Fatty acid-treated zinc oxide particles, method for manufacturing the same, and dispersions and cosmetics containing the same

A method for producing fatty acid-treated zinc oxide particles with controlled surface treatment and particle size ensures high dispersibility and stability, addressing viscosity and agglomeration issues, suitable for use in cosmetics and other applications.

JP2024144795APending Publication Date: 2024-10-15SAKAI CHEM IND CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023056907
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Fatty acid-treated zinc oxide particles face issues with excessive viscosity and instability in highly concentrated dispersions due to the formation of fatty acid soap, unreacted fatty acids, and particle agglomeration, limiting their use in cosmetics and other applications.

Method used

The production method involves preparing a slurry of zinc oxide particles without drying, neutralizing fatty acids with a base to form a fatty acid salt solution, and applying this solution to the zinc oxide slurry at temperatures equal to or above the fatty acid's melting point, ensuring uniform surface treatment and minimizing unreacted fatty acids and agglomeration, with specific FT-IR and particle size criteria to ensure effective bonding.

Benefits of technology

The method produces zinc oxide particles with excellent dispersibility and stability, maintaining low viscosity even at high concentrations, making them suitable for use in cosmetics and other applications without the environmental impact of silicone treatments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144795000004
    Figure 2024144795000004
  • Figure 2024144795000005
    Figure 2024144795000005
  • Figure 2024144795000006
    Figure 2024144795000006
Patent Text Reader

Abstract

To provide fatty acid-treated zinc oxide particles that have excellent dispersibility, and even in dispersions mixed at high concentrations, not causing excessive stickiness, making it possible to obtain dispersions with excellent stability over time.SOLUTION: Provided is a fatty acid treated zinc oxide particle, in which, in an FT-IR spectrum measured using an attenuated total reflection method (ATR method), a ratio (I2 / I1) of a maximum absorbance (I2) at 1,500 to 1,600 cm-1 to a maximum absorbance (I1) at 1,350 to 1,500 cm-1 is 0.8 to 1.2, and a ratio (I3 / I4) of a maximum absorbance (I3) at 1,700 to 1,720 cm-1 to a maximum absorbance (I4) at 1,750 to 1,800 cm-1 is 1.2 or less; a primary particle size measured using a transmission electron microscope is 0.1 μm or less; and a mode diameter of a dispersion liquid, which is obtained by placing the powder in isopropyl alcohol and dispersing it by irradiation with ultrasonic waves using ultrasonic homogenizer at a rated output of 600 W and a vibration amplitude of 100% for 1 minute at a room temperature, measured by a laser diffraction scattering method on a volume basis is 0.30 μm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to fatty acid-treated zinc oxide particles, a method for producing the same, and a dispersion and a cosmetic composition containing the same. [Background technology]

[0002] Traditionally, titanium dioxide particles and zinc oxide particles have been used as UV scattering agents in sunscreen cosmetics and other products because of their high UV shielding properties and transparency. When untreated, these powders have a hydrophilic surface and may be washed away by sweat or rain. For this reason, especially in cosmetics, the particle surface is often treated to make it water repellent.

[0003] Silicone treatment and alkoxysilane treatment are commonly used as such water repellent treatments. However, in recent years, silicone-treated products have tended to be avoided, and as an alternative, zinc oxide treated with fatty acids, which are naturally derived components, is in demand (for example, Patent Documents 1 and 2).

[0004] However, when fatty acid treatment is applied, problems occur such as a decrease in performance due to the formation of fatty acid soap consisting of zinc ions dissolved in water and fatty acids, thickening due to the presence of unreacted free fatty acids, and precipitation of solids, etc. Therefore, it is difficult to stably obtain a high-concentration dispersion, and since the performance is inferior to that of silicone-treated or alkoxysilane-treated zinc oxide, fatty acid-treated zinc oxide is not widely distributed on the market. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-196381 A [Patent Document 2] Patent Publication No. 2021-083334 Summary of the Invention [Problem to be solved by the invention]

[0006] In view of the above, an object of the present invention is to provide fatty acid-treated zinc oxide particles which have excellent dispersibility, do not show excessive thickening even when blended at a high concentration, and can give a dispersion with excellent stability over time. [Means for solving the problem]

[0007] The present invention relates to a method for measuring the attenuated total reflection (ATR) spectrum of 1350-1500 cm -1 For the maximum absorbance (I1), 1500-1600cm -1 The ratio (I2 / I1) of the maximum absorbance (I2) is 0.8 to 1.2, and 1750-1800cm -1 For the maximum absorbance (I4), 1700-1720cm -1 The ratio (I3 / I4) of the maximum absorbance (I3) is 1.2 or less, The present invention relates to fatty acid-treated zinc oxide particles, characterized in that the primary particle diameter measured using a transmission electron microscope is 0.1 μm or less, and the powder is placed in isopropyl alcohol and dispersed by irradiating the powder with ultrasonic waves at a rated output of 600 W and a vibration amplitude of 100% for 1 minute at room temperature, resulting in a dispersion having a mode diameter of 0.30 μm or less on a volume basis as measured using a laser diffraction scattering method. The fatty acid is preferably at least one selected from the group consisting of stearic acid, isostearic acid, and palmitic acid.

[0008] The present invention includes a step (1) of repulping zinc oxide particles, which are raw materials, in a dispersion medium to prepare a slurry; (2) neutralizing the fatty acid with a base to obtain an aqueous fatty acid salt solution; and and (3) adding the obtained fatty acid salt aqueous solution to the zinc oxide slurry to perform surface treatment. The zinc oxide particles as the raw material are obtained by a production method including a step of aging fine zinc oxide particles in water having a zinc salt dissolved therein, and are subjected to step (1) without a drying step, The method for producing fatty acid-treated zinc oxide particles is also characterized in that the steps (2) and (3) are carried out at a temperature equal to or higher than the melting point of the fatty acid. The zinc oxide particles, which are the raw material described above, are dispersed by placing the powder in a 0.0025 mass % aqueous solution of sodium hexametaphosphate and irradiating it with ultrasonic waves at a rated output of 600 W and a vibration amplitude of 100% for 3 minutes at room temperature, and the resulting dispersion preferably has a median diameter of 0.30 μm or less, as measured by a laser diffraction scattering method. The present invention also relates to a dispersion containing the above-mentioned fatty acid-treated zinc oxide particles. The present invention also relates to a cosmetic preparation comprising the above-mentioned fatty acid-treated zinc oxide particles. Effect of the Invention

[0009] According to the present invention, it is possible to provide a fatty acid-treated zinc oxide having a low environmental impact and sufficient water repellency. In addition, by using the fatty acid-treated zinc oxide particles of the present invention, it is possible to obtain a dispersion and a cosmetic composition having excellent dispersibility and stability over time. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a diagram showing an FT-IR spectrum of the fatty acid-treated zinc oxide particles obtained in the examples. [Diagram 2] FIG. 2 is a diagram showing an FT-IR spectrum of the fatty acid-treated zinc oxide particles obtained in the comparative example. [Diagram 3] FIG. 2 is a schematic diagram illustrating a method for measuring the primary particle diameter of the fatty acid-treated zinc oxide particles of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below.

[0012] (fatty acid treated zinc oxide particles) The fatty acid-treated zinc oxide particles of the present invention can suppress thickening of the dispersion even when incorporated at a high concentration, and can produce a dispersion having excellent stability over time. In order to achieve this effect, the following three conditions must be met: (1) Suppresses the production of fatty acid zinc (fatty acid soap). (2) Reduce the amount of unreacted fatty acids remaining. (3) The particles are easily dispersible.

[0013] The various problems described above are believed to be caused by fatty acid zinc, unreacted fatty acid, and agglomerated particles, and therefore the object of the present invention can be achieved by reducing these components.

[0014] When the treatment with fatty acid in the present invention is performed, it is preferable to obtain treated particles in which fatty acid is bound to the surface of zinc oxide particles. On the other hand, free fatty acid zinc produces undesirable effects. It is considered that free fatty acid zinc is formed when zinc oxide reacts with water to produce zinc ions, which then react with fatty acid to become fatty acid zinc. Therefore, in the present invention, the surface treatment process is adjusted to prevent such reactions as much as possible.

[0015] Furthermore, any remaining unreacted fatty acid also adversely affects performance, so it is desirable to avoid excess fatty acid.

[0016] In addition, if particles are aggregated, the aggregates break down during dispersion, resulting in untreated surfaces, which is thought to cause thickening when blended at high concentrations.Easily dispersible particles are not aggregated and are uniformly treated, so they do not thicken even when blended at high concentrations, making it possible to obtain a dispersion with low viscosity.

