Method for producing layered object, method for producing base material, and base material

A multilayer protective film formed with varying aqueous solutions on glass substrates addresses the issue of foreign substance adhesion, enhancing adhesiveness and releasability, ensuring effective protection and easy removal.

JP2024144785AInactive Publication Date: 2024-10-15SEKISUI CHEMICAL CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021140357
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-08-30
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The adhesion of foreign substances such as cut cullet to the surface of thin glass substrates used in high-definition liquid crystals poses a significant challenge in manufacturing and transportation, necessitating improved methods to suppress this adhesion.

Method used

A method involving the application of two or more aqueous solutions with different compositions to form a multilayer protective film on the glass substrate, enhancing adhesiveness, protective properties, and releasability, using plasticizers like polyhydric alcohols and polyvinyl alcohol resins to improve film toughness and solubility.

Benefits of technology

The multilayer film effectively reduces the adhesion of foreign matter, ensures easy removal, and maintains the integrity of the glass substrate during handling, while being environmentally friendly and adaptable to various base materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144785000001
    Figure 2024144785000001
Patent Text Reader

Abstract

To provide a method for producing a layered object, a method for producing a base material, and a base material with which it is possible to form a protective film with resistance to the adhesion of foreign substances derived from the base material both in a production line and a transportation line.SOLUTION: The present invention is a method for producing a layered object having a base material and a multi-tiered film, the method comprising a film formation step for forming the multi-tiered film by applying, to the base material, two or more types of aqueous solutions for protective film formation having different compositions.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a laminate, a method for producing a substrate, and a substrate. [Background technology]

[0002] Conventionally, substrates such as plate glass have been widely used for surface layers and substrates of optical display devices, window glass, and the like. In particular, when used as substrates for optical display devices and the like, it is necessary to remove dirt, dust, and the like from the surface of the substrate. For example, a clean state is achieved by washing the substrate in advance with a strong alkaline aqueous solution or treating the substrate at high temperatures to burn off and wash away surface contaminants. In response to this, for example, Patent Document 1 describes the use of polyvinyl alcohol having an average degree of polymerization of 600 or less and a degree of saponification of 40 mol % or more as a protective film for a glass substrate. Moreover, Patent Document 2 describes a method of protecting the surface of a glass substrate by covering it with a polyvinyl alcohol-based film. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 10-226537 [Patent Document 2] JP 2006-327881 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, as substrates such as glass for high definition liquid crystal displays become thinner, the management standards for surface adhesion foreign matter have become significantly stricter. In particular, adhesion of foreign matter such as cut cullet of the substrate to the substrate surface has become a problem in the substrate manufacturing and transport lines.

[0005] An object of the present invention is to provide a method for producing a laminate capable of forming a protective coating that can suppress adhesion of foreign matter in a production line or a transport line, a method for producing a substrate, and a substrate. [Means for solving the problem]

[0006] The present invention is a method for producing a laminate having a substrate and a multi-layer coating, which includes a coating formation step of applying two or more aqueous solutions for forming protective coatings, each having a different composition, to the substrate to form a multi-layer coating. The present invention will be described in detail below.

[0007] As a result of extensive research, the inventors discovered that by forming a multi-layer coating by applying two or more aqueous solutions for forming protective coatings having different compositions, it is possible to form a protective coating that is resistant to adhesion of foreign matter originating from the substrate in production lines and transportation lines, and thus completed the present invention.

[0008] The method for producing a laminate of the present invention includes a coating formation step in which two or more types of aqueous protective coating solutions having different compositions are applied to a substrate to form a multilayer coating. This makes it possible to adjust at least one property selected from the group consisting of adhesiveness, protectiveness, and releasability of the multilayer coating.

[0009] In the above-mentioned film-forming step, it is preferable to continuously apply two or more types of aqueous solutions for forming protective films having different compositions, which can increase the adhesion between the films and at the same time form a multi-layer film that is excellent in peelability from the substrate. In addition, when the coating is performed successively, examples of the method include a method in which a first aqueous solution for forming a protective coating is applied, and then a second aqueous solution for forming a protective coating is applied, and a method in which a first aqueous solution for forming a protective coating is applied, and then an aqueous solution for forming a protective coating is applied two or more times. In this specification, the second aqueous solution for forming a protective film or any of the aqueous solutions for forming a protective film that are applied second or thereafter is referred to as "any of the multiple aqueous solutions for forming a protective film that are applied second or thereafter."

[0010] The first applied aqueous solution for forming a protective film preferably contains a plasticizer and water. The first applied aqueous solution for forming a protective film contains a plasticizer, which can improve the toughness of the protective film. The first applied aqueous solution for forming a protective film contains a plasticizer, which can improve the solubility of the protective film in water. The first applied aqueous solution for forming a protective film contains a plasticizer, which can improve the peelability of the protective film from the substrate.

[0011] The plasticizer is not particularly limited, and examples thereof include polyhydric alcohols, polyethers, phenol derivatives, amide compounds, etc. Also included are compounds in which ethylene oxide is added to polyhydric alcohols. These may be used alone or in combination of two or more.

[0012] Examples of the polyhydric alcohol include glycerin, diglycerin, diethylene glycol, trimethylolpropane, triethylene glycol, dipropylene glycol, and propylene glycol. Examples of the polyether include polyethylene glycol and polypropylene glycol. Examples of the phenol derivative include bisphenol A and bisphenol S. Examples of the amide compound include N-methylpyrrolidone. Among these, it is more preferable to use at least one selected from the group consisting of glycerin, diglycerin, diethylene glycol, trimethylolpropane, triethylene glycol, propylene glycol, dipropylene glycol, polyethylene glycol, and polypropylene glycol, it is even more preferable to use at least one selected from the group consisting of glycerin and diglycerin, and it is even more preferable to use diglycerin.

[0013] The first applied aqueous solution for forming a protective film preferably has a plasticizer content of 0.1 to 80% by weight. When the plasticizer content is within the above range, the hydrophilicity of the substrate surface can be controlled, the film can be formed uniformly, and the adhesive strength of the protective film to the glass can be suppressed. The lower limit of the plasticizer content is more preferably 0.5% by weight, and the upper limit is more preferably 70% by weight. The lower limit is even more preferably 1% by weight, and the upper limit is even more preferably 60% by weight. The lower limit is even more preferably 1.5% by weight, and the upper limit is even more preferably 50% by weight. The lower limit is particularly preferably 2% by weight, and the upper limit is especially preferably 40% by weight. The lower limit is especially preferably 2.5% by weight, and the upper limit is especially preferably 30% by weight.

[0014] Furthermore, when the first aqueous solution for forming a protective film contains a polyvinyl alcohol resin, the plasticizer content of the first aqueous solution for forming a protective film is preferably greater than the plasticizer content of any of the second or subsequent aqueous solutions for forming a protective film. More preferably, the plasticizer content of the first aqueous solution for forming a protective film is greater than the plasticizer content of any of the second or subsequent aqueous solutions for forming a protective film. The difference in plasticizer content between the first applied aqueous solution for forming a protective film and the second or subsequent applied aqueous solutions for forming a protective film is preferably 0.1 to 80% by weight. A more preferred lower limit is 0.5% by weight, and a more preferred upper limit is 70% by weight. A more preferred lower limit is 1% by weight, and a more preferred upper limit is 60% by weight. A more preferred lower limit is 1.5% by weight, and a more preferred upper limit is 50% by weight. An especially preferred lower limit is 2% by weight, and a more preferred upper limit is 40% by weight. An especially preferred lower limit is 2.5% by weight, and a more preferred upper limit is 30% by weight.

