Slide member
A sliding member with a porous metal and PTFE/MoS2 layer maintains consistent friction forces despite wear, addressing the wear-induced friction force variation in shock absorbers for improved automotive comfort and stability.
Patent Information
- Application Number
- JP2023057229
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing sliding members for shock absorbers in automobiles fail to maintain a minimal difference between static and dynamic friction forces as they wear, affecting ride comfort and handling stability.
A sliding member with a porous metal layer impregnated with resin and a surface layer of polytetrafluoroethylene (PTFE) and molybdenum disulfide (MoS2), having a Martens hardness of 25 to 45 N/mm² and a creep deformation ratio of 10 to 30%, which maintains consistent friction forces despite wear.
The sliding member maintains constant static and dynamic friction forces, ensuring consistent performance and improved ride comfort and handling stability by adjusting the resin layer's properties through controlled wear.
Smart Images

Figure 2024145012000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates generally to a sliding member, and more particularly to a sliding member of a plain bearing. [Background technology]
[0002] It is desirable to minimize the difference between static and kinetic frictional forces in the sliding members of plain bearings used in shock absorbers of automobiles, etc., in order to improve the ride comfort of passengers. It has been known that the static and kinetic frictional forces of a sliding member can be increased or decreased by adjusting the composition and amount of an additive added to the sliding layer of the sliding member.
[0003] Cited Document 1 discloses a sliding member that can increase static frictional force and control the relationship between static frictional force and kinetic frictional force by adding a predetermined amount of pitch-based carbon fiber to the resin composition that forms the sliding layer. The examples show that the rate of change between static frictional force and kinetic frictional force can be reduced to 20% or less by changing the composition of additives other than fluororesin, pitch-based carbon fiber, aramid fiber, iron oxide, molybdenum disulfide, graphite, zinc (alloy), and resin.
[0004] Cited Document 2 discloses a sliding member capable of controlling the relationship between static friction force and kinetic friction force by forming an uneven surface on the sliding surface and suppressing the formation of an oil film. It describes that by forming an uneven surface on the sliding surface, the rate of change of kinetic friction force relative to static friction force can be suppressed to a smaller value compared to when the sliding surface is smooth. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-108438 A [Patent Document 2] International Publication No. 2012 / 147781 Summary of the Invention [Problem to be solved by the invention]
[0006] The sliding member of the cited document 1 reduces the rate of change between static and kinetic frictional forces by changing the composition of the sliding layer, but the effect is only 20% or less. When the sliding member is used in shock absorbers for automobiles, etc., it is necessary to further reduce the difference between static and kinetic frictional forces in order to improve the ride comfort and steering stability of passengers. In addition, the sliding member of the cited document 2 loses its uneven shape as the sliding surface wears, which may impair the control of static and kinetic frictional forces.
[0007] Therefore, an object of the present invention is to provide a sliding member having a sliding layer in which the difference between static friction force and kinetic friction force is kept small regardless of the degree of wear. [Means for solving the problem]
[0008] In order to achieve the above object, according to the present invention, there is provided a sliding member including a back metal layer and a sliding layer, the sliding layer including a resin material, the surface of the sliding layer being an exposed sliding surface, and the sliding layer having a Martens hardness of 25 to 45 N / mm 2 and a creep deformation rate of 10 to 30%.
[0009] Preferably, the sliding layer includes a porous metal, and the pores of the porous metal are impregnated with a resin material.
[0010] Preferably, the porous metal is exposed on the sliding surface of the sliding layer.
[0011] Preferably, the porous metal is not exposed on the sliding surface of the sliding layer.
[0012] Preferably, the sliding layer further contains hard particles.
[0013] Preferably, the sliding layer further contains a solid lubricant.
[0014] Preferably, the resin material is made of polytetrafluoroethylene (PTFE).
[0015] Preferably, the hard particles include alumina (Al2O3).
[0016] Preferably, the solid lubricant includes molybdenum disulfide (MoS2).