[0017] Since the fatty acid-treated zinc oxide particles of the present invention satisfy the above (1) and (2), the IR peak intensity derived from the fatty acid zinc or fatty acid is smaller than the IR peak intensity of zinc oxide particles that have not been subjected to a suitable surface treatment, and in the present invention, this is expressed by the parameters (I2 / I1) and (I3 / I4).

[0018] The fatty acid-treated zinc oxide particles of the present invention have a wavelength of 1350-1500 cm in the FT-IR spectrum measured using an attenuated total reflectance (ATR) method. -1 For the maximum absorbance (I1), 1500-1600cm -1 The ratio (I2 / I1) of the maximum absorbance (I2) is 0.8 to 1.2 and the wavelength range is 1750-1800 cm -1 For the maximum absorbance (I4), 1700-1720cm -1 The ratio (I3 / I4) of the maximum absorbance (I3) of the In the above ratio (I2 / I1), the absorbance I1 value is 1350-1500cm -1 Detected in CH3 symmetric bending vibration, COO - The absorbance I2 is the maximum peak absorbance of either the symmetric stretching vibration or the CH3 asymmetric bending vibration. The absorbance I2 value is 1500-1600cm -1 Detected by COO - This is the absorbance value of the maximum peak of the antisymmetric stretching vibration. When the ratio (I2 / I1) is 0.8 to 1.2, it means that the fatty acid is bonded to the zinc oxide surface, and when it is greater than 1.2, it means that free fatty acid zinc is precipitated. When the ratio is less than 0.8, it means that the fatty acid is not sufficiently bonded to the zinc oxide surface, and a large amount of unreacted fatty acid is present. The lower limit of the above ratio (I2 / I1) is preferably 0.9, and the upper limit is preferably 1.1.

[0019] The fatty acid-treated zinc oxide particles of the present invention further have a molecular weight of 1750-1800 cm -1 For the maximum absorbance (I4), 1700-1720cm -1 The ratio (I3 / I4) of the maximum absorbance (I3) of the The absorbance I3 value is 1700-1720cm -1 The absorbance of the C=O stretching vibration peak, absorbance I4, is detected at 1750-1800cm -1This is the absorbance value of the peak of the C=O stretching vibration of four-membered rings, five-membered rings, and acid anhydrides that is detected in the FTIR. Since no substances corresponding to four-membered rings, five-membered rings, or acid anhydrides exist in this manufacturing process, no peaks are detected. Therefore, if the I3 / I4 value exceeds 1.2, it means that unreacted fatty acids remain. The ratio (I3 / I4) is preferably 1.1 or less, and although there is no particular lower limit, it is preferably 0.8 or more.

[0020] Furthermore, since the fatty acid-treated zinc oxide particles of the present invention satisfy the above-mentioned (3), the particle size distribution in weak dispersion is close to the primary particle diameter, which is expressed in the present invention by a parameter called the mode diameter. The fatty acid-treated zinc oxide particles of the present invention are characterized in that the primary particle diameter measured from a transmission electron microscope photograph is 0.1 μm or less, and the powder is placed in isopropyl alcohol and dispersed by irradiating the powder with ultrasonic waves at a rated output of 600 W and a vibration amplitude of 100% for 1 minute at room temperature, resulting in a dispersion having a mode diameter of 0.30 μm or less on a volume basis as measured by a laser diffraction scattering method.

[0021] Specifically, the primary particle diameter in the present invention is a particle diameter (μm) defined as a unidirectional diameter (the distance between two parallel lines in a fixed direction sandwiching a particle as shown in FIG. 3; for any shape of particle in the image, the measurement was performed in a fixed direction) in a field of view of 2000 to 50000 times in a photograph taken with a transmission electron microscope JEM-1200EX II (manufactured by JEOL Ltd.), and is obtained by measuring the unidirectional diameters of 250 primary particles in the TEM photograph and calculating the average value of the cumulative distribution. The primary particle diameter is more preferably 0.005 μm or more and less than 0.1 μm.

[0022] The mode diameter in the present invention is specifically measured by the following method: 0.1 g of the above fatty acid-treated zinc oxide particles is placed in 50 ml of isopropyl alcohol, and ultrasonic waves with a vibration amplitude of 100% are irradiated for 1 minute at room temperature using an ultrasonic homogenizer US-600E (manufactured by Nippon Seiki Seisakusho, rated output 600 W) to prepare a slurry, and the mode diameter on a volume basis is measured using a laser diffraction / scattering particle size distribution measuring device LA-960S (manufactured by Horiba, Ltd.). Another feature of the fatty acid-treated zinc oxide particles of the present invention is that they have very high dispersibility, so that they are sufficiently dispersed simply by applying a weak impact from ultrasonic waves. It is more preferable that the mode diameter is 0.20 μm or less.

[0023] The fatty acid-treated zinc oxide particles of the present invention have a surface treatment layer made of a fatty acid on the surface. As a water-repellent surface treatment agent, a fatty acid having high environmental adaptability is most preferable. The surface treatment referred to here is a water-repellent treatment for reducing the affinity of the zinc oxide particle surface for water, and surface treatment using a material that is easily soluble in water or disperses in water after treatment does not fall under the "water-repellent treatment" of the present invention.

[0024] The fatty acid used in the present invention is preferably one that has strong water repellency. Compounds that form some kind of chemical bond with inorganic powder are preferred, but even compounds that physically adsorb can provide a certain degree of effect. The fatty acid is preferably a higher fatty acid having 10 to 30 carbon atoms, since this can further improve the dispersibility of zinc oxide particles in the dispersion. Specifically, it is preferably at least one type selected from saturated fatty acids such as stearic acid, isostearic acid, myristic acid, lauric acid, palmitic acid, etc., and unsaturated fatty acids such as oleic acid. Among these, stearic acid, palmitic acid, and isostearic acid are preferable from the viewpoints of being inexpensive, highly stable, and having strong water repellency due to their simple structure. In order to make a treatment agent that places a smaller burden on the environment, it is preferable to use fatty acids derived from plants.

[0025] The fatty acid-treated zinc oxide particles of the present invention may be obtained by coating the particle surface of zinc oxide particles as the raw material with another inorganic compound, i.e., the zinc oxide particles that have been surface-treated with another inorganic compound may be further surface-treated with a fatty acid. The coating material may be a known inorganic surface treatment material, for example, one or more of oxides or hydroxides of Al, Si, Zr, Sn, or the like.

[0026] Zinc oxide particles, the active ingredient, release zinc ions over time, which can destroy the emulsion system when incorporated into cosmetics. In addition, the surface catalytic activity of zinc oxide has the problem of denaturing other ingredients. However, if the active ingredient is coated with an inorganic compound, the loss of zinc ions can be prevented, and therefore, for such applications (e.g., cosmetics), coating with an inorganic compound is preferable.

[0027] In particular, it is preferable to use a material that has been surface-treated with one or both of aluminum hydroxide and hydrous silicic acid, since these are harmless to the environment and human body and have a high activity suppression effect.

[0028] The coating amount of the inorganic surface treatment material is preferably 1 to 30% by mass based on the zinc oxide, in which case sufficient activity suppression is achieved and the effect on the properties of the zinc oxide is small. The lower limit is more preferably 3% by mass, and the upper limit is more preferably 20% by mass.

[0029] The method of surface treatment with the inorganic surface treatment material is not particularly limited, and can be any well-known method.

[0030] The fatty acid-treated zinc oxide particles of the present invention preferably have an apparent density of 0.5 g / ml or more. When the apparent density is 0.5 g / ml or more, the bulk of the powder is reduced, which is preferable in that, for example, the amount of dust generated is reduced, and the powder can be easily packed into a packaging container, allowing a large amount of powder to be transported during transportation. In addition, it is preferable in that the powder can be easily handled, for example, when mixed with other components, in a container with a smaller volume. The apparent density is more preferably 0.6 g / ml or more. The higher the apparent density, the smaller the bulk of the powder. The apparent density can be measured by the method described in JIS K 5101-12-1 Pigment Test Method - Apparent Density or Apparent Specific Volume (Still Method).

[0031] The fatty acid-treated zinc oxide particles of the present invention have a BET specific surface area of ​​25 m 2 / g or less. The BET specific surface area is preferably 25 m 2 When the specific surface area exceeds 1 / g, the particle size becomes small and aggregation is likely to occur. The BET specific surface area can be measured by the method described in the Examples.