[0015] The first applied aqueous solution for forming a protective film preferably contains 1 part by weight or more and 1000 parts by weight or less of the plasticizer with respect to 100 parts by weight of polyvinyl alcohol resin. When the content of the plasticizer is within the above range, the adhesive strength of the protective film to the glass can be suppressed. The lower limit of the plasticizer content is more preferably 3 parts by weight, and the upper limit is more preferably 750 parts by weight. The lower limit is even more preferably 5 parts by weight, and the upper limit is even more preferably 500 parts by weight. The lower limit is even more preferably 10% by weight, and the upper limit is even more preferably 250% by weight. The lower limit is particularly preferably 15% by weight, and the upper limit is especially preferably 100% by weight. The lower limit is especially preferably 5% by weight, and the upper limit is especially preferably 75% by weight.

[0016] The first aqueous solution for forming a protective film to be applied preferably contains water. The water is not particularly limited, and examples thereof include ion-exchanged water, pure water, etc. These may be used alone or in combination of two or more kinds.

[0017] The first applied aqueous solution for forming a protective film preferably has a water content of 20 to 99.9% by weight. When the water content is within the above range, a uniform film can be formed. A more preferred lower limit of the water content is 30% by weight, and a more preferred upper limit is 99.5% by weight. A still more preferred lower limit is 40% by weight, and a still more preferred upper limit is 99.0% by weight. A still more preferred lower limit is 50% by weight, and a still more preferred upper limit is 98.5% by weight. An especially preferred lower limit is 60% by weight, and a particularly preferred upper limit is 98.0% by weight. An especially preferred lower limit is 70% by weight, and a particularly preferred upper limit is 98.0% by weight.

[0018] The first applied aqueous solution for forming a protective film may contain a water-soluble resin such as a polyvinyl alcohol resin. In a preferred embodiment of the present invention, the first applied aqueous solution for forming a protective film does not contain a polyvinyl alcohol resin, or the content of polyvinyl alcohol resin in the first applied aqueous solution for forming a protective film is preferably less than the content of polyvinyl alcohol resin in the second or subsequent applied aqueous solutions for forming a protective film. When the first aqueous solution for forming a protective film does not contain a polyvinyl alcohol resin, or when the polyvinyl alcohol resin content of the first aqueous solution for forming a protective film is less than the polyvinyl alcohol resin content of the second or subsequent aqueous solutions for forming a protective film, the peelability of the protective film from the substrate layer can be further improved. By using the polyvinyl alcohol resin, it is possible to improve the strength of the protective film and also to impart biodegradability in soil.

[0019] The saponification degree of the polyvinyl alcohol resin is preferably 50 mol % at the lower limit and 99.5 mol % at the upper limit. By setting the saponification degree within the above range, a uniform aqueous solution can be prepared, and an aqueous solution capable of forming a membrane can be prepared. The lower limit of the saponification degree is more preferably 60 mol%, even more preferably 70 mol%, and particularly preferably 80 mol%. The upper limit is more preferably 99 mol%, even more preferably 95 mol%, and particularly preferably 90 mol%. From the viewpoint of aqueous solution formation and storage stability of the aqueous solution at room temperature, the degree of saponification of the polyvinyl alcohol resin is preferably not 98 mol % or more but 98 mol % or less, and particularly preferably a partially saponified product of 90 mol % or less. The saponification degree is measured in accordance with JIS K 6726. The saponification degree indicates the average ratio of units that are actually saponified into vinyl alcohol units to units that are converted into vinyl alcohol units by saponification.

[0020] The degree of polymerization of the polyvinyl alcohol resin is not particularly limited, but the preferred lower limit is 100 and the preferred upper limit is 2500. The more preferred lower limit is 200 and the more preferred upper limit is 1800. The even more preferred lower limit is 250 and the even more preferred upper limit is 1300, the particularly preferred lower limit is 300 and the particularly preferred upper limit is 1000. Within the above ranges, both the film strength and the film formability can be achieved at a high level. The above degree of polymerization is measured in accordance with JIS K6726.

[0021] The polyvinyl alcohol resin may be a mixture of two or more resins having different degrees of saponification, polymerization, etc., or may be a mixture of a modified resin and an unmodified resin.

[0022] The polyvinyl alcohol resin is obtained by polymerizing a vinyl ester to obtain a polymer, and then saponifying the polymer, i.e., hydrolyzing the polymer, according to a conventionally known method. In general, an alkali or an acid is used for saponification. For saponification, an alkali is preferably used. As the polyvinyl alcohol, only one type may be used, or two or more types may be used in combination.

[0023] Examples of the vinyl ester include vinyl acetate, vinyl formate, vinyl propionate, vinyl butyrate, vinyl pivalate, vinyl versatate, vinyl laurate, vinyl stearate, and vinyl benzoate. The polymer obtained by polymerizing the vinyl ester is preferably a polyvinyl ester, since the degree of saponification can be easily controlled within a suitable range.

[0024] The polymerization method for the vinyl ester is not particularly limited, and examples of the polymerization method include solution polymerization, bulk polymerization, and suspension polymerization.

[0025] Examples of the polymerization catalyst used in polymerizing the vinyl ester include 2-ethylhexyl peroxydicarbonate (TrigonoxEHP manufactured by Tianjin McEIT Co., Ltd.), 2,2'-azobisisobutyronitrile (AIBN), t-butyl peroxyneodecanoate, bis(4-t-butylcyclohexyl)peroxydicarbonate, di-n-propyl peroxydicarbonate, di-n-butyl peroxydicarbonate, di-cetyl peroxydicarbonate, and di-s-butyl peroxydicarbonate. Only one of the polymerization catalysts may be used, or two or more of them may be used in combination.

[0026] The polyvinyl alcohol resin may include a modified polyvinyl alcohol resin. The modified polyvinyl alcohol resin may be a copolymer of the vinyl ester and another monomer, or may be a modified polyvinyl alcohol resin. Examples of the modified polyvinyl alcohol resin include acetoacetyl-modified polyvinyl alcohol, carboxyl-modified polyvinyl alcohol, sulfonic acid-modified polyvinyl alcohol, olefin-modified polyvinyl alcohol, nitrile-modified polyvinyl alcohol, amide-modified polyvinyl alcohol, pyrrolidone-modified polyvinyl alcohol, silicon-containing modified polyvinyl alcohol, and graft polymers of polyvinyl alcohol and copolymers of (acrylamide, vinylpyrrolidone, acrylonitrile).

[0027] Examples of the other monomers, i.e., comonomers to be copolymerized, include olefins, (meth)acrylic acid and its salts, (meth)acrylic acid esters, (meth)acrylamide derivatives, N-vinylamides, vinyl ethers, nitriles, vinyl halides, allyl compounds, maleic acid and its salts, maleic acid esters, itaconic acid and its salts, itaconic acid esters, vinylsilyl compounds, polyvinylpyrrolidone, and isopropenyl acetate, etc. Only one type of the other monomers may be used, or two or more types may be used in combination.

[0028] Examples of the olefins include ethylene, propylene, 1-butene, and isobutene. Examples of the (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. Examples of the (meth)acrylamide derivatives include acrylamide, n-methylacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, and (meth)acrylamidopropanesulfonic acid and its salts. Examples of the N-vinylamides include N-vinylpyrrolidone. Examples of the vinyl ethers include methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, i-propyl vinyl ether, and n-butyl vinyl ether. Examples of the nitriles include (meth)acrylonitrile. Examples of the vinyl halides include vinyl chloride and vinylidene chloride. Examples of the allyl compounds include allyl acetate and allyl chloride. The vinylsilyl compound includes, for example, vinyltrimethoxysilane.

[0029] The upper limit of the modification amount (proportion of modified structural units) in the modified polyvinyl alcohol resin is preferably 25 mol%, more preferably 20 mol%. An even more preferable upper limit is 15 mol%. Furthermore, a preferable lower limit of the modification amount is 2 mol%. By keeping it within the above range, it is possible to achieve both high levels of film properties and water solubility.

