Surface coated cutting tool
A multi-layered hard coating structure for cutting tools, with specific orientations and compositions, addresses the wear resistance and self-destruction issues of existing coatings, enhancing chipping resistance and wear resistance for improved cutting efficiency.
Patent Information
- Application Number
- JP2023056991
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing hard coatings for cutting tools, such as AlCrN-based coatings, face issues with wear resistance due to strong (111) orientation leading to increased compressive residual stress and self-destruction, particularly in TiSiN layers.
A surface-coated cutting tool with a multi-layered hard coating structure comprising a lower layer preferentially oriented in the (111) plane, an intermediate layer with alternating AlCrN and AlCrXN films, and an upper TiSiN layer oriented in the (200) plane, with controlled nitrogen content and grain sizes to alleviate lattice mismatch and residual stress.
The multi-layered coating enhances chipping resistance and wear resistance, improving cutting efficiency and tool lifespan by suppressing self-destruction and abnormal damage.
Smart Images

Figure 2024144847000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface-coated cutting tool. [Background technology]
[0002] Conventionally, AlCrN-based hard coatings have been known as hard coatings for cutting tools. The cutting tool disclosed in Patent Document 1 has a wear-resistant hard coating structure on at least a part of the substrate surface, and has a composition (Al 1-a-b-c Cr a B b Z c ) at least one layer of X, where X is at least one of N, C, CN, NO, CO, and CNO; and Z is at least one of W, Mo, Ta, and Nb, where each composition is in an atomic ratio of 0.2. <a≦0.5、0.01<b≦0.2、0.001≦c≦0.04である。 The hard-coated cutting tool disclosed in Patent Document 2 has a hard coating layer 1 on the cemented carbide substrate side and a hard coating layer 2 on the surface side. The composition of the hard coating layer 1 is (Al a Cr 1-a ) 1-x N x (The element content is expressed as 0.5≦a<0.7, 0.48≦x≦0.52 in atomic ratio.) The peak intensity I r , (200) plane peak intensity I s When I s / I r <1. The composition of the hard coating layer 2 is (Ti 1-b S b ) 1-y N y (The element content is expressed as 0.01≦b≦0.15, 0.48≦y≦0.52 in atomic ratio. The peak intensity I u , (200) plane peak intensity I v When I v / I u <1. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2008 / 037556 [Patent Document 2] JP 2012-045650 A Summary of the Invention [Problem to be solved by the invention]
[0004] The coating structure described in Patent Document 1 exhibits wear resistance due to its strong (111) orientation, but the wear resistance can be further enhanced by forming a TiSiN layer with excellent hardness as a surface layer as described in Patent Document 2. However, the coating described in Patent Document 2 has a problem in that the strong (111) orientation in the TiSiN layer increases compressive residual stress, making the coating prone to self-destruction. [Means for solving the problem]
[0005] (1) According to the present disclosure, there is provided a surface-coated cutting tool including a substrate and a hard coating formed on a surface of the substrate, the hard coating having a lower layer formed on the substrate and made of an alternating laminate film of an A layer and a B layer, an intermediate layer formed on the lower layer and made of an alternating laminate film of a C layer and a D layer, and an upper layer formed on the intermediate layer, the lower layer A layer having a composition formula: (Al a Cr 1-a ) v N 1-v The composite nitride layer has an average composition satisfying 0.50≦a≦0.75 and 0.40≦v≦0.55 when expressed by the formula: b Cr c X 1-b-c ] w N 1-wA composite nitride layer having an average composition satisfying 0.40≦b<0.75, 0.25≦c<0.6, 0<1-bc≦0.1, and 0.40≦w≦0.55 when expressed as (X is one or more elements selected from the group 4a, 5a, and 6a elements of the periodic table, and B and Si), wherein the lower layer has a crystal structure preferentially oriented to a (111) plane of a face-centered cubic structure, the upper layer has a crystal structure preferentially oriented to a (200) plane of a face-centered cubic structure, the arithmetic mean value of the nitrogen contents of the intermediate layers C and D is smaller than the arithmetic mean value of the nitrogen contents of the lower layers A and B, and the intermediate layer C has a composition formula: (Al d Cr 1-d ) x N 1-x The intermediate layer D is a composite nitride layer having an average composition satisfying 0.5≦d≦0.7 and 0.40≦x≦0.55 when expressed by the formula: [Al e Cr f X 1-e-f ] y N 1-y (X is one or more elements selected from the group consisting of elements of Groups 4a, 5a, and 6a of the periodic table, and B and Si), the upper layer is a composite nitride layer having an average composition satisfying 0.5≦e<0.7, 0.3≦f<0.5, 0<1-ef≦0.1, and 0.40≦y≦0.55, g S 1-g ) z N 1-z The present invention provides a surface-coated cutting tool, wherein the composite nitride layer has an average composition satisfying, when expressed as g, 0.60≦g≦0.95 and 0.35≦z≦0.50.
