Powder magnetic core, inductor, and manufacturing method of powder magnetic core
The powder magnetic core with a thin binder layer achieves miniaturization and low loss in high frequency regions by using low melting point glass and resin to bind magnetic powders, addressing the challenge of simultaneous miniaturization and high inductance in inductors.
Patent Information
- Application Number
- JP2024119488
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Inductors used in electronic devices, particularly personal computers, require miniaturization and high inductance characteristics while maintaining low loss in high frequency ranges, which existing technologies struggle to achieve simultaneously.
A powder magnetic core with a binder layer containing 88% magnetic powder and 6% or less binder layer thickness of 20 nm or less, using low melting point glass and resin material to bind magnetic powders, ensuring high filling rates and insulation.
The solution enables miniaturized inductors with low loss in high frequency regions by maintaining sufficient insulation and high inductance, reducing iron loss to 2500 kW/m³ or less.
Smart Images

Figure 2024144610000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a powder magnetic core, an inductor, and a method for manufacturing a powder magnetic core. [Background technology]
[0002] In recent years, inductors have been used in various electronic devices. In particular, inductors used in electronic devices such as personal computers are required to be compact and to exhibit high inductance characteristics even when a large current is passed through them. Patent Document 1 discloses a method for manufacturing a powder compact of an amorphous soft magnetic alloy that exhibits little decrease in magnetic permeability in the high frequency range. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 10-212503 Summary of the Invention [Problem to be solved by the invention]
[0004] As mentioned above, inductors are required to be compact and also to have high inductance characteristics even when a large current flows through them. In particular, inductors used in electronic devices such as personal computers are used in the high frequency range (e.g., 750 kHz to 2 MHz), so inductors with low loss in the high frequency range are required.
[0005] In view of the above problems, an object of the present invention is to provide a powder magnetic core, an inductor, and a method for manufacturing a powder magnetic core that can achieve miniaturization while achieving low loss in the high frequency range. [Means for solving the problem]
[0006] A powder magnetic core according to one embodiment of the present invention is a powder magnetic core in which magnetic powder is bound via a binder layer, the powder magnetic core containing 88 volume % or more of magnetic powder, and the proportion of binder layers present between the magnetic powder particles that have a thickness of 20 nm or less is 6% or less (not including 0).
[0007] A method for producing a dust core according to one embodiment of the present invention includes the steps of coating a magnetic powder with a low-melting glass, coating the magnetic powder coated with the low-melting glass with a resin material and granulating the magnetic powder, and hot-compacting the granulated magnetic powder. The compact after the hot-compacting contains 88 volume % or more of magnetic powder, binder layers containing the low-melting glass and the resin material are formed between the magnetic powder particles, and the proportion of binder layers between the magnetic powder particles that have a thickness of 20 nm or less is 6% or less (excluding 0). Effect of the Invention
[0008] The present invention can provide a powder magnetic core, an inductor, and a method for manufacturing a powder magnetic core that can realize miniaturization while achieving low loss in the high frequency range. [Brief description of the drawings]
[0009] [Figure 1] 1 is a perspective view illustrating an example of an inductor according to an embodiment; [Diagram 2] 1 is an electron microscope photograph of a powder magnetic core according to a conventional technique and a powder magnetic core according to the present invention. [Diagram 3] FIG. 2 is a schematic diagram for explaining the microstructure of a powder magnetic core according to the prior art and the microstructure of a powder magnetic core according to the present invention. [Figure 4] 1 is an electron microscope photograph showing a microstructure of a dust core according to an embodiment. [Diagram 5] 2 is a flowchart for explaining a method for manufacturing a powder magnetic core according to an embodiment. [Figure 6] FIG. 2 is a schematic diagram for explaining a method for producing a powder magnetic core according to an embodiment. [Figure 7]FIG. 2 is a horizontal cross-sectional view of a powder magnetic core according to an embodiment. [Figure 8] FIG. 2 is a horizontal cross-sectional view of a powder magnetic core according to an embodiment. [Figure 9] FIG. 2 is a horizontal cross-sectional view of a powder magnetic core according to an embodiment. [Figure 10] FIG. 2 is a horizontal cross-sectional view of a powder magnetic core according to an embodiment. [Figure 11] 1 is a graph plotting the iron loss and the proportion of the binder layer of 20 nm or less for samples with the same binder amount and magnetic powder particle size. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] <Inductor> Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a perspective view showing an example of an inductor according to the present embodiment. As shown in Fig. 1, the inductor 1 according to the present embodiment includes powder cores 10_1, 10_2, and a coil 13. The powder core 10_1 has a cavity that passes vertically through the center, and is disposed so as to surround the outside of the coil 13. The powder core 10_2 is provided inside the coil 13, and is disposed in a recess of the coil 13 having a U-shaped cross section.
[0011] For example, the inductor 1 shown in FIG. 1 can be formed by arranging the powder core 10_2 in the recess of the coil 13, and then pressing the powder core 10_1 from above. This allows the inductor 1 in which the coil 13 is surrounded by the powder cores 10_1 and 10_2 to be formed. In this specification, the powder cores 10_1 and 10_2 are also collectively referred to as the powder core 10. The configuration of the inductor 1 shown in FIG. 1 is an example, and the powder core 10 according to this embodiment may be used for an inductor having a configuration other than that shown in FIG. The powder core according to this embodiment is characterized in that it realizes low loss in the high frequency range while realizing miniaturization. Hereinafter, the powder core according to this embodiment will be described in detail.
[0012] <Powder magnetic core> The dust core according to the present embodiment is a dust core in which magnetic powder is bound via a binder layer. The dust core contains 88% or more by volume of magnetic powder, and the proportion of binder layers with a thickness of 20 nm or less among the binder layers present between the magnetic powder particles is 6% or less (not including 0). With this configuration, it is possible to provide a dust core that can realize miniaturization while realizing low loss in the high frequency range. The proportion of binder layers with a thickness of 20 nm or less among the binder layers present between the magnetic powder particles may preferably be 3.3% or less.