[0032] The carbon content in the fatty acid-treated zinc oxide particles of the present invention is preferably 0.5% by mass or more and less than 8.0% by mass. If the carbon content is less than 0.5% by mass, there is a risk that the water repellency effect may not be sufficient. If the carbon content is 8.0% by mass or more, there is a risk that the purity of the zinc oxide decreases, resulting in a decrease in performance, and addition of an excessive amount may lead to precipitation of free fatty acid zinc. More preferably, it is 1.0% by mass or more and less than 7.0% by mass. The carbon content can be measured by the method described in the Examples.

[0033] (Method of producing fatty acid zinc oxide particles) The fatty acid-treated zinc oxide particles of the present invention are not particularly limited in terms of their production method, and examples thereof include a method for producing fatty acid-treated zinc oxide particles, which includes a step (1) of repulping zinc oxide particles as the raw material in a dispersion medium to prepare a slurry, a step (2) of neutralizing the fatty acid with a base to obtain an aqueous fatty acid salt solution, and a step (3) of adding the obtained aqueous fatty acid salt solution to the zinc oxide slurry for surface treatment, in which the zinc oxide particles as the raw material are obtained by a production method including a step of maturing fine zinc oxide particles in water in which a zinc salt is dissolved, and are subjected to step (1) without a drying step, and the above steps (2) and (3) are carried out at a temperature equal to or higher than the melting point of the fatty acid. Such a production method is also one aspect of the present invention.

[0034] The above step (1) is a step of preparing a slurry by repulping zinc oxide particles, which are raw materials, in a dispersion medium. In the production method of the present invention, preparing a slurry of zinc oxide particles in step (1) is an important step. That is, the method is characterized in that the fatty acid coating is formed when the zinc oxide particles are in a dispersed slurry state, not in a dry aggregated state.

[0035] Here, the zinc oxide particles used as the raw material in step (1) are those which have undergone a synthesis reaction in an aqueous medium, and are used to prepare a slurry without undergoing a drying step. That is, it is preferable not to have a step of drying the particles between the particle production step and the fatty acid treatment step. In this way, aggregation between particles is suppressed, and surface treatment is not performed on the aggregated particles, so that the above-mentioned excellent dispersion performance can be obtained.

[0036] By this step (1), each zinc oxide particle is surface-treated, and therefore water repellency can be efficiently imparted without the need for an excessive amount of fatty acid coating. In the above step (1), the zinc oxide particle slurry is not limited, but it is preferable that the zinc oxide particle slurry contains, for example, zinc oxide particles in the range of 10 to 1000 g / L.

[0037] The method for preparing the slurry is not particularly limited. For example, zinc oxide particles obtained in a zinc oxide particle production process are filtered, and then added to water without drying, and dispersed at 5 to 30°C for 10 to 30 minutes to obtain a uniform slurry having a zinc oxide particle concentration of 10 to 1000 g / l. The dispersion medium is not particularly limited, and for example, alcohols such as isopropanol or organic solvents can be used, but it is preferable to use water from the standpoint of safety and production costs.

[0038] The above step (2) is a step of neutralizing a fatty acid with a base to obtain an aqueous solution of a fatty acid salt, and is carried out at a temperature equal to or higher than the melting point of the fatty acid. The concentration of the above aqueous solution of a fatty acid salt is preferably 15 wt% or less, more preferably 10 wt% or less, from the viewpoint of production. Therefore, the above temperature is more preferably a temperature at which the solubility of the fatty acid salt in water is 10 wt% or more. The above neutralization is preferably carried out using a commonly used base such as caustic soda (sodium hydroxide) or caustic potash (potassium hydroxide). The above melting point and solubility are determined by the composition of the fatty acid used, so the temperature of step (2) may vary. For example, when stearic acid is used as the fatty acid, the melting point of stearic acid is 70°C, so it is sufficient to carry out the neutralization at a temperature of 70°C or higher. Furthermore, when caustic soda is used as the base, the solubility of sodium stearate in water is 3 wt% at 70°C and 10 wt% at 75°C, so it is more preferable to carry out the neutralization at a temperature of 75°C or higher.

[0039] The above step (2) is preferably carried out with stirring, which allows the fatty acid and the fatty acid salt to be more thoroughly melted and dissolved. The stirring means in the above step (2) is not particularly limited, but examples thereof include stirring with a stirring blade, shaking stirring, stirring with a mixer, stirring with a stirrer, and the like.

[0040] The step (3) is a step of adding the obtained aqueous fatty acid salt solution to the zinc oxide slurry to perform surface treatment. In the surface treatment step, it is preferable to add the aqueous fatty acid salt solution to the zinc oxide particle slurry obtained in step (1) and then stir the mixture. Stirring facilitates uniform adsorption of the fatty acid onto the zinc oxide particles, and allows the surface treatment to be carried out more efficiently. The stirring time is not particularly limited, but is preferably 5 minutes or more. The stirring means is not particularly limited, but examples thereof include stirring with a stirring blade, shaking, mixing with a mixer, and stirring with a stirrer.

[0041] Like the step (2), the step (3) of carrying out the surface treatment is also carried out at a temperature equal to or higher than the melting point of the fatty acid, and it is more preferable that the temperature is such that the solubility of the fatty acid salt in water is 10 wt% or more. In the steps (2) and (3), the fatty acid is reacted with zinc oxide in a liquid state, not in a solid state, thereby enabling uniform surface treatment. If the temperature in the steps (2) and (3) is lower than the melting point of the fatty acid, the reaction between the fatty acid and the fatty acid salt and the zinc oxide may be insufficient. Insufficient reaction here includes a state in which the fatty acid or the fatty acid salt remains solid and is not uniformly chemically bonded or physically adsorbed to the zinc oxide. If the zinc oxide is not uniformly treated, even if the ratios (I2 / I1) and (I3 / I4) of the obtained fatty acid-treated zinc oxide particles are within the ranges of the present invention, problems such as aggregation due to untreated parts and difficulty in adsorbing the dispersant to the excessively treated parts may occur during the preparation of the dispersion, leading to increased viscosity. In the above step (3), it is preferable to heat both the aqueous fatty acid salt solution and the zinc oxide slurry to a temperature equal to or higher than the melting point of the fatty acid.

[0042] The step (3) is a step of adding an aqueous solution of a fatty acid salt, and it is preferable that the amount of fatty acid added is 1.0% by mass or more relative to the zinc oxide particles. If the amount added is less than 1.0% by mass, the water repellency may be insufficient. More preferably, it is 1.5% by mass or more. Furthermore, the amount added is preferably 10% by mass or less. If the amount added exceeds 10% by mass, simple fatty acid zinc that cannot be bonded to the zinc oxide surface remains even if the drying step is performed at a temperature equal to or higher than the melting points of the fatty acid and fatty acid zinc. This may result in the ratio (I2 / I1) being outside the range of the present invention. The amount added is more preferably 8% by mass or less.

[0043] After carrying out the surface treatment step in this manner, the resulting slurry is aged for 0.5 to several tens of hours while continuing to stir, to form a fatty acid coating on the surfaces of the zinc oxide particles. During the aging, small amounts of other components may be added within the range that does not impair the effects of the present invention. For example, a dispersant may be added.

[0044] The aging is preferably carried out at 45 to 110° C. In particular, the aging time can be 0.5 to 24 hours. Since zinc oxide particles that have been uniformly treated can be obtained depending on conditions such as the aging temperature, aging time, and zinc oxide concentration, it is preferable to appropriately set these conditions depending on the type and amount of fatty acid added.

[0045] The fatty acid-treated zinc oxide particles thus obtained may be subjected to post-treatments such as pH adjustment, filtration, and washing with water, if necessary. In the pH adjustment step, the pH of the aged slurry is preferably adjusted to 6-10, and more preferably 7-8. As the neutralizing agent, it is preferable to use a commonly used acid such as sulfuric acid or hydrochloric acid, and it is also possible to use a zinc salt such as zinc sulfate or zinc chloride. The method for producing fatty acid-treated zinc oxide particles of the present invention preferably further includes a drying step. Drying is preferably carried out at a temperature equal to or higher than the melting point of the fatty acid, and more preferably at a temperature equal to or higher than the melting point of the fatty acid zinc. By drying at a temperature equal to or higher than the melting points of the fatty acid and fatty acid zinc, the remaining fatty acid and the excess precipitated fatty acid zinc can be melted and chemically bonded to the zinc oxide surface. For example, when stearic acid is used as the fatty acid, drying is preferably carried out at a temperature equal to or higher than the melting point of stearic acid, which is 70°C, and more preferably at a temperature equal to or higher than the melting point of zinc stearate, which is 120°C.