[0006] (2) In (1), the average length L of the crystal grains in the direction parallel to the substrate surface of the intermediate layer L1 and the average length L of the crystal grains in a direction parallel to the substrate surface of the lower layer. L2 But, L L1 ≦10nm, 10nm≦L L2 ≦200nm, L L1 <L L2 It may be configured to satisfy the following.
[0007] (3) In (1) or (2), the lower layer may have a total thickness of 0.7 μm to 3.0 μm, the lower layer A may have a thickness of 3 nm to 100 nm, the lower layer B may have a thickness of 3 nm to 100 nm, the intermediate layer may have a total thickness of 0.1 μm to 4.0 μm, the intermediate layer C may have a thickness of 2 nm to 50 nm, the intermediate layer D may have a thickness of 2 nm to 50 nm, the upper layer may have a thickness of 0.1 μm to 2.0 μm, and the hard coating may have a total thickness of 1.0 μm to 10.0 μm.
[0008] (4) In any one of (1) to (3), the lower layer and the intermediate layer may have an X-ray diffraction peak intensity ratio I(200) / I(111) of a (200) plane to a (111) plane of 0.01 or more and 0.50 or less, and the upper layer may have an X-ray diffraction peak intensity ratio I(200) / I(111) of a (200) plane to a (111) plane of 1 or more and 100 or less.
[0009] (5) In any one of (1) to (4), the average length of the crystal grains in the intermediate layer in the direction perpendicular to the substrate surface is L V1 , the average length of the crystal grains in the direction parallel to the substrate surface is L L1 , ratio L V1 / L L1 m, and the average length of the crystal grains in the lower layer in the direction perpendicular to the substrate surface is L V2 , the average length of the crystal grains in the direction parallel to the substrate surface is L L2 , ratio L V2 / L L2 The configuration may be such that m / n satisfies 0.01≦m / n≦0.50, where m is the number of adjacent elements. Effect of the Invention
[0010] According to one aspect of the present invention, there is provided a surface-coated cutting tool that is provided with a hard coating having excellent chipping resistance and that can improve the efficiency of cutting processing. [Brief description of the drawings]
[0011] [Figure 1]FIG. 1 is a schematic diagram showing a cross-sectional structure of a surface-coated cutting tool according to an embodiment. [Diagram 2] FIG. 2 is a diagram showing an example of an X-ray diffraction profile of the hard coating of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, the surface-coated cutting tool according to the embodiment will be described in detail. In this specification and claims, when a numerical range is expressed as "L to M" (where L and M are both numerical values), the range includes an upper limit value (M) and a lower limit value (L), and the upper limit value (M) and the lower limit value (L) have the same units.
[0013] FIG. 1 is a schematic diagram showing a cross-sectional structure of a surface-coated cutting tool according to an embodiment. The surface-coated cutting tool 1 of this embodiment has a substrate 10 and a hard coating 20 formed on the surface of the substrate 10. The hard coating 20 is configured by laminating a lower layer 21, an intermediate layer 22, and an upper layer 23 in this order from the substrate 10 side.
[0014] The lower layer 21 is made of an alternately laminated film of an A layer made of an AlCrN film and a B layer made of an AlCrXN film (X is one or more elements selected from the group consisting of elements in groups 4a, 5a, and 6a of the periodic table, B (boron), and Si). The intermediate layer 22 is made of an alternating laminate film of a C layer made of an AlCrN film and a D layer made of an AlCrX'N film (X' is one or more elements selected from the group consisting of elements in groups 4a, 5a, and 6a of the periodic table, B (boron), and Si). The upper layer 23 is made of a TiSiN film.
[0015] Various conventionally known tool substrates can be used for the substrate 10. For example, cemented carbide (WC-based cemented carbide, WC, Co, and carbonitrides of Ti, Ta, Nb, etc.), cermet (mainly composed of TiC, TiN, TiCN, etc.), ceramics (titanium carbide, silicon carbide, silicon nitride, aluminum nitride, aluminum oxide, etc.), cBN sintered body, etc. can be used.
[0016] The hard coating 20 may include layers other than the lower layer 21, the intermediate layer 22, and the upper layer 23. For example, a layer for improving the adhesion between the lower layer 21 and the substrate 10, or a layer for improving the crystallinity of the lower layer 21 may be formed between the lower layer 21 and the substrate 10. For example, an AlCrN film may be formed as a base layer between the substrate 10 and the lower layer 21. Also, for example, another layer made of a nitride or carbonitride may be formed on the upper layer 23.