[0030] When the first aqueous solution for forming a protective film to be applied contains a polyvinyl alcohol resin, the content of the polyvinyl alcohol resin is preferably 0.1 to 30% by weight. By making the content 0.1% by weight or more, a film with a high coverage can be formed (when the substrate is at a high temperature, water vaporizes, so that the applied aqueous solution breaks bubbles, which makes it difficult to form a film). By making the content 30% by weight or less, a uniform film can be formed (if the concentration is too high, particularly those with a high degree of saponification will partially gel at room temperature, making it impossible to apply uniformly). A more preferable lower limit of the content is 1% by weight, and a more preferable upper limit is 20% by weight. An even more preferable lower limit is 2% by weight, and an even more preferable upper limit is 15% by weight. The polyvinyl alcohol resin content of the first applied aqueous solution for forming a protective film is preferably less than the polyvinyl alcohol resin content of the second or subsequent applied aqueous solution for forming a protective film, or the polyvinyl alcohol resin content of either of the second or subsequent applied aqueous solutions for forming a protective film, in which case the adhesion, protectiveness, and peelability of the film can be further improved. The difference in polyvinyl alcohol resin content between the second or subsequent applied aqueous solution for forming a protective film and the first applied aqueous solution for forming a protective film is preferably 0.1 to 50% by weight.

[0031] The above-mentioned aqueous solution for forming a protective film to be applied first may contain various known additives within the range that does not impair the effects of the present invention. Examples of the additives include surfactants, antioxidants, antiaging agents, UV absorbers, titanium coupling agents, leveling agents, thixotropic agents, antiskinning agents, thickeners, diluents, reactive diluents, crosslinking agents, fillers, colorants (pigments, dyes), preservatives, and antifungal agents. It is preferable that the first applied aqueous solution for forming a protective film further contains an antifungal agent. Examples of the antifungal agent include alcohol-based antifungal agents, aldehyde-based antifungal agents, thiazoline-based antifungal agents, imidazole-based antifungal agents, ester-based antifungal agents, chlorine-based antifungal agents, peroxide-based antifungal agents, carboxylic acid-based antifungal agents, carbamate-based antifungal agents, sulfamide-based antifungal agents, quaternary ammonium salt-based antifungal agents, pyridine-based antifungal agents, phenol-based antifungal agents, iodine-based antifungal agents, and triazole-based antifungal agents.

[0032] The first aqueous protective film-forming solution preferably has a viscosity of 0.1 mPa·s to 1 Pa·s as measured with a rotational viscometer (e.g., TVC-10, manufactured by Toki Sangyo Co., Ltd.) within the above range, allowing the formation of a uniform film. The lower limit of the viscosity is more preferably 0.5 mPa·s and the upper limit is more preferably 0.5 Pa·s. The lower limit is still more preferably 1 mPa·s and the upper limit is still more preferably 0.4 Pa·s. The lower limit is still more preferably 1.5 mPa·s and the upper limit is still more preferably 0.3 Pa·s. The above viscosity was measured at 23°C.

[0033] The first applied aqueous solution for forming a protective film preferably has a contact angle with a glass substrate (TEMPAX Float manufactured by SCHOTT) of 20° to 70° at a temperature of 23° C. and a humidity of 60% R / H. When the contact angle is within the above range, a uniform film is easily formed on the glass substrate. The lower limit of the contact angle is more preferably 25°, and the upper limit thereof is more preferably 60°, and the further more preferably 30°, and the further more preferably 50°. The contact angle can be measured by a contact angle meter. For example, the contact angle meter is DMo-502 (Kyowa Interface Science Co., Ltd., analysis software FAMAS), the contact angle measurement substrate is glass (Tempax) 0.5 mm, and the measurement method is the θ / 2 method (A half-angle method).

[0034] The temperature of the aqueous solution for forming a protective film when applied to the substrate is preferably 0° C. or higher, more preferably 10° C. or higher, even more preferably 20° C. or higher, even more preferably 40° C. or higher, particularly preferably 60° C. or higher, and is preferably 100° C. or lower, more preferably 95° C. or lower, even more preferably 90° C. or lower, even more preferably 85° C. or lower, particularly preferably 80° C. or lower. When the temperature of the aqueous solution for forming a protective film is within the above range, the protective film is formed uniformly and quickly, and processability is improved.

[0035] The method for producing the above-mentioned first aqueous solution for forming the protective film to be applied is not particularly limited, and examples thereof include a method in which, in addition to a plasticizer and water, a polyvinyl alcohol resin is mixed, if necessary, by a known method.

[0036] In the step of first applying the aqueous solution for forming a protective film to the substrate, examples of the application method include roll coating, dip coating, spin coating, fountain coating, spray coating, etc. Among these, spray coating is preferred from the viewpoints of application efficiency and uniformity of the film.

[0037] In the coating formation step, the temperature of the substrate when the first aqueous solution for forming a protective coating is applied is preferably 0° C. or higher and 400° C. or lower. Within this range, a foam layer can be produced when the solution is applied to a high-temperature substrate, and a foam can be produced by heating and drying after application at a low temperature. A more preferred lower limit for the above temperature is 15°C, a more preferred upper limit is 380°C, an even more preferred lower limit is 40°C, and an even more preferred upper limit is 360°C, an even more preferred lower limit is 75°C, and an even more preferred upper limit is 340°C, an especially preferred lower limit is 100°C, an especially preferred upper limit is 320°C, an especially more preferred lower limit is 150°C, and an especially more preferred upper limit is 300°C. If the substrate temperature is 400°C or lower, the bubbles break and the adhesion of foreign matter such as cut cullet to the substrate surface can be suppressed, and the film and substrate are bonded appropriately, making them easy to remove. If the substrate temperature is 0°C or higher, a foam can be easily formed without post-heating.

[0038] The method for adjusting the temperature of the substrate may be, for example, a method of applying the coating in the step of slowly cooling molten glass when glass is formed using a fusion method, or a method of heating the glass when solidified glass is used. The above temperature refers to the temperature of the substrate surface at the time of application. In the above-mentioned film forming step, the state of the substrate is not particularly limited, and includes, for example, the state before the glass is molded and solidified, as well as the state after the glass has solidified. Furthermore, the above-mentioned substrate may be polished or surface-treated as necessary.

[0039] The preferred lower limit of the thickness of the first coating solution for forming a protective film is 0.1 μm, and the preferred upper limit is 100 μm. If the foam thickness is within the above range, the foam layer can be peeled off or dissolved in water. The more preferred lower limit of the thickness of the first coating solution for forming a protective film is 1 μm, and the more preferred upper limit is 80 μm. The more preferred lower limit is 1.5 μm, the more preferred upper limit is 60 μm, the more preferred lower limit is 2.0 μm, the more preferred upper limit is 40 μm, the particularly preferred lower limit is 2.5 μm, the particularly preferred upper limit is 30 μm, the particularly preferred upper limit is 3 μm, and the particularly preferred upper limit is 25 μm.

[0040] In the above-mentioned film forming process, it is preferable to use a method in which a first aqueous solution for forming a protective film is applied and then a second aqueous solution for forming a protective film is applied, or a method in which a first aqueous solution for forming a protective film is applied and then an aqueous solution for forming a protective film is applied two or more times. By applying the first aqueous solution for forming a protective film as described above, followed by applying a second or subsequent aqueous solution for forming a protective film, it is possible to further improve the prevention of blocking when laminate substrates with protective films are stacked, and also to improve the peelability.

[0041] It is preferable that any one of the plurality of aqueous solutions for forming a protective film to be applied second or thereafter contains a polyvinyl alcohol resin, a plasticizer, and water. The polyvinyl alcohol resin, plasticizer, and water constituting any one of the plurality of aqueous solutions for forming a protective film to be applied second or thereafter may be the same as those in the aqueous solution for forming a protective film to be applied first.