[0013] The magnetic powder used in the dust core according to the present embodiment is a soft magnetic powder containing iron. For example, the particle size of the magnetic powder is 2 μm or more and 25 μm or less, preferably 5 μm or more and 15 μm or less. In the present invention, the particle size is the median diameter D50, which is a value measured by a laser diffraction / scattering method.
[0014] In this embodiment, metallic glass can be used as the magnetic powder. For example, amorphous metallic glass produced by atomization can be used as the metallic glass. For example, Fe-PB alloy, Fe-BP-Nb-Cr alloy, Fe-Si-B alloy, Fe-Si-BP alloy, Fe-Si-BP-Cr alloy, Fe-Si-BPC alloy can be used, and metallic glass having a glass transition point can be formed by powdering by atomization. In particular, in the present invention, it is preferable to use Fe-BP-Nb-Cr-based materials. Note that metallic glass obtained by atomization is not limited to these, and metallic glass having no glass transition point can also be used.
[0015] In addition, in this embodiment, for example, nanocrystalline powder may be used as the magnetic powder. For example, nanocrystalline powder produced by atomization may be used as the nanocrystalline powder. For example, by powdering Fe-Si-BPC-Cu-based, Fe-Si-B-Cu-Cr-based, Fe-Si-BP-Cu-Cr-based, Fe-BPC-Cu-based, Fe-Si-BP-Cu-based, Fe-BP-Cu-based, and Fe-Si-B-Nb-Cu-based materials by atomization, nanocrystalline powder having at least two exothermic peaks indicating crystallization in the heat treatment process of the magnetic powder can be formed. The nanocrystalline powder used is not particularly limited, but it is preferable to use, for example, Fe-Si-BP-Cu-Cr-based materials.
[0016] In this embodiment, the particle shape of the magnetic powder is preferably as close to spherical as possible. If the sphericity of the particles is low, protrusions are formed on the particle surface, and when a compaction pressure is applied, stress from the surrounding particles is concentrated on the protrusions, destroying the coating, and the insulation is not sufficiently maintained, which may result in deterioration of the magnetic properties (particularly loss) of the obtained dust core. The sphericity of the particles can be controlled within a suitable range by adjusting the manufacturing conditions of the magnetic powder, for example, in the case of a water atomization method, the amount of water and water pressure of the high-pressure water jet used for atomization, the temperature and supply speed of the molten raw material, and the like. The specific manufacturing conditions vary depending on the composition of the magnetic powder to be manufactured and the desired productivity.
[0017] In the dust core according to the present embodiment, the binder layer has a function of binding the magnetic powder together. The binder layer includes a low-melting glass and a resin material. In the present embodiment, the total amount of the low-melting glass and the resin material is less than 10% by volume with respect to the magnetic powder of the dust core. The low-melting glass may be a phosphate-based, tin-phosphate-based, borate-based, silicate-based, borosilicate-based, barium silicate-based, bismuth oxide-based, germanate-based, vanadate-based, aluminophosphate-based, arsenate-based, telluride-based, or the like. In particular, in the present invention, it is preferable to use a phosphate-based or tin-phosphate-based low-melting glass. The volume ratio of the low-melting glass to the magnetic powder is 0.5% by volume or more and 6% by volume or less, preferably 1.25% by volume or more and 3% by volume or less.
[0018] The resin material contained in the binder layer may be at least one selected from the group consisting of phenol resin, polyimide resin, epoxy resin, and acrylic resin, and the volume ratio of the resin material to the magnetic powder is 0.5% by volume or more and 9% by volume or less, preferably 1% by volume or more and 5% by volume or less.
[0019] The dust core according to the present embodiment having the above configuration contains 88 volume % or more of magnetic powder, and the proportion of the binder layer between the magnetic powder particles having a thickness of 20 nm or less is 6% or less (excluding 0). Therefore, it is possible to make the binder layer thin and increase the packing rate of the magnetic powder while maintaining sufficient insulation between the magnetic powder particles. Therefore, the dust core according to the present embodiment can reduce inductor loss in the high frequency range while realizing miniaturization.
[0020] Figure 2 shows electron microscope images of a conventional powder magnetic core and a powder magnetic core of the present invention. In the conventional technology shown in Figure 2, the packing rate of the magnetic powder is low. In contrast, the powder magnetic core of the present invention has a higher packing rate of the magnetic powder than the powder magnetic core of the conventional technology. Therefore, it shows high inductance characteristics even when a large current is passed through it.
[0021] 3 is a schematic diagram for explaining the microstructure of a dust core of the prior art and the microstructure of a dust core of the present invention. In the prior art of FIG. 3, the thickness of the binder layer 122 between the magnetic powder particles 121 is non-uniform. For example, the binder layer 122 is thick in region 131, but is thin in regions 132 and 133. That is, in this case, the proportion of the binder layer 122 between the magnetic powder particles 121 that is 20 nm or less thick (i.e., the proportion of areas where the binder layer is thin, such as regions 132 and 133) is high. As a result, the proportion of areas where the binder layer 122 is thick is high.
[0022] In contrast, in the dust core of the present invention, the thickness of the binder layer 22 between the magnetic powder particles 21 is uniform. In other words, the proportion of the binder layer 22 between the magnetic powder particles 21 that is 20 nm or less thick (i.e., the proportion of portions where the binder layer is thin) is small. As a result, the proportion of thick portions of the binder layer 22 is low, and the binder layer 22 is uniform overall. As an example, the dust core of the present invention has a median thickness of the binder layer 22 of 31 to 68 nm.