[0046] The heating temperature in the drying step is not particularly limited, but it is preferable that the surface treatment is not followed by a calcination step in which the surface is heated to 300° C. or higher. By using such a method, the particle size and shape of the zinc oxide particles as the raw material can be maintained, and the above-mentioned effects of the present invention can be particularly suitably obtained. Furthermore, after the drying step, it is preferable to carry out a pulverization step as necessary. As a dry pulverization method, for example, an atomizer can be used.

[0047] The zinc oxide particles as the raw material are not particularly limited, but it is preferable to use one having high dispersibility in itself, since the dispersibility of the obtained fatty acid-treated zinc oxide particles will also be increased. In particular, it is preferable to use zinc oxide particles having a median diameter of 0.30 μm or less, as measured by a laser diffraction scattering method, in a dispersion liquid obtained by irradiating an ultrasonic homogenizer with ultrasonic waves at a rated output of 600 W and a vibration amplitude of 100% at room temperature for 3 minutes in a 0.0025 mass % sodium hexametaphosphate aqueous solution.

[0048] As described above, by subjecting zinc oxide particles with excellent dispersibility to fatty acid treatment, a uniform fatty acid coating layer is formed on each particle, and the obtained fatty acid-treated zinc oxide particles also have excellent dispersibility, so that they can be dispersed with a weak impact when blended into cosmetics, etc. On the other hand, when no impact is applied, aggregated particles can be formed with a moderate cohesive force, and therefore the handling properties are good.

[0049] The shape of the zinc oxide particles as the raw material is not particularly limited, but a plate shape is preferable in terms of improving the feel of the resulting fatty acid-treated zinc oxide particles when used and their shielding properties against UV rays, etc. For example, the primary particle diameter is preferably less than 0.1 μm, the aspect ratio is preferably less than 2.5, and the oil absorption / BET specific surface area is preferably 1.5 ml / 100 m. 2 The oil absorption / BET specific surface area (ml / 100m) is preferably less than 1000m. 2 ) is the oil absorption (ml / 100g) value and the BET specific surface area (m 2 / g), and the smaller this value, the lower the oil absorption per unit area of ​​the particle surface, the less the particles aggregate, and the higher the particle independence and dispersibility. Examples of such zinc oxide raw material particles include those obtained by a production method including a step of aging fine zinc oxide particles having a primary particle diameter of 0.005 μm or more and 0.05 μm or less in water in which a zinc salt is dissolved. Specifically, it is preferable to use, for example, zinc oxide particles disclosed in International Publication WO 2012 / 147888.

[0050] WO 2012 / 147888 discloses a method for obtaining zinc oxide particles with excellent dispersibility by a manufacturing method including a step of aging fine zinc oxide particles in water in which a zinc salt is dissolved. After producing zinc oxide particles in water by such a method, it is preferable to perform surface treatment by the above-mentioned method without filtering and drying. This allows surface treatment of zinc oxide particles in a state of less aggregation, and the object of the present invention can be suitably achieved.

[0051] The primary particle size is less than 0.1 μm, the aspect ratio is less than 2.5, and the oil absorption / BET specific surface area is 1.5 ml / 100 m by the manufacturing method described in WO 2012 / 147888. 2 It is particularly preferable to obtain zinc oxide particles having the following characteristics, which are described below.

[0052] The fatty acid-treated zinc oxide particles of the present invention may further be subjected to other surface treatments, if necessary. The surface treatment is not particularly limited, and examples thereof include known treatment methods such as inorganic surface treatments for forming an inorganic oxide layer such as a silica layer, an alumina layer, a zirconia layer, a titania layer, and other various surface treatments. In addition, a plurality of types of surface treatments may be performed in sequence.

[0053] More specifically, the surface treatment may be a surface treatment using a surface treatment agent selected from an organic aluminum compound, an organic titanium compound, a polyhydric alcohol, or an alkanolamine. The amount of such a surface treatment agent to be used may be appropriately determined depending on the particle size of the zinc oxide particles.

[0054] The fatty acid-treated zinc oxide particles of the present invention may be dispersed in water or an oil agent to form a dispersion. Such dispersions are also part of the present invention.

[0055] (Dispersion, cosmetics) The dispersion of the present invention preferably contains the fatty acid-treated zinc oxide particles of the present invention in a proportion of 40 to 80% by mass based on the total amount of the dispersion, and the lower limit is more preferably 45% by mass, and further preferably 50% by mass. Since the fatty acid-treated zinc oxide particles have the above-mentioned effects, even in such a relatively high blend amount range, the dispersibility is good, the viscosity of the dispersion is low, and the viscosity is maintained over time.

[0056] The dispersion of the present invention preferably further contains polyhydroxystearic acid, which functions as a dispersant, and is preferred in that the fatty acid-treated zinc oxide particles are well dispersed in a solvent. The use of polyhydroxystearic acid is particularly preferred in that good dispersion can be achieved even with a small amount, and that the fatty acid-treated zinc oxide particles having a water-repellent surface treatment layer are less likely to be washed away by water during use.

[0057] The hydroxyl group of hydroxystearic acid is preferably bonded to the carbon at position 12, and the degree of polymerization of hydroxystearic acid is preferably 3 to 12, and more preferably 4 to 8. Examples of commercially available products include Salacos HS-6C (manufactured by Nisshin Oillio Co., Ltd.) and ARLACEL P-100 (manufactured by Uniqema Co., Ltd.).

[0058] The blending amount of the polyhydroxystearic acid in the dispersion is preferably 0.1 to 10% by mass. The lower limit is more preferably 1% by mass, and the upper limit is even more preferably 7% by mass or less. The above ratio is particularly preferred in that the solvent content is increased and compatibility with the formulation when blended into the cosmetic preparation is high.

[0059] The dispersion of the present invention preferably contains an oil as a medium for dispersing the fatty acid-treated zinc oxide particles. The oil is not particularly limited, but is preferably an oil having no polysiloxane skeleton from the viewpoint of environmental load, and liquid oils that are liquid at room temperature (15 to 25°C) are preferred from the viewpoint of dispersibility. Examples include ester oil, fruit oil, and other oils and fats. Among them, ester oil and fruit oil are preferred because they are easy to use when used in cosmetics. Specifically, the following can be mentioned, and one or more of them can be used.

[0060] Examples of the ester oils include ethylhexyl palmitate, isopropyl isostearate, ethyl oleate, octyldodecyl oleate, octyldodecyl myristate, diisostearyl malate, glyceryl tricaprylate, isooctyl isononanoate, isotridecyl isononanoate, isononyl isononanoate, ethylhexyl isononanoate, propylene glycol dicaprate, neopentylene glycol dicaprate, neopentylene glycol diethylhexanoate, cetyl ethylhexanoate, glyceryl tri-2-ethylhexanoate, jojoba oil, isopropyl myristate, isopropyl palmitate, isotridecyl isononanoate, polyglyceryl diisostearate, diglyceryl triisostearate, glyceryl tribehenate, hexa(hydroxystearic acid / stearic acid / rosin acid) dipentaerythrityl, neopentyl glycol dioctanoate, cholesteryl isostearate, cholesteryl hydroxystearate, cholesteryl stearate, cholesteryl lanolate, phytosteryl oleate, N-lauroyl-L-glutamate di(cholesteryl-behenyl-octyldodecyl), N-lauroyl-L-glutamate di(phytosteryl-2-octyldodecyl), etc.

[0061] Examples of the fruit oil include olive fruit oil, lily of the valley fruit oil, fennel fruit oil, caraway fruit oil, pepper fruit oil, coriander fruit oil, juniper fruit oil, vanilla fruit oil, bergamot fruit oil, and lemon fruit oil.

[0062] Examples of the other oils and fats include safflower oil, soybean oil, evening primrose oil, grape seed oil, rosehip oil, coconut oil, almond oil, sesame oil, wheat germ oil, corn oil, cottonseed oil, avocado oil, camellia oil, persic oil, castor oil, peanut oil, hazelnut oil, macadamia nut oil, medfoam oil, cacao butter, shea butter, wood wax, coconut oil, palm oil, palm kernel oil, beef tallow, horse tallow, mink oil, milk fat, egg yolk oil, turtle oil, Japan wax, and camellia oil.

[0063] The blending amount of the oil agent in the dispersion is preferably 5 to 60% by mass. This ratio is preferable because it makes the oil more compatible with the cosmetic composition when blended therewith. The lower limit is more preferably 10% by mass, and the upper limit is more preferably 55% by mass.

[0064] In addition to the above-mentioned components, the dispersion of the present invention may contain preservatives, pH adjusters, pure water, etc., depending on the purpose.

[0065] The dispersion of the present invention preferably has an initial viscosity of 1,500 mPa s or less, more preferably 1,000 mPa s or less, as measured by the following evaluation method. If the viscosity is in this range, the dispersion has low viscosity and beads can be easily separated after dispersion.

