lignin content, that is, a pulp fiber raw material suitable as a cellulose raw material, can be produced from the pulp fibers to be treated.
[0015] [Aspect 3] 3. The method of any one of the preceding claims, wherein the pulp fiber material has a cellulose content of 94.0% by weight or greater.
[0016] In the above-described production method, a pulp fiber raw material having a predetermined cellulose content, that is, a pulp fiber raw material suitable as a cellulose raw material, can be produced from the pulp fibers to be treated.
[0017] [Aspect 4] A method according to any one of aspects 1 to 3, wherein in the ozone treatment step, the ozone-containing gas is supplied to the treatment tank so that the pulp fibers after the ozone treatment have a hemicellulose content of 10.0% by mass or less.
[0018] In the above-mentioned production method, since the ozone treatment step is performed so that the pulp fibers after the ozone treatment have a predetermined hemicellulose content, the hemicellulose content of the pulp fibers after the ozone treatment can be efficiently reduced in the subsequent alkali treatment step. Therefore, in the above-mentioned production method, a pulp fiber raw material having a predetermined hemicellulose content, i.e., a pulp fiber raw material suitable as a cellulose raw material, can be easily produced from the pulp fibers to be treated.
[0019] [Aspect 5] The method according to any one of aspects 1 to 4, wherein in the ozone treatment step, the ozone-containing gas is contacted with the pulp fiber-containing material so that a CT value, which is the product of the ozone concentration in the ozone-containing gas and the treatment time, is 100 to 12,000 ppm min, thereby forming the pulp fibers after ozone treatment.
[0020] In the above-mentioned production method, in the ozone treatment step, a pulp fiber raw material is formed by contacting an ozone-containing gas with a pulp fiber-containing material under predetermined conditions. Therefore, in the above-mentioned production method, a pulp fiber raw material having a predetermined hemicellulose content, i.e., a pulp fiber raw material suitable as a cellulose raw material, can be easily produced from the pulp fibers to be treated.
[0021] [Aspect 6] A method according to any one of aspects 1 to 5, wherein in the alkali treatment step, the aqueous alkaline solution has a normality of 3.0 N or less. In the above-mentioned manufacturing method, since the aqueous alkaline solution in the alkaline treatment step has a predetermined normality, the pulp fibers and the treatment tank are less likely to be damaged after ozone treatment, and waste liquid from the alkaline treatment step is easily disposed of.
[0022] [Aspect 7] 7. The method according to claim 6, wherein in the alkali treatment step, the aqueous alkaline solution is added in a ratio of 10 to 40 L per 1 kg of dry mass of the ozone-treated pulp fibers. In the above manufacturing method, a predetermined amount of an alkaline aqueous solution having a predetermined normality is added in the alkaline treatment step, which makes it less likely to damage the pulp fibers, treatment tank, etc. after ozone treatment and makes it easier to treat the waste liquid from the alkaline treatment step.
[0023] [Aspect 8] The method according to any one of Aspects 1 to 7, wherein the pulp fiber raw material is a raw material for cellulose nanofibers, viscose rayon, cellulose derivatives, bioethanol, biobutanol, molding materials, or paper products.
[0024] In the above-mentioned production method, the pulp fiber raw material is a raw material for a predetermined application (for cellulose nanofibers, for viscose rayon, for cellulose derivatives, for bioethanol, for biobutanol, for molding materials, or for paper processed products). Therefore, the above-mentioned production method can produce a pulp fiber raw material that can be suitably used as a predetermined cellulose raw material.
[0025] [Aspect 9] The method according to any one of aspects 1 to 8, further comprising a cellulose-using step of forming cellulose nanofibers, viscose rayon, a cellulose derivative, bioethanol, biobutanol, a molding material, or a paper product from the pulp fiber raw material.
[0026] The above-mentioned production method includes a step of using a specific cellulose, and can efficiently produce a specific cellulose-derived product (cellulose nanofiber, viscose rayon, cellulose derivatives, bioethanol, biobutanol, molding materials, or paper products).
[0027] [Aspect 10] A pulp fiber raw material as a cellulose raw material, The pulp fiber raw material has a hemicellulose content of less than 8.0% by mass. The above pulp fiber raw material.
[0028] The above pulp fiber raw material has a predetermined hemicellulose content and is therefore suitable as a cellulose raw material.
[0029] [Aspect 11] A pulp fiber raw material as a cellulose raw material, The pulp fiber raw material has a cellulose content of 94.0% by mass or more. The above pulp fiber raw material.
[0030] The above pulp fiber raw material has a predetermined cellulose content and is therefore suitable as a cellulose raw material.
[0031] [Aspect 12] 12. The pulp fiber material of claim 10 or 11, wherein the pulp fiber material has a lignin content of less than or equal to 0.10% by weight. The above pulp fiber raw material has a predetermined lignin content and is therefore suitable as a cellulose raw material.
[0032] [Aspect 13] 13. The pulp fiber raw material according to any one of aspects 10 to 12, derived from a used sanitary product containing pulp fibers. The above pulp fiber raw material is derived from used sanitary products, which is preferable from the viewpoint of environmental protection.
[0033] [Aspect 14] The pulp fiber raw material according to any one of aspects 10 to 13, wherein the pulp fiber raw material is a raw material for cellulose nanofibers, viscose rayon, cellulose derivatives, bioethanol, biobutanol, molding materials, or paper products. The pulp fiber raw material is suitable as a cellulose raw material for certain applications.
[0034] [Aspect 15] A cellulose nanofiber, a viscose rayon, a cellulose derivative, bioethanol, biobutanol, a molding material, or a paper product, which is produced using the pulp fiber raw material according to any one of aspects 10 to 14 as a raw material. The cellulose nanofiber, viscose rayon, cellulose derivative, molding material, or paper product has a high cellulose content. The bioethanol and biobutanol have a high ethanol and butanol content, respectively.
[0035] [Aspect 16] The method includes the steps of: a preparation step of preparing the treatment tank having a pulp fiber-containing material supply port, a treatment liquid discharge port, and an ozone-containing gas supply port disposed below the treatment tank; a pulp fiber-containing material supplying step of supplying the pulp fiber-containing material from the pulp fiber-containing material supply port to the treatment tank; an ozone-containing gas supplying step of supplying the ozone-containing gas from the ozone-containing gas supply port to the treatment liquid in the treatment tank; the ozone treatment step of contacting the pulp fiber-containing material with the ozone-containing gas while allowing the ozone-containing gas to rise in the treatment tank, thereby forming the ozone-treated pulp fibers from the pulp fibers to be treated; a treatment liquid discharge step of discharging the treatment liquid containing the pulp fibers after the ozone treatment from the treatment liquid discharge port; 16. The method according to any one of aspects 1 to 15, comprising:
[0036] Since hemicellulose has a lower specific gravity than cellulose, pulp fibers with a relatively low hemicellulose content (pulp fibers with a relatively high cellulose content) tend to have a relatively higher specific gravity than pulp fibers with a relatively high hemicellulose content (pulp fibers with a relatively low cellulose content). On the other hand, in the solution, the ozone-containing gas rises while consuming ozone, so the ozone-containing gas present at the lower position tends to have a higher ozone content (i.e., is fresher) than the ozone-containing gas present at the upper position.
[0037] The above-mentioned manufacturing method includes a predetermined preparation step, a pulp fiber-containing material supply step, an ozone-containing gas supply step, an ozone treatment step, and a treatment liquid discharge step. In the ozone treatment step, the pulp fiber-containing material is contacted with the ozone-containing gas while the ozone-containing gas is raised.
[0038] In the above-mentioned production method, pulp fibers having a relatively low hemicellulose content (pulp fibers having a relatively high cellulose content) have a higher sedimentation tendency than pulp fibers having a relatively high hemicellulose content (pulp fibers having a relatively low cellulose content), and fresh ozone-containing gas comes into contact with the pulp fibers having a relatively low hemicellulose content, which facilitates further decomposition of the hemicellulose contained therein. Therefore, the above-mentioned production method can produce a pulp fiber raw material that can be suitably used as a cellulose raw material.
[0039] In general, the higher the lignin content of pulp fibers, the lower their specific gravity tends to be. Therefore, in the above-described production method, pulp fibers having a relatively low lignin content have a relatively higher sedimentation tendency than pulp fibers having a relatively high lignin content, and therefore fresher ozone-containing gas comes into contact with the pulp fibers having a relatively low lignin content, thereby further decomposing the lignin contained therein.
[0040] The ozone-containing gas supply port is located below the treatment tank, and specifically, this means within a range of preferably 30%, more preferably 20%, and even more preferably 10% of the height of the treatment tank from the bottom of the treatment tank. In addition, the pulp fiber-containing material supply port may be located below the ozone-containing gas supply port or may be located above it, and the treatment liquid discharge port may be located below the ozone-containing gas supply port or may be located above it.
[0041] The manufacturing method described in the sixteenth embodiment includes both so-called continuous and batch manufacturing methods. In addition, "rising the ozone-containing gas" means that the ozone-containing gas rises as a whole, and includes the case where the ozone-containing gas rises vertically as a whole while being stirred horizontally when the treatment liquid in the treatment tank is stirred.
[0042] [Aspect 17] The treatment liquid outlet is disposed below the pulp fiber-containing material supply port, In the ozone treatment step, the pulp fiber-containing material is contacted with the ozone-containing gas while being lowered. The method according to embodiment 16.
[0043] In the above-mentioned manufacturing method, the descending pulp fiber-containing material is brought into contact with the ascending ozone-containing gas, so that the frequency of contact between the pulp fiber-containing material and the ozone-containing gas increases, narrowing the distribution of the hemicellulose content of the pulp fibers (pulp fibers after ozone treatment) contained in the treatment liquid (reducing the variation). In addition, since fresh ozone-containing gas can come into contact with pulp fibers with a relatively low hemicellulose content, the hemicellulose content of the pulp fibers (pulp fibers after ozone treatment) contained in the treatment liquid tends to be low. Furthermore, since the treatment liquid outlet is disposed below the pulp fiber-containing material supply port, pulp fibers with a relatively low hemicellulose content (pulp fibers with a relatively high cellulose content) tend to be discharged from the treatment liquid outlet.
[0044] The manufacturing method described in embodiment 17 includes both so-called continuous and batch manufacturing methods. In addition, "descending the pulp fiber-containing material" means that at least a part of the pulp fiber-containing material is descending, and includes, for example, the entire treatment liquid in the treatment tank when the entire treatment liquid is descending, and the descending part of the pulp fiber-containing material when the treatment liquid in the treatment tank is undergoing vertical convection, etc.
[0045] [Aspect 18] The treatment liquid outlet is disposed above the pulp fiber-containing material supply port, In the ozone treatment step, the pulp fiber-containing material is contacted with the ozone-containing gas while the pulp fiber-containing material is allowed to rise. The method according to embodiment 16.
[0046] In the above-mentioned manufacturing method, the rising pulp fiber-containing material is brought into contact with the rising ozone-containing gas, so that the time that the pulp fiber-containing material is in contact with the ozone-containing gas is longer, which makes it easier to reduce the hemicellulose content in the pulp fibers.
[0047] The manufacturing method described in embodiment 18 includes both so-called continuous and batch manufacturing methods. In addition, "rising the pulp fiber-containing material" means that at least a part of the pulp fiber-containing material is rising, and includes, for example, the entire treatment liquid in the treatment tank when the entire treatment liquid is rising, and the rising part of the pulp fiber-containing material when the treatment liquid in the treatment tank is convecting up and down.
[0048] [Aspect 19] A method according to any one of aspects 16 to 18, wherein in the pulp fiber-containing material supplying step, the pulp fiber-containing material is continuously supplied from the pulp fiber-containing material supplying port to the treatment tank at a first flow rate, and in the treatment liquid discharging step, the treatment liquid is continuously discharged from the treatment liquid discharging port at a second flow rate.
[0049] In the above manufacturing method, in the pulp fiber-containing material supply step, the pulp fiber-containing material is continuously supplied from a pulp fiber-containing material supply port to a treatment tank at a first flow rate, and in the treatment liquid discharge step, the treatment liquid is continuously discharged from a treatment liquid discharge port at a second flow rate, so that the treatment time of the pulp fiber-containing material to be treated is made uniform and the distribution of the hemicellulose content of the pulp fiber raw material contained in the treatment liquid is narrowed (the variation is reduced). Therefore, the above-mentioned production method can produce a pulp fiber raw material that can be suitably used as a cellulose raw material.
[0050] [Aspect 20] The pulp fiber-containing material comprises the pulp fiber to be treated derived from a used sanitary product and a superabsorbent polymer; In the ozone treatment step, at least a portion of the superabsorbent polymer is dissolved in the treatment liquid. 20. The method according to any one of aspects 16 to 19.
[0051] In used sanitary products, in absorbents containing pulp fibers and superabsorbent polymers, (i) as the superabsorbent polymer absorbs liquids such as bodily fluids, it swells and entangles the pulp fibers, and (ii) the enlarged superabsorbent polymers entangle the pulp fibers together, causing gel blocking, and so on, and thus multiple superabsorbent polymers and multiple pulp fibers often form connected structures.