[0017] Preferably, the thickness of the sliding layer is 0.1 to 0.7 mm.
[0018] Preferably, the average particle size of the porous metal is 30 to 110 μm.
[0019] Preferably, the back metal layer has a thickness of 0.3 to 3.5 mm.
[0020] Preferably, the creep deformation ratio of the sliding layer is 15 to 25%. Effect of the Invention
[0021] According to the present invention, the Martens hardness of the sliding layer is set to 25 to 45 N / mm 2 In addition, by adjusting the creep deformation ratio to 10-30%, it is possible to provide a sliding member in which the difference between the static friction force and the kinetic friction force of the sliding surface is kept small. Even when wear of the sliding surface progresses, the Martens hardness and creep deformation ratio of the sliding layer do not change, so that the static friction force, the kinetic friction force, and the difference between the static friction force and the kinetic friction force of the sliding surface are constant, and the performance as a sliding member is maintained.
[0022] The invention and its advantages will be explained in more detail below with reference to the accompanying drawings, which show non-limiting examples for illustrative purposes only, and in which: [Brief description of the drawings]
[0023] [Figure 1] 1 is a schematic cross-sectional view of a sliding member according to an embodiment of the present invention; [Diagram 2] FIG. 4 is a schematic cross-sectional view of another sliding member according to an embodiment of the present invention. [Diagram 3]FIG. 11 is a schematic cross-sectional view of yet another slide member according to an embodiment of the present invention. [Figure 4] FIG. 11 is a schematic cross-sectional view of yet another slide member according to an embodiment of the present invention. [Diagram 5] 1 shows a cross section of a member and a sizing roller in a rolling process according to an embodiment of the present invention. [Figure 6] 4 shows creep test results according to one embodiment of the present invention. [Figure 7] 1 is a schematic cross-sectional view of a performance evaluation test machine according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments.
[0025] The structure and manufacturing method of a slide member 1 according to an embodiment of the present invention will be described in detail below.
[0026] (Structure of sliding members) Fig. 1 is a schematic cross-sectional view of a slide member 1. The slide member 1 includes a back metal layer 2 and a slide layer 3. The slide layer 3 includes a resin layer 4 containing a resin material, and the upper surface of the resin layer 4 exposed to the outside serves as a slide surface 6. The slide member 1 shown in Fig. 1 is formed in a flat shape, but the shape of the slide member 1 is not limited to this and may be a curved shape.
[0027] FIG. 2 is a schematic cross-sectional view of another sliding member 1. The sliding member 1 includes a back metal layer 2 and a sliding layer 3. The sliding layer 3 includes a resin layer 4 and a metal layer 5. The porous metal material 5a of the metal layer 5 may be spherical as shown in FIG. 2, or may be of another shape. The resin material 5b is impregnated into the upper surface of the metal layer 5 and is further deposited on the metal layer 5 to form the resin layer 4. The upper surface of the resin layer 4 is the sliding surface 6 exposed to the outside. The sliding member 1 shown in FIG. 2 is formed in a flat shape, but may be curved.
[0028] In FIG. 2, the metal layer 5 is completely covered by the resin layer 4, but a part of the upper surface of the metal layer 5 may be exposed to the outside to become a part of the sliding surface 6. For example, as shown in FIG. 3, a part of the resin layer 4 may be formed in a concave shape to expose a part of the upper surface of the metal layer 5. Alternatively, the amount of the resin material 5b impregnated into the porous metal material 5a may be adjusted so that the resin material 5b is impregnated to a height equivalent to that of the upper surface of the porous metal material 5a, as shown in FIG. 4. In any case, when the upper surface of the metal layer 5 is exposed, it is preferable that the height of the porous metal material 5a is equal to or less than the height of the upper surface of the resin layer 4. The upper surface of the metal layer 5 and the upper surface of the resin material 5b may both be flat or curved.