[0042] The content of the polyvinyl alcohol resin in any of the multiple aqueous solutions for forming protective films to be applied second or thereafter is preferably 0.1 to 50% by weight. By setting the content to 0.1% by weight or more, a film with a high coverage rate can be formed, and by setting the content to 50% by weight or less, a uniform film can be formed by uniform application. A more preferred lower limit of the content is 1% by weight, and a more preferred upper limit is 40% by weight. An even more preferred lower limit is 3% by weight, an even more preferred upper limit is 35% by weight, an even more preferred lower limit is 5% by weight, an even more preferred upper limit is 30% by weight, an especially preferred lower limit is 8% by weight, and an especially preferred upper limit is 25% by weight.

[0043] It is preferable that any of the multiple protective film forming aqueous solutions to be applied second or thereafter has a plasticizer content of 0.1 to 50% by weight. When the plasticizer content is within the above range, the hydrophilicity of the glass surface can be controlled and the film can be formed uniformly. A more preferable lower limit of the plasticizer content is 0.5% by weight, and a more preferable upper limit is 40% by weight. A more preferred lower limit is 1.0% by weight, and a more preferred upper limit is 30% by weight. A more preferred lower limit is 1.5% by weight, and a more preferred upper limit is 25.0% by weight. A particularly preferred lower limit is 3.0% by weight, and a particularly preferred upper limit is 20.0% by weight. A particularly preferred lower limit is 5.0% by weight, and a particularly preferred upper limit is 15.0% by weight.

[0044] It is preferable that any of the plurality of aqueous solutions for forming protective films to be applied second or thereafter contains 0.25 parts by weight or more and 50,000 parts by weight or less of the plasticizer per 100 parts by weight of polyvinyl alcohol resin. When the content of the plasticizer is within the above range, toughness can be imparted to the film. A more preferred lower limit of the plasticizer content is 1.25 parts by weight, and a more preferred upper limit is 40,000 parts by weight. A more preferred lower limit is 2.5 parts by weight, and a more preferred upper limit is 30,000 parts by weight. A more preferred lower limit is 3.75 parts by weight, and a more preferred upper limit is 25,000 parts by weight. A particularly preferred lower limit is 7.5 parts by weight, and a particularly preferred upper limit is 20,000 parts by weight. A particularly preferred lower limit is 12.5 parts by weight, and a particularly preferred upper limit is 15,000 parts by weight.

[0045] It is preferable that any of the multiple aqueous solutions for forming a protective film to be applied second or thereafter has a water content of 10 to 99.8% by weight. When the water content is within the above range, the solution can be applied uniformly to the surface of the substrate to form a homogeneous film. If the water content in the aqueous solution is too low, stringing problems may occur during spray application. A more preferable lower limit of the water content is 20% by weight, and a more preferable upper limit is 99.0% by weight. A more preferred lower limit is 30% by weight, and a more preferred upper limit is 97.0% by weight. A more preferred lower limit is 40% by weight, and a more preferred upper limit is 95.0% by weight. An even more preferred lower limit is 42.5% by weight, and a more preferred upper limit is 92.5% by weight. An even more preferred lower limit is 45.0% by weight, and a more preferred upper limit is 90.0% by weight. The total content of the components in the first applied aqueous solution for forming a protective film and the second or subsequent applied aqueous solutions for forming protective films is 100% by weight.

[0046] It is preferable that any of the multiple protective film forming aqueous solutions to be applied second or thereafter has a viscosity of 0.1 mPa s or more and 3.0 Pa s or less when measured with a rotational viscometer (e.g., TVC-10, manufactured by Toki Sangyo Co., Ltd.) If it is within the above range, a uniform film with a high coverage can be formed. A more preferred lower limit of the viscosity is 0.5 mPa·s, and a more preferred upper limit is 1.8 Pa·s. An even more preferred lower limit is 1.5 mPa·s, and a still more preferred upper limit is 1.0 Pa·s. An even more preferred lower limit is 1.0 mPa·s, and a still more preferred upper limit is 0.7 Pa·s. An especially preferred lower limit is 50.0 mPa·s, and a still more preferred upper limit is 0.5 Pa·s. The above viscosity was measured at 23°C.

[0047] It is preferable that any of the multiple protective film forming aqueous solutions to be applied second or thereafter has a contact angle with a glass substrate (e.g., TEMPAX Float manufactured by SCHOTT) of 10° to 75° at a temperature of 23° C. and a humidity of 60% RH. If it is within the above range, a homogeneous film is easily formed on the glass substrate. The lower limit of the contact angle is more preferably 20°, and the upper limit is more preferably 70°. The lower limit is still more preferably 25°, and the upper limit is still more preferably 65°, and the lower limit is still more preferably 30°, and the upper limit is still more preferably 60°. The contact angle can be measured by a contact angle meter. For example, the contact angle meter is DMo-502 (Kyowa Interface Science Co., Ltd., analysis software FAMAS), the contact angle measurement substrate is glass (Tempax) 0.5 mm, and the measurement method is the θ / 2 method (A half-angle method).

[0048] The method for producing the aqueous solutions for forming the second or subsequent protective coatings is not particularly limited, and may be, for example, a method in which a polyvinyl alcohol resin, a plasticizer, and water are mixed by a known method.

[0049] The step of applying the second or subsequent aqueous solutions for forming a protective film can be performed using a method similar to the method of applying the first aqueous solution for forming a protective film. The step of applying the second or subsequent aqueous solutions for forming a protective coating may be performed on only one side or on both sides of the substrate.

[0050] After the above-mentioned film forming step, a drying step (secondary drying) may be performed. This makes it possible to form a multi-layer film regardless of the substrate temperature. The drying temperature in the above-mentioned secondary drying is preferably 50°C or higher and 450°C or lower.

[0051] The method for producing a laminate of the present invention includes a base forming step of forming a base, and it is preferable to perform the base forming step and the film forming step consecutively. In this case, adhesion of foreign matter to the surface of the base and damage to the surface of the base can be suppressed. Examples of the substrate include glass, plastic substrates (organic polymer substrates), and metal substrates. Examples of the glass include soda-lime glass, alkali-free glass, borosilicate glass, fused silica, etc. The present invention can be particularly suitably used for thin glass for high-definition liquid crystal displays. The plastic substrate may be a polycarbonate plate or a poly(meth)acrylic resin plate. The poly(meth)acrylic resin plate may be a polymethyl(meth)acrylate plate. Examples of the metal substrate include substrates made of metals such as copper, iron, tin, aluminum, silver, stainless steel, brass, nickel, titanium, and alloys thereof. Specific examples include steel plates, copper plates, aluminum plates, and aluminum-plated steel plates.

[0052] As the substrate molding step, a known method can be used. When the substrate is glass, methods for forming the glass include the slot downdraw method, the fusion method, the float method, etc. Among these, it is preferable to use the fusion method. The fusion method is a method in which molten glass raw material is introduced into a long, thin trough-shaped outlet, overflowed on both sides along the longitudinal direction, and allowed to flow downward. The molten glass that has flowed down rejoins the bottom of the trough and continues to flow downward while being gradually cooled and solidified to produce glass. In the present invention, even when a commercially available glass, plastic, metal or other substrate is used, the substrate is considered to have been subjected to the step of molding the substrate.

[0053] According to the method for producing a laminate of the present invention, a laminate having a substrate and a single-layer coating or a substrate and a multi-layer coating can be obtained.