[0052] In the above-mentioned manufacturing method, in the ozone treatment step, the pulp fiber-containing material is contacted with the ozone-containing gas while the ozone-containing gas is raised. Among the free superabsorbent polymer, the free pulp fiber, and the connected structure, the free superabsorbent polymer and the connected structure, which have relatively low buoyancy, tend to sink more easily than the free pulp fiber, which has relatively high buoyancy. On the other hand, since the ozone-containing gas rises while consuming ozone and treating the pulp fiber-containing material, the ozone-containing gas present at the lower position tends to have a higher ozone content (i.e., is fresher) than the ozone-containing gas present at the upper position.
[0053] Therefore, in the above-mentioned manufacturing method, the free superabsorbent polymer and the superabsorbent polymer in the connected structure, which have a relatively high sedimentation tendency, can be accurately oxidized and decomposed with fresher ozone-containing gas to liberate the pulp fibers that constituted the connected structure, and the free pulp fibers, which have a relatively low sedimentation tendency and take a relatively long time to reach the treatment liquid outlet, can be treated over a long period of time with the ozone-containing gas to decompose the hemicellulose contained in the free pulp fibers.
[0054] Furthermore, as described above, pulp fibers having a relatively low hemicellulose content (pulp fibers having a relatively high cellulose content) have a higher sedimentation tendency than pulp fibers having a relatively high hemicellulose content (pulp fibers having a relatively low cellulose content), and in the above-mentioned manufacturing method, fresher ozone-containing gas comes into contact with the pulp fibers having a relatively low hemicellulose content, thereby further decomposing the hemicellulose contained therein. Therefore, the above-mentioned production method can produce a pulp fiber raw material that can be suitably used as a cellulose raw material.
[0055] [Aspect 21] 21. The method according to aspect 20, wherein the treatment liquid is acidic, weakly acidic or neutral. In the above-mentioned production method, the treatment liquid is acidic (specifically, pH is more than 0.0 and less than 3.0, preferably pH 2.5 or more and less than 3.0), weakly acidic (specifically, pH 3.0 or more and less than 6.0), or neutral (specifically, pH 6.0 or more and pH 8.0 or less, preferably pH 6.0 or more and pH 7.0 or less). Therefore, the superabsorbent polymer to be treated can be inactivated by the acid, or if the superabsorbent polymer to be treated has already been inactivated, the superabsorbent polymer can be continuously maintained in an inactivated state. As a result, even if the superabsorbent polymer and the pulp fiber form a connected structure, the ozone in the ozone-containing gas can remove the superabsorbent polymer constituting the connected structure, and the ozone in the ozone-containing gas can act on the pulp fiber constituting the connected structure to reduce the hemicellulose content of the pulp fiber. Therefore, the above-mentioned production method can produce a pulp fiber raw material that can be suitably used as a cellulose raw material.
[0056] [Aspect 22] 22. The method of claim 20 or 21, further comprising a deactivation step, prior to the pulp fiber-containing material providing step, of deactivating the superabsorbent polymer with an acid.
[0057] Because the above manufacturing method further includes a specified inactivation step, even if the superabsorbent polymer and the pulp fibers form a connected structure, the ozone in the ozone-containing gas can remove the superabsorbent polymer that constitutes the connected structure immediately after the pulp fiber-containing material containing the superabsorbent polymer and pulp fibers derived from the used sanitary products is supplied to the treatment tank, and the ozone in the ozone-containing gas can act on the pulp fibers that constitute the connected structure to reduce the hemicellulose content of the pulp fibers. Therefore, the above-mentioned production method can produce a pulp fiber raw material that can be suitably used as a cellulose raw material.
[0058] [Aspect 23] 23. The method of claim 22, wherein the acid is an acid capable of forming a complex with a metal ion contained in feces.
[0059] In the above-mentioned production method, since the above-mentioned acid is capable of forming a complex with the metal ions contained in the excrement, the produced pulp fiber raw material is less likely to contain metal ions. Therefore, in the process of using the pulp fiber raw material from the pulp fiber raw material, the metal ions and their precipitates are less likely to damage the equipment used in the process of using the pulp fiber raw material and are less likely to inhibit the pulp fiber raw material from being refined.
[0060] Hereinafter, a method for producing a pulp fiber raw material from pulp fibers to be treated (hereinafter, sometimes simply referred to as a "method for producing a pulp fiber raw material") will be described. The pulp fibers to be treated are not particularly limited as long as they are pulp fibers, and examples thereof include unused pulp fibers (e.g., virgin pulp fibers), used pulp fibers (e.g., pulp fibers derived from used sanitary products), and the like.
[0061] The above-mentioned used sanitary products are sanitary products that have been used by a user, and include sanitary products that have absorbed the user's liquid excrement, sanitary products that have been used but have not absorbed excrement, and sanitary products that have been discarded unused.
[0062] In this specification, the term "to be treated" in "to be treated" is a modifier used to distinguish between pulp fibers before treatment and raw pulp fiber material after treatment, and has no other meaning. In addition, in this specification, the "pulp fibers to be treated" include embodiments of used pulp fibers, particularly pulp fibers derived from used sanitary products, and in this case, the "pulp fibers to be treated" may be referred to simply as "pulp fibers."
[0063] A configuration example of a sanitary product will be described. The sanitary product includes, for example, a liquid-permeable sheet, a liquid-impermeable sheet, and an absorbent disposed between the liquid-permeable sheet and the liquid-impermeable sheet. Examples of the sanitary product include paper diapers, urine absorption pads, sanitary napkins, bed sheets, and pet sheets.
[0064] Examples of the constituent members of the liquid-permeable sheet include nonwoven fabrics or films, specifically liquid-permeable nonwoven fabrics, synthetic resin films having liquid-permeable holes, composite sheets thereof, etc. Examples of the constituent members of the liquid-impermeable sheet include nonwoven fabrics or films, specifically liquid-impermeable nonwoven fabrics, liquid-impermeable synthetic resin films, composite sheets thereof, etc.
[0065] The components of the absorbent body include an absorbent core (e.g., pulp fibers and superabsorbent polymers) and a core wrap. The pulp fibers are not particularly limited as long as they can be used in sanitary products, and examples of the pulp fibers include cellulosic fibers. Examples of the cellulosic fibers include wood pulp (e.g., softwood pulp, hardwood pulp), crosslinked pulp, non-wood pulp, etc. The superabsorbent polymers (SAPs) are not particularly limited as long as they can be used in sanitary products, and examples of the SAPs include polyacrylates, polysulfonates, and maleic anhydrides.
[0066] One side and the other side of the absorbent are respectively bonded to the liquid-permeable sheet and the liquid-impermeable sheet via an adhesive. In plan view, the portion (peripheral portion) of the liquid-permeable sheet that extends outwardly from the absorbent so as to surround the absorbent is bonded to the portion (peripheral portion) of the liquid-impermeable sheet that extends outwardly from the absorbent so as to surround the absorbent via an adhesive. Thus, the absorbent is enclosed inside the bonded body of the liquid-permeable sheet and the liquid-impermeable sheet. There is no particular restriction on the adhesive as long as it can be used as a sanitary product and is softened by hot water as described below to reduce the bonding strength, and examples of the adhesive include hot melt adhesives. Examples of hot melt adhesives include pressure-sensitive adhesives or heat-sensitive adhesives that are mainly made of rubber such as styrene-ethylene-butadiene-styrene, styrene-butadiene-styrene, and styrene-isoprene-styrene, or olefin-based adhesives such as polyethylene.
[0067] Fig. 1 is a flow chart showing a material separation method for separating a used sanitary product into its constituent materials. This material separation method is a method for separating a used sanitary product into a film, a nonwoven fabric, a pulp fiber, and a superabsorbent polymer. This material separation method includes a pretreatment step S11, a decomposition step S12, and a separation step S13. In the pretreatment step S11, the used sanitary product is swelled with water. In the decomposition step S12, the swollen used sanitary product is subjected to a physical impact to decompose the used sanitary product into a film, a nonwoven fabric, a core wrap, etc., and an absorbent core (e.g., pulp fiber and a superabsorbent polymer). In the separation step S13, the film, the nonwoven fabric, the pulp fiber, and the superabsorbent polymer are separated.
[0068] In addition, when a mixture of pulp fibers and a superabsorbent polymer (a pulp fiber-containing material) is obtained in advance by some method, the steps before the pretreatment step S11, the decomposition step S12, and the separation step S13 in the method for producing pulp fibers after ozone treatment are not necessary. Each step will be described below.
[0069] In the pre-treatment step S11, a number of used sanitary products are allowed to absorb water and swell in the state in which they were collected from the outside, i.e., without breaking, cutting, etc., and without inactivating the highly water-absorbent polymer in the absorbent body, if they are rolled or folded. In this embodiment, the used sanitary products are allowed to absorb hot water and swell, or the absorbed water is absorbed and expanded, and then the absorbed water is heated to turn it into hot water. Hot water refers to water at a temperature higher than room temperature (20°C±15°C (5 to 35°C): JIS Z 8703).
[0070] Usually, the amount of liquid excrement actually absorbed in the used sanitary product is very small compared to the maximum absorption amount that the sanitary product can absorb (for example, about 10 to 20% by mass of the maximum absorption amount). In the present embodiment, in the pretreatment step S11, the used sanitary product is immersed in hot water to absorb water to an amount close to the maximum absorption amount of the used sanitary product (for example, 80% by mass or more of the maximum absorption amount). Alternatively, the used sanitary product is immersed in water at room temperature to absorb water to an amount close to the maximum absorption amount of the used sanitary product, and then the used sanitary product as a whole is heated to the temperature of the hot water. This allows the used sanitary product to be in a very expanded state with hot water or water at room temperature (hereinafter also simply referred to as "hot water"). As a result, a very high internal pressure is generated in the used sanitary product. The purpose of turning the water into hot water is mainly to weaken the adhesive strength of the adhesive, as described later.
[0071] Here, when the used sanitary product is initially rolled or folded with the liquid-impermeable sheet on the outside (with the liquid-permeable sheet hidden inside), the absorbent body of the used sanitary product absorbs the warm water and expands in the warm water when immersed in warm water. As a result, the internal pressure of the used sanitary product increases, and a force acts on the used sanitary product to open outward, causing the rolled or folded used sanitary product to open outward and become roughly flat. That is, the used sanitary product can be made to be in a flat, unfolded state in the warm water. At this time, the absorbent body of the used sanitary product has absorbed a large amount of warm water and expanded significantly, so that its surface, i.e., any part of the liquid-permeable sheet or the liquid-impermeable sheet enveloping the absorbent body, is in a state that is likely to easily burst. That is, the pre-treatment step S11 can make the used sanitary product in a state where any part of the surface is likely to tear or break. Furthermore, if a used sanitary product is initially laid out flat, any part of its surface may easily burst apart in that state, which does not occur if the used sanitary product is broken or otherwise damaged.
[0072] Furthermore, when a used sanitary product is immersed in and / or absorbs hot water, the adhesive (e.g., hot melt adhesive) used to bond the components together can be softened by the heat of the hot water, thereby reducing the bonding strength of the adhesive. For example, the adhesive bonding the peripheral portion of the liquid-permeable sheet to the peripheral portion of the liquid-impermeable sheet can be softened by the heat of the hot water, thereby reducing the bonding strength of the adhesive. Furthermore, the adhesive bonding the liquid-permeable sheet to the absorbent and the adhesive bonding the liquid-impermeable sheet to the absorbent can be softened by the heat of the hot water, thereby reducing the bonding strength of those adhesives.
[0073] In this way, in the pre-treatment step S11, the expansion of the absorbent body of the used sanitary product can cause some part of the surface of the used sanitary product to be in a state where it is about to burst and the adhesive strength is reduced. By putting the used sanitary product in such a state, the used sanitary product can be reliably disassembled in the disassembly step described below.
[0074] The temperature of the hot water in the pretreatment step S11 is not particularly limited as long as the adhesive of the used sanitary product can be softened, but for example, it can be 60°C or higher, and preferably 70°C or higher and 98°C or lower. By setting the temperature of the hot water to 70°C or higher, the adhesive bonding between the components can be softened by the heat of the hot water, and the bonding strength of the adhesive can be further reduced. By setting the temperature of the hot water to 98°C or lower, the hot water is reliably present as a liquid, so that the hot water can be more reliably absorbed by the used sanitary product. The expansion of the absorbent and the heat of the hot water can more reliably create a state in which the surface of the used sanitary product is about to burst and the bonding strength of the adhesive is reduced. Regarding the temperature measurement, the temperature of the hot water in which the used sanitary product is immersed is measured, or the temperature (the tip of the temperature sensor is inserted) 5 mm inside the surface of the used sanitary product that has absorbed water to an amount close to the maximum absorption amount is measured.