[0023] FIG. 4 is an electron microscope photograph showing the microstructure of the powder magnetic core according to the present embodiment, and is a diagram for explaining a method for determining "the ratio of the binder layer having a thickness of 20 nm or less among the binder layers present between the magnetic powders". When measuring the thickness of the binder layer, an electron microscope photograph (SEM image) of the powder magnetic core is used to identify a region in which the binder is filled between the magnetic powders and the interval between the magnetic powders is 200 nm or less over a length of 100 nm or more. Then, in the identified region, the thickness of the binder layer is measured every 100 nm. An example of measurement is shown in the right diagram of FIG. 4. Whether or not the binder is present between the magnetic powders can be determined using the contrast of the SEM image or the results of elemental analysis by EDX (Energy dispersive X-ray spectroscopy). For example, it is preferable to measure the thickness of the binder layer at 400 points or more. The interval between the magnetic powders may be measured by assuming a normal line at a point on the surface of one of the magnetic powders, and measuring the distance between the two powders in the normal direction.
[0024] For example, if there are 400 measurement points and 20 of those have binder layer thicknesses of 20 nm or less, then the "proportion of binder layers between magnetic powder particles that have a thickness of 20 nm or less" = (20 / 400) × 100 = 5%.
[0025] As shown in the lower left diagram of FIG. 4, even if the spacing between magnetic powder particles is 200 nm or less (90 nm in the diagram), if no binder is filled, the particle is excluded from the measurement.
[0026] <Method of manufacturing powder core> Next, a method for producing a powder magnetic core according to the present embodiment will be described. Fig. 5 is a flow chart for explaining the method for producing a powder magnetic core according to the present embodiment. Fig. 6 is a schematic diagram for explaining the method for producing a powder magnetic core according to the present embodiment.
[0027] As shown in FIG. 5, when manufacturing a dust core, first, magnetic powder is prepared (step S1). The magnetic powder may be any of the magnetic powders described above. It is preferable to use a magnetic material that softens at 400° C. or higher (a material that is easily deformed during hot compaction) for the magnetic powder. For example, the raw material for the magnetic powder is vacuum melted, and then powdered and quenched simultaneously using a water atomization method to obtain amorphous magnetic powder. The magnetic powder obtained in this manner may be classified as necessary to remove abnormally coarse powder.
[0028] Next, the magnetic powder is coated with low-melting glass (step S2). For the low-melting glass, it is preferable to use a material that softens at 400°C or higher, that is, a material that softens during hot molding and acts as an insulating material and a binder after hot molding. For example, phosphate-based glass can be used as the low-melting glass. When coating the magnetic powder with low-melting glass, a wet thin film preparation method such as mechanofusion or sol-gel method, or a dry thin film preparation method such as sputtering can be used. For example, the mechanofusion method can form a layer of low-melting glass on the surface of the magnetic powder by mixing the magnetic powder and low-melting glass powder while applying strong mechanical energy.
[0029] For example, 1000 g of magnetic powder is mixed with 10 g of low-melting glass powder, and the magnetic powder is coated with the low-melting glass by mechanofusion, so that the volume ratio of the coated low-melting glass to the magnetic powder can be set to 0.5% by volume or more and 6% by volume or less.
[0030] Next, the magnetic powder coated with the low-melting glass is coated with a resin material and granulated (step S3). The resin material may be any of the above-mentioned resin materials. It is preferable to use a material that softens at about 100°C and acts as an insulating material and a binder after hot molding. It is also preferable to use a material that is not easily decomposed during hot molding (at high temperatures). When coating (granulating) the resin material, a rolling granulation method or a spray drying method may be used. Specifically, a resin layer can be formed on the low-melting glass of the magnetic powder by mixing the resin material dissolved in an organic solvent with the magnetic powder coated with the low-melting glass and drying it.
[0031] The magnetic powder 20 after granulation is shown in the left diagram of Fig. 6. As shown in Fig. 6, in the magnetic powder 20 after granulation, low-melting point glass 31 is coated on the magnetic powder 21, and resin material 32 is further coated on the low-melting point glass 31. As an example, the diameter of the magnetic powder 21 is 9 μm, the thickness of the low-melting point glass 31 is 20 nm, and the thickness of the resin material is 20 nm.
[0032] Next, the granulated magnetic powder is preformed (step S4). For example, the preformation is performed by putting the granulated magnetic powder into a mold and applying pressure (for example, 500 kgf / cm at room temperature). 2 ), and then, without applying pressure, the green compact is heated at a prescribed temperature (for example, 100°C to 150°C) to harden it. When the resin material used is a thermosetting resin, the intermediate molded body is formed by hardening the resin when heated. When the resin material used is a thermoplastic resin, the intermediate molded body is formed by softening the resin when heated and solidifying it when cooled.
[0033] That is, as shown in the center of Fig. 6, when preforming is performed, the magnetic powder 21 (coated with low-melting point glass 31) is bound via the outermost resin material 32 to form an intermediate molded body 25. Since the low-melting point glass does not soften at the preforming temperature (e.g., 150°C), it does not exhibit binding properties or fluidity. The preforming step (step S4) may be omitted.
[0034] Next, the preformed intermediate compact (or the granulated magnetic powder if step S4 is omitted) is hot-formed (step S5). The hot forming is performed by heating the preformed intermediate compact (or the granulated magnetic powder) while applying pressure in a metal mold. The heating temperature at this time is set, for example, as follows:
[0035] When the magnetic powder used is a metallic glass, the temperature during hot molding is set to be equal to or higher than the softening temperature of the low melting point glass and the glass transition temperature of the magnetic powder, whichever is higher, and equal to or lower than the crystallization temperature of the magnetic powder. By setting the hot molding temperature at or above the glass transition temperature of the magnetic powder, the magnetic powder is more likely to undergo plastic deformation, resulting in a high filling rate of the magnetic powder. For example, the temperature is 450°C or higher and 500°C or lower.