[0054] The multilayer coating preferably has a surface roughness Sa (arithmetic mean height as defined in ISO 25178) of 0.1 μm or more on the main surface opposite the substrate. There is no particular upper limit, but 30 μm is a practical upper limit. Within the above range, the self-adhesive force can be reduced. The surface roughness Sa is preferably 0.2 μm or more, more preferably 0.3 μm or more, even more preferably 0.4 μm or more, and particularly preferably 0.5 μm or more. Moreover, the multilayer coating formed in the present invention preferably has a surface roughness Sz (maximum height as defined in ISO 25178) of 10 μm or more on the main surface opposite the substrate. There is no particular upper limit, but 300 μm is a practical upper limit. When the thickness falls within the above range, the substrate can be protected from surface scratches applied to the substrate or damage caused by pressure applied to the substrate. The surface roughness Sz is preferably 20 μm or more, more preferably 30 μm or more, further preferably 40 μm or more, and particularly preferably 50 μm or more. In addition, the surface roughness Sdr (maximum height as defined in ISO 25178) of the main surface opposite the substrate of the multilayer coating is preferably 0.1 or more. There is no particular upper limit, but a practical upper limit is 30. When the surface roughness is within the above range, the substrate can be protected from surface scratches applied to the substrate and damage caused by pressure applied to the substrate, and the thermal insulation of the substrate can be improved. The surface roughness Sdr is more preferably 0.2 or more, further preferably 0.3 or more, even more preferably 0.5 or more, particularly preferably 0.7 or more, and especially preferably 0.9 or more. The surface roughnesses Sa, Sz, and Sdr are calculated in accordance with ISO 25178 by measuring the main surface of the multilayer coating over a range of 1 mm x 1 mm with a laser microscope (e.g., morphological analysis laser microscope, VK-X1050, manufactured by Keyence Corporation). This measurement was performed at 10 random locations, and the average value was used as each value.

[0055] The multilayer coating preferably has a surface roughness Sa (arithmetic mean height as defined in ISO 25178) of 0.05 μm or more on the main surface on the substrate side. There is no particular upper limit, but 15 μm is a practical upper limit. Within the above range, the adhesion of the multi-layer coating to the substrate can be reduced and the peelability can be improved. The surface roughness Sa is more preferably 0.1 μm or more, even more preferably 0.2 μm or more, even more preferably 0.3 μm or more, particularly preferably 0.4 μm or more, and particularly preferably 0.5 μm or more. Moreover, the multilayer coating preferably has a surface roughness Sz (maximum height as defined in ISO 25178) of 8 μm or more on the main surface on the substrate side. There is no particular upper limit, but 240 μm is a practical upper limit. Within the above range, the adhesion of the multi-layer coating to the substrate can be reduced and the peelability can be improved. The surface roughness Sz is more preferably 16 μm or more, even more preferably 24 μm or more, even more preferably 32 μm or more, particularly preferably 40 μm or more, and particularly preferably 48 μm or more. In addition, the multilayer coating preferably has a surface roughness Sdr (maximum height as defined in ISO 25178) of 0.05 or more on the substrate-side main surface. There is no particular upper limit, but a practical upper limit is 15. When the surface roughness is within the above range, the substrate can be protected from surface scratches and damage caused by pressure applied to the substrate, and the heat insulation of the substrate can be improved. The surface roughness Sdr is more preferably 0.1 or more, further preferably 0.2 or more, even more preferably 0.3 or more, particularly preferably 0.4 or more, and especially preferably 0.5 or more. The surface roughnesses Sa, Sz, and Sdr are calculated in accordance with ISO 25178 by measuring the area of ​​1 mm x 1 mm on the substrate-side main surface of the prepared multilayer coating with a laser microscope (e.g., morphological analysis laser microscope, VK-X1050, manufactured by Keyence Corporation). This was measured at 10 random locations, and the average value was used as each value.

[0056] The multilayer coating has a preferred lower limit of 0.05 μm and a preferred upper limit of 280 μm for the average bubble diameter (foam diameter). By having the average bubble diameter within this range, the protection of the substrate surface from scratches and the like can be improved. The more preferred lower limit of the average bubble diameter is 0.5 μm and the more preferred upper limit is 225 μm. A more preferable lower limit is 1.0 μm, a more preferable upper limit is 180 μm, a still more preferable lower limit is 1.5 μm, a still more preferable upper limit is 135 μm, a particularly preferable lower limit is 2.0 μm, a particularly preferable upper limit is 108 μm, a particularly more preferable lower limit is 2.5 μm, and a particularly preferable upper limit is 90 μm. The average bubble diameter can be measured by observing the bubble walls and voids in a cross-sectional photograph of the bubbles with a laser microscope (e.g., morphological analysis laser microscope, VK-X1050, manufactured by Keyence Corporation) and measuring the size of the voids.

[0057] The preferred lower limit of the thickness of the multi-layer coating is 1.0 μm, and the preferred upper limit is 300 μm. If the foam thickness is within the above range, the foam layer can be peeled off and dissolved in water. The more preferred lower limit of the thickness of the multi-layer coating is 2.0 μm, and the more preferred upper limit is 250 μm. A more preferable lower limit is 4.0 μm, a more preferable upper limit is 200 μm, a still more preferable lower limit is 6.0 μm, a still more preferable upper limit is 150 μm, a particularly preferable lower limit is 8.0 μm, a particularly preferable upper limit is 120 μm, a particularly more preferable lower limit is 10.0 μm, and a particularly preferable upper limit is 100 μm. The thickness of the film produced can be measured using a constant pressure thickness measuring instrument conforming to JIS K6783 (e.g., PG-02J, manufactured by Teclock Corporation).

[0058] In the laminate of the present invention, the peel strength between the multilayer coating and the substrate is preferably 2N or less in a 180° peel strength test. The peel strength of 2N or less allows the multilayer coating to be peeled from the substrate. The preferred upper limit of the peel strength is 1.5N, and the preferred lower limit is 0.01N, although not particularly limited. The 180° peel strength can be measured by a method in accordance with ISO29862:2007 or JIS Z 0237:2009. Similarly, the 90° peel strength can be measured using a method conforming to ISO29862:2007 or JIS Z 0237:2009.

[0059] The present invention also includes a method for producing a laminate of the present invention, a method for producing a substrate comprising a removal step of removing the multilayer coating from the substrate, and a substrate obtained by the method for producing a substrate of the present invention. The removing step may be carried out by manually or mechanically lifting and removing the end of the multi-layer coating, or by spraying air or the like onto the end of the multi-layer coating. Alternatively, a method of dissolving and removing the multi-layer film using a solvent such as water can also be used. Effect of the Invention

[0060] According to the present invention, it is possible to provide a method for producing a laminate, a method for producing a substrate, and a substrate capable of forming a protective coating that is resistant to adhesion of foreign matter originating from the substrate in a production line or a transport line. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0061] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0062] Example 1 (Preparation of aqueous solution for forming protective film [for inner layer, outer layer]) 100 parts by weight of unmodified polyvinyl alcohol (SELVOL 203 manufactured by Sekisui Chemical Co., Ltd., degree of polymerization 300, degree of saponification 88 mol%) and 30 parts by weight of diglycerin as a plasticizer were dissolved and mixed in 370 parts by weight of water to prepare an aqueous solution for forming a protective coating [for the inner layer] with a resin content of 20% by weight and a plasticizer content of 6% by weight. In addition, 100 parts by weight of unmodified polyvinyl alcohol (SELVOL 103 manufactured by Sekisui Chemical Co., Ltd., degree of polymerization 300, degree of saponification 98.4 mol%) and 10 parts by weight of diglycerin as a plasticizer were dissolved and mixed in 890 parts by weight of water to prepare an aqueous solution for forming a protective coating [for the outer layer] with a resin content of 10% by weight and a plasticizer content of 1% by weight.

[0063] (Creation of protective film [glass film]) A glass substrate (manufactured by Corning Incorporated, EagleXG 150 mm×150 mm×0.5 mm) was heated on a hot plate so that the center of the glass substrate reached 300° C. The heated glass substrate was moved to a spray table, and when the center of the glass reached 250°C, the obtained aqueous solution for forming a protective coating [for the inner layer] was sprayed once onto the glass substrate, and then the obtained aqueous solution for forming a protective coating [for the outer layer] was sprayed once on top of that, and then dried for 60 seconds in a batch-type hot air circulating drying oven (set to 150°C), resulting in a laminate in which two glass layers [inner layer, outer layer] were formed on the surface of the glass substrate. The spray gun used to apply the protective coating solution [for the inner layer and outer layer] was AGB50 (manufactured by Asahi Sunac Corporation, aperture 1.0 mmφ, cap HN400A), the paint supply equipment was a pressure pump PT-10DW (manufactured by Anest Iwata Corporation), and the painting robot was EPX-1250 DX100 (manufactured by Yaskawa Electric Corporation).