[0075] In addition, sterilization of the constituent materials is extremely important when recycling used sanitary products. By setting the temperature of the hot water at 70°C or higher, it is possible to sterilize (disinfect) the used sanitary products, which is preferable.
[0076] The treatment time in the pretreatment step S11, i.e., the time for which the used sanitary goods are immersed in warm water, is not particularly limited as long as the absorbent body of the used sanitary goods can expand, but is, for example, 2 to 60 minutes, and preferably 4 to 30 minutes. If the time is too short, the absorbent body cannot expand sufficiently, and if it is too long, time is wasted and the treatment cost increases unnecessarily.
[0077] The amount of hot water absorbed by the absorbent in the pre-treatment step S11 is not particularly limited as long as the absorbent can expand to an extent that the used sanitary goods can be decomposed in the decomposition step described below, but may be, for example, 80% by mass or more of the maximum absorption amount of the used sanitary goods, and preferably 90% by mass or more. This allows the used sanitary goods to be fully expanded with water. As a result, an extremely high internal pressure can be generated in the absorbent of the used sanitary goods.
[0078] However, the maximum absorption amount is measured according to the following procedure. (1) Dry unused sanitary products in an atmosphere of 100°C or higher, and measure the mass of the sanitary products. (2) If the sanitary product contains elastic material (e.g., elastic parts around the legs, waist, etc.) that can form pockets that make it difficult for water to reach the absorbent core, the elastic parts are cut to flatten the sanitary product. (3) Immerse the sanitary product with the liquid-permeable sheet facing down in a water bath filled with sufficient tap water and leave it for 30 minutes. (4) After leaving it, the sanitary product is placed on a net with the liquid-permeable sheet facing down, and after draining the water for 20 minutes, the mass of the sanitary product is measured. The difference in mass before and after immersion in tap water is defined as the maximum absorption amount.
[0079] Next, in the decomposition process S12, a physical impact is applied to the multiple used sanitary products that have been unfolded and swollen in the pre-treatment process S11, and the multiple used sanitary products are decomposed into a film (liquid-impermeable sheet), a nonwoven fabric (liquid-permeable sheet), a core wrap, and an absorbent core (e.g., an absorbent body and a superabsorbent polymer).
[0080] The used sanitary product is flattened in the pretreatment step S11, and some part of the surface is about to burst due to expansion. In this embodiment, the adhesive strength of the adhesive is reduced by the heat of the hot water. Therefore, in the disassembly step S12, a physical impact is applied to the used sanitary product in this state, and the bonded part between the liquid-permeable sheet (nonwoven fabric) and the liquid-impermeable sheet (film) where the bond strength is particularly reduced among some parts of the surface bursts. This makes it possible to tear (peel off) the bonded part. There is no particular limit to the physical impact, but examples include a method of hitting the used sanitary product against a surface made of a material harder than the used sanitary product, and a method of pressing the used sanitary product from both sides while passing it between a pair of rolls arranged facing each other.
[0081] In this embodiment, the disassembly step S12 includes a step of putting a plurality of swollen used sanitary products into the bottom of a rotating drum with a horizontal rotating shaft, and a step of rotating the rotating drum around the rotating shaft to pull up the plurality of used sanitary products to the top of the rotating drum and slam them against the bottom. This allows a stable, continuous (continuous) and easy application of physical impact to the plurality of used sanitary products. An example of the rotating drum is the rotating drum of a washing tub of a horizontal washing machine, and therefore the disassembly step S12 can be performed using an existing horizontal washing machine (for example, ECO-22B, manufactured by Inamoto Seisakusho Co., Ltd.). The size of the rotating drum is not particularly limited as long as the above impact can be realized, and the inner diameter and depth are, for example, 50 to 150 cm and 30 to 120 cm. The rotation speed of the rotating drum is not particularly limited as long as the above impact can be realized, and for example, 30 times / min to 100 times / min.
[0082] In addition, the temperature of the used sanitary goods is kept relatively high by the hot water absorbed in the used sanitary goods, but from the viewpoint of suppressing the temperature drop of the adhesive and maintaining the sterilization effect, the temperature of the atmosphere in the rotating drum is preferably 70 ° C or more, more preferably 75 ° C or more. From the viewpoint of handling the used sanitary goods, the temperature in the rotating drum is preferably 98 ° C or less, more preferably 90 ° C or less. It is preferable that the amount of water in the rotating drum is as small as possible, and it is preferable that the amount of water is small enough that the used sanitary goods are not below the water surface at least at the bottom. If the used sanitary goods are below the water surface, the impact on the used sanitary goods is absorbed by the water, making it difficult to give the desired impact to the used sanitary goods. The time for which the rotating drum is rotated is not particularly limited as long as the liquid-permeable sheet, the liquid-impermeable sheet, the core wrap, etc. can be disassembled from the absorbent core, but is, for example, 2 to 40 minutes, preferably 4 to 20 minutes.
[0083] In the used sanitary product, the joint between the liquid-permeable sheet (nonwoven fabric) and the liquid-impermeable sheet (film) bursts and tears due to physical impact. At the same time, the absorbent core (e.g., pulp fibers and superabsorbent polymer) in the used sanitary product is ejected (flew out) through the tear due to the internal pressure of the absorbent. This makes it possible to more reliably decompose the used sanitary product into the liquid-permeable sheet (nonwoven fabric), the liquid-impermeable sheet (film), the core wrap, etc., and the absorbent core (e.g., a pulp fiber-containing material containing pulp fibers and superabsorbent polymer).
[0084] Next, in a separation step S13, the plurality of films (liquid-impermeable sheets), the plurality of nonwoven fabrics (liquid-permeable sheets), the core wrap, etc. are separated from the absorbent core (e.g., pulp fibers and superabsorbent polymer). However, the nonwoven fabric may remain attached to the film. The above separation method is not particularly limited, but may be, for example, a method using a sieve that does not allow the liquid-permeable sheets, the liquid-impermeable sheets, the core wrap, etc. to pass but allows the absorbent core to pass.
[0085] In this embodiment, the separation step S13 may include an inactivation step S31 in which the superabsorbent polymer is inactivated with an aqueous solution containing an inactivating agent before separating the film, nonwoven fabric, core wrap, etc. from the absorbent core, and a first separation step S32 in which the film and nonwoven fabric are separated from a mixture containing pulp fibers, inactivated superabsorbent polymer, and wastewater discharged from the superabsorbent polymer by inactivation.
[0086] In the inactivation step S31, prior to the first separation step S32, the liquid-permeable sheet (nonwoven fabric), the liquid-impermeable sheet (film), and the absorbent (pulp fibers and superabsorbent polymer) are immersed in an aqueous solution containing an inactivating agent capable of inactivating the superabsorbent polymer. This makes it possible to inactivate the superabsorbent polymer attached to the liquid-permeable sheet, the liquid-impermeable sheet, and the pulp fibers. This makes it possible to convert the superabsorbent polymer, which is in a high viscosity state before inactivation, into a superabsorbent polymer in a low viscosity state by dehydration through inactivation.
[0087] Here, the inactivating agent is not particularly limited, but examples thereof include acids (e.g., inorganic acids and organic acids), lime, calcium chloride, magnesium sulfate, magnesium chloride, aluminum sulfate, aluminum chloride, and the like. The above-mentioned acids are preferred because they do not leave ash on the pulp fibers. When an acid is used as the inactivating agent, the pH is preferably 2.5 or less, and more preferably 1.3 to 2.4. If the pH is too high, the water absorption capacity of the superabsorbent polymer cannot be sufficiently reduced. In addition, there is a risk of the sterilizing ability being reduced. If the pH is too low, there is a risk of corrosion of the equipment, and a large amount of alkaline chemicals is required for neutralization treatment during wastewater treatment.
[0088] Examples of the inorganic acid include sulfuric acid, hydrochloric acid, and nitric acid, with sulfuric acid being preferred from the viewpoints of not containing chlorine and cost. On the other hand, examples of the organic acid include citric acid, tartaric acid, glycolic acid, malic acid, succinic acid, acetic acid, and ascorbic acid, with acids capable of forming complexes with metal ions contained in excrement, such as hydroxycarbonate-based organic acids such as citric acid, tartaric acid, and gluconic acid, being particularly preferred. Examples of metal ions contained in excrement include calcium ions. This is because the metal ions in excrement can be trapped and removed by the chelating effect of the acid capable of forming complexes with the metal ions contained in excrement. In addition, citric acid is expected to have a high dirt component removal effect due to its cleaning effect. In addition, since the pH changes depending on the water temperature, the pH in this disclosure refers to the pH measured at an aqueous solution temperature of 20°C.
[0089] The treatment temperature of the inactivation step S31, i.e., the temperature of the aqueous solution containing the inactivating agent, is not particularly limited as long as the inactivation reaction proceeds. The treatment temperature may be room temperature or higher than room temperature, and may be, for example, 15 to 30°C. The treatment time of the inactivation step S31, i.e., the time for immersing the liquid-permeable sheet, the liquid-impermeable sheet, and the absorbent in the aqueous solution containing the inactivating agent, is not particularly limited as long as the superabsorbent polymer is inactivated and dehydrated, and may be, for example, 2 to 60 minutes, and preferably 5 to 30 minutes. The amount of the aqueous solution in the inactivation step S31, i.e., the amount of the aqueous solution containing the inactivating agent, is not particularly limited as long as the inactivation reaction proceeds. The amount of the aqueous solution is, for example, preferably 300 to 3000 parts by mass, more preferably 500 to 2500 parts by mass, and even more preferably 1000 to 2000 parts by mass, relative to 100 parts by mass of the used sanitary goods.
[0090] In the first separation step S32, the liquid-permeable sheet (nonwoven fabric), the liquid-impermeable sheet (film) and the core wrap are separated from a mixture containing pulp fibers, the inactivated superabsorbent polymer and wastewater discharged from the superabsorbent polymer by inactivation. Note that the wastewater is wastewater containing the water released from the superabsorbent polymer by dehydration with an aqueous solution containing an inactivating agent in the inactivation step S31, i.e., liquid derived from excrement and water derived from warm water.
[0091] In the first separation step S32, the method of separating the liquid-permeable sheet and the liquid-impermeable sheet from the pulp fibers, the superabsorbent polymer, and the wastewater (pulp fiber-containing material) is not particularly limited. For example, the products (liquid-permeable sheet, liquid-impermeable sheet, pulp fibers, superabsorbent polymer, wastewater, etc.) generated by the inactivation step are discharged while passing through a screen with a mesh size of 5 to 100 mm, preferably 10 to 60 mm. As a result, the pulp fibers, superabsorbent polymer, and wastewater are discharged while the liquid-permeable sheet and the liquid-impermeable sheet remain on the screen, and the products can be separated. Note that other large-shaped objects such as nonwoven fabrics and films may remain on the screen. In particular, since the superabsorbent polymer is in a highly viscous state before inactivation, it cannot be said that it is easy to separate the superabsorbent polymer attached to the liquid-permeable sheet, the liquid-impermeable sheet, and the pulp fibers. However, after inactivation, the superabsorbent polymer becomes low in viscosity due to dehydration, so the superabsorbent polymer attached to the liquid-permeable sheet, the liquid-impermeable sheet, and the pulp fibers can be easily separated from the liquid-permeable sheet, the liquid-impermeable sheet, and the pulp fibers. Therefore, the components of the sanitary product can be efficiently separated and recovered.
[0092] In this embodiment, the separation step S13 may further include a second separation step S33 of removing the adhesive at the joints between the film and other members with a solvent that dissolves the adhesive at the joints. In this embodiment, the adhesive at each joint between the film, the nonwoven fabric, and the absorbent body is removed with a solvent that dissolves the adhesive at each joint.
[0093] In the second separation step S33, the adhesive at the joint between the film (liquid-impermeable sheet) and other members (nonwoven fabric of the liquid-permeable sheet, the liquid-permeable sheet, absorbent remaining on the surface of the liquid-impermeable sheet, etc.) is removed by a solvent. This allows the film and other members to be separated from each other while maintaining their original shapes without breaking or the like. This allows efficient recovery of components such as films for sanitary products. In addition, since the film and other members can be separated without leaving any adhesive on the film, the film can be reused as a high-purity resin. This prevents the adhesive from having a detrimental effect when the film is reused. The same applies to the nonwoven fabric as to the film.
[0094] The solvent used in the second separation step S33 is not particularly limited as long as it can dissolve the adhesive, and examples thereof include terpenes including at least one of terpene hydrocarbons, terpene aldehydes, and terpene ketones. In this step, an aqueous solution containing terpene is used, and the concentration of terpene in the aqueous solution is, for example, 0.05% by mass or more and 2% by mass or less. It is preferably 0.075 to 1% by mass. If the concentration of terpene is too low, it may not be possible to dissolve the adhesive in the joint. If the concentration of terpene is too high, the cost may increase. Terpene not only dissolves adhesives such as hot melt adhesives, but also has an oil stain cleaning effect. Therefore, for example, if a component of a sanitary product such as a liquid-impermeable sheet is printed, terpene can also decompose and remove the printing ink.