[0017] The total thickness of the hard coating 20 is preferably 1.0 μm or more and 10.0 μm or less. If the total thickness of the hard coating 20 is less than 1.0 μm, it is difficult to obtain sufficient wear resistance over a long period of time. If the total thickness of the hard coating 20 exceeds 10.0 μm, abnormal damage such as chipping and peeling is likely to occur.
[0018] The A layer of the lower layer 21 has the composition formula: (Al a Cr 1-a ) v N 1-v When expressed as above, it is an Al and Cr composite nitride layer having an average composition that satisfies 0.50≦a≦0.75 and 0.3≦v≦0.6 (where a is the Al content ratio in atomic ratio, and v is the total content ratio of metals and metalloids in atomic ratio). When the a value (atomic ratio) indicating the Al content ratio is less than 0.50, the wear resistance decreases due to the decrease in the Al content ratio. On the other hand, when the a value (atomic ratio) exceeds 0.75, the hardness decreases due to the appearance of crystal grains with a hexagonal structure due to the increase in the relative Al content ratio, and the wear resistance also decreases. The value of a is preferably 0.60 or more, and 0.70 or less. The v value indicates the ratio of metal and metalloid elements to nitrogen in the lower layer 21. If the v value is less than 0.40, the residual stress in the lower layer 21 increases, and the chipping resistance is likely to decrease. If the v value exceeds 0.55, the wear resistance is likely to decrease.
[0019] The B layer of the lower layer 21 has the composition formula: [Al b Cr c X 1-b-c ] w N 1-w When expressed as (X is one or more elements selected from the elements of Groups 4a, 5a, and 6a of the periodic table, and B and Si), it has an average composition that satisfies 0.40≦b<0.7, 0.2≦c<0.6, 0<1-bc≦0.1, and 0.3≦w≦0.6 (where b is the atomic ratio of the Al content, c is the atomic ratio of the Cr content, and w is the atomic ratio of the total content of metal and metalloid elements). Layer B is a layer mainly composed of a composite nitride of Al and Cr with element X added.
[0020] The reasons for setting the b value and c value within the above ranges are the same as those for setting the b value. The b value is preferably 0.50 or more. The b value is preferably 0.60 or less. The c value is preferably 0.35 or more. The c value is preferably 0.50 or less. The w value indicates the ratio of metal and metalloid elements to nitrogen in the B layer. If the w value is less than 0.40, the residual stress in the B layer increases, and the chipping resistance is likely to decrease. If the w value exceeds 0.55, the wear resistance is likely to decrease.
[0021] The element X is one or more elements selected from the elements of Groups 4a, 5a, and 6a of the periodic table, B, and Si, such as B (boron), Si, W, Mo, Ta, Zr, and Nb. By setting the content ratio of the element X within the above range, it becomes easier to preferentially orient the B layer in the (111) plane. This makes it easier to preferentially orient the entire lower layer 21, in which the A layer and the B layer are alternately laminated at the nano level, in the (111) plane. The content ratio (1-bc) of the element X is a value exceeding 0 in atomic ratio.
[0022] The content ratio of element X (1-bc) preferably satisfies 0.004≦1-bc≦0.10. If the content ratio of element X is less than 0.004 in atomic ratio, it becomes difficult to obtain the effect of adding element X. If the content ratio of element X exceeds 0.10 in atomic ratio, the toughness or hardness of the hard coating is likely to decrease.
[0023] The lower layer 21 is an alternating laminate film in which an A layer made of an AlCrN film and a B layer made of an AlCrXN film are alternately laminated. The thickness of each A layer is preferably 3 nm or more and 100 nm or less. The thickness of each B layer is preferably 3 nm or more and 100 nm or less. By setting the thickness within such a range, the lattice mismatch between the A layer and the B layer can be alleviated, and the toughness of the alternating laminate film as a whole can be improved. The thickness of each of the layers A and B is preferably 3 nm or more, and the thickness of each of the layers A and B is preferably 10 nm or less.
[0024] The total thickness of the lower layer 21 is preferably 0.7 μm or more and 3.0 μm or less. If the total thickness of the lower layer 21 is less than 0.7 μm, it is difficult to obtain sufficient wear resistance over a long period of time. If the total thickness of the lower layer 21 exceeds 3.0 μm, abnormal damage such as chipping and peeling is likely to occur. The total thickness of the lower layer 21 is preferably 0.8 μm or more. The total thickness of the lower layer 21 is preferably 1.5 μm or less.