[0064] Example 2 (Preparation of aqueous solution for forming protective film [for outer layer]) An aqueous solution for forming a protective coating film [for outer layer] was prepared in the same manner as in Example 1 (Preparation of an aqueous solution for forming a protective coating film [for inner layer]), except that 100 parts by weight of unmodified polyvinyl alcohol (SELVOL 203 manufactured by Sekisui Chemical Co., Ltd., polymerization degree 300, saponification degree 88 mol%) was used and no plasticizer was added.

[0065] (Creation of protective film [glass film]) A glass substrate (manufactured by Corning Incorporated, EagleXG 150 mm×150 mm×0.5 mm) was heated on a hot plate so that the center of the glass substrate reached 300° C. The heated glass substrate was moved to a spray table, and when the center of the glass reached 250°C, the aqueous solution for forming a protective coating film [for inner layer] obtained in Example 1 was sprayed once onto the glass substrate, and then the aqueous solution for forming a protective coating film [for outer layer] obtained was sprayed once on top of that, and then dried for 60 seconds in a batch-type hot air circulating drying oven (set at 150°C), resulting in a laminate in which two glass coating layers [inner layer, outer layer] were formed on the surface of the glass substrate. The spray gun used to apply the protective film forming aqueous solution [for inner layer, outer layer] was AGB50 (manufactured by Asahi Sunac Corporation, aperture 1.0 mmφ, cap HN400A), the paint supplying device was a pressure pump PT-10DW (manufactured by Anest Iwata Corporation), and the painting robot was EPX-1250 DX100 (manufactured by Yaskawa Electric Corporation). In the following examples and comparative examples, when spray application was performed, spray application was performed using the same spray gun, paint supplying device, and painting robot as above.

[0066] Example 3 (Preparation of aqueous solution for forming protective film [for inner layer, outer layer]) Without adding unmodified polyvinyl alcohol, 100 parts by weight of diglycerin was dissolved and mixed in 1,900 parts by weight of water as a plasticizer to prepare an aqueous solution for forming a protective film [for the inner layer] with a plasticizer content of 5% by weight. In addition, 100 parts by weight of unmodified polyvinyl alcohol (SELVOL 203 manufactured by Sekisui Chemical Co., Ltd., degree of polymerization 300, degree of saponification 88 mol%) and 15 parts by weight of diglycerin as a plasticizer were dissolved and mixed in 385 parts by weight of water to prepare an aqueous solution for forming a protective coating [for the outer layer] with a resin content of 20% by weight and a plasticizer content of 3% by weight.

[0067] (Creation of protective film [glass film]) A glass substrate (manufactured by Corning Incorporated, EagleXG 150 mm×150 mm×0.5 mm) was heated on a hot plate so that the center of the glass substrate reached 400° C. The heated glass substrate was moved to a spray table, and when the center of the glass reached 350°C, the obtained aqueous solution for forming a protective coating [for inner layer] was sprayed once onto the glass substrate, and then the obtained aqueous solution for forming a protective coating [for outer layer] was sprayed once on top of that, and then dried for 60 seconds in a batch-type hot air circulating drying oven (set to 150°C), resulting in a laminate in which two layers of glass coating [inner layer, outer layer] were formed on the surface of the glass substrate.

[0068] Example 4 An aqueous solution for forming a protective coating film [for outer layer] was prepared in the same manner as in Example 3, except that 100 parts by weight of unmodified polyvinyl alcohol (SELVOL 205, manufactured by Sekisui Chemical Co., Ltd., polymerization degree 500, saponification degree 88 mol%) was used instead of 100 parts by weight of unmodified polyvinyl alcohol (SELVOL 203, manufactured by Sekisui Chemical Co., Ltd., polymerization degree 300, saponification degree 88 mol%), and the amount of plasticizer added, resin content, and plasticizer content were as shown in Table 1. A laminate having two glass layers [inner layer, outer layer] formed on the surface of a glass substrate (Corning EagleXG 150 mm x 150 mm x 0.5 mm) was obtained in the same manner as in Example 3, except that the obtained aqueous solution for forming a protective film [for outer layer] was used.

[0069] Example 5 An aqueous solution for forming a protective coating film [for outer layer] was prepared in the same manner as in Example 3, except that 18 parts by weight of glycerin was used instead of 15 parts by weight of diglycerin as a plasticizer, and the amount of plasticizer added, resin content, and plasticizer content were as shown in Table 1. A laminate having a glass film formed thereon was produced in the same manner as in Example 3, except that the obtained aqueous solution for forming a protective film [for outer layer] was used.

[0070] Example 6 Without adding unmodified polyvinyl alcohol, 100 parts by weight of glycerin was dissolved and mixed in 1,940 parts by weight of water as a plasticizer to prepare an aqueous solution for forming a protective film [for the inner layer] with a plasticizer content of 3% by weight. An aqueous solution for forming a protective coating film [for outer layer] was prepared in the same manner as in Example 3, except that 100 parts by weight of unmodified polyvinyl alcohol (SELVOL 205, manufactured by Sekisui Chemical Co., Ltd., polymerization degree 500, saponification degree 88 mol%) was used instead of 100 parts by weight of unmodified polyvinyl alcohol (SELVOL 203, manufactured by Sekisui Chemical Co., Ltd., polymerization degree 300, saponification degree 88 mol%), 18 parts by weight of glycerin was used instead of 15 parts by weight of diglycerin as a plasticizer, and the amount of plasticizer added, resin content, and plasticizer content were as shown in Table 1. A laminate having a glass film formed thereon was produced in the same manner as in Example 3, except that the obtained aqueous solution for forming a protective film [for inner layer] and aqueous solution for forming a protective film [for outer layer] were used.

[0071] Comparative Example 1 Without using 100 parts by weight of unmodified polyvinyl alcohol (SELVOL 203, manufactured by Sekisui Chemical Co., Ltd., polymerization degree 300, saponification degree 88 mol%), only diglycerin, a plasticizer, was prepared as an aqueous solution as shown in Table 1. A glass substrate (manufactured by Corning Incorporated, EagleXG 150 mm×150 mm×0.5 mm) was heated on a hot plate so that the center of the glass substrate reached 300° C. The heated glass substrate was moved to a spray table, and when the temperature of the center of the glass reached 350°C, the obtained aqueous solution was sprayed once onto the glass substrate and dried for 60 seconds in a batch-type hot air circulating drying oven (set at 150°C) to obtain a laminate in which a glass film was formed on the surface of the glass substrate. The obtained glass film was composed only of diglycerin, a plasticizer, and water.

[0072] Comparative Example 2 An aqueous solution for forming a protective coating film with a plasticizer content of 40% by weight and a laminate on which a glass coating film was formed were prepared in the same manner as in Comparative Example 1, except that only diglycerin, a plasticizer, was prepared as an aqueous solution as shown in Table 1. The coating film was composed only of diglycerin, a plasticizer, and water.

[0073] Comparative Example 3 An aqueous solution for forming a protective coating film with a plasticizer content of 3% by weight and a laminate on which a glass coating film was formed were prepared in the same manner as in Comparative Example 1, except that glycerin was used instead of diglycerin as the plasticizer and an aqueous solution was prepared as shown in Table 1. The coating film was composed only of glycerin, which is a plasticizer, and water.

[0074] Comparative Example 4 An aqueous solution for forming a protective film with a plasticizer content of 20% by weight and a laminate on which a glass film was formed were prepared in the same manner as in Comparative Example 3, except that only glycerin, a plasticizer, was prepared as an aqueous solution as shown in Table 1. The film was composed only of glycerin, a plasticizer, and water.