[0036] When the magnetic powder used is a nanocrystalline powder, the temperature during hot molding is set to the higher of the softening temperature of the low-melting glass and the first crystallization temperature of the magnetic powder, and to the second crystallization temperature of the magnetic powder. By setting the hot molding temperature to about the first crystallization temperature, the α-Fe phase crystallizes and the magnetic powder is more likely to undergo plastic deformation, so that a high filling rate of the magnetic powder can be obtained. For example, the temperature is 400°C or higher and 500°C or lower. In addition, in the present invention, the temperature is preferably the higher of the softening temperature of the low-melting glass and the first crystallization temperature of the magnetic powder + 40°C. Here, the first crystallization temperature and the second crystallization temperature are as follows. That is, when a magnetic material with an amorphous structure is heat-treated, crystallization occurs two or more times. The temperature at which crystallization first starts is the first crystallization temperature, and the temperature at which crystallization starts thereafter is the second crystallization temperature. More specifically, the magnetic powder has at least two exothermic peaks indicating crystallization during the heating process of a DSC curve obtained by differential scanning calorimetry (DSC). The lowest exothermic peak among the exothermic peaks is the first crystallization temperature at which the α-Fe phase crystallizes, and the next exothermic peak is the second crystallization temperature at which borides and the like crystallize.
[0037] In this embodiment, it is preferable that the heating temperature is set within the above-mentioned temperature range and that the temperature condition is set so that the iron loss value of the powder magnetic core is low.
[0038] The pressure during hot forming is, for example, 5 to 10 ton f / cm 2 If the pressure is too low, the packing rate of the compact (dust core) will be low, and the iron loss of the dust core will be high. Conversely, if the pressure is too high, the die will wear out rapidly, which is not preferable from the standpoint of cost. Therefore, it is preferable to set the pressure within the above range.
[0039] The hot molding time is preferably in the range of 5 to 60 seconds, and more preferably 30 seconds or less. If the molding time is too short, the heat is not sufficiently transmitted to the inside of the molded body, and the deformation due to the softening of the magnetic powder is not sufficiently obtained, so that the filling rate of the molded body is low and the iron loss of the powder core is large. On the other hand, if the molding time is too long, the thermal decomposition of the resin material used in the binder layer progresses, so that the effect of suppressing the fluidity of the low-melting point glass is reduced, and the iron loss of the powder core is large. Therefore, the hot molding time may be set in a cost-preferable range in which the heat is sufficiently transmitted to the inside of the molded body, the deformation due to the softening of the magnetic powder is completed, and the thermal decomposition of the resin material used in the binder layer is suppressed, and it is preferable to set the molding time in the above-mentioned range.
[0040] For example, the hot forming conditions are: hot forming temperature: 480°C, hot forming pressure: 8 ton f / cm 2 , hot forming time: can be 10 seconds.
[0041] As shown in the right diagram of FIG. 6, in the compact (powder core) 10 after hot compaction, the magnetic powder particles 21 are bound together via a binder layer 22 containing a low melting point glass and a resin material. In this embodiment, the volume ratio of the magnetic powder contained in the powder core 10 is set to 88 volume % or more. In addition, the ratio of the binder layer having a thickness of 20 nm or less among the binder layers present between the magnetic powder particles is set to 6% or less. This makes it possible to increase the packing rate of the magnetic powder and to maintain sufficient insulation between the magnetic powder particles. Therefore, the method for producing a powder core according to this embodiment makes it possible to produce a powder core that can achieve miniaturization while achieving low loss in the high frequency range.
[0042] As explained in the Background Art, inductors are required to be small in size and to exhibit high inductance characteristics even when a large current is passed through them. In addition, inductors with low loss in the high frequency range are required. To realize such inductors, it is necessary to increase the packing rate of magnetic powder in the powder core used in the inductor and maintain sufficient insulation between the magnetic powder particles. However, with conventional technology, it has been difficult to simultaneously increase the packing rate of magnetic powder and maintain sufficient insulation between the magnetic powder particles.
[0043] In contrast, in the manufacturing method of the powder magnetic core according to the present embodiment, the binder layer is formed using low-melting glass and a resin material. In this way, by using low-melting glass and a resin material as the binder, a binder layer (insulating layer) of a thin and uniform thickness can be formed even if the amount of binder added is small. In other words, by mixing and using a binder component (low-melting glass) that is easy to flow at the hot molding temperature and a binder component (resin material) that is difficult to flow, the insulation between the magnetic powders can be maintained even if the amount of binder added is small. In other words, in the present embodiment, by intentionally leaving the resin during hot molding, the flow of the low-melting glass, which is relatively softer than the magnetic powder, can be suppressed to some extent, so that the magnetic powders can be suppressed from contacting each other without the binder layer (insulating layer).
[0044] Furthermore, in the method for producing a powder magnetic core according to the present embodiment, the amount of resin material used as a binder is small, which reduces the amount of gas generated due to the decomposition of the resin material during hot compaction, thereby suppressing cracks in the compact (powder magnetic core) caused by the generated gas.
[0045] In this embodiment, the iron loss of the powder magnetic core is 2500 kW / m 3 It is preferable that the rated current is less than 1500 kW / m 3 It is more preferable that:
[0046] <Dimensions of powder magnetic core> Next, the dimensions of the powder magnetic core according to this embodiment will be described. In this embodiment, when the vertical length of the powder magnetic core (distance h in the example shown in FIG. 1) is longer than 3.5 mm, the distance between the molding dies that sandwich the powder magnetic core in a horizontal cross section of the powder magnetic core, in a direction approximately perpendicular to the direction in which the portion that takes the longest time for heat to transfer to the inside of the powder magnetic core extends when the powder magnetic core is hot compacted, is set to 3.5 mm or less. A specific example will be described below.