[0025] The C layer of the intermediate layer 22 has the composition formula: (Al d Cr 1-d ) x N 1-x When expressed as above, it is a composite nitride layer of Al and Cr having an average composition that satisfies 0.5≦d≦0.7 and 0.40≦x≦0.55 (where b is the content ratio of Al in atomic ratio, and x is the total content ratio of metals and metalloids in atomic ratio). When the d value (atomic ratio) indicating the content ratio of Al is less than 0.5, the wear resistance decreases due to the decrease in the content ratio of Al. On the other hand, when the d value (atomic ratio) exceeds 0.7, the hardness decreases due to the appearance of crystal grains with a hexagonal structure due to the increase in the relative content ratio of Al, and the wear resistance also decreases. The d value is preferably 0.60 or more, and 0.70 or less. The x value indicates the ratio of metal and metalloid elements to nitrogen in the C layer. If the x value is less than 0.40, the residual stress in the C layer increases, and the chipping resistance is likely to decrease. If the x value exceeds 0.55, the wear resistance is likely to decrease.
[0026] The D layer of the intermediate layer 22 has the composition formula: [Al e Cr f X' 1-e-f ] y N 1-y When expressed as (X' is one or more elements selected from the elements of Groups 4a, 5a, and 6a of the periodic table, and B and Si), it has an average composition that satisfies 0.5≦e<0.7, 0.2≦f<0.5, 0<1-ef≦0.1, and 0.40≦y≦0.55 (where e is the Al content by atomic ratio, f is the Cr content by atomic ratio, and y is the total content by atomic ratio of metal and semi-metal elements). Layer D is a layer mainly composed of a composite nitride of Al and Cr with element X' added.
[0027] The reasons for setting the e value and f value in the above ranges are the same as those for setting the d value. The e value is preferably 0.55 or more. The e value is preferably 0.6 or less. The f value is preferably 0.25 or more. The f value is preferably 0.45 or less. The y value indicates the ratio of metal and metalloid elements to nitrogen in the D layer. If the y value is less than 0.40, the residual stress in the D layer increases, and the chipping resistance is likely to decrease. If the y value exceeds 0.55, the wear resistance is likely to decrease.
[0028] The element X' is one or more elements selected from the elements of Groups 4a, 5a, and 6a of the periodic table, B, and Si, such as B (boron), Si, W, Mo, Ta, Zr, and Nb. By setting the content ratio of the element X' within the above range, it becomes easier to preferentially orient the D layer to the (111) plane. This makes it easier to preferentially orient the entire intermediate layer 22, in which the C layer and the D layer are alternately laminated at the nano level, to the (111) plane. The content ratio (1-ef) of the element X' is a value exceeding 0 in atomic ratio.
[0029] The content ratio of element X' (1-ef) preferably satisfies 0.005≦1-ef≦0.10. If the content ratio of element X' is less than 0.005 in atomic ratio, it becomes difficult to obtain the effect of adding element X. If the content ratio of element X' exceeds 0.10 in atomic ratio, the toughness or hardness of the hard coating is likely to decrease.
[0030] The intermediate layer 22 is an alternating laminate film in which C layers made of AlCrN films and D layers made of AlCrX'N films are alternately laminated. The thickness of each C layer is preferably 2 nm to 50 nm. The thickness of each D layer is preferably 2 nm to 50 nm. By setting the thickness within such a range, the lattice mismatch between the C layers and the D layers can be alleviated, and the toughness of the alternating laminate film as a whole can be improved. The thickness of each of the layers C and D is preferably 3 nm or more, and the thickness of each of the layers C and D is preferably 40 nm or less.
[0031] The total thickness of the intermediate layer 22 is preferably 0.1 μm or more and 4.0 μm or less. If the total thickness of the intermediate layer 22 is less than 0.1 μm, it is difficult to obtain sufficient chipping resistance over a long period of time. If the total thickness of the intermediate layer 22 exceeds 4.0 μm, it becomes more susceptible to wear. The total thickness of the intermediate layer 22 is preferably 0.15 μm or more. The total thickness of the intermediate layer 22 is preferably 3.0 μm or less.
[0032] The upper layer 23 has the composition formula: (Ti g S 1-g ) z N1-z When expressed as above, it is a composite nitride layer of Ti and Si having an average composition that satisfies 0.60≦g≦0.95 and 0.35≦z≦0.50 (where g indicates the content ratio of Ti in atomic ratio, and z indicates the total content ratio of metals and metalloids in atomic ratio). By forming the upper layer 23 made of a nitride containing Ti and Si, the chipping resistance of the hard coating 20 is improved. If the g value is less than 0.60, the effect of improving the chipping resistance is reduced. If the g value exceeds 0.95, the lattice distortion becomes large and the upper layer 23 becomes more likely to peel off. The g value is preferably 0.85 or more. The g value is preferably 0.95 or less. The z value indicates the ratio of metal and metalloid elements to nitrogen in the upper layer 23. If the z value is less than 0.35, the residual stress in the upper layer 23 increases, and the chipping resistance is likely to decrease. If the z value exceeds 0.50, the wear resistance is likely to decrease.