[0066] Initial Viscosity Evaluation Method: 8 ml of the dispersion immediately after production was placed in a 9 ml screw bottle and rotated at 12 rpm using a B-type viscometer (Tokyo Keiki, TVB-10) with rotor No. 4, and the viscosity (25°C) was measured 60 seconds after the start of rotation.

[0067] Furthermore, the dispersion of the present invention preferably has a viscosity after 7 days of 2,000 mPa s or less, more preferably 1,800 mPa s or less, as measured by the following evaluation method. If the viscosity is within this range, the dispersion is not too viscous, is easy to remove from a container, and is easy to handle.

[0068] Viscosity evaluation method over time: 8 ml of the dispersion immediately after production was placed in a 9 ml screw bottle and stored in a 40°C thermostatic chamber for 7 days. The dispersion was then rotated at 12 rpm using a B-type viscometer (TVB-10 manufactured by Tokyo Keiki) with rotor No. 4, and the viscosity (25°C) was measured 60 seconds after the start of rotation.

[0069] The method for producing the dispersion of the present invention is not particularly limited. Specifically, for example, the fatty acid-treated zinc oxide particles, a dispersant, and a solvent are used as raw materials, and the raw materials are mixed with other components, stirred, and the like, to obtain the composition.

[0070] The dispersion of the present invention is preferably an oil-based dispersion that does not substantially contain water. Furthermore, the content of components other than the above-mentioned fatty acid-treated zinc oxide particles, dispersant, and solvent is preferably 1% by mass or less, more preferably 0.5% by mass or less. The dispersion may also consist of only the above-mentioned fatty acid-treated zinc oxide particles, dispersant, and solvent. The dispersion of the present invention can be used particularly as a raw material for producing cosmetics. For this reason, it is preferable that the dispersion contains as few components other than those mentioned above as possible so as not to cause any restrictions on the formulation.

[0071] The dispersion of the present invention may contain inorganic particles other than zinc oxide. Inorganic particles that can be used in combination are not particularly limited, but examples include titanium dioxide and the like. In particular, when titanium dioxide is used in combination with zinc oxide, the problem of thickening tends to become prominent, so the effect of the present invention becomes more prominent when used in combination with titanium dioxide. When zinc oxide is used as an ultraviolet shielding agent in ultraviolet protection cosmetics, titanium dioxide particles with different ultraviolet shielding ranges may be used in combination, so the present invention is also useful in such cases.

[0072] In the present invention, the titanium dioxide particles used in combination are not particularly limited, but it is preferable to use titanium dioxide particles whose surface has been treated with a fatty acid. The amount of fatty acid coated on the titanium dioxide particles is preferably 4.0 to 8.5% by mass relative to the titanium dioxide particles. The type of fatty acid may be the same as that used for zinc oxide. Similarly to zinc oxide particles, it is preferable to treat the particles with aluminum hydroxide or hydrous silicic acid and then with a fatty acid.

[0073] The surface treatment of the titanium dioxide particles can be carried out by a conventionally known method or a method similar to the treatment of the zinc oxide particles described above.

[0074] The titanium dioxide particles preferably have an average primary particle size of 200 nm or less. If the particle size of the titanium dioxide particles exceeds 200 nm, the hiding power is large, the particles become white, and the transparency is low. The lower limit of the average primary particle size of the titanium dioxide particles is not particularly limited, but is usually 5 nm. The average primary particle size of titanium dioxide particles is calculated by measuring the particle sizes of 200 randomly selected particles under an electron microscope and averaging the particle sizes.

[0075] The shape of titanium dioxide particles is not particularly limited, and any shape such as sphere, rod, needle, spindle, plate, etc. The above-mentioned average primary particle diameter in the case of a shape other than sphere is defined as the average length of the minor axis side in the case of rod-shaped, needle-shaped, and spindle-shaped particles, and is defined as the average diagonal length of the face in the case of plate-shaped particles. The titanium dioxide particles preferably have a major axis diameter / minor axis diameter (aspect ratio) of not more than 9. The aspect ratio of the titanium dioxide particles is calculated as the average major axis diameter / minor axis diameter value of 200 particles randomly selected under an electron microscope.

[0076] When inorganic particles other than zinc oxide, such as titanium dioxide, are used, the total amount of the fatty acid-treated zinc oxide particles and the inorganic particles other than zinc oxide, such as titanium dioxide, is preferably 40 to 70 mass % of the total amount of the dispersion. Furthermore, when inorganic particles other than zinc oxide, such as titanium dioxide, are used, the inorganic particles may be blended in an amount that does not impair the object of the present invention. For example, the blended amount of inorganic particles other than zinc oxide, such as titanium dioxide, is preferably no more than twice the mass of zinc oxide.

[0077] The dispersion of the present invention is preferably a non-silicone dispersion. Non-silicone means that it does not substantially contain silicone-based materials, and preferably does not substantially contain silicone-based oils, silicone-based surfactants, or inorganic particles surface-treated with silicone-based surface treatment agents. The silicone-based materials are preferably 1% by mass or less, more preferably 0.5% by mass or less, of the total amount of the dispersion.

[0078] The dispersion of the present invention is preferably used in cosmetics. The cosmetics are not particularly limited, but can be blended in cosmetics that are applied externally to the skin or hair, such as skin care products, hair products, makeup products, and UV protection products. The form of the product is also not particularly limited, but it can be applied in the form of a milky lotion, cream, solid, paste, gel, multi-layer, mousse, spray, etc.

[0079] The cosmetic of the present invention may be used in combination with any aqueous or oily component that can be used in the field of cosmetics as other raw materials of the dispersion of the present invention. The aqueous and oily components are not particularly limited, and examples thereof include oils, surfactants, moisturizing agents, higher alcohols, sequestering agents, water-soluble natural and semi-synthetic, synthetic polymers, water-soluble and oil-soluble polymers, organic ultraviolet screening agents, various extracts, etc. In addition, as necessary, various powders such as inorganic and organic pigments, inorganic and organic clay minerals, inorganic and organic pigments treated with metal soap or silicone, coloring agents such as organic dyes, and other pharmaceutical ingredients such as preservatives, antioxidants, coloring agents, thickeners, emulsifying thickeners, pH adjusters, fragrances, cooling agents, antiperspirants, bactericides, skin activators, anti-inflammatory agents, whitening agents, and film-forming agents may be contained. Specifically, the cosmetic product of interest can be produced by a conventional method by arbitrarily mixing one or more of the ingredients listed below. The amount of these ingredients is not particularly limited as long as it is within a range that does not impair the effects of the present invention. Furthermore, inorganic powders of ultraviolet scattering agents such as titanium dioxide and cerium oxide may be used as long as they do not impair the object of the present invention. The cosmetic preparation of the present invention may be a non-silicone-based formulation, or may be a formulation containing silicone-based materials, such as silicone-based oils, including methyl silicone and methyl phenyl silicone, depending on the purpose.

[0080] The oils are not particularly limited, and examples thereof include avocado oil, camellia oil, turtle oil, macadamia nut oil, corn oil, mink oil, olive oil, rapeseed oil, egg yolk oil, sesame oil, persic oil, wheat germ oil, sasanqua oil, castor oil, linseed oil, safflower oil, cottonseed oil, perilla oil, soybean oil, peanut oil, tea seed oil, kaya oil, rice bran oil, Chinese tung oil, Japanese tung oil, jojoba oil, germ oil, triglycerin, glycerin trioctanoate, glycerin triisopalmitate, cacao butter, coconut oil, horse tallow, hydrogenated coconut oil, palm oil, beef tallow, mutton tallow, hydrogenated beef tallow, palm kernel oil, lard, beef bone fat, Japan wax kernel oil, hydrogenated oil, beef leg fat, Japan wax, hydrogenated castor oil, beeswax, candelilla wax, cotton wax, carnauba wax, bayberry wax, and oleaginous wax. Examples of such wax include botara, whale wax, montan wax, bran wax, lanolin, kapok wax, lanolin acetate, liquid lanolin, sugarcane wax, lanolin fatty acid isopropyl, hexyl laurate, reduced lanolin, jojoba wax, hard lanolin, shellac wax, POE lanolin alcohol ether, POE lanolin alcohol acetate, POE cholesterol ether, lanolin fatty acid polyethylene glycol, POE hydrogenated lanolin alcohol ether, liquid paraffin, ozokerite, pristane, paraffin, ceresin, squalene, petrolatum, microcrystalline wax, propylene glycol dicaprate, ethylhexyl palmitate, and isotridecyl isononanoate.