[0075] Comparative Example 5 An aqueous solution for forming a protective coating film and a laminate having a glass coating formed thereon were prepared in the same manner as in Comparative Example 1, except that 100 parts by weight of unmodified polyvinyl alcohol (SELVOL 203, manufactured by Sekisui Chemical Co., Ltd., degree of polymerization 300, degree of saponification 88 mol%) was used instead of 100 parts by weight of unmodified polyvinyl alcohol (degree of polymerization 500, degree of saponification 88 mol%), and the amount of plasticizer added and the resin concentration were as shown in Table 1.

[0076] <Evaluation> The protective coating film-forming aqueous solutions (aqueous solutions) obtained in the Examples and Comparative Examples, and the laminates on which the glass coating film was formed, were evaluated as follows. The results are shown in Table 1.

[0077] 1. Evaluation of aqueous solutions for forming protective films (Contact angle measurement) Using a contact angle meter (Kyowa Interface Science Co., Ltd., DMo-502) and analysis software FAMAS (Kyowa Interface Science Co., Ltd.), contact angles were measured by the θ / 2 method (A half-angle method) at a temperature of 23° C. and a humidity of 60% R / H. The measurement conditions were as follows: the amount of droplet was 2 μL, a 0.5 mm thick glass (TEMPAX Float, manufactured by SCHOTT) was used as the contact angle measurement substrate, the measurement was performed in time-lapse measurement mode with a waiting time of 100 msec before measurement. The measurement interval was 1000 msec, and measurements were repeated five times. The five data points over 4100 msec were averaged to obtain the measurement results.

[0078] (viscosity measurement) The prepared aqueous solution for forming a protective film was dispensed into a mayonnaise bottle, which was then covered and aged for 2 days (48 hours) at a temperature of 23°C and a humidity of 60%RH. The aqueous solution for forming a protective film after aging was subjected to a viscosity evaluation using a rotational viscometer (Toki Sangyo Co., Ltd., TVC-10) under conditions of a temperature of 23°C and a humidity of 60%RH according to a method conforming to JIS K7117-1.

[0079] 2. Evaluation of coatings and laminates (Thickness evaluation) The glass film was peeled off from the laminate on which the glass film was formed, and the thickness of the glass film was measured using a constant pressure thickness gauge (e.g., PG-02J manufactured by Teclock Co., Ltd.) conforming to JIS K6783. When peeling was difficult, the thickness of the laminate on which the glass film was formed was measured using the above constant pressure thickness gauge, and the value obtained by subtracting the thickness of the glass substrate, which had been measured in advance using the same method, was used as the thickness.

[0080] (Surface roughness) The surface roughness Sa, Sz and Sdr were measured by peeling the glass coating from the laminate on which the glass coating was formed, and measuring the main surface opposite the substrate (air interface side surface) and the main surface on the glass substrate side (glass interface side surface) in an area of ​​1 mm x 1 mm with a laser microscope (e.g., morphological analysis laser microscope, VK-X1050, manufactured by Keyence Corporation). From the obtained measurement values, each surface roughness was calculated in accordance with ISO 25178. This was measured at 10 random locations, and the average value was used as each value.

[0081] (Coverage rate) The obtained glass coating was peeled off from the glass, and ten areas of 1 mm x 1 mm were measured using a laser microscope (e.g., morphological analysis laser microscope VK-X1050, manufactured by Keyence Corporation), and the proportion of the area without the coating was averaged and evaluated. ◎: 90% or more of the area is covered with a film ○: Less than 90% and 80% or more of the area is covered with a film △: Less than 80% and 70% or more of the area is covered with a coating ×: Less than 70% of the film is covered

[0082] (Foaming) The glass film of the obtained laminate was peeled off, and the cross section of the peeled film was observed with a laser microscope (e.g., morphological analysis laser microscope VK-X1050, manufactured by Keyence Corporation) to check for the presence or absence of bubbles, and evaluated according to the following criteria. ○: Foaming ×: No foaming was observed

[0083] (foam diameter) The glass film of the obtained laminate was cut with a razor blade along a plane parallel to the thickness direction. Thereafter, the maximum bubble diameter in the normal direction was measured for the cut surface in the thickness direction using a laser microscope (eg, morphological analysis laser microscope VK-X1050, manufactured by Keyence Corporation). This procedure was repeated 10 times at different measurement points, and the average of the observed bubble diameters was taken as the average bubble diameter. The bubble diameter of each bubble was taken as the diameter of the largest inscribed circle drawn around the observed bubble. The resulting bubble diameter (average bubble diameter) was evaluated according to the following criteria. ◎: The bubble diameter was 20% or more of the thickness of the glass film. ○: The bubble diameter was less than 20% and 5% or more of the thickness of the glass film. △: The bubble diameter was less than 5% and 1% or more of the thickness of the glass film. ×: The bubble diameter was less than 1% of the thickness of the glass film.

[0084] (Crystallization degree) For test pieces made from the glass film of the obtained laminate, diffracted light was measured at X-ray incidence angles 2θ = 2° to 40° using an XRD diffractometer (Rigaku Corporation, Rint2500), and the crystallinity was calculated from the peak and halo intensities and evaluated according to the following criteria. The measurement conditions were as follows: X-ray tube: CuKα radiation (λ=1.54 Å), X-ray output: 40 kV 200 mA, scanning method: step scan (FT method), step width: 0.02, reflection intensity for 2 seconds per step. The degree of crystallinity was measured by peeling the glass coating from the laminate, and the surface that had been in contact with the glass was measured as the "glass interface" and the opposite surface was measured as the "surface." In the case of a two-layer structure, the surface that had been in contact with the glass was measured as the "glass interface" and the opposite surface was measured as the "surface." High: 50% or more Medium: Less than 50% 30% or more Low: Less than 30%

[0085] (peelability / removability) [Peelability] The obtained laminate (150mm x 150mm) was cut from the film side using a glass cutter (MS500, manufactured by Mitsubishi Diamond Co., Ltd.) and a glass cutting tool (Mrcs-APIO "Mrcs-ADP030065080-115000000A4", manufactured by Mitsubishi Diamond Co., Ltd.) to cut 10mm from the periphery to prepare a 130mm square sample. Then, adhesive tape (Sekisui Chemical Co., Ltd., Cellotape (registered trademark) No. 252, 24mm wide) was attached to the corners and peeled off at an angle of about 135°, and evaluated according to the following criteria. ◎: The coating was completely peeled off ○: Although some of the film remained, the film was not completely torn off and could be peeled off in one peeling. △: Although some breakage occurred, the coating could be peeled off by peeling it off multiple times. ×: The coating broke and could not be peeled off.

[0086] [180° peel strength] To evaluate the adhesive strength between the prepared film and the glass substrate, the obtained laminate (150 mm x 150 mm) was cut to prepare a film-attached glass sample of 25 mm x 150 mm for the 180° peel test. The cutting method was the same as in the above-mentioned [Peelability]. A backing adhesive tape (Tape part number Splicing Tape No. 642, Teraoka Manufacturing Co., Ltd.) was applied to the entire surface of the film to provide a backing, and the 180° peel strength of the film backed with the adhesive tape and the adhesive tape was measured using a Tensilon universal material testing machine (RTF-2430, GL Sciences Co., Ltd.) The measurement method was in accordance with ISO29862:2007 or JIS Z 0237:2009. When peeling off the coating surface, the end of the tape was grasped and folded back 180° so that the back of the backing surface was overlapping, and 25 mm of the coating surface was peeled off. After that, the part from which the coating surface had been peeled off was fixed to the lower jig of the testing machine, and the adhesive tape with substrate was fixed to the upper jig. The evaluation conditions were 300 mm / sec, temperature 25°C, and humidity 50%.