[0029] The slide member 1 shown in Figures 1 to 4 has a two-layer structure in which a resin layer 4 is laminated on a back metal layer 2, or a three-layer structure in which a resin layer 4 and a metal layer 5 are laminated on a back metal layer 2, but the structure of the slide member 1 of the present invention is not limited to these. For example, in Figure 2, in addition to the resin layer 4 and the metal layer 5, another resin layer and a metal layer may be provided on the opposite side of the back metal layer 2. In this case, the slide member 1 has sliding surfaces on both sides.
[0030] (Sliding material) Carbon steel, stainless steel, aluminum alloy, copper alloy, etc. can be used for the back metal layer 2. Bronze alloy, brass alloy, other porous metal material such as copper alloy (Bi, Ni, etc.) can be used for the metal layer 5. The resin material constituting the resin layer 4 and the resin material impregnating the metal layer 5 can be made of polytetrafluoroethylene (PTFE) as a base resin, to which 1 to 20% of a solid lubricant such as molybdenum disulfide (MoS2), graphite, boron nitride, etc. is added, and hard particles such as alumina (Al2O3) are added at a rate of 0 to 20%.
[0031] (Thickness of sliding member) In this embodiment, the thickness of the back metal layer 2 may be, for example, 0.3 to 3.5 mm. The thickness of the sliding layer 3 may be, for example, 0.1 to 0.7 mm when the sliding layer 3 includes the resin layer 4 and the metal layer 5, and may be, for example, 0.1 to 0.5 mm when the sliding layer 3 includes only the resin layer 4 and does not include the metal layer 5. When the sliding layer 3 does not include the resin layer 4 but includes only the metal layer 5, the thickness of the metal layer 5 may be, for example, 0.1 to 0.4 mm. The average grain size of the metal layer 5 after sintering may be 30 to 110 μm.
[0032] (Method of manufacturing slide member) The sliding member 1 is manufactured by the following manufacturing process. (1) MoS2 is added to PTFE in a mixing ratio of n, and then the mixture is stirred and mixed to produce a resin material. (2) A porous copper-tin alloy layer is provided on the surface of a backing metal made of carbon steel, and the resin material obtained in step (1) is applied to this (member 10). This is then rolled with a pressure roller to fill the pores in the porous copper-tin alloy layer with the resin material, and to form a resin layer 4 of uniform thickness on the surface of the porous copper-tin alloy layer. (3) The member obtained in step (2) is sintered in a heating sintering furnace, cooled, and then processed to a specified size by size adjustment rollers. (4) The member obtained in step (3) is formed into a cylindrical or semicircular shape.
[0033] In the above step (1), the larger the mixing ratio n of MoS2 to PTFE, the higher the Martens hardness of the resin layer 4 of the slide member 1. In order to set the static friction force of the slide surface 6, which is the upper surface of the resin layer 4, within a predetermined range, the Martens hardness of the resin layer 4 is set to 25 to 45 N / mm 2 It is desirable to do so.
[0034] FIG. 5 shows a cross section of the member and the size adjustment roller in the rolling process of the above step (3). The member 10 is sandwiched between two rollers A and rolled. In FIG. 5, hi is the thickness of the member 10 before rolling, ho is the thickness of the member after rolling, R is the radius of the roller A, l is the roll contact length, and V is the speed of the roll surface. The rolling reduction r of the member 10 is calculated as r=(hi-ho) / hi, and the deformation time t of the member 10 is calculated as t=l / V. Here, the roll contact length l may be approximated by l=√(R(hi-ho)). At the stage of processing to a predetermined dimension by the size adjustment roller in the above step (3), the creep deformation rate is adjusted, but it is possible to adjust the creep deformation rate by providing another rolling process between the above step (3) and the above step (4).