[0081] The surfactant is not particularly limited, and examples thereof include lipophilic nonionic surfactants, hydrophilic nonionic surfactants, and other surfactants. The lipophilic nonionic surfactant is not particularly limited, and examples thereof include sorbitan fatty acid esters such as sorbitan monooleate, sorbitan monoisostearate, sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan sesquioleate, sorbitan trioleate, diglycerol sorbitan penta-2-ethylhexyl acid, and diglycerol sorbitan tetra-2-ethylhexyl acid; glycerin polyglycerin fatty acids such as glycerin monocottonseed oil fatty acid, glycerin monoerucate, glycerin sesquioleate, glycerin monostearate, α,α'-oleic acid pyroglutamic acid, and glycerin monostearate malic acid; propylene glycol fatty acid esters such as propylene glycol monostearate; hydrogenated castor oil derivatives; and glycerin alkyl ethers.

[0082] The hydrophilic nonionic surfactant is not particularly limited, and examples thereof include POE sorbitan fatty acid esters such as POE sorbitan monooleate, POE sorbitan monostearate, and POE sorbitan tetraoleate (e.g., polysorbate 60), POE sorbitan fatty acid esters such as POE sorbitan monolaurate, POE sorbitan monooleate, POE sorbitan pentaoleate, and POE sorbit monostearate, POE sorbitan fatty acid esters such as POE glycerin monostearate, POE glycerin monoisostearate, and POE glycerin triisostearate. POE glycerin fatty acid esters such as stearate, POE fatty acid esters such as POE monooleate, POE distearate, POE dioleate, and ethylene glycol distearate, POE lauryl ether, POE oleyl ether, POE stearyl ether, POE behenyl ether, POE 2-octyldodecyl ether, and POE cholestanol ether, and other POE alkyl phenyl ethers such as POE octylphenyl ether, POE nonylphenyl ether, and POE dinonylphenyl ether. POE·POP alkyl ethers such as POE·POP cetyl ether, POE·POP 2-decyl tetradecyl ether, POE·POP monobutyl ether, POE·POP hydrogenated lanolin, POE·POP glycerin ether, POE·POP alkyl ethers such as POE·POP glycerin ether, POE·POP tetraethylenediamine condensates such as Tetronic, POE castor oil, POE hydrogenated castor oil, POE hydrogenated castor oil monoisostearate, POE hydrogenated castor oil triisostearate, POE hydrogenated castor oil monopyroglutamic acid monoisostearyl Examples of suitable fatty acids include POE propylene glycol fatty acid esters, POE alkylamines, POE fatty acid amides, sucrose fatty acid esters, POE nonylphenyl formaldehyde condensates, alkyl ethoxydimethylamine oxides, and trioleyl phosphates.

[0083] Examples of the other surfactants that may be blended include anionic surfactants such as fatty acid soaps, higher alkyl sulfate ester salts, POE lauryl triethanolamine sulfate, and alkyl ether sulfate ester salts; cationic surfactants such as alkyl trimethyl ammonium salts, alkyl pyridinium salts, alkyl quaternary ammonium salts, alkyl dimethyl benzyl ammonium salts, POE alkyl amines, alkyl amine salts, and polyamine fatty acid derivatives; and amphoteric surfactants such as imidazoline-based amphoteric surfactants and betaine-based surfactants, within a range that does not cause problems in terms of stability and skin irritation.

[0084] The moisturizing agent is not particularly limited, and examples thereof include xylitol, sorbitol, maltitol, chondroitin sulfate, hyaluronic acid, mucoitin sulfate, caronic acid, atelocollagen, cholesteryl-12-hydroxystearate, sodium lactate, bile salts, dl-pyrrolidone carboxylate, short-chain soluble collagen, diglycerin (EO)PO adduct, Rosa rugosa extract, Achillea millefolium extract, and Melilot extract.

[0085] The higher alcohol is not particularly limited, and examples thereof include straight-chain alcohols such as lauryl alcohol, cetyl alcohol, stearyl alcohol, behenyl alcohol, myristyl alcohol, oleyl alcohol, and cetostearyl alcohol, and branched-chain alcohols such as monostearyl glycerin ether (batyl alcohol), 2-decyltetradecinol, lanolin alcohol, cholesterol, phytosterol, hexyldodecanol, isostearyl alcohol, and octyldodecanol.

[0086] The sequestering agent is not particularly limited, and examples thereof include 1-hydroxyethane-1,1-diphosphonic acid, 1-hydroxyethane-1,1-diphosphonic acid tetrasodium salt, sodium citrate, sodium polyphosphate, sodium metaphosphate, gluconic acid, phosphoric acid, citric acid, ascorbic acid, succinic acid, edetic acid, and the like.

[0087] The above-mentioned natural water-soluble polymer is not particularly limited, and examples thereof include plant-based polymers such as gum arabic, tragacanth gum, galactan, guar gum, carob gum, karaya gum, carrageenan, pectin, agar, quince seed, algae colloid (cassow extract), starch (rice, corn, potato, wheat), and glycyrrhizic acid; microbial polymers such as xanthan gum, dextran, succinoglucan, and pullulan; and animal polymers such as collagen, casein, albumin, and gelatin.

[0088] The semi-synthetic water-soluble polymer is not particularly limited, and examples thereof include starch-based polymers such as carboxymethyl starch and methylhydroxypropyl starch; cellulose-based polymers such as methyl cellulose, nitrocellulose, ethyl cellulose, methylhydroxypropyl cellulose, hydroxyethyl cellulose, sodium cellulose sulfate, hydroxypropyl cellulose, sodium carboxymethyl cellulose (CMC), crystalline cellulose, and cellulose powder; and alginic acid-based polymers such as sodium alginate and propylene glycol alginate.

[0089] The synthetic water-soluble polymer is not particularly limited, and examples thereof include vinyl polymers such as polyvinyl alcohol, polyvinyl methyl ether, and polyvinylpyrrolidone; polyoxyethylene polymers such as polyethylene glycol 20,000, 40,000, and 60,000; polyoxyethylene-polyoxypropylene copolymer polymers; acrylic polymers such as sodium polyacrylate, polyethyl acrylate, and polyacrylamide; polyethyleneimine; and cationic polymers.

[0090] The inorganic water-soluble polymer is not particularly limited, and examples thereof include bentonite, AlMg silicate (veegum), laponite, hectorite, and silicic anhydride.

[0091] The organic ultraviolet shielding agent is not particularly limited, and examples thereof include benzoic acid-based ultraviolet shielding agents such as para-aminobenzoic acid (hereinafter abbreviated as PABA), PABA monoglycerin ester, N,N-dipropoxy PABA ethyl ester, N,N-diethoxy PABA ethyl ester, N,N-dimethyl PABA ethyl ester, and N,N-dimethyl PABA butyl ester; anthranilic acid-based ultraviolet shielding agents such as homomenthyl-N-acetylanthranilate; amyl salicylate, menthyl salicylate, homomenthyl salicylate, and the like. salicylic acid-based ultraviolet screening agents such as p-isopropanol phenyl salicylate, octyl salicylate, phenyl salicylate, benzyl salicylate, and p-isopropanol phenyl salicylate; p-methoxycinnamate ethylhexyl, octyl cinnamate, ethyl 4-isopropyl cinnamate, methyl 2,5-diisopropyl cinnamate, ethyl 2,4-diisopropyl cinnamate, methyl 2,4-diisopropyl cinnamate, propyl p-methoxycinnamate, isopropyl p-methoxycinnamate, isoamyl cinnamic acid-based UV screening agents such as 2-ethylhexyl-p-methoxycinnamate, 2-ethoxyethyl-p-methoxycinnamate, cyclohexyl-p-methoxycinnamate, ethyl-α-cyano-β-phenylcinnamate, 2-ethylhexyl-α-cyano-β-phenylcinnamate, and glyceryl mono-2-ethylhexanoyl-di-paramethoxycinnamate; 2,4-dihydroxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, and 2,2'-dihydroxy-4,4'-dimethoxybenzophenone; benzophenone-based ultraviolet screening agents such as benzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-4'-methylbenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonate, 4-phenylbenzophenone, 2-ethylhexyl-4'-phenyl-benzophenone-2-carboxylate, 2-hydroxy-4-n-octoxybenzophenone, and 4-hydroxy-3-carboxybenzophenone;Examples of the benzoyl group include 3-(4'-methylbenzylidene)-d,l-camphor, 3-benzylidene-d,l-camphor, urocanic acid, urocanic acid ethyl ester, 2-phenyl-5-methylbenzoxazole, 2,2'-hydroxy-5-methylphenylbenzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, dibenzalazine, dianisoylmethane, 4-methoxy-4'-t-butyldibenzoylmethane, and 5-(3,3-dimethyl-2-norbornylidene)-3-pentan-2-one.