[0095] Examples of terpene hydrocarbons include myrcene, limonene, pinene, camphor, sapinene, phellandrene, paracymene, ocimene, terpinene, carene, zingiberene, caryophyllene, bisabolene, and cedrene. Among them, limonene, pinene, terpinene, and carene are preferred. Examples of terpene aldehydes include citronellal, citral, cyclocitral, safranal, phellandral, perillaldehyde, geranial, and neral. Examples of terpene ketones include camphor and tschutz. Among terpenes, terpene hydrocarbons are preferred, and limonene is particularly preferred. There are three types of limonene: d-limonene, l-limonene, and dipentene (dl-limonene), and any of them can be preferably used. Terpenes can be used alone or in combination of two or more types.
[0096] The treatment temperature of the second separation step S33, i.e., the temperature of the aqueous solution containing a solvent, is not particularly limited as long as the adhesive dissolves and the used sanitary product is decomposed into its constituent members. The treatment temperature may be room temperature or higher, for example, 15 to 30°C. The treatment time of the second separation step S33, i.e., the time for immersing the liquid-permeable sheet, the liquid-impermeable sheet, and the absorbent in the aqueous solution containing a solvent, is not particularly limited as long as the adhesive dissolves and the used sanitary product is decomposed into its constituent members. The treatment time is, for example, 2 to 60 minutes, and preferably 5 to 30 minutes. The amount of the aqueous solution of the second separation step S33, i.e., the amount of the aqueous solution containing a solvent, is not particularly limited as long as the adhesive dissolves and the used sanitary product is decomposed into its constituent members. The amount of the aqueous solution is, for example, preferably 300 to 3000 parts by mass, more preferably 500 to 2500 parts by mass, relative to 100 parts by mass of the used sanitary product. By the second separation step S33, the amount of adhesive remaining on the film, nonwoven fabric, absorbent body, etc. can be reduced to 1% by mass or less relative to the film, nonwoven fabric, absorbent body, etc.
[0097] In this embodiment, as another preferred embodiment, the second separation step S33 may be performed in the inactivation step S31. That is, the adhesive attached to the liquid-permeable sheet, the liquid-impermeable sheet, and the pulp fibers may be dissolved while inactivating the superabsorbent polymer attached to the liquid-permeable sheet, the liquid-impermeable sheet, and the pulp fibers. In this case, an aqueous solution containing both an inactivating agent and a solvent is used as the aqueous solution in which the liquid-permeable sheet, the liquid-impermeable sheet, the pulp fibers, and the superabsorbent polymer are immersed. Thereby, in the inactivation step S31, the liquid-impermeable sheet (film), the liquid-permeable sheet (nonwoven fabric), and the absorbent (pulp fibers and superabsorbent polymer) can be substantially separated in the aqueous solution. Then, in the subsequent first separation step, the liquid-impermeable sheet (film) and the liquid-permeable sheet (nonwoven fabric) can be separated from the absorbent (pulp fibers and superabsorbent polymer), and the second separation step S33 can be omitted. In this case, the liquid-impermeable sheet (film) and the liquid-permeable sheet (nonwoven fabric) are substantially separated by removing the adhesive.
[0098] In this embodiment, the separation step S13 may further include a first drying step S34 in which the film is dried in an atmosphere or with hot air at a temperature higher than room temperature to remove the solvent after the step of removing the adhesive from the bonded portion. In this embodiment, the nonwoven fabric is also dried in this step.
[0099] Sterilization is extremely important in the reuse of used sanitary products. In the first drying step S34, the separated film (liquid-impermeable sheet) and nonwoven fabric (liquid-permeable sheet) are dried in a high-temperature atmosphere or hot air or the like. The drying temperature is, for example, 105 to 210°C, and preferably 110 to 190°C. The drying time varies depending on the drying temperature, but is, for example, 10 to 120 minutes, and preferably 15 to 100 minutes. This not only allows the solvent remaining on the surfaces of the film and nonwoven fabric to be removed by evaporation, but also allows the film and nonwoven fabric to be sterilized in a high-temperature atmosphere or hot air or the like. This makes it possible to achieve the effect of sterilization (disinfection) while removing the solvent.
[0100] On the other hand, in this embodiment, the separation step S13 may include a third separation step S35 in which pulp fibers are separated from the separated mixture. In the third separation step S35, the method for separating the pulp fibers from the separated mixture (including pulp fibers, superabsorbent polymer, and wastewater) is not particularly limited, but for example, the separated mixture is discharged while passing through a screen with an opening of 0.1 to 4 mm, preferably 0.15 to 2 mm. As a result, the superabsorbent polymer and wastewater are discharged into the drainage, and the pulp fibers (mainly the superabsorbent polymer remaining on the surface) remain on the screen, so that the pulp fibers can be separated from the mixture. Although the pulp fibers contain a lot of impurities, they can be reused in this state depending on the application. The separated pulp fibers have superabsorbent polymer attached to them, and the separated pulp fibers and the superabsorbent polymer attached to the pulp fibers are mixed with water in a predetermined ratio and proceed to the ozone treatment step S36 as a pulp fiber-containing material.
[0101] In this embodiment, the separation process S13 includes an ozone treatment process S36 in which the pulp fiber-containing material, which includes superabsorbent polymer, pulp fibers, their connected structures, and water, is treated with an aqueous solution containing ozone to reduce the molecular weight of the superabsorbent polymer attached to the pulp fibers, solubilize it, and remove it.
[0102] In used sanitary products, in absorbents and the like containing pulp fibers and superabsorbent polymers, (i) as the superabsorbent polymer absorbs liquids such as bodily fluids, it swells and entangles the pulp fibers, and (ii) the enlarged superabsorbent polymers entangle the pulp fibers, causing gel blocking, etc., and thus multiple superabsorbent polymers and multiple pulp fibers form connected structures. The pulp fiber-containing material includes not only free pulp fibers and free superabsorbent polymers, but also connected structures composed of multiple superabsorbent polymers and multiple pulp fibers.
[0103] In the ozone treatment step S36, the superabsorbent polymer contained in the pulp fiber-containing material (treatment liquid) is oxidatively decomposed by the ozone in the aqueous solution, and is solubilized in the aqueous solution and removed. The state where the superabsorbent polymer is oxidatively decomposed and solubilized in the aqueous solution means the state where the superabsorbent polymer and the linked structure pass through a 2 mm screen. This allows impurities such as the superabsorbent polymer to be removed from the pulp fiber-containing material (treatment liquid) to produce high-purity pulp fibers. In addition, the ozone treatment can be used to perform secondary sterilization, bleaching, and deodorization of the pulp fibers.
[0104] 2 is a schematic diagram showing an example of the configuration of the device 2 that performs the ozone treatment step S36. The device 2 includes a pulp fiber-containing material storage section 3 that stores a pulp fiber-containing material 51 that contains water, the pulp fibers separated in the third separation step S35, and a superabsorbent polymer, and an ozone treatment section 4 that oxidatively decomposes the superabsorbent polymer contained in the pulp fiber-containing material 51 and removes it from the pulp fibers.
[0105] The pulp fiber-containing material storage section 3 includes a pulp fiber-containing material tank 12 and an agitator 13. The pulp fiber-containing material tank 12 stores the pulp fiber-containing material 51 supplied via piping 61. The agitator 13 agitates the pulp fiber-containing material 51 in the pulp fiber-containing material tank 12 so that the pulp fibers and the superabsorbent polymer in the pulp fiber-containing material 51 do not separate from the water and sink to the bottom of the pulp fiber-containing material 51.
[0106] On the other hand, the ozone treatment section 4 includes a supply pump 21, a treatment tank 31, an ozone supply device 41, a delivery pump 22, and an ozone decomposition device 34. The treatment tank 31 contains an acidic aqueous solution as a treatment liquid 52. The treatment tank 31 includes a pulp fiber-containing material supply port 32, a treatment liquid discharge port 33, and an ozone-containing gas supply port 43. The pulp fiber-containing material supply port 32 is disposed in the upper part of the treatment tank 31, and supplies the pulp fiber-containing material 51 to the treatment tank 31. The treatment liquid discharge port 33 is disposed in the lower part of the mixing tank 31, and discharges the treatment liquid 52. The ozone-containing gas supply port 43 is disposed in the lower part of the mixing tank 31, specifically, above the treatment liquid discharge port 33, and delivers the ozone-containing gas 53 into the treatment tank 31.
[0107] Specifically, the supply pump 21 continuously supplies the pulp fiber-containing material 51 from the pulp fiber-containing material tank 12 through the piping 62 into the treatment tank 31 from the pulp fiber-containing material supply port 32 at a first flow rate. The ozone supply device 41 supplies the ozone-containing gas 53 to the treatment tank 31. Examples of the ozone generator 42 of the ozone supply device 41 include an ozone water exposure tester ED-OWX-2 manufactured by Ecodesign Co., Ltd. and an ozone generator OS-25V manufactured by Mitsubishi Electric Corporation. The ozone-containing gas 53 is another type of gas containing ozone, such as oxygen gas containing ozone. The ozone-containing gas supply port 43 delivers the ozone-containing gas 53 supplied to the treatment tank 31 through the piping 65 into the treatment tank 31, and is disposed at the lower part (preferably the bottom) of the treatment tank 31. The ozone-containing gas supply port 43 continuously supplies the ozone-containing gas 53 as a plurality of fine bubbles from the bottom to the top of the treatment liquid 52 (treatment tank 31). The delivery pump 22 continuously discharges the treatment liquid 52 in the treatment tank 31 from the treatment liquid discharge port 33 to the outside of the treatment tank 31 through the piping 63 at a second flow rate. The ozone decomposition device 34 receives the ozone-containing gas 53 accumulated in the upper part of the treatment tank 31 through the piping 64, renders the ozone harmless, and releases it to the outside. Note that the treatment liquid 52 in the treatment tank 31 is only the treatment liquid 52 before the start of the ozone treatment step S36, and becomes a mixture of the treatment liquid 52 and the pulp fiber-containing material 51 after the start. However, in this embodiment, the liquid in the treatment tank 31, including the mixture of the treatment liquid 52 and the pulp fiber-containing material 51, is referred to as the treatment liquid 52.
[0108] Next, a specific method for the ozone treatment step S36 will be described. The pulp fibers and superabsorbent polymer separated in the third separation step S35 are mixed with water to a preset concentration to become pulp fiber-containing material 51. The concentration of pulp fibers in pulp fiber-containing material 51 is set to a preset concentration when it is introduced into treatment tank 31 and mixed with treatment liquid 52. The pulp fiber-containing material 51 is supplied to pulp fiber-containing material tank 12 via piping 61 and stored therein. Since the specific gravity of the pulp fibers and superabsorbent polymer is greater than 1, the pulp fiber-containing material 51 is stirred by a stirrer 13 in pulp fiber-containing material tank 12 to prevent the pulp fibers and superabsorbent polymer from separating from the water.
[0109] The pulp fiber-containing material 51 in the pulp fiber-containing material tank 12 is continuously supplied at a first flow rate from the pulp fiber-containing material supply port 32 to the treatment tank 31 via the piping 62, with the flow rate controlled by the supply pump 21. The treatment liquid 52 is an acidic aqueous solution, and has a specific gravity of approximately 1. Therefore, the pulp fibers and the superabsorbent polymer settle from the top to the bottom of the treatment liquid 52.
[0110] On the other hand, the ozone-containing gas 53 generated by the ozone generator 42 is supplied to the treatment tank 31 via the pipe 65 and is released in the form of fine bubbles (e.g., microbubbles or nanobubbles) from the ozone-containing gas supply port 43 of the treatment tank 31 into the treatment liquid 52. That is, the ozone-containing gas 53 rises from the bottom to the top of the treatment liquid 52.
[0111] Then, in the treatment liquid 52, the pulp fibers and the superabsorbent polymer moving downward, i.e., descending, and the ozone-containing gas 53 moving upward, i.e., ascending, collide with each other while moving in opposite directions. Then, the ozone-containing gas 53 adheres to the pulp fibers and the superabsorbent polymer, as well as to the surface of the connected structure. The ozone in the ozone-containing gas 53 oxidizes and decomposes the free superabsorbent polymer, dissolving it in the treatment liquid 52. As a result, the superabsorbent polymer on the pulp fibers is removed from the pulp fibers. Then, the pulp fibers descend to the bottom of the treatment tank 31, and the ozone-containing gas 53 escapes to the space above the treatment tank 31.
[0112] Among the free superabsorbent polymer and the free pulp fiber, and the connected structure, the free superabsorbent polymer, which has a relatively low buoyancy, and the connected structure containing the superabsorbent polymer tend to sink more than the free pulp fiber, which has a relatively high buoyancy. On the other hand, since the ozone-containing gas rises while consuming ozone and treating the superabsorbent polymer and the pulp fiber, the ozone-containing gas present at the lower position tends to have a higher ozone content (i.e., is fresher) than the ozone-containing gas present at the upper position.