[0033] The thickness of the upper layer 23 is preferably 0.1 μm or more and 2.0 μm or less. If the thickness of the upper layer 23 is less than 0.1 μm, it is difficult to obtain sufficient wear resistance over a long period of time. If the thickness of the upper layer 23 exceeds 2.0 μm, abnormal damage such as chipping and peeling is likely to occur. The thickness of the upper layer 23 is preferably 0.12 μm or more. The thickness of the upper layer 23 is preferably 1.8 μm or less.
[0034] In the hard coating 20, the crystal structure of the lower layer 21 is a face-centered cubic structure as determined by X-ray diffraction, and is preferentially oriented along the (111) plane, while the crystal structure of the upper layer 23 is a face-centered cubic structure as determined by X-ray diffraction, and is preferentially oriented along the (200) plane. Usually, when a TiSiN film is formed on an AlCrN film preferentially oriented in the (111) plane, the TiSiN film is preferentially oriented in the (111) plane. In this embodiment, by controlling the film formation apparatus and film formation conditions when forming the upper layer 23 made of the TiSiN film, a TiSiN film (upper layer 23) preferentially oriented in the (200) plane is formed on the AlCrN film preferentially oriented in the (111) plane. In this way, the upper layer 23 can be formed of a TiSiN film with a (200) orientation that has excellent deformability, and a surface-coated cutting tool with excellent chipping resistance can be obtained.
[0035] By making the TiSiN film of the upper layer 23 (200) oriented, self-destruction due to residual stress of the upper layer 23 can be suppressed, but since there is a relatively large lattice mismatch between the (111) oriented AlCrN film and the (200) oriented TiSiN film, there is a risk that self-destruction of the upper layer 23 due to the lattice mismatch may occur with only the combination of the lower layer 21 and the upper layer 23. Therefore, in this embodiment, the intermediate layer 22 is formed between the lower layer 21 and the upper layer 23. This can reduce the lattice mismatch between the lower layer 21 and the upper layer 23, and can suppress self-destruction of the upper layer 23 due to the lattice mismatch.
[0036] In this embodiment, the nitrogen content of the intermediate layer 22 is smaller than the nitrogen content of the lower layer 21. In addition, the average length of the crystal grains in the direction parallel to the substrate surface of the intermediate layer 22 is smaller than the average length of the crystal grains in the direction parallel to the substrate surface of the lower layer 21. Since the nitrogen content of intermediate layer 22 is low, intermediate layer 22 is a layer rich in metal components, and is therefore more susceptible to deformation than lower layer 21. As a result, intermediate layer 22 can mitigate deformation of upper layer 23, and self-destruction of upper layer 23 can be suppressed. Since intermediate layer 22 is a layer made of finer crystal grains than lower layer 21, grain boundary sliding of crystals is likely to occur in intermediate layer 22. This also makes it possible to reduce deformation of upper layer 23 and suppress self-destruction of upper layer 23. As described above, according to this embodiment, a surface-coated cutting tool having excellent chipping resistance and wear resistance can be obtained.
[0037] In the surface-coated cutting tool of this embodiment, the average length L of the crystal grains in the intermediate layer 22 in the direction parallel to the substrate surface is L1 and the average length L of the crystal grains in the direction parallel to the substrate surface of the lower layer 21. L2 But, L L1 ≦10nm, 10nm≦L L2 ≦200nm, L L1 <L L2 It is preferable to satisfy the following: The average length L of the crystal grains in the intermediate layer 22 in a direction parallel to the substrate surface L1 In this method, a cross-sectional image of the hard coating is obtained using a scanning electron microscope (SEM) or a transmission electron microscope (TEM), and image analysis software (such as ImageJ, manufactured by the National Institutes of Health, USA) is used to match the length indicated by the scale bar outputted with the image with the number of pixels on the screen. After that, in the image analysis software, a line is drawn to connect the endpoints of the crystal grains in a direction parallel to the substrate surface, and the length of the line converted from the number of pixels on the line is calculated as the average length of the crystal grains. The average length of the crystal grains is the arithmetic mean value of the lengths of the crystal grains obtained above. The average length L of the crystal grains in the lower layer 21 in the direction parallel to the substrate surface L2 corresponds to the grain width. The average length L L2 can be calculated by the same method as above using image analysis software. However, the average length L L2 In calculating the grain length, a line for measuring the grain width is drawn in a direction parallel to the substrate surface to obtain the grain length.