[0092] The various extracts are not particularly limited, and examples thereof include houttuynia extract, phellodendron bark extract, melilot extract, white lamb extract, licorice extract, peony extract, soapwort extract, loofah extract, cinchona extract, saxifrage extract, sophora flavescens extract, watercress extract, fennel extract, primrose extract, rose extract, rehmannia extract, lemon extract, lithospermum root extract, aloe extract, calamus root extract, eucalyptus extract, horsetail extract, sage extract, thyme extract, tea extract, seaweed extract, cucumber extract, clove extract, raspberry extract, melissa extract, carrot extract, horse chestnut extract, peach extract, peach leaf extract, mulberry extract, knotweed extract, witch hazel extract, placenta extract, thymus extract, silk extract, and licorice extract.

[0093] Examples of the various powders include glittering color pigments such as red iron oxide, yellow iron oxide, black iron oxide, titanium mica, iron oxide-coated titanium mica, and titanium oxide-coated glass flakes, inorganic powders such as mica, talc, kaolin, sericite, titanium dioxide, and silica, and organic powders such as polyethylene powder, nylon powder, cross-linked polystyrene, cellulose powder, and silicone powder. Preferably, in order to improve sensory properties and cosmetic durability, a part or all of the powder components may be treated to be water-repellent by a known method with a substance such as a silicone, a fluorine compound, a metal soap, an oil, or an acyl glutamate.

[0094] Other pharmaceutical ingredients are not particularly limited, and examples thereof include vitamins such as vitamin A oil, retinol, retinol palmitate, inositol, pyridoxine hydrochloride, benzyl nicotinate, nicotinamide, DL-α-tocopherol nicotinate, magnesium ascorbyl phosphate, 2-O-α-D-glucopyranosyl-L-ascorbic acid, vitamin D2 (ergocaciferol), dl-α-tocopherol, dl-α-tocopherol acetate, pantothenic acid, and biotin; hormones such as estradiol and ethinyl estradiol; amino acids such as arginine, aspartic acid, cystine, cysteine, methionine, serine, leucine, and tryptophan; anti-inflammatory agents such as allantoin and azulene, whitening agents such as arbutin; astringents such as tannic acid; cooling agents such as L-menthol and camphor, sulfur, lysozyme chloride, and pyridoxine chloride.

[0095] The cosmetic of the present invention is not particularly limited in its manufacturing method, and may be manufactured by a manufacturing method appropriate for the form of the cosmetic. Specifically, for example, the cosmetic can be obtained by mixing the dispersion of the present invention with other components. EXAMPLES

[0096] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" are by mass, unless otherwise specified.

[0097] (Example of manufacturing raw zinc oxide cake) 80 g of FINEX-50 (manufactured by Sakai Chemical Industry Co., Ltd., primary particle size 0.020 μm) was repulped in 1200 ml of an aqueous zinc acetate solution with a zinc acetate concentration of 0.135 mol / l to form a slurry. The slurry was then heated to 70°C over 42 minutes while stirring, and aged at 70°C for 2 hours while stirring. After aging, it was filtered and washed with water. The obtained solid was then repulped in 3 liters of water to form a slurry, which was heated to 95°C while stirring, and heated and washed at 95°C for 60 minutes while stirring. After heating and washing, it was filtered and washed with water to obtain a zinc oxide cake.

[0098] Example 1 The zinc oxide cake obtained in the manufacturing example was weighed out to a zinc oxide content of 30 g, and repulped in pure water to a powder concentration of 100 g / L to obtain zinc oxide slurry. 0.45 g of 30% caustic soda was added to the pure water and heated to 90°C, and 0.9 g (3.0% relative to zinc oxide) of stearic acid (Fujifilm Wako Pure Chemical Industries, Ltd., stearic acid, plant-derived) was added to obtain an aqueous sodium stearate solution. The aqueous sodium stearate solution (90°C) was added to the zinc oxide slurry heated to 90°C, and the mixture was aged for 2 hours while maintaining the temperature at 90°C. After aging, the mixture was cooled to 70°C, adjusted to pH 7.0 with sulfuric acid, filtered, washed with water, and dried at 120°C for 16 hours to obtain stearic acid-treated zinc oxide particles. The evaluation results of the physical properties of the obtained particles and the physical properties of the coating film are shown in Table 1. The melting point of stearic acid is 70°C.

[0099] Example 2 Stearic acid-treated zinc oxide particles were obtained in the same manner as in Example 1, except that 0.3 g of 30% caustic soda was added to pure water, heated to 90°C, and then 0.6 g of stearic acid (2.0% relative to zinc oxide) was added to obtain an aqueous sodium stearate solution, filtered, washed with water, and then dried at 80°C.

[0100] Example 3 Isostearic acid-treated zinc oxide particles were obtained in the same manner as in Example 1, except that isostearic acid (isostearic acid (mixture of isomers) manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) was used instead of stearic acid. The melting point of isostearic acid is 7°C.

[0101] Example 4 Palmitic acid-treated zinc oxide particles were obtained in the same manner as in Example 1, except that palmitic acid (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) was used instead of stearic acid. The melting point of palmitic acid is 64°C.

[0102] Comparative Example 1 Stearic acid-treated zinc oxide particles were obtained in the same manner as in Example 1, except that they were dried at 80° C. for 16 hours.

[0103] Comparative Example 2 Stearic acid-treated zinc oxide particles were obtained in the same manner as in Example 1, except that the amount of 30% caustic soda was 1.5 g and the amount of stearic acid was 3.0 g (10.0% based on zinc oxide).

[0104] Comparative Example 3 The zinc oxide cake obtained in the Production Example was dried at 120°C for 16 hours to obtain zinc oxide powder. 30 g of the obtained zinc oxide powder was placed in a plastic bag, and 1.2 g of stearic acid (4.0% based on zinc oxide) was added and mixed, and the mixture was heat-treated in a dryer at 120°C for 16 hours to obtain stearic acid-treated zinc oxide particles.

[0105] Comparative Example 4 Stearic acid-treated zinc oxide particles were obtained in the same manner as in Example 1, except that the zinc oxide cake obtained in the production example was changed to FINEX-30 (manufactured by Sakai Chemical Industry Co., Ltd., average particle diameter 35 nm), the amount of 30% caustic soda was changed to 0.6 g, and the amount of stearic acid was changed to 1.2 g (4.0% based on zinc oxide).

[0106] Comparative Example 5 Stearic acid-treated zinc oxide particles were obtained in the same manner as in Example 1, except that 0.45 g of 30% caustic soda was added to the zinc oxide slurry, heated to 40°C, 0.9 g of stearic acid (3.0% relative to zinc oxide) was added, and the mixture was aged for 2 hours while maintaining the temperature at 40°C.

[0107] Comparative Example 6 Isostearic acid-treated zinc oxide particles were obtained in the same manner as in Comparative Example 2, except that stearic acid was changed to isostearic acid.

[0108] (Evaluation method 1) Composition of obtained particles The composition of the obtained particles in Table 1 shows the results of analysis using an X-ray diffraction apparatus, Ultima III (manufactured by Rigaku Corporation), equipped with a copper tube.

[0109] (Evaluation method 2) Primary particle size In this specification, the primary particle diameter is calculated as the average particle diameter of 250 particles randomly selected from a 20,000 to 50,000x field of view in a photograph taken with a transmission electron microscope JEM-1200EX II (manufactured by JEOL Ltd.).

[0110] (Evaluation method 3) BET specific surface area BET specific surface area (m 2 / g) is a value measured using a fully automatic BET specific surface area measuring device Macsorb Model HM-1200 (manufactured by Mountech Co., Ltd.).

[0111] (Evaluation method 4) Carbon content The carbon contents in Table 1 are values ​​measured using a carbon amount measuring device, CARBON ANALYZER EMIA-110 (manufactured by Horiba, Ltd.).

[0112] (Evaluation method 5) Mode diameter In this specification, the mode diameter is a value measured by a laser diffraction / scattering type particle size distribution analyzer LA-960S (manufactured by Horiba, Ltd.). 0.1 g of zinc oxide particles of the examples and comparative examples was placed in 50 ml of isopropyl alcohol, and the slurry was ultrasonically dispersed for 1 minute using an ultrasonic homogenizer US-600E (manufactured by Nippon Seiki Seisakusho, Ltd.), and the slurry was measured. The refractive index of zinc oxide of the examples and comparative examples was set to 2.00, and the refractive index of isopropyl alcohol was set to 1.378, and the measurement was made on a volume basis. When the mode diameter of the slurry ultrasonically dispersed for 1 minute is 0.30 μm or less, it means that the dispersibility is high because many particles close to the primary particle size are present even in a weak dispersion. On the other hand, when the mode diameter exceeds 0.30 μm, it means that the particles are strongly aggregated and the dispersibility is low.