[0035] By changing the rolling reduction rate r and deformation time t of the member 10, the creep deformation ratio of the resin layer 4 of the sliding member 1 can be adjusted. When the creep deformation ratio of the resin layer 4 increases, the behavior of the resin layer 4 becomes viscoelastic, and the kinetic friction force of the sliding surface 6 increases. In order to increase the kinetic friction force of the sliding surface 6 and bring it closer to the static friction force, the creep deformation ratio is set to 10% or more. When the creep deformation ratio of the resin layer 4 is set to 15% or more, the kinetic friction force of the sliding surface 6 becomes even larger. On the other hand, when the creep deformation ratio of the resin layer 4 exceeds 30%, it becomes difficult to shape the sliding surface 6 after rolling. In addition, when the sliding member 1 is used as a material for a shock absorber, it is preferable that the creep deformation ratio of the resin layer 4 is set to 25% or less in order to ensure a certain level of resin strength.
[0036] When rolling the member 10, molecular chains of the resin may be cut, causing cracks to occur inside the resin layer 4. In order to suppress such cracks, it is preferable to set the rolling reduction rate r to 5 to 8% and the deformation time t to 0.05 sec or more. By performing rolling under such relatively gentle conditions, it is possible to suppress the occurrence of cracks inside the resin layer 4 while maintaining the resin strength and creep deformation rate at a certain level or higher.
[0037] In this manner, by adjusting the three parameters of the mixture ratio n of MoS2 to PTFE in the resin layer 4, the rolling reduction ratio r of the member 10, and the deformation time t of the slide member 1, the Martens hardness and the creep deformation rate of the resin layer 4 after the rolling process can be changed.
[0038] (Method of measuring Martens hardness and creep deformation rate) The Martens hardness and creep deformation ratio of the sliding member 1 can be measured by a measurement method conforming to the international standard ISO14577 for microindentation testing. The test was performed from the cross-sectional direction of the resin layer 4 using a Shimadzu Dynamic Ultra-Microhardness Tester DUH-211 manufactured by Shimadzu Corporation as the test device, with a maximum test force of 5 mN and a holding time of 60 seconds. The Martens hardness and creep deformation ratio did not change significantly before and after the shape adjustment in the above manufacturing process (4).
[0039] The Martens hardness HM is calculated from the test load P and the surface area A penetrated by the indenter as HM=P / A.
[0040] The results of the creep test are shown in Figure 6. The symbols in Figure 6 are as follows: Horizontal axis (h): Depth Vertical axis (F): Load t1: Start holding t2: End of hold h1: Displacement when test load is reached h2: Displacement after holding The creep deformation ratio C (%) is calculated as C = (h2-h1) / h1 x 100. EXAMPLES
[0041] (Performance evaluation test) In order to evaluate the static friction force, kinetic friction force, and the rate of change between the static friction force and the kinetic friction force of the sliding member according to the present invention, performance evaluation tests were carried out for Examples 1 to 6 and Comparative Examples 1 to 4.
[0042] 7 shows a schematic cross-sectional view of a performance evaluation test machine 100. The test machine 100 includes a laser displacement meter 101, a ball screw motor 102, a load cell 103, a test shaft 104, a test bush 105, a vertical guide 106, a reflector 107, and a spring 108. The test bush 105 is a cylindrical shape having an inner diameter of 22 mm and an axial length of 15 mm, which is obtained by processing the sliding member manufactured by the above-mentioned manufacturing steps (1) to (4). The test bush 105 is assembled in the test machine 100, and the test bush 105 is caused to slide back and forth in the horizontal direction while a load Fa is applied vertically upward from below, and the horizontal movement distance of the test bush 105 is measured by the laser displacement meter 101.