[0047] For example, when the shape of the horizontal cross section of the powder core is like the powder core 10_1 shown in FIG. 7 (the powder core 10_1 shown in FIG. 7 corresponds to the powder core 10_1 shown in FIG. 1), the powder core 10_1 is molded while being sandwiched between the molding dies 61 during hot compacting. At this time, heat is transferred from the molding dies 61 to the powder core 10_1, but the part inside the powder core 10_1 to which heat is least likely to be transferred is the part indicated by the reference symbol 71. In this embodiment, the distance b between the molding dies in a direction approximately perpendicular to the extension direction of the part 71 that takes the longest time for heat to be transferred inside the powder core 10_1 is set to 3.5 mm or less. By setting such dimensions, heat can be rapidly transferred to the entire powder core 10_1 during hot compacting.
[0048] Also, for example, when the shape of the horizontal cross section of the powder core is like that of the powder core 52 shown in FIG. 8 (that is, a shape without a cavity in the center), the powder core 52 is molded while being sandwiched between the molding dies 62 during hot compacting. At this time, heat is transferred from the molding dies 62 to the powder core 52, but the part inside the powder core 52 to which heat is least likely to be transferred is the part indicated by the reference symbol 72. In this embodiment, the distance b2 between the molding dies in a direction approximately perpendicular to the extension direction of the part 72 that takes the longest time for heat to be transferred inside the powder core 52 is set to 3.5 mm or less. By setting such dimensions, heat can be transferred quickly to the entire powder core 52 during hot compacting.
[0049] Furthermore, for example, when the shape of the horizontal cross section of the powder core is like that of the powder core 53 shown in FIG. 9 (that is, a shape with two cavities in the center), the powder core 53 is molded while being sandwiched between the molding dies 63 during hot compacting. At this time, heat is transferred from the molding dies 63 to the powder core 53, but the part inside the powder core 53 to which heat is least likely to be transferred is the part indicated by the reference symbol 73. In this embodiment, the distance b3 between the molding dies in a direction approximately perpendicular to the extension direction of the part 73 that takes the longest time for heat to be transferred inside the powder core 53 is set to 3.5 mm or less. By setting such dimensions, heat can be transferred quickly to the entire powder core 53 during hot compacting.
[0050] Furthermore, for example, when the shape of the horizontal cross section of the powder core is like that of the powder core 54 shown in Fig. 10 (i.e., an E-shaped core), the powder core 54 is molded while being sandwiched between molding dies 64 during hot compacting. At this time, heat is transferred from the molding dies 64 to the powder core 54, but the part inside the powder core 54 to which heat is least likely to be transferred is the part indicated by reference numeral 74. In this embodiment, the distance b4 between the molding dies in a direction approximately perpendicular to the direction in which the part 74 that takes the longest time for heat to transfer inside the powder core 54 extends is set to 3.5 mm or less. By setting such dimensions, heat can be transferred quickly to the entire powder core 54 during hot compacting.
[0051] The configuration examples shown in Figs. 7 to 10 are merely examples, and the dimensions of the powder core according to this embodiment can be applied to powder cores having other configurations. For example, when the shape of the horizontal cross section of the powder core is circular, the part that takes the longest time for heat to be transferred to the inside of the powder core 54 is a point. In this case, the diameter of the circle passing through this point is set to 3.5 mm or less. In this embodiment, the vertical length of the powder core may be set to 3.5 mm or less. In this way, when the vertical length of the powder core is set to 3.5 mm or less, the distance between the molding dies in the horizontal cross section of the powder core can be set arbitrarily.
[0052] As described above, by setting the dimensions of the powder magnetic core according to the present embodiment to the above dimensions, heat can be easily transferred to the powder magnetic core during hot compaction. This makes it possible to shorten the hot compaction time and suppress the thermal decomposition of the resin material. This enhances the effect of suppressing the fluidity of the low melting point glass, and reduces the iron loss of the powder magnetic core. EXAMPLES
[0053] Next, an embodiment of the present invention will be described.
[0054] <Experiment 1> A sample for Experiment 1 was produced using the above-mentioned manufacturing method for the powder magnetic core (see FIG. 5). The shape of the powder magnetic core for Experiment 1 was a toroidal shape with an outer diameter of 13 mm, an inner diameter of 8 mm, and a length of 5 mm. Specifically, first, magnetic powder was prepared. For the magnetic powder, Fe-BP-Nb-Cr-based powder, which is a metallic glass powder with a particle size of 9 μm (median diameter D50), was used. Next, the magnetic powder was mixed with low-melting-point glass powder, and the magnetic powder was coated with the low-melting-point glass by using a mechanofusion method. Phosphate-based glass was used for the low-melting-point glass. At this time, 2.5 volume % of the low-melting-point glass was mixed with the magnetic powder.
[0055] The magnetic powder coated with the low melting point glass was then coated with a resin material and granulated. The resins used were those shown in Table 1. At this time, 2.5 volume % of each resin material was mixed with the magnetic powder. Note that the "resin weight loss on heating at 500°C" in Table 1 is the result of thermogravimetric analysis of the resin (measurement conditions: air atmosphere, heating rate 100°C / min), and the smaller the weight loss on heating, the higher the heat resistance of the resin.
[0056] Next, the granulated magnetic powder is poured into a die and pressurized at 500 kgf / cm 2 After pressing under these conditions, the green compact was preformed by heating it to a temperature of 150°C without applying pressure and hardening it. The preformed intermediate compact was then placed in a die and hot formed. The hot forming conditions were a forming temperature of 490°C and a pressure of 8 tonf / cm. 2 The pressure application time was 30 seconds.
[0057] For each sample prepared as described above, the powder filling rate of the magnetic core, magnetic permeability, iron loss, the ratio of the binder layer with a thickness of 20 nm or less among the binder layers present between the magnetic powders, and the median thickness of the binder layer were measured. The thickness of the binder layer was measured at 1000 points.