[0038] The average length of the crystal grains in the intermediate layer 22 in the direction perpendicular to the substrate surface is L V1 , the average length of the crystal grains in the direction parallel to the substrate surface is L L1 , ratio L V1 / L L1 m, and the average length of the crystal grains in the lower layer 21 in the direction perpendicular to the substrate surface is L V2 , the average length of the crystal grains in the direction parallel to the substrate surface is LL2 , ratio L V2 / L L2 When m / n is n, it is preferable that 0.01≦m / n≦0.50 is satisfied. Average grain length L perpendicular to the substrate surface V1 , L V2 is the average length L of the grains in the intermediate layer parallel to the substrate surface. L1 It can be calculated in the same manner as the calculation of the average length L V1 , L V2 In calculating the grain length, a line for measuring the grain width is drawn in a direction perpendicular to the substrate surface to obtain the grain length.
[0039] In the surface-coated cutting tool of this embodiment, it is preferable that the ratio I(200) / I(111) of the X-ray diffraction peak intensity I(200) of the (200) plane of the lower layer 21 and intermediate layer 22 collectively to the X-ray diffraction peak intensity I(111) of the (111) plane is 0.01 or more and 0.50 or less. In the upper layer 23, the ratio I(200) / I(111) of the X-ray diffraction peak intensity I(200) of the (200) plane to the X-ray diffraction peak intensity I(111) of the (111) plane is preferably 1 or more and 100 or less.
[0040] The composition and film thickness of each layer constituting the hard coating 20, the film thickness of each layer of the alternating laminate film, and the total film thickness can be measured by cross-sectional measurement of a longitudinal section of the hard coating perpendicular to the substrate surface using a scanning electron microscope (SEM), a transmission electron microscope (TEM), or energy dispersive X-ray spectroscopy (EDS). Here, the substrate surface is the reference line of the interface roughness between the substrate 10 (tool substrate) and the hard coating layer in the observation image of the cross section. That is, when the tool substrate has a flat surface like an insert, element mapping is performed on the longitudinal section using EDS, and the obtained element map is subjected to known image processing to determine the interface between the lower layer 21 and the tool substrate. The average line is arithmetically obtained for the roughness curve of the interface between the lower layer 21 and the tool substrate thus obtained, and this is taken as the surface of the tool substrate. Then, the direction perpendicular to this average line is taken as the direction perpendicular to the tool substrate. Even if the tool substrate has a curved surface like a drill, if the tool diameter is sufficiently large compared to the layer thickness of the hard coating, the interface between the hard coating and the tool substrate in the measurement region will be approximately flat, so the surface of the tool substrate can be determined by a similar method. That is, for example, in the case of a drill, element mapping is performed using EDS on a longitudinal section of the hard coating perpendicular to the axial direction, the obtained element map is subjected to known image processing to determine the interface between the lower layer 21 and the tool base, and the average line is arithmetically determined for the roughness curve of the interface between the lower layer 21 and the tool base thus obtained, which is regarded as the surface of the tool base. The direction perpendicular to this average line is regarded as the direction perpendicular to the tool base. The measurement area in the longitudinal section is set so as to include the entire area in the thickness direction of the hard coating. In consideration of the total layer thickness of the hard coating and the measurement accuracy of the layer thickness, it is preferable to observe and measure multiple fields of view (e.g., three fields of view) with a field of view of about 10 μm × 10 μm.
[0041] The crystal structure of each layer constituting the hard coating 20 can be measured using X-ray diffraction (XRD) and electron backscattered diffraction pattern (EBSD). For example, the crystal structure of each layer constituting the hard coating 20 is identified by electron beam diffraction using a transmission electron microscope (TEM) to confirm that the crystal structure of each of the lower layer 21, the intermediate layer 22, and the upper layer 23 is a NaCl type face-centered cubic structure. X-ray diffraction is performed using Cu-Kα radiation by a 2θ / θ focusing method. FIG. 2 shows an example of an X-ray diffraction profile of the hard coating 20 of this embodiment. A (111) diffraction line that collectively includes the lower layer 21 and the intermediate layer 22 can be confirmed at around 37.5 degrees, a (111) diffraction line of the upper layer 23 can be confirmed at around 36.5 degrees, a (200) diffraction line that collectively includes the lower layer 21 and the intermediate layer 22 can be confirmed at around 43.5 degrees, and a (200) diffraction line of the upper layer 23 can be confirmed at around 42 degrees. The peaks at around 36 degrees and 48 degrees are due to hexagonal WC. EXAMPLES
[0042] As the substrate, a drill-shaped tool substrate made of WC cemented carbide with a tool diameter of φ0.8 mm was prepared. On the above tool substrate, hard coatings having the configurations shown in the following Tables 1 to 3 were formed. Table 1 shows the configuration of the lower layer, Table 2 shows the configuration of the intermediate layer, and Table 3 shows the configuration of the upper layer.