[0113] Therefore, the free superabsorbent polymer and the connected structure, which move downward relatively quickly, can be oxidized and decomposed by fresher ozone-containing gas to form free pulp fibers. On the other hand, since the free pulp fibers move downward relatively slowly, the ozone-containing gas can treat the free pulp fibers over time. Specifically, the ozone in the ozone-containing gas collides with the pulp fibers while facing them, thereby decomposing hemicellulose, lignin, etc. of the pulp fibers.
[0114] Thereafter, the treatment liquid 52 (containing pulp fibers after ozone treatment) at the bottom of the treatment tank 31 is continuously discharged from the treatment liquid outlet 33 of the treatment tank 31 to the outside of the treatment tank 31 at a second flow rate through the piping 63 by flow control of the delivery pump 22. The ozone in the ozone-containing gas 53 accumulated in the upper part of the treatment tank 31 is rendered harmless by the ozone decomposition device 34 and released to the outside.
[0115] In this manner, the pulp fiber-containing material 51 is continuously supplied into the treatment tank 31 from the upper part of the treatment tank 31 at a first flow rate, and the treatment liquid 52 is continuously discharged from the lower part (bottom) of the treatment tank 31 to the outside of the treatment tank 31 at a second flow rate. This makes it possible to forcibly generate a continuous and stable flow of fluid (including pulp fibers) from the top to the bottom within the treatment tank 31.
[0116] The treatment liquid 52 discharged from the treatment tank 31 contains ozone-treated pulp fibers from which the superabsorbent polymer, hemicellulose, lignin, etc. have been removed, and also contains low molecular weight organic matter produced by oxidative decomposition of the superabsorbent polymer. The ozone-treated pulp fibers are recovered in a process downstream of the delivery pump 22, for example, in the fourth separation process S37 described below.
[0117] In this method, a pulp fiber-containing material 51 containing at least pulp fibers and a superabsorbent polymer is continuously supplied at a first flow rate into a treatment tank 31 containing a treatment liquid 52 capable of dissolving the superabsorbent polymer, while a treatment liquid 52 containing ozone-treated pulp fibers from which the superabsorbent polymer has been removed and containing low-molecular-weight organic matter produced by oxidative decomposition of the superabsorbent polymer is continuously discharged at a second flow rate outside the treatment tank 31. With this configuration, a continuous and stable flow of fluid (containing pulp fibers) can be forcibly generated from a pulp fiber-containing material supply port 32 that supplies the pulp fiber-containing material 51 in the treatment tank 31 toward a treatment liquid discharge port 33 that discharges the treatment liquid 52. The flow of the fluid, i.e., a water flow, can treat (solubilize) the superabsorbent polymer and treat the pulp fibers, even if the treatment amounts of the pulp fibers and the superabsorbent polymer are increased.
[0118] Here, it is preferable that the first flow rate and the second flow rate are the same. By making the first flow rate and the second flow rate the same, the amount of the processing liquid 52 in the processing tank 31 can be kept constant, and stable continuous processing is possible. However, if the amount of the processing liquid 52 in the processing tank 31 can be kept substantially constant, that is, if the amount of the processing liquid 52 in the processing tank 31 does not increase or decrease significantly, the first flow rate and the second flow rate may vary over time. In other words, the first flow rate and the second flow rate do not need to be completely the same all the time, and only need to be substantially the same on average over time. Here, substantially the same means that the difference between the first flow rate and the second flow rate is within 5 mass %. In this case, stable continuous processing is also possible.
[0119] When the ozone-containing gas 53 is supplied to the treatment liquid 52, the ozone concentration in the treatment liquid 52 is not particularly limited as long as it is a concentration that can oxidatively decompose the superabsorbent polymer, but for example, 1 to 50 mass ppm can be mentioned, preferably 2 to 40 mass ppm, and more preferably 3 to 30 mass ppm. If the ozone concentration in the treatment liquid 52 is too low, the superabsorbent polymer cannot be completely solubilized, and there is a risk that the superabsorbent polymer will remain in the pulp fibers. On the other hand, if the ozone concentration in the treatment liquid 52 is too high, the oxidizing power will also increase, which may damage the pulp fibers and may cause safety problems. The ozone treatment temperature is not particularly limited as long as it is a temperature that can oxidatively decompose the superabsorbent polymer, but for example, it may be room temperature or may be higher than room temperature.
[0120] The concentration of ozone in the treatment liquid 52 (aqueous solution) is measured by the following method. (1) 85 mL of the treatment liquid 52 with ozone dissolved therein is placed in a 100 mL measuring cylinder containing about 0.15 g of potassium iodide and 5 mL of a 10% citric acid solution, and the mixture is allowed to react. (2) After the reaction, the treated liquid 52 is transferred to a 200 mL Erlenmeyer flask, and the starch solution is added to the Erlenmeyer flask to color it purple. Then, the liquid is titrated with 0.01 mol / L sodium thiosulfate while stirring until it becomes colorless, and the amount a (mL) added is recorded. (3) Calculate the concentration of ozone in the aqueous solution using the following formula: The concentration of ozone in the aqueous solution (ppm by mass) is calculated using the following formula: Concentration of ozone in aqueous solution (ppm by mass) = a(mL) × 0.24 × 0.85(mL) It is calculated as follows.
[0121] The ozone concentration in the ozone-containing gas 53 is preferably 40 to 200 g / m 3 and more preferably 80 to 200 g / m 3 and more preferably 100 to 200 g / m 3If the ozone concentration in the ozone-containing gas 53 is too low, the superabsorbent polymer cannot be completely solubilized, and the superabsorbent polymer may remain. If the concentration in the ozone-containing gas 53 is too high, it may lead to damage to the pulp fibers, reduced safety, and increased manufacturing costs. The ozone concentration in the ozone-containing gas 53 can be measured, for example, by an ultraviolet absorption ozone concentration meter (for example, Ozone Monitor OZM-5000G manufactured by Ecodesign Co., Ltd.).
[0122] The concentration of the pulp fiber-containing material (e.g., pulp fiber and superabsorbent polymer) in the treatment liquid 52 is not particularly limited as long as the superabsorbent polymer can be oxidatively decomposed by the ozone in the treatment liquid 52, and may be, for example, 0.1 to 20% by mass, preferably 0.2 to 10% by mass, and more preferably 0.3 to 5% by mass. If the concentration of the pulp fiber is too high, the superabsorbent polymer cannot be completely solubilized, and there is a risk that the superabsorbent polymer will remain in the pulp fiber. On the other hand, if the concentration of the pulp fiber is too low, the oxidizing power will also increase, which may damage the pulp fiber and may cause a safety problem. The concentration of the pulp fiber and superabsorbent polymer in the pulp fiber-containing material 51 is appropriately set based on the concentration of the pulp fiber and superabsorbent polymer in the treatment liquid 52 and the amount of the treatment liquid 52.
[0123] When ozone is supplied to the treatment liquid 52 containing pulp fibers and a superabsorbent polymer, the treatment liquid 52 is preferably acidic (specifically, pH is greater than 0.0 and less than 3.0, preferably pH 2.5 or more and less than 3.0), weakly acidic (specifically, pH 3.0 or more and less than 6.0), or neutral (specifically, pH 6.0 or more and pH 8.0 or less, preferably pH 6.0 or more and pH 7.0 or less). More preferably, the pH of the treatment liquid 52 is greater than 0.0 and 7.0 or less, and even more preferably 2.5 to 6.0. By treating in an acidic state, the deactivation of ozone is suppressed, the effect of oxidative decomposition of the superabsorbent polymer by ozone is improved, and the superabsorbent polymer can be oxidatively decomposed in a short time. In order to maintain the pH of the treatment liquid, the pH of the pulp fiber-containing material 51 may be made the same as that of the treatment liquid 52, and the pulp fiber-containing material 51 may be supplied to the treatment tank 31. Alternatively, the pH of the treatment liquid 52 may be monitored by a pH sensor, and when the pH fluctuates toward the neutral side, a predetermined acidic solution may be added to the treatment liquid 52 in an amount corresponding to the fluctuation range.
[0124] The amount of the treatment liquid 52 (including the pulp fiber-containing material 51) in the treatment tank 31 is not particularly limited as long as it is an amount that can oxidatively decompose the superabsorbent polymer, but it is preferable that the volume V (unit: L) of the treatment liquid 52 in the treatment tank 31 and the mass W (unit: kg) of the pulp fiber satisfy 30≦V / W≦1000. More preferably, it is 50≦V / W≦400, and even more preferably, it is 100≦V / W≦200. If V / W is too small, the superabsorbent polymer may not be completely solubilized and may remain. If V / W is too large, the manufacturing cost may increase. The volume V of the treatment tank 31 is not particularly limited, but may be, for example, 50 to 80 L.
[0125] Flow rate of ozone-containing gas R O (unit: L / min) and the volume V (unit: L) of the treatment liquid 52 in the treatment tank 31 are 0.01≦R O / V≦1.25. More preferably, 0.03≦R O / V≦1.0, and more preferably 0.06≦R O / V≦0.75.O If R / V is too small, the superabsorbent polymer cannot be completely solubilized, and the superabsorbent polymer may remain in the pulp fibers. O If the flow rate of the ozone-containing gas, R, is too large, it may cause damage to the pulp fibers, reduce safety, and increase production costs. O There is no particular limitation on the flow rate, but an example would be 3 to 6 L / min.
[0126] The time that the pulp fiber-containing material is present in the treatment tank 31, i.e., the time that the pulp fiber-containing material is treated in the treatment liquid 52 (hereinafter also referred to as "tank treatment time") varies depending on the purpose, such as decomposition of hemicellulose in the pulp fibers, decomposition of lignin, and oxidative decomposition of superabsorbent polymer, and is not particularly limited. The tank treatment time may be short if the ozone concentration of the treatment liquid 52 is high, and is long if the ozone concentration of the treatment liquid 52 is low. The tank treatment time is, for example, 15 to 180 minutes, and preferably 30 to 60 minutes.
[0127] The ozone-containing gas and the pulp fiber-containing material can be contacted based on a CT value, which is the product of the ozone concentration (ppm by mass) in the ozone-containing gas and the treatment time in the tank (min.) The CT value is preferably 100 ppm min or more, more preferably 1,000 ppm min or more, even more preferably 2,000 ppm min or more, even more preferably 4,000 ppm min or more, even more preferably 5,000 ppm min or more, and even more preferably 6,000 ppm min or more.
[0128] The CT value is preferably 12,000 ppm·min or less, more preferably 11,000 ppm·min or less, even more preferably 10,000 ppm·min or less, and even more preferably 9,000 ppm·min or less. If the CT value is too small, the decomposition of hemicellulose, lignin, and superabsorbent polymers, especially hemicellulose, may be insufficient, whereas if the CT value is too large, it may lead to damage to pulp fibers, reduced safety, and increased production costs.
[0129] The method for measuring the ozone concentration in the ozone-containing gas at the CT value is as described above. In addition, the treatment time in the tank in the CT value means the time (minutes) during which the ozone-containing gas is supplied in the case of a batch type, and means the value obtained by dividing the volume (L) of the treatment liquid in the treatment tank by the discharge amount per hour (L / min) in the case of a continuous type.
[0130] In the present disclosure, in the ozone treatment step, the pulp fiber after ozone treatment preferably has a hemicellulose content of 10.0% by mass or less, more preferably 9.0% by mass or less, even more preferably 8.0% by mass or less, even more preferably 6.0% by mass or less, even more preferably 5.0% by mass or less, and even more preferably 4.0% by mass or less. This makes it easier to form a pulp fiber raw material in the subsequent alkali treatment step. The lower limit of the hemicellulose content is 0.0% by mass.
[0131] While the pulp fibers are present in the treatment tank 31, the superabsorbent polymer is oxidatively decomposed by the ozone into low molecular weight components, which dissolve in the treatment liquid 52. The hemicellulose in the pulp fibers is also decomposed by the ozone, and a part of it dissolves in the treatment liquid 52. The lignin in the pulp fibers is also decomposed by the ozone, and dissolves in the treatment liquid 52. The low molecular weight components of the superabsorbent polymer, decomposition products of hemicellulose, decomposition products of lignin, etc., dissolved in the treatment liquid 52 are discharged together with the treatment liquid 52. Furthermore, in this process, the used sanitary goods are primarily disinfected by the sterilizing action of ozone. As described above, pulp fibers are formed after ozone treatment.
[0132] The manufacturing method of the present disclosure includes the following steps. an ozone treatment step in which an ozone-treated pulp fiber is formed from the pulp fiber to be treated by supplying an ozone-containing gas to a treatment tank containing a treatment liquid containing a pulp fiber-containing material containing the pulp fiber to be treated; an alkali treatment step of treating the ozone-treated pulp fiber with an aqueous alkali solution to form a pulp fiber raw material having a hemicellulose content of less than 8.0% by mass;
[0133] The above-mentioned ozone treatment step is not particularly limited as long as it is a step in which a predetermined post-ozone-treated pulp fiber is formed from the pulp fibers by supplying an ozone-containing gas to a treatment tank containing a treatment liquid containing a pulp fiber-containing material including the pulp fibers to be treated, and can be carried out, for example, in a so-called batch-type or continuous type.