[0058] The powder filling rate of the magnetic core was calculated by comparing the volume of the magnetic powder contained in the magnetic core with the volume of the entire magnetic core measured by the Archimedes method. The volume of the magnetic powder contained in the magnetic core was calculated by subtracting the weight of the low-melting glass added as a binder and the weight of the remaining resin material from the weight of the entire magnetic core to calculate the weight of the magnetic powder contained in the magnetic core, and then dividing the weight of the magnetic powder by the true density of the magnetic powder.
[0059] The magnetic permeability was determined using an impedance analyzer at a frequency of 1 MHz, and the core loss was determined by preparing a toroidal powder magnetic core and measuring the prepared powder magnetic core by the two-coil method using a BH analyzer (manufactured by Iwasaki Electric Co., Ltd.) The measurement conditions were 1 MHz, 50 mT sinusoidal wave excitation conditions.
[0060] The ratio of the binder layers between the magnetic powder particles that are 20 nm or less thick (hereinafter referred to as "the ratio of the binder layers that are 20 nm or less") was measured using the above-mentioned method with the aid of an electron microscope photograph. The median thickness of the binder layers was also measured with the aid of an electron microscope photograph.
[0061] Table 1 shows the type of resin used in each sample and the measurement results of each sample. As shown in Table 1, in Example 1-1 using a phenol resin as the binder resin, Example 1-2 using a polyimide resin, Example 1-3 using an epoxy resin, and Example 1-4 using an acrylic resin, the iron loss value was 1100 or less, which was a good value. In addition, in Examples 1-1 to 1-4, the ratio of the binder layer of 20 nm or less was 2.2% or less, which was good. In particular, in Examples 1-1 to 1-3, the ratio of the binder layer of 20 nm or less was lower than 1%, and the iron loss value was also smaller than 1000.
[0062] On the other hand, in Comparative Example 1-1, in which a silicone resin was used as the binder resin, Comparative Example 1-2, in which a PVB (polyvinyl butyral) resin was used, and Comparative Example 1-3, in which no resin was used, the iron loss value was 5500 or more, which was a large value.
[0063] From the above results, it can be said that it is preferable to use a phenol resin, a polyimide resin, an epoxy resin, or an acrylic resin as the resin used for the binder layer.
[0064] [Table 1]
[0065] <Experiment 2> In Experiment 2, a dust core was produced in which the particle size (median diameter D50) of the metallic glass powder, which is the magnetic powder, was changed. In Experiment 2, phosphate-based glass and phenolic resin were used as materials for the binder. The dust core was produced and the samples were measured using the same method as in Experiment 1. In Comparative Example 2-1 and Example 2-1, the volume ratio of the phosphate-based glass to the magnetic powder was 5 volume %, and the volume ratio of the phenolic resin to the magnetic powder was 2.5 volume %. In Example 2-2, the volume ratio of the phosphate-based glass to the magnetic powder was 2.5 volume %, and the volume ratio of the phenolic resin to the magnetic powder was 2.5 volume %. In addition, as shown in Table 2, the softening temperature of the phosphate-based glass is 400 ° C., the glass transition temperature of the magnetic powder is 480 ° C., and the crystallization temperature of the magnetic powder is 510 ° C., so the molding temperature was set to 490 ° C.
[0066] As shown in Table 2, in Comparative Example 2-1 in which the particle size of the metallic glass powder is 4 μm, the iron loss value is 12000, and the ratio of the binder layer of 20 nm or less is 13.5%, both of which are large values. On the other hand, in Example 2-1 in which the particle size of the metallic glass powder is 7 μm, and Example 2-2 in which the particle size of the metallic glass powder is 9 μm, the iron loss values are 1100 and 900, respectively, which are good values. In addition, in Examples 2-1 and 2-2, the ratio of the binder layer of 20 nm or less is 1.7% and 0.92%, respectively, which are good values. Therefore, in Experiment 2, when the particle size of the metallic glass powder is 7 μm or more, the iron loss and the ratio of the binder layer of 20 nm or less are good values.
[0067] In addition, while phosphate glass and phenol resin were used as binder materials in experiment 2, the inventors also conducted an experiment using 5 volume % phosphate glass and 2.5 volume % polyimide resin as binders relative to the magnetic powder. In this case, it was confirmed that even when the particle size of the metallic glass (magnetic powder) is 2 μm, the filling rate of the powder core is 88 volume % or more, the proportion of the binder layer of 20 nm or less is 6% or less, and the iron loss is 2500 or less.
[0068] [Table 2]
[0069] <Experiment 3> In experiment 3, dust cores were produced by changing the particle size (median diameter D50) of nanocrystalline powder, which is a Fe-Si-BP-Cu-Cr magnetic powder. In experiment 3, phosphate glass and phenol resin were used as binder materials. The same method as in experiment 1 was used to produce dust cores and measure the samples. In experiment 3, the volume ratio of the phosphate glass to the magnetic powder was 2.5 volume %, and the volume ratio of the phenol resin to the magnetic powder was 2.5 volume %. In addition, as shown in Table 3, the molding temperature was set to a temperature between the higher of the softening temperature of the low-melting glass (400°C) and the first crystallization temperature of the magnetic powder, and the second crystallization temperature of the magnetic powder.
[0070] As shown in Table 3, in Example 3-1 in which the particle size of the nanocrystalline powder is 11 μm, Example 3-2 in which the particle size of the nanocrystalline powder is 14 μm, and Example 3-3 in which the particle size of the nanocrystalline powder is 23 μm, the iron loss value is 2500 or less, and the ratio of the binder layer of 20 nm or less is 1% or less, which are good values. In particular, in Example 3-1 in which the particle size of the nanocrystalline powder is 11 μm, the iron loss value is 860, which is a very good value. On the other hand, in Comparative Example 3-1 in which the particle size of the nanocrystalline powder is 41 μm, the iron loss value is large at 5300, and the ratio of the binder layer of 20 nm or less is also 0%.