[0043] (Hard coating of the example) In this example, a sputtering device capable of mounting 12 sputter evaporation sources was used. An AlCr alloy target, an AlCrBW alloy target, and a TiSi alloy target were installed in the device as evaporation sources. The target used had a dimension of Φ16 cm and a thickness of 12 mm. The tool base was fixed to a sample holder in the sputtering device, and a bias power supply was connected to the tool base. The bias power supply is structured to apply a negative bias voltage to the tool base independently of the target. The tool base rotates at two revolutions per minute and revolves around the fixing jig and the sample holder. Ar and N2 were used as the introduced gases, and were introduced from a gas supply port provided in the sputtering device.
[0044] <Bombardment Processing> First, before the tool substrate was coated with a hard coating, the tool substrate was bombarded in the following manner. The sputtering device was heated for 30 minutes at a furnace temperature of 430°C using a heater in the sputtering device. The sputtering device was then evacuated to a vacuum and the furnace pressure was adjusted to 0.05 Pa or less. Ar gas was then introduced into the sputtering device furnace to adjust the furnace pressure to 0.55 Pa. A DC bias voltage of -200 V was then applied to the tool, and cleaning (bombardment) of the tool was performed using Ar ions.
[0045] <Deposition of lower and middle layers> Next, a lower layer and an intermediate layer made of layer-by-layer films were coated on the tool substrate by the following procedure. While the temperature inside the furnace was kept at 430°C, Ar gas was introduced into the furnace of the sputtering device at 360 sccm, and then N2 gas was introduced at 380 sccm to set the pressure inside the furnace to 0.70 Pa. A DC bias voltage of -50 V was applied to the tool, and the discharge time per cycle of the power applied to the alloy target containing Al and Cr and the alloy target containing Al, Cr, B, and W was set to 0.2 milliseconds. Power was applied continuously while switching between three AlCr-based alloy targets and three AlCrBW-based alloy targets, and a lower layer consisting of an alternating laminated film having a thickness of 0.9 μm was coated on the underlayer. Thereafter, the N2 gas flow rate was changed to 250 sccm, and the pressure inside the furnace was set to 0.55 Pa. Film formation was continued under these conditions, and an intermediate layer made of an alternating laminate film with a thickness of 0.1 μm was formed on the lower layer made of an alternating laminate film of AlCrN and AlCrBWN.
[0046] <Deposition of upper layer> A hard coating was then coated on the intermediate layer in the following manner. While the temperature inside the furnace was kept at 430° C., Ar gas was introduced into the furnace of the sputtering device at 360 sccm, and then N2 gas was introduced at 170 sccm to set the pressure inside the furnace to 0.5 Pa. A DC bias voltage of −70 V was applied to the tool, and the discharge time per cycle of the power applied to the alloy target containing Ti and Si was set to 4.5 ms. Power was applied continuously while switching between six TiSi-based alloy targets, and a hard coating having a thickness of about 0.1 μm was coated on the intermediate layer 22.
[0047] (Hard coating of comparative example) The hard coatings of the comparative examples were formed using the same equipment as in Examples 1 to 3, and in the same steps as in the examples up to the formation of the underlayer. In Comparative Examples 1 and 2, the coatings were formed under conditions that prevented the formation of some layers. In Comparative Example 3, the coating was formed without using an alloy target containing Al, Cr, B, and W. In Comparative Examples 4 to 8, the coatings were formed by changing the composition of the alloy target used.
[0048] [Table 1]
[0049] [Table 2]
[0050] [Table 3]
[0051] [Table 4]
[0052] [Table 5]
[0053] (evaluation) Using the surface-coated cutting tools of each sample prepared, drilling was performed under the conditions shown in Table 6 below. Table 7 shows the tool life of each sample when the life of the surface-coated cutting tool of Comparative Example 1, which is a control sample, is taken as 100. All of the samples of this example had excellent tool life compared to samples in which a drill base of the same shape was coated with a conventional coating. The surface-coated cutting tool of this example had a life of up to 150% compared to the surface-coated cutting tool of the comparative example prepared using a base of the same shape. On the other hand, Comparative Examples 1 and 2 in which some layers were omitted, Comparative Example 3 in which the intermediate layer was a single layer of AlCrN, and Comparative Examples 4 to 8 in which the composition range was outside the range of the present invention all showed results inferior to the samples of the present invention.