[0113] (Evaluation method 6) Water repellency 80 mL of distilled water was placed in a 100 mL beaker, 0.2 g of fatty acid-treated zinc oxide particles were floated on it, and the water was stirred 10 times with a spatula. The turbidity of the water was visually observed and evaluated according to the following criteria. 〇: The water is clear and transparent △: The water is slightly cloudy and translucent ×: Water is cloudy

[0114] (Evaluation method 7) Apparent density (Apparent density) The measurement was performed according to the method described in JIS K 5101-12-1 Pigment Test Method - Apparent Density or Apparent Specific Volume (Static Method).

[0115] (Evaluation method 8) FT-IR The FT-IR spectra in Figures 1 and 2 were measured using a Fourier transform infrared spectrophotometer FT-IR Nicolet iS 10 (manufactured by Thermo Fisher Scientific) under the following conditions: detector: DTGS KBr, resolution: 4 cm -1 The measurement was performed with 16 scans. The accessory equipment is a single reflection horizontal ATR Smart iTR, the plate (IRE) used is a diamond crystal, and the incidence angle is 45°. The absorbance I1 value is 1350-1500cm -1 Detected in CH3 symmetric bending vibration, COO - The absorbance I2 value of the maximum peak of either the symmetric stretching vibration or the CH3 asymmetric bending vibration is 1500-1600 cm -1 Detected by COO - It is the absorbance value of the maximum peak of the antisymmetric stretching vibration. When the I2 / I1 value is 0.8 to 1.2, it means that the fatty acid is bound to the zinc oxide surface, when it is greater than 1.2, it means that free fatty acid Zn is precipitated, and when it is less than 0.8, it means that the fatty acid is not sufficiently bound to the zinc oxide surface. Furthermore, the absorbance I3 value is 1700-1720cm -1 The absorbance of the C=O stretching vibration peak, absorbance I4, is detected at 1750-1800cm -1This is the absorbance value of the peak of the C=O stretching vibration of four-membered rings, five-membered rings, and acid anhydrides that is detected in the FTIR. Since no substances corresponding to four-membered rings, five-membered rings, or acid anhydrides exist in this manufacturing process, no peaks are detected. Therefore, if the I3 / I4 value exceeds 1.2, it means that unreacted fatty acids remain.

[0116] (Examples 5 to 8 and Comparative Examples 7 to 12) Dispersions of fatty acid-treated zinc oxide particles having the compositions shown in Table 2 were prepared by the manufacturing method described below. Each sample was evaluated for "initial viscosity," "viscosity over time at 40°C," and "stability over time." The results are also shown in Table 2. (Manufacturing method) The fatty acid-treated zinc oxide particles of the Examples and Comparative Examples, polyhydroxystearic acid (Salacos HS-6C, manufactured by Nisshin Oillio Co., Ltd.), and isotridecyl isononanoate (Salacos 913, manufactured by Nisshin Oillio Co., Ltd.) were placed in a mayonnaise bottle in the ratios shown in Table 2, and zirconia beads (0.5 mm, manufactured by Toray Industries, Inc.) were added in an amount twice the total amount of the components, and after thorough mixing, the mixture was fixed to a paint conditioner (manufactured by RED DEVIL Co., Ltd.) and vibrated for 60 minutes to prepare a dispersion. The evaluation results of the physical properties of the obtained dispersion are shown in Table 2.

[0117] (Initial viscosity) After dispersion, the dispersion was placed in a 9 ml screw bottle, and the viscosity (25° C.) was measured 60 seconds after the start of rotation at 12 rpm using a B-type viscometer (Tokyo Keiki Co., Ltd.) with a rotor No. 4.

[0118] (40℃ Viscosity over time) The dispersion was placed in a 9 ml screw bottle and stored in a 40° C. thermostatic chamber for 7 days, and the viscosity was measured 60 seconds after the start of rotation at 12 rpm using a B-type viscometer (Tokyo Keiki Co., Ltd.) with a rotor No. 4.

[0119] (Stability over time) The condition after storage in a 40°C thermostatic chamber for 7 days was evaluated according to the following criteria. ◎: No sedimentation and viscosity less than 1000 mPa s Good: No settling and viscosity is 1000 mPa s or more but less than 2000 mPa s △: No settling and viscosity is 2000 mPa s or more but less than 3000 mPa s ×: Sedimentation or viscosity is 3000 mPa s or more

[0120] [Table 1]

[0121] [Table 2]

[0122] Table 1 shows that the fatty acid-treated zinc oxide particles of the examples have excellent dispersibility and sufficient water repellency. Furthermore, Table 2 shows that there was no significant increase in either the initial viscosity or the viscosity over time, and that the particles have excellent stability.

[0123] Example 9 (Sunscreen O / W Cream) A sunscreen O / W cream was obtained using the ingredients shown in Table 3 below and by the manufacturing method described below. (Manufacturing method) (1) Mix ingredients 1 to 6 uniformly and heat to dissolve. (2) Mix ingredients 7 to 12 evenly and heat. (3) The above (1) was added to the above (2) and emulsified, and then cooled to obtain a sunscreen O / W cream.

[0124] [Table 3] (Note 1) (Sodium acrylate / sodium acryloyldimethyltaurate) copolymer: SIMULGEL EG QD (manufactured by SEPPIC) (Note 2) Plant-derived cellulose (2% aq): RHEOCRYSTA C-2SP (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.)

[0125] The sunscreen O / W cream of Example 9 obtained in the above manner was stable without any change over time, and in terms of the feel in use, it spread well and smoothly on the skin when applied, there was no sticky or squeaky feeling on the skin after application, it was a highly transparent organic UV absorber-free sunscreen O / W cream with excellent durability of sunscreen effect. [Industrial Applicability]

[0126] The dispersion of the present invention can be suitably used by being blended in a cosmetic composition.

Claims

1. In the FT-IR spectrum measured using the attenuated total reflection method (ATR method), -1 The maximum absorbance (I 1 ) at 1500-1600 cm -1 The maximum absorbance (I 2 ) ratio (I 2 / I 1 ) is 0.8 to 1.2, and 1750-1800cm -1 The maximum absorbance (I 4 ) 1700-1720 cm -1 The maximum absorbance (I 3 ) ratio (I 3 / I 4 ) is 1.2 or less; The fatty acid-treated zinc oxide particles are characterized in that the primary particle diameter measured by a transmission electron microscope is 0.1 μm or less, and the powder is placed in isopropyl alcohol, and dispersed by irradiating the powder with ultrasonic waves at a rated output of 600 W and a vibration amplitude of 100% for 1 minute at room temperature, and the mode diameter of the dispersion liquid is 0.30 μm or less on a volume basis as measured by a laser diffraction scattering method.

2. 2. The fatty acid-treated zinc oxide particles according to claim 1, wherein the fatty acid is at least one selected from the group consisting of stearic acid, isostearic acid, and palmitic acid.

3. A step (1) of repulping zinc oxide particles as a raw material in a dispersion medium to prepare a slurry; (2) neutralizing the fatty acid with a base to obtain an aqueous fatty acid salt solution; and The method includes a step (3) of adding the obtained fatty acid salt aqueous solution to the zinc oxide slurry to perform a surface treatment, The zinc oxide particles as the raw material are obtained by a production method including a step of aging fine zinc oxide particles in water having a zinc salt dissolved therein, and are subjected to step (1) without a drying step, The method for producing fatty acid-treated zinc oxide particles, wherein the steps (2) and (3) are carried out at a temperature equal to or higher than the melting point of the fatty acid.

4. The method for producing fatty acid-treated zinc oxide particles according to claim 3, wherein the raw material zinc oxide particles are dispersed by placing the powder in a 0.0025 mass% aqueous solution of sodium hexametaphosphate and irradiating it with ultrasonic waves at a rated output of 600 W and a vibration amplitude of 100% for 3 minutes at room temperature, and the resulting dispersion has a median diameter of 0.30 μm or less as measured by a laser diffraction scattering method.

5. A dispersion comprising the fatty acid-treated zinc oxide particles according to claim 1 or 2.

6. A cosmetic preparation comprising the fatty acid-treated zinc oxide particles according to claim 1 or 2.

Citation Information

Patent Citations

  • Production method of surface-coated zinc oxide particle

    JP2016196381A

  • Seedling transplanter

    JP2021083334A