[0071] From the results of Experiments 2 and 3, it was found that if the particle size is too small, the median thickness of the binder layer becomes too thin, which means that the insulation between the magnetic powder particles is not sufficiently maintained, and the iron loss of the powder core increases due to eddy current loss between the magnetic powder particles. On the other hand, if the particle size is too large, the median thickness of the binder layer becomes too thick, which means that the insulation between the magnetic powder particles is sufficiently ensured, but the iron loss of the powder core increases due to eddy current loss within the magnetic powder particles. From the above, it can be said that the particle size of the magnetic powder is preferably 2 μm or more and 25 μm or less, and more preferably 5 μm or more and 15 μm or less.
[0072] [Table 3]
[0073] <Test 4> In experiment 4, powder magnetic cores were produced by changing the compounding ratio of phosphate glass and phenol resin, which are binder materials. In experiment 4, metallic glass powder with a particle size of 9 μm (median diameter D50) was used as the magnetic powder. The same methods as in experiment 1 were used to produce the powder magnetic cores and measure the samples. Table 4 shows the compounding ratio of phosphate glass and phenol resin for each sample.
[0074] As shown in Table 4, in Comparative Example 4-1, in which the compounding ratio (volume %) of phosphate-based glass and phenolic resin is 2.5:0 (i.e., phenolic resin is not added), the iron loss value is 17000, and the ratio of the binder layer of 20 nm or less is 13.3%, both of which are large values. In Example 4-1, in which the compounding ratio (volume %) of phosphate-based glass and phenolic resin is 2.5:2.5, the iron loss value is 900, and the ratio of the binder layer of 20 nm or less is 0.92%, which are good values. In Example 4-2, in which the compounding ratio (volume %) of phosphate-based glass and phenolic resin is 2.5:5, the iron loss value is 1100, and the ratio of the binder layer of 20 nm or less is 0.57%, which are good values. On the other hand, in Comparative Example 4-2, in which the compounding ratio (volume %) of phosphate-based glass and phenolic resin was 2.5:10, the iron loss value was 2100, but the proportion of the binder layer of 20 nm or less was 0%, and the powder filling rate was a low value of 84.2%.
[0075] [Table 4]
[0076] <Test 5> In experiment 5, powder magnetic cores were produced by changing the compounding ratio of the binder materials, phosphate glass and phenol resin. In experiment 5, nanocrystalline powder with a particle size of 11 μm (median diameter D50) was used as the magnetic powder. The same methods as in experiment 1 were used to produce the powder magnetic cores and measure the samples. Table 5 shows the compounding ratio of phosphate glass and phenol resin for each sample.
[0077] As shown in Table 5, in Examples 5-1 to 5-5, the iron loss was 2500 or less, and the proportion of the binder layer of 20 nm or less was 6% or less (excluding 0), which were good values. In particular, in Example 5-3, in which the compounding ratio (volume %) of the phosphate glass and the phenolic resin was 2.5:2.5, the iron loss value was 860, which was a very good value. On the other hand, in Comparative Examples 5-1 to 5-3, the iron loss was 2500 or less, but the filling factor of the powder magnetic core was lower than 88 volume %, and the magnetic permeability was also low at 78 or less. From the results of Experiments 4 and 5, it can be said that the total amount of low-melting glass and resin material relative to the magnetic powder is preferably less than 10% by volume.
[0078] [Table 5]
[0079] <Experiment 6> In experiment 6, cylindrical samples with an outer diameter of 40 mm and varying vertical length (thickness h) were prepared. In experiment 6, nanocrystalline powder with a particle size of 11 μm (median diameter D50) was used as the magnetic powder. Phosphate glass and phenolic resin were used as binder materials. The volume ratio of the phosphate glass to the magnetic powder was 2.5 volume %, and the volume ratio of the phenolic resin to the magnetic powder was 2.5 volume %. The same method as in experiment 1 was used to prepare the powder core. In experiment 6, the prepared powder core was cut into the same shape as in experiment 1 (a toroidal shape with an outer diameter of 13 mm, an inner diameter of 8 mm, and a length of 5 mm) to prepare a sample for measurement. The sample was then measured using the same method as in experiment 1.
[0080] As shown in Table 6, the compaction time for each sample was changed according to the thickness of the thinnest part. In other words, the compaction time for the sample was made longer as the thickness h became thicker so that the heat was transferred to the part that takes the longest time to transfer inside the powder core and was transferred to the entire powder core. More specifically, the compaction time was set so that the heat was transferred to the middle part of the vertical length (thickness h) of the powder core and sufficient deformation due to softening of the magnetic powder throughout the powder core was obtained.
[0081] As shown in Table 6, in Example 6-1 with a thickness h of 1.7 mm, Example 6-2 with a thickness h of 2.5 mm, Example 6-3 with a thickness h of 3.0 mm, and Example 6-4 with a thickness h of 3.5 mm, the iron loss value was 2500 or less, and the ratio of the binder layer of 20 nm or less was 6% or less (excluding 0). In particular, in Example 6-1 with a thickness h of 1.7 mm, the iron loss value was 860, which was a very good value.
[0082] On the other hand, in Comparative Example 6-1 with a thickness h of 4.5 mm, Comparative Example 6-2 with a thickness h of 7 mm, and Comparative Example 6-3 with a thickness h of 14 mm, the iron loss value was greater than 2500, and the proportion of the binder layer of 20 nm or less was greater than 6%.