[0054] [Table 6]
[0055] [Table 7] [Explanation of symbols]
[0056] 1...Surface coated cutting tool, 10...Base, 20...Hard coating, 21...Lower layer, 22...Middle layer, 23...Upper layer
Claims
1. A surface-coated cutting tool comprising a substrate and a hard coating formed on a surface of the substrate, the hard coating has a lower layer formed on the substrate and made of an alternate laminate film of an A layer and a B layer, an intermediate layer formed on the lower layer and made of an alternate laminate film of a C layer and a D layer, and an upper layer formed on the intermediate layer, The lower A layer has the composition formula: (Al a Cr 1-a ) v N 1-v a composite nitride layer having an average composition satisfying 0.50≦a≦0.75 and 0.40≦v≦0.55, The lower layer B has the composition formula: [Al b Cr c X' 1-b-c ] w N 1-w (X' is one or more elements selected from the group consisting of elements in Groups 4a, 5a, and 6a of the periodic table, and B and Si), a composite nitride layer having an average composition that satisfies 0.40≦b<0.7, 0.2≦c<0.6, 0<1-b-c≦0.1, and 0.40≦w≦0.55, the lower layer has a crystal structure preferentially oriented along a (111) plane of a face-centered cubic structure, and the upper layer has a crystal structure preferentially oriented along a (200) plane of a face-centered cubic structure; the arithmetic average value of the nitrogen content of the intermediate layer C and the intermediate layer D is smaller than the arithmetic average value of the nitrogen content of the lower layer A and the lower layer B, The intermediate layer C has the composition formula: (Al d Cr 1-d ) x N 1-x wherein the average composition satisfies 0.5≦d≦0.7 and 0.40≦x≦0.55, The intermediate layer D has the composition formula: [Al e Cr f X 1-e-f ] y N 1-y(X is one or more elements selected from the group consisting of elements in groups 4a, 5a, and 6a of the periodic table, and B and Si), a composite nitride layer having an average composition that satisfies 0.5≦e<0.7, 0.2≦f<0.5, 0<1−e−f≦0.1, and 0.40≦y≦0.55, The upper layer has the composition formula: (Ti g S 1-g ) z N 1-z When expressed by the formula (I), it is a composite nitride layer having an average composition satisfying 0.60≦g≦0.95 and 0.35≦z≦0.
50. Surface coated cutting tools.
2. The average length L of the crystal grains in the direction parallel to the substrate surface of the intermediate layer L1 and the average length L of the crystal grains in a direction parallel to the substrate surface of the lower layer. L2 But, L L1 ≦10 nm, 10 nm≦L L2 ≦200 nm, L L1 <L L2 Satisfying The surface-coated cutting tool according to claim 1 .
3. The total thickness of the lower layer is 0.7 μm or more and 3.0 μm or less, the lower layer A has a thickness of 3 nm or more and 100 nm or less; the lower layer B has a thickness of 3 nm or more and 100 nm or less; The total thickness of the intermediate layer is 0.1 μm or more and 4.0 μm or less, the thickness of the intermediate layer C is 2 nm or more and 50 nm or less; the thickness of the intermediate layer, D layer, is 2 nm or more and 50 nm or less; The thickness of the upper layer is 0.1 μm or more and 2.0 μm or less, The total thickness of the hard coating is 1.0 μm or more and 10.0 μm or less.
3. The surface-coated cutting tool according to claim 1 or 2.
4. a ratio I(200) / I(111) of X-ray diffraction peak intensities of a (200) plane and a (111) plane of the lower layer and the intermediate layer as a whole is 0.01 or more and 0.50 or less, the ratio I(200) / I(111) of the X-ray diffraction peak intensities of the (200) and (111) planes of the upper layer is 1 or more and 100 or less; 3. The surface-coated cutting tool according to claim 1 or 2.
5. The average length of the crystal grains in the intermediate layer in the direction perpendicular to the substrate surface is L V1 , the average length of the crystal grains in the direction parallel to the substrate surface is L L1 , ratio L V1 / L L1 Let m be the The average length of the crystal grains in the lower layer in the direction perpendicular to the substrate surface is L V2 , the average length of the crystal grains in the direction parallel to the substrate surface is L L2 , ratio L V2 / L L2 When n is taken as The relationship 0.01≦m / n≦0.50 is satisfied.
3. The surface-coated cutting tool according to claim 1 or 2.
Citation Information
Patent Citations
Hard film-coated cutting tool
JP2012045650A
Workpiece with hard coating
WO2008037556A2
Cited By
Surface coated cutting tools
JP2026512133A
Hard coating film and tool coated with hard coating film
WO2026140236A1