[0134] When the pulp fibers to be treated are virgin pulp fibers, the pulp fiber-containing material may be virgin pulp fibers alone. When the pulp fibers to be treated are used pulp fibers, for example, pulp fibers derived from used sanitary products, the pulp fiber-containing material contains at least pulp fibers and may be pulp fibers alone. The pulp fiber-containing material may contain a superabsorbent polymer in addition to pulp fibers, and may also contain a connected structure in which multiple superabsorbent polymers and multiple pulp fibers are connected, materials constituting sanitary products (for example, core wrap, liquid-permeable sheet, liquid-impermeable sheet, etc.), etc. The ozone-containing gas may be supplied into the processing liquid in the processing tank, or may be supplied to the space above the processing liquid in the processing tank. The alkaline treatment step is described below.
[0135] The manufacturing method of the present disclosure may include the following steps: a preparation step, a pulp fiber-containing material supply step, an ozone-containing gas supply step, an ozone treatment step, and a treatment liquid discharge step. a preparation step of preparing the treatment tank having a pulp fiber-containing material supply port, a treatment liquid discharge port, and an ozone-containing gas supply port disposed below the treatment tank; a pulp fiber-containing material supplying step of supplying the pulp fiber-containing material to the treatment tank through the pulp fiber-containing material supply port; an ozone-containing gas supplying step of supplying the ozone-containing gas from the ozone-containing gas supply port to the treatment liquid in the treatment tank; the ozone treatment step in which the pulp fiber-containing material is contacted with the ozone-containing gas while the ozone-containing gas is being raised in the treatment tank, thereby forming the ozone-treated pulp fibers from the pulp fibers to be treated; a treated liquid discharge step of discharging the treated liquid containing the pulp fibers after the ozone treatment from the treated liquid discharge port;
[0136] The treatment liquid outlet may be located below the pulp fiber-containing material supply inlet, and in the ozone treatment step, the pulp fiber-containing material may be brought into contact with the ozone-containing gas while being lowered, and the treatment liquid outlet may be located above the pulp fiber-containing material supply inlet, and in the ozone treatment step, the pulp fiber-containing material may be brought into contact with the ozone-containing gas while being raised.
[0137] In the present embodiment, as one aspect, the ozone treatment step S36 (continuous treatment step) includes a step of continuously supplying a pulp fiber-containing material 51 from the upper part of the treatment tank 31 while continuously discharging a treatment liquid 52 from the lower part of the treatment tank 31. The pulp fibers and the superabsorbent polymer in the pulp fiber-containing material 51 have small buoyancy, and the pulp fibers, the superabsorbent polymer, and the connected structure naturally sink.
[0138] In the present embodiment, as one aspect, the treatment liquid 52 capable of dissolving the superabsorbent polymer is an aqueous solution containing an ozone-containing gas that oxidatively decomposes the superabsorbent polymer to dissolve it. The ozone treatment step S36 (continuous treatment step) further includes a sending step of continuously sending out a plurality of bubbles of the ozone-containing gas from the lower part to the upper part of the treatment liquid 52. In such one aspect of the present method, the ozone-containing gas rises in the treatment liquid 52, and the pulp fibers and the superabsorbent polymer fall, that is, they flow in a countercurrent. This can increase the probability of contact between the pulp fibers and the superabsorbent polymer and the ozone-containing gas. In addition, the deeper the pulp fibers and the superabsorbent polymer sink, the higher the concentration of the ozone-containing gas that can be contacted. Therefore, the superabsorbent polymer, hemicellulose, lignin, etc. that cannot be completely dissolved in the treatment liquid 52 by the ozone-containing gas that contacts the treatment liquid 52 at a shallow part can be contacted with the high concentration of the ozone-containing gas at a deep part of the treatment liquid 52. This allows the highly absorbent polymer, hemicellulose, lignin, etc. to be decomposed, dissolved in the treatment liquid 52, and removed from the pulp fibers.
[0139] In the present embodiment, as one aspect, the above-mentioned sending step includes a step of sending the ozone-containing gas in the form of microbubbles or nanobubbles. However, the microbubbles are bubbles having a diameter of about 1 to 1000 μm, preferably about 10 to 500 μm, and the nanobubbles are bubbles having a diameter of about 100 to 1000 nm, preferably about 100 to 500 nm. The microbubbles or nanobubbles are such fine bubbles, and have the properties of a large surface area per unit volume and a slow rising speed in the liquid. Therefore, in one aspect of the present method, such fine bubbly ozone-containing gas is sent from the lower part to the upper part of the treatment liquid 52 in the treatment tank 31.
[0140] Since the fine bubbles occupy a small area on the surface of the pulp fibers, more bubbles can contact the surface of the pulp fibers. As a result, the pulp fibers, the superabsorbent polymer, and the connected structures can be evenly wrapped with the fine bubbles, and the contact area between them and the ozone-containing gas can be increased. In addition, when the pulp fiber-containing material is lowered in the ozone treatment step, more bubbles contact the surface of the pulp fibers, and the buoyancy of the bubbles reduces the sedimentation of the pulp fibers, the superabsorbent polymer, and the connected structures, and the contact time between them and the ozone-containing gas can be increased. As a result, the superabsorbent polymer, hemicellulose, lignin, etc. can be decomposed, dissolved in the treatment liquid 52, and removed from the pulp fibers.
[0141] In the present embodiment, as one aspect, the treatment liquid 52 is an acidic aqueous solution, for example, an acidic aqueous solution having a pH of 2.5 or less. In this case, even if the superabsorbent polymer in the pulp fiber-containing material 51 partially retains water absorption capacity, the water absorption and expansion of the superabsorbent polymer can be suppressed. As a result, the superabsorbent polymer can be dissolved in the treatment liquid 52 in a short time, and the superabsorbent polymer can be removed more reliably. In particular, when the treatment liquid 52 is an ozone-containing aqueous solution, the ozone in the ozone-containing aqueous solution is less likely to be deactivated, so that the superabsorbent polymer can be oxidatively decomposed in a short time, and thus hemicellulose, lignin, and the like can be decomposed.
[0142] As another preferred embodiment, the configuration of the treatment tank 31 may be other than that shown in FIG. 2. FIG. 3 is a schematic diagram showing another example of the configuration of the ozone treatment device 2 in FIG. 1. The device 2 in FIG. 3 is different from the device 2 in FIG. 2 in that the piping 63 of the ozone treatment unit 4 has a continuous U-shaped tube structure in which two U-shaped tubes are connected inversely and continuously to each other, and the delivery pump 22 is omitted. In this case, when the piping 63 is filled with the treatment liquid 52 and the liquid level of the treatment liquid 52 in the treatment tank 31 is higher than the liquid level of the liquid in the tank of the next process connected by the piping 63, the treatment liquid 52 is discharged to the tank of the next process through the piping 63 due to the principle of a siphon. Therefore, if the liquid level of the processing liquid 52 in the processing tank 31 and the liquid level of the liquid in the tank for the next process are initially set to the same level before the start of processing, when the pulp fiber-containing material 51 is continuously supplied into the processing tank 31 at the first flow rate upon the start of processing, the processing liquid 52 will be discharged into the tank for the next process via the piping 63 at the second flow rate = the first flow rate due to the siphon principle. However, the liquid level of the liquid in the tank for the next process is maintained at the level before the start of processing even during processing. In this case, the delivery pump 22 is not required, and control of the second flow rate of the delivery pump 22 is not required.
[0143] In this embodiment, the separation process S13 may further include a fourth separation process S37 for separating the ozone-treated pulp fibers from the treatment liquid 52 discharged from the treatment tank 31, and a second drying process S38 for drying the separated ozone-treated pulp fibers.
[0144] In the fourth separation step S37, the method for separating the ozone-treated pulp fibers from the treatment liquid 52 discharged from the treatment tank 31 is not particularly limited, but may be, for example, a method of passing the treatment liquid 52 containing the ozone-treated pulp fibers through a screen mesh having an opening of 0.15 to 2 mm. When the treatment liquid 52 containing the ozone-treated pulp fibers is passed through a screen mesh having an opening of 0.15 to 2 mm, wastewater containing oxidized decomposition products of the superabsorbent polymer, decomposition products of hemicellulose, decomposition products of lignin, etc. passes through the screen. On the other hand, the ozone-treated pulp fibers remain on the screen.
[0145] In the subsequent second drying step S38, the separated ozone-treated pulp fibers are dried in a high-temperature atmosphere or hot air, etc. The drying temperature is, for example, 105 to 210°C, and preferably 110 to 190°C. The drying time varies depending on the drying temperature, but is, for example, 10 to 120 minutes, and preferably 15 to 100 minutes. This allows the moisture remaining on the surface of the ozone-treated pulp fibers to evaporate and be removed, making it possible to recover high-purity ozone-treated pulp fibers with an extremely low superabsorbent polymer mixing ratio. In addition, the ozone-treated pulp fibers can be sterilized (disinfected) in a high-temperature atmosphere or hot air, etc. In addition, when the pulp fibers are not stored after the ozone treatment and the next alkali treatment step S39 is performed, the second drying step S38 can be omitted.
[0146] In the alkali treatment step S39, the ozone-treated pulp fibers are treated with an alkaline aqueous solution to form a pulp fiber raw material having a hemicellulose content of less than 8.0% by mass. By subjecting the ozone-treated pulp fibers that have been subjected to the ozone treatment step to the alkali treatment step, hemicellulose can be decomposed under milder conditions than in conventionally known alkali treatment steps. It is also expected that the decomposition of cellulose can be suppressed by performing the alkali treatment step under milder conditions.
[0147] The conditions of the alkali treatment step are not particularly limited, so long as they are capable of forming a pulp fiber raw material having a hemicellulose content of less than 8.0% by weight. The alkali treatment step can be carried out by immersing the ozone-treated pulp fibers in an aqueous alkali solution having a normality of preferably 0.1 N or more, more preferably 0.2 N or more, and even more preferably 0.3 N or more. The alkali treatment step can be carried out by immersing the ozone-treated pulp fibers in an aqueous alkali solution having a normality of preferably 8.0 N or less, more preferably 6.0 N or less, even more preferably 5.0 N or less, even more preferably 4.0 N or less, and even more preferably 3.0 N or less.
[0148] By keeping the normality of the alkaline aqueous solution within the above range, damage to the pulp fibers and processing equipment after ozone treatment is reduced, waste liquid from the alkaline treatment step can be easily disposed of, and the risk of performing the alkaline treatment step can be reduced. The normality of the alkaline aqueous solution includes a range lower than that used in conventional methods for forming cellulose nanofibers that do not use ozone treatment.
[0149] The amount of the alkaline aqueous solution is not particularly limited as long as it can form a pulp fiber raw material having a hemicellulose content of less than 8.0% by mass, and preferably 10 to 200 L, and more preferably 20 to 100 L, of the alkaline aqueous solution can be added per 1 kg (dry mass) of pulp fiber after ozone treatment.
[0150] The temperature of the alkali treatment step is not particularly limited, and the alkali treatment step can be carried out, for example, at room temperature (25° C.). The alkali treatment step can be carried out at a temperature of preferably 10° C. or higher, more preferably 15° C. or higher, and even more preferably 20° C. or higher. The alkali treatment step can be carried out at a temperature of preferably 80° C. or lower, more preferably 60° C. or lower, and even more preferably 50° C. or lower, and even more preferably 40° C. or lower.
[0151] The time for the alkali treatment step is not particularly limited, and the alkali treatment step can be carried out for preferably 5 to 240 minutes, more preferably 10 to 120 minutes, and further preferably 15 to 60 minutes.
[0152] For example, when a high temperature condition, e.g., 40°C or higher, is selected in the alkaline treatment step, a normality condition of, e.g., 0.3N to 4.5N can be selected as the concentration of the alkaline aqueous solution, thereby decomposing hemicellulose in the pulp fibers after ozone. In the alkaline treatment step, the ozone-treated pulp fibers may be immersed in an aqueous alkaline solution, and the ozone-treated pulp fibers may be stirred with the aqueous alkaline solution.
[0153] The alkaline aqueous solution can be prepared by dissolving an alkali that exhibits alkalinity when dissolved in water, such as hydroxides and salts of alkali metals and alkaline earth metals, in water. Examples of the alkali metal include lithium, sodium, potassium, etc., and sodium is preferred. Examples of the alkaline earth metal include magnesium, calcium, barium, etc. When the alkaline aqueous solution is an aqueous solution of sodium hydroxide, the concentration of the alkaline aqueous solution is, for example, 2 to 10% by mass.