[0087] [Water soluble] The glass film was removed from the obtained laminate by 1 cm2 The film was peeled off, immersed in a beaker containing 10°C water, and the water solubility [water solubility at 10°C] was evaluated according to the following criteria. The water solubility when the film was placed in 95°C water [water solubility at 95°C] was also evaluated. ○: Dissolved within 60 seconds △: Dissolved within 61 to 120 seconds ×: Not dissolved within 120 seconds

[0088] (Residue after removing the coating) The glass film of the obtained laminate was removed from the glass substrate, and the residue was evaluated. The glass film was removed by three methods: "1. Removal by peeling," "2. Removal by washing with water," and "3. Removal by washing with water after peeling (water washing after peeling)." [1. Removal by peeling] The obtained laminate (150 mm×150 mm) was cut to prepare a glass sample with a glass film of 10 mm×10 mm, and the glass film was removed by peeling. [2. Removal by washing with water] Steam at 85 to 90°C was sprayed onto the glass coating surface of the obtained laminate (150 mm x 150 mm) from a nozzle with a slit width of 0.1 mm at a maximum steam pressure of 0.2 MPa and a rate of 2 L / min. The glass coating was then removed by washing with hot water at 90°C and then with room temperature water using a slit nozzle. "3. Removal by rinsing with water after peeling (rinsing with water after peeling)" The obtained laminate (150 mm×150 mm) was cut to prepare a glass sample with a glass film of 10 mm×10 mm, and the glass film was removed by peeling. Next, the sample from which the glass coating had been removed by peeling was sprayed with steam at 85 to 90°C from a nozzle with a slit width of 0.1 mm at a maximum steam pressure of 0.2 MPa and a rate of 2 L / min, after which it was washed with hot water at 90°C and then washed with room temperature water using a slit nozzle.

[0089] [XPS evaluation] The glass surfaces of the areas that had been subjected to "1. Removal by peeling," "2. Removal by water rinsing," and "3. Removal by water rinsing after peeling (water rinsing after peeling)" were measured using X-ray electron spectroscopy (XPS, PHI5000 VersaProbe II, manufactured by ULVAC-PHI, Inc.) to determine the composition and quantification of the remaining material on the outermost surface. The measurement conditions were as follows: monochromatic AlKα (1486.6 eV) was used as the light source, the photoelectron take-off angle was 45 degrees, and the X-ray beam diameter was 200 μm. In addition, a glass substrate of the same type as that used for the production was subjected to the above-mentioned "1. Removal by peeling," "2. Removal by water rinsing," and "3. Removal by water rinsing after peeling (water rinsing after peeling)" to prepare a reference sample. The glass surface was evaluated using XPS, and the carbon atom amount (%) was calculated based on the carbon atom amount (atom%) of the reference sample [(measured carbon atom amount / carbon atom amount of reference sample) x 100], and evaluated according to the following criteria. Note that the carbon atom amount (%) based on the reference sample is proportional to the amount of the coating remaining on the glass that cannot be seen with the naked eye after the coating is removed, and the smaller this is, the easier it is to clean the glass surface by washing after the coating is removed. ◎: Carbon atom content is 150% or less ○: Carbon atom content is more than 150% and 250% or less △: Carbon atom content is more than 250% and less than 400% ×: Carbon atom content is more than 400%

[0090] (Storage) The two laminates (150mm x 150mm) obtained were stacked so that the glass film surfaces were in close contact with each other, and a 3.0kg SUS plate of the same size or larger was placed on top of them, and left in an environment of 25°C and 50% RH for one week. After that, the two laminates were peeled off, and the damage rate of the glass film was confirmed and evaluated according to the following criteria. ◎: The percentage of glass film damage is 10% or less. ○: The percentage of glass film damage is more than 10% and 30% or less. △: The percentage of glass film damage is more than 30% and less than 50%. ×: The percentage of glass film broken is more than 50%.

[0091] (Foreign matter removal effect) 0.05 g of silica particles (average particle size: 3 μm) were dry-sprayed onto the glass film side of the obtained laminate to adhere to the film. The film was then peeled off, and the presence or absence of silica particles was confirmed under an optical microscope in a 5 cm square area at the center of a 15 cm square glass sheet, and evaluated according to the following criteria. ◎: Less than 10 silica particles were found ○: 11 to 20 silica particles were confirmed △: 21 to 50 silica particles were confirmed ×: 51 or more silica particles were confirmed

[0092] (Surface protection: Scratch resistance) 0.05 g of silica particles (average particle size: 3 μm) were dry-sprayed onto the glass film side of the obtained laminate to adhere to the film, and a glass substrate of the same size (Corning, EagleXG 150 mm × 150 mm × 0.5 mm) was further laminated on top of it and rubbed in the surface direction. The film was then peeled off, and the surface was observed and evaluated according to the following criteria. 〇: No scratches on the surface ×: Scratches on the surface

[0093] (Environmental adaptability) The peeled off coating was evaluated for its soil biodegradability. If it is soil biodegradable, it can be said to be environmentally compatible. Furthermore, the film that can be removed by washing with water can be completely dissolved in water and can be disposed of in normal sewer systems, just like the film that encases the detergent in detergent gel balls, making it environmentally compatible. ○: Biodegradable in soil ×: Not biodegradable in soil

[0094] [Table 1] [Industrial Applicability]

[0095] According to the present invention, it is possible to provide a method for manufacturing a laminate, a method for manufacturing a substrate, and a substrate capable of forming a protective coating that is resistant to adhesion of foreign matter originating from the substrate in a production line or a transport line.

Claims

1. A method for producing a laminate having a substrate and a multi-layer coating, comprising a coating formation step of applying two or more aqueous solutions for forming protective coatings, each having a different composition, to a substrate to form a multi-layer coating.

2. The method for producing a laminate according to claim 1, wherein the multi-layer coating is capable of adjusting at least one property selected from the group consisting of adhesiveness, protectiveness, and peelability.

3. 3. The method for producing a laminate according to claim 1, wherein two or more types of aqueous solutions for forming a protective film having different compositions are applied in succession.

4. The method for producing a laminate according to any one of claims 1 to 3, wherein the temperature of the substrate is 0°C or higher and 400°C or lower in the coating formation step.

5. The method for producing a laminate according to any one of claims 1 to 4, further comprising a base forming step of forming a base, the base forming step and the film forming step being carried out successively.

6. The method for producing a laminate according to any one of claims 1 to 5, wherein the first applied aqueous solution for forming a protective film contains a plasticizer and water.

7. The method for producing a laminate according to any one of claims 1 to 6, wherein any one of the plurality of aqueous solutions for forming a protective film to be applied secondly or thereafter contains a polyvinyl alcohol resin and water.

8. The method for producing a laminate according to any one of claims 1 to 7, wherein the first aqueous solution for forming a protective film does not contain a polyvinyl alcohol resin, or the polyvinyl alcohol resin content of the first aqueous solution for forming a protective film is less than the polyvinyl alcohol resin content of the second or subsequent aqueous solutions for forming a protective film.

9. The method for producing a laminate according to any one of claims 1 to 8, wherein the plasticizer content of the first applied aqueous solution for forming a protective film is greater than the plasticizer content of the second or subsequent applied aqueous solutions for forming a protective film.

10. 10. The method for producing a laminate according to claim 1, wherein the first applied aqueous solution for forming a protective film has a plasticizer content of 0.1 to 80% by weight and a water content of 20 to 99.9% by weight.

11. The method for producing a laminate according to any one of claims 1 to 10, wherein the second or subsequent aqueous protective film forming solutions have a polyvinyl alcohol resin content of 0.1 to 50% by weight, a plasticizer content of 0.1 to 50% by weight, and a water content of 10 to 99.8% by weight.

12. A method for producing a substrate, comprising: the method for producing a laminate according to any one of claims 1 to 11; and a removing step of removing the multi-layer coating from the substrate.

13. A substrate obtained by the method for producing a substrate according to claim 12.

Citation Information

Patent Citations

  • Glass product and its production