[0043] (Test conditions) Load: 490N Sliding speed: 1mm / sec Stroke: 15mm Lubricant: Shock absorber oil Static friction force: Calculate by adding the maximum values of the forward and backward movements and dividing by 2 Kinetic friction: Calculate by adding the friction forces at the center of the stroke on the forward and backward strokes and dividing the sum by 2 Rate of change (%): (Static friction force - Dynamic friction force) / Static friction force x 100
[0044] The manufacturing conditions and test results of the present Examples 1 to 6 and Comparative Examples 1 to 4 are shown in Table 1-2. In Table 2, the "static friction force" was evaluated as "good" when the value was in the range of 30N or more and 60N or less, and was evaluated as "poor" when the value was outside the range. The "rate of change" was evaluated as "good" when the ratio of the difference between the static friction force and the kinetic friction force to the static friction force was 13% or less, as "good" when it was 13 to 15%, and as "poor" when it exceeded 15%. In addition, the resin layer peeled off when the test piece was processed into a cylindrical shape in Comparative Example 4, so evaluation could not be performed. [Table 1]
[0045] [Table 2]
[0046] As shown in Table 2, in Examples 1 to 6, the magnitude of static friction force and the rate of change between static friction force and kinetic friction force are within the standards. In Comparative Example 1, the Martens hardness is small, and the static friction force is outside the standards. In Comparative Example 2, the Martens hardness is large, and the static friction force is outside the standards. In Comparative Example 3, the creep deformation rate is small, and the rate of change is outside the standards.
[0047] In this way, by setting the MoS2 content in the resin layer to 5-15%, the rolling reduction to 5-8%, and the deformation time to 0.05 seconds or more, the Martens hardness is 25-45N / mm 2 Moreover, it was found that a sliding layer with a creep deformation rate of 10 to 30% was obtained, and the rate of change between static friction force and kinetic friction force could be kept within a desired range.
[0048] The above describes in detail the embodiments and examples of the present invention with reference to the drawings and in relation to the performance evaluation tests. However, the specific configurations are not limited to these, and modifications that do not depart from the gist of the present invention described in the claims are included in the present invention. [Explanation of symbols]
[0049] 1 Sliding member 2 Backing layer 3. Sliding layer 4 Resin layer 5 metal layer 5a Porous metal material 5b Resin material 6 Sliding surface 10. Materials 100 Testing Machine 101 Laser Displacement Meter 102 Ball screw motor 103 Load Cell 104 Test axis 105 Test bush 106 Up and down guide 107 Reflector 108 Spring
Claims
1. A sliding member including a backing metal layer and a sliding layer, The sliding layer includes a resin material, The surface of the sliding layer is an exposed sliding surface, The sliding layer has a Martens hardness of 25 to 45 N / mm 2 and a creep deformation rate of 10 to 30%.
2. 2. The sliding member according to claim 1, wherein the sliding layer includes a porous metal, and the pores of the porous metal are impregnated with the resin material.
3. The slide member according to claim 2 , wherein the porous metal is exposed on the sliding surface of the slide layer.
4. The sliding member according to claim 2 , wherein the porous metal is not exposed on the sliding surface of the sliding layer.
5. The sliding member according to claim 1 or 2, wherein the sliding layer further comprises hard particles.
6. The sliding member according to claim 1 or 2, wherein the sliding layer further comprises a solid lubricant.
7. 3. The sliding member according to claim 1, wherein the resin material is made of polytetrafluoroethylene (PTFE).
8. The hard particles are made of alumina (Al 2 O 3 6. The sliding member according to claim 5, comprising:
9. The solid lubricant is molybdenum disulfide (MoS 2 7. The sliding member according to claim 6, comprising:
10. 3. The sliding member according to claim 1, wherein the sliding layer has a thickness of 0.1 to 0.7 mm.
11. 3. The sliding member according to claim 2, wherein the average particle size of the porous metal is 30 to 110 μm.
12. 3. The sliding member according to claim 1, wherein the back metal layer has a thickness of 0.3 to 3.5 mm.
13. 3. The sliding member according to claim 1, wherein the creep deformation rate of the sliding layer is 15 to 25%.
Citation Information
Patent Citations
Multi-layer resin bearing
JP2004156650A
Slide member and shaft bearing
JP2019108438A
Process cartridge, image forming apparatus, and image forming method
JP2021012342A
Slide member
JP2023005362A
Sliding member
WO2012147781A1
Cited By
Sliding member
JP2026138212A
Sliding member
JP7939421B2