[0154] In addition, in the alkaline treatment step S39, the second drying step S38 may be omitted and the undried (wet) recycled pulp fibers obtained in the fourth separation step S37 may be subjected to the alkaline treatment step S39, and the fourth separation step S37 and the second drying step S38 may be omitted and the treatment liquid 52 containing the recycled pulp fibers obtained in the ozone treatment step S36 may be subjected to the alkaline treatment step S39.
[0155] After the alkali treatment step, a washing step can be performed to wash the alkali and hemicellulose decomposition product. After the washing step, a drying step can be performed. The drying step can be the same as the second drying step S38.
[0156] In the present disclosure, the pulp fiber raw material preferably has a cellulose content of 94.0% by mass or more, more preferably 95.0% by mass or more, even more preferably 96.0% by mass or more, and even more preferably 97.0% by mass or more. This allows the pulp fiber raw material to be suitably used as a cellulose raw material for cellulose-derived products. The upper limit of the cellulose content is 100.0% by mass.
[0157] In the present disclosure, the pulp fiber raw material preferably has a hemicellulose content of less than 8.0% by mass, more preferably less than 6.0% by mass, even more preferably less than 5.0% by mass, even more preferably less than 4.0% by mass, and even more preferably less than 3.0% by mass. This allows the pulp fiber raw material to be suitably used as a cellulose raw material for cellulose-derived products. The lower limit of the hemicellulose content is 0.0% by mass.
[0158] In the present disclosure, the pulp fiber raw material, and preferably the ozone-treated pulp fiber and the pulp fiber raw material, preferably have a lignin content of 0.10% by mass or less, more preferably 0.08% by mass or less, and even more preferably 0.06% by mass or less. This allows the pulp fiber raw material to be suitably used as a cellulose raw material for cellulose-derived products. The lower limit of the lignin content is 0.00% by mass.
[0159] In the present disclosure, the ozone-treated pulp fibers prior to forming the pulp fiber raw material preferably have a cellulose content of 87.0% by mass or more, more preferably 90.0% by mass or more, and even more preferably 93.0% by mass or more, so that the pulp fiber raw material can be suitably used as a cellulose raw material for cellulose-derived products.
[0160] In the present disclosure, the cellulose content, hemicellulose content, and lignin content in pulp fiber raw materials, pulp fibers after ozone treatment, etc. can be measured according to known detergent analysis methods.
[0161] In the present disclosure, the pulp fiber raw material, and preferably the pulp fibers and pulp fiber raw material after ozone treatment, preferably have a beating rate reduction rate of 300 mL or more, more preferably 320 mL or more, even more preferably 340 mL or more, and even more preferably 360 mL or more, which makes the pulp fiber raw material more likely to fluff and makes it easier to extract cellulose in a subsequent process using the pulp fiber raw material, such as a cellulose use step for forming cellulose nanofibers, viscose rayon, cellulose derivatives, bioethanol, biobutanol, molding materials, or paper products.
[0162] In the manufacturing method of the present disclosure, the pulp fiber raw material, and preferably the pulp fibers and pulp fiber raw material after ozone treatment, preferably have a beating rate reduction rate of 990 mL or less, more preferably 800 mL or less, even more preferably 700 mL or less, and even more preferably 600 mL or less, which can suppress damage to the pulp fiber raw material and the cellulose to be extracted. The above-mentioned rate of decrease in the beating degree is obtained by a low hemicellulose content, a low lignin content, etc. in the pulp fiber raw material or the pulp fiber after ozone treatment.
[0163] The above-mentioned freeness reduction rate is measured according to the following freeness reduction test. <Beating Degree Reduction Test> (1) The pulp fiber raw material or the pulp fiber after ozone treatment is beaten for at least 1 hour, preferably for 2 hours, in accordance with JIS P 8221-1:1998 Pulp-Beating Method-Part 1: Beater Method. (2) After beating starts, samples are taken every 20 minutes and the beating degree (Canadian Standard freeness) of each sample is measured according to JIS P 8121-2:2012 Pulp - Freeness test method - Part 2: Canadian Standard Freeness Method. Note that the test may be stopped when the beating degree of the sample falls below 100 mL. (3) Plot time (h) on the horizontal axis and the degree of beating (mL) on the vertical axis, and approximate a linear function using the least squares method. The absolute value of the slope is used as the rate of decrease in the degree of beating (mL / m). The higher the beating degree reduction rate, the faster the reduction in the beating degree per unit time, that is, the easier it is for the pulp fiber raw material or the pulp fibers after ozone treatment to be beaten (to become fluffed).
[0164] In the present disclosure, the pulp fiber raw material preferably has a water contact angle of 20° or less, more preferably 15° or less, and even more preferably 10° or less. This allows the cellulose to be easily dispersed in an aqueous solution when the pulp fiber raw material is dried and stored and then extracted. From the above viewpoint, the water contact angle of the pulp fiber raw material may be 0°.
[0165] The water contact angle of a pulp fiber material can be measured as follows. (1) In a constant temperature and humidity chamber (temperature: 20±5°C, humidity: 65±5% RH), prepare an aluminum ring (outer diameter: 43 mm, inner diameter: 40 mm, height: 5 mm) and pulp fiber for saccharification that has been dried at 120°C for 60 minutes, and leave it for 24 hours. (2) 1.5 g of the pulp fiber raw material is evenly packed into an aluminum ring, and the pulp fiber raw material together with the aluminum ring is compressed for 1 minute at a pressure of 3 MPa using a press with a smooth bottom surface to smooth the surface of the pulp fiber raw material. (3) The water contact angle of the compressed pulp fiber raw material is measured in accordance with 6. Sessile drop method of JIS R 3257:1999 "Test method for wettability of glass substrate surface". An example of a contact angle measuring device is an automatic contact angle meter CA-V type manufactured by Kyowa Interface Science Co., Ltd. The water contact angle is the value 200 ms after deionized water is dropped. (4) The water contact angle is measured for 20 different samples, and the average value is used.
[0166] In the present disclosure, the pulp fiber raw material preferably has an ash content of 0.65 mass% or less, more preferably 0.50 mass% or less, even more preferably 0.30 mass% or less, and even more preferably 0.20 mass% or less, which makes it difficult for metal ions and their precipitates to damage equipment and inhibit the pulp fiber raw material from being pulverized when cellulose is extracted from the pulp fiber raw material. The ash content can be reduced, for example, by selecting an acid capable of forming a complex with metal ions contained in the excrement, particularly citric acid, as the inactivating agent in the inactivation step S31 in which the superabsorbent polymer is inactivated.
[0167] In this specification, ash content means the amount of inorganic or non-combustible residue remaining after organic matter is incinerated, and ash percentage means the ratio (mass ratio) of ash contained in the material to be incinerated. The ash percentage is measured according to "5. Ash content test method" in "2. General test method" of the Sanitary Treatment Product Material Standards. Specifically, the ash percentage is measured as follows. (1) First, heat a platinum, quartz, or porcelain crucible to 500-550°C for one hour, allow it to cool, and then accurately weigh its mass. (2) Take 2 to 4 g of pulp fiber raw material that has been dried at 120°C for 60 minutes, place it in a crucible, accurately measure the mass, and if necessary, remove or move the lid of the crucible. Heat gently at first, then gradually increase the temperature and ignite at 500 to 550°C for at least 4 hours, until no carbonized material remains, and then ash the material. (3) Allow it to cool, then weigh it accurately. The residue is again incinerated until it reaches a constant weight, allowed to cool, then weigh it accurately and use this as the ash content (% by mass).
[0168] In the present embodiment, as a preferred embodiment, the method further includes an inactivation step S31 in which the mixture is treated with an aqueous solution capable of inactivating the water absorption performance of the superabsorbent polymer to inactivate the water absorption performance of the superabsorbent polymer in the mixture before the ozone treatment step S36 (continuous treatment step), and a first separation step S32 in which the inactivated superabsorbent polymer and the pulp fibers are separated from the aqueous solution before the ozone treatment step S36 (continuous treatment step). Thus, in a preferred embodiment, the method includes a step in which the water absorption performance of the superabsorbent polymer is suppressed with an aqueous solution capable of inactivating the water absorption performance of the superabsorbent polymer in the inactivation step S31, so that the superabsorbent polymer can be more easily dissolved in the treatment liquid 52 in a short time at the subsequent ozone treatment step S36 (continuous treatment step).
[0169] In the present embodiment, as a preferred embodiment, in the inactivation step S31, the aqueous solution capable of inactivating the water absorption performance of the superabsorbent polymer is an acidic aqueous solution, for example, an acidic aqueous solution having a pH of 2.5 or less. Thus, in the present method, as a preferred embodiment, the aqueous solution capable of inactivating the water absorption performance of the superabsorbent polymer is an acidic aqueous solution, so that the superabsorbent polymer is more easily inactivated, and thus the water absorption performance of the superabsorbent polymer can be more reliably suppressed at the stage of the inactivation step S31. As a result, the superabsorbent polymer can be more easily dissolved in the treatment liquid in a short time at the stage of the subsequent ozone treatment step S36 (continuous treatment step).
[0170] As another preferred embodiment, the treatment tank 31 may include at least a first treatment tank 31-1 and a second treatment tank 31-2 connected in series to each other. FIG. 4 is a schematic diagram showing another example of the configuration of the apparatus 2 for the ozone treatment step in FIG. 1. The apparatus 2 in FIG. 4 is different from the apparatus 2 in FIG. 2 in that two ozone processors 4 are connected in series, in other words, the first treatment tank 31-1 and the second treatment tank 31-2 are connected in series. In this case, for example, the first treatment tank 31-1 is supplied with the pulp fiber-containing material 51 and discharges a first treated liquid (treated liquid 52-1 of the first treatment tank 31-1), and the second treatment tank 31-2 is supplied with the first treated liquid and discharges a second treated liquid (treated liquid 52-2 of the second treatment tank 31-2), and thus the pulp fiber-containing material 51 is treated in multiple stages. In this case, compared to when one large-capacity treatment tank 31 is provided, treatment is performed with new treatment liquids 52-1, 52-2 for each of the first and second treatment tanks 31-1, 31-2. Therefore, for example, the superabsorbent polymer that was not completely dissolved in the first treatment tank (initial treatment tank) 31-1 can be easily dissolved in the second treatment tank (next treatment tank) 31-2, and the superabsorbent polymer can be more reliably dissolved and removed from the fibers.
[0171] In another preferred embodiment, the treatment tank 31 may include an ejector. For example, the ejector includes a drive fluid supply port, a mixed fluid discharge port connected to the treatment tank, and a suction fluid supply port therebetween, and while supplying the pulp fiber-containing material 51 to the drive fluid supply port of the ejector, ozone is supplied to the suction fluid supply port, and a mixed liquid formed by mixing the pulp fiber-containing material 51 and the ozone in the ejector is discharged from the mixed fluid discharge port into the treatment liquid in the treatment tank.
[0172] By supplying the pulp fiber-containing material 51 as the driving fluid and the ozone as the suction fluid to the ejector and mixing them in the ejector, a mixed liquid as a mixed fluid in which the pulp fiber-containing material 51 and the ozone are very well mixed can be efficiently formed. That is, a mixed liquid in which the pulp fiber-containing material 51 and the ozone are very closely in contact can be formed. Then, by discharging the mixed liquid into the treatment liquid in the treatment tank, the treatment liquid can be agitated. Furthermore, when the ozone is discharged into the treatment liquid, it is continuously discharged in the form of fine bubbles, so that it can be diffused very widely in the treatment liquid. As a result, the reaction between the superabsorbent polymer and the gaseous substance can be very efficiently promoted not only in the pulp fiber-containing material 51 in the mixed liquid discharged from the ejector but also in the pulp fibers containing the superabsorbent polymer in the treatment liquid in the treatment tank.
[0173] In the present embodiment, as a preferred embodiment, in the material separation step S1, in the pretreatment step S11, the used sanitary product can be made to have a very swollen state with water without breaking or otherwise breaking the shape of the sanitary product and without inactivating the superabsorbent polymer. This generates a very high internal pressure inside the used sanitary product, and makes it possible to make any part of the surface of the product burst. Then, in the decomposition step S12, a physical impact is applied to the used sanitary product in such a state, causing any part of the surface to break and causing the internal absorbent core to be ejected to the outside. This allows the used sanitary product to be decomposed into at least a film (liquid-impermeable sheet) and an absorbent core. At this time, the film generally maintains its original shape, so that it can be easily separated from the absorbent core in the subsequent separation step S13. This allows the constituent members such as the film to be separated from the other constituent members while maintaining their original shape without breaking or otherwise breaking. Therefore, the constituent members such as the film of the sanitary product can be efficiently collected.