[0083] From the above results, it can be said that it is preferable to set the vertical length (thickness h) of the powder core, which is the part that takes the longest time for heat to be transmitted inside the powder core when the powder core is hot-molded, to 3.5 mm or less. In other words, by quickly transmitting heat to the entire powder core during hot molding, it is possible to prevent a decrease in the effect of suppressing the thermal decomposition of the binder resin and suppressing the fluidity of the low-melting point glass, and to obtain a good iron loss value. In addition, since heat is quickly transmitted to the entire powder core, the time for hot molding can be shortened, making it possible to reduce manufacturing time and costs. In addition, in Experiment 6, the experiment was performed by changing the vertical length of the powder core, but for the same reason, it can also be said that it is preferable to set the distance between the molding dies in the direction approximately perpendicular to the direction in which the part that takes the longest time for heat to be transmitted inside the powder core extends to 3.5 mm or less.
[0084] [Table 6]
[0085] <Experiment 7> For experiment 7, samples were produced by changing the type of low-melting glass used as the binder material. In experiment 7, metallic glass powder with a particle size of 9 μm (median diameter D50), a first crystallization temperature (Tg) of 480°C, and a second crystallization temperature (Tx) of 510°C was used as the magnetic powder. Phenol resin was used as the binder resin. The volume ratio of each low-melting glass to the magnetic powder was 2.5% by volume, and the volume ratio of the phenol resin to the magnetic powder was 2.5% by volume. The same methods as in experiment 1 were used to produce the dust cores and measure the samples.
[0086] As shown in Table 7, in Example 7-1, in which phosphate-based glass was used as the low-melting point glass, and Example 7-2, in which tin-phosphate-based glass was used, the iron loss values were 900 and 1600, respectively, and the proportions of the binder layer of 20 nm or less were 0.92% and 3.6%, respectively, which were good values.
[0087] On the other hand, in Comparative Example 7-1, in which bismuth oxide glass was used as the low-melting point glass, Comparative Example 7-2, in which borosilicate glass was used, and Comparative Example 7-3, in which barium silicate glass was used, the iron loss value was greater than 2500, and the proportion of the binder layer of 20 nm or less was greater than 6%.
[0088] [Table 7]
[0089] FIG. 11 is a graph plotting the iron loss and the ratio of the binder layer of 20 nm or less of the samples with the same binder amount and magnetic powder particle size in the above experiments 1 to 7. In the graph shown in FIG. 11, the binder amount of the sample is 2.5 volume % of low melting point glass and 2.5 volume % of resin material relative to the magnetic powder, and the particle size of the magnetic powder is 9 μm. As shown in the graph of FIG. 11, the iron loss tends to increase as the ratio of the binder layer of 20 nm or less increases. In the present invention, the iron loss can be made 2500 or less by setting the ratio of the binder layer of 20 nm or less to 6% (excluding 0), and this range is the range of the embodiment.
[0090] While the present invention has been described above with reference to the above-described embodiment, the present invention is not limited to the configuration of the above-described embodiment, and naturally includes various modifications, alterations, and combinations that may be made by a person skilled in the art within the scope of the invention as defined in the claims of the present application. [Explanation of symbols]
[0091] 1 Inductor 10_1, 10_2 Powder magnetic core 13 Coil 20 Granulated magnetic powder 21 Magnetic powder 22 Binder layer 25 Intermediate molding 31 Low-melting glass 32 Resin materials
Claims
1. A powder magnetic core in which magnetic powder is bound via a binder layer, The ratio of binder layers having a thickness of 20 nm or less among the binder layers present between the magnetic powder particles is 6% or less (not including 0); Powder magnetic core.
2. 2. The dust core according to claim 1, wherein a ratio of binder layers present between the magnetic powder particles and having a thickness of 20 nm or less is 3.3% or less.
3. The magnetic powder is a soft magnetic powder containing an iron element, The particle size of the magnetic powder is 2 μm or more and 25 μm or less. The dust core according to claim 1 or 2.
4. 4. The dust core of claim 3, wherein the magnetic powder is a metallic glass or a nanocrystalline powder.
5. The powder magnetic core according to any one of claims 1 to 4, wherein the binder layer contains a low-melting point glass and a resin material.
6. 6. The powder magnetic core according to claim 5, wherein a total amount of the low-melting point glass and the resin material is less than 10% by volume relative to the magnetic powder.
7. 7. The powder magnetic core according to claim 6, wherein a volume ratio of the low-melting glass to the magnetic powder is 0.5 volume % or more and 6 volume % or less.
8. 8. The powder magnetic core according to claim 6, wherein a volume ratio of the resin material to the magnetic powder is 0.5 volume % or more and 9 volume % or less.
9. The powder magnetic core according to any one of claims 5 to 8, wherein the low melting point glass is a phosphate-based or tin-phosphate-based glass.
10. The powder magnetic core according to any one of claims 5 to 9, wherein the resin material is at least one selected from the group consisting of a phenolic resin, a polyimide resin, an epoxy resin, and an acrylic resin.
11. The iron loss of the powder magnetic core is 2500 kW / m 3 The powder magnetic core according to any one of claims 1 to 10, wherein:
12. 12. The powder magnetic core according to claim 1, wherein, when the vertical length of the powder magnetic core is longer than 3.5 mm, the distance between the molding dies that sandwich the powder magnetic core in a horizontal cross section of the powder magnetic core is 3.5 mm or less in a direction approximately perpendicular to a direction in which a part that takes the longest time for heat to be transferred to the inside of the powder magnetic core when the powder magnetic core is hot-molded.
13. The powder magnetic core according to any one of claims 1 to 11, wherein the powder magnetic core has a length in the vertical direction of 3.5 mm or less.
14. The powder magnetic core according to any one of claims 1 to 11, wherein the binder layer has a median thickness of 85 nm or less.
15. An inductor comprising the powder magnetic core according to any one of claims 1 to 14 and a coil.
Citation Information
Patent Citations
Powder magnetic core for reactor
CN105051839A
Production of amorphous soft magnetic alloy powder molded body
JP1999256202A
Dust core and its manufacturing method
JP2002246219A
Soft magnetic material and powder magnetic core
JP2006202956A
Mixed powder for dust core, and method of manufacturing dust core using mixed the powder
JP2010225673A