[0174] In the present embodiment, as a preferred embodiment, terpene is used to remove the adhesive, so that the hot melt adhesive that bonds the components of the sanitary product can be dissolved at room temperature. This allows the sanitary product to be easily and neatly disassembled, and the pulp fiber and the highly absorbent polymer can be separated from the sanitary product, and the nonwoven fabric and the film can be separated while retaining their respective component forms. In other words, the pulp fiber, the film, and the nonwoven fabric can be easily collected separately without crushing the sanitary product or going through a complicated separation process. When limonene is used as the terpene, a secondary effect of limonene is that it has a refreshing citrus odor, which can mask the odor originating from excrement to some extent, reducing the odor burden on workers and the odor impact on neighbors. Limonene is a monoterpene with a structure similar to styrene, so it can dissolve styrene-based hot melt adhesives that are commonly used in sanitary products. Since the sanitary product can be washed at room temperature, energy costs can be reduced and the generation and diffusion of odors can be suppressed. Terpene is highly effective at cleaning oil stains, and in addition to dissolving hot melt adhesives, it can also decompose and remove the printing ink on printed films, allowing the printed films to be recovered as high-purity plastic materials.
[0175] In addition, when an organic acid solution with a pH of 2.5 or less is used to inactivate the superabsorbent polymer, the pulp fiber is less likely to deteriorate. In addition, when citric acid is used as the organic acid, the chelating effect and cleaning power of citric acid can be expected to remove dirt components derived from excrement. In addition, a disinfecting effect and a deodorizing effect against alkaline odors can be expected.
[0176] Furthermore, by oxidatively decomposing superabsorbent polymers with ozone, it is possible to prevent contamination of pulp fibers and a sudden increase in wastewater due to the absorption of water by superabsorbent polymers. By adjusting the concentration of ozone, it is possible to simultaneously perform oxidative decomposition and sterilization of superabsorbent polymers. In addition, when using ozone, no chlorine-based chemicals are used, so it is possible to produce high-quality RPF from recovered plastic components that is less likely to damage combustion furnaces. Since no salts are used during the treatment process, no residue is left on the pulp fibers, and high-quality pulp fiber raw material with low ash content can be recovered.
[0177] The cellulose using step can be performed by subjecting the pulp fiber raw material to a cellulose using process to produce a cellulose-derived product, as shown in FIG. 1 .
[0178] The pulp fiber raw material produced by the production method of the present disclosure has a predetermined hemicellulose content and is therefore suitable as a cellulose raw material. The cellulose raw material is not particularly limited as long as it contains cellulose as a part of the raw material, and examples of the raw material include raw materials for various applications, such as cellulose nanofibers, viscose rayon, cellulose derivatives, bioethanol, biobutanol, molding materials, paper products, etc. The various applications will be described later.
[0179] The manufacturing method of the present disclosure can include a cellulose using step of utilizing cellulose from a pulp fiber raw material after the alkali treatment step. The cellulose using step is not particularly limited as long as it uses cellulose, and examples thereof include a cellulose nanofiber forming step of forming a cellulose nanofiber, a viscose rayon forming step of forming a viscose rayon, a cellulose derivative forming step of forming a cellulose derivative, a bioethanol forming step of forming bioethanol, a biobutanol forming step of forming biobutanol, a molding material forming step of forming a molding material, and a paper product forming step of forming a paper product.
[0180] The cellulose nanofiber forming step is not particularly limited and includes cellulose nanofiber forming methods known in the art, such as those described in JP 2010-235681 A and JP 2010-254726 A.
[0181] Regarding the cellulose use step, the viscose rayon forming step is not particularly limited and includes viscose rayon forming methods known in the art (e.g., regenerated cellulose fiber forming method, cellophane forming method, cellulose sponge forming method). Examples of the viscose rayon forming method include the viscose method and the cuprammonium method. Examples of the viscose rayon include regenerated cellulose fiber, cellophane, and cellulose sponge.
[0182] Examples of the regenerated cellulose fibers include rayon fibers, such as viscose rayon fibers obtained from viscose, polynosic fibers and modal fibers, cuprammonium rayon fibers (also called "cupra fibers") obtained from a cuprammonium salt solution of cellulose, and lyocell fibers and tencel fibers obtained by an organic solvent spinning method using an organic solvent that is a mixed solution of an organic compound and water, without going through a cellulose derivative. Examples of the cellophane include cellophane tape and cellophane film.
[0183] Regarding the cellulose use step, the cellulose derivative forming step is not particularly limited and includes a cellulose derivative forming method known in the art (e.g., a method for forming semi-synthetic cellulose fiber).The cellulose derivative forming method includes, for example, the method described in JP-A-10-251301. The cellulose derivatives include, for example, semi-synthetic cellulose fibers, such as acetate fibers, for example, triacetate fibers and diacetate fibers. Examples of the cellulose derivatives include carboxymethyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose.
[0184] Regarding the cellulose use step, the bioethanol formation step is not particularly limited and includes bioethanol formation methods known in the art. Examples of the bioethanol formation method include the method described in JP 2018-64514 A.
[0185] With respect to the cellulose use step, the biobutanol formation step is not particularly limited and includes biobutanol formation methods known in the art, such as those described in JP 2015-517303 A.
[0186] With respect to the cellulose-using step, the molding material forming step is not particularly limited and includes molding material forming methods known in the art. Examples of the molding material include packaging cushioning materials, containers, and the like.
[0187] With respect to the cellulose use step, the paper product forming step is not particularly limited and includes methods of forming paper products known in the art. Examples of the paper products include filter base paper and functional paper. EXAMPLES
[0188] [Production Example 1] Recycled pulp fibers were produced from various types of used disposable diapers collected from nursing homes according to the methods shown in Figures 1 and 2. The conditions related to the ozone treatment step S36 were as follows. (i) Pulp fiber content 51 Concentration: 1% by mass (concentration of pulp fiber and superabsorbent polymer) pH: 2.4 (ii) Treatment tank 31 ·Capacity: 60L Height: 2.6m Primary flow rate: 2L / min Secondary flow rate: 2L / min - Processing time in tank: 30 minutes V / W:100 ·R O / V:0.033 (iii) Ozone-containing gas Ozone concentration: 200g / m 3 Shape: Nanobubbles
[0189] The inactivation step S31 was carried out using citric acid at pH 2.0, and the ozone treatment step S36 was carried out under the above-mentioned conditions. The obtained recycled pulp fiber was dried at 120° C. for 60 minutes to obtain pulp fiber No. 1 after ozone treatment.
[0190] [Production Example 2] Pulp fiber No. 2 after ozone treatment was obtained in the same manner as in Production Example 1, except that the treatment time in the tank was changed to 15 minutes. [Comparative Manufacturing Example 1] The virgin pulp fiber of NBKP was treated with ozone and designated as pulp fiber No. 3.
[0191] After the ozone treatment, the cellulose content, hemicellulose content, and lignin content (mass%) of pulp fibers No. 1 to No. 3 were measured. The results are shown in Table 1.
[0192] [Table 1]
[0193] As shown in Table 1, the ozonated pulp fiber No. 1 of Production Example 1 has a cellulose content of 92.7 mass%, a hemicellulose content of 7.1 mass%, and a lignin content of less than 0.1 mass%. Therefore, the hemicellulose content can be further reduced by subjecting the ozonated pulp fiber No. 1 to a conventionally known alkali treatment process.
[0194] Furthermore, it is expected that by subjecting the post-ozone pulp fiber No. 1 to an alkali treatment process under milder conditions than those conventionally known, it is possible to decompose hemicellulose while suppressing the decomposition of cellulose, thereby obtaining a pulp fiber raw material with a high cellulose yield and a high cellulose content (low hemicellulose content).
[0195] [Example 1] The ozone-treated pulp fiber No. 2 produced in Production Example 2 was subjected to an alkali treatment step.
[0196] Details of the alkali treatment step are as follows. (1) After the ozone treatment, the pulp fiber No. 2 is dried at 40° C. for 1 hour and then crushed in a centrifugal crusher to form a measurement sample. (2) In a constant temperature room at 20°C, about 1.0 g of a sample and 25 mL of an aqueous sodium hydroxide (NaOH) solution having a normality specified in Table 2 are added to a container, and the sample is crushed in the container for 5 minutes. (3) After crushing, the sample is left to stand for 30 minutes.
[0197] (4) Add 25 mL of water at 20° C. to the container and stir the contents of the container for 1 minute. The water mentioned above corresponds to type A3 of "Water for use in testing water and wastewater" in JIS K0557:1998. (5) The contents of the container are filtered through a glass filter under suction to obtain the filtrate. (6) The filtrate is washed with water and then neutralized. (7) 40 mL of a 10% by mass aqueous solution of acetic acid is added to the neutralized filtrate and allowed to stand for 5 minutes. (8) The filtered residue after standing is washed with boiling water and then dried to form pulp fiber raw material No. 2. (9) Analyze the composition of pulp fiber raw material No. 2 using a known detergent method. The normality of the aqueous sodium hydroxide solution and the results of the alkaline treatment step are shown in Table 2. It should be noted that a composition with a NaOH concentration of 0.0N refers to the composition before the start of the alkaline treatment step.
[0198] [Table 2]
[0199] It was confirmed that in the above-mentioned alkali treatment process, pulp fiber raw material No. 2 with a low hemicellulose concentration can be formed not only at a high NaOH concentration (5.3N) but also at a low NaOH concentration (0.5N). When ozone-treated pulp fiber No. 3 (NBKP virgin pulp fiber) from Comparative Manufacturing Example 1 was subjected to the above-mentioned alkali treatment process, the hemicellulose concentration was not easily reduced at low NaOH concentrations (0.5N to 2.8N), and a high NaOH concentration (5.3N) was required to reduce the hemicellulose concentration. [Explanation of symbols]
[0200] 31 Treatment tank 32 Pulp fiber content supply port 33 Processing liquid outlet 43 Ozone-containing gas supply port 51 Pulp fiber content 52 Processing liquid 53 Ozone-containing gas S36 Ozone treatment process
Claims
1. A method for producing a pulp fiber raw material as a cellulose raw material from a pulp fiber to be treated, comprising the steps of: an ozone treatment step of forming ozone-treated pulp fibers from the pulp fibers to be treated by supplying an ozone-containing gas to a treatment tank containing a treatment liquid containing a pulp fiber-containing material containing the pulp fibers to be treated; an alkali treatment step of treating the ozone-treated pulp fibers with an aqueous alkali solution to form the pulp fiber raw material having a hemicellulose content of less than 8.0% by weight; The method according to claim 1, further comprising:
2. 10. The method of claim 1, wherein the pulp fiber source has a lignin content of 0.10% by weight or less.
3. 3. The method of claim 1 or 2, wherein the pulp fiber material has a cellulose content of 94.0% by weight or greater.
4. The method according to any one of claims 1 to 3, wherein in the ozone treatment step, the ozone-containing gas is supplied to the treatment tank so that the pulp fibers after the ozone treatment have a hemicellulose content of 10.0 mass% or less.
5. The method according to any one of claims 1 to 4, wherein in the ozone treatment step, the ozone-containing gas is contacted with the pulp fiber-containing material so that a CT value, which is the product of the ozone concentration in the ozone-containing gas and the treatment time, is 100 to 12,000 ppm min, thereby forming the pulp fibers after the ozone treatment.
6. The method according to any one of claims 1 to 5, wherein in the alkaline treatment step, the aqueous alkaline solution has a normality of 3.0N or less.
7. The method according to claim 6, wherein in the alkali treatment step, the alkaline aqueous solution is added at a ratio of 10 to 40 L per kg of dry mass of the pulp fibers after the ozone treatment.
8. The method according to any one of claims 1 to 7, wherein the pulp fiber raw material is a raw material for cellulose nanofibers, viscose rayon, cellulose derivatives, bioethanol, biobutanol, molding materials, or paper products.
9. The method according to any one of claims 1 to 8, further comprising a cellulose use step of forming cellulose nanofibers, viscose rayon, cellulose derivatives, bioethanol, biobutanol, molding materials, or paper products from the pulp fiber raw material.
10. A pulp fiber raw material as a cellulose raw material, The pulp fiber raw material has a hemicellulose content of less than 8.0% by weight. The pulp fiber raw material.
11. A pulp fiber raw material as a cellulose raw material, The pulp fiber raw material has a cellulose content of 94.0% by mass or more. The pulp fiber raw material.
12. 12. The pulp fiber material of claim 10 or 11, wherein the pulp fiber material has a lignin content of 0.10% by weight or less.
13. The pulp fiber raw material according to any one of claims 10 to 12, which is derived from a used hygiene product containing pulp fibers.
14. The pulp fiber raw material according to any one of claims 10 to 13, wherein the pulp fiber raw material is a raw material for cellulose nanofibers, viscose rayon, cellulose derivatives, bioethanol, biobutanol, molding materials, or paper products.
15. A cellulose nanofiber, a viscose rayon, a cellulose derivative, a bioethanol, a biobutanol, a molding material, or a paper product using the pulp fiber raw material according to any one of claims 10 to 14 as a raw material.
Citation Information
Patent Citations
Method and equipment for recycling waste
JP1994269746A
Method for saccharifying lignocellulose and the resultant saccharide
JP2006141244A
Method and means for recycling fibers from sewage sludge
JP2008532743A
Saccharification and fermentation system
JP2010017084A
Fluffed pulp
JP2015151655A
Cited By
Optical device